Laminated sheet

The laminated sheet with polycarbonate layers and UV absorbers enhances weather resistance and durability, addressing the weaknesses of polycarbonate in outdoor applications.

JP2024145039APending Publication Date: 2024-10-15SUMITOMO BAKELITE CO LTD

Patent Information

Application Number
JP2023057267
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Polycarbonate materials used in transparent protective covers for electronic devices and outdoor building materials suffer from inferior surface hardness, abrasion resistance, and scratch resistance, leading to issues like deformation, discoloration, and deterioration when exposed to outdoor conditions.

Method used

A laminated sheet configuration comprising a first surface layer, an intermediate layer, and a second surface layer, where each layer includes polycarbonate, UV absorbers (such as triazine, benzoxazinone, benzotriazole, or benzophenone), and a lubricant, with specific content ratios and thicknesses to enhance weather resistance.

Benefits of technology

The laminated sheet provides improved weather resistance, maintaining transparency, impact resistance, and processability, while reducing scratch and abrasion, and preventing deformation and discoloration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145039000001_ABST
    Figure 2024145039000001_ABST
Patent Text Reader

Abstract

To provide a laminated sheet that containing polycarbonate and excellent in weather resistance.SOLUTION: There is provided a laminated sheet composed of a first surface layer, an intermediate layer, and a second surface layer, which are laminated in this order in a thickness direction of the laminated sheet. The first surface layer and the second surface layer comprise a polycarbonate, an ultraviolet absorber, and a lubricant. The ultraviolet absorber is one kind or two kinds or more selected from a group consisting of a triazine-based ultraviolet absorber, a benzoxazinone-based ultraviolet absorber, a benzotriazole-based ultraviolet absorber, and a benzophenone-based ultraviolet absorber. The intermediate layer contains a polycarbonate, a compound represented by a following general formula (I), a compound represented by a following general formula (II) or a compound represented by a following general formula (III), a lubricant, and a colorant.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminated sheet. [Background technology]

[0002] From the viewpoints of their light weight, transparency, processability, resistance to breakage, and safety in the event of breakage, various transparent plastic materials are used as protective covers for the exterior parts of portable devices, household electrical appliances, industrial electronic devices, automotive electronic devices, etc., particularly for information display parts such as monitors. In particular, polycarbonate resin materials are one of the most widely used materials due to their excellent transparency, impact resistance, heat resistance, and processability.

[0003] Patent Document 1 discloses a polycarbonate resin composition that is free from coloration and has excellent hydrolysis resistance, which is obtained by adding a pentaerythritol phosphite compound and a bisphenol organic cyclic phosphite compound or an organic phosphite compound to a polycarbonate resin. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2003-41108 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, polycarbonate has the disadvantage that it is inferior to glass in terms of surface hardness, abrasion resistance, and scratch resistance, and is easily scratched. When used as a material for outdoor buildings, polycarbonate has the problem of undergoing changes in its properties, such as deformation, discoloration, and deterioration.

[0006] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a laminate sheet which contains polycarbonate and has excellent weather resistance. [Means for solving the problem]

[0007] In order to solve the above problems, the present invention employs the following configuration. [1] A laminate sheet comprising a first surface layer, an intermediate layer, and a second surface layer, which are laminated in this order in a thickness direction, the first surface layer and the second surface layer each containing a polycarbonate, an ultraviolet absorber, and a lubricant, the ultraviolet absorber being one or more selected from the group consisting of a triazine-based ultraviolet absorber, a benzoxazinone-based ultraviolet absorber, a benzotriazole-based ultraviolet absorber, and a benzophenone-based ultraviolet absorber, and the intermediate layer containing a polycarbonate, a compound represented by the following general formula (I), a compound represented by the following general formula (II), or a compound represented by the following general formula (III), a lubricant, and a colorant:

[0008] [ka] (In formula (I), R 11 and R 12 are each independently a hydrogen atom, an alkyl group, or an aryl group.

[0009] [ka] (In formula (II), R 21 is an alkyl group having 1 to 4 carbon atoms; R 22 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms; R 23 is a fluorine atom or an alkoxy group having 1 to 30 carbon atoms.

[0010] [ka] (In formula (III), R 31 is an alkyl group having 1 to 20 carbon atoms; and n is an integer of 1 to 5. [2] The laminate sheet according to [1], wherein in the first surface layer, the content ratio of the ultraviolet absorber relative to the total mass of the first surface layer is 2 mass% or more, and in the second surface layer, the content ratio of the ultraviolet absorber relative to the total mass of the second surface layer is 2 mass% or more. [3] The laminate sheet according to [1] or [2], wherein the ratio of the thickness of the first surface layer to the thickness of the laminate sheet is 0.7% or more and 1.5% or less, and the ratio of the thickness of the second surface layer to the thickness of the laminate sheet is 0.7% or more and 1.5% or less. [4] The laminate sheet according to any one of [1] to [3], wherein the thickness of the laminate sheet is 1 mm or more and 20 mm or less. [5] The laminate sheet according to any one of [1] to [4], wherein the lubricant is one or more selected from the group consisting of fatty acid esters, hydroxy fatty acids, and polyethylene oxide. Effect of the Invention

[0011] According to the present invention, there is provided a laminate sheet which contains polycarbonate and has excellent weather resistance. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a cross-sectional view illustrating a schematic example of a laminate sheet according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] <<Laminated sheet>> A laminate sheet according to one embodiment of the present invention is a laminate sheet comprising a first surface layer, an intermediate layer, and a second surface layer laminated in this order in a thickness direction, the first surface layer and the second surface layer each containing a polycarbonate, an ultraviolet absorber, and a lubricant, the ultraviolet absorber being one or more selected from the group consisting of a triazine-based ultraviolet absorber, a benzoxazinone-based ultraviolet absorber, a benzotriazole-based ultraviolet absorber, and a benzophenone-based ultraviolet absorber, and the intermediate layer contains a polycarbonate, a compound represented by the following general formula (I), a compound represented by the following general formula (II), or a compound represented by the following general formula (III), a lubricant, and a colorant.

