Stretched film

JP2024144838AActive Publication Date: 2024-10-15C I TAKIRON CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023056979
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
2043-03-31

AI Technical Summary

Benefits of technology

【0010】 本発明によれば、水蒸気バリア性とリサイクル性に優れた延伸フィルムを提供することができる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144838000001_ABST
    Figure 2024144838000001_ABST
Patent Text Reader

Abstract

To provide a stretched film excellent in water vapor barrier properties and recyclability.SOLUTION: A stretched film includes, as a main component, an ultra-high molecular weight polyethylene having a viscosity-average molecular weight (Mv) of 500,000 to 3,000,000, and has a water vapor permeability per 50 μm of 2.15 g / m2 day or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a stretched film obtained by stretching an ultra-high molecular weight polyethylene film (hereinafter, sometimes simply referred to as "polyethylene film"), which is a raw film formed from a raw material containing as a main component polyethylene having an ultra-high molecular weight. [Background technology]

[0002] Conventionally, as a packaging film used for a pouch or the like, for example, a laminate has been adopted in which a base film made of a resin material and a sealant film made of a material different from the resin material that constitutes the base film are laminated together.

[0003] There is a demand for reducing the environmental impact of plastics in general, and recyclability is also required for packaging films. However, in the case of laminates in which films made of different materials are laminated as described above, there is a problem that recycling is difficult because it is difficult to separate the materials.

[0004] In recent years, therefore, there has been an active movement toward mono-material packaging films, which are made from a single material. Examples of resins used in mono-material packaging films include polyethylene, polypropylene, and polyethylene terephthalate. Of these, polyethylene is the material most frequently used in existing packaging films, and is particularly in demand as a mono-material.

[0005] As a packaging film using this polyethylene, for example, a laminate has been proposed that includes a base film and a sealant film, the base film and the sealant film being made of polyethylene, and the base film being stretched. It is described that such a configuration allows the base film and the sealant film to be made of the same material, thereby improving the recyclability of the laminate (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2019-171860 A Summary of the Invention [Problem to be solved by the invention]

[0007] When the packaged item is a medicine or food, the packaging film is required to have water vapor barrier properties. In the stretched film described in the above Patent Document 1, the resin constituting the base film has a water vapor barrier property of 0.945 g / cm 3 However, the base film has insufficient water vapor barrier properties, so it is necessary to provide a barrier coat layer made of a material different from the polyethylene that constitutes the base film. This reduces recyclability, making it difficult to achieve both water vapor barrier properties and recyclability.

[0008] Therefore, the present invention has been made in consideration of the above problems, and an object of the present invention is to provide a stretched film having excellent water vapor barrier properties and recyclability. [Means for solving the problem]

[0009] In order to achieve the above object, the stretched film of the present invention is a stretched film mainly composed of ultra-high molecular weight polyethylene having a viscosity average molecular weight (Mv) of 500,000 to 3,000,000, and having a water vapor transmission rate of 2.15 g / m per 50 μm. 2 The characteristic of this method is that it is less than 10 days. Effect of the Invention

[0010] According to the present invention, it is possible to provide a stretched film having excellent water vapor barrier properties and recyclability. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is a cross-sectional view illustrating a laminate using a stretched film according to the present invention. [Diagram 2] FIG. 2 is a diagram for explaining an endothermic peak in a DSC chart of the stretched film according to the present invention (according to Example 1). [Diagram 3] FIG. 2 is a plan view illustrating a laminate using a stretched film according to the present invention. [Figure 4] FIG. 1 is a schematic diagram showing an apparatus for producing an ultra-high molecular weight polyethylene solid-phase rolled film according to the present invention. [Diagram 5] 1 is a DSC chart of the stretched film in Example 8. [Figure 6] 1 is a DSC chart of a stretched film in Comparative Example 9. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The stretched film of the present invention will be specifically described below. Note that the present invention is not limited to the following embodiments, and can be appropriately modified and applied within the scope of the present invention.

[0013] The stretched film of the present invention is a stretched film obtained by stretching an ultra-high molecular weight polyethylene film containing solid powder of ultra-high molecular weight polyethylene as a main component.

[0014] FIG. 1 is a cross-sectional view showing a laminate using the stretched film of the present invention.

[0015] The laminate 1 includes a stretched film 3 of the present invention which serves as a base film, and a sealant film 2 laminated on the stretched film 3 .

