Flame-retardant antibacterial polycarbonate resin composition and molded product composed of the same

A polycarbonate resin composition with rubber-containing graft polymers, silver-supported zirconium phosphate, and phosphorus-based flame retardants addresses the lack of impact resistance and antibacterial durability in existing polycarbonate resins, providing enhanced flame retardancy and sustained antibacterial properties for durable applications.

JP2024144801APending Publication Date: 2024-10-15TEIJIN LTD

Patent Information

Application Number
JP2023056915
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing polycarbonate resin compositions lack sufficient impact resistance, flame retardancy, and antibacterial durability, particularly when exposed to environments with water and sunlight, and existing antibacterial agents do not effectively maintain these properties over time.

Method used

A flame-retardant and antibacterial polycarbonate resin composition is formulated using rubber-containing graft polymers, silver-supported zirconium phosphate antibacterial agents, silicate minerals, phosphorus-based flame retardants, and anti-drip agents, with specific ratios and components to enhance impact resistance and maintain antibacterial properties.

Benefits of technology

The composition achieves high flame retardancy, impact resistance, and stable antibacterial properties under various environmental conditions, suitable for applications requiring durability and hygiene, such as plastic parts in public use and electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144801000001
    Figure 2024144801000001
  • Figure 2024144801000002
    Figure 2024144801000002
  • Figure 2024144801000003
    Figure 2024144801000003
Patent Text Reader

Abstract

To provide a flame-retardant antibacterial polycarbonate resin composition that exhibits enhanced antibacterial properties and extended antibacterial durability while maintaining high flame retardancy and impact resistance, and a molded product composed of the same.SOLUTION: A flame-retardant antibacterial polycarbonate resin composition comprises, based on (A) 100 pts.wt. of a polycarbonate resin (component A), (B) a rubber-containing graft polymer (component B) of 1-70 pts.wt., (C) a silver-carrying zirconium phosphate antibacterial agent (component C) of 0.2-7 pts.wt., (D) a silicate mineral (component D) of 8-90 pts.wt., (E) a phosphorus-based flame retardant (component E) of 8-70 pts.wt. and (F) a drip inhibitor (component F) of 0.2-2 pts.wt.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a flame-retardant and antibacterial polycarbonate resin composition which maintains high flame retardancy and impact resistance while exhibiting excellent antibacterial activity and durability of antibacterial activity, and to a molded article made of the same. [Background technology]

[0002] Polycarbonate resins are generally used in many applications, such as machine parts, automobile parts, electric and electronic parts, and office equipment parts, due to their excellent properties, such as excellent transparency, impact resistance, heat resistance, dimensional stability, and flame retardancy. In recent years, in order to prevent the spread of known and unknown pathogens, as well as in consideration of hygiene and cleanliness, there is a demand for materials with antibacterial properties for the exterior and various parts of products that can be used by an unspecified number of people, such as home appliances such as toilets, home appliances such as refrigerators and air conditioners, medical equipment, ATMs (automated teller machines) installed in convenience stores, POS terminals, mobile phones, and smartphones.

[0003] As a method for imparting antibacterial properties to polycarbonate resin, a method of adding various phosphorus-based or phenol-based antioxidants, heat stabilizers, and acid-modified olefin waxes to inorganic antibacterial agents (for example, calcium phosphate, zeolite, zirconium phosphate, etc. carrying antibacterial metal ions such as silver, copper, and zinc) has been disclosed (see Patent Documents 1 to 3), but the mechanical properties of the polycarbonate resin composition, particularly the flame retardancy and impact resistance, were not taken into consideration, and the antibacterial properties were not sufficient. As a method for improving antibacterial properties, a method of using silver-based and zinc-based antibacterial agents in combination has also been disclosed (see Patent Document 4), but the various properties when blended with polycarbonate resin were not sufficient, and the focus was only on the initial antibacterial properties of the molded product of the resin composition, and the stable expression of antibacterial properties when the molded product of the resin composition is used as an exterior or part in various products in a real environment, that is, antibacterial sustainability (antibacterial properties in an environment exposed to water and sunlight) was not discussed. As methods for imparting antibacterial properties to polycarbonate resin without impairing its characteristics, a method of adding an antibacterial agent containing glass that elutes silver ions (see Patent Document 5) and a method of blending a zinc-based glass antibacterial agent and a silver-based zirconium phosphate antibacterial agent in a specific ratio (see Patent Document 6) have been disclosed. However, although these methods maintain impact resistance and provide a certain degree of flame retardancy, the durability of the antibacterial properties is insufficient. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 6-240125 [Patent Document 2] Japanese Patent Application Publication No. 10-168294 [Patent Document 3] Japanese Patent Application Publication No. 11-323117 [Patent Document 4] JP 2007-217300 A [Patent Document 5] JP 2011-137068 A [Patent Document 6] JP 2017-132913 A Summary of the Invention [Problem to be solved by the invention]

[0005] In view of the above, an object of the present invention is to provide a flame-retardant, antibacterial polycarbonate resin composition that maintains high flame retardancy and impact resistance while exhibiting excellent antibacterial activity and antibacterial activity durability, and a molded article made of the same. [Means for solving the problem]

[0006] As a result of intensive research conducted by the present inventors to solve the above problems, they discovered that by adding a rubber-containing graft polymer, a silver-supported zirconium phosphate antibacterial agent, a silicate mineral, a phosphorus-based flame retardant and an anti-drip agent in specific compounding amounts to a polycarbonate resin, it is possible to obtain a flame-retardant, antibacterial resin composition that maintains high flame retardancy and impact resistance while exhibiting excellent antibacterial activity and antibacterial activity durability, and thus completed the present invention.

[0007] According to the present invention, the above problems are solved by the following configuration. (Configuration 1) A flame-retardant, antibacterial polycarbonate resin composition comprising 100 parts by weight of (A) polycarbonate resin (component A), 1 to 70 parts by weight of (B) rubber-containing graft polymer (component B), 0.2 to 7 parts by weight of (C) silver-supported zirconium phosphate antibacterial agent (component C), 8 to 90 parts by weight of (D) silicate mineral (component D), 8 to 70 parts by weight of (E) phosphorus-based flame retardant (component E), and 0.2 to 2 parts by weight of (F) anti-drip agent (component F). (Configuration 2) 2. The flame-retardant antibacterial polycarbonate resin composition according to configuration 1, characterized in that it contains 0.01 to 10 parts by weight of an adhesion improver (G) (Component G) per 100 parts by weight of Component A. (Configuration 3) 3. The flame-retardant, antibacterial polycarbonate resin composition according to claim 1 or 2, wherein component B is at least one resin selected from the group consisting of ABS resin, MBS resin, and MB resin. (Configuration 4) The flame-retardant antibacterial polycarbonate resin composition according to any one of Configurations 1 to 3, characterized in that the C component is a silver-supported zirconium phosphate antibacterial agent having an average particle diameter (D50) measured by the laser diffraction / scattering method of 1 to 3 μm. (Configuration 5) The flame-retardant antibacterial polycarbonate resin composition according to any one of Configurations 1 to 4, characterized in that the C component is a silver-supported zirconium phosphate antibacterial agent having a silver content of 8 to 12% by weight. (Configuration 6) A molded article obtained by molding the flame-retardant antibacterial polycarbonate resin composition according to any one of Configurations 1 to 5.

Advantages of the Invention

[0008] The flame-retardant antibacterial polycarbonate resin composition of the present invention has high flame retardancy and impact resistance, and satisfies sufficient antibacterial stability and sustainability in various environments. Therefore, it is useful for plastic parts related to toilets and washbasins, exteriors of tablets, notebook computers, smartphones, digital cameras, medical monitors, POS terminals, office equipment, printers, TVs, etc., which can be used and contacted by an unspecified number of people, as well as irons, hair dryers, rice cookers, microwave ovens, air conditioners, air purifiers, negative ion generators, various buttons and switches, doorknobs, amusement-related plastic parts, and various plastic parts related to mobility. In particular, since it can impart high flame retardancy that meets the UL94 combustion standard V-0, it is useful for OA and EE applications. Therefore, the industrial effect achieved by the present invention is remarkable.

Embodiments for Carrying Out the Invention

[0009] Hereinafter, the details of the present invention will be described.

[0010] <Component A: Polycarbonate-based resin> The polycarbonate resin used in the present invention is obtained by reacting a dihydric phenol with a carbonate precursor. Examples of the reaction method include an interfacial polymerization method, a melt transesterification method, a solid-phase transesterification method of a carbonate prepolymer, and a ring-opening polymerization method of a cyclic carbonate compound.

[0011] Representative examples of the dihydric phenols used herein include hydroquinone, resorcinol, 4,4'-biphenol, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)propane (commonly known as bisphenol A), 2,2-bis(4-hydroxy-3-methylphenyl)propane, 2,2-bis(4-hydroxyphenyl)butane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 2,2-bis(4-hydroxyphenyl)pentane, 4,4'-(p-phenylene) Examples of the dihydric phenol include 4,4'-(m-phenylenediisopropylidene)diphenol, 1,1-bis(4-hydroxyphenyl)-4-isopropylcyclohexane, bis(4-hydroxyphenyl)oxide, bis(4-hydroxyphenyl)sulfide, bis(4-hydroxyphenyl)sulfoxide, bis(4-hydroxyphenyl)sulfone, bis(4-hydroxyphenyl)ketone, bis(4-hydroxyphenyl)ester, bis(4-hydroxy-3-methylphenyl)sulfide, 9,9-bis(4-hydroxyphenyl)fluorene, and 9,9-bis(4-hydroxy-3-methylphenyl)fluorene. The preferred dihydric phenol is a bis(4-hydroxyphenyl)alkane, and among them, bisphenol A is particularly preferred from the viewpoint of impact resistance and is widely used.

[0012] In the present invention, in addition to bisphenol A-based polycarbonate resins, which are general-purpose polycarbonate resins, it is possible to use special polycarbonate resins produced using other dihydric phenols as the A component.

[0013] For example, polycarbonate resins (homopolymers or copolymers) using 4,4'-(m-phenylenediisopropylidene)diphenol (hereinafter sometimes abbreviated as "BPM"), 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane (hereinafter sometimes abbreviated as "Bis-TMC"), 9,9-bis(4-hydroxyphenyl)fluorene and 9,9-bis(4-hydroxy-3-methylphenyl)fluorene (hereinafter sometimes abbreviated as "BCF") as part or all of the dihydric phenol components are suitable for applications where dimensional changes due to water absorption and dimensional stability are particularly demanding. These dihydric phenols other than BPA are preferably used in an amount of 5 mol% or more, particularly 10 mol% or more, of the total dihydric phenol components constituting the polycarbonate resin.

[0014] In particular, when high rigidity and better hydrolysis resistance are required, it is particularly suitable that the component A constituting the resin composition is a copolymer polycarbonate resin of the following (1) to (3). (1) A copolymerized polycarbonate resin in which, relative to 100 mol % of a dihydric phenol component constituting the polycarbonate resin, BPM is 20 to 80 mol % (more preferably 40 to 75 mol %, and even more preferably 45 to 65 mol %) and BCF is 20 to 80 mol % (more preferably 25 to 60 mol %, and even more preferably 35 to 55 mol %). (2) A copolymerized polycarbonate resin in which, relative to 100 mol % of a dihydric phenol component constituting the polycarbonate resin, BPA is 10 to 95 mol % (more preferably 50 to 90 mol %, and even more preferably 60 to 85 mol %) and BCF is 5 to 90 mol % (more preferably 10 to 50 mol %, and even more preferably 15 to 40 mol %). (3) A copolymer polycarbonate resin in which, relative to 100 mol % of the dihydric phenol component constituting the polycarbonate resin, BPM is 20 to 80 mol % (more preferably 40 to 75 mol %, and even more preferably 45 to 65 mol %) and Bis-TMC is 20 to 80 mol % (more preferably 25 to 60 mol %, and even more preferably 35 to 55 mol %).

[0015] These special polycarbonate resins may be used alone or in a suitable mixture of two or more kinds, or may be used in a mixture with a commonly used bisphenol A type polycarbonate resin.

[0016] The production methods and properties of these special polycarbonate resins are described in detail in, for example, JP-A-6-172508, JP-A-8-27370, JP-A-2001-55435, and JP-A-2002-117580.

[0017] Among the various polycarbonate resins mentioned above, those in which the copolymer composition and the like are adjusted to bring the water absorption rate and Tg (glass transition temperature) into the ranges described below have good hydrolysis resistance of the polymer itself and are also remarkably excellent in terms of low warpage after molding, and are therefore particularly suitable in fields where dimensional stability is required. (i) a polycarbonate having a water absorption rate of 0.05 to 0.15%, preferably 0.06 to 0.13%, and a Tg of 120 to 180° C., or (ii) A polycarbonate resin having a Tg of 160 to 250° C., preferably 170 to 230° C., and a water absorption of 0.10 to 0.30%, preferably 0.13 to 0.30%, and more preferably 0.14 to 0.27%.

[0018] Here, the water absorption rate of the polycarbonate resin is a value measured by using a disk-shaped test piece having a diameter of 45 mm and a thickness of 3.0 mm and immersing it in water at 23°C for 24 hours in accordance with ISO62-1980, and measuring the moisture content. Also, Tg (glass transition temperature) is a value determined by differential scanning calorimetry (DSC) measurement in accordance with JIS K7121.

[0019] The carbonate precursor may be a carbonyl halide, a carbonic acid diester or a haloformate, and specific examples thereof include phosgene, diphenyl carbonate or a dihaloformate of a dihydric phenol.

[0020] When the dihydric phenol and carbonate precursor are used to produce a polycarbonate resin by interfacial polymerization, a catalyst, a terminal terminator, an antioxidant for preventing oxidation of the dihydric phenol, etc. may be used as necessary. The polycarbonate resin of the present invention includes a branched polycarbonate resin copolymerized with a trifunctional or higher polyfunctional aromatic compound, a polyester carbonate resin copolymerized with an aromatic or aliphatic (including alicyclic) bifunctional carboxylic acid, a copolymerized polycarbonate resin copolymerized with a bifunctional alcohol (including alicyclic), and a polyester carbonate resin copolymerized with such a bifunctional carboxylic acid and a bifunctional alcohol. The polycarbonate resin may also be a mixture of two or more of the obtained polycarbonate resins.

