Hole transport material, hole transport layer, and power generation device
A hole transport material with tailored conductivity and ionization potential, using carbazole and spirotriarylamine compounds, enhances power generation efficiency in low-light conditions by optimizing charge transport and reducing energy loss in power generation devices.
Patent Information
- Application Number
- JP2023057106
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Power generation devices with conventional hole transport layers experience decreased efficiency in low-light environments such as indoors, particularly when used with light sources like fluorescent lamps and LEDs.
A hole transport material is developed with specific conductivity and ionization potential ranges, composed of multiple compounds including those with carbazole and spirotriarylamine structures, combined with an organic-inorganic hybrid semiconductor compound to enhance power generation efficiency under low-light conditions.
The proposed hole transport material improves power generation efficiency in low-light environments by efficiently transporting charges and reducing energy loss, achieving high efficiency even under low illuminance.
Smart Images

Figure 2024144926000015 
Figure 2024144926000016 
Figure 2024144926000017
Abstract
Description
[Technical field]
[0001] The present invention relates to a hole transport material, a hole transport layer, and a power generation device. [Background technology]
[0002] There are power generation devices (photoelectric conversion elements) in which an active layer and a buffer layer are arranged between a pair of electrodes. Organic-inorganic hybrid semiconductor compounds have been developed as materials for this active layer, and among them, compounds with a perovskite structure (perovskite semiconductor compounds) are useful. Meanwhile, as a material for the hole transport layer, which is one of the buffer layers, a phthalocyanine-based organic semiconductor compound and the like have been proposed (Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-066096 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, when power generation devices equipped with conventional hole transport layers are applied to light sources such as fluorescent lamps and LEDs, which are particularly important for energy harvesting applications, the power generation efficiency can sometimes decrease in low-illumination environments, such as indoors.
[0005] An object of the present invention is to improve the power generation efficiency under light irradiation, particularly in a low-illuminance environment, in a power generation device having an active layer containing an organic-inorganic hybrid semiconductor compound. [Means for solving the problem]
[0006] The present inventors have discovered that by combining an active layer containing an organic-inorganic hybrid semiconductor compound with a hole transport layer formed using a specific hole transport material, a power generation device having excellent power generation efficiency even under light irradiation, particularly in a low-illumination environment such as indoors, can be obtained, and have completed the present invention.
[0007] The present invention has the following aspects. [1] A hole transport material, the electrical conductivity of a spin-coated film of the hole transport material being 5×10 -6 S / cm or more 5×10 -4 and the ionization potential of a spin-coated film of the hole transport material is -5.80 eV or more and less than -5.30 eV. [2] The hole transport material according to [1], which contains at least two or more compounds. [3] The hole transport material according to [1] or [2], comprising at least two or more compounds, wherein a first compound has an ionization potential of −5.60 to −5.40 eV and a second compound has an ionization potential of −5.25 to −5.05 eV. [4] The hole transport material according to any one of [1] to [3], comprising at least two or more compounds, wherein a first compound is a compound having a carbazole skeleton and a second compound is a spirotriarylamine compound having a fluorene skeleton. [5] A hole transport material comprising at least two or more compounds, the first compound being a compound having a carbazole skeleton represented by the following formula (I) and the second compound being a spirotriarylamine compound having a fluorene skeleton represented by the following formula (II):
[0008] [ka]
[0009] In formula (I), Ar 1 and Ar 2R are each independently an aromatic group which may have a monovalent substituent, and the aromatic group may have a condensed ring structure. The monovalent substituent is an arbitrary substituent which replaces an arbitrary hydrogen atom of the aromatic group, and may be an alkyl group, an aromatic group, an alkoxy group, or a thioalkyl group. 1 , R 2 , R 3 , R 4 , R 5 , R 6 are each independently a hydrogen atom, a halogen atom, or an alkyl group, an alkenyl group, an alkynyl group, an alkoxy group, an aryloxy group or an aromatic group which may have a substituent.
[0010] In formula (II), Ar 3 are each independently an aromatic group which may have a monovalent substituent, and the aromatic group may have a condensed ring structure. The monovalent substituent is any substituent which replaces any hydrogen atom of the aromatic group, and may be an alkyl group, an aromatic group, an alkoxy group, or a thioalkyl group.
[0011] [6] The hole transport material according to any one of [2] to [5], further comprising a third compound, the third compound being a compound capable of imparting charge by a chemical reaction or by donating and receiving electrons. [7] The hole transport material according to [6], wherein the ratio of the third compound is 0.001 to 70 parts by mass with respect to 100 parts by mass of the total of the first compound and the second compound. [8] The hole transport material according to any one of [2] to [7], further comprising a third compound, the third compound being a diaryliodonium salt represented by the following formula (Q1):
[0012] [ka]
[0013] In formula (Q1), Ar 4 , Ar 5 , Ar 6each independently represents an aromatic hydrocarbon group having 6 to 20 carbon atoms or a heteroaromatic hydrocarbon group having 2 to 20 carbon atoms, which may have a substituent.
[0014] [9] The hole transport material according to any one of [2] to [8], further comprising a third compound, the third compound comprising at least one selected from the group consisting of a compound represented by the following formula (Q2) and a compound represented by the following formula (Q3):
[0015] [ka]
[0016] In formula (Q3), R 7 , R 8 , R 9 , R 10 are each independently a hydrogen atom, a halogen atom, or an alkyl group, an alkenyl group, an alkynyl group, an alkoxy group, an aryloxy group or an aromatic group which may have a substituent; and n is an integer of 0 to 5.
[0017]
[10] The hole transport material according to any one of [1] to [9], further comprising a solvent.
[11] A hole transport layer comprising the hole transport material according to any one of [1] to
[10] .
[12] A power generation device, comprising: a pair of electrodes composed of an upper electrode and a lower electrode; an active layer located between the pair of electrodes and containing an organic-inorganic hybrid semiconductor compound; and a hole transport layer located between the pair of electrodes, wherein the hole transport layer contains the hole transport material according to any one of [1] to
[10] . Effect of the Invention
[0018] According to the present invention, in a power generating device having an active layer containing an organic-inorganic hybrid semiconductor compound, the power generating efficiency under light irradiation, particularly under a low illuminance environment, is improved. [Brief description of the drawings]
[0019] [Figure 1] FIG. 1 is a cross-sectional view illustrating an example of a power generation device. [Diagram 2] FIG. 1 is a cross-sectional view that illustrates a schematic example of a solar cell equipped with a power generation device. [Diagram 3] FIG. 1 is a cross-sectional view illustrating a schematic example of a solar cell module including a power generation device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The meanings of the terms are as follows: In this specification, the compound represented by formula (I) is referred to as compound (I). Compounds represented by other formulas are also referred to in the same manner. The symbol "~" indicating a range of numerical values means that the numerical values before and after it are included as the lower limit and upper limit.
[0021] A semiconductor compound is a compound that can be used as a semiconductor material that exhibits semiconductor properties. Semiconductor properties are defined by the magnitude of carrier mobility in the solid state. Carrier mobility is an index of how fast (or how much) charges (electrons or holes) can be moved. The carrier mobility of a semiconductor at room temperature (25°C) is preferably 1.0 x 10 -6 cm 2 / V s or more, preferably 1.0×10 -5 cm 2 / V s or more, and more preferably 5.0×10 -5 cm 2 / V s or more, and preferably 1.0×10 -4 cm 2 / V s or more. The carrier mobility can be measured by measuring the IV characteristics of a field effect transistor, a time-of-flight method, or the like.
[0022] Hereinafter, some embodiments will be described in detail. The following description relates to an example of an embodiment, and the present invention is not limited to the following disclosure unless the gist of the present invention is lost.
[0023] [Hole transport material] The hole transport material according to one embodiment satisfies the following two requirements. The conductivity of the spin-coated film of the hole transport material is 5×10 -6 S / cm or more 5×10 -4 S / cm or less. The ionization potential of the spin-coated film of the hole transport material is -5.80 eV or more and less than -5.30 eV.
[0024] The conductivity of the spin-coated film of the hole transport material is 7×10 -6 ~5×10 -4 S / cm is more preferable, 1×10 -5 ~5×10 -4 S / cm is more preferred. When the electrical conductivity is equal to or higher than the lower limit of the above-mentioned range, positive charges provided to the hole transport layer upon light irradiation can be efficiently transported to the electrode.When the electrical conductivity is equal to or lower than the upper limit of the above-mentioned range, leakage current is unlikely to occur under extremely low illuminance irradiation conditions.
[0025] The electrical conductivity of the spin-coated film of the hole transport material is a value calculated by IV measurement of the thin film using a source meter. More specifically, the electrical conductivity is determined by the method described in the Examples.
[0026] The ionization potential of the spin-coated film of the hole transport material is preferably −5.80 to −5.35 eV, more preferably −5.80 to −5.40 eV. When the ionization potential is equal to or greater than the lower limit of the above-mentioned range, the ionization potential of the corresponding active layer is sufficient to absorb the long wavelength region of the visible light source that provides a white light source indoors, and the power generation efficiency is likely to be high. Under the condition that a low value is preferable, it is preferably -5.7 eV or less, which provides good matching in terms of receiving and transferring charges obtained in the active layer. When the ionization potential is equal to or less than the upper limit of the above-mentioned range, the energy loss of the active layer is likely to be reduced.
