Composite oxide particles
Composite oxide particles with cordierite and indialite phases, produced via controlled heating and mixing, address the issues of agglomeration and thermal expansion, ensuring spherical shape and low thermal expansion for effective use in semiconductor substrates.
Patent Information
- Application Number
- JP2023056929
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing composite oxides with a cordierite component have a low softening point, leading to particle agglomeration and loss of spherical structure, making them unsuitable for use as inorganic fillers, and they do not meet the requirements for low thermal expansion and high crystallinity.
Development of composite oxide particles with a polycrystalline structure containing cordierite and indialite phases, having a thermal expansion coefficient of 1.5 ppm or less, spherical shape, and high crystallinity, achieved through specific heating and mixing processes.
The composite oxide particles maintain a spherical, whitish appearance and low thermal expansion, preventing substrate warping and facilitating defect detection in semiconductor packages.
Smart Images

Figure 2024144807000001
Abstract
Description
[Technical field]
[0001] The present invention relates to composite oxide particles. [Background technology]
[0002] In recent years, various next-generation semiconductor packaging materials have been studied. For example, Patent Document 1 describes a crystallized glass containing at least one of the crystals of cordierite and its polymorph, indialite. It is described that the crystallized glass described in Patent Document 1 is useful as a member of a high-frequency electronic device of a high-frequency substrate, for example.
[0003] The softening point of the composite oxide containing the cordierite component is relatively low at around 900°C. Therefore, when the indialite phase, which is a crystalline polymorph of cordierite, begins to form, the particles stick together and become lumpy, and the particulate (spherical) structure cannot be maintained. Therefore, the crystallized glass described in Patent Document 1 cannot be used in a powdery and spherical form like an inorganic filler. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2022 / 059724 DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0005] An object of the present invention is to provide composite oxide particles which are spherical, highly crystalline, whitish, and have a low coefficient of thermal expansion. [Means for solving the problem]
[0006] As a result of intensive research into solving the above problems, the present inventors have found a solution comprising the following configuration, and have completed the present invention. (1) Composite oxide particles which are polycrystalline and have a main crystal phase containing at least one of cordierite and indialite, and have a thermal expansion coefficient of 1.5 ppm or less as measured by the TMA method. (2) The composite oxide particles according to (1) above, having a particle diameter of 0.1 μm or more and 500.0 μm or less. (3) The composite oxide particles according to (1) or (2) above, which have a crystallinity of 40 or more when measured by an X-ray diffraction method and calculated by the following formula (I) within a diffraction angle 2θ range of 15 to 40°: Crystallinity = crystalline peak area / (crystalline peak area + amorphous peak area) (I) (4) The composite oxide particles according to any one of (1) to (3) above, in which, in a particle size distribution measured by a laser diffraction method, the difference D90-D10 between a particle size D90 that is the 90% cumulative diameter and a particle size D10 that is the 10% cumulative diameter is 1000.0 μm or less. (5) The composite oxide particles according to any one of (1) to (4) above, which have a circularity of 0.70 or more. (6) The composite oxide particles according to any one of (1) to (5) above, in which the half-width of the main crystal peak in the diffraction angle 2θ range of 27.5 to 29.5° measured by X-ray diffraction method is 0.20° or less. (7) The composite oxide particles according to any one of (1) to (6) above, wherein the nanoparticles are contained in an amount of 0.1% by mass or more and 30% by mass or less. (8) The composite oxide particles according to any one of (1) to (7) above, in which, in the L*a*b* color space, L* is 91.00 or more and 100.00 or less, a* is -10.00 or more and 3.00 or less, and b* is -10.00 or more and 5.00 or less. (9) A method for producing composite oxide particles, comprising the steps of: mixing cordierite particles and nanoparticles to obtain mixed particles; and heating the mixed particles. (10) The method according to (9) above, wherein the heating step is carried out at 1000°C or higher and 1400°C or lower. Effect of the Invention
[0007] The composite oxide particles according to the present invention are spherical, highly crystalline, whitish, and have a low thermal expansion coefficient. Therefore, the composite oxide particles according to the present invention can be dispersed in a substrate to efficiently prevent thermal warping of, for example, a semiconductor package substrate. Furthermore, since the composite oxide particles according to the present invention are whitish, they do not become colored even when used in a semiconductor package substrate. As a result, defects and stains occurring on the semiconductor package substrate can be easily optically identified. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The composite oxide particles according to the present invention are polycrystalline and contain at least one of cordierite and indialite as a main crystal phase, i.e., contain a plurality of fine single crystals (crystal grains) of at least one of cordierite and indialite.