[0016] <Sealant film> From the viewpoint of mono-material, the sealant film 2 of the present invention is preferably a polyethylene-based resin. More specifically, high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE), linear low density polyethylene (LLDPE), etc. are included.

[0017] From the viewpoint of improving heat sealability, it is preferable to use low density polyethylene (LDPE) or linear low density polyethylene (LLDPE) having a lower melting point than the base film in order to provide a difference in melting point with the base film.

[0018] Furthermore, the polyethylene content in the sealant film 2 is preferably 70% or more, more preferably 90% or more, even more preferably 95% or more, and most preferably 100%.

[0019] The thickness of the sealant film 2 is preferably from 20 μm to 200 μm, and more preferably from 30 μm to 150 μm.

[0020] Furthermore, the sealant film 2 may contain components other than the above-mentioned polyethylene resin, as long as the properties of the sealant film 2 are not impaired.

[0021] Other components include olefin resins, amide antiblocking agents (such as stearic acid amide), plasticizers, UV absorbers, antioxidants, weather stabilizers, antistatic agents, colorants, antifogging agents, metal soaps, waxes, mildew inhibitors, antibacterial agents, nucleating agents, flame retardants, lubricants, etc.

[0022] <Ultra-high molecular weight polyethylene> The ultra-high molecular weight polyethylene, which is the main component of the stretched film 3 of the present invention, is a solid powder, and one having a viscosity average molecular weight (Mv) of 500,000 to 3,000,000 can be used. This is because if the viscosity average molecular weight (Mv) is less than 500,000, extended chain crystals are not generated during the stretching process described below, so the crystallization degree of the polyethylene does not improve, and it may be difficult to improve the water vapor barrier property. Also, if the viscosity average molecular weight (Mv) is more than 3,000,000, the melt viscosity is too high, so molding by solid-phase roll rolling may be difficult with rolls of a general size.

[0023] In other words, by using a solid powder of ultra-high molecular weight polyethylene with a viscosity average molecular weight (Mv) of 500,000 to 3,000,000, formability by roll rolling can be ensured, and extended chain crystals are generated during stretching treatment, making it possible to improve the water vapor barrier properties of the stretched film.

[0024] As the ultra-high molecular weight polyethylene, for example, a commercially available product such as Mipelon XM-220 (manufactured by Mitsui Chemicals, Inc., viscosity average molecular weight: 2 million) can be used.

[0025] In addition, cross-linked polyethylene cross-linked by a cross-linking agent or electron beam irradiation or the like, or one that has been polymerized (synthesized) to have a viscosity average molecular weight of 500,000 to 3,000,000 may be used.

[0026] The viscosity average molecular weight is preferably from 1,000,000 to 2,500,000, and more preferably from 1,500,000 to 2,000,000.

[0027] The above "viscosity average molecular weight" refers to one calculated in accordance with JIS K 7367-3:1999.

[0028] The density of ultra-high molecular weight polyethylene is 0.930 to 0.950 g / cm 3 and 0.945 g / cm 3 Preferably, it is less than 0.940 g / cm 3When the molecular chains of ultra-high molecular weight polyethylene are folded to form crystals, the ultra-high molecular weight polyethylene becomes bulky due to its high molecular weight, and the amount of crystals formed is smaller than that of ordinary high density polyethylene, resulting in a lower density.

[0029] The ultra-high molecular weight polyethylene preferably has a melting point of 135° C. to 150° C. in the form of a solid powder immediately after polymerization, more preferably 137° C. to 150° C., and even more preferably 140° C. to 150° C. The melting point after recrystallization is preferably 130° C. to 140° C.

[0030] More specifically, the ultra-high molecular weight polyethylene described below (manufactured by Mitsui Chemicals, Inc., product name: Hi-Zex Million 030S, viscosity average molecular weight: 500,000, density: 0.949 g / cm 3 ) has a melting point of 136.2°C as a solid powder and 132.8°C after recrystallization.

[0031] In addition, the ultra-high molecular weight polyethylene described below (manufactured by Mitsui Chemicals, Inc., product name: Hi-Zex Million 145M, viscosity average molecular weight: 1.15 million, density: 0.940 g / cm 3 ) has a melting point of 138.4°C as a solid powder and 132.5°C after recrystallization.

