Polylactic acid resin foam sheet and polylactic acid resin foam molding
By controlling cell diameters and aspect ratios, the polylactic acid resin foam sheet achieves high compressive strength, addressing the low strength issue in conventional molded articles.
Patent Information
- Application Number
- JP2023056950
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Conventional polylactic acid resin foam molded articles have low compressive strength, leading to cracks during punching operations.
A polylactic acid resin foam sheet with controlled average cell diameters and aspect ratios in the MD, TD, and VD directions, along with specific heat treatment and composition, enhances mechanical strength.
The solution provides polylactic acid resin foam molded articles with high compressive strength, reducing the likelihood of cracks during punching.
Smart Images

Figure 2024144815000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a polylactic acid resin foam sheet and a polylactic acid resin foam molded article. [Background technology]
[0002] Resin foam sheets are lightweight, have excellent cushioning properties, and can be easily molded into a variety of shapes, so they are used as a raw material for various molded products, including packaging materials.
[0003] In recent years, resin foam sheets, which are used in large quantities and then discarded in large quantities, have placed a heavy burden on the environment and become a cause of various social problems such as global warming, resource depletion, waste disposal, etc. In response to this, a polylactic acid resin foam sheet has been proposed that uses polylactic acid resin, which is biodegradable, has a small environmental impact, and can be produced relatively inexpensively (for example, Patent Document 1).
[0004] However, polylactic acid resin foam molded products obtained by molding conventional polylactic acid resin foam sheets have low compressive strength, and have a problem in that, for example, when punched, cracks are likely to occur around the punched portion. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 6971947 Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a polylactic acid resin foam sheet capable of imparting high compressive strength to a polylactic acid resin foam molded article obtained by molding, and to provide a polylactic acid resin foam molded article having high compressive strength obtained by molding such a polylactic acid resin foam sheet. [Means for solving the problem]
[0007] [1] A polylactic acid resin foam sheet according to an embodiment of the present invention is a polylactic acid resin foam sheet obtained by foaming a polylactic acid resin composition containing a polylactic acid resin (P), and after a heat treatment in which the polylactic acid resin foam sheet is heated until the sheet surface temperature reaches 110°C±10°C, the aspect ratios MV=dM / dV and TV=dT / dV calculated from the average cell diameter dM in the MD direction, the average cell diameter dT in the TD direction, and the average cell diameter dV in the VD direction of the polylactic acid resin foam sheet are all 1.0 to 2.0. [2] The polylactic acid resin foam sheet described in [1] above may have an average cell diameter of 150 μm to 850 μm. [3] The polylactic acid resin foamed sheet according to the above item [1] or [2] may have an average cell diameter of 200 μm to 1100 μm after the heat treatment. [4] The polylactic acid resin foam sheet according to any one of [1] to [3] above has an apparent density of 0.063 g / cm 3 ~0.5g / cm 3 may be also possible. [5] The polylactic acid resin foam sheet according to any one of the above items [1] to [4] may have a thickness of 0.5 mm to 7 mm. [6] The polylactic acid resin foam sheet according to any one of [1] to [5] above may have an open cell ratio of 50% or less. [7] In the polylactic acid resin foam sheet according to any one of the above items [1] to [6], the polylactic acid resin (P) may be a modified polylactic acid resin. [8] The polylactic acid resin foam molded article according to the embodiment of the present invention is obtained by molding the polylactic acid resin foam sheet described in any one of [1] to [7] above. Effect of the Invention
[0008] According to an embodiment of the present invention, it is possible to provide a polylactic acid resin foam sheet that can impart high compressive strength to a polylactic acid resin foam molded article obtained by molding, and also to provide a polylactic acid resin foam molded article having high compressive strength obtained by molding such a polylactic acid resin foam sheet. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a schematic diagram showing one preferred configuration of an extruder used in a method for producing a modified polylactic acid resin. [Diagram 2] FIG. 1 is a schematic diagram showing a preferred configuration of a production apparatus suitable for producing a polylactic acid resin foam sheet according to an embodiment of the present invention. [Diagram 3] FIG. 1 is a schematic diagram showing a preferred configuration of a production apparatus suitable for producing a polylactic acid resin foam sheet according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.
[0011] In this specification, "polylactic acid resin (P)" means "modified polylactic acid resin" or "unmodified polylactic acid resin". In this specification, when "polylactic acid resin (P)" is not described, but simply "polylactic acid resin", it means unmodified polylactic acid resin. Here, "unmodified polylactic acid resin" means polylactic acid resin that has not been modified, typically a polylactic acid resin that is generally available, and not a polylactic acid resin that has been modified as described in this specification.
[0012] In this specification, "containing as a main component" means that the content ratio thereof is preferably more than 50% by mass, more preferably 70% by mass or more, even more preferably 90% by mass or more, particularly preferably 95% by mass or more, and most preferably substantially 100% by mass.
[0013] In this specification, the term "substantially 100% by mass" means that the presence of a trace amount (for example, less than 1% by mass) of unintentionally mixed impurities may be ignored.
[0014] ≪≪1. Polylactic acid resin foam sheet≫≫ The polylactic acid resin foam sheet according to an embodiment of the present invention is obtained by melt-kneading a polylactic acid resin (P) containing as a main component the modified polylactic acid resin obtained by the manufacturing method according to an embodiment of the present invention with a foaming agent in an extruder, and extruding and foaming the resulting mixture.
[0015] In the polylactic acid resin foam sheet according to the embodiment of the present invention, the aspect ratio MV=dM / dV and aspect ratio TV=dT / dV calculated from the average cell diameter dM in the MD direction, the average cell diameter dT in the TD direction, and the average cell diameter dV in the VD direction of the polylactic acid resin foam sheet after the heat treatment in which the polylactic acid resin foam sheet is heated until the sheet surface temperature reaches 110°C±10°C are all 1.0 to 2.0, preferably 1.0 to 1.9, more preferably 1.0 to 1.8, particularly preferably 1.0 to 1.75, and most preferably 1.0 to 1.7. In the polylactic acid resin foam sheet according to the embodiment of the present invention, the aspect ratio MV and the aspect ratio TV are both within the above ranges, so that the polylactic acid resin foam molded product obtained by molding can be given high compressive strength. If the aspect ratio MV or the aspect ratio TV is too small outside the above range, the bubbles are likely to buckle, and mechanical properties may be deteriorated. If the aspect ratio MV or the aspect ratio TV is too large outside the above range, not only will the flexibility decrease, but the material will also become too hard, resulting in decreased toughness and the material being likely to become brittle. The methods for measuring the average cell diameter dM in the MD direction, the average cell diameter dT in the TD direction, and the average cell diameter dV in the VD direction will be described later.
[0016] The aspect ratio MV represents the ratio of the average bubble diameter dM in the MD direction (lengthwise direction of the sheet, flow direction) to the average bubble diameter dV in the VD direction (thickness direction of the sheet). The aspect ratio TV represents the ratio of the average bubble diameter dT in the TD direction (widthwise direction of the sheet, direction perpendicular to the flow direction) to the average bubble diameter dV in the VD direction (thickness direction of the sheet).
[0017] The present inventors have repeatedly investigated the cause of the low compressive strength of polylactic acid resin foam molded products obtained by molding conventional polylactic acid resin foam sheets, and have noticed that the average cell diameter dV in the VD direction of polylactic acid resin foam molded products is significantly smaller than the average cell diameter dM in the MD direction and the average cell diameter dT in the TD direction. Then, the inventors have repeatedly investigated the average cell diameter dV in the VD direction of polylactic acid resin foam molded products to be as close as possible to the average cell diameter dM in the MD direction and the average cell diameter dT in the TD direction. As a result, it has been found that the compressive strength of polylactic acid resin foam molded products is improved when the aspect ratios MV and TV are within the above ranges, and have completed the present invention.