[0009] Cordierite and indialite are compounds having a composition of 2MgO·2Al2O3·5SiO2 and have different crystal structures. Whether the main crystal phase mainly contains cordierite or indialite is presumed to depend on, for example, the heating temperature (sintering temperature) when producing the composite oxide particles according to the present invention. Specifically, when heated at about 1000°C or more and 1200°C or less, composite oxide particles having the indialite phase as the main crystal phase tend to be obtained. On the other hand, when heated at about 1200°C or more and 1400°C or less, composite oxide particles having the cordierite phase as the main crystal phase tend to be obtained.
[0010] The composite oxide particles according to the present invention have a thermal expansion coefficient of 1.5 ppm or less as measured by the TMA method. With a thermal expansion coefficient of 1.5 ppm or less, the composite oxide particles according to the present invention can efficiently prevent warping of the substrate due to heat when dispersed in, for example, a semiconductor package substrate. The composite oxide particles according to the present invention preferably have a thermal expansion coefficient of less than 0.0 ppm as measured by the TMA method.
[0011] The TMA method (Thermomechanical Analysis) is a method for measuring the amount of thermal expansion of a test sample from the difference in the amount of thermal expansion when a standard sample and a test sample are heated at a constant rate. Quartz glass, alumina, etc. are used as the standard sample.
[0012] The composite oxide particles according to the present invention may contain other crystalline phases or may contain amorphous phases, as long as at least one of cordierite and indialite constitutes the main crystalline phase. The other crystalline phases and amorphous phases may remain as impurities (e.g., unavoidable impurities) in the grain boundaries of the main crystalline phase, or may be intentionally added within a range that does not impair the effects of the present invention. The other crystalline phases and amorphous phases are not limited, and examples thereof include a protenstenite phase, a forestenite phase, a mullite phase, and a cristobalite phase.
[0013] The composite oxide particles according to the present invention may further contain nanoparticles. The nanoparticles are fine particles having a particle diameter of 1.0 nm to 600.0 nm, preferably 50.0 nm to 500.0 nm. The nanoparticles are used when producing the composite oxide particles according to the present invention and do not adversely affect the effects of the present invention. Therefore, it is acceptable for the nanoparticles to remain in the composite oxide particles according to the present invention. By adding the nanoparticles, for example, the surface properties such as wettability can be adjusted, and it is also possible to adjust the surface properties so that the composite oxide particles can be easily added to resin substrates.
[0014] The nanoparticles are not limited, and examples thereof include nano-sized silica particles, nano-sized titania particles, nano-sized magnesia particles, and nano-sized alumina particles. Nano-sized silica particles are preferred. Nano-sized magnesia and alumina particles, which are components of cordierite, are also preferred. The composite oxide particles according to the present invention contain nanoparticles in a ratio of, for example, 0.1% by mass or more and 30% by mass or less based on the total of the nano-sized silica particles (nanoparticles) and the composite oxide particles.