[0021] The branched polycarbonate resin can impart drip prevention properties to the resin composition of the present invention. Examples of trifunctional or higher polyfunctional aromatic compounds used in such branched polycarbonate resins include phloroglucin, phloroglucide, 4,6-dimethyl-2,4,6-tris(4-hydroxyphenyl)heptene-2,2,4,6-trimethyl-2,4,6-tris(4-hydroxyphenyl)heptane, 1,3,5-tris(4-hydroxyphenyl)benzene, 1,1,1-tris(4-hydroxyphenyl)ethane, 1,1,1-tris(3,5-dimethyl-4-hydroxyphenyl)ethane, 2,6-bis(2-hydroxy-5-methylbenzyl)-4-methylphenol, 4-{4-[1,1-bis(4- Examples of the trisphenols include trisphenols such as 1,4-dimethylbenzylphenol, tetra(4-hydroxyphenyl)methane, bis(2,4-dihydroxyphenyl)ketone, 1,4-bis(4,4-dihydroxytriphenylmethyl)benzene, trimellitic acid, pyromellitic acid, benzophenonetetracarboxylic acid, and acid chlorides thereof. Among these, 1,1,1-tris(4-hydroxyphenyl)ethane and 1,1,1-tris(3,5-dimethyl-4-hydroxyphenyl)ethane are preferred, and 1,1,1-tris(4-hydroxyphenyl)ethane is particularly preferred.

[0022] The constituent units derived from a polyfunctional aromatic compound in the branched polycarbonate resin preferably account for 0.01 to 1 mol %, more preferably 0.05 to 0.9 mol %, and even more preferably 0.05 to 0.8 mol %, based on a total of 100 mol % of the constituent units derived from a dihydric phenol and the constituent units derived from the polyfunctional aromatic compound.

[0023] In particular, in the case of the melt transesterification method, branched structural units may be generated as a side reaction, and the amount of such branched structural units is preferably 0.001 to 1 mol %, more preferably 0.005 to 0.9 mol %, and even more preferably 0.01 to 0.8 mol %, based on the total of 100 mol % including the structural units derived from the dihydric phenol. 1 It can be calculated by H-NMR measurement.

[0024] The aliphatic difunctional carboxylic acid is preferably an α,ω-dicarboxylic acid. Examples of the aliphatic difunctional carboxylic acid include linear saturated aliphatic dicarboxylic acids such as sebacic acid (decanedioic acid), dodecanedioic acid, tetradecanedioic acid, octadecanedioic acid, and icosane diacid, and alicyclic dicarboxylic acids such as cyclohexane dicarboxylic acid. The bifunctional alcohol is more preferably an alicyclic diol, such as cyclohexane dimethanol, cyclohexane diol, and tricyclodecane dimethanol.

[0025] The reaction modes of the methods for producing the polycarbonate resin of the present invention, such as the interfacial polymerization method, the melt transesterification method, the carbonate prepolymer solid-phase transesterification method, and the ring-opening polymerization method of a cyclic carbonate compound, are well known in various literatures and patent publications.

[0026] The viscosity average molecular weight (M) of the polycarbonate resin is not particularly limited, but is preferably 1.8×10 4 ~4.0×10 4 and more preferably 2.0×10 4~3.5×10 4 , and more preferably 2.2×10 4 ~3.0×10 4 The viscosity average molecular weight is 1.8 × 10 4 Polycarbonate resins with a viscosity average molecular weight of less than 4.0×10 may not provide good mechanical properties. 4 Resin compositions obtained from polycarbonate-based resins exceeding this limit are inferior in terms of flowability during injection molding and therefore are inferior in versatility.

[0027] The polycarbonate resin may be a mixture of resins having a viscosity average molecular weight outside the above range. 4 ) the entropy elasticity of the resin is improved. As a result, good molding processability is exhibited in gas-assisted molding and foam molding, which are sometimes used when molding reinforced resin materials into structural members. Such improvement in molding processability is even better than that of the branched polycarbonate resin. In a more preferred embodiment, component A has a viscosity average molecular weight of 7×10 4 ~3×10 5 Polycarbonate resin (A-1-1-1 component) and viscosity average molecular weight of 1 × 10 4 ~3×10 4 The viscosity average molecular weight of the polycarbonate resin (A-1-1-2 component) is 1.6 × 10 4 ~3.5×10 4 It is also possible to use a polycarbonate-based resin (A-1-1 component) (hereinafter sometimes referred to as a "polycarbonate-based resin containing a high molecular weight component").

[0028] In the polycarbonate resin containing a high molecular weight component (A-1-1 component), the molecular weight of the A-1-1-1 component is 7×10 4 ~2×10 5 is preferable, and more preferably 8×10 4 ~2×10 5 , and more preferably 1×10 5 ~2×10 5 , particularly preferably 1×10 5~1.6×10 5 The molecular weight of component A-1-1-2 is 1×10 4 ~2.5×10 4 is preferable, and more preferably 1.1×10 4 ~2.4×10 4 , and more preferably 1.2×10 4 ~2.4×10 4 , particularly preferably 1.2×10 4 ~2.3×10 4 It is.

[0029] The high molecular weight component-containing polycarbonate resin (A-1-1 component) can be obtained by mixing the A-1-1-1 and A-1-1-2 components in various ratios and adjusting to satisfy a predetermined molecular weight range. Preferably, the A-1-1-1 component is 2 to 40% by weight, more preferably 3 to 30% by weight, even more preferably 4 to 20% by weight, and particularly preferably 5 to 20% by weight, of 100% by weight of the A-1-1 component.

[0030] Methods for preparing the A-1-1 component include (1) a method in which the A-1-1-1 and A-1-1-2 components are polymerized independently and then mixed; (2) a method in which a polycarbonate resin that shows multiple polymer peaks in a molecular weight distribution chart determined by GPC, as typified by the method shown in JP-A-5-306336, is produced in the same system, and the polycarbonate resin is produced so as to satisfy the conditions of the A-1-1 component of the present invention; and (3) a method in which the polycarbonate resin obtained by the above production method (production method (2)) is mixed with the A-1-1-1 and / or A-1-1-2 components produced separately.

[0031] The viscosity average molecular weight in the present invention is calculated by the specific viscosity (η SP ) was measured at 20°C using an Ostwald viscometer from a solution of 0.7 g of polycarbonate resin dissolved in 100 ml of methylene chloride. Specific viscosity (η SP)=(t-t0) / t0 [t0 is the number of seconds that methylene chloride falls, and t is the number of seconds that the sample solution falls] The specific viscosity (η SP ) and calculate the viscosity average molecular weight M using the following formula: η SP / c=[η]+0.45×[η] 2 c (where [η] is the intrinsic viscosity) [η]=1.23×10 -4 M 0.83 c=0.7

[0032] The viscosity average molecular weight of the polycarbonate resin in the flame-retardant antibacterial polycarbonate resin composition of the present invention is calculated as follows. That is, the composition is mixed with methylene chloride in an amount 20 to 30 times its weight, and the soluble matter in the composition is dissolved. The soluble matter is collected by filtration through Celite. The solvent in the resulting solution is then removed. The solid after the solvent removal is thoroughly dried to obtain a solid of components that dissolve in methylene chloride. 0.7 g of the solid is dissolved in 100 ml of methylene chloride to obtain a solution, and the specific viscosity at 20°C is determined in the same manner as above, and the viscosity average molecular weight M is calculated from the specific viscosity in the same manner as above.

[0033] The polycarbonate-based resin of the present invention may be a polycarbonate-polydiorganosiloxane copolymer resin. The polycarbonate-polydiorganosiloxane copolymer resin is preferably a copolymer resin prepared by copolymerizing a dihydric phenol represented by the following general formula (1) and a hydroxyaryl-terminated polydiorganosiloxane represented by the following general formula (3).

[0034] [ka] [In the above general formula (1), R 1 and R 2each independently represents a group selected from the group consisting of a hydrogen atom, a halogen atom, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a cycloalkyl group having 6 to 20 carbon atoms, a cycloalkoxy group having 6 to 20 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an aryl group having 6 to 14 carbon atoms, an aryloxy group having 6 to 14 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, an aralkyloxy group having 7 to 20 carbon atoms, a nitro group, an aldehyde group, a cyano group, and a carboxy group, and when there are a plurality of each, they may be the same or different, e and f each represent an integer of 1 to 4, and W represents a single bond or at least one group selected from the group consisting of groups represented by the following general formula (2):

[0035] [ka] [In the above general formula (2), R 11 ,R 12 ,R 13 ,R 14 ,R 15 ,R 16 ,R 17 and R 18 each independently represents a group selected from the group consisting of a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, an aryl group having 6 to 14 carbon atoms, and an aralkyl group having 7 to 20 carbon atoms; R 19 and R 20 each independently represents a group selected from the group consisting of a hydrogen atom, a halogen atom, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, a cycloalkyl group having 6 to 20 carbon atoms, a cycloalkoxy group having 6 to 20 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an aryl group having 6 to 14 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, an aralkyloxy group having 7 to 20 carbon atoms, a nitro group, an aldehyde group, a cyano group, and a carboxy group, and when there are a plurality of groups, they may be the same or different, g is an integer from 1 to 10, and h is an integer from 4 to 7.

[0036] [ka] [In the above general formula (3), R 3 , R 4 , R 5 , R 6 , R 7 and R 8 are each independently a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 12 carbon atoms; R 9 and R 10 are each independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms, p is a natural number, q is 0 or a natural number, and p+q is a natural number of 10 to 300. X is a divalent aliphatic group having 2 to 8 carbon atoms.]

[0037] Examples of the dihydric phenol (I) represented by the general formula (1) include 4,4'-dihydroxybiphenyl, bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 2,2-bis(4-hydroxy-3,3'-biphenyl)propane, 2,2- Bis(4-hydroxy-3-isopropylphenyl)propane, 2,2-bis(3-t-butyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)octane, 2,2-bis(3-bromo-4-hydroxyphenyl)propane, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, 2,2-bis(3-cyclohexyl-4-hydroxyphenyl)propane, 1,1-bis(3-cyclohexyl-4-hydroxyphenyl)cyclohexane, bis(4-hydroxyphenyl)propane, 4,4'-dihydroxydiphenylmethane, 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)cyclopentane, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxy-3,3'-dimethyldiphenyl ether, 4,4'-sulfonyldiphenol, 4,4'-dihydroxydiphenyl sulfoxide, 4,4'-dihydroxydiphenyl sulfide, 2,2'- Dimethyl-4,4'-sulfonyldiphenol, 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfoxide, 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfide, 2,2'-diphenyl-4,4'-sulfonyldiphenol, 4,4'-dihydroxy-3,3'-diphenyldiphenyl sulfoxide, 4,4'-dihydroxy-3,3'-diphenyldiphenyl sulfide, 1,3-bis{2-(4-hydroxyphenyl)propyl}benzene, 1,4-bis{2-(4-hydroxyphenyl)propyl}benzene, 1,Examples of such cyclohexane derivatives include 4-bis(4-hydroxyphenyl)cyclohexane, 1,3-bis(4-hydroxyphenyl)cyclohexane, 4,8-bis(4-hydroxyphenyl)tricyclo[5.2.1.02,6]decane, 4,4'-(1,3-adamantanediyl)diphenol, and 1,3-bis(4-hydroxyphenyl)-5,7-dimethyladamantane. Among these, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 4,4'-sulfonyldiphenol, 2,2'-dimethyl-4,4'-sulfonyldiphenol, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 1,3-bis{2-(4-hydroxyphenyl)propyl}benzene, and 1,4-bis{2-(4-hydroxyphenyl)propyl}benzene are preferred, and 2,2-bis(4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)cyclohexane (BPZ), 4,4'-sulfonyldiphenol, and 9,9-bis(4-hydroxy-3-methylphenyl)fluorene are particularly preferred. Among these, 2,2-bis(4-hydroxyphenyl)propane, which has excellent strength and good durability, is the most suitable. These may be used alone or in combination of two or more kinds.

[0038] As the hydroxyaryl-terminated polydiorganosiloxane represented by the above general formula (3), for example, the compounds shown below are suitably used.

[0039] [ka]

[0040] Hydroxyaryl-terminated polydiorganosiloxane (II) is easily produced by hydrosilylation reaction of phenols having an olefinic unsaturated carbon-carbon bond, preferably vinylphenol, 2-allylphenol, isopropenylphenol, or 2-methoxy-4-allylphenol, with the end of a polysiloxane chain having a predetermined degree of polymerization. Among them, (2-allylphenol)-terminated polydiorganosiloxane and (2-methoxy-4-allylphenol)-terminated polydiorganosiloxane are preferred, and (2-allylphenol)-terminated polydimethylsiloxane and (2-methoxy-4-allylphenol)-terminated polydimethylsiloxane are particularly preferred. The molecular weight distribution (Mw / Mn) of the hydroxyaryl-terminated polydiorganosiloxane (II) is preferably 3 or less. In order to achieve even better low outgassing properties during high-temperature molding and low-temperature impact properties, the molecular weight distribution (Mw / Mn) is more preferably 2.5 or less, and even more preferably 2 or less. If the upper limit of this preferred range is exceeded, the amount of outgassing during high-temperature molding will be large, and low-temperature impact resistance may be poor.

[0041] Furthermore, in order to achieve a high level of impact resistance, the diorganosiloxane polymerization degree (p+q) of the hydroxyaryl-terminated polydiorganosiloxane (II) is suitably 10 to 300. The diorganosiloxane polymerization degree (p+q) is preferably 10 to 200, more preferably 12 to 150, and even more preferably 14 to 100. Below the lower limit of this preferred range, the impact resistance that is a characteristic of the polycarbonate-polydiorganosiloxane copolymer is not effectively exhibited, while above the upper limit of this preferred range, poor appearance appears.

[0042] The polydiorganosiloxane content in the total weight of the polycarbonate-polydiorganosiloxane copolymer resin is preferably 0.1 to 50% by weight. The polydiorganosiloxane content is more preferably 0.5 to 30% by weight, and even more preferably 1 to 20% by weight. At or above the lower limit of this preferred range, excellent impact resistance and flame retardancy are obtained, while at or below the upper limit of this preferred range, a stable appearance that is not easily affected by molding conditions is easily obtained. The polydiorganosiloxane polymerization degree and polydiorganosiloxane content are 1 It can be calculated by H-NMR measurement.