[0027] The ionization potential of the spin-coated film of the hole transport material is calculated from the minimum energy (eV) required for the irradiation energy to eject photoelectrons when the thin film is irradiated with light. More specifically, the ionization potential is determined by the method described in the Examples.
[0028] The hole transport material according to one embodiment preferably contains at least two or more compounds for controlling the electrical conductivity and ionization potential. By using at least two or more compounds, a hole transport material having electrical conductivity and ionization potential that satisfy the desired numerical ranges is easily obtained. In this case, the ionization potential of the first compound is preferably -5.60 to -5.40 eV, more preferably -5.60 to -5.45 eV, and even more preferably -5.60 to -5.50 eV. The ionization potential of the second compound is preferably −5.25 to −5.05 eV, more preferably −5.25 to −5.10 eV, and further preferably −5.25 to −5.15 eV.
[0029] The hole transport material according to one embodiment preferably contains at least two or more compounds for controlling the electrical conductivity and the ionization potential, and in this case, it is preferable that the first compound is a compound having a carbazole skeleton, and the second compound is a spirotriarylamine compound having a fluorene skeleton. Representative examples of compounds that can be components of the hole transport material will be described below, but the compounds that can be components of the hole transport material are not limited to the following descriptions.
[0030] (Compounds having a carbazole skeleton) The compound having a carbazole skeleton in the hole transport material is not particularly limited as long as it is an organic semiconductor compound having a carbazole skeleton. In the compound having a carbazole skeleton, the number of carbazole structures is preferably one or more, more preferably two or more, from the viewpoints of hole transport ability and robustness.
[0031] The hole transport material according to one embodiment may include the following compound (I) as a compound having a carbazole skeleton. Compound (I) has two carbazole structures, and the two carbazole structures are positioned point symmetrically, so that it is suitable from the viewpoints of hole transport ability, robustness, and ease of synthesis. Compound (I) is also preferred in that it has no molecular weight distribution, is easily purified, and is inexpensively produced, as compared with polymeric compounds such as polytriarylamines.
[0032] [ka]
[0033] In formula (I), Ar 1 and Ar 2 are each independently an aromatic group which may have a monovalent substituent, and the aromatic group may have a condensed ring structure. The monovalent substituent is any substituent which replaces any hydrogen atom of the aromatic group, and may be an alkyl group, an aromatic group, an alkoxy group, or a thioalkyl group.
[0034] Ar 1 and Ar 2 The aromatic group constituting the formula (I) may have either a monocyclic structure or a polycyclic structure, or may have a condensed ring structure, or may have a structure in which these are linked by any divalent linking group or single bond (direct bond). The aromatic group may be an aromatic hydrocarbon group or an aromatic heterocyclic group.
[0035] Examples of the aromatic hydrocarbon group include polycyclic aromatic hydrocarbon groups in which a benzene ring is bonded via a carbon-carbon single bond, such as a phenyl group, a biphenyl group, and a terphenyl group; groups derived from a single 6-membered ring or 2 to 5 condensed rings, such as a naphthalene ring, an anthracene ring, a phenanthrene ring, a perylene ring, a tetracene ring, a pyrene ring, a benzpyrene ring, a chrysene ring, a triphenylene ring, an acenaphthene ring, a fluoranthene ring, or a fluorene ring; etc.
[0036] Examples of the aromatic heterocyclic group include a 5- or 6-membered monocyclic or 2- to 4-condensed ring-derived group, such as a furan ring, a benzofuran ring, a thiophene ring, a benzothiophene ring, a pyrrole ring, a pyrazole ring, an imidazole ring, an oxadiazole ring, an indole ring, a carbazole ring, a pyrroloimidazole ring, a pyrrolopyrazole ring, a pyrrolopyrrole ring, a thienopyrrole ring, a thienothiophene ring, a furopyrrole ring, a furofuran ring, a thienofuran ring, a benzisoxazole ring, a benzisothiazole ring, a benzimidazole ring, a pyridine ring, a pyrazine ring, a pyridazine ring, a pyrimidine ring, a triazine ring, a quinoline ring, an isoquinoline ring, a cinnoline ring, a quinoxaline ring, a phenanthridine ring, a benzimidazole ring, a perimidine ring, a quinazoline ring, a quinazolinone ring, or an azulene ring.
[0037] Ar 1 , Ar 2 From the viewpoints of high film-forming properties of the hole transport layer and ease of setting the ionization potential of the hole transport material within a predetermined range, each of the carbon atoms is preferably 30 or less, more preferably 20 or less, and even more preferably 10 or less.
[0038] Preferred Ar 1 , Ar 2 Each of the Ar groups independently includes, for example, a phenyl group, a biphenyl group, a terphenyl group, and a tetraphenyl group. 1 and Ar 2 A phenyl group is most preferable for both. It is preferable that the hydrogen atoms of the phenyl group are not substituted with a substituent.
[0039] Ar 1 , Ar 2 are different substituents that substitute the phenyl group. 1 , Ar 2 may be independently located at any of the ortho, meta, and para positions relative to the nitrogen atom of each carbazole structure. In consideration of the conformational stability of the compound and ease of synthesis, the meta and para positions are preferred, and the meta position is more preferred.
[0040] Ar 1 , Ar 2 The formula weight of Ar is preferably higher in terms of robustness and heat resistance, while it is preferably lower in terms of solubility in a solvent. 1 , Ar 2 The formula weight of the formula (I) is preferably 72 or more, and more preferably 144 or more, including the substituent if any, and is preferably 1000 or less, and more preferably 600 or less.
[0041] Examples of the monovalent substituent that the aromatic group may have include an alkyl group (preferably a chain having 1 to 12 carbon atoms, more preferably 1 to 6 carbon atoms), an aromatic group (a monovalent aromatic hydrocarbon group, an aromatic heterocyclic group), an alkoxy group (preferably having 1 to 12 carbon atoms), a thioalkyl group, a halogen atom, a hydroxyl group, a cyano group, an amino group (preferably a dialkylamino group having 2 to 12 carbon atoms, an alkylarylamino group having 7 to 20 carbon atoms, or a diarylamino group having 12 to 30 carbon atoms), a carboxyl group, an ester group, an alkylcarbonyl group, an acetyl group, a sulfonyl group, a silyl group, a boryl group, a nitrile group, an alkenyl group, an alkynyl group, a thio group, a seleno group, etc. Among these, an alkyl group, an aromatic group, an alkoxy group, and a thioalkyl group are preferred.
[0042] The substituent may be one or more kinds selected from the following substituent group Z. Substituent group Z: an alkyl group preferably having 1 to 24 carbon atoms, more preferably having 1 to 12 carbon atoms, such as a methyl group or an ethyl group; an alkenyl group preferably having 2 to 24 carbon atoms, more preferably having 2 to 12 carbon atoms, such as a vinyl group; an alkynyl group preferably having 2 to 24 carbon atoms, more preferably having 2 to 12 carbon atoms, such as an ethynyl group; an alkoxy group preferably having 1 to 24 carbon atoms, more preferably 1 to 12 carbon atoms, such as a methoxy group or an ethoxy group; an aryloxy group preferably having 4 to 36 carbon atoms, more preferably 5 to 24 carbon atoms, such as a phenoxy group, a naphthoxy group, or a pyridyloxy group; alkoxycarbonyl groups preferably having 2 to 24 carbon atoms, more preferably having 2 to 12 carbon atoms, such as a methoxycarbonyl group or an ethoxycarbonyl group; dialkylamino groups preferably having 2 to 24 carbon atoms, more preferably having 2 to 12 carbon atoms, such as a dimethylamino group or a diethylamino group; diarylamino groups preferably having 10 to 36 carbon atoms, more preferably 12 to 24 carbon atoms, such as a diphenylamino group, a ditolylamino group, or an N-carbazolyl group; an arylalkylamino group preferably having 6 to 36 carbon atoms, more preferably 7 to 24 carbon atoms, such as a phenylmethylamino group; an acyl group, such as an acetyl group or a benzoyl group, preferably having 2 to 24 carbon atoms, and preferably having 2 to 12 carbon atoms; Halogen atoms such as fluorine atoms and chlorine atoms; a haloalkyl group preferably having 1 to 2 carbon atoms, more preferably 1 to 6 carbon atoms, such as a trifluoromethyl group; an alkylthio group preferably having 1 to 24 carbon atoms, more preferably having 1 to 12 carbon atoms, such as a methylthio group or an ethylthio group; an arylthio group preferably having 4 to 36 carbon atoms, more preferably 5 to 24 carbon atoms, such as a phenylthio group, a naphthylthio group, or a pyridylthio group; silyl groups preferably having 2 to 36 carbon atoms, more preferably 3 to 24 carbon atoms, such as a trimethylsilyl group or a triphenylsilyl group; siloxy groups preferably having 2 to 36 carbon atoms, and more preferably having 3 to 24 carbon atoms, such as a trimethylsiloxy group or a triphenylsiloxy group; Cyano group; an aromatic hydrocarbon group preferably having 6 to 36 carbon atoms, more preferably 6 to 24 carbon atoms, such as a phenyl group or a naphthyl group; an aromatic heterocyclic group preferably having 3 to 36 carbon atoms, more preferably 4 to 24 carbon atoms, such as a thienyl group or a pyridyl group;
[0043] Each of the substituents in the substituent group Z may further have a substituent, and examples thereof include the same groups as those exemplified in the above-mentioned substituent group Z. From the viewpoint of the solubility and film-forming properties of compound (I), the formula weight of each substituent is preferably 500 or less, and more preferably 250 or less, including the case where the substituent is further substituted with another substituent.