[0015] The composite oxide particles according to the present invention are not limited in size as long as they are spherical. For example, the composite oxide particles according to the present invention preferably have an average particle diameter (D50) of 0.1 μm or more and 500.0 μm or less in terms of the volume average particle diameter cumulative 50% diameter (D50). When the composite oxide particles according to the present invention have an average particle diameter (D50) of 0.1 μm or more and 500.0 μm or less, the film thickness when kneaded into a resin can be reduced to 1 mm or less. The composite oxide particles according to the present invention more preferably have a particle diameter of 1.0 μm or more and 250.0 μm or less.
[0016] The particle size is measured, for example, as follows. First, the composite oxide particles are dispersed in an aqueous solution of sodium hexametaphosphate. Next, the particle size distribution is measured by a laser diffraction method using a laser diffraction particle size distribution measuring device. An example of the laser diffraction particle size distribution measuring device is the "Microtrac: MT-3300EXII" manufactured by Nikkiso Co., Ltd.
[0017] The composite oxide particles according to the present invention are desired to have a relatively small variation in particle size depending on the application. For example, in the composite oxide particles according to the present invention, the difference D90-D10 between the particle size D90, which is the cumulative 90% diameter, and the particle size D10, which is the cumulative 10% diameter, in the particle size distribution by the laser diffraction method is preferably 1000.0 μm or less. When D90-D10 is 1000.0 μm or less, the composite oxide particles according to the present invention are easily filled into a resin. D90-D10 is more preferably 800.0 μm or less. D10 and D90 are calculated from a cumulative frequency distribution curve based on volume.
[0018] The composite oxide particles according to the present invention are not limited in shape as long as they are spherical. The composite oxide particles according to the present invention are preferably close to perfect spheres depending on the application. For example, the composite oxide particles according to the present invention preferably have a circularity of 0.70 or more. When the composite oxide particles according to the present invention have a circularity of 0.70 or more, the loading amount of the composite oxide particles according to the present invention is easily increased when the composite oxide particles according to the present invention are mixed with a resin to prepare a resin composite. The composite oxide particles according to the present invention more preferably have a circularity of 0.80, and even more preferably have a circularity of 0.85 or more.
[0019] The roundness is measured, for example, by a device based on the principle of dynamic image analysis in accordance with ISO 13322-2. An example of such a device is the "CAMSIZER X2" manufactured by Verder Scientific. Specifically, the roundness is measured as follows. First, a predetermined amount of composite oxide particles is weighed. Next, the composite oxide particles are sequentially placed in the device, and the particles passing in front of the camera are measured while dispersing the aggregated particles with dry air at 50 kPa. The measurement is performed in a dry manner. This measurement is repeated three times, and the roundness is analyzed from the integrated average of the measurement results.
[0020] The particle size is the equivalent circle size. The equivalent circle size means the particle size of a perfect circle that has the same area as the projected particle image. The particle size is based on the volume. The circularity is analyzed in accordance with ISO 9276-6. The circularity is 4πA / P 2 where A is the measured area of the projected particle image, and P is the measured perimeter of the projected particle image.
[0021] Although particles have a three-dimensional shape, the particles passing in front of the camera are measured in a two-dimensional manner. Therefore, in this specification, "roundness" is used, and the closer the roundness is to 1.00, the closer the particle is to being a perfect sphere.
[0022] Whether the oxide has crystallinity or amorphousness can be determined, for example, by X-ray diffraction spectrum. When the oxide has amorphousness, a halo peak is observed in the X-ray diffraction spectrum. The composite oxide particles according to the present invention may contain an amorphous phase as long as the composite oxide particles have crystallinity. In the composite oxide particles according to the present invention, the crystallinity as a measure of crystallinity is not limited. The composite oxide particles according to the present invention preferably have a crystallinity of 40 or more. When the composite oxide particles have a crystallinity of 40 or more, the composite oxide particles according to the present invention have the advantage of being less affected by the amorphous portion. The composite oxide particles according to the present invention more preferably have a crystallinity of 80 or more, and even more preferably have a crystallinity of 90 or more.