[0043] In the present invention, the hydroxyaryl-terminated polydiorganosiloxane (II) may be used alone or in combination of two or more kinds. In addition, comonomers other than the dihydric phenol (I) and hydroxyaryl-terminated polydiorganosiloxane (II) may be used in an amount of up to 10% by weight based on the total weight of the copolymer, provided that the use does not interfere with the present invention.

[0044] In the present invention, a mixed solution containing an oligomer having a terminal chloroformate group is prepared in advance by reacting a dihydric phenol (I) with a carbonate-forming compound in a mixed solution of a water-insoluble organic solvent and an aqueous alkaline solution.

[0045] In producing an oligomer of the dihydric phenol (I), the entire amount of the dihydric phenol (I) used in the method of the present invention may be converted into an oligomer at once, or a part of it may be added as a post-added monomer as a reaction raw material to the interfacial polycondensation reaction in the latter stage. The post-added monomer is added to quickly advance the polycondensation reaction in the latter stage, and there is no need to add it if it is not necessary. The method of this oligomer formation reaction is not particularly limited, but it is usually preferable to carry out the reaction in a solvent in the presence of an acid binder.

[0046] The proportion of the carbonate ester-forming compound used may be appropriately adjusted in consideration of the stoichiometric ratio (equivalent) of the reaction. When a gaseous carbonate ester-forming compound such as phosgene is used, it is preferable to employ a method of blowing the gaseous compound into the reaction system.

[0047] As the acid binder, for example, an alkali metal hydroxide such as sodium hydroxide or potassium hydroxide, an alkali metal carbonate such as sodium carbonate or potassium carbonate, an organic base such as pyridine, or a mixture thereof can be used. The proportion of the acid binder used can be appropriately determined in consideration of the stoichiometric ratio (equivalent) of the reaction, as described above. Specifically, it is preferable to use 2 equivalents or a slightly excess amount of the acid binder relative to the number of moles of the dihydric phenol (I) used to form the oligomer (usually 1 mole corresponds to 2 equivalents).

[0048] As the solvent, a solvent inert to various reactions, such as those used in the production of known polycarbonate resins, may be used alone or as a mixed solvent. Representative examples include hydrocarbon solvents such as xylene, and halogenated hydrocarbon solvents such as methylene chloride and chlorobenzene. In particular, halogenated hydrocarbon solvents such as methylene chloride are preferably used.

[0049] The reaction pressure for oligomer formation is not particularly limited, and may be normal pressure, elevated pressure, or reduced pressure, but it is usually advantageous to carry out the reaction under normal pressure. The reaction temperature is selected from the range of -20 to 50°C, and since heat is generated during polymerization in many cases, it is desirable to cool the reaction with water or ice. The reaction time depends on other conditions and cannot be generally specified, but is usually carried out for 0.2 to 10 hours. The pH range for the oligomer formation reaction is the same as that of known interfacial reaction conditions, and the pH is always adjusted to 10 or higher.

[0050] In the present invention, after obtaining a mixed solution containing an oligomer of dihydric phenol (I) having terminal chloroformate groups in this manner, the mixed solution is stirred while adding hydroxyaryl-terminated polydiorganosiloxane (II) represented by general formula (3) that has been highly refined to a molecular weight distribution (Mw / Mn) of 3 or less to the dihydric phenol (I), and the hydroxyaryl-terminated polydiorganosiloxane (II) and the oligomer are subjected to interfacial polycondensation to obtain a polycarbonate-polydiorganosiloxane copolymer.

[0051] [ka] (In the above general formula (3), R 3 , R 4 , R 5 , R 6 , R 7 and R 8 are each independently a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 12 carbon atoms; R 9 and R 10 are each independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms, p is a natural number, q is 0 or a natural number, and p+q is a natural number of 10 to 300. X is a divalent aliphatic group having 2 to 8 carbon atoms.

[0052] In carrying out the interfacial polycondensation reaction, an acid binder may be appropriately added in consideration of the stoichiometric ratio (equivalent) of the reaction. For example, alkali metal hydroxides such as sodium hydroxide and potassium hydroxide, alkali metal carbonates such as sodium carbonate and potassium carbonate, organic bases such as pyridine, or mixtures thereof, are used as the acid binder. Specifically, when the hydroxyaryl-terminated polydiorganosiloxane (II) used or a part of the dihydric phenol (I) as described above is added to this reaction stage as a post-added monomer, it is preferable to use 2 equivalents or more of alkali relative to the total mole number of the post-added dihydric phenol (I) and the hydroxyaryl-terminated polydiorganosiloxane (II) (usually 1 mole corresponds to 2 equivalents).

[0053] The polycondensation by the interfacial polycondensation reaction between the oligomer of the dihydric phenol (I) and the hydroxyaryl-terminated polydiorganosiloxane (II) is carried out by vigorously stirring the above mixture.

[0054] In such a polymerization reaction, a terminal terminator or a molecular weight regulator is usually used. Examples of the terminal terminator include compounds having a monovalent phenolic hydroxyl group, such as ordinary phenol, p-tert-butylphenol, p-cumylphenol, tribromophenol, etc., as well as long-chain alkylphenols, aliphatic carboxylic acid chlorides, aliphatic carboxylic acids, hydroxybenzoic acid alkyl esters, hydroxyphenyl alkyl acid esters, and alkyl ether phenols. The amount of the terminal terminator is in the range of 100 to 0.5 mol, preferably 50 to 2 mol, relative to 100 mol of all dihydric phenol compounds used, and it is naturally possible to use two or more compounds in combination.

[0055] To accelerate the polycondensation reaction, a catalyst such as a tertiary amine, such as triethylamine, or a quaternary ammonium salt may be added. The reaction time of such a polymerization reaction is preferably 30 minutes or more, more preferably 50 minutes or more. If desired, a small amount of an antioxidant such as sodium sulfite or hydrosulfide may be added.

[0056] A branching agent can be used in combination with the above dihydric phenol compound to produce a branched polycarbonate-polydiorganosiloxane. Examples of polyfunctional aromatic compounds having three or more functional groups that can be used in such branched polycarbonate-polydiorganosiloxane copolymer resins include phloroglucin, phloroglucide, 4,6-dimethyl-2,4,6-tris(4-hydroxyphenyl)heptene-2,2,4,6-trimethyl-2,4,6-tris(4-hydroxyphenyl)heptane, 1,3,5-tris(4-hydroxyphenyl)benzene, 1,1,1-tris(4-hydroxyphenyl)ethane, 1,1,1-tris(3,5-dimethyl-4-hydroxyphenyl)ethane, 2,6-bis(2-hydroxy-5-methylbenzyl)-4-methylphenol, 4-{4-[1 Examples of the hydroxyphenyl ether include trisphenols such as {α,α-dimethylbenzylphenol}-α-dimethylbenzylphenol, tetra(4-hydroxyphenyl)methane, bis(2,4-dihydroxyphenyl)ketone, 1,4-bis(4,4-dihydroxytriphenylmethyl)benzene, trimellitic acid, pyromellitic acid, benzophenonetetracarboxylic acid, and acid chlorides thereof. Among these, 1,1,1-tris(4-hydroxyphenyl)ethane and 1,1,1-tris(3,5-dimethyl-4-hydroxyphenyl)ethane are preferred, and 1,1,1-tris(4-hydroxyphenyl)ethane is particularly preferred. The proportion of the polyfunctional compound in the branched polycarbonate-polydiorganosiloxane copolymer resin is preferably 0.001 to 1 mol %, more preferably 0.005 to 0.9 mol %, further preferably 0.01 to 0.8 mol %, and particularly preferably 0.05 to 0.4 mol %, based on the total amount of the polycarbonate-polydiorganosiloxane copolymer resin. 1 It can be calculated by H-NMR measurement.

[0057] The reaction pressure may be reduced, normal, or increased, but is usually preferably normal pressure or the reaction system's own pressure. The reaction temperature is selected from the range of -20 to 50°C, and in many cases, since heat is generated during polymerization, it is desirable to cool the reaction system with water or ice. The reaction time varies depending on other conditions such as the reaction temperature and cannot be generally specified, but is usually carried out for 0.5 to 10 hours.

[0058] In some cases, the obtained polycarbonate-polydiorganosiloxane copolymer resin is subjected to a suitable physical treatment (mixing, fractionation, etc.) and / or chemical treatment (polymer reaction, crosslinking treatment, partial decomposition treatment, etc.) to obtain a desired reduced viscosity [η SP It can also be obtained as a polycarbonate-polydiorganosiloxane copolymer resin of formula [1 / c].

[0059] The obtained reaction product (crude product) can be subjected to various post-treatments such as known separation and purification methods to recover a polycarbonate-polydiorganosiloxane copolymer resin of the desired purity (purity). The average size of the polydiorganosiloxane domains in the polycarbonate-polydiorganosiloxane copolymer resin molded product is preferably in the range of 1 to 60 nm. The average size is more preferably 3 to 55 nm, and even more preferably 5 to 50 nm. If it is less than the lower limit of the preferred range, impact resistance and flame retardancy may not be fully exhibited, and if it exceeds the upper limit of the preferred range, impact resistance may not be stably exhibited.

[0060] Furthermore, as the polycarbonate-based resin in the present invention, polycarbonate resins recycled from used products, i.e., recycled polycarbonate resins, can also be used.Preferably used products include soundproof walls, automobile windows, light-transmitting roofing materials, various glazing materials such as automobile sunroofs, transparent members such as windshields and automobile headlamp lenses, containers such as water bottles, light guide plates, eyeglass lenses, and optical recording media.Furthermore, crushed products obtained from non-conforming products, sprues, runners, etc., or pellets obtained by melting them can also be used.

[0061] <Component B: Rubber-containing graft polymer> The flame-retardant and antibacterial polycarbonate resin composition of the present invention contains a rubber-containing graft polymer as Component B. It is preferable from the viewpoints of impact resistance and flame retardancy that such a rubber-containing graft polymer is at least one resin selected from the group consisting of ABS resin, MBS resin, and MB resin.

[0062] <ABS resin> The ABS resin used in the present invention is a mixture of a thermoplastic graft copolymer obtained by graft polymerizing a vinyl cyanide compound and an aromatic vinyl compound onto a diene rubber component and a copolymer of a vinyl cyanide compound and an aromatic vinyl compound. As the diene rubber component forming this ABS resin, for example, rubbers having a glass transition temperature of -30°C or lower such as polybutadiene, polyisoprene, and styrene-butadiene copolymer are used, and the proportion thereof is preferably 5 to 80% by weight, more preferably 8 to 50% by weight, and particularly preferably 10 to 30% by weight in 100% by weight of the ABS resin component. As the vinyl cyanide compound grafted onto the diene rubber component, acrylonitrile can be particularly preferably used. As the aromatic vinyl compound grafted onto the diene rubber component, styrene and α-methylstyrene can be particularly preferably used. The proportion of the components grafted onto such a diene rubber component is preferably 95 to 20% by weight, particularly preferably 50 to 90% by weight in 100% by weight of the ABS resin component. Further, it is preferable that the vinyl cyanide compound is 5 to 50% by weight and the aromatic vinyl compound is 95 to 50% by weight with respect to 100% by weight of the total amount of such a vinyl cyanide compound and aromatic vinyl compound. Further, maleic anhydride, N-substituted maleimide, etc. can be mixed and used for a part of the components grafted onto the above diene rubber component, and the content ratio thereof is preferably 15% by weight or less in the ABS resin component. Further, various conventionally known initiators, chain transfer agents, emulsifiers, etc. used in the reaction can be used as necessary.

[0063] In the ABS resin used in the present invention, the rubber particle size is preferably 0.1 to 5.0 μm, more preferably 0.15 to 1.5 μm, and particularly preferably 0.2 to 0.8 μm. The rubber particle size distribution may be either a single distribution or a distribution having two or more peaks, and the morphology may be either a single phase of rubber particles or a salami structure having an occluded phase around the rubber particles.

[0064] It has been well known that ABS resins contain vinyl cyanide compounds and aromatic vinyl compounds that are not grafted to diene rubber components, and the ABS resin of the present invention may also contain free polymer components generated during such polymerization. The reduced viscosity (30°C) of such a copolymer consisting of a free vinyl cyanide compound and an aromatic vinyl compound is preferably 0.2 to 1.0 dl / g, more preferably 0.3 to 0.7 dl / g, as determined by the method described above.

[0065] The proportion of the grafted vinyl cyanide compound and aromatic vinyl compound is preferably 20 to 200%, more preferably 20 to 70%, in terms of graft rate (wt %) relative to the diene rubber component.

[0066] The ABS resin may be produced by any of the methods of bulk polymerization, suspension polymerization, and emulsion polymerization, but the method of bulk polymerization is particularly preferred. Representative examples of the bulk polymerization method include the continuous bulk polymerization method (so-called Toray method) described in Chemical Engineering, Vol. 48, No. 6, p. 415 (1984), and the continuous bulk polymerization method (so-called Mitsui Toatsu method) described in Chemical Engineering, Vol. 53, No. 6, p. 423 (1989). Any of the ABS resins can be suitably used as the ABS resin of the present invention. The copolymerization method can be either one-stage or multi-stage copolymerization. Also, a blend of the ABS resin obtained by the above production method and a vinyl compound polymer obtained by separately copolymerizing an aromatic vinyl compound and a vinyl cyanide component can be preferably used.

[0067] ABS resin with a reduced amount of alkali (alkaline earth) metal is more suitable in terms of good thermal stability and hydrolysis resistance. The amount of alkali (alkaline earth) metal in the resin is preferably less than 100 ppm, more preferably less than 80 ppm, still more preferably less than 50 ppm, and particularly preferably less than 10 ppm. From this point of view, the ABS resin obtained by the bulk polymerization method is preferably used. Further, in relation to such good thermal stability and hydrolysis resistance, when an emulsifier is used in the ABS resin, the emulsifier is preferably sulfonates, more preferably alkyl sulfonates. When a coagulant is used, sulfuric acid or an alkaline earth metal salt of sulfuric acid is suitable as the coagulant.