[0044] In formula (I), R 1 , R 2 , R 3 , R 4 , R 5 , R 6 are each independently a hydrogen atom, a halogen atom, or an alkyl group, an alkenyl group, an alkynyl group, an alkoxy group, an aryloxy group, or an aromatic group which may have a substituent. The aromatic group may be a monovalent aromatic hydrocarbon group or an aromatic heterocyclic group. The substituent may be the same as the substituent group Z, and the details thereof are the same as those of the substituent group Z described above.
[0045] R 1 , R 2 , R 3 , R 4 , R 5 , R 6 are each independently preferably one or more selected from the group consisting of a hydrogen atom, a halogen atom, an alkyl group having 1 to 3 carbon atoms, and an alkoxy group having 1 to 3 carbon atoms, and more preferably a hydrogen atom.
[0046] The molecular weight of compound (I) is preferably higher in terms of robustness and heat resistance, while it is preferably lower in terms of solubility in a solvent. The molecular weight of compound (I) is preferably 200 or more, more preferably 400 or more, and is preferably 3000 or less, more preferably 2000 or less.
[0047] Compound (I) can be synthesized by a known method as described in the Examples below. The fact that compound (I) is contained in the hole transport material means that 1 H-NMR, 13 This can be confirmed by analytical methods such as C-NMR, X-ray crystal structure analysis using single crystals, and LC-MS.
[0048] (Spirotriarylamine compounds having a fluorene skeleton) The hole transport material according to one embodiment may contain the following compound (II) as a spirotriarylamine compound having a fluorene skeleton.
[0049] [ka]
[0050] In formula (II), Ar 3 are each independently an aromatic group which may have a monovalent substituent, and the aromatic group may have a condensed ring structure. The monovalent substituent is any substituent which replaces any hydrogen atom of the aromatic group, and may be an alkyl group, an aromatic group, an alkoxy group, or a thioalkyl group.
[0051] Ar 3 As the aromatic group and condensed ring structure, Ar 1 , Ar 2 The same as those in Ar 1 , Ar 2 This is the same as that explained above.
[0052] Ar 3 From the viewpoints of providing a high film-formable hole transport layer and making it easy to set the ionization potential in a suitable range described below, each of the carbon atoms is preferably 30 or less, and more preferably 20 or less.
[0053] Ar 3 The formula weight of Ar is preferably higher in terms of robustness and heat resistance, while it is preferably lower in terms of solubility in a solvent. 3 The formula weight of the formula (I) is preferably 72 or more, and more preferably 144 or more, including the substituent if any, and is preferably 1000 or less, and more preferably 600 or less.
[0054] Ar 3 The details of the monovalent substituent that the aromatic group may have are 1 , Ar2 and the substituent group Z are the same as those explained above.
[0055] Preferred Ar 3 are each independently exemplified by a phenyl group, a biphenyl group, a terphenyl group, a tetraphenyl group, etc. 3 are most preferably all phenyl groups. The hydrogen atoms of the phenyl groups may or may not be substituted with a substituent.
[0056] The molecular weight of compound (II) is preferably higher in terms of robustness and heat resistance, while it is preferably lower in terms of solubility in a solvent. The molecular weight of compound (II) is preferably 200 or more, more preferably 400 or more, and is preferably 3000 or less, more preferably 2000 or less.
[0057] As compound (II), 2,2',7,7'-tetrakis(N,N-di-p-methoxyphenylamino)-9,9'-spirobifluorene (Spiro-OMeTAD) is preferred.
[0058] Compound (II) can be synthesized by a known method as described in the Examples below. The fact that compound (II) is contained in the hole transport material means that 1 H-NMR, 13 This can be confirmed by analytical methods such as C-NMR, X-ray crystal structure analysis using single crystals, and LC-MS.
[0059] (Other semiconductor compounds) The hole transport material may further include a semiconductor compound other than the compound having a carbazole skeleton and the spirotriarylamine compound having a fluorene skeleton, as long as the effect of the present invention is not impaired. The other semiconductor compound may be any semiconductor compound. Other organic semiconductor compounds include various low molecular weight compounds and high molecular weight compounds.
[0060] Examples of low molecular weight organic semiconductor compounds include polycyclic aromatic compounds. For example, acene compounds such as tetracene and pentacene, oligothiophene compounds, phthalocyanine compounds, perylene compounds, rubrene compounds, and arylamine compounds such as triarylamine compounds (excluding spirotriarylamine compounds having a fluorene skeleton).
[0061] Examples of the polymeric organic semiconductor compound include conjugated polymers such as polythiophene-based polymers, polyacetylene-based polymers, polyaniline-based polymers, polyphenylene-based polymers, polyphenylenevinylene-based polymers, polyfluorene-based polymers, and polypyrrole-based polymers; and arylamine polymers such as triarylamine polymers.
[0062] (Dopant) The hole transport material according to one embodiment may further include a dopant. A dopant is a compound that can impart charge to a compound by chemical reaction or by donating or receiving electrons. By using a dopant, the properties of the hole transport material, such as the electrical conductivity and hole transport ability, can be controlled, so that the electrical conductivity and hole transport ability of the hole transport layer relative to the active layer can be further optimized.
[0063] Examples of the dopant include hypervalent iodine compounds, boron compounds such as tetrakis(pentafluorophenyl)borate (TPFB), molybdenum compounds such as tris[1-(methoxycarbonyl)-2-(trifluoromethyl)-ethane-1,2-dithiolene]molybdenum, and organic compounds having a tetracyanoquinodimethane skeleton such as 2,3,4,6-tetrafluoro-7,7,8,8-tetracyanoquinodimethane.
[0064] The dopant preferably undergoes a charge transfer reaction with at least one of the organic semiconductor compounds before or after the formation of the hole transport layer. As the dopant, a hypervalent iodine compound is preferable because it has excellent solubility and easily generates an electron-accepting active site that functions as an oxidizing agent by heating or the like.
[0065] Hypervalent iodine compounds act as dopants for organic semiconductor compounds and exhibit electron-accepting properties (i.e., function as oxidizing agents). In addition, electron-accepting dopants can improve the electrical conductivity and hole transport ability of organic semiconductor compounds by removing electrons from the organic semiconductor compounds.
[0066] A hypervalent iodine compound is a compound containing hypervalent iodine, and is defined as a compound containing iodine with an oxidation number of three or more. For example, the dopant is preferably an iodine(III) compound or an iodine(V) compound. An example of an iodine(V) compound containing pentavalent iodine is a periodinane compound such as Dess-Martin periodinane. In addition, an example of an iodine(III) compound containing trivalent iodine is a compound having a structure in which iodobenzene is oxidized, such as (diacetoxyiodo)benzene, and a diaryliodonium salt. In terms of showing good electron accepting properties and being unlikely to cause a reverse reaction when the molecule is destroyed in the oxidation process, an organic compound containing trivalent iodine is preferable as the dopant, and among them, diaryliodonium salts are more preferable.
[0067] Diaryliodonium salts are compounds in which the + -Ar]X 1- Here, each of the two Ar represents an aromatic group. The aromatic group is not particularly limited, and examples thereof include Ar 1 , Ar 2 Examples of the aromatic groups include those exemplified as X. 1- represents any anion. X 1- Examples of the cations include halide ions, trifluoroacetate ions, tetrafluoroborate ions, and tetrakis(pentafluorophenyl)borate ions. X is preferred because it has high solubility and the reaction for producing the coating solution can proceed smoothly. - is preferably an anion having a fluorine atom.
[0068] A preferred example of the dopant is the following compound (Q):1- represents any anion, the details of which are as described above. [R 11 -I + -R 12 ]X 1- Formula (Q)
[0069] In formula (Q), R 11 and R 12 are each independently a monovalent organic group. Examples of the monovalent organic group include an aliphatic group and an aromatic group.
[0070] Examples of the aliphatic group include an aliphatic hydrocarbon group having 1 to 20 carbon atoms and an aliphatic heterocyclic group having 4 to 20 carbon atoms. Examples of the aliphatic group include an alkyl group including a cycloalkyl group, an alkenyl group, and an alkynyl group. More specifically, examples of the aliphatic group include a methyl group, an ethyl group, a butyl group, a cyclohexyl group, and a tetrahydrofuryl group.