[0014] [ka] (In formula (I), R 11 and R 12 are each independently a hydrogen atom, an alkyl group, or an aryl group.

[0015] [ka] (In formula (II), R 21 is an alkyl group having 1 to 4 carbon atoms; R 22 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms; R 23 is a fluorine atom or an alkoxy group having 1 to 30 carbon atoms.

[0016] [ka] (In formula (III), R 31 is an alkyl group having 1 to 20 carbon atoms; and n is an integer of 1 to 5.

[0017] The present invention will be described in detail below with reference to the drawings. Note that the drawings used in the following description may show essential parts in an enlarged scale for the sake of convenience in order to make the features of the present invention easier to understand, and the dimensional ratios of each component may not necessarily be the same as in reality.

[0018] FIG. 1 is a cross-sectional view that illustrates an example of the laminate sheet of the present embodiment.

[0019] The laminate sheet 1 shown here is constructed by laminating a first surface layer 11, an intermediate layer 12, and a second surface layer 13 in this order in the thickness direction. Each layer will be described below.

[0020] <1st surface layer> The laminate sheet 1 has a first surface layer 11. The first surface layer 11 imparts transparency, impact resistance, heat resistance, and processability to the laminate sheet 1, as well as weather resistance.

[0021] First surface layer 11 contains polycarbonate, an ultraviolet absorbing agent, and a lubricant.

[0022] (Polycarbonate) First surface layer 11 includes polycarbonate. When first surface layer 11 contains polycarbonate, the transparency, impact resistance, heat resistance, and processability of laminate sheet 1 can be improved.

[0023] The polycarbonate is not particularly limited and various types can be used, but among them, aromatic polycarbonate resins are preferred.

[0024] The weight average molecular weight of the polycarbonate is preferably from 10,000 to 100,000, more preferably from 30,000 to 80,000, and further preferably from 40,000 to 60,000.

[0025] The polycarbonate contained in first surface layer 11 may be only one type, or may be two or more types. When two or more types are contained, the combination and ratio thereof can be arbitrarily selected depending on the purpose.

[0026] The polycarbonate can be produced by using a dihydric phenol compound as a raw material, by a known method such as a phosgene method, a chloroformate method, or a pyridine method.

[0027] The ratio of the polycarbonate content (parts by mass) in first surface layer 11 to the total mass (parts by mass) of first surface layer 11 ([polycarbonate content (parts by mass) of first surface layer 11)] / [total mass (parts by mass) of first surface layer 11)]×100) is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, and may be, for example, any one of 97% by mass or more and 99% by mass or more. When the ratio is equal to or more than the lower limit, the transparency, impact resistance, heat resistance and processability of first surface layer 11 and laminate sheet 1 can be further improved. On the other hand, the proportion is 99% by mass or less. The above ratio is usually the same as the ratio of the polycarbonate content (parts by mass) to the total content (parts by mass) of components that do not vaporize at room temperature in the resin composition for forming the surface layer described below ([polycarbonate content (parts by mass) in the resin composition for forming the surface layer)]) / [total content (parts by mass) of components that do not vaporize at room temperature in the resin composition for forming the surface layer)]×100).

[0028] (UV absorber) First surface layer 11 contains an ultraviolet absorbing agent in addition to polycarbonate. When the first surface layer 11 contains an ultraviolet absorbing agent, the weather resistance of the laminate sheet 1 can be improved.

[0029] Examples of the ultraviolet absorbing agent include triazine-based ultraviolet absorbing agents, benzoxazinone-based ultraviolet absorbing agents, benzotriazole-based ultraviolet absorbing agents, benzophenone-based ultraviolet absorbing agents, etc. Among these, triazine-based ultraviolet absorbing agents are preferred.

[0030] The ultraviolet absorbing agent contained in first surface layer 11 may be only one type, or may be two or more types. When there are two or more types, the combination and ratio thereof can be arbitrarily selected depending on the purpose.

[0031] The ultraviolet absorber may be present uniformly or non-uniformly in first surface layer 11. When present non-uniformly, the ultraviolet absorber is preferably unevenly distributed in a region on the surface side of first surface layer 11 opposite intermediate layer 12.

[0032] In first surface layer 11, the content of the ultraviolet absorbing agent relative to the total mass of first surface layer 11 is preferably 2 mass % or more, and more preferably 3 mass % or more and 10 mass % or less. When the ratio is equal to or more than the lower limit, it is possible to further improve the weather resistance of the laminate sheet 1. When the ratio is equal to or less than the upper limit, the excessive use of the ultraviolet absorbing agent is further suppressed.

[0033] (lubricant) First surface layer 11 contains a lubricant in addition to polycarbonate and an ultraviolet absorbing agent. When first surface layer 11 contains a lubricant, excellent slipperiness against a die, roller, etc. can be exhibited during extrusion molding of first surface layer 11, thereby improving moldability.

[0034] Examples of the lubricant include polyethylene oxide, fatty acid esters, hydroxy fatty acids, metal soaps, higher aliphatic alcohols, synthetic waxes, and the like. Among these, one or a combination of two or more can be used. Among them, polyethylene oxide, fatty acid esters, and hydroxy fatty acids are preferred.

[0035] Examples of the types of oxidized polyethylene include a highly oxidized type, a slightly oxidized type, and an acid-modified type.

[0036] The weight average molecular weight of the polyethylene oxide is preferably from 1000 to 3000, more preferably from 1500 to 2500, and even more preferably from 1800 to 2300. This can further improve the effect of the lubricant contained in the laminate sheet 1.

