Polymer cement mortar composition, and polymer cement mortar

The polymer cement mortar composition balances workability and strength development by using cement, cement polymer, and amorphous aluminosilicate, addressing the limitations of existing mortars in concrete repair.

JP2024145051AInactive Publication Date: 2024-10-15TAIHEIYO MATERIALS CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023057284
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing polymer cement mortars struggle to balance good workability with high strength development, which is crucial for effective repair and reinforcement of concrete structures.

Method used

A polymer cement mortar composition comprising cement, cement polymer, amorphous aluminosilicate, and fine aggregate, with specific ratios and properties, ensuring good workability and strength development.

Benefits of technology

The composition achieves both excellent workability and long-term strength development, making it suitable for repairing and reinforcing concrete structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145051000001
    Figure 2024145051000001
  • Figure 2024145051000002
    Figure 2024145051000002
Patent Text Reader

Abstract

To provide a polymer cement mortar composition and a polymer cement mortar which can satisfy desirable workability and strength development.SOLUTION: A polymer cement mortar composition contains cement, polymers for cement, amorphous aluminosilicate and fine aggregate, where the content of the polymers for cement is 1 to 18 pts.mass relative to 100 pts.mass of the cement in terms of solid content, and the content of the amorphous aluminosilicate is 1 to 15 pts.mass relative to 100 pts.mass of cement.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polymer cement mortar composition and a polymer cement mortar. [Background technology]

[0002] Cracks occur in concrete structures (for example, floor slabs, walls, and ceilings such as reinforced concrete (RC) floor slabs or intermediate floor slabs of box culverts) due to factors such as fatigue and drying shrinkage. When this type of deterioration progresses or the cracks are rubbed together, causing the crack width to increase, deterioration factors such as water and chloride ions penetrate into the concrete structure from the deteriorated area. This results in corrosion of the reinforcing bars embedded in the concrete structure. If damage caused by cracks in a concrete structure is left unattended, the reinforcing bars inside will eventually corrode, causing cross-sectional defects and making it impossible to maintain the safety of the structure. For this reason, the deteriorated areas are removed and then the recesses are filled with repair or reinforcing materials.

[0003] Polymer cement mortar has been proposed as a repair material or reinforcing material. For example, Patent Document 1 discloses a polymer cement mortar containing cement, a polymer for cement, aggregate, and water, the aggregate containing aggregate classified as lightweight aggregate and aggregate classified as fine aggregate, and characterized in that the water / cement mass ratio is 18-45%, the polymer / cement mass ratio is 10-28%, the fine aggregate / cement volume ratio is 0.3-1.2, and the lightweight aggregate / total aggregate volume ratio is 0.4-0.9. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-000820 A Summary of the Invention [Problem to be solved by the invention]

[0005] Repair or reinforcing materials are required to have good workability because they are used to fill recesses or to treat them with a trowel. In addition, due to their intended use, repair or reinforcing materials are also required to have high strength expression to improve durability after repair.

[0006] Therefore, an object of the present invention is to provide a polymer cement mortar composition and a polymer cement mortar that can achieve both good workability and strength development. [Means for solving the problem]

[0007] As a result of extensive investigations into the above problems, the present inventors have found that it is possible to achieve both good workability and strength development by adjusting the blend ratio of a cement polymer and an amorphous aluminosilicate.

[0008] That is, the present invention is as follows. [1] A polymer cement mortar composition comprising cement, a polymer for cement, an amorphous aluminosilicate and a fine aggregate, wherein the content of the polymer for cement is 1 to 18 parts by mass, calculated as solid content, per 100 parts by mass of cement, and the content of the amorphous aluminosilicate is 1 to 15 parts by mass, per 100 parts by mass of cement. [2] When hardened, the compressive strength at 28 days is 55 N / mm2, measured at 20°C in accordance with the Japan Society of Civil Engineers standard JSCE-G505-2013 "Test method for compressive strength of mortar or cement paste using cylindrical specimens (draft)." 2 The polymer cement mortar composition according to [1] above. [3] The polymer cement mortar composition according to [1] or [2], wherein the mass ratio of the amorphous aluminosilicate to the polymer for cement ([mass of amorphous aluminosilicate] / [mass of polymer for cement (solid content equivalent)]) is 0.1 to 2.5. [4] A polymer cement mortar comprising the polymer cement mortar composition according to [1] or [2] and water, wherein the water content is 25 to 50 parts by mass per 100 parts by mass of cement. Effect of the Invention