[0018] The heat treatment is a treatment in which the polylactic acid resin foam sheet according to the embodiment of the present invention is heated until the sheet surface temperature reaches 110° C.±10° C., and is preferably a treatment in which heating is performed in a heating furnace (typically, upper and lower heaters) with an atmospheric temperature set at 300° C., until the sheet surface temperature reaches 110° C.±10° C. The heating time varies depending on the specifications of the device, the shape of the sheet, etc., but typically, it is preferably 1 second to 60 minutes, more preferably 5 seconds to 10 minutes, even more preferably 10 seconds to 5 minutes, and particularly preferably 15 seconds to 1 minute.
[0019] In the polylactic acid resin foamed sheet according to the embodiment of the present invention, the average bubble diameter of the polylactic acid resin foamed sheet after heat treatment is preferably 200 μm to 1100 μm, more preferably 300 μm to 1000 μm, further preferably 350 μm to 950 μm, and particularly preferably 400 μm to 900 μm, in order to further exhibit the effects of the present invention. When the average bubble diameter of the polylactic acid resin foamed sheet after heat treatment is within the above range, the mechanical strength can be further improved. A method for calculating the average bubble diameter will be described later.
[0020] In the polylactic acid resin foam sheet according to the embodiment of the present invention, the average cell diameter dM in the MD direction of the polylactic acid resin foam sheet after heat treatment is preferably 200 μm to 1200 μm, more preferably 300 μm to 1100 μm, further preferably 350 μm to 1050 μm, and particularly preferably 400 μm to 1000 μm, in order to realize the effects of the present invention. When the average cell diameter dM of the polylactic acid resin foam sheet after heat treatment is within the above range, the mechanical strength can be further improved.
[0021] In the polylactic acid resin foam sheet according to the embodiment of the present invention, the average cell diameter dT in the TD direction of the polylactic acid resin foam sheet after heat treatment is preferably 400 μm to 1300 μm, more preferably 500 μm to 1200 μm, further preferably 550 μm to 1150 μm, and particularly preferably 600 μm to 1100 μm, in order to further exhibit the effects of the present invention. When the average cell diameter dT of the polylactic acid resin foam sheet after heat treatment is within the above range, the mechanical strength can be further improved.
[0022] In the polylactic acid resin foam sheet according to the embodiment of the present invention, the average cell diameter dV in the VD direction of the polylactic acid resin foam sheet after heat treatment is preferably 150 μm to 900 μm, more preferably 200 μm to 850 μm, further preferably 250 μm to 800 μm, and particularly preferably 300 μm to 750 μm, in order to further exhibit the effects of the present invention. When the average cell diameter dV of the polylactic acid resin foam sheet after heat treatment is within the above range, the mechanical strength can be further improved.
[0023] The polylactic acid resin foam sheet according to the embodiment of the present invention has an average cell diameter of preferably 150 μm to 850 μm, more preferably 200 μm to 800 μm, further preferably 250 μm to 750 μm, and particularly preferably 300 μm to 700 μm. When the average cell diameter of the polylactic acid resin foam sheet is within the above range, the mechanical strength can be further improved.
[0024] The polylactic acid resin foam sheet according to the embodiment of the present invention has an average cell diameter dM in the MD direction of preferably 200 μm to 1100 μm, more preferably 250 μm to 1050 μm, further preferably 300 μm to 1000 μm, and particularly preferably 350 μm to 950 μm. When the average cell diameter dM of the polylactic acid resin foam sheet is within the above range, the mechanical strength can be further improved.
[0025] The polylactic acid resin foam sheet according to the embodiment of the present invention has an average cell diameter dT in the TD direction of preferably 350 μm to 1150 μm, more preferably 400 μm to 1100 μm, further preferably 450 μm to 1050 μm, and particularly preferably 500 μm to 1000 μm. When the average cell diameter dT of the polylactic acid resin foam sheet is within the above range, the mechanical strength can be further improved.
[0026] The polylactic acid resin foam sheet according to the embodiment of the present invention has an average cell diameter dV in the VD direction of preferably 125 μm to 650 μm, more preferably 150 μm to 600 μm, even more preferably 175 μm to 550 μm, and particularly preferably 200 μm to 500 μm, in order to further exhibit the effects of the present invention. When the average cell diameter dV of the polylactic acid resin foam sheet is within the above range, the mechanical strength can be further improved.
[0027] The apparent density of the polylactic acid resin foam sheet according to the embodiment of the present invention is preferably 0.063 g / cm 3 ~0.5g / cm 3 and more preferably 0.068 g / cm 3 ~0.41g / cm3 and more preferably 0.072 g / cm 3 ~0.35g / cm 3 and particularly preferably 0.078 g / cm 3 ~0.31g / cm 3 When the apparent density of the polylactic acid resin foam sheet according to the embodiment of the present invention is within the above range, the effects of the present invention can be more effectively exhibited.
[0028] The thickness of the polylactic acid resin foam sheet according to the embodiment of the present invention can be appropriately set depending on the purpose. The thickness of the polylactic acid resin foam sheet obtained by the manufacturing method according to the embodiment of the present invention is typically preferably 0.5 mm to 7 mm, more preferably 0.5 mm to 5 mm, even more preferably 0.7 mm to 5 mm, and particularly preferably 0.7 mm to 3 mm. When the thickness of the polylactic acid resin foam sheet is equal to or greater than the above lower limit, the shape retention can be excellent. When the thickness of the polylactic acid resin foam sheet is equal to or less than the above upper limit, the thermoformability can be further improved.
[0029] The open cell ratio of the polylactic acid resin foamed sheet according to the embodiment of the present invention is preferably 50% or less, more preferably 40% or less, even more preferably 30% or less, and particularly preferably 25% or less. The lower limit of the open cell ratio is preferably as low as possible, and is preferably 0% or more. When the open cell ratio of the polylactic acid resin foamed sheet according to the embodiment of the present invention is within the above range, the effects of the present invention can be more effectively exhibited. The method for measuring the open cell ratio will be described later.
[0030] The polylactic acid resin foam sheet according to the embodiment of the present invention is produced by foaming a polylactic acid resin composition containing a polylactic acid resin (P).
[0031] The polylactic acid resin (P) may be a modified polylactic acid resin, or may be a polylactic acid resin (unmodified polylactic acid resin), or may be a mixture of these.
[0032] Representative examples of polylactic acid resin foam sheets according to the embodiments of the present invention include embodiment A in which the polylactic acid resin (P) contains modified polylactic acid resin as a main component, and embodiment B in which the polylactic acid resin (P) contains polylactic acid resin (unmodified polylactic acid resin) as a main component.
[0033] 1-1. Polylactic acid resin foam sheet in embodiment A In embodiment A, the polylactic acid resin foamed sheet according to the embodiment of the present invention is produced by foaming a polylactic acid resin composition containing a polylactic acid resin (P) containing a modified polylactic acid resin as a main component.
[0034] <1-1-a. Modified polylactic acid resin> The modified polylactic acid resin is preferably obtained by melt-kneading a polylactic acid resin composition containing a polylactic acid resin and a modifier in an extruder.
[0035] The polylactic acid resin may be a homopolymer of lactic acid or a copolymer of lactic acid and other monomers, such as aliphatic hydroxycarboxylic acids other than lactic acid, aliphatic polyhydric alcohols, aliphatic polycarboxylic acids, and polyfunctional polysaccharides.