[0037] Examples of fatty acid esters include butyl stearate and triglycerides.

[0038] An example of the hydroxy fatty acid is hydroxystearic acid.

[0039] The lubricant is preferably present uniformly in first surface layer 11.

[0040] In the first surface layer 11, the content of the lubricant relative to the total mass of the first surface layer 11 is preferably 0.0005 mass% or more and 5.0 mass% or less, more preferably 0.01 mass% or more and 3.0 mass% or less, and even more preferably 0.05 mass% or more and 2.0 mass% or less. When the ratio is equal to or greater than the lower limit, excellent slippage against a die, roller, etc. can be exhibited during extrusion molding of first surface layer 11, thereby further improving moldability. When the ratio is equal to or less than the upper limit, excessive use of the lubricant can be further suppressed.

[0041] (Other ingredients) The first surface layer 11 may contain only polycarbonate, an ultraviolet absorber, and a lubricant (i.e., it may consist of polycarbonate, an ultraviolet absorber, and a lubricant), or it may contain polycarbonate, an ultraviolet absorber, a lubricant, and other components (sometimes referred to as "other components" in this specification) (i.e., it may consist of polycarbonate, an ultraviolet absorber, a lubricant, and the other components).

[0042] The other components contained in first surface layer 11 are not particularly limited and can be arbitrarily selected depending on the purpose, and may be, for example, either a resin component or a non-resin component. The other component, which is a resin component, is a resin other than polycarbonate. The other component, which is a resin component, may be a homopolymer, which is a polymer of one type of monomer, or a copolymer, which is a polymer of two or more types of monomers.

[0043] Examples of the other components that are non-resin components include additives known in the art. Examples of the additives include antifogging agents, antioxidants, antistatic agents, crystal nucleating agents, inorganic particles, viscosity reducing agents, thickening agents, heat stabilizers, and infrared absorbing agents.

[0044] The resin film 1 may contain only one type of other component, or two or more types. When there are two or more types, the combination and ratio thereof can be arbitrarily selected depending on the purpose.

[0045] The first surface layer 11 may be made of one layer (single layer) or may be made of two or more layers. When the first surface layer 11 is made of multiple layers, these multiple layers may be the same or different, and the combination of these multiple layers is not particularly limited as long as it does not impair the effects of the present invention.

[0046] The ratio of the thickness of the first surface layer 11 to the thickness of the laminate sheet 1 is preferably 0.5% or more and 3.0% or less, more preferably 0.7% or more and 2.0% or less, and particularly preferably 0.7% or more and 1.5% or less. When the ratio is equal to or greater than the lower limit, a greater effect is obtained by providing first surface layer 11. When the ratio is equal to or less than the upper limit, an excessive thickness of first surface layer 11 is further prevented. When first surface layer 11 is made up of a plurality of layers, the ratio of the total thickness of these layers to the thickness of laminate sheet 1 preferably falls within the above-mentioned numerical range.

[0047] <Middle Class> The laminate sheet 1 includes an intermediate layer 12. The intermediate layer 12 imparts transparency, impact resistance, heat resistance, and processability to the laminate sheet 1.

[0048] The intermediate layer 12 contains a polycarbonate, a compound represented by the following general formula (I), a compound represented by the following general formula (II), a lubricant, and a colorant, or contains a polycarbonate, a compound represented by the following general formula (I), a compound represented by the following general formula (III), a lubricant, and a colorant.

[0049] [ka] (In formula (I), R 11 and R 12 are each independently a hydrogen atom, an alkyl group, or an aryl group.

[0050] [ka] (In formula (II), R 21 is an alkyl group having 1 to 4 carbon atoms; R 22 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms; R 23 is a fluorine atom or an alkoxy group having 1 to 30 carbon atoms.

[0051] [ka] (In formula (III), R 31 is an alkyl group having 1 to 20 carbon atoms; and n is an integer of 1 to 5.

[0052] (Polycarbonate) The intermediate layer 12 comprises polycarbonate. The polycarbonate contained in intermediate layer 12 may be the same as the polycarbonate contained in first surface layer 11 described above. The polycarbonate contained in intermediate layer 12 and the polycarbonate contained in first surface layer 11 may be the same as or different from each other.

[0053] The ratio of the polycarbonate content (parts by mass) in intermediate layer 12 to the total mass (parts by mass) of intermediate layer 12 ([polycarbonate content (parts by mass) in intermediate layer 12)] / [total mass (parts by mass) of intermediate layer 12)]×100) is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, and may be, for example, any of 97% by mass or more and 99% by mass or more. When the ratio is equal to or more than the lower limit, the transparency, impact resistance, heat resistance and processability of intermediate layer 12 can be further improved. On the other hand, the proportion is 99% by mass or less. The above ratio is usually the same as the ratio of the polycarbonate content (parts by mass) to the total content (parts by mass) of components that do not vaporize at room temperature in the resin composition for forming an intermediate layer described below ([polycarbonate content (parts by mass) in the resin composition for forming an intermediate layer)]) / [total content (parts by mass) of components that do not vaporize at room temperature in the resin composition for forming an intermediate layer)]×100).

[0054] (Compound represented by general formula (I)) The intermediate layer 12 contains, in addition to polycarbonate, a compound represented by general formula (I). The compound represented by the general formula (I) is an antioxidant. When the intermediate layer 12 contains the compound represented by the general formula (I), thermal deterioration of the intermediate layer 12 during extrusion molding can be prevented.

[0055] [ka] (In formula (I), R 11 and R 12 are each independently a hydrogen atom, an alkyl group, or an aryl group.