[0032] In addition, the ultra-high molecular weight polyethylene described below (manufactured by Mitsui Chemicals, Inc., product name: Mipelon XM220, viscosity average molecular weight: 2 million, density: 0.938 g / cm 3 ) has a melting point of 140.3°C as a solid powder and 132.7°C after recrystallization.

[0033] The above-mentioned "recrystallization" refers to a phenomenon that occurs when the crystal structure changes during the temperature rise process when a polymer immediately after polymerization is melted, and once the crystal structure has been recrystallized, it does not return to the state it was in immediately after polymerization.

[0034] The above "melting point" refers to a value measured in accordance with JIS K 7121:1987, and is determined by measuring the temperature at which a main endothermic peak appears using a differential scanning calorimeter (DSC).

[0035] <Other ingredients> The stretched film of the present invention may contain various additives in addition to the ultra-high molecular weight polyethylene that is the main component. As the additives, known additives that are usually used in stretched films can be used, and examples thereof include calcium stearate (metal soap), higher aliphatic alcohols such as stearyl alcohol and ceryl alcohol, n-alkanes such as n-decane and n-dodecane, liquid paraffin, kerosene, paraffin wax, etc. These additives may be used alone or in combination of two or more.

[0036] <Stretched film> The blending ratio of ultra-high molecular weight polyethylene to additives in the stretched film 3 is not particularly limited as long as it does not impair the characteristics of the stretched film of the present invention, but from the viewpoint of suppressing a decrease in the mechanical strength (tensile strength) of the stretched film caused by the additives, the blending amount of ultra-high molecular weight polyethylene relative to the entire stretched film is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 98% by mass or more. It is also possible to provide a stretched film consisting only of ultra-high molecular weight polyethylene (i.e., 100% by mass) without containing processing aids, etc.

[0037] Furthermore, in the stretched film of the present invention, in a DSC measurement, there is at least one endothermic peak between 137° C. and less than 160° C. More specifically, as shown in the DSC chart of Fig. 2 (DSC chart of the stretched film in Example 1 described later), the stretched film of the present invention has two endothermic peaks, the endothermic peak near 137 to 145° C. is the melting peak of extended chain crystals (orthorhombic), and the endothermic peak near 150 to 160° C. is the transition peak of extended chain crystals (orthorhombic to hexagonal).

[0038] In addition, as shown in the DSC chart of FIG. 2 (DSC chart of the raw film in Comparative Example 1 described later), the solid-phase rolled film (raw film) before stretching has at least two endothermic peaks between 130 and 160°C, and the endothermic peak near 130 to 135°C is the melting peak of the lamellar crystals.

[0039] Since the heat of fusion of extended chain crystals is smaller than that of lamellar crystals, only the transition peak (endothermic peak near 150 to 155° C.) may be observed.

[0040] In the DSC chart shown in FIG. 2, the stretched film of the present invention has two endothermic peaks (i.e., at least one endothermic peak between 137°C or higher and less than 160°C): a melting peak of extended chain crystals at around 137 to 145°C and a transition peak of extended chain crystals at around 150 to 155°C (i.e., at least one endothermic peak between 137°C or higher and 160°C). This increases the crystallinity and density of the stretched film, and is believed to result in the development of water vapor barrier properties.

[0041] The above "DSC chart" refers to one measured in accordance with JIS K7121.

[0042] As described above, in the present invention, the ultra-high molecular weight polyethylene having a viscosity average molecular weight (Mv) of 500,000 to 3,000,000 is used, and the water vapor barrier property is expressed by the above-mentioned extended chain crystals, and the water vapor transmission rate per 50 μm of the stretched film is 2.15 g / m 2 This makes it possible to provide a stretched film with excellent water vapor barrier properties and recyclability.

[0043] From the viewpoint of improving the water vapor barrier property, the water vapor permeability per 50 μm of the stretched film is 2.00 g / m 2 ·day or less is preferable, 1.00g / m 2 ·day or less is preferable, 0.50g / m 2 ·days or less is even better.

[0044] The term "water vapor permeability" as used herein refers to a value measured using a water vapor permeability measuring device in accordance with JIS K 7129-1 at a temperature of 40° C. and a humidity of 90%.