[0068] <MB resin and MBS resin> The MB resin and MBS resin used in the present invention are a methyl methacrylate-butadiene copolymer and a methyl methacrylate-butadiene-styrene copolymer, respectively. Such copolymers are graft polymers, and graft polymers having a core-shell structure are more preferred. Further, the content of methyl methacrylate in the MBS resin is preferably 10% by weight or more, more preferably 15% by weight or more, based on 100% by weight of the graft component (in the case of a core-shell type polymer, based on 100% by weight of the shell). In the core-shell type graft polymer, the particle diameter of the core is preferably 240 to 300 nm, more preferably 250 to 290 nm, and still more preferably 260 to 280 nm in terms of the weight average particle diameter. Better impact strength may be achieved within the range of 240 to 300 nm. Further, the particle size distribution is desirably a multi-modal type having two peaks, and particularly preferably a multi-modal type having two peaks around 100 nm and 300 nm, and better impact strength may be achieved than a single-peak monodisperse type.

[0069] The MB resin and MBS resin may be produced by any polymerization method such as bulk polymerization, solution polymerization, suspension polymerization, or emulsion polymerization, and the copolymerization method may be either a one-stage graft or a multi-stage graft. Further, it may be a mixture with a copolymer of only the graft component by-produced during production. Furthermore, examples of the polymerization method include, in addition to the general emulsion polymerization method, a soap-free polymerization method using an initiator such as potassium persulfate, a seed polymerization method, a two-stage swelling polymerization method, etc. In the suspension polymerization method, a method of separately holding the aqueous phase and the monomer phase and accurately supplying both to a continuous disperser and controlling the particle size by the rotation speed of the disperser, and a method of supplying the monomer phase through a small-diameter orifice or a porous filter with a diameter of several to several tens of μm into an aqueous liquid having dispersibility in a continuous production method to control the particle size may also be performed. In the case of a core-shell type graft polymer, the reaction may be either one-stage or multi-stage for both the core and the shell.

[0070] Such polymers are commercially available and can be easily obtained. However, it is better that the total amount of sodium ions and potassium ions contained in the polymer is small, as advantages such as good thermal stability and hydrolysis resistance can be obtained, and the decrease in flame retardancy is suppressed.

[0071] The content of component B is 1 to 70 parts by weight, preferably 2 to 60 parts by weight, more preferably 3 to 50 parts by weight, based on 100 parts by weight of component A. If the content of component B is less than 1 part by weight, the impact resistance is not improved. If it exceeds 70 parts by weight, the flame retardancy decreases, and the heat resistance decreases, resulting in a decrease in antibacterial sustainability.

[0072] <Component C: Silver-supported zirconium phosphate antibacterial agent> The flame-retardant antibacterial polycarbonate resin composition of the present invention contains a silver-supported zirconium phosphate antibacterial agent as component C. Although the silver support in the antibacterial agent is known to be silica gel, glass (alumina borosilicate glass, etc.), zeolite, apatite, zirconium phosphate, etc., it is necessary that the antibacterial agent be zirconium phosphate, which can suppress resin decomposition during kneading into the resin and maintain impact resistance. That is, in order to achieve the object of the present invention, it is essential that component C is a silver-supported zirconium phosphate antibacterial agent. If the support is not zirconium phosphate, not only will the impact resistance decrease due to decomposition when kneaded into the resin, but the release of silver ions will be promoted, thereby decreasing the antibacterial durability.

[0073] Zirconium phosphate is a crystalline compound that forms a three-dimensional network structure with each constituent ion, and is widely known as an inorganic ion exchanger. The silver-loaded zirconium phosphate antibacterial agent used in the present invention can be obtained by exchanging antibacterial silver ions into the crystalline structure using ion exchange. The silver ions are eluted from the silver-loaded zirconium phosphate antibacterial agent, thereby exhibiting antibacterial properties. Known methods for synthesizing the silver-loaded zirconium phosphate antibacterial agent include a calcination method, a wet method, and a hydrothermal method. For example, lithium in the crystalline lithium zirconium phosphate obtained by hydrothermal synthesis as described in JP-A-2002-53756 is treated with an acid to replace it with a proton, and the proton is further replaced with a silver ion, and then the mixture is dried and calcined at a high temperature to produce the silver-loaded zirconium phosphate antibacterial agent. As the silver-loaded zirconium phosphate antibacterial agent, "Novalon AG series (AG100, AG300 and AG1100)" manufactured by Toagosei Co., Ltd. is commercially available and can be easily obtained.

[0074] The average particle size (D50) of the silver-supported zirconium phosphate antibacterial agent of the present invention, measured by a laser diffraction / scattering method, is preferably 0.5 to 4 μm, more preferably 0.75 to 3.5 μm, and even more preferably 1 to 3 μm. If the average particle size (D50) is less than 0.5 μm, the exposure efficiency of the resin composition on the surface of the molded article decreases, making it difficult to express antibacterial properties, and if it exceeds 5 μm, there may be a significant decrease in impact resistance.

[0075] In the silver-supported zirconium phosphate antibacterial agent of the present invention, the silver content is preferably 2 to 14% by weight, more preferably 5 to 13% by weight, and even more preferably 8 to 12% by weight based on 100% by weight of the silver-supported zirconium phosphate antibacterial agent. If such silver content is less than 2% by weight, the antibacterial property and the antibacterial property persistence become insufficient, and if an attempt is made to compensate for this by increasing the addition amount of the antibacterial agent, the impact resistance decreases, so that the effect of the present invention may not be maximally exerted. If it exceeds 14% by weight, the thermal decomposition of the resin tends to proceed, which has an adverse effect on the thermal stability, and may cause a decrease in impact resistance and flame retardancy, and significant discoloration.

[0076] The content of component C is 0.2 to 7 parts by weight, preferably 0.3 to 5 parts by weight, and more preferably 0.4 to 3 parts by weight with respect to 100 parts by weight of component A. When the content of component C is less than 0.2 parts by weight, the antibacterial property and the antibacterial property persistence are not sufficiently exhibited. When it exceeds 7 parts by weight, not only does the decrease in impact resistance and flame retardancy become remarkable, but it is also obvious that since it contains the precious metal silver, it leads to a significant cost increase of the resin composition.

[0077] <Component D: Silicate mineral> The flame-retardant antibacterial polycarbonate resin composition of the present invention contains a silicate mineral as component D. Such a silicate mineral is a mineral composed of at least a metal oxide component and an SiO2 component, and orthosilicate, disilicate, cyclic silicate, chain silicate, etc. are suitable. The silicate mineral takes a crystalline state, and the shape of the crystal can take various shapes such as fibrous and plate-like.

[0078] Silicate minerals may be any of the following compounds: composite oxides, oxyacid salts (composed of ion lattices), and solid solutions. Furthermore, composite oxides may be any of a combination of two or more single oxides, or a combination of two or more single oxides and oxyacid salts. Furthermore, solid solutions may be any of a solid solution of two or more metal oxides, or a solid solution of two or more oxyacid salts. Silicate minerals may also be hydrates. The form of crystal water in hydrates may be Si-OH, which is hydrogen silicate ion, or hydroxide ion (OH) against metal cations. - ) or enters the gaps in the structure as H2O molecules.

[0079] The silicate mineral may be an artificially synthesized product corresponding to a natural product. As the artificially synthesized product, silicate minerals obtained by various conventionally known methods, such as various synthesis methods using solid-state reactions, hydrothermal reactions, and ultra-high pressure reactions, may be used.

[0080] Specific examples of silicate minerals in each metal oxide component (MO) include the following. The notation in parentheses here is the name of the mineral, etc. that contains such silicate minerals as the main component, and means that the compound in parentheses can be used as the exemplified metal salt.

[0081] Examples of rocks that contain K2O include K2O·SiO2, K2O·4SiO2·H2O, K2O·Al2O3·2SiO2 (kalsilite), K2O·Al2O3·4SiO2 (leucite), and K2O·Al2O3·6SiO2 (orthoclase).

[0082] Minerals containing Na2O as a component include Na2O·SiO2 and its hydrates, Na2O·2SiO2, 2Na2O·SiO2, Na2O·4SiO2, Na2O·3SiO2·3H2O, Na2O·Al2O3·2SiO2, Na2O·Al2O3·4SiO2 (jadeite), 2Na2O·3CaO·5SiO2, 3Na2O·2CaO·5SiO2, and Na2O·Al2O3·6SiO2 (albite).

[0083] Examples of minerals that contain Li2O include Li2O·SiO2, 2Li2O·SiO2, Li2O·SiO2·H2O, 3Li2O·2SiO2, Li2O·Al2O3·4SiO2 (petalite), Li2O·Al2O3·2SiO2 (eucryptite), and Li2O·Al2O3·4SiO2 (spodumene).

[0084] Examples of stones containing BaO include BaO·SiO2, 2BaO·SiO2, BaO·Al2O3·2SiO2 (celsian), and BaO·TiO2·3SiO2 (bentite).

[0085] Examples of materials containing CaO include tobermorite group such as 3CaO·SiO2 (alite, a cement clinker mineral), 2CaO·SiO2 (belite, a cement clinker mineral), 2CaO·MgO·2SiO2 (akermanite), 2CaO·Al2O3·SiO2 (gehlenite), a solid solution of akermanite and gehlenite (melilite), CaO·SiO2 (wollastonite (including both α-type and β-type)), CaO·MgO·2SiO2 (diopside), CaO·MgO·SiO2 (magnesium olivine), 3CaO·MgO·2SiO2 (merwinite), CaO·Al2O3·2SiO2 (anorthite), 5CaO·6SiO2·5H2O (tobermorite, and others such as 5CaO·6SiO2·9H2O). loop hydrates, wollastonite group hydrates such as 2CaO·SiO2·H2O (hillebrandite), xonotlite group hydrates such as 6CaO·6SiO2·H2O (xonotlite), gyrolite group hydrates such as 2CaO·SiO2·2H2O (gyrolite), CaO·Al2O3·2SiO2·H2O (lawsonite), CaO·FeO·2SiO2 (hedengite), 3CaO·2SiO2 (chilcoanite), 3CaO·Al2O3·3SiO2 (grossula), 3CaO·Fe2O3·3SiO2 (andradite), 6CaO·4Al2O3·FeO·SiO2 (pleochroite), as well as clinozoisite, pomegranate, allanite, vesuvianite, onoite, scotite, and augite.

[0086] Portland cement can also be used as a silicate mineral containing CaO as a component. There is no particular limitation on the type of Portland cement, and any type can be used, such as normal, early strength, super early strength, moderate heat, sulfate resistant, white, etc. Furthermore, various types of blended cements, such as blast furnace cement, silica cement, and fly ash cement, can also be used as component D. Other silicate minerals that contain CaO include blast furnace slag and ferrite.

[0087] Examples of compounds that contain ZnO include ZnO·SiO2, 2ZnO·SiO2 (troostite), and 4ZnO·2SiO2·H2O (hemimorphite).

[0088] Examples of rocks that contain MnO include MnO·SiO2, 2MnO·SiO2, CaO·4MnO·5SiO2 (rhodonite) and coesrite.

[0089] Examples of rocks containing FeO include FeO·SiO2 (ferrosilite), 2FeO·SiO2 (ferroolitic olivine), 3FeO·Al2O3·3SiO2 (almandine), and 2CaO·5FeO·8SiO2·H2O (tetractinocene).

[0090] Examples of materials that contain CoO include CoO·SiO2 and 2CoO·SiO2.

[0091] Stones containing MgO include MgO·SiO2 (steatite, enstatite), 2MgO·SiO2 (forsterite), 3MgO·Al2O3·3SiO2 (byrope), 2MgO·2Al2O3·5SiO2 (cordierite), 2MgO·3SiO2·5H2O, 3MgO·4SiO2·H2O (talc), 5MgO·8SiO2·9H2O (attapulgite), 4MgO·6SiO2·7H2O (sepiolite), and These include 3MgO·2SiO2·2H2O (chrysolite), 5MgO·2CaO·8SiO2·H2O (tremelite), 5MgO·Al2O3·3SiO2·4H2O (chlorite), K2O·6MgO·Al2O3·6SiO2·2H2O (phlogovite), Na2O·3MgO·3Al2O3·8SiO2·H2O (ransene), as well as magnesium tourmaline, anthosphite, cumingtonite, vermiculite, and smectite.

[0092] Examples of materials that contain Fe2O3 include Fe2O3·SiO2.

[0093] Examples of refractories that contain ZrO2 include ZrO2·SiO2 (zircon) and AZS refractories.

[0094] Examples of minerals containing Al2O3 include Al2O3·SiO2 (sillimanite, andalusite, kyanite), 2Al2O3·SiO2, Al2O3·3SiO2, 3Al2O3·2SiO2 (mullite), Al2O3·2SiO2·2H2O (kaolinite), Al2O3·4SiO2·H2O (pyrophyllite), Al2O3·4SiO2·H2O (bentonite), K2O·3Na2O·4Al2O3·8SiO2 (nepheline), K2O·3Al2O3·6SiO2·2H2O (muscovite, sericite), K2O·6MgO·Al2O3·6SiO2·2H2O (phlogovite), as well as various zeolites, fluorphlogopite, and biotite.

[0095] Among the above silicate minerals, talc, mica and wollastonite are preferred, and talc is particularly preferred from the viewpoint of maintaining impact resistance.

[0096] (talc) The talc in the present invention is a hydrous magnesium silicate in terms of chemical composition, generally represented by the chemical formula 4SiO2·3MgO·2H2O, and is a scaly particle having a layered structure. It is composed of 56-65% by weight of SiO2, 28-35% by weight of MgO, and about 5% by weight of H2O. Other minor components include 0.03-1.2% by weight of Fe2O3, 0.05-1.5% by weight of Al2O3, 0.05-1.2% by weight of CaO, 0.2% by weight or less of K2O, and 0.2% by weight or less of Na2O. The particle size of the talc is preferably in the range of 0.1-15 μm (more preferably 0.2-12 μm, even more preferably 0.3-10 μm, and particularly preferably 0.5-5 μm) in terms of average particle size measured by a sedimentation method. Furthermore, the bulk density is preferably 0.5 (g / cm 3It is particularly preferable to use talc having a particle size of D50 or more as the raw material. The average particle size of talc refers to D50 (median size of particle size distribution) measured by X-ray transmission method, which is one of the liquid phase precipitation methods. A specific example of an apparatus for performing such measurements is Sedigraph 5100 manufactured by Micromeritics.