[0036] The lactic acid constituting the polylactic acid resin may be either the L-form or the D-form, or may be both the L-form and the D-form. That is, the polylactic acid resin, which is a homopolymer of lactic acid, may be any of poly(L-lactic acid) resin, poly(D-lactic acid) resin, and poly(DL-lactic acid) resin.
[0037] Examples of hydroxycarboxylic acids other than lactic acid include glycolic acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 4-hydroxyvaleric acid, 5-hydroxyvaleric acid, and 6-hydroxycaproic acid.
[0038] Examples of the aliphatic polyhydric alcohol include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, 1,3-butanediol, 1,4-butanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,9-nonanediol, neopentyl glycol, tetramethylene glycol, and 1,4-cyclohexanedimethanol.
[0039] Examples of the aliphatic polycarboxylic acid include oxalic acid, succinic acid, malonic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, undecanedioic acid, and dodecanedioic acid. The aliphatic polycarboxylic acid may be an acid anhydride.
[0040] Examples of polyfunctional polysaccharides include cellulose, cellulose nitrate, methylcellulose, ethylcellulose, celluloid, viscose rayon, regenerated cellulose, cellophane, cupra, cuprammonium rayon, cuprophane, Bemberg, hemicellulol, starch, acropectin, dextrin, dextran, glycogen, pectin, chitin, chitosan, gum arabic, guar gum, locust bean gum, and acacia gum.
[0041] In the polylactic acid resin, the content of structural portions derived from lactic acid (L- and D-form) in the molecule is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, particularly preferably 80% by mass or more, and most preferably 90% by mass or more.
[0042] At least a part of the polylactic acid resin used as the raw material may be recycled.
[0043] The modifier exerts the effect of increasing the molecular weight of the polylactic acid resin and imparting a cross-linked structure or a long-chain branched structure to the molecular structure of the polylactic acid resin.
[0044] The modifier may be of only one type, or of two or more types.
[0045] To increase the molecular weight of polylactic acid resin, a chain extender such as carbodiimide can be used as a modifier. In the modification using a chain extender, a compound having one or more functional groups capable of undergoing a condensation reaction with a hydroxyl group or a carboxyl group present in the molecular structure of polylactic acid resin, such as an acrylic organic compound, an epoxy organic compound, or an isocyanate organic compound, can be used. That is, the molecular weight of polylactic acid resin can be increased by using a chain extender such as carbodiimide to bond an acrylic organic compound, an epoxy organic compound, an isocyanate organic compound, or the like to the polylactic acid resin.
[0046] In order to provide a crosslinked structure or a long-chain branched structure in the molecular structure of polylactic acid resin, for example, a radical initiator can be used as a modifier. In this case, polylactic acid resins are reacted with each other using a radical initiator having appropriate reactivity. When polylactic acid resins are reacted with each other using a radical initiator having appropriate reactivity, for example, the decomposition starting point of the polylactic acid resin in the extruder is attacked by the free radicals generated by the radical initiator, and the site becomes a crosslinked point (branching point) and can be stabilized. By performing such modification, the thermal stability of the polylactic acid resin is increased and the molecular weight is less likely to be reduced when passing through the extruder.
[0047] Examples of the radical initiator include organic peroxides, azo compounds, and halogen molecules, with organic peroxides being preferred.
[0048] Examples of organic peroxides include peroxy esters, hydroperoxides, dialkyl peroxides, diacyl peroxides, peroxydicarbonates, peroxyketals, and ketone peroxides.
[0049] Examples of peroxy esters include t-butylperoxy 2-ethylhexyl carbonate, t-hexylperoxy isopropyl monocarbonate, t-hexylperoxybenzoate, t-butylperoxybenzoate, t-butylperoxylaurate, t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxyacetate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, and t-butylperoxyisopropyl monocarbonate.
[0050] Examples of hydroperoxides include permethane hydroperoxide, diisopropylbenzene hydroperoxide, cumene hydroperoxide, and t-butyl hydroperoxide.
[0051] Examples of dialkyl peroxides include dicumyl peroxide, di-t-butyl peroxide, and 2,5-dimethyl-2,5-di(t-butylperoxy)-hexyne-3.
[0052] Examples of diacyl peroxides include dibenzoyl peroxide, di(4-methylbenzoyl) peroxide, and di(3-methylbenzoyl) peroxide.
[0053] Examples of peroxydicarbonates include di(2-ethylhexyl) peroxydicarbonate and diisopropyl peroxydicarbonate.
[0054] Examples of peroxyketals include 1,1-di-t-butylperoxy-3,3,5-trimethylcyclohexane, 1,1-di-t-butylperoxycyclohexane, 2,2-di(t-butylperoxy)-butane, n-butyl 4,4-di-(t-butylperoxy)valerate, and 2,2-bis(4,4-di-t-butylperoxycyclohexyl)propane.
[0055] Examples of the ketone peroxide include methyl ethyl ketone peroxide and acetylacetone peroxide.
[0056] In the modification with organic peroxide, there is a risk that the modified polylactic acid resin may be mixed with components having an excessively large molecular weight that may gel when thermally melted, or that odor problems may occur due to decomposition residues of the organic peroxide. The organic peroxide is preferably a peroxyester, in that it can suppress the occurrence of such problems and can easily modify the polylactic acid resin to a state suitable for foaming. Among peroxyesters, peroxycarbonate-based organic peroxides such as peroxymonocarbonate and peroxydicarbonate are preferred. Furthermore, among peroxycarbonate-based organic peroxides, peroxymonocarbonate-based organic peroxides are preferred, and t-butylperoxyisopropylmonocarbonate is more preferred.
[0057] The amount of organic peroxide used depends on the molecular weight, etc., but in order to more effectively exhibit the effects of the present invention, it is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, and even more preferably 0.3 parts by mass or more, relative to 100 parts by mass of polylactic acid resin. The upper limit of the amount of organic peroxide used is preferably 2.0 parts by mass or less, more preferably 1.5 parts by mass or less, and even more preferably 1.0 part by mass or less.
[0058] The polylactic acid resin composition containing the polylactic acid resin and the modifier may contain any appropriate other components than the polylactic acid resin and the modifier within a range that does not impair the effects of the present invention. The total content of the polylactic acid resin and the modifier in the polylactic acid resin composition containing the polylactic acid resin and the modifier is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 100% by mass, even more preferably 90% by mass to 100% by mass, and particularly preferably 95% by mass to 100% by mass.
[0059] The polylactic acid resin composition containing the polylactic acid resin and the modifier may be prepared by previously mixing the polylactic acid resin, the modifier, and other components as necessary. Examples of the method for mixing include a mixing method using a mixer such as a tumbler, a ribbon blender, a V blender, a Henschel mixer, or a Redigay mixer.
[0060] As the extruder, any appropriate extruder may be used as long as the effects of the present invention are not impaired. In terms of being able to more effectively exhibit the effects of the present invention, the extruder is preferably a twin-screw extruder.
[0061] The twin-screw extruder may be equipped with a strand die or a T-die. In this case, the extruded strand- or sheet-shaped kneaded product may be cooled and cut with a pelletizer or the like to be pelletized.
[0062] The twin-screw extruder may be equipped with a pelletizing die (hot-cut die), in which case the kneaded material is pelletized immediately after extrusion.
[0063] The temperature conditions for melt kneading may vary depending on the size of the extruder, the discharge amount, etc., and any appropriate conditions may be adopted as long as the effects of the present invention are not impaired. For example, the temperature of the raw material feed section is preferably set to 100°C to 200°C.
[0064] The rotation speed of the extruder may vary depending on the size of the extruder, the discharge amount, etc., and any appropriate condition may be adopted as long as the effects of the present invention are not impaired. For example, such a rotation speed is preferably 20 rpm to 800 rpm.