[0009] ADVANTAGEOUS EFFECTS OF THE PRESENT DISCLOSURE According to the present invention, it is possible to provide a polymer cement mortar composition and a polymer cement mortar that can achieve both good workability and strength development. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, one embodiment of the present invention will be described.

[0011] The polymer cement mortar composition of the present embodiment contains cement, a cement polymer, an amorphous aluminosilicate, and a fine aggregate.

[0012] Various types of cement can be used, including, for example, various Portland cements such as ordinary, early strength, extra early strength, low heat and moderate heat, ecocement, rapid hardening cement, fly ash cement, etc. One type of cement may be used alone, or two or more types may be used in combination. The cement is preferably a fast-setting cement from the viewpoint of better strength development in an early stage. The fast-setting cement preferably contains calcium aluminates as an active ingredient, and more preferably contains 11CaO·7Al2O3·CaX2 (X represents a halogen atom) or 3CaO·3Al2O3·CaSO4 (auyne) as an active ingredient. 11CaO·7Al2O3·CaX2 is a so-called calcium aluminate halide cement. The halogen atom is preferably a fluorine atom. Auyne is also called calcium sulfoaluminate cement (auyne cement). These are called ultra-fast-setting cements, and are commercially available under the trade names Jet Cement or Super Jet Cement. As a fast-setting cement, auyne cement is the most preferable. Other calcium aluminates include C3A, C2A, and C, where CaO is C, Al2O3 is A, and Fe2O3 is F. 12These include calcium aluminates with mineral compositions indicated as A7, CA, CA2, etc., calcium aluminoferrites indicated as C4AF, etc., alumina cements, and those in which SiO2, K2O, Fe2O3, TiO2, etc. are dissolved or combined. Calcium aluminates may be either crystalline or amorphous, or may be a mixture of crystalline and amorphous. Rapid hardening admixtures prepared by blending these calcium aluminates with inorganic salts such as gypsum can also be added to Portland cement to be used as rapid hardening cement.

[0013] The polymer for cement is preferably a polymer specified in JIS A 6203:2015 "Polymer dispersions and re-emulsified powdered resins for cement admixture". Examples of such polymers for cement include polymer dispersions and re-emulsified powdered resins. Examples of polymer dispersions include synthetic rubbers such as styrene butadiene rubber (SBR); natural rubbers; rubber asphalts; ethylene vinyl acetates; acrylic esters; and resin asphalts. Among them, the polymer dispersions are preferably synthetic rubbers, ethylene vinyl acetates, and acrylic esters, and more preferably synthetic rubber latex, polyacrylic esters, and ethylene vinyl acetates. Examples of re-emulsified powdered resins include synthetic rubbers such as styrene butadiene rubber; acrylic esters; ethylene vinyl acetates; vinyl acetate / vinyl versatate esters; vinyl acetate / vinyl versatate / acrylic esters. As the polymer for cement, a polymer dispersion may be used, a re-emulsified powdered resin may be used, or a polymer dispersion and a re-emulsified powdered resin may be used in combination. Among the polymers for cement, a polymer dispersion and / or a re-emulsified powder resin of styrene-butadiene rubber is preferred from the viewpoint of further improving the adhesiveness to concrete. Styrene-butadiene rubber is a type of synthetic rubber obtained by copolymerizing styrene and butadiene, and the quality can be appropriately adjusted by adjusting the styrene content and the amount of vulcanization. For cement admixture, most of them have a bound styrene content of 50 to 70% by mass, and are used to improve stability and adhesiveness. The polymers for cement may be used alone or in combination of two or more.