[0071] Examples of the aromatic group include an aromatic hydrocarbon group having 6 to 20 carbon atoms and an aromatic heterocyclic group having 2 to 20 carbon atoms. More specific examples include a phenyl group, a naphthyl group, a biphenyl group, a thienyl group, and a pyridyl group.
[0072] R 11 and R 12 The aliphatic group and aromatic group may have a substituent, for example, a halogen atom, a hydroxyl group, a cyano group, an amino group, a carboxyl group, an ester group, an alkylcarbonyl group, an acetyl group, a sulfonyl group, a silyl group, a boryl group, a nitrile group, an alkyl group, an alkenyl group, an alkynyl group, an alkoxy group, a thio group, a seleno group, an aromatic hydrocarbon group, an aromatic heterocyclic group, and the like.
[0073] R 11 and R 12 R is preferably an aromatic hydrocarbon group having 6 to 20 carbon atoms, more preferably a phenyl group. Here, it is preferable that the aromatic hydrocarbon group does not have a substituent or has an alkyl group having 1 to 6 carbon atoms. 11 and R 12is particularly preferably a phenyl group having an alkyl group at the para position.
[0074] Among the compounds (Q), the following compound (Q1) is preferred.
[0075] [ka]
[0076] In formula (Q1), Ar 4 , Ar 5 , Ar 6 each independently represents an aromatic hydrocarbon group having 6 to 20 carbon atoms or a heteroaromatic hydrocarbon group having 2 to 20 carbon atoms, which may have a substituent.
[0077] Furthermore, the compound (Q) is preferably at least one selected from the group consisting of the following compound (Q2) and the following compound (Q3). [ka]
[0078] In formula (Q3), R 7 , R 8 , R 9 , R 10 are each independently a hydrogen atom, a halogen atom, or an alkyl group, an alkenyl group, an alkynyl group, an alkoxy group, an aryloxy group or an aromatic group which may have a substituent; and n is an integer of 0 to 5.
[0079] (Composition of hole transport material) The content of the compound having a carbazole skeleton is preferably high because it is easy to set the ionization potential of the hole transport material within a predetermined range. In the hole transport material according to an example, the content of the compound having a carbazole skeleton is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more of the total mass of the hole transport material. Here, the upper limit of the content of the compound having a carbazole skeleton may be 100% by mass, 90% by mass or less, 85% by mass or less, or 80% by mass or less.
[0080] The content of the spiro triarylamine compound having a fluorene skeleton is preferably large because it is easy to set the conductivity of the hole transport material to a predetermined range. In an example of the hole transport material, the proportion of the spiro triarylamine compound having a fluorene skeleton is preferably 40 mass% or more of the total mass of the hole transport material, more preferably 50 mass% or more, and even more preferably 60 mass% or more. Here, the upper limit of the proportion of the spiro triarylamine compound having a fluorene skeleton may be 100 mass%, 90 mass% or less, 85 mass% or less, or 80 mass% or less.
[0081] The amount of the dopant is preferably large because the conductivity and hole transport ability of the hole transport layer are easily improved. In the hole transport material according to one example, the ratio of the dopant is preferably 0.001 parts by mass or more, more preferably 0.01 parts by mass or more, even more preferably 0.05 parts by mass or more, and particularly preferably 0.1 parts by mass or more, based on 100 parts by mass of the compound having a carbazole skeleton and the spirotriarylamine compound having a fluorene skeleton in total.
[0082] On the other hand, the amount of the dopant is preferably small because it suppresses the generation of leakage current in the power generation device and is likely to improve the power generation efficiency, particularly in a low-illumination environment. In one example of the hole transport material, the ratio of the dopant is preferably 75 parts by mass or less, more preferably 60 parts by mass or less, and even more preferably 50 parts by mass or less, relative to 100 parts by mass in total of the compound having a carbazole skeleton and the spirotriarylamine compound having a fluorene skeleton.
[0083] Therefore, when the hole transport material contains a dopant, the proportion of the dopant is most preferably 0.1 to 50 parts by mass per 100 parts by mass in total of the compound having a carbazole skeleton and the spirotriarylamine compound having a fluorene skeleton.
[0084] (solvent) The hole transport material may further include a solvent. For example, a hole transport material including at least one selected from the group consisting of a compound having a carbazole skeleton, a spirotriarylamine compound having a fluorene skeleton, and a dopant, and a solvent, is useful as a coating liquid for forming a hole transport layer of a power generating device.
[0085] The solvent is not particularly limited as long as it can dissolve the compounds that are components for obtaining the desired hole transport layer. For example, the following polar solvents can be mentioned. Examples of polar solvents include linear esters such as methyl acetate, ethyl acetate, propyl acetate, butyl acetate, phenyl acetate, methyl propionate, ethyl propionate, propyl propionate, phenyl propionate, methyl 3-methoxypropionate, methyl 3-ethoxypropionate, methyl lactate, and ethyl lactate; aromatic esters such as ethyl benzoate and ethyl picolinate; cyclic esters such as γ-butyrolactone and caprolactone; and ether esters such as ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, propylene glycol-1-monomethyl ether acetate, and propylene glycol-1-monoethyl ether acetate. Examples of suitable organic solvents include alcohols such as methanol, ethanol, and isopropanol, ketones such as acetone, methyl ethyl ketone, methyl isoamyl ketone, methyl amyl ketone, and cyclohexanone, ethers such as tetrahydrofuran, dioxane, anisole, ethylene glycol dimethyl ether, and diethylene glycol dimethyl ether, ether alcohols such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, and 3-methoxy-3-methyl-1-butanol, amides such as N,N-dimethylformamide and N-methylpyrrolidone, nitriles such as acetonitrile and benzonitrile, and dimethyl sulfoxide. Other suitable organic solvents include polyhaloaliphatic hydrocarbons such as chloroform and dichloromethane, and polyhaloaromatic compounds such as bromobenzene, iodobenzene, chlorobenzene, and dichlorobenzene. The organic solvent may be used alone or in combination of two or more kinds.
[0086] [Power generation device] The power generation device of the present invention is a photoelectric conversion element having a pair of electrodes composed of an upper electrode and a lower electrode, an active layer located between the pair of electrodes and containing an organic-inorganic hybrid semiconductor compound, and a hole transport layer located between the pair of electrodes. In the power generating device of the present invention, the hole transport layer contains the above-mentioned hole transport material of the present invention. Therefore, the power generating device can be used in a low illuminance environment. A low illuminance environment usually means an environment of 10 to 5000 lux, preferably an environment of 100 to 300 lux, and more preferably an environment of 200 lux.
[0087] In the power generating device 100 shown in FIG. 1, a lower electrode 101, an active layer 103, and an upper electrode 105 are arranged in this order.
[0088] Although the buffer layer 102 is disposed between the lower electrode 101 and the active layer 103, in other examples the buffer layer 102 is not essential and is an optional component. Also, the buffer layer 104 is disposed between the upper electrode 105 and the active layer 103, but in other examples the buffer layer 104 is not essential and is an optional component. For example, the buffer layer 102 can be a hole transport layer, and the buffer layer 104 can be an electron transport layer. Conversely, the buffer layer 102 and the buffer layer 104 can be an electron transport layer and a hole transport layer, respectively.
[0089] Although the power generating device 100 includes a substrate 106, in other examples the substrate 106 is not essential and the substrate 106 is an optional component. The power generating device 100 may further include other components, such as an insulator layer and a work function tuning layer, which are not shown.
[0090] (electrode) In the power generating device 100, the electrodes have the function of collecting holes and electrons generated by light absorption in the active layer 103. As in the power generating device 100, one of a pair of electrodes is called an upper electrode and the other is called a lower electrode. When the power generating device 100 has a substrate or is provided on a substrate, the electrode closer to the substrate can be called the lower electrode and the electrode farther from the substrate can be called the upper electrode. Also, a transparent electrode can be called the lower electrode, and an electrode less transparent than the lower electrode can be called the upper electrode. The power generating device 100 shown in FIG. 1 has a lower electrode 101 and an upper electrode 105.
[0091] The pair of electrodes may be an anode suitable for collecting holes and a cathode suitable for collecting electrons. In this case, the power generating device 100 may have a forward configuration in which the lower electrode 101 is the anode and the upper electrode 105 is the cathode, or may have an inverted configuration in which the lower electrode 101 is the cathode and the upper electrode 105 is the anode.
[0092] In a pair of electrodes, it is sufficient that either one of them is light-transmitting, and both may be light-transmitting. Being light-transmitting usually means that the transmittance of visible light (wavelength 350 to 700 nm) is 40% or more. The visible light transmittance of the electrode is preferably high, and particularly preferably 70% or more, since more light passes through the transparent electrode and reaches the active layer. The visible light transmittance can be measured with a spectrophotometer (e.g., U-4100 manufactured by Hitachi High-Tech Corporation).
[0093] There are no particular limitations on the constituent members and manufacturing methods of the lower electrode 101, the upper electrode 105, the anode, and the cathode, and various techniques can be used. For example, the members and manufacturing methods described in each document such as International Publication No. 2013 / 171517, International Publication No. 2013 / 180230, and JP-A-2012-191194 can be used.