[0023] The degree of crystallinity is measured by X-ray diffraction of the composite oxide particles according to the present invention, and calculated by the following formula (I) within the range of a diffraction angle 2θ of 15 to 40°. Crystallinity = crystalline peak area / (crystalline peak area + amorphous peak area) (I)
[0024] In the composite oxide particles according to the present invention, the half-width of the main crystal peak in the diffraction angle 2θ range of 27.5 to 29.5° measured by X-ray diffraction is preferably 0.20° or less. When this half-width is 0.20° or less, the composite oxide particles according to the present invention can be said to have high crystallinity of the crystal plane of the main peak that characterizes the composite oxide. The composite oxide particles according to the present invention more preferably have a half-width of 0.18° or less.
[0025] The color of the composite oxide particles according to the present invention is whitish. Therefore, the composite oxide particles according to the present invention do not color a substrate such as a semiconductor package substrate when dispersed therein, and defects and contamination of the substrate are easily detected optically. Furthermore, since the color of the composite oxide particles according to the present invention is whitish, it is also preferable to use the composite oxide particles according to the present invention as a filler to be mixed when preparing a composite. Specifically, in the composite oxide particles according to the present invention, preferably, L* in the L*a*b* color space is 91.00 or more and 100.00 or less, more preferably 92.50 or more and 100.00 or less, a* is -10.00 or more and 3.00 or less, more preferably -5.00 or more and less than 1.50, even more preferably -2.00 or more and less than 1.00, and b* is -10.00 or more and 5.00 or less, more preferably -5.00 or more and 3.50 or less, even more preferably -1.50 or more and less than 3.00. When L*, a* and b* are within such ranges, the composite oxide particles according to the present invention can be judged to have a stronger whiteness.
[0026] The method for producing the composite oxide particles according to the present invention is not limited, and includes, for example, a step of mixing cordierite particles and nanoparticles to obtain mixed particles, and a step of heating the mixed particles.
[0027] In the step of mixing cordierite particles and nanoparticles to obtain mixed particles, the raw cordierite particles and nanoparticles are mixed. The cordierite particles may be used as they are, or may be flame-melted and solidified into granules. Specifically, the cordierite particles may be flame-melted at 1200°C or higher and 1500°C or lower, dropped, and solidified into granules by cooling during the drop.
[0028] As described above, examples of the nanoparticles include nanosilica. Details of the nanoparticles are as described above, and detailed description will be omitted. In the mixed particles containing cordierite particles and nanoparticles, the mixing ratio of the cordierite particles and the nanoparticles is not limited. For example, the nanoparticles are preferably contained in a ratio of 0.1 mass% or more and 30 mass% or less. By using the nanoparticles in such a ratio, the spherical shape can be maintained.
[0029] In the step of heating the mixed particles, the obtained mixed particles are heated. The heating temperature is not limited, and is preferably 1000° C. or more and 1400° C. or less. By heating at such a temperature, composite oxide particles which are polycrystalline and contain at least one of cordierite and indialite as a main crystal phase can be produced more efficiently, and amorphous particles are less likely to be obtained.
[0030] In order to efficiently obtain composite oxide particles containing indialite as the main crystal phase, it is preferable to heat the mixture at 1000° C. or more and 1200° C. or less. On the other hand, in order to obtain composite oxide particles containing cordierite as the main crystal phase, it is preferable to heat the mixture at 1200° C. or more and 1400° C. or less.
[0031] Heating may be performed in an air atmosphere or in an inert gas atmosphere. The inert gas is not limited, and examples thereof include nitrogen gas and argon gas. The heating time is not limited, and is, for example, 1 hour or more and 24 hours or less.