[0014] The content of the polymer for cement is 1 to 18 parts by mass in terms of solid content relative to 100 parts by mass of cement. If the content of the polymer for cement is outside the above range, the initial and long-term strength development is reduced. From the viewpoint of being easy to ensure fluidity, being good in workability, and tending to be excellent in initial and long-term strength development, the content of the polymer for cement is preferably 3 to 15 parts by mass, more preferably 6 to 12 parts by mass in terms of solid content relative to 100 parts by mass of cement.

[0015] The amorphous aluminosilicate is not particularly limited as long as it is derived from a clay mineral and contains an amorphous portion, and any of them can be used. Examples of the clay mineral as the raw material include kaolin minerals, mica clay minerals, smectite minerals, and mixed layer minerals formed by mixing these. The amorphous aluminosilicate is obtained by, for example, calcining and dehydrating these crystalline aluminosilicates to make them amorphous. From the viewpoint of further excellent reactivity, the amorphous aluminosilicate is preferably derived from a kaolin mineral such as kaolinite, halloysite, dickite, etc., and more preferably metakaolin obtained by calcining kaolinite. The amorphous aluminosilicate may be used alone or in combination of two or more kinds. The BET specific surface area of ​​the amorphous aluminosilicate is 1 to 4 m 2 / g, and 1.5 to 3m 2 It is more preferable that the molecular weight is / g. In this specification, "amorphous" means that the peaks derived from the raw clay mineral are almost not observed in the measurement by a powder X-ray diffractometer. The amorphous aluminosilicate mineral powder according to this embodiment may have an amorphous ratio of 70% by mass or more, preferably 90% by mass or more, more preferably 100% by mass, that is, most preferably has no peaks observed in the measurement by a powder X-ray diffractometer. Here, the amorphous ratio is a value obtained by the standard addition method. Aluminosilicates with a high amorphous ratio, i.e., aluminosilicates with a low crystalline ratio, tend to have better strength development at the same mixing amount than aluminosilicates with a low amorphous ratio. Examples of heating for amorphizing aluminosilicate include firing in an externally heated kiln, an internally heated kiln, an electric furnace, etc., and melting using a melting furnace.

[0016] The content of the amorphous aluminosilicate is 1 to 15 parts by mass relative to 100 parts by mass of cement. If the content of the amorphous aluminosilicate is outside the above range, mixing becomes difficult and workability cannot be ensured. From the viewpoint of further improving initial and long-term strength development while ensuring fluidity and workability, the content of the amorphous aluminosilicate is preferably 3 to 12 parts by mass, more preferably 5 to 10 parts by mass relative to 100 parts by mass of cement.

[0017] The mass ratio of the amorphous aluminosilicate to the polymer for cement ([mass of amorphous aluminosilicate] / [mass of polymer for cement (solid content equivalent)]) is preferably 0.1 to 2.5, more preferably 0.3 to 2.0, and even more preferably 0.5 to 1.8. When the mass ratio of the amorphous aluminosilicate to the polymer for cement is within the above range, both better workability and strength development can be achieved.

[0018] Examples of fine aggregates include river sand, silica sand, crushed sand, kansui stone, limestone sand, and slag aggregate. Of these, it is preferable to use aggregates such as silica sand and limestone that have been adjusted to a particle size that does not contain fine powder or coarse aggregate. One type of fine aggregate may be used alone, or two or more types may be used in combination. It is preferable to use fine aggregates with a particle size of less than 5 mm (passing a 5 mm sieve), which is the type commonly used. Aggregates with a particle size of less than 5 mm refer to those that pass a 5 mm sieve when sieving aggregates.

[0019] The particle size of the fine aggregate is not particularly limited, and can be adjusted within the required particle size range of the fine aggregate. The particle size of the fine aggregate can be considered from the coarse aggregate ratio defined by JIS A 1102:2014 "Sieving test method for aggregates". From the viewpoint of obtaining better fluidity and suppressing bleeding during mortar, the coarse aggregate ratio of the fine aggregate is preferably 1 to 4, more preferably 1.5 to 3.8, and most preferably 2 to 3.5.

[0020] The content of the fine aggregate is preferably 150 to 450 parts by mass, more preferably 200 to 400 parts by mass, and even more preferably 250 to 350 parts by mass, relative to 100 parts by mass of cement. If the content of the fine aggregate is within the above range, the flowability and workability are likely to be excellent.