[0045] In addition, the stretched film of the present invention preferably has a tensile breaking stress of 200 MPa or more in at least one of the mechanical axis (longitudinal) direction (hereinafter referred to as "MD") of the film or the direction perpendicular to the MD (hereinafter referred to as "TD") as shown in Figure 3. If the tensile breaking stress is 200 MPa or more, the orientation of the film is promoted and the water vapor barrier property is improved.

[0046] From the viewpoint of further promoting the orientation of the film, the tensile breaking stress of the stretched film is more preferably 300 MPa or more, and further preferably 400 MPa or more.

[0047] The above "tensile breaking stress" refers to a stress measured in accordance with JIS K 7127.

[0048] The thickness of the stretched film of the present invention is preferably 10 to 100 μm, more preferably 15 to 80 μm, and even more preferably 20 to 50 μm. If the thickness is 10 μm or less, the strength and water vapor barrier property of the stretched film may decrease, while if the thickness is more than 100 μm, the rigidity of the film may increase, resulting in decreased processability and increased costs.

[0049] <Method of manufacturing stretched film> Next, the method for producing a stretched film of the present invention will be described in detail.

[0050] The stretched film of the present invention is produced by first forming a raw material mainly composed of ultra-high molecular weight polyethylene having a viscosity average molecular weight of 500,000 to 3,000,000 as described above, either alone or in combination with the additives as described above, in the form of a solid powder using a roll mill to produce an ultra-high molecular weight polyethylene solid-phase rolled film, and then subjecting this raw film mainly composed of ultra-high molecular weight polyethylene having a viscosity average molecular weight (Mv) of 500,000 to 3,000,000 to a stretching treatment.

[0051] The method for producing an ultra-high molecular weight polyethylene solid-phase roll-milled film according to the present invention is a dry method for producing a film without using any processing aids or without a step for removing the processing aids later, as opposed to a wet method in which processing aids are used and subsequently removed.

[0052] FIG. 4 is a schematic diagram showing an apparatus (rolling machine) for producing the ultra-high molecular weight polyethylene film according to this embodiment.

[0053] 4, in a raw material supplying machine 11, a roll rolling machine 10 supplies solid powder of ultra-high molecular weight polyethylene M from an outlet 11a of the raw material supplying machine 11 between a pair of rolls 12, 13 constituting the roll rolling machine, and the raw material ultra-high molecular weight polyethylene M is compressed and passed between the pair of rolls 12, 13 to form a film by the rolls. Then, while forming a film, the film is transported in the direction of arrow Y via transfer rolls 4-7 and taken up in the direction of arrow Z by a take-up roll 8 to obtain an ultra-high molecular weight polyethylene solid-phase roll-rolled film P.

[0054] 1, the pair of rolls 12, 13 are provided in the supply direction of the ultra-high molecular weight polyethylene M (the direction of the arrow X in the figure) and are disposed opposite each other. The pair of rolls 12, 13 are also provided at a predetermined interval.

[0055] Moreover, the pair of rolls 12, 13, the transport rolls 4 to 7, and the take-up roll 8 can be made of metal or rubber.

[0056] Regarding the temperature for film formation by the roll rolling machine (the temperature of the rolls during film formation), heating near the melting point of the raw material ultra-high molecular weight polyethylene is a feature of film formation by solid-phase roll rolling, and is important for forming a film without leaving any raw material on the rolls. When the melting point of ultra-high molecular weight polyethylene (the melting point of solid powder immediately after polymerization of ultra-high molecular weight polyethylene) is Mp [°C], the lower limit of the film formation temperature must be a temperature of Mp-5°C or higher. In addition, the upper limit must be in the range of less than Mp+10°C. This is because forming at a temperature higher than Mp+10°C may cause holes to form in the film due to aggregation of the raw material, making film formation difficult. Also, forming at a temperature lower than Mp-5°C may cause the powder part of the raw material to remain, making film formation difficult.

[0057] In the present invention, the raw material ultra-high molecular weight polyethylene is passed between a pair of rolls 12, 13 that constitute a rolling mill to perform roll molding. From the viewpoint of compressing the solid powder into a film by solid-state roll rolling, the linear pressure between the two rolls 12, 13 that constitute the pair of rolls is preferably 4 kg / cm or more and 300 kg / cm or less, more preferably 4 kg / cm or less, and even more preferably 100 kg / cm or less.