[0056] Examples of the alkyl group include a chain alkyl group (a linear or branched alkyl group), a cycloalkyl group (a cyclic alkyl group), and a chain alkyl group-substituted cycloalkyl group (a group in which one or more hydrogen atoms in a cycloalkyl group are substituted with a chain alkyl group).

[0057] Examples of the aryl group include unsubstituted aryl groups and alkyl group-substituted aryl groups (groups in which one or more hydrogen atoms in an aryl group are substituted with a chain alkyl group or cycloalkyl group).

[0058] Examples of the compound represented by general formula (I) include compounds represented by the following structural formula:

[0059] [ka]

[0060] [ka]

[0061] [ka]

[0062] [ka]

[0063] [ka]

[0064] The intermediate layer 12 may contain only one type of compound represented by general formula (I), or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily depending on the purpose.

[0065] The compound represented by general formula (I) is preferably present uniformly in first surface layer 11.

[0066] In the intermediate layer 12, the content ratio of the compound represented by general formula (I) relative to the total mass of the intermediate layer 12 is preferably 0.005 mass% or more and 0.1 mass% or less, and more preferably 0.01 mass% or more and 0.05 mass% or less. When the ratio is equal to or more than the lower limit, it is possible to better prevent thermal deterioration during extrusion molding of the mid layer 12. When the ratio is equal to or less than the upper limit, it is possible to better suppress excessive use of the compound represented by general formula (I).

[0067] (Compounds represented by general formula (II) and compounds represented by general formula (III)) The intermediate element 12 contains, in addition to the polycarbonate and the compound represented by general formula (I), a compound represented by general formula (II) or a compound represented by general formula (III). The compound represented by the general formula (II) and the compound represented by the general formula (III) are antioxidants. When the intermediate layer 12 contains the compound represented by the general formula (II) or the compound represented by the general formula (III), thermal deterioration during extrusion of the intermediate layer 12 can be prevented.

[0068] [ka] (In formula (II), R 21 is an alkyl group having 1 to 4 carbon atoms; R 22 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms; R 23 is a fluorine atom or an alkoxy group having 1 to 30 carbon atoms.

[0069] [ka] (In formula (III), R 31 is an alkyl group having 1 to 20 carbon atoms; and n is an integer of 1 to 5.

[0070] In general formula (II), two R 21 may be the same as or different from each other.

[0071] Examples of the compound represented by the general formula (II) include compounds represented by the following structural formula:

[0072] [ka]

[0073] [ka]

[0074] [ka]

[0075] [ka]

[0076] [ka]

[0077] Examples of the compound represented by general formula (III) include tris(2,4-di-tert-butylphenyl)phosphite, tris-(2-tert-butyl-4-methylphenyl)phosphate, and the like.

[0078] When the intermediate layer 12 contains a compound represented by general formula (II), the compound represented by general formula (II) may be only one type, or may be two or more types. When there are two or more types, the combination and ratio thereof can be arbitrarily selected depending on the purpose. When the intermediate layer 12 contains a compound represented by general formula (III), the compound represented by general formula (III) may be of only one type or of two or more types, and when there are two or more types, the combination and ratio thereof can be arbitrarily selected depending on the purpose.

[0079] When the intermediate layer 12 contains the compound represented by general formula (II), it is preferable that the compound represented by general formula (II) is present uniformly in the intermediate layer 12 . When the intermediate layer 12 contains the compound represented by general formula (III), it is preferable that the compound represented by general formula (III) is present uniformly in the intermediate layer 12.

[0080] When the intermediate layer 12 contains a compound represented by general formula (II), the content ratio of the compound represented by general formula (II) in the intermediate layer 12 relative to the total mass of the intermediate layer 12 is preferably 0.005 mass% or more and 0.1 mass% or less, and more preferably 0.007 mass% or more and 0.03 mass% or less. When the ratio is equal to or more than the lower limit, it is possible to better prevent thermal deterioration during extrusion molding of the mid layer 12. When the ratio is equal to or less than the upper limit, it is possible to better suppress excessive use of the compound represented by general formula (II).

[0081] When the intermediate layer 12 contains a compound represented by general formula (III), the content ratio of the compound represented by general formula (III) in the intermediate layer 12 relative to the total mass of the intermediate layer 12 is preferably 0.005 mass% or more and 0.1 mass% or less, and more preferably 0.007 mass% or more and 0.03 mass% or less. When the ratio is equal to or more than the lower limit, it is possible to better prevent thermal deterioration during extrusion molding of the mid layer 12. When the ratio is equal to or less than the upper limit, it is possible to better suppress excessive use of the compound represented by general formula (III).

[0082] The intermediate layer 12 may contain both one or more compounds represented by general formula (II) and one or more compounds represented by general formula (III). In this case, it is preferable that the ratio of the total content of the compound represented by general formula (II) and the compound represented by general formula (III) to the total mass of the intermediate layer 12 is in the same numerical range as the content ratio of the compound represented by general formula (II) or the content ratio of the compound represented by general formula (III) described above.

[0083] (lubricant) The intermediate layer 12 contains a lubricant in addition to the polycarbonate, the compound represented by the general formula (I), and the compound represented by the general formula (II) or the compound represented by the general formula (III). The lubricant contained in intermediate layer 12 may be the same as the lubricant contained in first surface layer 11 described above. The lubricant contained in intermediate layer 12 and the lubricant contained in first surface layer 11 may be the same as or different from each other.

[0084] The lubricant is preferably present uniformly in the intermediate layer 12 .

[0085] In the intermediate layer 12, the content of the lubricant relative to the total mass of the intermediate layer 12 is preferably 0.0005 mass% or more and 5.0 mass% or less, more preferably 0.01 mass% or more and 3.0 mass% or less, and even more preferably 0.03 mass% or more and 2.0 mass% or less. When the ratio is equal to or greater than the lower limit, excellent slippage against a die, roller, etc. can be exhibited during extrusion molding of the mid layer 12, thereby further improving moldability. When the ratio is equal to or less than the upper limit, excessive use of the lubricant can be further suppressed.