[0094] (active layer) In the power generation device 100, the active layer 103 is a layer where photoelectric conversion takes place. When the power generation device 100 receives light, the light is absorbed by the active layer 103 and carriers are generated. The generated carriers are extracted from the lower electrode 101 and the upper electrode 105.
[0095] The active layer includes an organic-inorganic hybrid semiconductor compound, which is a compound in which an organic component and an inorganic component are combined at a molecular or nano level and which exhibits semiconductor properties.
[0096] The organic-inorganic hybrid semiconductor compound is preferably a compound having a perovskite structure (hereinafter, sometimes referred to as a perovskite semiconductor compound). The perovskite semiconductor compound refers to a semiconductor compound having a perovskite structure. There is no particular limitation on the perovskite semiconductor compound, but it can be selected from, for example, those listed in Galasso et al. Structure and Properties of Inorganic Solids, Chapter 7- Perovskite type and related structures. In addition, for example, the perovskite semiconductor compound can be selected from those listed in the general formula AMX 2 3 Represented by AMX 2 3 Of the type, general formula A 2 MX 2 4 A represented by 2 MX 2 4 Here, M is a divalent cation, A is a monovalent cation, and X 2 refers to a monovalent anion.
[0097] There is no particular limitation on the monovalent cation A, but those described in the above-mentioned book by Galasso can be used. For example, cations containing elements of Groups 1 and 13 to 16 of the periodic table can be mentioned. Among these, cesium ion, rubidium ion, potassium ion, ammonium ion which may have a substituent, and phosphonium ion which may have a substituent are preferable. Examples of the ammonium ion that may have a substituent include primary ammonium ion and secondary ammonium ion. There is no particular restriction on the substituent. Examples of the ammonium ion that may have a substituent include alkyl ammonium ion and aryl ammonium ion. In order to avoid steric hindrance, monoalkyl ammonium ion that forms a three-dimensional crystal structure is preferred, and from the viewpoint of improving stability, it is preferred to use an alkyl ammonium ion substituted with one or more fluorine groups. In addition, two or more types of cations may be used in combination as the cation A.
[0098] Examples of the monovalent cation A include a methylammonium ion, a methylammonium monofluoride ion, a methylammonium difluoride ion, a methylammonium trifluoride ion, an ethylammonium ion, an isopropylammonium ion, an n-propylammonium ion, an isobutylammonium ion, an n-butylammonium ion, a t-butylammonium ion, a dimethylammonium ion, a diethylammonium ion, a phenylammonium ion, a benzylammonium ion, a phenethylammonium ion, a guanidinium ion, a formamidinium ion, an acetamidinium ion, and an imidazolium ion.
[0099] There is no particular limitation on the divalent cation M, but a divalent metal cation or semimetal cation is preferred. For example, a cation of an element in Group 14 of the periodic table is included. More specifically, for example, a lead cation (Pb 2+ ), tin cation (Sn 2+ ), germanium cation (Ge 2+) can be mentioned. Two or more kinds of cations may be used in combination as the cation M. From the viewpoint of obtaining a stable power generating device, it is particularly preferable to use a lead cation or two or more kinds of cations including a lead cation.
[0100] Monovalent anion X 2 Examples of the cations include halide ions, acetate ions, nitrate ions, sulfate ions, borate ions, acetylacetonate ions, carbonate ions, citrate ions, sulfur ions, tellurium ions, thiocyanate ions, titanate ions, zirconate ions, 2,4-pentanedionate ions, and silicofluoride ions. 2 Examples of the anion include halide ions and combinations of halide ions with other anions. 2 The active layer may be formed of one or more of these in any combination and ratio. 2 The band gap of the active layer can be adjusted by changing the type and combination of X. 2 is preferably a halide ion such as chloride ion, bromide ion or iodide ion, and more preferably bromide ion or iodide ion.
[0101] As the perovskite semiconductor compound, for example, an organic-inorganic perovskite semiconductor compound is preferable, and a halide-based organic-inorganic perovskite semiconductor compound is particularly preferable. As the perovskite semiconductor compound, for example, CH 3 NH 3 PbI 3 , C.H. 3 NH 3 PbBr 3 , C.H. 3 NH 3 PbCl 3 , C.H. 3 NH 3 SnI 3 , C.H. 3 NH 3 SnBr 3 , C.H. 3 NH 3 SnCl 3 , C.H.3 NH 3 PbI (3-x) Cl x , C.H. 3 NH 3 PbI (3-x) Br x , C.H. 3 NH 3 PbBr (3-x) Cl x , C.H. 3 NH 3 Pb (1-y) Sn y I 3 , C.H. 3 NH 3 Pb (1-y) Sn y Br 3 , C.H. 3 NH 3 Pb (1-y) Sn y Cl 3 , C.H. 3 NH 3 Pb (1-y) Sn y I( 3-x) Cl x , C.H. 3 NH 3 Pb (1-y) Sn y I (3-x) Br x , C.H. 3 NH 3 Pb (1-y) Sn y Br (3-x) Cl x Examples include: In addition, in the above compounds, CH 3 NH 3 Instead of CFH 2 NH 3 , C.F. 2 HNH 3 , C.F. 3 NH 3 , N.H. 2 CH=NH 3、 In the formula, x is an arbitrary value of 0 to 3, and y is an arbitrary value of 0 to 1. 3 NH 3 PbI 3 , C.H. 3 NH3 PbBr 3 , C.H. 3 NH 3 PbCl 3 , C.H. 3 NH 3 PbI (3-x) Cl x , C.H. 3 NH 3 PbI (3-x) Br x , C.H. 3 NH 3 PbBr (3-x) Cl x , C.H. 3 NH 3 Pb (1-y) Sn y Br 3 , C.H. 3 NH 3 Pb (1-y) Sn y Cl 3 , C.H. 3 NH 3 Pb (1-y) Sn y I (3-x) Cl x , C.H. 3 NH 3 Pb (1-y) Sn y I (3-x) Br x , C.H. 3 NH 3 Pb (1-y) Sn y Br (3-x) Cl x And in the above compounds, CH 3 NH 3 Instead of NH 2 CH=NH 3、 Compounds using Cs and Rb are preferred. 3 NH 3 PbI 3 , C.H. 3 NH 3 PbBr 3 , C.H. 3 NH 3 PbI (3-x) Cl x , C.H. 3 NH 3 PbI (3-x) Brx , C.H. 3 NH 3 PbBr (3-x) Cl x , and CH in the above compounds 3 NH 3 Instead of NH 2 CH=NH 3、 Compounds using Cs and Rb are examples.
[0102] The active layer may contain two or more organic-inorganic hybrid semiconductor compounds. For example, A, B and X 2 The active layer may contain two or more organic-inorganic hybrid semiconductor compounds, at least one of which is different. The active layer may have a laminate structure formed of multiple layers containing different materials or different components.
[0103] The amount of the organic-inorganic hybrid semiconductor compound contained in the active layer is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more, based on the total mass of the active layer, so that good semiconductor properties can be obtained. There is no particular upper limit. The active layer may also contain additives other than the organic-inorganic hybrid semiconductor compound. Examples of additives include inorganic compounds such as inorganic salts such as halides, oxides, sulfides, sulfates, nitrates, and ammonium salts, and organic compounds.
[0104] The ionization potential of the active layer is preferably high in order to fully satisfy the absorption range in the long wavelength region for a light source in the visible light region that provides white light and to easily increase the power generation efficiency. In one example, the ionization potential is preferably -6.0 eV or higher, more preferably -5.95 eV or higher, and even more preferably -5.9 eV or higher. On the other hand, the ionization potential of the active layer is preferably low in order to reduce the loss of the voltage obtained from a light source in the visible light region and to increase the power generation efficiency. In one example, the ionization potential is preferably −5.7 eV or less, more preferably −5.75 eV or less, and even more preferably −5.9 eV or less.
[0105] The band gap of the active layer is preferably large in that the energy required for separating excitons generated in the semiconductor by low-intensity light such as indoor light into positive and negative charges is sufficiently satisfied, and power generation efficiency is likely to be high. In one example, the band gap is preferably 1.6 eV or more, more preferably 1.65 eV or more, even more preferably 1.7 eV or more, and most preferably 1.75 eV or more. On the other hand, the band gap of the active layer is preferably small in order to provide appropriate energy (not excessive energy) for excitons generated by indoor light, etc., and to facilitate high power generation efficiency. In one example, it is preferably 2.3 eV or less, more preferably 2.25 eV or less, even more preferably 2.2 eV or less, and most preferably 2.15 eV or less.
[0106] It is particularly preferable that the ionization potential and band gap of the active layer are both in the above-mentioned preferred ranges, since this makes it easier to improve power generation efficiency particularly under low-illuminance light sources such as fluorescent lamps and LED lamps, which are visible light sources widely used indoors and outdoors. In one example, it is particularly preferable that the ionization potential of the active layer is in the range of -6.0 eV or more and -5.7 eV or less, and the band gap is in the range of 1.6 eV or more and 2.3 eV or less.