[0097] There is no particular restriction on the manufacturing method when talc is pulverized from raw stones, and axial flow mill method, annular mill method, roll mill method, ball mill method, jet mill method, and container rotation type compression shear mill method can be used. Furthermore, the talc after pulverization is preferably classified by various classifiers and has a uniform particle size distribution. There is no particular restriction on the classifier, and examples thereof include impactor type inertial force classifiers (variable impactor, etc.), Coanda effect type inertial force classifiers (elbow jet, etc.), and centrifugal field classifiers (multi-stage cyclone, microplex, dispersion separator, Accucut, turbo classifier, turboplex, micron separator, and super separator, etc.). Furthermore, talc is preferably in an agglomerated state in terms of its handling properties, and examples of such manufacturing methods include a method using deaeration compression and a method using a bundling agent for compression. In particular, the method of degassing and compressing is preferred because it is simple and does not allow unnecessary sizing agent resin components to be mixed into the resin composition of the present invention.

[0098] (Mica) The mica preferably has an average particle size of 10 to 100 μm as measured by a microtrack laser diffraction method. More preferably, the average particle size is 20 to 50 μm. If the average particle size of the mica is less than 10 μm, the effect of improving the rigidity is insufficient, and if it exceeds 100 μm, the improvement in rigidity is insufficient and the mechanical strength such as impact properties is significantly reduced, which is not preferable. The mica preferably has a thickness of 0.01 to 1 μm as measured by observation with an electron microscope. More preferably, the thickness is 0.03 to 0.3 μm. The aspect ratio is preferably 5 to 200, more preferably 10 to 100. The mica used is preferably muscovite mica, and its Mohs hardness is about 3. Muscovite mica can achieve higher rigidity and higher strength than other micas such as phlogovite, and solves the problem of the present invention at a better level. The mica may be produced by either a dry grinding method or a wet grinding method. The dry grinding method is more common and has a lower cost, whereas the wet grinding method is effective for grinding the mica more thinly and finely, which results in a greater effect in improving the rigidity of the resin composition.

[0099] (Wollastonite) The fiber diameter of wollastonite is preferably 0.1 to 10 μm, more preferably 0.1 to 5 μm, and even more preferably 0.1 to 3 μm. The aspect ratio (average fiber length / average fiber diameter) is preferably 3 or more. The upper limit of the aspect ratio is 30 or less. Here, the fiber diameter is measured by observing the reinforcing filler with an electron microscope, determining the individual fiber diameters, and calculating the number average fiber diameter from the measured values. The electron microscope is used because it is difficult to accurately measure the size of the target level with an optical microscope. The fiber diameter is measured by randomly extracting the filler to be measured for the image obtained by observation with the electron microscope, measuring the fiber diameter near the center, and calculating the number average fiber diameter from the measured values. The magnification of the observation is about 1000 times, and the number of measured fibers is 500 or more (600 or less is suitable for work). On the other hand, the average fiber length is measured by observing the filler with an optical microscope, determining the individual lengths, and calculating the number average fiber length from the measured values. Observation with an optical microscope begins with preparing a sample in which the fillers are dispersed so that they do not overlap too much. Observation is performed with a 20x objective lens, and the observed image is captured as image data by a CCD camera with approximately 250,000 pixels. The obtained image data is analyzed by an image analyzer, and the fiber length is calculated using a program that determines the maximum distance between two points on the image data. Under these conditions, the size per pixel corresponds to a length of 1.25 μm, and the number of fibers measured is 500 or more (600 or less is suitable for practical purposes).

[0100] In order to fully reflect the inherent whiteness of the wollastonite of the present invention in the resin composition, it is preferable to remove as much iron as possible from the raw ore and from the equipment wear during the crushing of the raw ore using a magnetic separator. The iron content in the wollastonite after the magnetic separator treatment is preferably 0.5% by weight or less, calculated as Fe2O3.

[0101] The silicate mineral (more preferably mica, talc, wollastonite) is preferably not surface-treated, but may be surface-treated with various surface treatment agents such as silane coupling agents, higher fatty acid esters, and waxes. Further, it may be granulated with a flocculant such as various resins, higher fatty acid esters, and waxes to be in a granular form.

[0102] The content of component D is 8 to 90 parts by weight, preferably 11 to 80 parts by weight, more preferably 14 to 70 parts by weight, based on 100 parts by weight of component A. When the content of component D is less than 8 parts by weight, the effect of improving antibacterial persistence is not observed, and when it exceeds 90 parts by weight, the flame retardancy and impact resistance decrease.

[0103] <Component E: Phosphorus-based flame retardant> The flame-retardant antibacterial polycarbonate resin composition of the present invention contains a phosphorus-based flame retardant as component E. Such phosphorus-based flame retardants include organic phosphorus compounds such as phosphate esters, condensed phosphate esters, phosphazene compounds, and red phosphorus. Among them, phosphate esters and phosphazenes are preferred. Phosphate esters refer to ester compounds of phosphoric acid and alcohol compounds or phenolic compounds. Such phosphate esters and phosphazenes are effective in improving flame retardancy and have a plasticizing effect. Therefore, although there is a decrease in heat resistance, it is advantageous in that the molding processability of the flame-retardant antibacterial polycarbonate resin composition of the present invention can be enhanced.

[0104] Specific examples of phosphoric acid esters include trimethyl phosphate, triethyl phosphate, tributyl phosphate, tri(2-ethylhexyl)phosphate, tributoxyethyl phosphate, triphenyl phosphate, tricresyl phosphate, trixylenyl phosphate, tris(isopropylphenyl)phosphate, tris(phenylphenyl)phosphate, trinaphthyl phosphate, cresyl diphenyl phosphate, xylenyl diphenyl phosphate, diphenyl(2-ethylhexyl)phosphate, di(isopropylphenyl)phenyl phosphate, monoisodecyl phosphate, 2-acryloyloxyethyl acid phosphate, 2- Examples of the condensed phosphate esters include methacryloyloxyethyl acid phosphate, diphenyl-2-acryloyloxyethyl phosphate, diphenyl-2-methacryloyloxyethyl phosphate, melamine phosphate, dimelamine phosphate, melamine pyrophosphate, triphenylphosphine oxide, tricresylphosphine oxide, diphenyl methanephosphonate, diethyl phenylphosphonate, resorcinol polyphenyl phosphate, resorcinol poly(di-2,6-xylyl)phosphate, bisphenol A polycresyl phosphate, hydroquinone poly(2,6-xylyl)phosphate, and condensates thereof. Examples of the condensed phosphate esters include resorcinol bis(di-2,6-xylyl)phosphate, resorcinol bis(diphenyl phosphate), bisphenol A bis(diphenyl phosphate), etc.

[0105] An example of a commercially available product of resorcinol bis(di-2,6-xylyl)phosphate is "PX-200" manufactured by Daihachi Chemical Industry Co., Ltd. An example of a commercially available product of resorcinol bis(diphenyl phosphate) is "CR-733S" manufactured by Daihachi Chemical Industry Co., Ltd. An example of a commercially available product of bisphenol A bis(diphenyl phosphate) is "CR-741" manufactured by Daihachi Chemical Industry Co., Ltd.

[0106] Phosphazene compounds can impart flame retardancy to resin compositions by containing phosphorus atoms and nitrogen atoms in the molecule. The phosphazene compound is not particularly limited as long as it does not contain a halogen atom and has a phosphazene structure in the molecule. The phosphazene structure referred to here represents a structure represented by the formula: -P(R2)=N- [wherein, R2 is an organic group]. The phosphazene compound is represented by general formulas (4) and (5).

[0107] [Chemical formula] [Chemical formula] (In the formula, X1, X2, X3, and X4 represent hydrogen, a hydroxyl group, an amino group, or an organic group not containing a halogen atom. Further, n represents an integer of 3 to 10.)

[0108] In the above general formulas (4) and (5), examples of the organic group not containing a halogen atom represented by X1, X2, X3, and X4 include an alkoxy group, a phenyl group, an amino group, an allyl group, and the like.

[0109] Commercially available phosphazene compounds include "FP-100", "FP-110", "FP-110T", etc. manufactured by Fushimi Pharmaceutical Co., Ltd.

[0110] The content of component E is 8 to 70 parts by weight, preferably 12 to 60 parts by weight, more preferably 16 to 50 parts by weight, based on 100 parts by weight of component A. If the content of component E is less than 8 parts by weight, the flame retardancy is not improved. If it exceeds 70 parts by weight, the plasticizing effect of the resin is too high, so that the silver-supported zirconium phosphate antibacterial agent is likely to settle and be buried inside the molded article of the resin composition, making it difficult to appear on the surface of the molded article and reducing the antibacterial property and antibacterial durability.

[0111] [Component F: Anti-dripping agent] The flame-retardant, antibacterial polycarbonate resin composition of the present invention contains an anti-drip agent as component F. By containing this anti-drip agent, it becomes possible to achieve good flame retardancy without impairing the physical properties of the molded article.

[0112] The drip prevention agent may be a fluorine-containing polymer having fibril-forming ability, and examples of such a polymer include polytetrafluoroethylene, tetrafluoroethylene copolymers (e.g., tetrafluoroethylene / hexafluoropropylene copolymers, etc.), partially fluorinated polymers as shown in U.S. Patent No. 4,379,910, polycarbonate resins produced from fluorinated diphenols, etc. Among these, polytetrafluoroethylene (hereinafter sometimes referred to as PTFE) is preferred.

[0113] The molecular weight of the fibril-forming PTFE is extremely high, and it shows a tendency to bond PTFE to each other and become fibrous by external action such as shear force. The molecular weight is 1 million to 10 million, preferably 2 million to 9 million, in terms of number average molecular weight calculated from the standard specific gravity. Such PTFE can be used in the form of a solid or an aqueous dispersion. In addition, such fibril-forming PTFE can be used in the form of a PTFE mixture mixed with other resins to improve dispersibility in resins and obtain better flame retardancy and mechanical properties.

[0114] A typical example of a commercially available PTFE product having such fibril-forming ability is the "Polyflon MPA FA series (FA-500H, FA-5601, etc.)" manufactured by Daikin Industries, Ltd. A typical example of a commercially available aqueous dispersion of PTFE is the "Polyflon PTFE D series (D-111, D-210C, etc.)" manufactured by Daikin Industries, Ltd.

[0115] The mixed form of PTFE can be prepared by (1) mixing an aqueous dispersion of PTFE with an aqueous dispersion or solution of an organic polymer and co-precipitating to obtain a co-agglomerated mixture (methods described in JP-A-60-258263, JP-A-63-154744, etc.), (2) mixing an aqueous dispersion of PTFE with dried organic polymer particles (method described in JP-A-4-272957), or (3) homogeneously mixing an aqueous dispersion of PTFE with an organic polymer particle solution and extracting each medium from the mixture at the same time. (4) a method of polymerizing a monomer that forms an organic polymer in an aqueous dispersion of PTFE (method described in JP-A-06-220210, JP-A-08-188653, etc.), and (5) a method of homogeneously mixing an aqueous dispersion of PTFE and an organic polymer dispersion, and then polymerizing a vinyl monomer in the mixed dispersion to obtain a mixture (method described in JP-A-11-29679, etc.). Commercially available products of these mixed forms of PTFE include "Metabrene A Series (A-3750 and A-3800)" manufactured by Mitsubishi Chemical Corporation.

[0116] The proportion of PTFE in the mixed form is preferably 1 to 60% by weight, more preferably 5 to 55% by weight, in 100% by weight of the PTFE mixture. When the proportion of PTFE is within this range, good dispersibility of PTFE may be achieved. The proportion of the above F component indicates the net amount of the drip prevention agent, and in the case of the mixed form PTFE, indicates the net amount of PTFE.

[0117] The content of component F is 0.2 to 2 parts by weight, preferably 0.3 to 1.5 parts by weight, and more preferably 0.4 to 1 part by weight, relative to 100 parts by weight of component A. If the content of component F is less than 0.2 parts by weight, sufficient flame retardancy cannot be obtained, and if it exceeds 2 parts by weight, impact resistance decreases.

[0118] In addition, examples of the styrene monomer used in the organic polymer used in the polytetrafluoroethylene blend of the present invention include styrenes that may be substituted with one or more groups selected from the group consisting of alkyl groups having 1 to 6 carbon atoms, alkoxy groups having 1 to 6 carbon atoms, and halogens, such as ortho-methylstyrene, meta-methylstyrene, para-methylstyrene, dimethylstyrene, ethyl-styrene, para-tert-butylstyrene, methoxystyrene, fluorostyrene, monobromostyrene, dibromostyrene, and tribromostyrene, vinylxylene, and vinylnaphthalene, but are not limited thereto. The styrene monomers can be used alone or in combination of two or more types.

[0119] The acrylic monomer used in the organic polymer used in the polytetrafluoroethylene mixture of the present invention includes a (meth)acrylate derivative which may be substituted. Specifically, the acrylic monomer includes a (meth)acrylate derivative which may be substituted with one or more groups selected from the group consisting of an alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 8 carbon atoms, an aryl group, and a glycidyl group, such as (meth)acrylonitrile, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, amyl (meth)acrylate, hexyl (meth)acrylate, 2-ethyl ... Examples of the acrylic monomer include, but are not limited to, (meth)acrylate, cyclohexyl (meth)acrylate, octyl (meth)acrylate, dodecyl (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate and glycidyl (meth)acrylate, maleimides which may be substituted with an alkyl group having 1 to 6 carbon atoms or an aryl group, such as maleimide, N-methyl-maleimide and N-phenyl-maleimide, maleic acid, phthalic acid and itaconic acid. The acrylic monomer may be used alone or in a mixture of two or more kinds. Among these, (meth)acrylonitrile is preferred.

[0120] The amount of the acrylic monomer-derived units contained in the organic polymer used in the coating layer is preferably 8 to 11 parts by weight, more preferably 8 to 10 parts by weight, and even more preferably 8 to 9 parts by weight, based on 100 parts by weight of the styrene monomer-derived units. If the amount of the acrylic monomer-derived units is less than 8 parts by weight, the coating strength may decrease, and if it is more than 11 parts by weight, the surface appearance of the molded article may deteriorate.

[0121] The polytetrafluoroethylene mixture in the present invention preferably has a residual moisture content of 0.5% by weight or less, more preferably 0.2 to 0.4% by weight, and even more preferably 0.1 to 0.3% by weight. If the residual moisture content is more than 0.5% by weight, it may adversely affect the flame retardancy.