[0086] (Coloring agent) The intermediate layer 12 contains a colorant in addition to polycarbonate, the compound represented by general formula (I), the compound represented by general formula (II) or the compound represented by general formula (III), and a lubricant. The appearance of the laminate sheet 1 may be impaired by the yellowish tinge of the polycarbonate contained in the laminate sheet 1. On the other hand, by including a colorant in the intermediate layer 12, the yellowish tinge of the polycarbonate can be suppressed, and the appearance of the laminate sheet 1 can be improved.

[0087] Examples of the colorant include bluing agents, carbon black, and titanium oxide.

[0088] The colorant contained in the intermediate layer 12 may be one type only, or two or more types. When there are two or more types, the combination and ratio thereof can be arbitrarily selected depending on the purpose.

[0089] The colorant is preferably present uniformly in the intermediate layer 12 .

[0090] In the intermediate layer 12, the ratio of the content of the colorant to the total mass of the intermediate layer 12 is 1.0×10 -5 Mass% or more 5.0×10 -2 It is preferably 1.0×10 -4 Mass% or more 5.0×10 -3 It is more preferable that the content is not more than % by mass. When the ratio is equal to or greater than the lower limit, it is possible to further improve the appearance of the laminate sheet 1. When the ratio is equal to or less than the upper limit, it is possible to further suppress excessive use of the colorant.

[0091] (Other ingredients) The intermediate layer 12 may contain only polycarbonate, a compound represented by general formula (I), a compound represented by general formula (II), or a compound represented by general formula (III), a lubricant, and a colorant (i.e., it may consist of polycarbonate, a compound represented by general formula (I), a compound represented by general formula (II), or a compound represented by general formula (III), a lubricant, and a colorant), or it may contain polycarbonate, a compound represented by general formula (I), a compound represented by general formula (II), or a compound represented by general formula (III), a lubricant, and a colorant, and other components (sometimes referred to as "other components" in this specification) (i.e., it may consist of polycarbonate, a compound represented by general formula (I), a compound represented by general formula (II), or a compound represented by general formula (III), a lubricant, and a colorant, and the other components).

[0092] The other components contained in the intermediate layer 12 are not particularly limited and can be arbitrarily selected depending on the purpose, and may be, for example, either a resin component or a non-resin component. The other component, which is a resin component, is a resin other than polycarbonate. The other component, which is a resin component, may be a homopolymer, which is a polymer of one type of monomer, or a copolymer, which is a polymer of two or more types of monomers.

[0093] Examples of the other components that are non-resin components include additives known in the art. Examples of the additives include antifogging agents, antistatic agents, crystal nucleating agents, inorganic particles, viscosity reducing agents, thickening agents, heat stabilizers, infrared absorbing agents, and ultraviolet absorbing agents.

[0094] The intermediate layer 12 may contain only one type of other component, or two or more types. When there are two or more types, the combination and ratio thereof can be arbitrarily selected depending on the purpose.

[0095] The intermediate layer 12 may be composed of one layer (single layer) or may be composed of two or more layers. When the intermediate layer 12 is composed of multiple layers, these multiple layers may be the same or different from each other, and the combination of these multiple layers is not particularly limited as long as it does not impair the effects of the present invention.

[0096] The ratio of the thickness of the intermediate layer 12 to the thickness of the laminate sheet 1 is preferably 93% or more and 99.7% or less, and more preferably 96% or more and 99.5% or less. When the ratio is equal to or greater than the lower limit, the effect obtained by providing the intermediate layer 12 is enhanced. When the ratio is equal to or less than the upper limit, the thickness of the intermediate layer 12 is further prevented from becoming excessive. When the intermediate layer 12 is made up of a plurality of layers, the ratio of the total thickness of these layers to the thickness of the laminate sheet 1 is preferably within the above-mentioned numerical range.

[0097] <Second surface layer> The laminate sheet 1 has a second surface layer 13. The second surface layer 13 imparts transparency, impact resistance, heat resistance, and processability to the laminate sheet 1, as well as weather resistance.

[0098] Second surface layer 13 contains polycarbonate, an ultraviolet absorbing agent, and a lubricant.

[0099] (Polycarbonate) The second surface layer 13 includes polycarbonate. The polycarbonate contained in second surface layer 13 may be the same as the polycarbonate contained in first surface layer 11 described above. The polycarbonate contained in second surface layer 13 and the polycarbonate contained in first surface layer 11 may be the same as or different from each other.

[0100] The ratio of the polycarbonate content (parts by mass) in second surface layer 13 to the total mass (parts by mass) of second surface layer 13 ([polycarbonate content (parts by mass) of second surface layer 13)] / [total mass (parts by mass) of second surface layer 13)]×100) is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, and may be, for example, any one of 97% by mass or more and 99% by mass or more. When the ratio is equal to or more than the lower limit, the transparency, impact resistance, heat resistance and processability of second surface layer 13 and laminate sheet 1 can be further improved. On the other hand, the proportion is 99% by mass or less. The above ratio is usually the same as the ratio of the polycarbonate content (parts by mass) to the total content (parts by mass) of components that do not vaporize at room temperature in the resin composition for forming the surface layer described below ([polycarbonate content (parts by mass) in the resin composition for forming the surface layer)]) / [total content (parts by mass) of components that do not vaporize at room temperature in the resin composition for forming the surface layer)]×100).

[0101] (UV absorber) Second surface layer 13 contains an ultraviolet absorbing agent in addition to polycarbonate. Examples of the ultraviolet absorbing agent contained in second surface layer 13 include the same ultraviolet absorbing agents contained in first surface layer 11 as described above. The ultraviolet absorbing agent contained in second surface layer 13 and the ultraviolet absorbing agent contained in first surface layer 11 may be the same as or different from each other.