[0032] By such a process, the composite oxide particles according to the present invention can be obtained. Immediately after heating, the composite oxide particles may be solidified, for example, in the shape of the container. Even if the composite oxide particles are solidified in this way, they can be easily broken up by hand or a mallet after cooling, and smooth composite oxide particles can be obtained. The composite oxide particles obtained are spherical, crystalline, and whitish, and the main crystal phase contains at least one of cordierite and indialite. By having such a structure, the composite oxide particles according to the present invention have a thermal expansion coefficient measured by the TMA method of 1.5 ppm or less, preferably less than 0.0 ppm. EXAMPLES
[0033] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0034] (Preparation Example) First, irregular cordierite particles (manufactured by Marusu Yuyaku Co., Ltd., product number: SS400) were flame-melted at 1500° C., and the flame-molten material was allowed to fall. The material was cooled during the fall and solidified into granules, preparing raw material particles.
[0035] Example 1 The raw material particles obtained in Preparation Example were placed in a mortar at a ratio of 95% by mass and nanosilica at 5% by mass, and mixed for 10 minutes. SO-E1 manufactured by Admatechs Co., Ltd. was used as the nanosilica.
[0036] Next, the raw material particles were placed in an alumina crucible and fired at 1200°C for 10 hours to obtain spherical composite oxide particles. XRD measurement was performed on the obtained spherical composite oxide particles. It was confirmed that the obtained spectrum did not contain a broad halo peak, and that the obtained spherical composite oxide particles had high crystallinity. Furthermore, it was confirmed from the firing temperature and the XRD spectrum that the obtained spherical composite oxide particles contained at least one of an indialite phase and a cordierite phase.
[0037] Example 2 Spherical composite oxide particles were obtained in the same manner as in Example 1, except that the particles were fired at 1400°C for 10 hours. The obtained spherical composite oxide particles were subjected to XRD measurement, and a spectrum without a broad halo peak was obtained. From this spectrum, it was confirmed that the obtained spherical composite oxide particles had high crystallinity. Furthermore, from the firing temperature and the XRD spectrum, it was confirmed that the obtained spherical composite oxide particles contained at least one of an indialite phase and a cordierite phase.
[0038] Example 3 Spherical composite oxide particles were obtained in the same manner as in Example 2, except that the raw material particles obtained in Preparation Example were used at a ratio of 70 mass% and nanosilica at 30 mass%. The obtained spherical composite oxide particles were subjected to XRD measurement, and a spectrum without a broad halo peak was obtained. From this spectrum, it was confirmed that the obtained spherical composite oxide particles have high crystallinity. Furthermore, from the firing temperature and the XRD spectrum, it was confirmed that the obtained spherical composite oxide particles contain at least one of an indialite phase and a cordierite phase.
[0039] Example 4 Spherical composite oxide particles were obtained in the same manner as in Example 1, except that the raw material particles obtained in Preparation Example were used at a ratio of 99% by mass and nanosilica at 1% by mass. The obtained spherical composite oxide particles were subjected to XRD measurement, and a spectrum without a broad halo peak was obtained. From this spectrum, it was confirmed that the obtained spherical composite oxide particles have high crystallinity. Furthermore, from the firing temperature and the XRD spectrum, it was confirmed that the obtained spherical composite oxide particles contain at least one of an indialite phase and a cordierite phase.
[0040] Comparative Example 1 The raw material particles obtained in the preparation example were placed in an alumina crucible and fired at 850°C for 10 hours to obtain spherical composite oxide particles. The obtained spherical composite oxide particles were subjected to XRD measurement. The obtained spectrum showed a broad halo peak, and it was confirmed that the obtained spherical composite oxide particles contained an amorphous phase and a crystalline phase.
[0041] Comparative Example 2 An attempt was made to obtain spherical composite oxide particles in the same manner as in Comparative Example 1, except that the firing was performed at 1400° C. for 10 hours. However, a lump-like composite oxide was obtained, and spherical particles were not obtained.
[0042] The spherical composite oxide particles obtained in Examples 1 to 4 and Comparative Example 1 were examined for particle size, specific surface area, circularity, thermal expansion coefficient, crystallinity, and color.