[0122] The process for producing a polytetrafluoroethylene-based mixture in the present invention includes a step of forming a coating layer containing one or more monomers selected from the group consisting of styrene-based monomers and acrylic monomers on the outside of branched polytetrafluoroethylene in the presence of an initiator. Furthermore, it is preferable to include a step of drying after the step of forming the coating layer so that the residual moisture content is 0.5% by weight or less, preferably 0.2 to 0.4% by weight, more preferably 0.1 to 0.3% by weight. The drying step can be performed using a method known in the art, such as hot air drying or vacuum drying.

[0123] The initiator used in the polytetrafluoroethylene mixture of the present invention may be any initiator used in the polymerization reaction of styrene-based and / or acrylic monomers without limitation. Examples of the initiator include cumyl hydroperoxide, di-tert-butyl peroxide, benzoyl peroxide, hydrogen peroxide, and potassium peroxide, but are not limited thereto. In the polytetrafluoroethylene mixture of the present invention, one or more of the initiators may be used depending on the reaction conditions. The amount of the initiator is freely selected within the range used in consideration of the amount of polytetrafluoroethylene and the type / amount of monomer, and it is preferable to use 0.15 to 0.25 parts by weight based on the amount of the total composition.

[0124] The polytetrafluoroethylene mixture of the present invention was produced by the suspension polymerization method according to the following procedure. First, water and a branched polytetrafluoroethylene dispersion (solid concentration: 60%, polytetrafluoroethylene particle size: 0.15 to 0.3 μm) were placed in a reactor, and then acrylic monomer, styrene monomer, and cumene hydroperoxide as a water-soluble initiator were added while stirring, and the reaction was carried out at 80 to 90°C for 9 hours. After the reaction was completed, the water was removed by centrifugation for 30 minutes in a centrifuge, and a paste-like product was obtained. The paste product was then dried in a hot air dryer at 80 to 100°C for 8 hours. The dried product was then pulverized to obtain a polytetrafluoroethylene-based mixture of the present invention.

[0125] Such suspension polymerization does not require a polymerization step by emulsion dispersion in the emulsion polymerization method exemplified in Patent No. 3469391, and does not require an emulsifier and electrolyte salts for coagulating and precipitating the latex after polymerization. In addition, in the polytetrafluoroethylene mixture produced by the emulsion polymerization method, the emulsifier and electrolyte salts in the mixture tend to be mixed and are difficult to remove, so it is difficult to reduce the sodium ions and potassium ions derived from such emulsifiers and electrolyte salts. Since the polytetrafluoroethylene mixture used in the present invention is produced by the suspension polymerization method, it does not use such emulsifiers and electrolyte salts, so the content of sodium ions and potassium ions in the mixture can be reduced, and the thermal stability and hydrolysis resistance can be improved.

[0126] In addition, in the present invention, coated branched PTFE can be used as the drip prevention agent. The coated branched PTFE is a polytetrafluoroethylene mixture consisting of branched polytetrafluoroethylene particles and an organic polymer, and has a coating layer consisting of an organic polymer, preferably a polymer containing a unit derived from a styrene monomer and / or a unit derived from an acrylic monomer, on the outside of the branched polytetrafluoroethylene. The coating layer is formed on the surface of the branched polytetrafluoroethylene. In addition, the coating layer preferably contains a copolymer of a styrene monomer and an acrylic monomer.

[0127] The polytetrafluoroethylene contained in the coated branched PTFE is branched polytetrafluoroethylene. When the contained polytetrafluoroethylene is not branched polytetrafluoroethylene, the anti-dripping effect may be insufficient when the addition of polytetrafluoroethylene is small. The branched polytetrafluoroethylene is in particulate form, preferably having a particle size of 0.1 to 0.6 μm, more preferably 0.3 to 0.5 μm, and even more preferably 0.3 to 0.4 μm. When the particle size is smaller than 0.1 μm, the surface appearance of the molded product is excellent, but it is difficult to commercially obtain polytetrafluoroethylene having a particle size smaller than 0.1 μm. Also, when the particle size is larger than 0.6 μm, the surface appearance of the molded product may deteriorate. The number average molecular weight of the polytetrafluoroethylene used in the present invention is 1×10 4 ~1×10 7 is preferred, more preferably 2×10 6 ~9×10 6 and generally, polytetrafluoroethylene with a higher molecular weight is more preferred in terms of stability. Either the powder or dispersion form can be used. The content of the branched polytetrafluoroethylene in the coated branched PTFE is preferably 20 to 60 parts by weight, more preferably 40 to 55 parts by weight, even more preferably 47 to 53 parts by weight, particularly preferably 48 to 52 parts by weight, and most preferably 49 to 51 parts by weight, based on 100 parts by weight of the total weight of the coated branched PTFE. When the proportion of the branched polytetrafluoroethylene is within such a range, good dispersibility of the branched polytetrafluoroethylene may be achieved.

[0128] <G component: adhesion improver> The flame-retardant and antibacterial polycarbonate resin composition of the present invention can contain an adhesion improver as the G component. Such adhesion improvers include acid-modified polyolefin resins and epoxy resins, and by adding them, the adhesion between the polycarbonate-based resin and the inorganic substance can be improved, and an improvement in impact resistance and antibacterial durability may be achieved. In the flame-retardant and antibacterial polycarbonate resin composition of the present invention, the inorganic substances are silver-supported zirconium phosphate antibacterial agents and silicate minerals.

[0129] (Acid-modified polyolefin resin) As the acid-modified polyolefin resin, an olefin wax having a carboxyl group and / or a derivative group thereof is preferably used. Examples of the carboxyl group derivative include a carboxylic anhydride group, a metal salt of a carboxylic acid, an alkyl ester or an aryl ester of a carboxylic acid, etc. The carboxyl group and / or the derivative group may be bonded to any part of the olefin wax, and the concentration is not particularly limited, but is preferably in the range of 0.1 to 6 meq / g per 1 g of the olefin wax. If it is less than 0.1 meq / g, the improvement of rigidity and impact resistance may be insufficient, and if it is more than 6 meq / g, the thermal stability of the olefin wax itself may be deteriorated. In the present invention, the olefin wax may be used alone or as a mixture of two or more kinds.

[0130] (Epoxy resin) The epoxy resin used is preferably an epoxy polymer containing a glycidyl group, more preferably an epoxy polymer containing glycidyl methacrylate in the copolymer, and polystyrene is preferably used as the other component of the copolymer. Among them, polyglycidyl methacrylate-polystyrene copolymer is preferably used. When an epoxy polymer not containing a glycidyl group is used, the compatibility with component A may be poor and the transparency may be poor. Examples of monomer components of polymers containing glycidyl groups include allyl glycidyl ether, glycidyl methacrylate, glycidyl acrylate, 4-hydroxybutyl acrylate glycidyl ether, 1,2-epoxy-5-hexene, 1,2-epoxy-9-decene, and epoxy succinic acid, and examples of polymers include terminal epoxy-modified polydimethylsiloxane and side chain epoxy-modified polydimethylsiloxane.

[0131] The content of component G is preferably 0.01 to 10 parts by weight, more preferably 0.05 to 7 parts by weight, and even more preferably 0.1 to 5 parts by weight, relative to 100 parts by weight of component A. If the content of component G is less than 0.01 part by weight, the antibacterial activity may not be sustained, whereas if it exceeds 10 parts by weight, the flame retardancy and flowability may decrease.

[0132] <Other ingredients> The flame-retardant, antibacterial polycarbonate resin composition of the present invention may further contain phosphorus-based stabilizers, phenol-based stabilizers, release agents, ultraviolet absorbers, dyes and pigments, etc., within limits that do not impair the object of the present invention. The specific details will be explained below.

[0133] (i) Phosphorus-based stabilizers The flame-retardant antibacterial polycarbonate resin composition of the present invention may contain a phosphorus-based stabilizer to the extent that it does not promote hydrolysis. The inclusion of such a phosphorus-based stabilizer is effective in suppressing thermal decomposition during molding and maintaining good impact resistance and flame retardancy.

[0134] Examples of phosphorus-based stabilizers include phosphorous acid, phosphoric acid, phosphonous acid, phosphonic acid and their esters, and tertiary phosphines. Specific examples of the phosphite compound include triphenyl phosphite, tris(nonylphenyl)phosphite, tridecyl phosphite, trioctyl phosphite, trioctadecyl phosphite, didecyl monophenyl phosphite, dioctyl monophenyl phosphite, diisopropyl monophenyl phosphite, monobutyl diphenyl phosphite, monodecyl diphenyl phosphite, monooctyl diphenyl phosphite, 2,2-methylenebis(4,6-di-tert-butylphenyl)octyl phosphite, tris(diethylphenyl)phosphite, tris(di-iso-propylphenyl)phosphite, and tris(di-n-butylphenyl)phosphite. pentaerythritol diphosphite, tris(2,4-di-tert-butylphenyl)phosphite, tris(2,6-di-tert-butylphenyl)phosphite, distearyl pentaerythritol diphosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-ethylphenyl)pentaerythritol diphosphite, phenyl bisphenol A pentaerythritol diphosphite, bis(nonylphenyl)pentaerythritol diphosphite, dicyclohexyl pentaerythritol diphosphite, and the like.

[0135] Other phosphite compounds that react with dihydric phenols to form a cyclic structure can also be used, such as 2,2'-methylenebis(4,6-di-tert-butylphenyl)(2,4-di-tert-butylphenyl)phosphite, 2,2'-methylenebis(4,6-di-tert-butylphenyl)(2-tert-butyl-4-methylphenyl)phosphite, 2,2'-methylenebis(4-methyl-6-tert-butylphenyl)(2-tert-butyl-4-methylphenyl)phosphite, and 2,2'-ethylidenebis(4-methyl-6-tert-butylphenyl)(2-tert-butyl-4-methylphenyl)phosphite.

[0136] Examples of the phosphate compound include tributyl phosphate, trimethyl phosphate, tricresyl phosphate, triphenyl phosphate, trichlorophenyl phosphate, triethyl phosphate, diphenyl cresyl phosphate, diphenyl monoorthoxenyl phosphate, tributoxyethyl phosphate, dibutyl phosphate, dioctyl phosphate, diisopropyl phosphate, etc. Preferred are triphenyl phosphate and trimethyl phosphate.

[0137] The phosphonite compounds include tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenylene diphosphonite, tetrakis(2,4-di-tert-butylphenyl)-4,3'-biphenylene diphosphonite, tetrakis(2,4-di-tert-butylphenyl)-3,3'-biphenylene diphosphonite, tetrakis(2,6-di-tert-butylphenyl)-4,4'-biphenylene diphosphonite, tetrakis(2,6-di-tert-butylphenyl)-4,3'-biphenylene diphosphonite, and tetrakis(2 ,6-di-tert-butylphenyl)-3,3'-biphenylene diphosphonite, bis(2,4-di-tert-butylphenyl)-4-phenyl-phenylphosphonite, bis(2,4-di-tert-butylphenyl)-3-phenyl-phenylphosphonite, bis(2,6-di-n-butylphenyl)-3-phenyl-phenylphosphonite, bis(2,6-di-tert-butylphenyl)-4-phenyl-phenylphosphonite, bis(2,6-di-tert-butylphenyl)-3-phenyl-phenylphosphonite, etc. Among these, tetrakis(di-tert-butylphenyl)-biphenylene diphosphonite and bis(di-tert-butylphenyl)-phenyl-phenylphosphonite are preferred, and tetrakis(2,4-di-tert-butylphenyl)-biphenylene diphosphonite and bis(2,4-di-tert-butylphenyl)-phenyl-phenylphosphonite are more preferred. Such a phosphonite compound can be preferably used in combination with the above-mentioned phosphite compound having an aryl group substituted with two or more alkyl groups.

[0138] Examples of the phosphonate compound include dimethyl benzenephosphonate, diethyl benzenephosphonate, and dipropyl benzenephosphonate.

[0139] Examples of tertiary phosphines include triethylphosphine, tripropylphosphine, tributylphosphine, trioctylphosphine, triamylphosphine, dimethylphenylphosphine, dibutylphenylphosphine, diphenylmethylphosphine, diphenyloctylphosphine, triphenylphosphine, tri-p-tolylphosphine, trinaphthylphosphine, and diphenylbenzylphosphine. A particularly preferred tertiary phosphine is triphenylphosphine. The phosphorus-based stabilizer may be used alone or in combination with two or more kinds. Among the phosphorus-based stabilizers, it is preferable to use a phosphite compound and a phosphonite compound in combination.

[0140] The content of the phosphorus-based stabilizer is preferably 0.01 to 1 part by weight, more preferably 0.02 to 0.9 parts by weight, and even more preferably 0.03 to 0.8 parts by weight, relative to 100 parts by weight of component A. If the content is less than 0.01 part by weight, thermal decomposition during molding processing may not be sufficiently suppressed, and no effect in maintaining impact resistance and flame retardancy may be observed, while if the content exceeds 1 part by weight, thermal decomposition during molding processing may be promoted, and impact resistance and flame retardancy may decrease.

[0141] (ii) Phenolic stabilizers The flame-retardant antibacterial polycarbonate resin composition of the present invention may contain a phenol-based stabilizer. The phenol-based stabilizer generally includes hindered phenol, semi-hindered phenol, and less hindered phenol compounds, but in terms of providing a heat stabilizing formulation to resins including polycarbonate-based resins and styrene-based resins, the hindered phenol compounds are particularly preferably used.

