Polystyrene-based resin foam plate for box and producing method thereof as well as box
The polystyrene resin foam board with tailored molecular weights and a non-foamed layer addresses processing challenges, enhancing flexibility and rigidity to produce complex folding boxes with reduced wrinkles and improved appearance.
Patent Information
- Application Number
- JP2023057228
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Polystyrene resin foam boards used for folding boxes face challenges in processing suitability and aesthetics, particularly when forming complex shapes, leading to issues like wrinkles and poor appearance.
A polystyrene resin foam board with specific molecular weight distributions (Mn, Mw, Mz) and a non-foamed layer, utilizing recycled materials and controlled foaming processes to enhance flexibility and rigidity, ensuring a broad molecular weight distribution towards the lower side.
The solution improves processing suitability, reduces wrinkles, and maintains bending strength, resulting in aesthetically pleasing and functional folding boxes.
Smart Images

Figure 2024145011000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a polystyrene-based resin foam board for folding boxes, a method for producing the same, and a folding box. [Background technology]
[0002] A known type of folding box has a container body with an opening at the top and a lid that closes the opening of the container body. The container body has, for example, a bottom plate that is approximately rectangular in plan view, two side plates rising from two opposing sides of the bottom plate, and two end plates rising from the other two sides of the bottom plate (the members formed by the side plates and end plates are sometimes called "peripheral side plates"), and has a rectangular parallelepiped shape as a whole. Alternatively, the container body has a bottom plate that is circular in plan view and peripheral side plates rising from the periphery of the bottom plate, and has a cylindrical shape as a whole.
[0003] The base material for the folding box is a polystyrene-based resin foam board having a foamed layer of polystyrene-based resin and a non-foamed layer on one or both sides of the foamed layer. This polystyrene-based resin foam board is folded or curved to form a folding box. When polystyrene foam boards are molded into folding boxes, wrinkles on the folded edges or curved surfaces result in poor appearance. In response to these problems, a polystyrene-based resin foam board has been proposed in which the ratio of the average cell diameter in the MD direction to the average cell diameter in the TD direction is within a specific range, and the thickness of the skin layer on either the front or back of the sheet is within a specific range (Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 5478320 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the shapes of folding boxes are becoming more complex, so there is a demand for polystyrene foam boards for folding boxes to have improved processability and to make folding boxes of complex shapes look beautiful. SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide a polystyrene-based resin foam board for folding boxes having improved processability. [Means for solving the problem]
[0006] <1> A foam layer is provided. The foam layer contains a polystyrene-based resin, The polystyrene resin has a number average molecular weight (Mn) of 75,000 to 105,000; The polystyrene resin has a mass average molecular weight (Mw) of 200,000 to 320,000; The Z-average molecular weight (Mz) of the polystyrene resin is 450,000 to 600,000; a molecular weight distribution (Mw / Mn) obtained by dividing the mass average molecular weight (Mw) of the polystyrene resin by the number average molecular weight (Mn) of the polystyrene resin is 2.78 to 3.20; A polystyrene-based resin foam board for folding boxes, wherein the molecular weight distribution (Mz / Mw) obtained by dividing the Z-average molecular weight (Mz) of the polystyrene-based resin by the mass-average molecular weight (Mw) of the polystyrene-based resin is 1.80 to 2.20. <2> The polystyrene-based resin includes a reduced molecular weight polystyrene-based resin, The molecular weight reduced polystyrene resin is at least one selected from recycled raw materials and polystyrene resins that have been subjected to molecular weight reduction processing in advance by heat melting treatment. <1> The polystyrene-based resin foam board for folding boxes described in the above. <3> The content of the molecular weight reduced polystyrene resin is 10 to 100% by mass based on the total mass of the polystyrene resin. <2> The polystyrene-based resin foam board for folding boxes described in the above. <4> A non-foamed layer is provided on one or both sides of the foamed layer. <1> ~ <3> The polystyrene-based resin foam board for folding boxes according to any one of the preceding claims. <5> <1> ~ <4> A folding box having the polystyrene-based resin foam board for folding boxes according to any one of claims 1 to 5.
[0007] <6> <1> ~ <5> A method for producing a polystyrene-based resin foam board for folding boxes according to any one of the above claims, A step of extruding a foamable resin composition containing a raw material polystyrene-based resin and a foaming agent into a plate shape and foaming the composition to obtain a foamed sheet; a step of subjecting the foamed sheet to secondary foaming to form the foamed layer; A method for producing a polystyrene-based resin foam board for folding boxes, comprising the steps of: Effect of the Invention
[0008] The polystyrene-based resin foam board of the present invention can improve processability. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a cross-sectional view of a polystyrene-based resin foam board for folding boxes according to one embodiment of the present invention. [Diagram 2] FIG. 1 is a schematic diagram showing an example of an apparatus for producing a polystyrene-based resin foam board for folding boxes according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] (Polystyrene resin foam board for folding boxes) The polystyrene-based resin foam board for folding boxes of the present invention (hereinafter, simply referred to as "foam board") has a foam layer containing a polystyrene-based resin. The foam board may have a single-layer structure consisting of a foam layer alone, or a multi-layer structure having a non-foamed layer on one or both sides of the foam layer. Hereinafter, the foam board of the present invention will be described with reference to one embodiment.