[0021] The polymer cement mortar composition of the present embodiment may contain a water reducing agent. The water reducing agent includes a high-performance water reducing agent, a high-performance AE water reducing agent, an AE water reducing agent, and a superplasticizer. Examples of such water reducing agents include those specified in JIS A 6204:2011 "Chemical admixtures for concrete". Examples of the water reducing agent include polycarboxylic acid-based water reducing agents, naphthalenesulfonic acid-based water reducing agents, ligninsulfonic acid-based water reducing agents, melamine-based water reducing agents, and acrylic-based water reducing agents. Among these, naphthalenesulfonic acid-based water reducing agents are preferred. The water reducing agents may be used alone or in combination of two or more types.

[0022] The content of the water reducing agent is preferably 0.1 to 5 parts by mass, more preferably 0.3 to 3 parts by mass, and most preferably 0.5 to 1.5 parts by mass, in terms of solid content, relative to 100 parts by mass of cement. If the content of the water reducing agent is within the above range, better fluidity is easily obtained when the mortar is made, and initial and long-term strength development is also easily improved.

[0023] The polymer cement mortar composition of the present embodiment may contain a setting retarder. By containing a setting retarder, it is easy to ensure the working time even when the mixing temperature of the polymer cement mortar is high in summer, etc. Examples of setting retarders include organic acids or salts thereof such as citric acid, gluconic acid, malic acid, and tartaric acid; boric acid, borates such as sodium borate, phosphates, alkali metal carbonates, and alkali metal bicarbonates; and sugars. Among these, citric acid, citrates, tartaric acid, tartrates, and alkali metal carbonates are preferred. The setting retarder may be in the form of a powder or a liquid (for example, an aqueous solution, an emulsion, or a suspension). The setting retarder may be used alone or in combination of two or more types.

[0024] The content of the retarder is preferably 0.1 to 2.5 parts by mass, more preferably 0.3 to 2 parts by mass, and even more preferably 0.5 to 1.5 parts by mass, relative to 100 parts by mass of cement. If the content of the retarder is within the above range, the pot life is more easily ensured and the early strength development is less likely to decrease.

[0025] The polymer cement mortar composition of the present embodiment may contain various admixtures (materials) within the scope of not impairing the effects of the present invention. Examples of the admixtures (materials) include defoamers, waterproofing agents, rust inhibitors, shrinkage reducing agents, thickeners, water retention agents, pigments, water repellents, efflorescence inhibitors, and fibers.

[0026] The polymer cement mortar composition of the present embodiment can be prepared by mixing the above-mentioned components with a commonly used kneading tool, which is not particularly limited. Examples of the kneading tool include a Hobart mixer, a hand mixer, a tilting mixer, and a twin-shaft mixer.

[0027] The polymer cement mortar composition of the present embodiment has a compressive strength of 55 N / mm2 at 28 days after hardening, measured in a 20°C environment in accordance with the Japan Society of Civil Engineers standard JSCE-G505-2013 "Test method for compressive strength of mortar or cement paste using cylindrical specimens (draft)." 2 It is preferable that the resistance is 60N / mm or more. 2 More preferably, it is 65N / mm 2 More preferably, the compressive strength at 28 days is 100N / mm 2 It may be the following. If the compressive strength of the polymer cement mortar composition when hardened is within the above range, the long-term strength development will be even better.

[0028] The polymer cement mortar composition of the present embodiment can be mixed with water to prepare a polymer cement mortar, and the water content may be appropriately adjusted depending on the application. The water content is preferably 20 to 50 parts by mass, more preferably 25 to 45 parts by mass, and even more preferably 30 to 40 parts by mass, relative to 100 parts by mass of cement. If the water content is within the above range, it is easier to ensure fluidity, and it is easier to suppress the occurrence of material separation, the increase in shrinkage of the hardened body, and the decrease in early strength development.

[0029] The polymer cement mortar of the present embodiment can be prepared using the same kneading equipment as that used for ordinary polymer cement mortar, and is not particularly limited. As the kneading equipment, for example, the above-mentioned kneading equipment can be used.