[0058] In addition, the rolling speed is preferably set in the range of 0.1 to 3.0 m / min when the roll diameter is 3 inches. This is because if the rolling speed exceeds 3.0 m / min, the film may break, and if the rolling speed is less than 0.1 m / min, the production efficiency may decrease.

[0059] The thickness of the raw film before stretching is preferably 50 to 300 μm, more preferably 100 to 200 μm. If the thickness of the raw film is 50 μm or more, the handling properties such as wrinkles during winding and trimming cutability during slitting can be ensured. If the thickness of the raw film is 300 μm or less, sufficient water vapor barrier properties can be obtained in the stretched film after stretching.

[0060] In addition, the method for producing the raw film before the stretching treatment is not limited to the above-mentioned roll rolling, and for example, a skive method may be used in which billet-shaped ultra-high molecular weight polyethylene compressed by hot compression molding is sliced ​​and processed into a sheet or film.

[0061] Next, the taken-up ultra-high molecular weight polyethylene solid-phase rolled film is uniaxially stretched in MD or TD to produce the stretched film of the present invention shown in Figs.

[0062] More specifically, for example, by stretching a raw film of high molecular weight polyethylene solid-phase rolled film in the MD, molecular orientation in the MD progresses and lamellar crystals change into extended chain crystals.

[0063] The stretching temperature and stretch ratio in the MD stretching treatment can be appropriately changed depending on the ultra-high molecular weight polyethylene used.

[0064] More specifically, the ultra-high molecular weight polyethylene described below (manufactured by Mitsui Chemicals, Inc., product name: Hi-Zex Million 030S, viscosity average molecular weight: 500,000, density: 0.949 g / cm 3 In the above-mentioned method, the stretching temperature is preferably 120 to 130° C., and more preferably 120° C. The stretching ratio is preferably 2.0 to 3.0 times, and more preferably 3.0 times.

[0065] In addition, the ultra-high molecular weight polyethylene described below (manufactured by Mitsui Chemicals, Inc., product name: Hi-Zex Million 145M, viscosity average molecular weight: 1.15 million, density: 0.940 g / cm 3), the stretching temperature is preferably 120 to 135° C., more preferably 120° C. The stretching ratio is preferably 1.5 to 2.0 times, more preferably 1.7 to 2.0 times, and even more preferably 2.0 times.

[0066] In addition, the ultra-high molecular weight polyethylene described below (manufactured by Mitsui Chemicals, Inc., product name: Mipelon XM220, viscosity average molecular weight: 2 million, density: 0.938 g / cm 3 In the above-mentioned method, the stretching temperature is preferably 120 to 150° C., and more preferably 130 to 150° C. The stretching ratio is preferably 1.5 to 2.0 times.

[0067] In addition, the ultra-high molecular weight polyethylene film described below (manufactured by Sakushin Kogyo Co., Ltd., product name: New Light Film #25W, viscosity average molecular weight: 500,000 to 3,000,000, density: 0.940 g / cm 3 In the above-mentioned method, the stretching temperature is preferably 120 to 130° C., and more preferably 120° C. The stretching ratio is preferably 4.0 to 4.5 times, and more preferably 4.5 times.

[0068] This is because, when the film is molded at a temperature higher than the upper limit of each of the above-mentioned stretching temperatures, the molecular chains of the ultra-high molecular weight polyethylene that had maintained the shape of the film become entangled and break, causing the film to lose its water vapor barrier properties or to melt. Also, when the film is molded at a temperature lower than the lower limit of each of the above-mentioned stretching temperatures, the film may break due to insufficient stretching.

[0069] If the stretching ratio is less than the lower limit of each of the above-mentioned stretching ratios, the density and molecular orientation of the stretched film will be insufficient, making it difficult to exhibit water vapor barrier properties, and if the stretching ratio is greater than the upper limit of each of the above-mentioned stretching ratios, the film may break.

[0070] The term "stretching ratio" used herein refers to the multiple of the length of the film after stretching relative to the length of the film before stretching in the stretching direction (i.e., MD).

[0071] The stretched film of the present invention produced by the above-mentioned method exhibits water vapor barrier properties due to the above-mentioned extended chain crystals, and the water vapor transmission rate per 50 μm of the stretched film is 2.15 g / m 2 ·day or less, it is possible to obtain excellent water vapor barrier properties.