[0065] The modified polylactic acid resin may be a dried product. Typically, the modified polylactic acid resin may be a product obtained by cooling a strand-shaped kneaded product extruded from a twin-screw extruder equipped with a strand die, cutting the product with a pelletizer or the like, and drying the pellets.
[0066] The modified polylactic acid resin can be produced using any appropriate device as long as the effects of the present invention are not impaired. For example, the modified polylactic acid resin can be produced using a production device as shown in FIG.
[0067] In FIG. 1, polylactic acid resin as a raw material is charged into a hopper 11 and melt-kneaded by a twin-screw extruder 30. The strand-shaped kneaded material extruded from a strand die 3 is cooled by a cooling device 6, and then pelletized by a pelletizer 4 and dried by a drying device 5 to obtain polylactic acid resin.
[0068] The melt tension of the modified polylactic acid resin is preferably 5 cN to 100 cN, more preferably 10 cN to 80 cN, further preferably 20 cN to 70 cN, and particularly preferably 25 cN to 60 cN, in order to further exert the effects of the present invention. The method for measuring the melt tension will be described later.
[0069] <1-1-b. Details of polylactic acid resin foam sheet in embodiment A> In embodiment A, the polylactic acid resin foamed sheet according to the embodiment of the present invention is produced by foaming a polylactic acid resin composition containing a polylactic acid resin (P) containing a modified polylactic acid resin as a main component.
[0070] The polylactic acid resin (P) contains a modified polylactic acid resin as a main component. The content of the modified polylactic acid resin in the polylactic acid resin (P) is preferably more than 50% by mass, more preferably 70% by mass or more, even more preferably 90% by mass or more, particularly preferably 95% by mass or more, and most preferably substantially 100% by mass.
[0071] The polylactic acid resin (P) may contain a polylactic acid resin (unmodified polylactic acid resin) in addition to a modified polylactic acid resin.
[0072] In embodiment A, the polylactic acid resin foam sheet according to the embodiment of the present invention is preferably prepared by foaming a polylactic acid resin composition containing a polylactic acid resin (P) and a foaming agent.
[0073] In embodiment A, the polylactic acid resin foam sheet according to the embodiment of the present invention is preferably obtained by melt-kneading a polylactic acid resin composition containing a polylactic acid resin (P) and a foaming agent in an extruder, and extrusion-foaming the polylactic acid resin composition.
[0074] The foaming agent may be of only one type, or of two or more types.
[0075] As the foaming agent, any appropriate foaming agent can be used within a range that does not impair the effects of the present invention. Examples of the foaming agent include a volatile foaming agent that becomes gas at room temperature (23°C) and normal pressure (1 atm) and a decomposition type foaming agent that generates gas by thermal decomposition, and a volatile foaming agent is preferred.
[0076] The volatile foaming agent is preferably an organic compound whose boiling point is equal to or lower than the softening point of polylactic acid resin and is in a gaseous or liquid state at normal pressure.Specific examples include aliphatic hydrocarbons such as propane, n-butane, isobutane, pentane (n-pentane, isopentane, neopentane), and n-hexane; alicyclic hydrocarbons such as cyclopentane and cyclopentadiene; ketones such as acetone and methyl ethyl ketone; alcohols such as methanol, ethanol, and isopropyl alcohol; low-boiling ether compounds such as dimethyl ether, diethyl ether, dipropyl ether, and methyl ethyl ether; halogen-containing hydrocarbons such as trichloromonofluoromethane and dichlorodifluoromethane.The volatile foaming agent may also be an inorganic gas such as carbon dioxide, nitrogen, or ammonia. Among these, in terms of further exerting the effects of the present invention, the volatile blowing agent is preferably at least one selected from n-butane, isobutane, n-pentane, isopentane, neopentane, cyclopentane, and cyclopentadiene, and more preferably at least one selected from n-butane, isobutane, n-pentane, and isopentane.
[0077] Decomposition type foaming agents include, for example, azodicarbonamide, dinitrosopentamethylenetetramine, sodium bicarbonate, or a mixture of an organic acid or its salt, such as citric acid, and a bicarbonate.
[0078] The amount of the foaming agent used can be appropriately set depending on the purpose. The amount of the foaming agent used is preferably 0.1 to 10.0 parts by mass, more preferably 0.3 to 7.0 parts by mass, even more preferably 0.5 to 5.0 parts by mass, and particularly preferably 0.8 to 3.0 parts by mass, based on 100 parts by mass of the modified polylactic acid resin.
[0079] The polylactic acid resin composition may contain any other appropriate components other than the modified polylactic acid resin and the foaming agent within a range that does not impair the effects of the present invention. The total content of the modified polylactic acid resin and the foaming agent in the total of the modified polylactic acid resin, the foaming agent, and other components contained as necessary in the polylactic acid resin composition is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 99.9% by mass, even more preferably 90% by mass to 99.9% by mass, particularly preferably 97% by mass to 99.8% by mass, and most preferably 97.6% by mass to 99.7% by mass.
[0080] The polylactic acid resin composition preferably contains a bubble regulator as another component. The bubble regulator may be one type or two or more types. Examples of the bubble regulator include higher fatty acid amides, partial esters of higher fatty acids and alcohols, talc, calcium carbonate, mica, citric acid, sodium bicarbonate, polytetrafluoroethylene, aluminum hydroxide, and silica. Examples of higher fatty acid amides include fatty acid monoamides such as oleic acid amide, stearic acid amide, and hydroxystearic acid amide; and fatty acid bisamides such as methylene bisstearic acid amide and ethylene bisstearic acid amide. Examples of higher fatty acids in the partial esters of higher fatty acids and alcohols include fatty acids having 15 or more carbon atoms, such as palmitic acid, stearic acid, oleic acid, linoleic acid, linolenic acid, and behenic acid. Examples of the partial esters of higher fatty acids and alcohols include stearic acid monoglyceride and stearic acid diglyceride.
[0081] The content of the cell regulator in the polylactic acid resin composition is preferably 0.01% by mass to 20% by mass, more preferably 0.1% by mass to 10% by mass, even more preferably 0.2% by mass to 5.0% by mass, and particularly preferably 0.3% by mass to 4.0% by mass, in order to further exert the effects of the present invention.
[0082] The polylactic acid resin composition may contain a foaming aid as another component. The foaming aid may be one type or two or more types. Examples of the foaming aid include diisobutyl adipate, toluene, cyclohexane, ethylbenzene, liquid paraffin, and coconut oil.
[0083] Examples of other components other than those mentioned above include other resins, pigments, radiant heat transfer suppressing components, crosslinking agents, plasticizers, stabilizers, fillers, lubricants, colorants, antioxidants, antistatic agents, spreading agents, weather resistance agents, flame retardants, ultraviolet absorbing agents, light stabilizers, antiaging agents, anti-fogging agents, fragrances, and antibacterial agents.
[0084] The modified polylactic acid resin, the cell regulator, and other components as necessary may be mixed in advance. Examples of the mixing method include a mixing method using a mixer such as a tumbler, a ribbon blender, a V blender, a Henschel mixer, or a Redigay mixer.
[0085] As the extruder, any appropriate extruder may be used as long as the effects of the present invention are not impaired. In terms of being able to more effectively exhibit the effects of the present invention, a tandem extruder is preferably used as the extruder.
[0086] The tip of the tandem extruder is provided with any appropriate die so as to ultimately obtain a polylactic acid resin foam sheet, as long as the effects of the present invention are not impaired. Preferably, the extruder may further be provided with a cooling mandrel, a take-up roller for winding up the polylactic acid resin foam sheet into a raw roll, and the like.