[0043] <Particle size> The obtained spherical composite oxide particles were dispersed in an aqueous solution of sodium hexametaphosphate. Then, the particle size distribution was measured by a laser diffraction method using a laser diffraction particle size distribution measuring device (Microtrack: MT-3300EXII, manufactured by Nikkiso Co., Ltd.). D10, D50 and D90 were calculated from the cumulative frequency distribution curve based on volume. The value of D50 and the difference between D90 and D10 (D90-D10) are shown in Table 1.
[0044] <Specific surface area> The specific surface area of the obtained spherical composite oxide particles was measured in accordance with the specific surface area measurement method for powders (solids) by gas adsorption (JIS Z 8830:2013). Specifically, nitrogen was used as the adsorption gas, 1 g of spherical composite oxide particles was placed in a sample tube, and an adsorption / desorption isotherm was obtained. The specific surface area (m 2 / g) was calculated. The results are shown in Table 1.
[0045] <Circularity> The circularity of the obtained spherical composite oxide particles was measured using a device based on the principle of dynamic image analysis in accordance with ISO 13322-2 (CAMSIZER X2 (Verder Scientific)). Specifically, 3 g of spherical composite oxide particles were weighed. Next, the composite oxide particles were sequentially placed into the device, and the particles passing in front of the camera were measured while dispersing the aggregated particles with dry air at 50 kPa. The measurement was performed in a dry state. This measurement was repeated three times, and the circularity was analyzed from the integrated average of the measurement results. The circularity was expressed as 4πA / P 2 A represents the measured area of the projected particle image, and P represents the measured perimeter of the projected particle image. The results are shown in Table 1.
[0046] <Thermal expansion coefficient> The obtained spherical composite oxide particles were each prepared from raw materials (raw material particles and nanosilica as necessary) at the same temperatures as in Examples 1 to 4, Comparative Example 1, and Comparative Example 2 to obtain rectangular sintered bodies (20 mm x 4 mm x 4 mm). The linear expansion coefficients of the obtained sintered bodies (samples) were measured using a TD5020SE (manufactured by NETZSCH). Specifically, the linear expansion coefficients of the obtained samples were measured in the air at temperatures ranging from 30 to 300°C in accordance with thermomechanical analysis (JIS R1618). Sapphire was used as the standard sample. This linear expansion coefficient was taken as the thermal expansion coefficient. The results are shown in Table 1.
[0047] <Crystalline> The crystallinity of the obtained spherical composite oxide particles was measured by X-ray diffraction. Specifically, the diffraction spectrum was obtained by measuring with a powder X-ray diffractometer X'PertPROMPD (manufactured by Spectris Co., Ltd.). The measurement conditions were as follows: X-ray source was CuKα, X-ray output was 45 kV and 40 mA, and scanning speed was 0.2 deg / s. If a clear and sharp peak was shown, it was judged to be crystalline, and if a broad halo peak was shown, it was judged to be amorphous. From the results of the built-in software HighScorePlus, the crystallinity was calculated by the above-mentioned formula (I) (crystallinity = crystalline peak area / (crystalline peak area + amorphous peak area)). The results are shown in Table 1.
[0048] <Color> The color of the obtained spherical composite oxide particles was determined based on the L*a*b* color space. Specifically, the obtained spherical composite oxide particles were placed on a glass plate in a 1.5 cm x 1.5 cm square shape so that there was no gap, and a cover glass was placed on top of it to fix the sample to obtain a sample piece. The obtained sample piece was subjected to black correction and white correction using a spectrophotometer CM-3700A (manufactured by Konica Minolta, Inc.), and then, in accordance with JIS Z8722 condition c, diffuse lighting was received in an 8° direction, and SCI reflection measurement was performed to obtain the lightness L* and chromaticity a* and b*. L*=0.00 indicates black, L*=100.00 indicates white, and 0.00≦L*≦100.00, -100.00≦a*≦100.00, and -100.00≦b*≦100.00. A color was judged to be white if it satisfied the following criteria: L*>91.00, a*<3.00, and b*<5.00. The results are shown in Table 1.