[0072] The stretched film serving as the base film may be a single layer or may be a multilayer film having two or more layers. When the stretched film is a multilayer film, the composition and thickness of each layer may be the same or different. When the stretched film is a multilayer film, the thickness refers to the total thickness of the multilayer film.

[0073] Next, a raw material containing a polyethylene resin such as the above-mentioned high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE), and linear low density polyethylene (LLDPE) is prepared, and the raw material is formed into a film by melt extrusion using an extruder equipped with a T-die, thereby producing a sealant film.

[0074] Then, for example, the stretched film and the sealant film are laminated together via an adhesive to produce the laminate 1 shown in FIG. EXAMPLES

[0075] The present invention will be described below based on examples. Note that the present invention is not limited to these examples, and these examples can be modified or changed based on the spirit of the present invention, and they are not excluded from the scope of the present invention.

[0076] Example 1 <Preparation of Stretched Film> Ultra-high molecular weight polyethylene (Mitsui Chemicals, Inc., product name: Hi-Zex Million 030S, viscosity average molecular weight: 500,000, melting point after recrystallization: 132.8°C, density: 0.949g / cm 3Using as a raw material, under the manufacturing conditions shown in Table 1, a polyethylene film (the original film before stretching) having the thickness shown in Table 1 was produced by forming it into a film shape using a rolling mill (roll diameter: 75 mm).

[0077] Next, with respect to this original film, under the conditions of stretching temperature and stretching ratio shown in Table 1, a stretching treatment was performed in the MD direction to produce a stretched film having the thickness shown in Table 1.

[0078] <Calculation of water vapor permeability per 50 μm> Next, the water vapor permeability [g / m 2 ·day] of the produced stretched film was measured using a water vapor permeability measuring machine (manufactured by SYSTEC Illinois, product name: Water Vapor Permeability Meter Lyssy L80 - 6000) in accordance with JIS K 7129 - 1 under an atmosphere of temperature 40°C and humidity 90%. Then, the measured water vapor permeability was multiplied by the thickness [μm] of the stretched film / 50 [μm] to calculate the water vapor permeability per 50 μm [g / m 2 ·day]. The above results are shown in Table 1.

[0079] In Example 1, since the measured water vapor permeability was 2.17 [g / m 2 ·day] and the thickness of the stretched film was 40.2 μm, the water vapor permeability per 50 μm was 2.17×(40.2 / 50) = 1.74 [g / m 2 ·day].

[0080] <Measurement of tensile breaking stress> In accordance with JIS K 7127, the tensile breaking stress [MPa] of the produced stretched film was measured. More specifically, a test film of test piece type No. 3 dumbbell was prepared, and a tensile test was performed using a tensile testing machine (manufactured by Shimadzu Corporation, product name: Autograph AG - 5000A) under the conditions of temperature 25°C and tensile speed 100 mm / min, and the tensile breaking stress [MPa] in the MD direction was measured. The above results are shown in Table 1.

[0081] <DSC measurement> In addition, the stretched film was subjected to DSC measurement. More specifically, in accordance with the JIS K 7121 test method, about 1 mg of sample was taken and sealed in a differential scanning calorimeter (manufactured by Hitachi High-Tech Science Corporation, product name: DSC7000X), and a DSC chart was obtained under the conditions of a carrier gas of nitrogen flowing at 30 cc / min and a heating rate of 10°C / min. In addition, under the same conditions, a DSC chart was obtained for the solid-phase rolled film (raw film) before stretching. The above results are shown in Figure 2.

[0082] As shown in FIG. 2, the DSC curve of the produced stretched film has two endothermic peaks at 137°C or higher but lower than 155°C (141°C or higher but lower than 152°C) (i.e., the melting peak of extended chain crystals around 137-145°C and the transition peak of extended chain crystals around 150-155°C). As a result, it is believed that the water vapor barrier property of the stretched film is expressed.

[0083] (Examples 2 to 3) Ultra-high molecular weight polyethylene (Mitsui Chemicals, Inc., product name: Hi-Zex Million 145M, viscosity average molecular weight: 1.15 million, melting point after recrystallization: 132.5°C, density: 0.940 g / cm 3 ) was used as a raw material and molded into a film shape using a rolling machine (roll diameter: 75 mm) under the manufacturing conditions shown in Table 1 to produce a polyethylene film as a raw film having the thickness shown in Table 1. This raw film was then stretched in MD under the stretching temperature and stretch ratio conditions shown in Table 1 to produce a stretched film having the thickness shown in Table 1.