[0011] A foamed board 2A in FIG. 1 has a foamed layer 22 and a non-foamed layer 21 located on one side of the foamed layer 22.
[0012] The thickness T1 of the foamed board 2A is not particularly limited, but is preferably 2.0 to 5.5 mm, more preferably 2.2 to 5.3 mm, and even more preferably 2.4 to 5.2 mm. When the thickness T1 is equal to or greater than the lower limit, the strength of the resulting folding box can be increased. When the thickness T1 is equal to or less than the upper limit, the flexibility of the foamed board 2A can be increased, and the workability during folding and other processes can be improved. The thickness T1 is determined as an average value of measurements taken at any ten points in the TD direction of the foamed board 2A using a thickness measuring device SM-114 (manufactured by TECLOCK).
[0013] The basis weight of the foam board 2A is not particularly limited, but is 180 to 350 g / m 2 is preferable, and 200 to 330 g / m 2 More preferably, 210 to 310 g / m 2 It is more preferable that the foam board 2A has a basis weight of not less than the lower limit, so that the rigidity of the folding box can be further increased. If the basis weight of the foam board 2A is not more than the upper limit, the flexibility of the foam board 2A can be increased, so that the suitability for processing such as bending can be further increased.
[0014] <Foam layer> The foam layer 22 is a layer formed by foaming a resin composition (foamable resin composition) containing a resin (the resin constituting the foam layer may be referred to as a "foam layer resin") and a foaming agent. The foam layer resin includes a polystyrene-based resin.
[0015] Thickness T of the foam layer 22 22 Although not particularly limited, the thickness T is preferably 2.0 to 5.5 mm, more preferably 2.2 to 5.3 mm, and further preferably 2.4 to 5.2 mm. 22 When the thickness T is equal to or greater than the lower limit, the rigidity of the folding box can be further increased. 22 When the thickness T is equal to or less than the upper limit, the flexibility of the foamed plate 2A is increased, and the processability when bending or curving the plate can be improved. 22 The method for measuring thickness T1 is the same as that for measuring thickness T1.
[0016] The expansion ratio of the foamed layer 22 is not particularly limited, but is preferably 8.0 to 29.0 times, more preferably 9.0 to 27.0 times, and even more preferably 10.1 to 25.0 times. When the expansion ratio is equal to or greater than the lower limit, the rigidity of the folding box can be further increased. When the expansion ratio is equal to or less than the upper limit, the flexibility of the foamed board 2A is increased, and the processability when bending or curving can be further improved. The expansion ratio is calculated by dividing 1 by the apparent density (g / cm) of the foamed layer 22. 3 ) is the value divided by Apparent density is mass (g) ÷ apparent volume (cm 3 ) is calculated by
[0017] The basis weight of the foam layer 22 is, for example, 140 to 300 g / m 2 is preferable, and 145 to 280 g / m 2 More preferably, 150 to 270 g / m 2 It is more preferable that the basis weight is equal to or more than the lower limit, the rigidity of the folding box can be further increased. If the basis weight is equal to or less than the upper limit, the flexibility of the foamed board 2A can be increased, and the workability when bending or curving can be further increased.
[0018] The average bubble diameter of the foamed layer 22 is, for example, preferably 60 to 650 μm, more preferably 80 to 550 μm, and even more preferably 100 to 500 μm. When the average bubble diameter of the foamed layer 22 is equal to or greater than the above lower limit, the impact resistance of the folding box can be improved. When the average bubble diameter of the foamed layer 22 is equal to or less than the above upper limit, the smoothness of the surface of the foamed layer 22 can be improved. The average cell diameter of the foam layer 22 can be measured in accordance with the method described in ASTM D2842-69.
[0019] The closed cell ratio of the foamed layer 22 is preferably 70% or more, more preferably 80% or more, even more preferably 90% or more, and may be 100%. The closed cell ratio of the foamed layer 22 can be measured in accordance with the method described in JIS K7138:2006 "Rigid foamed plastics - Determination of open cell ratio and closed cell ratio."
[0020] Examples of the polystyrene resin constituting the foam layer resin include homopolymers or copolymers of styrene monomers, copolymers of styrene monomers and other vinyl monomers, and mixtures of these. The polystyrene resin preferably contains structural units based on styrene monomers in an amount of 50% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more, of the total structural units of the polystyrene resin.
[0021] Examples of the homopolymers or copolymers of the styrene-based monomers include homopolymers or copolymers of styrene-based monomers such as styrene, α-methylstyrene, vinyltoluene, chlorostyrene, ethylstyrene, i-propylstyrene, dimethylstyrene, bromostyrene, etc. Among these, those having 50% by mass or more of structural units based on styrene relative to the total structural units are preferred, and polystyrene is more preferred. Moreover, as the polystyrene-based resin, high impact polystyrene containing a rubber component may be used.