[0107] The ionization potential of the active layer can be adjusted to the desired range by, for example, adjusting the type of organic-inorganic hybrid semiconductor compound. For example, when the above-mentioned perovskite semiconductor compound is used, the ionization potential can be adjusted by adjusting the type of cation. More specifically, the composition of the organic ammonium salt and the inorganic ammonium salt, which are precursors used to form the perovskite semiconductor compound described later, can be mixed in a desired composition ratio and appropriately adjusted by processing.
[0108] The band gap of the active layer can be adjusted to the desired range by, for example, adjusting the type of organic-inorganic hybrid semiconductor compound. For example, when the above-mentioned perovskite semiconductor compound is used, the band gap can be adjusted by adjusting the type and ratio of the anions. More specifically, the band gap can be adjusted by selecting the halogen species ratio of the metal halide compound used as a precursor for forming the perovskite semiconductor compound described later, mixing the composition of the organic ammonium salt and inorganic ammonium salt used as the precursor with the corresponding halogen composition in the desired composition ratio, and processing the mixture.
[0109] There is no particular limit to the thickness of the active layer. In terms of being able to absorb more light, it is preferable that the active layer 103 is thicker. In one example, it is preferably 10 nm or more, more preferably 50 nm or more, even more preferably 100 nm or more, particularly preferably 150 nm or more, and most preferably 200 nm or more. On the other hand, it is preferable that the active layer 103 is thinner in terms of reducing the series resistance and increasing the charge extraction efficiency. In one example, it is preferably 1500 nm or less, more preferably 1200 nm or less, and even more preferably 800 nm or less. Therefore, it is most preferable that the thickness of the active layer 103 is 200 nm or more and 800 nm or less.
[0110] The method of forming the active layer is not particularly limited, and can be formed by any method. For example, coating method, vapor deposition method, and co-deposition method can be mentioned. The coating method is preferable because the active layer can be easily formed. For example, a method of forming an active layer by coating a coating liquid containing an organic-inorganic hybrid semiconductor compound or its precursor, and drying by heating as necessary can be mentioned. In addition, after coating the coating liquid, a solvent in which the organic-inorganic hybrid semiconductor compound has low solubility can be further coated to precipitate the organic-inorganic hybrid semiconductor compound.
[0111] The organic-inorganic hybrid semiconductor compound precursor refers to a compound that becomes an organic-inorganic hybrid semiconductor compound after being applied as a coating liquid. For example, an organic-inorganic hybrid semiconductor compound precursor that becomes an organic-inorganic hybrid semiconductor compound by heating can be used. For example, a compound represented by the general formula AX 2 and a compound represented by the general formula MX 2 2 The coating liquid can be prepared by mixing a compound represented by the general formula AMX with a solvent and heating and stirring the mixture. After coating the coating liquid, the mixture is dried by heating to prepare a compound represented by the general formula AMX 2 3 The solvent is not particularly limited as long as it dissolves the organic-inorganic hybrid semiconductor compound and the optional additives, and examples of the solvent include organic solvents such as N,N-dimethylformamide.
[0112] The coating liquid can be applied by any method, for example, spin coating, inkjet coating, doctor blade coating, drop casting, reverse roll coating, gravure coating, kiss coating, roll brushing, spray coating, air knife coating, wire barber coating, pipe doctor coating, impregnation, coating, and curtain coating.
[0113] (Buffer layer) In the power generating device 100, the buffer layer is a layer located between the active layer 103 and at least one of the pair of electrodes 101, 105. The buffer layer can be used, for example, to improve the efficiency of carrier movement from the active layer 103 to the lower electrode 101 or the upper electrode 105. The buffer layer may have a single layer structure or a multilayer structure of two or more layers. The buffer layer may be a hole transport layer or an electron transport layer. A hole transport layer is more preferable.
[0114] (Hole transport layer) The hole transport layer comprises the hole transport material of the present invention described above. In the power generating device of the present invention, the hole transport layer contains the hole transport material of the present invention, and therefore the ionization potential and electrical conductivity of the hole transport layer can be set within suitable ranges, allowing the device to achieve high power generation efficiency under low illuminance.
[0115] The conductivity of the hole transport layer is set to 5×10 from the viewpoint of efficiently transporting charges generated upon light irradiation to the electrode and suppressing leakage even of charges generated by light with extremely low illuminance. -6 ~5×10 -4 S / cm is preferred, and 7×10 -6 ~5×10 -4 S / cm is more preferable, 1×10 -5 ~5×10 -4 S / cm is more preferred. As described above, the conductivity of the hole transport layer can be adjusted by using a spirotriarylamine compound having a fluorene skeleton.
[0116] From the viewpoint of matching with the ionization potential of the active layer, the ionization potential of the hole transport layer is preferably −5.80 eV or more and less than −5.30 eV, more preferably −5.80 to −5.35 eV, and even more preferably −5.80 to −5.40 eV.
[0117] The ionization potential of the hole transport layer can be adjusted by using a compound having a carbazole skeleton, as described above. A more detailed method for adjusting the ionization potential to the desired range is, for example, controlling the electronic state of the compound by appropriately arranging the type and position of the substituent of the aromatic compound in the compound having a carbazole skeleton. In addition, the electronic state of the compound of the hole transport layer can be adjusted by using a dopant, which will be described later, in combination with the hole transport layer, i.e., oxidizing or reducing the whole or part of the compound.
[0118] The thickness of the hole transport layer of the power generating device according to the present invention is preferably thicker in the sense that when the active layer located between the upper and lower electrodes has a high charge transporting ability, current leakage due to the formation of a conductive path through the upper and lower electrodes and the active layer is unlikely to occur. In one example, the thickness is preferably 20 nm or more, more preferably 40 nm or more, and even more preferably 60 nm or more. On the other hand, it is preferable that the thickness is thin in the sense that resistance in charge transport by the hole transport layer is unlikely to occur and cost reduction is achieved by saving the amount of compound in the hole transport layer. In one example, the thickness is preferably 1000 nm or less, more preferably 750 nm or less, and even more preferably 500 nm or less.
[0119] (electron transport layer) The power generating device according to the present invention may have an electron transport layer. Any material capable of improving the efficiency of electron extraction from the active layer to the cathode can be used as the material of the electron transport layer. For example, inorganic compounds, organic compounds, and organic-inorganic perovskite semiconductor compounds described in each of the documents such as International Publication No. 2013 / 171517, International Publication No. 2013 / 180230, and JP-A No. 2012-191194 can be mentioned.
[0120] Examples of inorganic compounds for the electron transport layer include salts of alkali metals such as lithium, sodium, potassium, and cesium, and metal oxides such as zinc oxide, titanium oxide, aluminum oxide, and indium oxide. Examples of organic compounds for the electron transport layer include bathocuproine (BCP), bathophenanthrene (Bphen), and (8-hydroxyquinolinato)aluminum (Alq 3 ), boron compounds, oxadiazole compounds, benzimidazole compounds, naphthalenetetracarboxylic anhydride (NTCDA), perylenetetracarboxylic anhydride (PTCDA), fullerene compounds, phosphine oxide compounds, and phosphine sulfide compounds having a double bond with an element of Group 16 of the periodic table.
[0121] When the power generating device includes an electron transport layer, the thickness of the layer is preferably thick, because when the active layer located between the upper and lower electrodes has a high charge transporting ability, current leakage due to the formation of a conductive path between the upper and lower electrodes and the active layer is unlikely to occur, the effect of the unevenness of the lower electrode can be covered, and the wettability of the active layer is easy to control. In one example, the thickness is preferably 1 nm or more, more preferably 5 nm or more, and even more preferably 10 nm or more. On the other hand, it is preferable that the thickness is thin, because resistance in charge transport by the electron transport layer is unlikely to occur, and cost reduction can be achieved by saving the amount of compound in the electron transport layer. In one example, the thickness is preferably 200 nm or less, more preferably 150 nm or less, and even more preferably 100 nm or less.
[0122] (base material) The power generating device may have a substrate. In Fig. 1, the power generating device 100 has a substrate 106 serving as a support, but the power generating device according to the present invention may not have the substrate 106. The material of the substrate is not particularly limited as long as it does not significantly impair the effects of the present invention, and for example, materials described in each of the documents such as WO 2013 / 171517, WO 2013 / 180230, and JP 2012-191194 A can be used without restrictions.
[0123] (Photoelectric conversion characteristics) The photoelectric conversion characteristics of the power generation device 100 can be obtained as follows. The power generation device 100 is irradiated with light of an appropriate spectrum at a certain irradiation intensity, and the current-voltage characteristics are measured. From the obtained current-voltage curve, photoelectric conversion characteristics such as the photoelectric conversion efficiency (PCE), short-circuit current density (Jsc), open circuit voltage (Voc), fill factor (FF), series resistance, and shunt resistance can be obtained. As an example, the power generation device 100 is irradiated with white LED light with a color temperature of 5000 K at an appropriate irradiation intensity (illuminance), and the current-voltage characteristics at each illuminance can be measured.