[0102] The ultraviolet absorber may be present uniformly or non-uniformly in second surface layer 13. When present non-uniformly, the ultraviolet absorber is preferably unevenly distributed in a region on the surface side of second surface layer 13 opposite intermediate layer 12.

[0103] In second surface layer 13, the content of the ultraviolet absorbing agent relative to the total mass of second surface layer 13 is preferably 2 mass % or more, and more preferably 3 mass % or more and 10 mass % or less. When the ratio is equal to or more than the lower limit, it is possible to further improve the weather resistance of the laminate sheet 1. When the ratio is equal to or less than the upper limit, the excessive use of the ultraviolet absorbing agent is further suppressed.

[0104] (lubricant) Second surface layer 13 contains a lubricant in addition to polycarbonate and an ultraviolet absorbing agent. Examples of the lubricant contained in second surface layer 13 include the same lubricants as those contained in first surface layer 11 described above. The lubricant contained in second surface layer 13 and the lubricant contained in first surface layer 11 may be the same as or different from each other.

[0105] The lubricant is preferably present uniformly in second surface layer 13 .

[0106] In the second surface layer 13, the content of the lubricant relative to the total mass of the second surface layer 13 is preferably 0.0005 mass% or more and 5.0 mass% or less, more preferably 0.01 mass% or more and 3.0 mass% or less, and even more preferably 0.05 mass% or more and 2.0 mass% or less. When the ratio is equal to or greater than the lower limit, excellent slippage against a die, roller, etc. can be exhibited during extrusion molding of second surface layer 13, thereby further improving moldability. When the ratio is equal to or less than the upper limit, excessive use of lubricant can be further suppressed.

[0107] (Other ingredients) The second surface layer 13 may contain only polycarbonate, UV absorber and lubricant (i.e., it may consist of polycarbonate, UV absorber and lubricant), or it may contain polycarbonate, UV absorber and lubricant as well as other components (sometimes referred to as "other components" in this specification) (i.e., it may consist of polycarbonate, UV absorber, lubricant and the other components).

[0108] Examples of the other components contained in second surface layer 13 include the same components as those contained in first surface layer 11 described above.

[0109] The second surface layer 13 may be made of one layer (single layer) or may be made of two or more layers. When the second surface layer 13 is made of multiple layers, these multiple layers may be the same or different, and the combination of these multiple layers is not particularly limited as long as it does not impair the effects of the present invention.

[0110] The ratio of the thickness of second surface layer 13 to the thickness of laminate sheet 1 is preferably 0.5% or more and 3% or less, more preferably 0.7% or more and 2% or less, and particularly preferably 0.7% or more and 1.5% or less. When the ratio is equal to or greater than the lower limit, the effect obtained by providing second surface layer 13 is enhanced. When the ratio is equal to or less than the upper limit, the thickness of second surface layer 13 is further prevented from becoming excessive. When second surface layer 13 is made up of a plurality of layers, the ratio of the total thickness of these layers to the thickness of laminate sheet 1 preferably falls within the above-mentioned numerical range.

[0111] <Other layers> The laminate sheet 1 may have another layer that does not fall under any of the first surface layer 11, the intermediate layer 12, and the second surface layer 13, as long as the effect of the present invention is not impaired.

[0112] It is preferable that the other layers are not provided between first surface layer 11 and intermediate layer 12, and between intermediate layer 12 and second surface layer 13.

[0113] The other layer is preferably disposed on the side of first surface 11 opposite intermediate layer 12 or on the side of second surface 13 opposite intermediate layer 12 .

[0114] The types and number of the other layers included in the laminate sheet 1 are not particularly limited, and can be arbitrarily selected depending on the purpose. The other layer included in the laminate sheet 1 may be of only one type, or of two or more types. When there are two or more types, the combination and ratio thereof can be arbitrarily selected depending on the purpose.

[0115] The other layers may each be one layer (single layer) or two or more layers. When the other layers are multiple layers, the multiple layers may be the same or different from each other, and the combination of the multiple layers is not particularly limited as long as it does not impair the effects of the present invention.

[0116] The thickness of the other layer can be set arbitrarily depending on the type of the other layer, and is not particularly limited.

[0117] When the laminate sheet 1 includes the other layer, it may further include an adhesive layer for adhering the other layer to other layers.

[0118] <Characteristics of laminated sheets> The thickness of the laminate sheet 1 is preferably 0.5 mm or more and 25 mm or less, and more preferably 1 mm or more and 20 mm or less. When the thickness of the laminate sheet 1 is equal to or greater than the lower limit, it is possible to further improve the transparency, impact resistance, heat resistance, and processability of the laminate sheet 1. When the thickness of the laminate sheet 1 is equal to or less than the upper limit, it is possible to further prevent the laminate sheet 1 from becoming excessively thick.

[0119] (weather resistance) The laminate sheet 1 is subjected to an accelerated test in accordance with JIS K7350 using, for example, a carbon arc sunshine weather meter, and the change in haze value (weatherability) of the laminate sheet 1 can be measured from the appearance after 3000 hours of ultraviolet irradiation. The change in haze value (weatherability) is preferably 15 or less, more preferably 10 or less, and even more preferably 5 or less.

[0120] The weather resistance of the laminate sheet 1 can be adjusted by adjusting the type or content of a component contained in any of the layers constituting the laminate sheet 1. For example, the weather resistance of the laminate sheet 1 can be easily adjusted by adjusting the type or content of an ultraviolet absorbing agent contained in the first surface layer 11 and the second surface layer 13.