[0022] Examples of copolymers of styrene-based monomers and other vinyl-based monomers include styrene-(meth)acrylic acid ester copolymers, styrene-vinyl chloride copolymers, styrene-butadiene copolymers, styrene-acrylonitrile copolymers, styrene-maleic anhydride copolymers, styrene-maleic acid ester copolymers, styrene-fumaric acid ester copolymers, styrene-divinylbenzene copolymers, and styrene-alkylene glycol dimethacrylate copolymers. In this specification, (meth)acrylic acid means acrylic acid or methacrylic acid.
[0023] As the copolymer of a styrene-based monomer and another vinyl-based monomer, it is preferable that the copolymer contains structural units based on the styrene-based monomer in an amount of 50% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more, of the total structural units of the copolymer.
[0024] As the copolymer of a styrene-based monomer and another vinyl-based monomer, a styrene-(meth)acrylic acid ester copolymer is preferable. As the styrene-(meth)acrylic acid ester copolymer, a styrene-methyl acrylate copolymer, a styrene-ethyl acrylate copolymer, a styrene-butyl acrylate copolymer, a styrene-methyl methacrylate copolymer, a styrene-ethyl methacrylate copolymer, and a styrene-butyl methacrylate copolymer are preferable, and a styrene-butyl acrylate copolymer is more preferable. The styrene-(meth)acrylic acid ester copolymer preferably has a mass content of structural units based on a (meth)acrylic acid ester in the copolymer of 1 to 14 mass%, more preferably 1 mass% or more and less than 14 mass%, and even more preferably 4 to 10 mass%.
[0025] The number average molecular weight (Mn) of the polystyrene resin is 75,000 to 105,000, preferably 76,000 to 104,000, and more preferably 77,000 to 103,000. When the number average molecular weight (Mn) is equal to or greater than the lower limit, the flexural strength of the foamed layer 22 can be increased. When the number average molecular weight (Mn) is equal to or less than the upper limit, the flexibility of the foamed layer 22 can be increased, and the processability can be improved.
[0026] The mass average molecular weight (Mw) of the polystyrene resin is 200,000 to 320,000, preferably 205,000 to 317,000, and more preferably 208,000 to 315,000. When the mass average molecular weight (Mw) is equal to or greater than the lower limit, the bending strength of the foamed layer 22 can be increased. When the mass average molecular weight (Mw) is equal to or less than the upper limit, the flexibility of the foamed layer 22 can be increased, and the processability can be improved.
[0027] The Z-average molecular weight (Mz) of the polystyrene resin is 450,000 to 600,000, preferably 455,000 to 595,000, and more preferably 460,000 to 590,000. When the Z-average molecular weight (Mn) is equal to or greater than the lower limit, the flexural strength of the foamed layer 22 can be increased. When the Z-average molecular weight (Mz) is equal to or less than the upper limit, the flexibility of the foamed layer 22 can be increased, and the processability can be improved.
[0028] The molecular weight distribution (Mw / Mn) obtained by dividing the mass average molecular weight (Mw) of the polystyrene resin by the number average molecular weight (Mn) of the polystyrene resin is 2.78 to 3.20, preferably 2.79 to 3.19, and more preferably 2.80 to 3.18. When Mw / Mn is equal to or greater than the lower limit, the flexibility of the foamed layer 22 can be increased, and the processability can be improved. When Mw / Mn is equal to or less than the upper limit, the bending strength of the foamed layer 22 can be increased.
[0029] The molecular weight distribution (Mz / Mw) obtained by dividing the Z-average molecular weight (Mz) of the polystyrene resin by the mass-average molecular weight (Mw) of the polystyrene resin is 1.80 to 2.20, preferably 1.83 to 2.18, and more preferably 1.85 to 2.16. When Mz / Mw is equal to or greater than the lower limit, the bending strength of the foamed layer 22 can be increased. When Mz / Mw is equal to or less than the upper limit, the flexibility of the foamed layer 22 can be increased, thereby improving processability.
[0030] When the number average molecular weight (Mn), mass average molecular weight (Mw) and Z average molecular weight (Mz) of the polystyrene resin satisfy the above-mentioned relationship, the molecular weight distribution of the polystyrene resin becomes broader toward the lower molecular weight side than the mode value. Such a molecular weight distribution increases the flexibility of the foamed layer 22, improves the workability of the foamed board 2A, and maintains the bending strength required for folding boxes.
[0031] The scum average molecular weight (Mn), mass average molecular weight (Mw) and Z average molecular weight (Mz) of the polystyrene resin are values measured by GPC (gel permeation chromatography) and converted based on a calibration curve using standard polystyrene.