[0087] The polylactic acid resin foam sheet can be produced using any appropriate apparatus as long as the effects of the present invention are not impaired. For example, the polylactic acid resin foam sheet can be produced using a production apparatus as shown in FIG.
[0088] The manufacturing apparatus shown in Fig. 2 includes a tandem extruder 10 and a circular die CD for discharging the polylactic acid resin composition melt-kneaded in the tandem extruder 10 into a cylindrical shape. The manufacturing apparatus further includes a cooling device CL for air-cooling the foamed sheet discharged from the circular die CD into a cylindrical shape, a mandrel MD for expanding the diameter of the cylindrical foamed sheet into a cylindrical shape of a predetermined size, a slitting device for slitting the foamed sheet after passing through the mandrel MD and dividing it into two sheets, and a take-up roller 22 for winding up the slit foamed sheet 1 after passing through a plurality of rollers 21. The extruder upstream of the tandem extruder 10 (hereinafter also referred to as "first extruder 10a") includes a hopper 11 for introducing the modified polylactic acid resin that is the raw material of the foamed sheet, and a gas introduction section 12 for supplying a foaming agent into the cylinder. An extruder (hereinafter also referred to as "second extruder 10b") is provided downstream of the first extruder 10a for melt-kneading a polylactic acid resin composition containing a modified polylactic acid resin and a foaming agent.
[0089] The temperature conditions of the melt kneading may vary depending on the size and discharge amount of the extruder, and therefore any appropriate conditions may be adopted within a range that does not impair the effects of the present invention. For example, the temperature of the raw material feed section of the upstream extruder 10a is preferably set to 100°C to 200°C, more preferably 140°C to 200°C, the temperature after the upstream extruder 10a is preferably set to 120°C to 300°C, more preferably 140°C to 270°C, and the temperature of the downstream extruder 10b is preferably set to 100°C to 250°C, more preferably 120°C to 220°C.
[0090] The rotation speed of the extruder may vary depending on the size of the extruder, the discharge amount, etc., and any appropriate condition may be adopted within a range that does not impair the effects of the present invention. For example, the rotation speed of the upstream extruder 10a is preferably 10 rpm to 300 rpm, and the rotation speed of the downstream extruder 10b is preferably 5 rpm to 200 rpm.
[0091] 1-2. Polylactic acid resin foam sheet in embodiment B In embodiment B, the polylactic acid resin foamed sheet according to the embodiment of the present invention is produced by foaming a polylactic acid resin composition containing a polylactic acid resin (P) containing a polylactic acid resin (unmodified polylactic acid resin) as a main component.
[0092] The polylactic acid resin (P) contains polylactic acid resin (unmodified polylactic acid resin) as a main component. The content of polylactic acid resin (unmodified polylactic acid resin) in the polylactic acid resin (P) is preferably more than 50% by mass, more preferably 70% by mass or more, even more preferably 90% by mass or more, particularly preferably 95% by mass or more, and most preferably substantially 100% by mass.
[0093] The polylactic acid resin (P) may contain a modified polylactic acid resin in addition to the polylactic acid resin (unmodified polylactic acid resin).
[0094] In embodiment B, the polylactic acid resin foam sheet according to the embodiment of the present invention is preferably prepared by foaming a polylactic acid resin composition containing a polylactic acid resin (P) and a foaming agent.
[0095] In embodiment B, the polylactic acid resin foam sheet according to the embodiment of the present invention is preferably obtained by melt-kneading a polylactic acid resin composition containing a polylactic acid resin (P) and a foaming agent in an extruder, and extrusion-foaming the polylactic acid resin composition.
[0096] For the polylactic acid resin, the explanation in the above section <1-1-a. Modified polylactic acid resin> can be directly applied.
[0097] Regarding the type of foaming agent, the explanation in the above section <1-1-b. Details of the polylactic acid resin foamed sheet in embodiment A> can be directly applied.
[0098] The amount of the foaming agent used can be appropriately set depending on the purpose. The amount of the foaming agent used is preferably 0.1 to 10.0 parts by mass, more preferably 0.3 to 7.0 parts by mass, even more preferably 0.5 to 5.0 parts by mass, and particularly preferably 0.8 to 3.0 parts by mass, based on 100 parts by mass of the polylactic acid resin.
[0099] The polylactic acid resin composition may contain any other appropriate components other than the polylactic acid resin and the foaming agent within a range that does not impair the effects of the present invention. The total content of the polylactic acid resin and the foaming agent in the total of the polylactic acid resin, the foaming agent, and other components contained as necessary in the polylactic acid resin composition is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 99.9% by mass, even more preferably 90% by mass to 99.5% by mass, particularly preferably 93% by mass to 99.2% by mass, and most preferably 95% by mass to 99% by mass.
[0100] The polylactic acid resin composition preferably contains a modifier as another component. By containing the modifier, the polylactic acid resin can have a high molecular weight and can have a crosslinked structure or a long chain branched structure in the molecular structure of the polylactic acid resin.
[0101] For the modifier, the explanation in the above section <1-1-a. Modified polylactic acid resin> can be used as is.
[0102] The polylactic acid resin composition preferably contains a cell regulator as another component. For the cell regulator, the description in the above section <1-1-b. Details of the polylactic acid resin foam sheet in embodiment A> may be used as is.
[0103] The polylactic acid resin composition may contain a foaming assistant as another component. For the foaming assistant, the explanation in the above section <1-1-b. Details of the polylactic acid resin foam sheet in embodiment A> may be used as is.
[0104] Examples of other components other than those mentioned above include other resins, pigments, radiant heat transfer suppressing components, crosslinking agents, plasticizers, stabilizers, fillers, lubricants, colorants, antioxidants, antistatic agents, spreading agents, weather resistance agents, flame retardants, ultraviolet absorbing agents, light stabilizers, antiaging agents, anti-fogging agents, fragrances, and antibacterial agents.
[0105] The polylactic acid resin, the modifier, the cell regulator, and other components as necessary may be mixed in advance. Examples of the mixing method include a mixing method using a mixer such as a tumbler, a ribbon blender, a V blender, a Henschel mixer, or a Redigay mixer.
[0106] As the extruder, any appropriate extruder may be used as long as the effects of the present invention are not impaired. In terms of being able to more effectively exhibit the effects of the present invention, a twin-screw extruder is preferable as the extruder.
[0107] The tip of the twin-screw extruder is provided with any appropriate die so as to ultimately obtain a polylactic acid resin foam sheet, as long as the effects of the present invention are not impaired. Preferably, the extruder may further be provided with a cooling mandrel, a winding roller for winding up the polylactic acid resin foam sheet into a raw roll, and the like.
[0108] The polylactic acid resin foam sheet can be produced using any appropriate apparatus as long as the effects of the present invention are not impaired. For example, the polylactic acid resin foam sheet can be produced using a production apparatus as shown in FIG.
[0109] The manufacturing apparatus shown in FIG. 3 includes a twin-screw extruder 30 and a circular die CD for discharging the polylactic acid resin composition melt-kneaded in the twin-screw extruder 30 into a cylindrical shape. The manufacturing apparatus further includes a cooling device CL for air-cooling the foamed sheet discharged from the circular die CD into a cylindrical shape, a mandrel MD for expanding the diameter of the cylindrical foamed sheet into a cylindrical shape of a predetermined size, a slitting device for slitting the foamed sheet after passing through the mandrel MD and dividing it into two sheets, and a winding roller 22 for winding up the slit foamed sheet 1 after passing through a plurality of rollers 21. A hopper 11 for feeding the polylactic acid resin, which is the raw material of the foamed sheet, is provided on the upstream side of the twin-screw extruder 30. A gas introduction section 12 for supplying a foaming agent into the cylinder is provided on the downstream side of the twin-screw extruder 30. When the extrusion foaming process is carried out with such an apparatus, the polylactic acid resin is modified and mixed with a foaming agent, etc., in the twin-screw extruder 30 to prepare a polylactic acid resin composition as the raw material for the foamed sheet, and extrusion foaming is carried out through the circular die CD.