[0049] [Table 1]
[0050] As described above, the composite oxide particles obtained in Examples 1 to 4 (corresponding to the composite oxide particles according to the present invention) contain at least one of a cordierite phase and an indialite phase. As shown in Table 1, the composite oxide particles obtained in Examples 1 to 4 all have a D50 of 0.1 μm or more and 500.0 μm or less, and the difference between D90 and D10, D90-D10, is 1000.0 μm or less. The composite oxide particles obtained in Examples 1 to 4 all have a white color, are spherical, have a circularity of 0.7 or more, and have a thermal expansion coefficient (linear expansion coefficient) of 0.0 ppm or less. Furthermore, the composite oxide particles obtained in Examples 1 to 4 are crystalline, have a crystallinity of 40 or more in the range of a diffraction angle 2θ of 15 to 40°, and have a half-width of the main crystal peak in the range of a diffraction angle 2θ of 27.5 to 29.5° of 0.20° or less.
[0051] On the other hand, the composite oxide particles obtained in Comparative Example 1 are pink, not white, and have a thermal expansion coefficient (linear expansion coefficient) of 4.0 ppm, which exceeds 1.5 ppm, indicating the presence of amorphous parts. As shown in Table 1, the composite oxide particles obtained in Comparative Example 2 were lumpy after firing and could not be broken up with a wooden mallet, so they were crushed into particles with a hammer. The composite oxide particles obtained in Comparative Example 2 are crystalline and white, but have a thermal expansion coefficient (linear expansion coefficient) of 1.7 ppm, which exceeds 1.5 ppm. Comparative Example 3 shown in Table 1 is a result of judging the color of the raw material particles obtained in the preparation example based on the L*a*b* color space.
Claims
1. It is polycrystalline, and its main crystal phase contains at least one of cordierite and indialite, and its thermal expansion coefficient measured by the TMA method is 1.5 ppm or less. Composite oxide particles.
2. The composite oxide particles according to claim 1, having an average particle diameter (D50) of 0.1 μm or more and 500.0 μm or less.
3. 2. The composite oxide particles according to claim 1, which have a crystallinity of 40 or more when measured by an X-ray diffraction method and calculated by the following formula (I) at a diffraction angle 2θ of 15 to 40°: Crystallinity=crystalline peak area / (crystalline peak area+amorphous peak area) (I)
4. 2. The composite oxide particles according to claim 1, wherein in a particle size distribution by a laser diffraction method, the difference D90-D10 between a particle size D90 that is the 90% cumulative diameter and a particle size D10 that is the 10% cumulative diameter is 1000.0 μm or less.
5. 2. The composite oxide particles according to claim 1, having a circularity of 0.70 or more.
6. 2. The composite oxide particles according to claim 1, wherein the half-width of the main crystal peak in the diffraction angle 2θ range of 27.5 to 29.5°, as measured by X-ray diffraction, is 0.20° or less.
7. The composite oxide particles according to claim 1 , wherein the nanoparticles are contained in an amount of 0.1% by mass or more and 30% by mass or less.
8. 2. The composite oxide particles according to claim 1, wherein in the L*a*b* color space, L* is 91.00 or more and 100.00 or less, a* is −10.00 or more and 3.00 or less, and b* is −10.00 or more and 5.00 or less.
9. A step of mixing particulate cordierite and nanoparticles to obtain mixed particles; heating the mixed particles; The method for producing composite oxide particles comprises:
10. The method according to claim 9 , wherein the heating step is carried out at 1000° C. or more and 1400° C. or less.
Citation Information
Patent Citations
Crystallized glass, high frequency substrate, antenna for liquid crystals, and method for producing crystallized glass