[0032] The polystyrene resin may contain a molecular weight reduced polystyrene resin. By containing the molecular weight reduced polystyrene resin, the molecular weight of the polystyrene resin can be more easily adjusted to a desired distribution. The molecular weight reduced polystyrene resin is at least one selected from recycled raw materials and polystyrene resins that have been previously subjected to molecular weight reduction processing by heat melting treatment (heat melted PS). The recycled raw materials are subjected to heat melting treatment during the manufacturing process, so there is an increase in polymers with smaller molecular weights than the polystyrene resin used as the raw material. Also, heat melting PS is subjected to heat melting treatment, so there is an increase in polymers with smaller molecular weights than before the heat melting treatment. By including such molecular weight reduced polystyrene resin, the polystyrene resin in the foam layer resin has a broad distribution on the low molecular weight side.
[0033] The recycled raw material can be a polystyrene-based resin foam obtained by recycling used polystyrene-based foam boards, polystyrene-based resin foam molded products (food packaging trays, etc.), etc. Examples of the recycled raw material include recycled raw materials obtained by collecting used polystyrene-based foam boards and polystyrene-based resin foam molded products and regenerating them using a limonene dissolution method or a heat volume reduction method.
[0034] An example of the heat-melted PS is a commercially available polystyrene resin that is heated and melted in an extruder, extruded, and repelletized. The heating temperature in the extruder is appropriately determined taking into consideration the type of polystyrene resin, and is preferably 200 to 320°C, for example. When the heating temperature is equal to or higher than the lower limit, the average molecular weight of the resulting heat-melted PS can be made smaller. When the heating temperature is equal to or lower than the upper limit, the molecular weight reduction process can be performed more efficiently.
[0035] The content of the reduced molecular weight polystyrene resin in the foam layer 22 is preferably 10 to 100 mass %, more preferably 30 to 100 mass %, and even more preferably 50 to 100 mass %, based on the total mass of the polystyrene resin in the foam layer resin. When the content of the reduced molecular weight polystyrene resin is equal to or more than the above lower limit, the molecular weight distribution of the polystyrene resin can be more easily adjusted.
[0036] As the polystyrene resin, in addition to the molecular weight reduced polystyrene resin, commercially available polystyrene resin, polystyrene resin synthesized by suspension polymerization method or the like, and polystyrene resin (virgin polystyrene) that is not a recycled raw material can be used.
[0037] When the molecular weight reduced polystyrene resin is used as the foam layer resin, the average molecular weight of the molecular weight reduced polystyrene resin is measured in advance to confirm the molecular weight distribution before production. Depending on the state of the molecular weight distribution of the molecular weight reduced polystyrene resin, the molecular weight distribution is adjusted by appropriately combining with virgin polystyrene or other molecular weight reduced polystyrene resins.
[0038] The foam layer resin may contain a resin other than the polystyrene resin, so long as the polystyrene resin is the main component. The range in which the polystyrene resin is the main component means a range in which the content of the polystyrene resin is 50% by mass or more relative to the total mass (100% by mass) of the foam layer resin. The content of the polystyrene resin is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and particularly preferably 100% by mass, relative to the total mass of the foam layer resin.
[0039] Examples of foam layer resins other than polystyrene-based resins include polyethylene-based resins, polypropylene-based resins, polybutadiene-based resins, ethylene-propylene-non-conjugated diene three-dimensional copolymers, acrylic-based resins, and polyphenylene ether-based resins.
[0040] The blowing agent is, for example, a hydrocarbon such as propane, butane, or pentane; or a halogenated hydrocarbon such as tetrafluoroethane, chlorodifluoroethane, or difluoroethane. Among them, butane is preferable. The butane may be normal butane or isobutane alone, or a combination of normal butane and isobutane. These foaming agents may be used alone or in combination of two or more. The amount of foaming agent to be mixed is determined taking into consideration the type of foaming agent and the overall density required for the foam layer 22. The content of the foaming agent is preferably 1.0 to 7.0 parts by mass with respect to 100 parts by mass of the foam layer resin.
[0041] In addition to the foam layer resin and the foaming agent, additives such as a foam nucleating agent (cell regulator), crosslinking agent, filler, flame retardant, flame retardant assistant, lubricant (hydrocarbon, fatty acid, fatty acid amide, ester, alcohol, metal soap, silicone oil, wax such as low molecular weight polyethylene, etc.), spreading agent (liquid paraffin, polyethylene glycol, polybutene, etc.), colorant (pigment, etc.) may be added to the foam layer 22. Among them, it is preferable that the foam board of the present invention contains a foam nucleating agent.
[0042] Examples of the foaming nucleating agent include talc, sodium hydrogen carbonate, ammonium hydrogen carbonate, calcium carbonate, clay, citric acid, etc. Among these, talc is preferable. The cell regulator may be used alone or in combination of two or more kinds. The amount of the cell regulator added is preferably 0.01 to 5 parts by mass with respect to 100 parts by mass of the foamed layer resin.
[0043] <Non-foamed layer> The foamed board 2A may have a non-foamed layer 21. By having the non-foamed layer 21, the foamed board 2A can have a smoother surface when made into a folding box, thereby increasing the strength of the folding box.