[0142] Examples of such hindered phenol compounds include α-tocopherol, butyl hydroxytoluene, sinapyl alcohol, vitamin E, octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2-tert-butyl-6-(3'-tert-butyl-5'-methyl-2'-hydroxybenzyl)-4-methylphenylacrylate, 2,6-di-tert-butyl-4-(N,N-dimethylaminomethyl)phenol, 3,5-di-tert-butyl-4-hydroxybenzylphosphonate diethyl ester. esters, 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), 4,4'-methylenebis(2,6-di-tert-butylphenol), 2,2'-methylenebis(4-methyl-6-cyclohexylphenol), 2,2'-dimethylenebis(6-α-methyl-benzyl-p-cresol), 2,2'-ethylidenebis(4,6-di-tert-butylphenol), 2,2'-butylidenebis(4-methyl-6-tert-butylphenol), 4,4'-butylidenebis(3-methyl-6-tert-butylphenol), triethylene glycol-N-bis-3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate, 1,6-hexanediol bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], bis[2-tert-butyl-4-methyl 6-(3-tert-butyl-5-methyl-2-hydroxybenzyl)phenyl]terephthalate, 3,9-bis{2-[3-(3-tert-butyl-4-hydroxyphenyl)propionate} 4,4'-thiobis(6-tert-butyl-m-cresol), 4,4'-thiobis(3-methyl-6-tert-butylphenol), 2,2'-thiobis(4-methyl-6-tert-butylphenol), bis(3,5-di-tert-butyl-4-hydroxybenzyl)sulfide, 4,4'-di-thiobis(2,6-di-tert-butylphenol), 4,4'-tri-thiobis(2,6-di-tert-butylphenol), 2,2-thiodiethylene bis-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 2,4-bis(n-octylthio)-6-(4-hydroxy-3,5-di-tert-butylanilino)-1,3,5-triazine, N,N'-hexamethylene bis-(3,5-di-tert-butyl-4-hydroxyhydrocinnamide), N,N'-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, 1,1, 3-Tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, tris(3,5-di-tert-butyl-4-hydroxyphenyl)isocyanurate, tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate, 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanurate, 1,3,5-tris2[3 (3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxy]ethyl isocyanurate, tetrakis[methylene-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]methane, triethylene glycol-N-bis-3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate, triethylene glycol-N-bis-3-(3-tert-butyl-4-hydroxy-5-methylphenyl)acetate, 3,9-bis[2-{3-(3-tert-butyl Examples of the tetrakis[methylene-3-(3-tert-butyl-4-hydroxy-5-methylphenyl)acetyloxy]-2,4,8,10-tetraoxaspiro[5,5]undecane, tetrakis[methylene-3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate]methane, 1,3,5-trimethyl-2,4,6-tris(3-tert-butyl-4-hydroxy-5-methylbenzyl)benzene, and tris(3-tert-butyl-4-hydroxy-5-methylbenzyl)isocyanurate are listed below.

[0143] Among the above compounds, tetrakis[methylene-3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate]methane, octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane are preferably used.

[0144] The above phenol-based stabilizers can be used alone or in combination of two or more kinds. The content of the phenol-based stabilizer is preferably 0.01 to 1 part by weight, more preferably 0.03 to 0.9 parts by weight, and even more preferably 0.05 to 0.8 parts by weight, relative to 100 parts by weight of component A. If the content is less than 0.01 part by weight, the thermal decomposition during molding may not be sufficiently suppressed, and the effect of maintaining impact resistance and flame retardancy may not be observed, whereas if the content exceeds 1 part by weight, the thermal decomposition during molding may be promoted, and the impact resistance and flame retardancy may be reduced.

[0145] (iii) Release agent The flame-retardant antibacterial polycarbonate resin composition of the present invention may contain a mold release agent to improve mold releasability during molding and reduce distortion of molded products within the range in which the effects of the present invention are exhibited.

[0146] As such a mold release agent, a known one can be used. For example, a saturated fatty acid ester, an unsaturated fatty acid ester, a polyolefin wax (polyethylene wax, 1-alkene polymer, etc., modified with a functional group-containing compound such as an acid modification can also be used), a silicone compound (silicone oil, organosiloxane, etc.), a fluorine compound (fluorine oil represented by polyfluoroalkyl ether, etc.), a paraffin wax, a beeswax, etc. can be mentioned. Among them, a fatty acid ester can be mentioned as a preferable mold release agent.

[0147] Such fatty acid esters are esters of aliphatic alcohols and aliphatic carboxylic acids. Such aliphatic alcohols may be monohydric alcohols or polyhydric alcohols having dihydric or higher valences, and the number of carbon atoms is preferably in the range of 3 to 32, more preferably in the range of 5 to 30. Examples of such monohydric alcohols include dodecanol, tetradecanol, hexadecanol, octadecanol, eicosanol, tetracosanol, ceryl alcohol, and triacontanol. Examples of such polyhydric alcohols include pentaerythritol, dipentaerythritol, tripentaerythritol, polyglycerol (triglycerol to hexaglycerol), ditrimethylolpropane, xylitol, sorbitol, and mannitol. In the fatty acid esters of the present invention, polyhydric alcohols are more preferable.

[0148] On the other hand, the aliphatic carboxylic acid preferably has 3 to 32 carbon atoms, and particularly preferably has 10 to 22 carbon atoms. Examples of the aliphatic carboxylic acid include saturated aliphatic carboxylic acids such as decanoic acid, undecanoic acid, dodecanoic acid, tridecanoic acid, tetradecanoic acid, pentadecanoic acid, hexadecanoic acid (palmitic acid), heptadecanoic acid, octadecanoic acid (stearic acid), nonadecanoic acid, behenic acid, icosanoic acid, and docosanoic acid, and unsaturated aliphatic carboxylic acids such as palmitoleic acid, oleic acid, linoleic acid, linolenic acid, eicosenoic acid, eicosapentaenoic acid, and cetoleic acid. Among the above, the aliphatic carboxylic acid is preferably one having 14 to 20 carbon atoms. Among them, saturated aliphatic carboxylic acids are more preferable. In particular, stearic acid and palmitic acid are even more preferable.

[0149] The above-mentioned aliphatic carboxylic acids such as stearic acid and palmitic acid are usually produced from natural oils and fats such as animal oils and fats such as beef tallow and lard, and vegetable oils and fats such as palm oil and sunflower oil, and therefore these aliphatic carboxylic acids are usually mixtures containing other carboxylic acid components with different numbers of carbon atoms. Therefore, in the production of the fatty acid ester of the present invention, aliphatic carboxylic acids produced from such natural oils and fats and in the form of a mixture containing other carboxylic acid components, particularly stearic acid and palmitic acid, are preferably used.

[0150] The fatty acid ester may be either a partial ester or a full ester (full ester). However, since partial esters usually have a high hydroxyl value and tend to induce decomposition of the resin at high temperatures, full esters are more preferred. The acid value of such fatty acid esters is preferably 20 or less, more preferably 4 to 20, and even more preferably 4 to 12, from the viewpoint of thermal stability. The acid value can be substantially 0. In addition, the hydroxyl value of such fatty acid esters is preferably 0.1 to 30, and the iodine value of such fatty acid esters is preferably 10 or less. The iodine value can be substantially 0. These properties can be determined by the method specified in JIS K 0070. The above releasing agents may be used alone or in combination of two or more.

[0151] The content of the release agent is preferably 0.01 to 2 parts by weight, more preferably 0.05 to 1.5 parts by weight, and even more preferably 0.1 to 1 part by weight, relative to 100 parts by weight of component A. Within such ranges, good mold and roll releasability may be imparted without impairing impact resistance and flame retardancy.

[0152] (iv) Ultraviolet absorber The flame-retardant antibacterial polycarbonate resin composition of the present invention can contain an ultraviolet absorbing agent for the purpose of imparting light resistance. Examples of the ultraviolet absorbing agent include benzophenone-based ultraviolet absorbing agents, cyclic iminoester-based ultraviolet absorbing agents, cyanoacrylate-based ultraviolet absorbing agents, benzotriazole-based ultraviolet absorbing agents, and triazine-based ultraviolet absorbing agents. Among these, benzotriazole-based ultraviolet absorbing agents and triazine-based ultraviolet absorbing agents are preferred.

[0153] Benzotriazole-based ultraviolet absorbers include 2-(2-hydroxy-5-methylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-3,5-dicumylphenyl)phenylbenzotriazole, 2-(2-hydroxy-3-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole, 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol], 2-(2-hydroxy-3,5-di-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-3,5-di-tert-butylphenyl)benzotriazole, Examples of such benzotriazoles include 2-(2-hydroxy-3,5-di-tert-amylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-4-octoxyphenyl)benzotriazole, 2,2'-methylenebis(4-cumyl-6-benzotriazolephenyl), 2,2'-p-phenylenebis(1,3-benzoxazin-4-one), and 2-[2-hydroxy-3-(3,4,5,6-tetrahydrophthalimidomethyl)-5-methylphenyl]benzotriazole. Other examples include polymers having a 2-hydroxyphenyl-2H-benzotriazole skeleton, such as a copolymer of 2-(2'-hydroxy-5-methacryloxyethylphenyl)-2H-benzotriazole and a vinyl monomer copolymerizable with said monomer, and a copolymer of 2-(2'-hydroxy-5-acryloxyethylphenyl)-2H-benzotriazole and a vinyl monomer copolymerizable with said monomer.

[0154] As the triazine-based ultraviolet absorber, hydroxyphenyl triazine-based compounds such as 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-hexyloxyphenol, 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-methyloxyphenol, 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-ethyloxyphenol, 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-propyloxyphenol, and 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-butyloxyphenol are preferred examples.Furthermore, compounds in which the phenyl group of the hydroxyphenyl triazine-based compounds listed above is a 2,4-dimethylphenyl group are also exemplified, such as 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl)-5-hexyloxyphenol. The above ultraviolet absorbents may be used alone or in combination of two or more kinds.

[0155] The content of the ultraviolet absorber is preferably 1.5 parts by weight or less, more preferably 1 part by weight or less, and even more preferably 0.5 parts by weight or less, based on 100 parts by weight of component A. If the content exceeds 1.5 parts by weight, not only will the mechanical properties of the resin composition be significantly reduced, but coloring may occur due to light absorption by the ultraviolet absorber.

[0156] (v) Dyes and pigments The flame-retardant antibacterial polycarbonate resin composition of the present invention can provide molded products containing various dyes and pigments and exhibiting a variety of designs. By blending a fluorescent whitening agent or other fluorescent dye that emits light, it is possible to impart even better design effects by taking advantage of the emitted color. It is also possible to provide a resin composition that is colored with a very small amount of dyes and pigments and has vivid color development.

[0157] Examples of the fluorescent dyes (including fluorescent whitening agents) in the present invention include coumarin-based fluorescent dyes, benzopyran-based fluorescent dyes, perylene-based fluorescent dyes, anthraquinone-based fluorescent dyes, thioindigo-based fluorescent dyes, xanthene-based fluorescent dyes, xanthone-based fluorescent dyes, thioxanthene-based fluorescent dyes, thioxanthone-based fluorescent dyes, thiazine-based fluorescent dyes, and diaminostilbene-based fluorescent dyes. Among these, coumarin-based fluorescent dyes, benzopyran-based fluorescent dyes, and perylene-based fluorescent dyes are preferred because they have good heat resistance and are less likely to deteriorate during molding of polycarbonate resins.

[0158] Examples of dyes other than the fluorescent dyes include perylene dyes, coumarin dyes, thioindigo dyes, anthraquinone dyes, thioxanthone dyes, ferrocyanides such as Prussian blue, perinone dyes, quinoline dyes, quinacridone dyes, dioxazine dyes, isoindolinone dyes, and phthalocyanine dyes. Furthermore, the resin composition of the present invention can be blended with a metallic pigment to obtain a good metallic color. As the metallic pigment, those having a metal coating or a metal oxide coating on various plate-like fillers are suitable. The content of the dye or pigment is preferably from 0.00001 to 2 parts by weight, and more preferably from 0.00005 to 1 part by weight, per 100 parts by weight of the A component.

[0159] (vi) Other resins and elastomers The flame-retardant, antibacterial polycarbonate resin composition of the present invention may contain small amounts of other resins or elastomers as long as the effects of the present invention are exhibited.

[0160] Examples of such other resins include polyester resins such as polyethylene terephthalate and polybutylene terephthalate, polyamide resins, polyimide resins, polyetherimide resins, polyurethane resins, silicone resins, polyphenylene ether resins, polyphenylene sulfide resins, polysulfone resins, polymethacrylate resins, and phenol resins.

[0161] Examples of such elastomers include isobutylene / isoprene rubber, ethylene / propylene rubber, acrylic elastomers, polyester elastomers, and polyamide elastomers.

[0162] (vii) Other additives In addition, the flame-retardant antibacterial polycarbonate resin composition may contain small amounts of known additives in order to impart various functions to the molded product or to improve the properties of the molded product. These additives may be added in normal amounts as long as they do not impair the object of the present invention.

[0163] Such additives include sliding agents (e.g., PTFE particles), colorants (e.g., pigments and dyes other than the above-mentioned dyes and pigments, such as carbon black), light diffusing agents (e.g., acrylic crosslinked particles, silicone crosslinked particles, ultrathin glass flakes, etc.), inorganic phosphors (e.g., phosphors having an aluminate as a host crystal), antistatic agents, crystal nucleating agents, radical generators, infrared absorbing agents (heat ray absorbing agents), and photochromic agents.

[0164] <Production of flame-retardant antibacterial polycarbonate resin composition> Any method may be adopted to produce the flame-retardant antibacterial polycarbonate resin composition of the present invention. For example, the A to F components, and optionally the G component and other additives are thoroughly mixed using a premixing means such as a V-type blender, a Henschel mixer, a mechanochemical device, or an extrusion mixer, and then the premix is ​​granulated as necessary using an extrusion granulator or a briquetting machine, and then melt-kneaded using a melt kneader such as a vented twin-screw extruder, and then pelletized using a device such as a pelletizer.

[0165] <Production of Molded Articles Made from Flame-Retardant and Antibacterial Polycarbonate Resin Composition> The flame-retardant antibacterial polycarbonate resin composition of the present invention can be injection molded from pellets obtained by the above-mentioned method to produce various molded products. In such injection molding, not only can the molding method of the usual cold runner system be used, but also a hot runner that enables runnerless production can be used. In addition, in the injection molding, not only can the usual molding method be used, but also gas-assisted injection molding, injection compression molding, ultra-high speed injection molding, injection press molding, two-color molding, sandwich molding, in-mold coating molding, insert molding, foam molding (including those using supercritical fluids), rapid heating and cooling mold molding, heat-insulating mold molding, and in-mold remelting molding, as well as molding methods consisting of combinations thereof, etc. can be used.

[0166] The resin composition of the present invention can also be used in the form of various profile extrusion molded products, sheets, films, etc. by extrusion molding. For molding sheets and films, inflation methods, calendaring methods, casting methods, etc. can also be used. Furthermore, it is possible to mold it into a heat shrinkable tube by subjecting it to a specific stretching operation. The resin composition of the present invention can also be made into a molded product by rotational molding, blow molding, etc.