[0110] The temperature conditions for melt kneading may vary depending on the size of the extruder, the discharge amount, etc., and any appropriate conditions may be adopted within a range that does not impair the effects of the present invention. For example, the temperature of the raw material feed section of the twin-screw extruder 30 is preferably set to 100°C to 200°C, more preferably 120°C to 200°C, and the temperature after the twin-screw extruder 30 is preferably set to 120°C to 300°C, more preferably 120°C to 250°C.
[0111] The rotation speed of the extruder may vary depending on the size of the extruder, the discharge amount, etc., and any appropriate condition may be adopted within a range that does not impair the effects of the present invention. For example, the rotation speed of the twin-screw extruder 30 is preferably 20 rpm to 800 rpm.
[0112] ≪≪2. Polylactic acid resin foam molding≫≫ The polylactic acid resin foam molded article according to the embodiment of the present invention is obtained by molding the polylactic acid resin foam sheet according to the embodiment of the present invention.
[0113] The polylactic acid resin foam molded article according to the embodiment of the present invention can be obtained by, typically, heating and softening the polylactic acid resin foam sheet according to the embodiment of the present invention, and subjecting it to thermoforming using a mold, such as a vacuum molding method and / or a pressure molding method, or a matched mold molding method or a plug-assisted molding method that are applications of these methods.
[0114] The polylactic acid resin foam molded article according to the embodiment of the present invention may be used as, for example, food containers such as trays, cups, bowls, lunch boxes, fruit containers, vegetable containers, etc.; cushioning materials such as cushioning materials for electrical products and cushioning materials for precision instruments; and the like. EXAMPLES
[0115] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring and evaluating each property are as follows.
[0116] <Measurement of the average cell diameter of polylactic acid resin foam sheet> A piece was cut from the widthwise center of the original polylactic acid resin foam sheet perpendicular to the surface of the original sheet along the MD direction (extrusion flow direction) and TD direction (width direction perpendicular to the MD direction on the surface of the sheet). One of the cross sections to be observed was a cross section of the sample cut along a plane parallel to the MD direction (extrusion flow direction) and perpendicular to the surface of the polylactic acid resin foam sheet (hereinafter referred to as the "MD cross section"), and the other cross section to be observed was a cross section of the sample cut along a plane parallel to the TD direction (width direction perpendicular to the MD direction on the surface of the sheet) and perpendicular to the surface of the polylactic acid resin foam sheet (hereinafter referred to as the "TD cross section"). The cross section was photographed at a magnification of 20x using a scanning electron microscope (SU1510, Hitachi High-Technologies Corporation). The microscopic images were photographed so that the specified magnification would be achieved when two images (four images in total) were printed side by side on a single sheet of A4 paper in landscape orientation. Specifically, on the image, 60mm arbitrary straight lines parallel to each of the MD and TD directions and 60mm straight lines perpendicular to each direction (VD direction) were drawn, and two microscope images of four fields of view were taken for each of the cross sections cut along the MD direction (MD cross section) and the cross sections cut along the TD direction (TD cross section), and printed on A4 paper. Three arbitrary straight lines (60mm long) parallel to the MD direction were drawn on each of the two images of the MD cross section, and three arbitrary straight lines (60mm long) parallel to the TD direction were drawn on each of the two images of the TD cross section. In addition, three straight lines (60mm long) parallel to the VD direction were drawn on one image of the MD cross section and one image of the TD cross section, and six arbitrary straight lines of 60mm long parallel to the MD, TD, and VD directions were drawn in each direction. In addition, an attempt was made to avoid any bubbles touching any straight line at the point of contact, and if any bubbles did come into contact, these bubbles were also counted. The number of bubbles D counted for six arbitrary straight lines in each of the MD, TD, and VD directions was calculated as the arithmetic mean, which was used as the number of bubbles in each direction. The average chord length t of the bubbles in each direction was calculated from the image magnification at which the number of bubbles was counted and the number of bubbles using the following formula. Average chord length t (μm) = 60000 / (number of bubbles x image magnification) (Average chord length in MD direction tM (μm) = 60000 / (number of bubbles in MD direction × image magnification)) (Average chord length in TD direction tT (μm) = 60000 / (number of bubbles in TD direction × image magnification)) (Average chord length in the VD direction tV (μm) = 60000 / (number of bubbles in the VD direction × image magnification)) The image magnification was calculated by measuring the scale bar on the image to the nearest 1 / 100 mm using a Digimatic Caliper (manufactured by Mitutoyo Corporation) and using the following formula: Image magnification = Scale bar actual value (mm) / Scale bar display value (mm) The bubble diameter in each direction was calculated using the following formula. Average bubble diameter in MD direction dM (μm) = tM (μm) / 0.616 Average bubble diameter in TD direction dT (μm) = tT (μm) / 0.616 Average bubble diameter in VD direction dV (μm) = tV (μm) / 0.616 Furthermore, the cube root of the product was determined as the average bubble diameter. Average bubble diameter d(μm)=(dM(μm)×dT(μm)×dV(μm)) 1 / 3
[0117] <Measurement of the average cell diameter of polylactic acid resin foam sheet after heat treatment> A flat square test piece measuring 340 mm long x 340 mm wide was cut out from the original roll of polylactic acid resin foam sheet. A single shot molding machine (manufactured by Tosei Sangyo Co., Ltd., product name "FM-3A") was used, and the average temperature of the upper heater of this single shot molding machine was set to 300°C, and the average temperature of the lower heater was set to 300°C. Next, the test piece was introduced into the single shot molding machine and heated until the sheet surface temperature reached 110°C ± 10°C, to obtain a secondary foam sheet. The average cell diameter of the resulting post-foamed sheet was measured in the same manner as described above.