[0044] Thickness T of the non-foamed layer 21 21 is determined taking into consideration the use of the foamed sheet, and is, for example, preferably 5 to 100 μm, more preferably 10 to 80 μm, and further preferably 15 to 60 μm. 21 When the thickness T is equal to or greater than the lower limit, the strength of the folded box can be further increased, the surface of the folded box can be made smoother, and the strength of the folded box can be further increased. 21 When the thickness T is equal to or less than the upper limit, the weight of the folding box can be reduced. 21 is the thickness from T1 to T 22 Calculate by subtracting .
[0045] Examples of the resin constituting the non-foamed layer 21 (non-foamed layer resin) include polystyrene-based resin, polyolefin-based resin, polyamide-based resin, polyester-based resin, ethylene vinyl alcohol resin (EVOH), etc. The polystyrene-based resin of the non-foamed layer resin is the same as the polystyrene-based resin of the foamed layer resin. The polystyrene-based resin of the non-foamed layer resin may be the same as or different from the polystyrene-based resin of the foamed layer resin.
[0046] In addition to the non-foamed layer resin, the non-foamed layer 21 may contain additives such as crosslinking agents, fillers, flame retardants, flame retardant assistants, lubricants (hydrocarbons, fatty acids, fatty acid amides, esters, alcohols, metal soaps, silicone oils, waxes such as low molecular weight polyethylene, etc.), spreading agents (liquid paraffin, polyethylene glycol, polybutene, etc.), colorants (pigments, etc.), etc.
[0047] The non-foamed layer 21 may have a single-layer structure or a multi-layer structure of two or more layers. When the non-foamed layer 21 has a multi-layer structure, for example, the non-foamed layer 21 may be a laminated film in which a polyolefin resin film or the like is dry-laminated on a polystyrene resin film. When the non-foamed layer 21 is a laminated film, examples of the polyolefin resin film to be dry laminated include high-density polyethylene resin (HDPE) film, polystyrene film (OPS, CPS), polypropylene resin (PP) film, cycloolefin polymer (COP) film, and cycloolefin copolymer (COC) film.
[0048] The resin film constituting the non-foamed layer 21 may be any of a non-stretched film, a weakly stretched film, a uniaxially stretched film, and a biaxially stretched film.
[0049] A printed layer may be provided on the surface of the non-foamed layer 21, or a non-foamed layer may be further provided on the surface of the printed layer. Alternatively, a printed layer may be provided between the non-foamed layer 21 and the foamed layer 22.
[0050] (Method of manufacturing foam board) The foam board is produced by a conventionally known production method. 2 is an apparatus for obtaining a foamed sheet by extrusion molding. The manufacturing apparatus 1 includes an extruder 10, a foaming agent supply source 18, a circular die 20, a mandrel 30, and two winders 40. The extruder 10 is a so-called single-type extruder. The extruder 10 includes a hopper 14. A foaming agent supply source 18 is connected to the extruder 10. A circular die 20 is connected to the extruder 10. A mandrel 30 equipped with a cutter 32 is provided downstream of the circular die 20. A cooling blower (not shown) is provided between the circular die 20 and the mandrel 30. The extruder 10 of the production apparatus 1 may be an extruder other than a single type extruder, or may be a so-called tandem type extruder. Moreover, the extruder 10 of the production apparatus 1 may be a single screw extruder, or may be a multi-screw extruder such as a twin screw extruder.
[0051] The raw materials constituting the foam layer (foam layer resin, optional foam layer components) are fed into extruder 10 from hopper 14. The raw materials for the foam layer resin (i.e., raw material resins including raw material polystyrene-based resin) are the same as those for the foam layer resin. In the extruder 10, the raw materials are mixed while being heated to a given temperature to form a resin melt, and a foaming agent is supplied to the extruder 10 from a foaming agent supply source 18, and the foaming agent is mixed with the resin melt to form a foamable resin composition. The heating temperature is appropriately determined in consideration of the type of resin, etc., so long as the resin melts and the optional components are not denatured.
[0052] The foamable resin composition is further mixed in the extruder 10. The foamable resin composition is brought to a given temperature and then guided to a resin flow path in a circular die 20. The foamable resin composition guided to the resin flow path is discharged from the discharge port of the circular die 20, and the foaming agent foams to form a cylindrical foamed sheet 2a (extrusion foaming step). The cylindrical foamed sheet 2a is guided to the mandrel 30 while being blown with cooling air sent from a cooling blower. The cylindrical foamed sheet 2a passes over the outer surface of the mandrel 30, is cooled to a given temperature, becomes a foamed and cured product, and is cut into two pieces by a cutter 32 to become the foamed sheet 2 (cutting step). The foamed sheet 2 is passed around a guide roll 42 and a guide roll 44, and is taken up by a winder 40 to become the foamed sheet roll 4.
[0053] The shear rate for the foamable resin composition at the discharge port of the circular die 20 is 7500 s -1 Less than 6500s is preferred -1 Less than 6000 is preferable. -1 The following are even more preferred:
[0054] Next, the foamed sheet 2a is unwound from the foamed sheet roll 4 and heated for secondary foaming to form a foamed board for folding boxes (secondary foaming step). Examples of the heating method for secondary foaming include a method of heating the foamed sheet 2a in a tunnel-type electric heating furnace, a method of sandwiching the foamed sheet 2a between heating plates and heating them, etc. The heating temperature for the foamed sheet 2a is, for example, 150 to 200°C.