[0121] (yellowing degree) The laminate sheet 1 is subjected to an accelerated test in accordance with JIS K7350 using, for example, a carbon arc sunshine weather meter, and the yellowing degree of the laminate sheet 1 can be measured from the appearance after 3000 hours of ultraviolet irradiation. The yellowing index is preferably 10 or less, more preferably 5 or less, and even more preferably 3 or less.

[0122] The yellowing degree of the laminate sheet 1 can be adjusted by adjusting the type or content of the components contained in any of the layers constituting the laminate sheet 1. For example, the weather resistance of the laminate sheet 1 can be easily adjusted by adjusting the type or content of the colorant contained in the intermediate layer 12.

[0123] (Heat resistance) The heat resistance of the laminate sheet 1 can be measured, for example, from the appearance of the laminate sheet 1 after it has been exposed in a hot air oven at 120° C. for 24 hours. The heat resistance is preferably such that there is no noticeable deformation or discoloration.

[0124] The heat resistance of the laminate sheet 1 can be adjusted by adjusting the type or content of the components contained in any of the layers constituting the laminate sheet 1. For example, the heat resistance of the laminate sheet 1 can be easily adjusted by adjusting the type or content of the compound represented by general formula (I), or the compound represented by general formula (II), or the compound represented by general formula (III) contained in the intermediate layer 12.

[0125] <Method of manufacturing laminated sheet> The laminated sheet of this embodiment can be produced, for example, by a feed block method in which resins or resin compositions that are materials for forming each layer are melt-extruded using several extruders, a co-extrusion T-die method such as a multi-manifold method, or an air-cooled or water-cooled co-extrusion inflation method.

[0126] In addition, the laminate sheet of this embodiment can also be produced by coating a resin, resin composition, etc., which is a material for forming one of the layers, on the surface of another layer that constitutes the laminate sheet, and drying it as necessary to form a laminate structure in the laminate sheet, and if necessary, further stacking the other layers so as to obtain the desired arrangement. For example, when the laminate sheet has the other layer on the side opposite the intermediate layer side of the first surface layer, or on the side opposite the intermediate layer side of the second surface layer, the other layer can be formed by coating the surface opposite the intermediate layer side of the first surface layer, or the surface opposite the intermediate layer side of the second surface layer, with a resin, a resin composition, etc. that will be used to form the other layer, and drying it as necessary.

[0127] The laminated sheet of the present embodiment can also be produced by separately preparing two or more sheets for constituting any two or more of the layers in advance, laminating these sheets together using an adhesive by any of the dry lamination method, the extrusion lamination method, the hot melt lamination method, and the wet lamination method, and further laminating other layers as necessary so as to achieve the desired arrangement. An adhesive may be used at this time.

[0128] In addition, the laminated sheet of this embodiment can also be produced by laminating two or more films that have been prepared separately in advance, as described above, by a thermal lamination method or the like without using an adhesive, and, if necessary, further laminating other layers so as to achieve the desired arrangement.

[0129] When producing the laminate sheet of this embodiment, two or more of the methods for forming any of the layers (sheets) in the laminate sheet described above may be combined.

[0130] Regardless of the manufacturing method, the resin composition that is the material for forming any layer in the laminate sheet may be manufactured by adjusting the type and content of the components contained so that the layer to be formed contains the desired components (constituent materials) in the desired content. For example, the content ratio of the components that do not vaporize at room temperature in the resin composition is usually the same as the content ratio of the components in the layer formed from this resin composition.

[0131] Examples of resin compositions (sometimes referred to in this specification as "resin compositions for forming surface layers") for forming the first surface layer (first surface layer 11 in the laminate sheet 1 shown in FIG. 1) and the second surface layer (second surface layer 13 in the laminate sheet 1 shown in FIG. 1) include resin compositions containing the above-mentioned polycarbonate, the above-mentioned UV absorber, the above-mentioned lubricant, and, if necessary, the other components.

[0132] Examples of resin compositions (sometimes referred to in this specification as "resin compositions for forming an intermediate layer") for forming an intermediate layer (intermediate layer 12 in the laminate sheet 1 shown in FIG. 1) include resin compositions containing the above-mentioned polycarbonate, the compound represented by the above-mentioned general formula (I), the compound represented by the above-mentioned general formula (II), or the compound represented by the above-mentioned general formula (III), a lubricant, a colorant, and, if necessary, the other components. EXAMPLES

[0133] The present invention will be described in more detail below with reference to specific examples, although the present invention is not limited to the following examples.

[0134] [Example 1] <<Laminated sheet manufacturing>> A laminate sheet having the configuration shown in FIG. 1 was produced by the following procedure.

[0135] Polycarbonate ("PC" manufactured by Mitsubishi Engineering Co., Ltd.) was prepared as the resin constituting the first surface layer and the second surface layer.

[0136] The polycarbonate (96.900% by mass), a triazine-based ultraviolet absorber (manufactured by BASF) (3.00% by mass), and a lubricant (monostearic acid (manufactured by Riken Vitamin Co., Ltd.)) (0.100% by mass) were mixed at room temperature to produce a resin composition for forming a surface layer.

[0137] A resin composition for forming an intermediate layer was produced by mixing the polycarbonate (99.853% by mass), lubricant (monostearic acid (manufactured by Riken Vitamin Co., Ltd.)) (0.1% by mass), antioxidant A (0.030% by mass), antioxidant B (0.015% by mass), and colorant (blueing agent) (0.002% by mass) at room temperature.

[0138] The antioxidant A is 3,9-bis(2,6-di-tert-butyl-4-phenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5,5]undecane, which is represented by the following structural formula. [ka]

[0139] The antioxidant B is 2,2'-methylenebis(4,6-di-tert-butyl-1-phenyloxy)(2-ethylhexyloxy)phosphorus, which is represented by the following structural formula. [ka]

[0140] The die temperature was set to 300°C, and the resin composition for forming the surface layer, the resin composition for forming the intermediate layer, and the resin composition for forming the surface layer were co-extruded in this order (co-extrusion T-die method) to obtain a laminated sheet (thickness 2000 μm) composed of a first surface layer (thickness 30 μm), an intermediate layer (thickness 1940 μm), and an outer layer (thickness 30 μm) stacked in this order in the thickness direction.