[0084] Thereafter, the water vapor transmission rate per 50 μm was calculated, the tensile breaking stress was measured, and the DSC measurement was performed in the same manner as in Example 1. The results are shown in Table 1.

[0085] (Examples 4 to 9) Ultra-high molecular weight polyethylene (Mitsui Chemicals, Inc., product name: Mipelon XM220, viscosity average molecular weight: 2 million, melting point after recrystallization: 132.7°C, density: 0.938g / cm 3) was used as a raw material and molded into a film shape using a rolling machine (roll diameter: 75 mm) under the manufacturing conditions shown in Table 1 to produce a polyethylene film as a raw film having the thickness shown in Table 1. This raw film was then stretched in MD under the stretching temperature and stretch ratio conditions shown in Table 1 to produce a stretched film having the thickness shown in Table 1.

[0086] Thereafter, the water vapor transmission rate per 50 μm was calculated, the tensile breaking stress was measured, and the DSC measurement was performed in the same manner as in Example 1. The results are shown in Table 1.

[0087] (Examples 10 to 11) The raw film was an ultra-high molecular weight polyethylene film produced by the skive method (manufactured by Sakushin Kogyo Co., Ltd., product name: New Light Film #25W, viscosity average molecular weight: 500,000 to 3,000,000, melting point after recrystallization: 136°C, density: 0.940 g / cm 3 ) was used, and this raw film was stretched in the MD under the conditions of the stretching temperature and stretch ratio shown in Table 1 to produce a stretched film having the thickness shown in Table 1.

[0088] Thereafter, the water vapor transmission rate per 50 μm was calculated, the tensile breaking stress was measured, and the DSC measurement was performed in the same manner as in Example 1. The results are shown in Table 1.

[0089] Comparative Example 1 A polyethylene film (raw film before stretching) was prepared in the same manner as in Example 1, and the water vapor transmission rate per 50 μm of this raw film was calculated, the tensile breaking stress was measured, and a DSC measurement was performed. The results are shown in Table 2. Note that this raw film was not stretched in the MD, and a stretched film was not prepared.

[0090] Comparative Example 2 A polyethylene film (raw film before stretching) was prepared in the same manner as in Example 2, and the water vapor transmission rate per 50 μm of this raw film was calculated, the tensile breaking stress was measured, and a DSC measurement was performed. The results are shown in Table 2. Note that this raw film was not stretched in the MD, and a stretched film was not prepared.

[0091] Comparative Example 3 A polyethylene film (raw film before stretching) was prepared in the same manner as in Example 4, and the water vapor transmission rate per 50 μm of this raw film was calculated, the tensile breaking stress was measured, and a DSC measurement was performed. The results are shown in Table 2. Note that this raw film was not stretched in the MD, and a stretched film was not prepared.

[0092] Comparative Example 4 In the same manner as in Example 2, a polyethylene film (raw film before stretching) was prepared, and an attempt was made to produce a stretched film by subjecting this raw film to a stretching process in MD under the conditions of the stretching temperature and stretch ratio shown in Table 2; however, the film melted because the stretching temperature was higher than 135°C.

[0093] Comparative Example 5 In the same manner as in Example 4, a polyethylene film (raw film before stretching) was prepared, and an attempt was made to produce a stretched film by stretching this raw film in the MD under the conditions of the stretching temperature and stretch ratio shown in Table 2. However, since the stretch ratio was greater than 2 times, the film broke during the MD stretching process.

[0094] Comparative Example 6 In the same manner as in Example 4, a polyethylene film (raw film before stretching) was prepared, and an attempt was made to produce a stretched film by subjecting this raw film to a stretching process in MD under the conditions of the stretching temperature and stretch ratio shown in Table 2; however, the film melted because the stretching temperature was higher than 150°C.

[0095] (Comparative Examples 7 to 8) As in Example 10, an ultra-high molecular weight polyethylene film produced by the skive method was used as the raw film, and an attempt was made to produce a stretched film by stretching this raw film in MD under the conditions of the stretching temperature and stretching ratio shown in Table 2. However, in Comparative Example 7, the stretching ratio was greater than 4.5 times, so the film broke during the MD stretching treatment. In Comparative Example 8, the stretching temperature was higher than 130°C, so the film melted.