[0055] When providing a non-foamed layer on a foam board, a resin film may be heat-sealed to the foam sheet 2a and then secondary foaming may be performed, or a resin film may be heat-sealed to the secondary foamed foam board.
[0056] (Folded box) The folding box of the present invention includes the foam board of the present invention. The folding box may be composed only of the foam board of the present invention, or only a part of the folding box may be composed of the foam board of the present invention.
[0057] An example of a folding box is one having a container body and a lid body that closes the opening of the container body. The container body may have any configuration as long as it has a flat bottom plate and peripheral side plates rising from the peripheral edge of the bottom plate. The shape of the container body is not particularly limited, and may be a polygonal tube with a bottom or a cylindrical tube with a bottom.
[0058] The bottomed polygonal cylindrical container body can be manufactured by a conventional method. A pressed line or a groove is formed by cutting at the boundary between the bottom plate, which is polygonal in plan view, and the side plate and end plate, and the container body is manufactured by folding along the line or groove. In this case, since the foamed board of the present invention has excellent flexibility and high processability, the occurrence of deformation such as folds, wrinkles, distortions, or cracks near the folded edges is suppressed. Therefore, the surface of the manufactured folding box is beautiful.
[0059] The cylindrical container body with a bottom can be manufactured by a conventional method. A long foamed board is curved to form an annular peripheral plate, and a circular bottom plate is attached to one of the openings of the annular peripheral plate to manufacture the cylindrical container body with a bottom. In this case, the foamed board of the present invention has excellent flexibility and high processability, so that the curved surface is prevented from wrinkles or distortion. Therefore, the surface of the manufactured folding box is beautiful.
[0060] As described above, the foamed board of the present invention has excellent processability, and therefore deformation such as folds, wrinkles, warping, and cracks is suppressed in the resulting folding box. In addition, the foam plate of the present invention has the bending strength required for folding boxes. Furthermore, the present invention makes it possible to effectively utilize recycled materials, reduce the amount of plastic used, and reduce the environmental burden. EXAMPLES
[0061] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples.
[0062] (Raw materials used) <Polystyrene resin> PS-1: Product name "HRM-26", general-purpose polystyrene (GPPS), manufactured by Toyo Styrene Co., Ltd. PS-2: Product name "HRM-10N", general-purpose polystyrene (GPPS), manufactured by Toyo Styrene Co., Ltd. PS-3: Product name "HRM-48N", general-purpose polystyrene (GPPS), manufactured by Toyo Styrene Co., Ltd. PS-4: Product name "HRM-18", general-purpose polystyrene (GPPS), manufactured by Toyo Styrene Co., Ltd. ·PS-5: Recycled polystyrene resin material.
[0063] <Foaming agent> Butane: isobutane / normal butane = 70 / 30 (mass ratio).
[0064] <Other> Pigment: Product name "ESH-K-4799LB", manufactured by Polycol Corporation. Foaming nucleating agent: Product name "MO-60-SH-HC", manufactured by Kihara Chemical Co., Ltd.
[0065] (Measurement method) <Molecular weight of polystyrene resin> The method for measuring the Z-average molecular weight Mz of the polystyrene resin in the foam board is described below. The mass-average molecular weight Mw of the polystyrene resin and the number-average molecular weight Mn of the polystyrene resin were measured in the same manner as the Z-average molecular weight Mz of the polystyrene resin. The foamed board of each example was cut with a slicer or a razor to be collected as a sample. The sample was pretreated to obtain a filtrate under the following measurement conditions, and the Z-average molecular weight Mz of the polystyrene resin was measured.
[0066] <Measurement conditions> [Preprocessing] 6 mg of the collected sample was dissolved in 6 mL of tetrahydrofuran (THF) (immersion time: 6±1 hr (complete dissolution)) to obtain a sample solution. The sample solution was filtered with a non-aqueous 0.45 μm syringe filter manufactured by Shimadzu GLC Co., Ltd. to obtain a filtrate. The filtrate obtained in the above pretreatment was used to measure the Z-average molecular weight Mz of the polystyrene resin with the following measuring device under the following measuring conditions.
[0067] [Measuring equipment] GPC equipment: Tosoh Corporation, HLC-8320GPC (built-in RI detector and UV detector). Guard column: TOSOH TSK guard column SuperMP(HZ)-H (4.6mm I.D. x 2cm) x 1. Column (reference): TOSOH TSKgel Super HZ1000 (6.0mm I.D. x 15cm) x 1. Column (sample): TSKgel SuperMultiporeHZ-H (4.6mm I.D. x 15cm) x 2 in series.