[0141] <<Evaluation of laminated sheets>> <Weather resistance measurement> The laminate sheet was subjected to an accelerated test in accordance with JIS K7350 using a carbon arc sunshine weather meter, and the change in haze value (weather resistance) of the laminate sheet was measured from the appearance after 3000 hours of ultraviolet irradiation. The results are shown in Table 1.

[0142] <Yellowing degree measurement> The laminate sheet was subjected to an accelerated test in accordance with JIS K7350 using a carbon arc sunshine weather meter, and the yellowing degree of the laminate sheet was measured from the appearance after 3000 hours of ultraviolet irradiation. The results are shown in Table 1.

[0143] <Heat resistance measurement> The laminate sheet was exposed to a hot air oven at 120° C. for 24 hours, and then its heat resistance was measured based on its appearance according to the following criteria. The results are shown in Table 1. ○: No noticeable deformation or discoloration. △: No obvious deformation, but obvious discoloration. ×: Obvious deformation or discoloration.

[0144] [Example 2] A laminated sheet was produced in the same manner as in Example 1, except that the polycarbonate (90.9% by mass), triazine-based ultraviolet absorber (9.0% by mass), and lubricant (monostearic acid (manufactured by Riken Vitamin Co., Ltd.)) (0.100% by mass) were mixed at room temperature to produce a resin composition for forming a surface layer, and the laminated sheet was evaluated. The results are shown in Table 1.

[0145] [Example 3] A laminated sheet was produced in the same manner as in Example 1, except that antioxidant B was changed to antioxidant C, in which a first surface layer (thickness 30 μm), an intermediate layer (thickness 1940 μm), and a second surface layer (thickness 30 μm) were laminated in this order in the thickness direction, and this laminated sheet was evaluated. The results are shown in Table 1.

[0146] The antioxidant C is tris(2,4-di-tert-butylphenyl)phosphite, which is represented by the following structural formula. [ka]

[0147] [Comparative Example 1] A laminated sheet was produced in the same manner as in Example 1, except that the polycarbonate (99.9% by mass) and a lubricant (monostearic acid (manufactured by Riken Vitamin Co., Ltd.) (0.100% by mass) were mixed at room temperature to produce a resin composition for forming a surface layer, and the laminated sheet was evaluated. The results are shown in Table 1.

[0148] [Table 1]

[0149] As is clear from the above results, in Examples 1 to 3, the change in haze value was smaller than in Comparative Example 1 due to the effect of the ultraviolet absorbing agent, and the weather resistance was excellent.

[0150] Moreover, in Examples 1 to 3, the degree of yellowing was smaller than that in Comparative Example 1 due to the effect of the coloring agent.

[0151] Furthermore, in Examples 1 to 3, due to the effect of the antioxidant, there was no noticeable deformation or discoloration compared to Comparative Example 1, and the heat resistance was excellent. [Industrial Applicability]

[0152] The laminate sheet of the present invention can be used as a material for outdoor buildings such as carports, verandas, terraces, and arcades. [Explanation of symbols]

[0153] 1...Laminated sheet 11...1st surface layer 12. Middle class 13…Second surface layer

Claims

1. A laminated sheet, The laminate sheet is configured by laminating a first surface layer, an intermediate layer, and a second surface layer in this order in a thickness direction, The first surface layer and the second surface layer contain polycarbonate, an ultraviolet absorbing agent, and a lubricant, the ultraviolet absorber is one or more selected from the group consisting of triazine-based ultraviolet absorbers, benzoxazinone-based ultraviolet absorbers, benzotriazole-based ultraviolet absorbers, and benzophenone-based ultraviolet absorbers; The intermediate layer is a laminate sheet including a polycarbonate, a compound represented by the following general formula (I), a compound represented by the following general formula (II), or a compound represented by the following general formula (III), a lubricant, and a colorant. 【Chemistry 1】 (In formula (I), R 11 and R 12 are each independently a hydrogen atom, an alkyl group, or an aryl group. 【Chemistry 2】 (In formula (II), R 21 is an alkyl group having 1 to 4 carbon atoms; R 22 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms; R 23 is a fluorine atom or an alkoxy group having 1 to 30 carbon atoms. 【Chemistry 3】 (In formula (III), R 31 is an alkyl group having 1 to 20 carbon atoms; and n is an integer from 1 to 5.

2. In the first surface layer, a ratio of a content of the ultraviolet absorber to a total mass of the first surface layer is 2 mass% or more, The laminate sheet according to claim 1 , wherein a content of the ultraviolet absorbing agent in the second surface layer is 2 mass % or more relative to a total mass of the second surface layer.

3. A ratio of a thickness of the first surface layer to a thickness of the laminate sheet is 0.7% or more and 1.5% or less, 3. The laminate sheet according to claim 1, wherein a ratio of a thickness of the second surface layer to a thickness of the laminate sheet is 0.7% or more and 1.5% or less.

4. The laminate sheet according to claim 1 or 2, wherein the thickness of the laminate sheet is from 1 mm to 20 mm.

5. 3. The laminate sheet according to claim 1, wherein the lubricant is one or more selected from the group consisting of fatty acid esters, hydroxy fatty acids, and polyethylene oxide.

Citation Information

Patent Citations

  • Polycarbonate resin composition

    JP2003041108A

Cited By

  • Preparation method of uvioresistant UV master batch for polycarbonate plate

    CN121495096A