[0124] One embodiment of the power generation device according to the present invention has excellent power generation efficiency at low illuminance (10 to 5000 lux), and can achieve a photoelectric conversion efficiency of 20% or more when using a white light source such as a white LED light with a color temperature of 5000 K. Furthermore, when irradiated with white LED light with a color temperature of 5000 K and the illuminance of the light receiving surface is 200 lux, the photoelectric conversion efficiency can be 25% or more. This photoelectric conversion efficiency (PCE) is the output (maximum output) at the optimal operating point of the current-voltage curve of a power generating device measured with a specified irradiated light, divided by the total amount of energy contained in the irradiated light (%). For example, the total energy of sunlight with an intensity of AM1.5G is 100mW / cm 2 If white LED light with a color temperature of 5000K is irradiated and the illuminance on the light receiving surface is 200 lux, the illuminance is 100μW / cm 2 It is. A color temperature of 5000K is defined by the JIS Z8725:2015 standard.
[0125] (Method of manufacturing a power generating device) The method for producing the power generating device is not particularly limited as long as it is a method that can incorporate the hole transport material of the present invention into a hole transport layer, and various methods for producing power generating devices using a perovskite semiconductor compound can be applied. For example, a coating solution containing the above-mentioned compound having a carbazole skeleton, the spiro triarylamine compound having a fluorene skeleton, a dopant and a solvent is prepared, and a wet film forming method such as a spin coating method or an inkjet method is used to form a hole transport layer. An electron transport layer can also be formed by a similar coating method. In addition, these buffer layers can also be formed by a dry film forming method such as a vacuum deposition method.
[0126] The hole transport layer is preferably formed by a coating method, more preferably by coating a liquid containing the above-mentioned compound having a carbazole skeleton, the spirotriarylamine compound having a fluorene skeleton, and a dopant. Therefore, a suitable method for producing a power generating device includes a step of forming a hole transport layer using a liquid containing the above-mentioned compound having a carbazole skeleton, a spirotriarylamine compound having a fluorene skeleton, and a dopant. The hole transport layer can be formed by a coating method using the liquid.
[0127] 1, the power generating device 100 can be manufactured by stacking the layers that constitute the power generating device 100. For example, various methods such as a sheet-to-sheet method or a roll-to-roll method can be applied.
[0128] When manufacturing the power generating device 100, after stacking the upper electrode 105, the power generating device 100 may be heated, for example, in a temperature range of 50°C to 80°C and 280°C to 300°C (this heating step may be referred to as an annealing step). The annealing step is preferably performed at a high temperature in order to easily obtain the effect of improving the adhesion between the layers of the power generating device 100, for example, between the buffer layer 102 and the lower electrode 101, between the buffer layer 102 and the active layer 103, etc. For example, it is preferably performed at 50°C or higher. By improving the adhesion between the layers, the thermal stability, durability, etc. of the power generating device can be improved. On the other hand, the temperature of the annealing step is preferably low in order to prevent the organic compound contained in the power generating device 100 from being thermally decomposed. For example, it is preferably performed at 300°C or lower. In the annealing step, stepwise heating using different temperatures within the above temperature range may be performed.
[0129] The heating time in the above-mentioned suitable temperature range is preferably 1 to 3 minutes or more and 60 to 180 minutes or less, in terms of easily improving adhesion while suppressing thermal decomposition. The annealing process is preferably terminated when the open circuit voltage, short circuit current, and fill factor, which are parameters of the solar cell performance, reach a certain value. In addition, the annealing process is preferably performed under normal pressure and in an inert gas atmosphere in order to prevent thermal oxidation of the constituent materials. As a heating method, the power generation device may be placed on a heat source such as a hot plate, or may be placed in a heating atmosphere such as an oven. In addition, heating may be performed in a batch manner or a continuous manner.
[0130] [Solar cell] The power generation device according to the present invention is suitable as an indoor solar cell because it has excellent photoelectric conversion efficiency under low illuminance. FIG. 2 shows an example of a solar cell equipped with the power generation device of the present invention. The thin-film solar cell 14 shown in FIG. 2 is equipped with a power generation device 100 (not shown). The thin-film solar cell 14 is equipped with a weather-resistant protective film 1, an ultraviolet cut film 2, a gas barrier film 3, a getter material film 4, a sealing material 5, a solar cell element 6 having a power generation device 100 (not shown), a sealing material 7, a getter material film 8, a gas barrier film 9, and a back sheet 10 in this order. The thin-film solar cell 14 is configured such that light is irradiated from the side where the protective film 1 is formed (lower side in FIG. 2) and the solar cell element 6 generates electricity. However, the thin-film solar cell 14 does not need to have all of these components, and necessary components can be selected arbitrarily.
[0131] The thin-film solar cell 14 may be used alone, or a plurality of thin-film solar cells 14 may be connected together for use, or may be combined with other components to form a solar cell module. For example, as shown in Fig. 3, a solar cell module 13 having thin-film solar cells 14 on a substrate 12 may be fabricated, and this solar cell module 13 may be installed at the location of use.
[0132] The selection of each of the above-mentioned components and the manufacturing method thereof can be performed using well-known techniques, such as those described in WO 2013 / 171517, WO 2013 / 180230, and JP 2012-191194 A.
[0133] There are no limitations on the applications of the power generation device of the present invention and the solar cell and solar cell module equipped with the same, and examples of the applications include solar cells for building materials, solar cells for automobiles, solar cells for interior decoration, solar cells for railways, solar cells for ships, solar cells for airplanes, solar cells for spacecraft, solar cells for home appliances, solar cells for mobile phones, and solar cells for toys. The power generating device of the present invention and the solar cell and solar cell module including the same exhibit excellent photoelectric conversion efficiency even in low-illumination environments, and are therefore particularly suitable for energy harvesting applications.
[0134] Although several embodiments have been described above, the present invention is not limited to the embodiments disclosed in this specification, and can be appropriately modified and implemented without departing from the gist of the invention. The embodiments disclosed in this specification can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the gist of the invention. EXAMPLES
[0135] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following description.
[0136] [Explanation of compounds and abbreviations] (First Compound) Compound A represented by the following formula (A) was synthesized by the method described in Yang, J. Wet. al., Phys. Chem. Chem. Phys. 2015, 17, 24468. Compound A is an example of compound (I).
[0137] [ka]
[0138] (Second Compound) [2,2',7,7'-tetrakis(N,N-di-p-methoxyphenylamino)-9,9'-spirobifluorene] (manufactured by Aldrich) represented by the following formula (B) was used as compound B. Compound B is an example of compound (II).
[0139] [ka]
[0140] (Third Compound) TPFB: 4-isopropyl-4'-methyldiphenyliodonium tetrakis(pentafluorophenyl)borate (TCI product)
[0141] LiTFSI: Lithium bistrifluoromethanesulfonimide (Sigma-Aldrich product)
[0142] The chemical structure of Compound 1 is shown below.
[0143] [ka]
[0144] [Example 1] (Preparation of Coating Solution for Hole Transport Layer) An o-dichlorobenzene solution containing compound A, compound B, and compound 1 was prepared. Next, the solution was heated and stirred at 150° C. for 1 hour to prepare a coating solution for a hole transport layer in advance. In the coating solution for a hole transport layer, the content of compound A was 20 mM, and the content of compound B was 20 mM. In addition, the content of compound 1 in the coating solution for a hole transport layer was 2.8 parts by mass relative to 100 parts by mass of the total of compound A and compound B.
[0145] (Preparation of Coating Solution for Electron Transport Layer) A 7.5% by mass aqueous dispersion of tin oxide was prepared in advance by adding ultrapure water to a 15% by mass aqueous dispersion of tin oxide (IV) (manufactured by Alfa Aesar).
[0146] (Preparation of Coating Solution 1 for Active Layer) Lead iodide (II) was weighed out and placed in a vial, which was then introduced into the glove box. N,N-dimethylformamide was added as a solvent so that the concentration of lead iodide (II) was 1.3 mol / L, and the mixture was then heated and stirred at 100°C for 1 hour to prepare coating solution 1 for the active layer.
[0147] (Preparation of Coating Solution 2A for Active Layer) Formamidine hydrobromide (FABr), methylamine hydrobromide (MABr), and methylamine hydrochloride (MACl) were weighed out in a separate vial in a mass ratio of 7.25:1:1.5 and introduced into the glove box. By adding isopropyl alcohol as a solvent to this, active layer coating solution 2A with a total concentration of FABr, MABr, and MACl of 0.49 mol / L was prepared in advance.
[0148] (Preparation of Coating Solution 2B for Active Layer) In addition, formamidine hydroiodide (FAI), methylamine hydrobromide (MABr), and methylamine hydrochloride (MACl) were weighed out in a mass ratio of 7.25:1:1.5 into another vial and introduced into the glove box. By adding isopropyl alcohol as a solvent to this, active layer coating solution 2B with a total concentration of FAI, MABr, and MACl of 0.49 mol / L was prepared.
[0149] (Creating a power generation device) A glass substrate (Geomatec Corporation) having a patterned indium tin oxide (ITO) transparent conductive film was subjected to ultrasonic cleaning using ultrapure water, drying by nitrogen blowing, and UV-ozone treatment. Then, the previously prepared coating solution for the electron transport layer was spin-coated on the glass substrate at room temperature at a speed of 2000 rpm to a thickness of about 35 nm, and then heated on a hot plate at 150° C. for 10 minutes to form an electron transport layer.