[0118] <Melt tension (MT) measurement> The melt tension was measured using Capilograph 1D (Toyo Seiki Seisakusho Co., Ltd.) and Rheotens 71.97 (Gottfert Co., Ltd.) as measuring devices. The measurement samples were vacuum dried at 90°C for 5 hours or more in advance, and after drying, they were placed in nylon plastic bags for vacuum packing, vacuum packed, and stored in a desiccator until just before the measurement. First, a measurement sample is filled into a 9.55 mm diameter barrel heated to a test temperature of 190°C, and then preheated for 5 minutes. The molten resin is extruded into a string shape from the capillary die (diameter 2.095 mm, length 8 mm, inlet angle 90 degrees (conical)) of the above measurement device while maintaining a constant piston descending speed (20 mm / min). This string shape is passed through a wheel (wheel interval: upper 0.6 mm to 0.8 mm, lower 1.0 mm) installed so that the distance from the outlet of the capillary die to the measurement part is 80 mm, and the initial speed is set to 6.92 mm / s, and the acceleration is set to 10 mm / s. 2The Rheotens was passed through the wire while gradually increasing the tension, and the average of the maximum and minimum tension values just before the point where the string-like object broke was taken as the melt tension (MT) of the measured sample. If the Rheotens could not be brought closer to 80 mm due to interference, measures were taken to avoid interference and set the Rheotens in a specified location. If there was only one maximum point on the tension chart, the maximum value was taken as the melt tension, and if the string-like object became thinner and the take-up was in an idle state, that point was taken as the break point, and the average of the maximum and minimum tension values just before that was taken as the melt tension of the measured sample. [Measurement conditions for "Capillograph 1D"] Die: diameter 2.095mm, length 8mm, inlet angle 90 degrees (conical) Barrel diameter: 9.55mm Piston speed: 20mm / min Measurement temperature: 190℃ [Measurement conditions for "Rheotens 71.97"] Wheel spacing: Top 0.6mm~0.8mm, bottom 1.0mm Acceleration: 10mm / s 2 Pulling speed: Initial speed 6.92mm / s
[0119] <Measurement of open cell ratio> Cut out several sheet-like samples of 25 mm length and 25 mm width from the polylactic acid resin foam sheet, stack the cut samples without leaving any gaps to make a measurement sample of 25 mm thickness, measure the outer dimensions of this measurement sample to 1 / 100 mm using a "Digimatic Caliper" made by Mitutoyo Corporation, and calculate the apparent volume (cm 3 ) was sought. Next, the volume (cm) of the sample to be measured was measured using an air comparison type specific gravity meter Model 1000 (Tokyo Science Co., Ltd.) by the 1-1 / 2-1 atmospheric pressure method. 3 ) was sought. The open cell ratio (%) was calculated from these determined values and the following formula, and the average value for five test pieces was calculated. In addition, the measurement was carried out under the environment of JIS K7100-1999 symbol 23 / 50, grade 2 after conditioning the measurement sample for 16 hours under the environment of JIS K7100-1999 symbol 23 / 50, grade 2. Also, the air comparison type pycnometer was calibrated with standard spheres (large: 28.9 cc, small: 8.5 cc). Apparent porosity (%) = [(Apparent volume - Measured volume by air comparison type pycnometer) / Apparent volume] × 100 (%)
[0120] <Measurement of MFR (Melt Mass Flow Rate)> MFR was measured in accordance with the standard of JIS K 7210:1999. Specifically, it was measured by the method of "b) Measuring the time for the piston to move a predetermined distance" described in Method B of the same standard. MFR was measured using a melt flow index tester (automatic) 120-SAS (manufactured by Yasuda Seiki Seisakusho Co., Ltd.). The sample used was one that had been vacuum dried at 90°C for 5 hours and then sealed and stored in a desiccator until immediately before the measurement. The number of measurements was 3 times, and the average was taken as the value of MFR (g / 10 min). The measurement conditions were as follows. Sample: 3 g to 8 g Preheating (1): 200 seconds Preheating (2): 30 seconds Test temperature: 190°C Test load: 21.18 N Piston movement distance (interval): 4 mm
[0121] <Measurement of Foaming Ratio> The foaming ratio of the polylactic acid resin foamed sheet can be obtained by determining the apparent density (ρ1) of the polylactic acid resin foamed sheet and the density (true density: ρ0) of the polylactic acid resin composition constituting the polylactic acid resin foamed sheet, and dividing the true density (ρ0) by the apparent density (ρ1). Foaming ratio = True density (ρ0) / Apparent density (ρ1) The density of the foamed sheet can be determined by the method described in JIS-K7222:1999 "Foamed Plastics and Rubbers - Measurement of Apparent Density", and specifically, it was determined by the following method. (Density Measurement Method) From polylactic acid resin foam sheet, 100cm 3 The above samples were cut without changing the original cell structure, and the samples were conditioned for 16 hours in a JIS K7100:1999, symbol 23 / 50, class 2 environment, after which the dimensions and mass were measured, and the density was calculated according to the following formula. Apparent density (kg / m 3 ) = mass of sample (kg) / volume of sample (m 3 ) The dimensions of the samples were measured using a "DIGIMATIC" CD-15 type manufactured by Mitutoyo Corporation. The density of the polylactic acid resin composition constituting the polylactic acid resin foam sheet was determined by measuring a sample of the polylactic acid resin foam sheet that had been made non-foamed by, for example, heat pressing, based on the Archimedes method (the liquid weighing method of JIS-K8807:2012 "Methods for determining density and specific gravity of solids").
[0122] <Punching evaluation> A flat square test piece measuring 340 mm long x 340 mm wide was cut out from the original roll of polylactic acid resin foam sheet. A single shot molding machine (manufactured by Tosei Sangyo Co., Ltd., product name "FM-3A") was used, and the average temperature of the upper heater of this single shot molding machine was set to 300°C, and the average temperature of the lower heater was set to 300°C. Next, the test piece was introduced into the single shot molding machine and heated for 30 seconds until the sheet surface temperature reached 110°C ± 10°C, and five foamed containers having an opening at the top were produced by thermoforming for each of the examples and comparative examples. The container shape is an inverted pyramidal foam container with a square bottom (opening 140 mm x 150 mm, bottom 110 mm x 110 mm, height 60 mm). The obtained foamed container was punched using a punching blade (160 mm x 170 mm), and the occurrence of cracks around the punched portion was evaluated according to the following criteria. ◯: None of the five pieces had cracks around the punched area, indicating that the compressive strength was very high. △: The number of cracks around the punched area was three or less, indicating high compressive strength. ×: Cracks occurred around the punched portion in 4 or more out of 5 pieces, which indicates low compressive strength.
[0123] [Production Example 1] Polylactic acid resin (Nature Works "Biopolymer Ingeo 6202D", MFR = 15-30g / 10min, density = 1.24g / cm 3 A mixture was obtained by stirring and mixing 100 parts by mass of 1,000g of tert-butylperoxyisopropyl monocarbonate (manufactured by Kayaku Nouryon, "Trigonox BPIC-75", 1-minute half-life temperature T1 = 158.8°C) in a ribbon blender. The mixture was fed from the feed port of a twin-screw extruder (L / D=31.5) with a diameter of 57 mm. The twin-screw extruder has, from the upstream side to the downstream side, a feed section to which the mixture is fed, a reaction section in which the polylactic acid resin is modified, and a kneading section in which the resin composition obtained in the reaction section is kneaded. The above mixture was melt-kneaded in a twin-screw extruder under conditions of a feed section temperature of 140°C, a reaction section temperature of 200°C, a kneading section temperature of 185°C, and a rotation speed of 150 rpm, and the kneaded product was extruded in the form of strands at an output rate of 30 kg / h from a die with a diameter of 3 mm and 18 holes attached to the tip of the twin-screw extruder. Next, the extruded strand-like kneaded product was passed through a 2 m long cooling water tank containing water at 30° C. to cool it. The cooled strands were cut with a pelletizer to obtain pellets of the modified polylactic acid resin. The melt tension of the resulting modified polylactic acid resin was 49.9 cN.
[0124] [Production Example 2] Using the twin-screw extruder used in Production Example 1, polylactic acid resin (Nature Works "Biopolymer Ingeo 6202D", MFR = 15 to 30 g / 10 min, density = 1.24 g / cm 3The polylactic acid resin (moisture content: 0.02 wt%) and a bubble regulator ("Crown Talc" manufactured by Matsumura Sangyo Co., Ltd.) were kneaded in a mass ratio of 1:1 to produce a master batch of polylactic acid resin and bubble regulator (polylactic acid resin: bubble regulator (mass ratio) = 1:1).