[0068] [Measurement conditions] Column temperature: 40°C. Detector temperature: 40℃. Pump injection temperature: 40℃. Solvent: THF (Tetrahydrofuran). Flow rate (reference): 0.2mL / min. Flow rate (sample): 0.2mL / min. Run Time: 21 min. Data collection time: 6~25min. -Data interval: 200msec. ·Injection volume: 20μL. Detector: RI.
[0069] [Standard polystyrene sample for calibration curve] The standard polystyrene samples used for the calibration curve were "STANDARD SM-105" and "STANDARD SH-75" manufactured by Showa Denko K.K., and had mass average molecular weights Mw of 5,620,000, 3,120,000, 1,250,000, 442,000, 151,000, 53,500, 17,000, 7,660, 2,900, and 1,320. The above-mentioned standard polystyrene for the calibration curve was grouped into A (5,620,000, 1,250,000, 151,000, 17,000, 2,900) and B (3,120,000, 442,000, 53,500, 7,660, 1,320). A was weighed (2 mg, 3 mg, 4 mg, 4 mg, 4 mg) and dissolved in 30 mL of THF. B was weighed (3 mg, 4 mg, 4 mg, 4 mg, 4 mg) and dissolved in 30 mL of THF. The standard polystyrene calibration curve was obtained by injecting 20 μL of each of the prepared A and B solutions and creating a calibration curve (linear equation) from the retention time obtained after measurement. The Z-average molecular weight (Mz) was calculated using the calibration curve.
[0070] <Bending strength> The bending strength was measured using a Tensilon universal testing machine "RTC-1310A" manufactured by Orientec Co., Ltd. The test pieces were cut to a size of 50 mm wide x 150 mm long x thickness (thickness of each example) in the extrusion direction (MD direction) and the direction perpendicular to the extrusion direction (TD direction). The number of test pieces was three for each direction. The measurement conditions were a test speed of 50 mm / min, a radius of the tip of the pressure wedge and the fulcrum of 3.2R, and a distance between the fulcrums of 100 mm. Three-point bending measurement was performed for each test piece, and the maximum point load was taken as the bending strength (N) of the foam board. Next, the average value (N) of the bending strength (N) in the MD direction and the bending strength (N) in the TD direction was used to make a judgment based on the following evaluation criteria.
[0071] Evaluation Criteria A: The average bending strength is 10N or more...The bending strength is extremely high and excellent. B: The average bending strength is 9N or more but less than 10N...The bending strength is low, but acceptable. C: Average bending strength value is less than 9N...Bending strength is extremely low and poor.
[0072] <Break> The foamed board of each example was cut into a rectangular shape with a width of 55 mm and a length of 510 mm, with the MD direction being the short side direction and the TD direction being the long side direction. Along the short side direction of the cut foamed board, vertical grooves with a width of 4 mm and a depth of 1 mm were made along the short side direction at positions 35 mm and 235 mm from one end in the long side direction to make a sample. Thereafter, the sample was bent into a ring shape, and both ends were heat-sealed to make a peripheral side plate, and an elliptical bottom plate with a major axis of 183 mm, a minor axis of 133 mm, and a circumference of 502 mm was inserted into the peripheral side plate to make a container consisting of the peripheral side plate and the bottom plate. Note that both ends of the heat-sealed peripheral side plate were overlapped in the minor axis direction of the bottom plate. The folding angle of the grooved portion of the peripheral side of this container was measured with a protractor. The evaluation criteria were as follows.
[0073] Evaluation Criteria A (no break): 163° or more. B (Bent): Less than 163°.
[0074] <Wrinkles> The containers produced for the evaluation of "folding" above were visually observed for the occurrence of wrinkles on the inner surface of the peripheral plate. The evaluation criteria were as follows:
[0075] Evaluation Criteria A (no wrinkles): There are absolutely no wrinkles on the curved inner surface. B (Wrinkled): There are one or more wrinkles on the inner curved surface.
[0076] <Appearance> The appearance of each foam plate was visually observed and evaluated according to the following criteria. A (No problem): No unevenness or lines on appearance. B (Problematic): There are irregularities or lines in the appearance.
[0077] <Overall rating> The evaluation was performed according to the following evaluation criteria. Evaluation Criteria A: The bending strength, folding, wrinkles and appearance are all rated as "A". B: One of the evaluations of bending strength, creases, wrinkles, and appearance is other than "A". C: Two of the evaluations of bending strength, creases, wrinkles, and appearance are other than "A". D: Three of the evaluations of bending strength, creases, wrinkles, and appearance are other than "A". E: Four of the evaluations of bending strength, creases, wrinkles, and appearance were other than "A".