[0096] Comparative Example 9 High density polyethylene (Prime Polymer Co., Ltd., product name: Hi-Zex 3600F, number average molecular weight: 100,000, melting point after recrystallization: 133°C, density: 0.958g / cm 3 ) was used as the raw material, and this high-density polyethylene was formed into a film by melt extrusion (extrusion temperature: 230°C) in an extruder (manufactured by Prime Polymer) equipped with a T-die. The film was then taken up on a take-up roll to produce a polyethylene film (raw film before stretching) having the thickness shown in Table 3.

[0097] Next, this raw film was stretched in the MD under the conditions of the stretching temperature and stretch ratio shown in Table 3, to produce a stretched film having a thickness shown in Table 3.

[0098] Thereafter, the water vapor transmission rate per 50 μm was calculated, the tensile breaking stress was measured, and the DSC measurement was performed in the same manner as in Example 1. The results are shown in Table 3.

[0099] [Table 1]

[0100] [Table 2]

[0101] [Table 3]

[0102] As shown in Table 1, the stretched films of Examples 1 to 11 have at least one endothermic peak between 137°C and 160°C in the DSC chart, and the water vapor permeability per 50 μm of the stretched film is 2.15 g / m 2 This indicates that the film has excellent water vapor barrier properties.

[0103] The DSC chart of the stretched film in Example 8 is shown in Figure 5. As shown in Figure 5, the endothermic peak temperatures in the DSC chart are 142.8°C and 152.3°C, and there is at least one endothermic peak between 137°C and less than 160°C. In other words, due to the presence of extended chain crystals, the water vapor transmission rate per 50 μm of the stretched film is 2.15 g / m 2 This shows that the film has excellent water vapor barrier properties.

[0104] On the other hand, as shown in Table 2, in Comparative Examples 1 to 3, the raw film was not stretched in the MD, so the water vapor permeability per 50 μm of the raw film was 2.15 g / m 2 This shows that the water vapor barrier properties are poor.

[0105] In addition, as shown in Table 3, in Comparative Example 9, ultra-high molecular weight polyethylene was not used, and high-density polyethylene with a small average molecular weight was used, so that the water vapor permeability per 50 μm of the stretched film was 2.15 g / m 2 ·day, which indicates that the water vapor barrier property is poor. The DSC chart of the stretched film in Comparative Example 9 is shown in FIG. 6. As shown in FIG. 6, the endothermic peak temperature in the DSC chart is 134.9°C, and there is no endothermic peak between 137°C and less than 155°C. In other words, since there are no extended chain crystals, the water vapor transmission rate per 50 μm of the stretched film is 2.15 g / m 2 This shows that the water vapor barrier properties are poor. [Industrial Applicability]

[0106] As described above, the present invention is suitable for a stretched film obtained by stretching a raw film containing ultra-high molecular weight polyethylene as a main component. [Explanation of symbols]

[0107] 1. Laminate 2. Sealant film 3. Stretched Film 4~7 Transfer roll 8. Take-off roll 10 Roll Mill 11 Raw material feeder 12~13 Pair of rolls M Ultra-high molecular weight polyethylene P Ultra-high molecular weight polyethylene solid-phase rolled film

Claims

1. A stretched film mainly composed of ultra-high molecular weight polyethylene having a viscosity average molecular weight (Mv) of 500,000 to 3,000,000, Water vapor permeability per 50 μm is 2.15 g / m 2 ・Day or less A stretched film characterized by:

2. The viscosity average molecular weight (Mv) is 1,000,000 to 2,500,000; The water vapor transmission rate per 50 μm is 1.00 g / m 2 ・Day or less 2. The stretched film according to claim 1 .

3. The viscosity average molecular weight (Mv) is 1.5 million to 2 million, The water vapor transmission rate per 50 μm is 0.50 g / m 2 ・Day or less 2. The stretched film according to claim 1 .

Citation Information

Patent Citations

  • Ultrahigh molecular-weight biaxially oriented polyethylene film and its manufacture

    JP1990030514A

  • Shape retaining barrier film, method for producing the same, packaging laminate and packaging material, and metod for producing the same

    JP2013091729A

  • Resin film

    JP2021046510A

  • Packaging material

    JP2021191688A

  • A barrier film and process of preparation thereof

    WO2018109747A1