[0150] Next, the glass substrate on which the electron transport layer was formed was introduced into a glove box. Active layer coating solution 1 (150 μL) heated to 100 ° C. was dropped onto the electron transport layer, spin-coated at a speed of 2000 rpm, and annealed on a hot plate at 100 ° C. for 10 minutes to form a lead iodide layer. Furthermore, after the glass substrate on which the lead iodide layer was formed was returned to room temperature, active layer coating solution 2A (120 μL) was spin-coated on the lead iodide layer at a speed of 2000 rpm, heated on a hot plate at 150 ° C. for 20 minutes, and then cooled to room temperature (25 ° C.) to form an active layer (thickness 650 nm) of an organic-inorganic perovskite semiconductor compound.
[0151] Next, the hole transport layer coating solution (120 μL) was spin-coated on the active layer at a speed of 2000 rpm, and then heated on a hot plate at 90° C. for 5 minutes, and then cooled to room temperature (25° C.) to form a hole transport layer (thickness 100 nm). The conductivity and ionization potential of this hole transport layer were measured by the methods described below.
[0152] Next, a 10 nm thick MoO 3 A 30 nm thick IZO layer and a 100 nm thick silver layer were evaporated in this order to form a top electrode. In this manner, a power generating device was fabricated.
[0153] [Examples 2 to 5, Comparative Examples 1 and 2] As shown in Table 1, a power generating device was produced in the same manner as in Example 1, except that the compositions of the coating liquid 2 for active layer (2A, 2B), the coating liquid for hole transport layer, and the configuration of the upper electrode were changed.
[0154] [Measurement method] (conductivity) The conductivity was calculated by forming the thin film to be evaluated by spin coating or the like on a glass substrate having electrodes patterned in a comb shape, reading the amount of change in current value when a voltage was applied over a certain range using a source meter or the like, and dividing the amount by the electrode distance and film thickness, which are constants. Glass substrates with metal electrodes patterned in a comb shape, commercially available from Geomatec Co., Ltd., can be used.
[0155] (Ionization potential: Ip) A hole transport layer containing the semiconductor compound to be evaluated was formed on a glass substrate with a thin ITO film formed on it, and the number of photoelectrons generated was measured using an open counter that requires oxygen. This open counter measures ionized oxygen molecules by trapping photoelectrons in oxygen molecules in the atmosphere. As the energy of the irradiated light is increased, a threshold is observed at which the emission of photoelectrons begins, and this threshold, i.e., the minimum energy (eV) required for the irradiation energy to eject photoelectrons, corresponds to the ionization potential (eV). This type of ionization potential measurement using the photoelectron coefficient method was performed using Riken Keiki's AC-2, AC-3, and other series. The thickness of the hole transport layer to be measured does not substantially affect the measured value, and for example, an active layer formed to a thickness of 400 nm to 600 nm and a hole transport layer formed to a thickness of 5 nm to 100 nm may be measured. The hole transport layer to be measured may be exposed to the atmosphere, and does not need to be formed in contact with the surface of the thin film ITO. For example, an active layer laminated on the surface of a hole transport layer formed on a thin film ITO may be measured. In the measurement of this active layer, the type and performance of the hole transport layer do not substantially affect the measured value. The ionization potential of the active layer and the hole transport layer is not affected by the lamination environment (the presence or absence and type of the lower layer). The conductive glass with thin film ITO used above can be a commercially available product, and the resistance value (surface resistivity) of the thin film ITO is not particularly limited and can be, for example, 2 Ω / sq. to 1000 Ω / sq.
[0156] (Photoelectric conversion characteristics) The photoelectric conversion efficiency was measured when the light receiving surface was irradiated with white LED light with a color temperature of 5000 K and the illuminance was 200 lux. The details of the measurement method are as follows. First, the power generation device was irradiated with white LED light with a color temperature of 5000K. At this time, the irradiation intensity was adjusted using a light meter so that the illuminance on the light receiving surface of the power generation device was 200 lux. Under this environment, a source meter was used to measure the current-voltage curve (IV curve) and determine its maximum output value. This value was divided by the total energy content of the irradiated light to obtain the photoelectric conversion efficiency (%) of the power generation device. The color temperature was measured in accordance with JIS Z8725:2015.
[0157] [result] Table 1 shows the measurement results of the electrical conductivity, ionization potential, and photoelectric conversion efficiency of the hole transport layer in the power generation device.
[0158] [Table 1]
[0159] In the power generation devices of Examples 1 to 3, the power generation efficiency in a low illuminance environment was improved compared to Comparative Example 1. Similarly, in the power generation devices of Examples 4 and 55, the power generation efficiency in a low illuminance environment was improved compared to Comparative Example 2. [Industrial Applicability]
[0160] According to the present invention, in a power generating device having an active layer containing an organic-inorganic hybrid semiconductor compound, the power generating efficiency is improved under light irradiation, particularly in a low-illuminance environment such as indoors. [Explanation of symbols]
[0161] 1 Weatherproof protective film 2. UV protection film 3,9 Gas barrier film 4,8 Getter material film 5,7 Encapsulating materials 6. Solar cell elements (power generation devices) 10 Backsheet 12 Base material 13. Solar Cell Module 14 Thin-film solar cells 100 Power generation devices 101 Lower electrode 102 Buffer Layer 103 Active layer 104 Buffer Layer 105 Upper electrode 106 Base material
Claims
1. A hole transport material comprising: The conductivity of the spin-coated film of the hole transport material is 5×10 -6 S / cm or more 5×10 -4 S / cm or less, and The hole transport material, wherein the ionization potential of a spin-coated film of the hole transport material is −5.80 eV or more and less than −5.30 eV.
2. The hole transport material according to claim 1 , comprising at least two or more compounds.
3. Contains at least two or more compounds, The ionization potential of the first compound is −5.60 to −5.40 eV; 2. The hole transport material according to claim 1, wherein the second compound has an ionization potential of −5.25 to −5.05 eV.
4. Contains at least two or more compounds, the first compound is a compound having a carbazole skeleton, The hole transport material according to claim 1 , wherein the second compound is a spirotriarylamine compound having a fluorene skeleton.
5. Contains at least two or more compounds, The first compound is a compound having a carbazole skeleton represented by the following formula (I), A hole transport material, wherein the second compound is a spirotriarylamine compound having a fluorene skeleton represented by the following formula (II): [Formula 1] In formula (I), Ar 1 and Ar 2 R are each independently an aromatic group which may have a monovalent substituent, and the aromatic group may have a condensed ring structure. The monovalent substituent is an arbitrary substituent which replaces an arbitrary hydrogen atom of the aromatic group, and may be an alkyl group, an aromatic group, an alkoxy group, or a thioalkyl group. 1 , R 2, R 3 , R 4 , R 5 , R 6 are each independently a hydrogen atom, a halogen atom, or an alkyl group, an alkenyl group, an alkynyl group, an alkoxy group, an aryloxy group or an aromatic group which may have a substituent. In formula (II), Ar 3 are each independently an aromatic group which may have a monovalent substituent, and the aromatic group may have a condensed ring structure. The monovalent substituent is any substituent which substitutes any hydrogen atom of the aromatic group, and may be an alkyl group, an aromatic group, an alkoxy group, or a thioalkyl group.
6. further comprising a third compound; The hole transport material according to any one of claims 2 to 5, wherein the third compound is a compound capable of imparting charge by chemical reaction or by donating and receiving electrons.
7. 7. The hole transport material according to claim 6, wherein the ratio of the third compound is 0.001 to 70 parts by mass with respect to 100 parts by mass of the total of the first compound and the second compound.
8. further comprising a third compound; The hole transport material according to any one of claims 2 to 5, wherein the third compound is a diaryliodonium salt represented by the following formula (Q1): [Case 2] In formula (Q1), Ar 4 , Ar 5 , Ar 6 each independently represents an aromatic hydrocarbon group having 6 to 20 carbon atoms or a heteroaromatic hydrocarbon group having 2 to 20 carbon atoms, which may have a substituent.
9. further comprising a third compound; The hole transport material according to any one of claims 2 to 5, wherein the third compound comprises at least one selected from the group consisting of a compound represented by the following formula (Q2) and a compound represented by the following formula (Q3): [C3] In formula (Q3), R 7 , R 8 , R 9 , R 10 each independently represents a hydrogen atom, a halogen atom, or an alkyl group, an alkenyl group, an alkynyl group, an alkoxy group, an aryloxy group or an aromatic group which may have a substituent, and n is an integer of 0 to 5.
10. The hole transport material according to any one of claims 1 to 5, further comprising a solvent.
11. A hole transport layer comprising the hole transport material according to any one of claims 1 to 5.
12. 1. A power generation device, comprising: A pair of electrodes including an upper electrode and a lower electrode; an active layer located between the pair of electrodes and including an organic-inorganic hybrid semiconductor compound; a hole transport layer located between the pair of electrodes, A photoelectric conversion element, wherein the hole transport layer comprises the hole transport material according to any one of claims 1 to 5.
Citation Information
Patent Citations