[0167] Furthermore, molded articles formed from resin compositions can be subjected to various surface treatments, such as decorative painting, hard coating, water-repellent / oil-repellent coating, hydrophilic coating, ultraviolet absorbing coating, infrared absorbing coating, electromagnetic wave absorbing coating, heat-generating coating, antistatic coating, antistatic coating, conductive coating, and metallizing (plating, chemical vapor deposition (CVD), physical vapor deposition (PVD), thermal spraying, etc.).

[0168] <Antibacterial> The antibacterial activity value of the test piece made of the flame-retardant antibacterial polycarbonate resin composition of the present invention against Staphylococcus aureus and Escherichia coli in accordance with JIS Z 2801 is preferably 2.0 or more, more preferably 3.0 or more, and even more preferably 4.0 or more. If the antibacterial activity value is less than 2.0, the antibacterial effect is insufficient. Note that such a test piece is not subjected to conditioning or pretreatment (hereinafter, it may be referred to as "no pretreatment" or "no pretreatment test piece").

[0169] <Sustained antibacterial properties> Test pieces made of the flame-retardant antibacterial polycarbonate resin composition of the present invention were subjected to a "water-resistant treatment" (immersion treatment in 50°C water for 16 hours) and a "light-resistant treatment" (irradiation intensity of 60 W / m2 in the wavelength range of 300 to 400 nm using a xenon arc lamp tester) were subjected to a "light-resistant treatment". 2 For each of the light-resistant test pieces subjected to a light-fastening treatment under conditions of 63°C black panel temperature, 50% relative humidity and no water spray for 100 hours, the antibacterial activity values ​​against Staphylococcus aureus and Escherichia coli in accordance with JIS Z 2801 are preferably 2.0 or more, more preferably 3.0 or more, and even more preferably 4.0 or more. If the antibacterial activity value is less than 2.0, the antibacterial effect is insufficient, and sustained stable expression of antibacterial properties in actual use for various purposes cannot be achieved, and the antibacterial properties may be impaired in environments where water is present, high humidity environments, or environments exposed to ultraviolet rays such as sunlight.

[0170] <Flame retardancy> In the flame-retardant antibacterial polycarbonate resin composition of the present invention, the flame rating of a test piece (thickness 1.2 mm) made of the resin composition is preferably V-0 in a vertical flame test in accordance with UL 94. If the flame rating is below V-0, it is difficult to apply the composition to applications requiring high flame retardancy.

[0171] <Impact resistance> The unnotched Charpy impact strength of a test piece made of the flame-retardant antibacterial polycarbonate resin composition of the present invention and conditioned at 23°C in accordance with ISO179 is 30 kJ / m 2 More than 40 kJ / m is preferable. 2More preferably, 50 kJ / m or more. 2 If the strength is less than the preferred range, it is difficult to apply the material to various applications, and it is particularly difficult to apply the material to housings and the like that require strength. The upper limit of the measured value of the unnotched Charpy impact strength is not particularly limited except for the upper detection limit of the measuring device, but is preferably 100 kJ / m 2 The following performs adequately: EXAMPLES

[0172] The present invention will be described in more detail below with reference to examples, but these are not intended to limit the present invention. Unless otherwise specified, parts in the examples are parts by weight and % is % by weight. Evaluations were performed according to the following methods.

[0173] (Evaluation of flame-retardant and antibacterial polycarbonate resin compositions) (1) Antibacterial properties (no pretreatment, antibacterial activity value) Test pieces (width 50 mm, length 50 mm, thickness 2 mm) were cut from square plate molded products (width 150 mm, length 150 mm, thickness 2 mm) prepared by the method described below, and tests were conducted under the following conditions in accordance with JIS Z 2801. *Bacteria concentration: 1 / 500 normal bouillon medium (1 / 500NB) * Amount of bacterial solution dropped: 0.4 mL (covering film: surface area 16 cm 2 polyethylene film) *Culture temperature and humidity: 35℃, 90%RH *Culture time: 24 hours *Bacteria used: Staphylococcus aureus (NBRC12732), Escherichia coli (NBRC3972) *Cleaning method: Wipe with absorbent cotton soaked in ethanol The antibacterial properties were evaluated based on the antibacterial activity value according to the following criteria. Antibacterial activity value = log 10 (Number of live bacteria on untreated test pieces after 24 hours)-log 10 (Viable bacteria count on antibacterial test piece after 24 hours) ◎: Antibacterial activity value is 3.5 or higher against both of the above two types of bacteria. ○: Antibacterial activity value is 2.0 or more against both of the above two types of bacteria. ×: Antibacterial activity value is less than 2.0 against at least one of the two types of bacteria used above. The antibacterial treated test piece refers to a test piece made of a resin composition containing an antibacterial agent (the resin composition in the following Examples and Comparative Examples), while the untreated test piece refers to a test piece made of a resin composition from which only the antibacterial agent has been removed.

[0174] (2) Antibacterial durability (water resistance / light resistance, antibacterial activity value) A square plate molded product (width 150 mm, length 150 mm, thickness 2 mm) produced by the method described below was cut to obtain a test piece (width 50 mm, length 50 mm, thickness 2 mm). The test piece was subjected to a water resistance treatment or light resistance treatment under the following conditions. *Water resistance treatment: The sample was immersed in ion-exchanged water kept at 50°C in a batch for 16 hours. *Light resistance treatment: Xenon arc lamp tester, irradiation intensity 60W / m in the wavelength range of 300-400nm 2 The treatment was carried out for 100 hours at a black panel temperature of 63°C, a relative humidity of 50%, and without water spray. The irradiated surface of the test piece was used as the test surface (bacteria inoculated surface) in the JIS Z 2801 compliant test. Using the obtained water-resistant test pieces and light-resistant test pieces, tests in accordance with JIS Z 2801 were carried out in the same manner as in (1) Antibacterial property above, and evaluated according to the same criteria.

[0175] (3) Flame retardancy In accordance with the UL 94 vertical flame test established by the US UL LLC (Underwriters Laboratories Limited Liability Company), a flame test was conducted using a 1.2 mm thick molded product (width 12.5 mm, length 125 mm, thickness 1.5 mm) prepared as described below as a test piece. Flame retardancy was evaluated by determining the flammability rating from the test results and classifying into V-0, V-1, V-2 and not V.

[0176] (4) Impact resistance (unnotched Charpy impact strength) The unnotched Charpy impact strength of test pieces (width 10 mm, length 80 mm, thickness 4.0 mm) prepared by the method described below was measured in accordance with ISO179.

[0177] [Examples 1 to 19, Comparative Examples 1 to 11] In the composition shown in Tables 1 and 2, the A to G components, excluding F-1 of the F component, and the other components were uniformly mixed using a V-type blender to obtain a mixture. Using a vented twin-screw extruder with a screw diameter of 30 mm (manufactured by Japan Steel Works, Ltd.; TEX30α-38.5BW-3V), the mixture was fed from the first feed port using a measuring device to a predetermined ratio, and melt-kneaded at a cylinder temperature and die temperature of 240 to 260 ° C, a screw rotation speed of 200 rpm, a discharge rate of 25 kg / h, and a vent vacuum of 3 kPa. The strand discharged from the die was cooled in a water bath, and then strand cut with a pelletizer to obtain pellets. When F-1 of the F component was added, it was heated to 80 ° C and fed to the extruder from the third feed port located between the first and second feed ports using a liquid injection device to a predetermined ratio. The first supply port here is the supply port farthest from the die, and the second supply port is the supply port located between the die and the first supply port of the extruder. A part of the obtained pellets was dried in a hot air circulation dryer at 80 to 120°C for 5 hours, and then molded products for various evaluations were produced using an injection molding machine (Sumitomo Heavy Industries, Ltd.; SE130EV-A) at a cylinder temperature of 240 to 260°C and a mold temperature of 60°C.

[0178] The evaluation results are shown in Tables 1 and 2. The symbols used for each component in Tables 1 and 2 are as follows: (Component A) A: Aromatic polycarbonate resin [Teijin Limited; Panlite L-1225WP (product name), a linear aromatic polycarbonate resin powder with a viscosity average molecular weight of 22,400 and a repeating skeleton of 2,2-bis(4-hydroxyphenyl)propane]

[0179] (B component) B-1: MBS resin [Kaneka Corporation; Kane Ace M-724 (product name), a graft copolymer with a core-shell structure in which the core is mainly composed of butadiene rubber and the shell is mainly composed of methyl methacrylate and styrene] B-2: MB resin [Kaneka Corporation; Kane Ace M-711 (product name), a graft copolymer with a core-shell structure in which the core is mainly made of butadiene rubber and the shell is mainly made of methyl methacrylate] B-3: ABS resin [Toray Industries, Inc.; Toyolac 700-314 (product name), acrylonitrile-butadiene-styrene copolymer produced by emulsion polymerization method] B-4: ABS resin [TRINSEO HOLDINGS ASIA PTE.LTD. manufactured by MAGNUM A371 (product name), acrylonitrile-butadiene-styrene copolymer manufactured by bulk polymerization method]

[0180] (C component) C-1: Silver-loaded zirconium phosphate antibacterial agent [manufactured by Toagosei Co., Ltd.; Nobaron AG1100 (product name), average particle size (D50) measured by laser diffraction / scattering method is 1.1 μm, silver content is 10%] C-2 (for comparison): Silver-loaded glass antibacterial agent [manufactured by Sinanen Zeomic Co., Ltd.; Zeomic KM10D (product name), average particle size (D50) measured by laser diffraction / scattering method is 10 μm]

[0181] (D component) D-1: Talc [Victorite TK-RC (product name), manufactured by Shokozan Mining Co., Ltd.] D-2: Mica [Muscovite MC-40 (product name) manufactured by Hayashi Kasei Co., Ltd.]

[0182] (E component) E-1: Phosphorus-based flame retardant [manufactured by Daihachi Chemical Industry Co., Ltd.; CR-741 (product name), a phosphoric acid ester whose main component is bisphenol A bis(diphenyl phosphate)] E-2: Phosphorus-based flame retardant [manufactured by Daihachi Chemical Industry Co., Ltd.; PX-200 (product name), a phosphoric acid ester whose main component is resorcinol bis(di-2,6-xylyl phosphate)]

[0183] (F component) F-1: Anti-drip agent [manufactured by Daikin Industries, Ltd.; Polyflon MPA FA-500H (product name), polytetrafluoroethylene] F-2: Anti-drip agent [manufactured by Mitsubishi Chemical Corporation; Metablen A-3750 (product name), polytetrafluoroethylene coated with methyl methacrylate and butyl acrylate copolymer (polytetrafluoroethylene content 50% by weight)]

[0184] (G component) G-1: Acid-modified polyolefin resin [Mitsubishi Chemical Corporation; Diacalna 30M (product name), an olefin wax obtained by copolymerization of α-olefin and maleic anhydride] G-2: Epoxy resin (NOF Corporation: Marproof G-0250SP (product name), epoxy group-containing acrylic polymer)

[0185] (Other Ingredients) STB-1: Phosphorus stabilizer [ADEKA Corporation; Adeka STAB 2112 (product name), tris(2,4-di-tert-butylphenyl)phosphite] STB-2: Phenol-based stabilizer [ADEKA Corporation; Adeka STAB AO-50 (product name), octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] STB-3: [JC-224 (trade name), manufactured by Johoku Chemical Industry Co., Ltd., triethyl phosphonoacetate] WAX: Fatty acid ester release agent [NOF Corp.; Unistar H-476-S (product name), pentaerythritol tetrastearate]

[0186] [Table 1]

[0187] [Table 2]

[0188] From Tables 1 and 2, it can be seen that by incorporating predetermined amounts of a rubber-containing graft polymer, a silver-supported zirconium phosphate antibacterial agent, a silicate mineral, a phosphorus-based flame retardant, and an anti-drip agent into a polycarbonate resin, it is possible to obtain a polycarbonate resin composition that maintains high flame retardancy and impact resistance while having excellent antibacterial properties and antibacterial durability that leads to stable expression of antibacterial properties in actual usage environments (antibacterial properties of a resin composition molded product after exposure to water and light).

Claims

1. A flame-retardant, antibacterial polycarbonate resin composition comprising 100 parts by weight of (A) a polycarbonate resin (component A), 1 to 70 parts by weight of (B) a rubber-containing graft polymer (component B), 0.2 to 7 parts by weight of (C) a silver-supported zirconium phosphate antibacterial agent (component C), 8 to 90 parts by weight of (D) a silicate mineral (component D), 8 to 70 parts by weight of (E) a phosphorus-based flame retardant (component E), and 0.2 to 2 parts by weight of (F) an anti-drip agent (component F).

2. 2. The flame-retardant antibacterial polycarbonate resin composition according to claim 1, further comprising 0.01 to 10 parts by weight of an adhesion improver (G) (Component G) per 100 parts by weight of Component A.

3. 3. The flame-retardant, antibacterial polycarbonate resin composition according to claim 1, wherein component B is at least one resin selected from the group consisting of ABS resins, MBS resins and MB resins.

4. 3. The flame-retardant antibacterial polycarbonate resin composition according to claim 1, wherein component C is a silver-supported zirconium phosphate antibacterial agent having an average particle size (D50) of 1 to 3 μm as measured by a laser diffraction / scattering method.

5. 3. The flame-retardant antibacterial polycarbonate resin composition according to claim 1, wherein component C is a silver-loaded zirconium phosphate antibacterial agent having a silver content of 8 to 12% by weight.

6. A molded article obtained by molding the flame-retardant, antibacterial polycarbonate resin composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Antistatic polycarbonate resin composition

    JP1999323117A

  • Flame-retardant polycarbonate resin composition having excellent antistaticity

    JP2007320980A

  • Polycarbonate-based resin composition, product, resin for forming housing, method for using polycarbonate-based resin composition as resin for forming housing, and method for producing polycarbonate-based resin composition

    JP2017110118A

  • Antibacterial polycarbonate resin composition

    JP2017132913A

  • Antibacterial polycarbonate resin composition and molded article of the same

    JP2024113722A

Cited By

  • Flame-retardant polycarbonate resin composition, and molded article obtained by molding same

    WO2026163719A1