[0030] The polymer cement mortar composition and polymer cement mortar of the present embodiment have excellent workability and exhibit good strength development from the early stage to the long term. Therefore, the polymer cement mortar composition and polymer cement mortar of the present embodiment can be suitably used for repairing and reinforcing various structures including concrete structures. The application method is not particularly limited, and a method of spreading the composition evenly using a trowel or a vibrator can be selected. EXAMPLES

[0031] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. All examples were carried out in a 20°C environment.

[0032] The materials used in the examples are as follows: Cement: Ultra fast hardening cement (Auin type) · Polymer for cement: Styrene butadiene rubber emulsion Amorphous aluminosilicate: Metakaolin, BET specific surface area 2.5cm 2 / g ·Fine aggregate: silica sand, coarse grain ratio 2.2 Water reducing agent: Naphthalene sulfonic acid water reducing agent · Retarder: Citric acid

[0033] [Mixture design of polymer cement mortar composition] The mix was designed with 100 parts by mass of cement, fine aggregate, cement polymer, and amorphous aluminosilicate in the proportions shown in Table 1, 1 part by mass of water reducing agent, and 1 part by mass of setting retarder. In the examples, all the amounts are calculated as solids.

[0034] [Preparation of polymer cement mortar] In a 20°C environment, the cement polymer was added to a 10 L cylindrical container, and each material of the polymer cement mortar composition designed in Table 1 and water were added, and the mixture was mixed with a hand mixer for 60 to 90 seconds to produce approximately 3 L of polymer cement mortar.

[0035] [Table 1]

[0036] [Evaluation method] The tests were carried out according to the methods described below, and the test results are shown in Table 2. ·Liquidity In accordance with JIS R 5201:2021 "Physical testing methods for cement" 12. Flow test, the flow values ​​(0 hits, 15 hits) of polymer cement mortar were measured in a 20°C environment. ·Workability Using the mixed mortar, a portion of the mortar was placed on a trowel board. If it broke apart when spread out with the trowel, it was rated as poor (×), if it did not break apart when spread out on the trowel board, it was rated as good (○). Of the mortar with good workability, if there was little mortar adhering to the trowel, it was rated as the best (◎). Compressive strength The compressive strength was measured at 1 day and 28 days of age in accordance with the Japan Society of Civil Engineers standard JSCE-G505-2013 "Method of compressive strength test for mortar or cement paste using cylindrical specimens (draft)". The dimensions of the specimen were 50 mm in diameter and 100 mm in height. The specimen was sealed and cured, and demolded on the day of age.

[0037] [Table 2]

[0038] The polymer cement mortars of the Examples had good workability and good initial and long-term strength development. On the other hand, among the polymer cement mortars of the Comparative Examples, No. 7 was difficult to mix, and the workability and strength development were poor in the other test examples.

Claims

1. The present invention includes a cement, a cement polymer, an amorphous aluminosilicate, and a fine aggregate, The content of the polymer for cement is 1 to 18 parts by mass in terms of solid content per 100 parts by mass of the cement, The polymer cement mortar composition has an amorphous aluminosilicate content of 1 to 15 parts by mass per 100 parts by mass of the cement.

2. When hardened, the compressive strength at 28 days after hardening is 55 N / mm2, measured at 20°C in accordance with the Japan Society of Civil Engineers standard JSCE-G505-2013 "Test method for compressive strength of mortar or cement paste using cylindrical specimens (draft)". 2 The polymer cement mortar composition according to claim 1 .

3. 3. The polymer cement mortar composition according to claim 1, wherein the mass ratio of the amorphous aluminosilicate to the polymer for cement ([mass of the amorphous aluminosilicate] / [mass of the polymer for cement (solid content equivalent)]) is 0.1 to 2.

5.

4. The polymer cement mortar composition according to claim 1 or 2, and water, The polymer cement mortar has a water content of 25 to 50 parts by mass per 100 parts by mass of the cement.

Citation Information

Patent Citations

  • Polymer cement mortar, and construction method using the same

    JP2015000820A