[0078] (Examples 1 to 5, Comparative Examples 1 to 6) A foamed sheet was obtained as follows using a production apparatus similar to that shown in FIG. A tandem extruder in which an extruder with an inner diameter of 65 mm and an extruder with an inner diameter of 90 mm were connected was used as the extruder. According to the polystyrene resin formulation in Tables 1 to 2, 100 parts by mass of polystyrene resin, 1.36 parts by mass of foaming nucleating agent, and 2.7 parts by mass of pigment were fed to the extruder, melted at a maximum temperature of 264°C in the extruder, and kneaded to obtain a molten kneaded product. To the molten kneaded product, 6.3 parts by mass of foaming agent (total amount of resin is 100 parts by mass) was added, and further kneaded. Thereafter, the mixture was cooled to a resin temperature of 167.1°C suitable for foaming, to obtain a foamable resin composition. The extrusion rate was 100 kg / h and the shear rate was 626 s from the circular die (diameter 128 mm, slit clearance 0.75 mm) attached to the tip of the extruder. -1 The foamable resin composition was extruded at 1.4 m / s, foamed, and cooled to form a cylindrical foam sheet. 3 / min. The cylindrical foam sheet was cut with cutters on the left and right to make two foam sheets. Each foam sheet was stretched between multiple rolls and wound on a winding roll. During this winding, the take-up speed was set to 7.2 m / min in order to stretch the foam sheet in the MD direction. The dimension of the foam sheet in the TD direction was 690 mm. The foam sheet obtained was then passed through a tunnel-type electric heating furnace and electrically heated under conditions of a temperature of 178°C, a length of 3.5 m, and a moving speed of 27.04 m / min to cause secondary foaming, and then cut into a foam plate. The dimensions of the foam plate were 635 mm in the TD direction and 1365 mm in the MD direction. The resulting foamed board was evaluated for bending strength, folds, wrinkles, appearance and overall evaluation, and the results are shown in the table.
[0079] [Table 1]
[0080] [Table 2]
[0081] As shown in Tables 1 and 2, in Examples 1 to 6 in which the present invention was applied, no folds or wrinkles occurred, the appearance was good, and the overall evaluation was A. That is, the foam boards of Examples 1 to 6 were excellent in processability. In Comparative Example 1, in which the molecular weight distribution (Mz / Mw) of the polystyrene resin was 1.79, the bending strength was evaluated as "C" and the wrinkles and appearance were evaluated as "B." In Comparative Example 2, the molecular weight distribution (Mw / Mn) of the polystyrene resin was 3.39, and the evaluation of breakage was "B." In Comparative Example 3, in which the molecular weight distribution (Mw / Mn) of the polystyrene resin was 3.46 and Mz / Mw was 2.52, the evaluation of breakage was "B." Comparative Example 4, in which the polystyrene resin had a molecular weight distribution (Mw / Mn) of 2.72 and a molecular weight distribution (Mz / Mw) of 2.22, was rated "B" for bending strength, wrinkles and appearance, and "B" for wrinkles. In Comparative Example 5, in which the molecular weight distribution (Mz / Mw) of the polystyrene resin was 2.44, the evaluation of folding was "B." Comparative Example 6, in which the molecular weight distribution (Mw / Mn) of the polystyrene resin was 2.75, was evaluated as "B" in terms of bending strength, wrinkles and appearance. From these results, it was confirmed that application of the present invention can improve processability. [Explanation of symbols]
[0082] 2A Polystyrene resin foam board for folding boxes 21 Non-foamed layer 22 Foam layer
Claims
1. A foam layer is provided. The foam layer contains a polystyrene-based resin, The number average molecular weight (Mn) of the polystyrene resin is 75,000 to 105,000, The polystyrene resin has a mass average molecular weight (Mw) of 200,000 to 320,000; The Z-average molecular weight (Mz) of the polystyrene resin is 450,000 to 600,000; a molecular weight distribution (Mw / Mn) obtained by dividing the mass average molecular weight (Mw) of the polystyrene resin by the number average molecular weight (Mn) of the polystyrene resin is 2.78 to 3.20; The molecular weight distribution (Mz / Mw) obtained by dividing the Z-average molecular weight (Mz) of the polystyrene resin by the mass average molecular weight (Mw) of the polystyrene resin is 1.80 to 2.
20.
2. The polystyrene-based resin includes a reduced molecular weight polystyrene-based resin, The polystyrene-based resin foam board for folding boxes according to claim 1, wherein the molecular weight reduced polystyrene-based resin is at least one selected from recycled raw materials and polystyrene-based resins that have been subjected to molecular weight reduction processing in advance by heating and melting treatment.
3. The polystyrene-based resin foam board for folding boxes according to claim 2, wherein the content of the reduced molecular weight polystyrene-based resin is 10 to 100% by mass with respect to the total mass of the polystyrene-based resin.
4. 3. The polystyrene-based resin foam board for folding boxes according to claim 1 or 2, wherein a non-foamed layer is provided on one or both sides of the foamed layer.
5. A folding box comprising the polystyrene-based resin foam board for folding boxes according to claim 1 or 2.
6. A method for producing the polystyrene-based resin foam board for folding boxes according to claim 1, A step of extruding a foamable resin composition containing a raw material polystyrene-based resin and a foaming agent into a plate shape and foaming the composition to obtain a foamed sheet; a step of subjecting the foamed sheet to secondary foaming to form the foamed layer; A method for producing a polystyrene-based resin foam board for folding boxes, comprising the steps of:
Citation Information