[0125] [Example 1] A mixture was prepared by dry blending 95.5 parts by mass of the modified polylactic acid resin obtained in Production Example 1 and 4.5 parts by mass of the master batch (polylactic acid resin:cell control agent (mass ratio) = 1:1) obtained in Production Example 2. In a tandem extruder equipped with a first extruder (upstream) with a diameter of φ90 mm and a second extruder (downstream) with a diameter of φ115 mm, the obtained mixture was supplied to the first extruder with a diameter of φ90 mm through a hopper and heated and melted at 200°C to 230°C. Thereafter, butane (isobutane / normal butane=70 / 30) as a foaming agent was pressure-fed into the first extruder and melt-mixed together with the above mixture. Next, this molten mixture was transferred to a second extruder with an aperture of 115 mm and cooled to about 165°C, after which it was extruded and foamed through a circular die with an aperture of 270 mm at a discharge rate of 100 kg / h to obtain a cylindrical foam. The obtained cylindrical foam was placed on a φ672 mm mandrel whose inside was cooled with water at about 20°C, and its outer surface was cooled and molded by blowing air onto it using an air ring larger than its diameter. It was then cut at one point on the circumference with a cutter to obtain a strip-shaped polylactic acid resin foam sheet (1). The results are shown in Table 1.
[0126] [Example 2] A strip-shaped polylactic acid resin foam sheet (2) was obtained in the same manner as in Example 1, except that the amount of the modified polylactic acid resin obtained in Production Example 1 was changed to 95.2 parts by mass, and the amount of the master batch (polylactic acid resin:cell control agent (mass ratio) = 1:1) obtained in Production Example 2 was changed to 4.8 parts by mass. The results are shown in Table 1.
[0127] [Example 3] The same procedure as in Example 1 was carried out, except that the amount of the modified polylactic acid resin obtained in Production Example 1 was changed to 97.0 parts by mass, and the amount of the master batch (polylactic acid resin:cell bubble regulator (mass ratio) = 1:1) obtained in Production Example 2 was changed to 3.0 parts by mass, to obtain a strip-shaped polylactic acid resin foam sheet (3). The results are shown in Table 1.
[0128] [Example 4] A mixture was prepared by dry blending 97.7 parts by mass of the modified polylactic acid resin obtained in Production Example 1 and 2.3 parts by mass of the master batch obtained in Production Example 2 (polylactic acid resin:cell control agent (mass ratio) = 1:1). In a tandem extruder equipped with a first extruder (upstream) with a diameter of φ50 mm and a second extruder (downstream) with a diameter of φ65 mm, the obtained mixture was supplied to the first extruder with a diameter of φ50 mm through a hopper and heated and melted at 200°C to 230°C. Thereafter, butane (isobutane / normal butane=70 / 30) as a foaming agent was pressure-fed into the first extruder and melt-mixed together with the above mixture. Next, this molten mixture was transferred to a second extruder with a diameter of 65 mm and cooled to about 165°C, after which it was extruded and foamed through a circular die with a diameter of 70 mm at a discharge rate of 30 kg / h to obtain a cylindrical foam. The obtained cylindrical foam was placed on a φ206 mm mandrel whose inside was cooled with water at about 20°C, and its outer surface was cooled and molded by blowing air onto it using an air ring larger in diameter than the mandrel. Then, it was cut at one point on the circumference using a cutter to obtain a belt-shaped polylactic acid resin foam sheet (4). The results are shown in Table 1.
[0129] [Example 5] The same procedure as in Example 4 was carried out, except that the amount of the modified polylactic acid resin obtained in Production Example 1 was changed to 99.0 parts by mass, and the amount of the master batch (polylactic acid resin:cell bubble regulator (mass ratio) = 1:1) obtained in Production Example 2 was changed to 1.0 part by mass, to obtain a strip-shaped polylactic acid resin foam sheet (5). The results are shown in Table 1.
[0130] [Example 6] The same procedure as in Example 4 was carried out, except that the amount of the modified polylactic acid resin obtained in Production Example 1 was changed to 96.0 parts by mass, and the amount of the master batch (polylactic acid resin:cell bubble regulator (mass ratio) = 1:1) obtained in Production Example 2 was changed to 4.0 parts by mass, to obtain a strip-shaped polylactic acid resin foam sheet (6). The results are shown in Table 1.
[0131] [Comparative Example 1] The same procedure as in Example 1 was carried out, except that the amount of the modified polylactic acid resin obtained in Production Example 1 was changed to 95.0 parts by mass, and the amount of the master batch (polylactic acid resin:cell control agent (mass ratio) = 1:1) obtained in Production Example 2 was changed to 5.0 parts by mass, to obtain a strip-shaped polylactic acid resin foam sheet (C1). The results are shown in Table 1.
[0132] [Comparative Example 2] The same procedure as in Example 4 was carried out, except that the amount of the modified polylactic acid resin obtained in Production Example 1 was changed to 94.5 parts by mass, and the amount of the master batch (polylactic acid resin:cell control agent (mass ratio) = 1:1) obtained in Production Example 2 was changed to 5.5 parts by mass, to obtain a strip-shaped polylactic acid resin foam sheet (C2). The results are shown in Table 1.
[0133] [Comparative Example 3] The same procedure as in Example 4 was carried out, except that the amount of the modified polylactic acid resin obtained in Production Example 1 was changed to 95.0 parts by mass, and the amount of the master batch (polylactic acid resin:cell control agent (mass ratio) = 1:1) obtained in Production Example 2 was changed to 5.0 parts by mass, to obtain a strip-shaped polylactic acid resin foam sheet (C3). The results are shown in Table 1.
[0134] [Comparative Example 4] The same procedure as in Example 4 was carried out, except that the amount of the modified polylactic acid resin obtained in Production Example 1 was changed to 90.0 parts by mass, and the amount of the master batch (polylactic acid resin:cell control agent (mass ratio) = 1:1) obtained in Production Example 2 was changed to 10.0 parts by mass, to obtain a strip-shaped polylactic acid resin foam sheet (C4). The results are shown in Table 1.
[0135] [Table 1] [Industrial Applicability]
[0136] The polylactic acid resin foam sheet of the present invention can be easily molded into a variety of shapes and can therefore be used as a raw material for various molded products, including packaging materials. [Explanation of symbols]
[0137] 1 Foam sheet 3 Strand Die 4 Pelletizer 5 Drying equipment 6 Cooling device 10 Tandem Extruder 10a First Extruder 10b Second Extruder 11 Hopper 12 Gas inlet 21 Laura 22 Winding roller 30 Twin screw extruder
Claims
1. A polylactic acid resin foam sheet obtained by foaming a polylactic acid resin composition containing a polylactic acid resin (P), The polylactic acid resin foamed sheet is heated until the surface temperature of the sheet reaches 110°C±10°C. After the heat treatment, the aspect ratios MV=dM / dV and TV=dT / dV calculated from the average cell diameter dM in the MD direction, the average cell diameter dT in the TD direction, and the average cell diameter dV in the VD direction of the polylactic acid resin foamed sheet are each 1.0 to 2.
0. Polylactic acid resin foam sheet.
2. 2. The polylactic acid resin foam sheet according to claim 1, wherein the average bubble diameter of the polylactic acid resin foam sheet is 150 μm to 850 μm.
3. 2. The polylactic acid resin foam sheet according to claim 1, wherein the polylactic acid resin foam sheet after the heat treatment has an average cell diameter of 200 μm to 1100 μm.
4. The apparent density of the polylactic acid resin foam sheet is 0.063 g / cm 3 ~0.5g / cm 3 2. The polylactic acid resin foam sheet according to claim 1,
5. 2. The polylactic acid resin foam sheet according to claim 1, wherein the polylactic acid resin foam sheet has a thickness of 0.5 mm to 7 mm.
6. 2. The polylactic acid resin foam sheet according to claim 1, wherein the polylactic acid resin foam sheet has an open cell ratio of 50% or less.
7. The polylactic acid resin foam sheet according to claim 1 , wherein the polylactic acid resin (P) is a modified polylactic acid resin.
8. A polylactic acid resin foamed molded article obtained by molding the polylactic acid resin foamed sheet according to any one of claims 1 to 7.
Citation Information
Patent Citations
Polylactic acid resin foam
JP6971947B2