【0011】 本発明の実施形態によれば、NiおよびSiの添加量を合計で6.50質量%以下にしつつ、十分な強度が得られる銅合金板およびその製造方法を提供することが可能である。
Smart Images

Figure 2024145273000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a copper alloy sheet and a method for producing the same. [Background technology]
[0002] For example, as described in Patent Document 1, sheet material made of a Cu-Ni-Si-based copper alloy (hereinafter also referred to as a "Corson-based copper alloy") in which Ni and Si are added to Cu has an excellent balance of spring properties, stress relaxation resistance, processability required for terminal molding, and thermal conductivity properties that dissipate heat generated by current flow, and is therefore widely used as a terminal material for electronic devices installed in automobiles.
[0003] Corson copper alloys are made of Ni-Si compounds (e.g. Ni 2 It is possible to improve strength by precipitating Ni and Si compounds. For example, when the total amount of Ni and Si added is 6.50 mass% or less, the strength may be insufficient depending on the application, but by increasing the amount of Ni and Si added and increasing the amount of precipitates, it is possible to obtain sufficient strength. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2002-266042 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the increase in the amount of Ni and Si added not only increases the material cost, but also reduces the workability, which is a characteristic of Corson copper alloys. Therefore, a method is desired that can obtain sufficient strength without increasing the amount of Ni and Si added (for example, by keeping the total amount of Ni and Si added to 6.50 mass% or less).
[0006] The present disclosure has been made in view of the above circumstances, and one of its objectives is to provide a copper alloy sheet and a manufacturing method thereof, which can obtain sufficient strength while limiting the total amount of Ni and Si to 6.50 mass% or less. [Means for solving the problem]
[0007] Aspect 1 of the present invention is The composition of the components is Ni: 2.00~5.00% by mass, Si: 0.50 to 1.50 mass%; and The balance is composed of Cu and unavoidable impurities. The average particle diameter of the precipitate particles measured by small angle X-ray scattering is 1.0 nm to 4.5 nm; The copper alloy sheet has an area ratio of (111) planes of 3% or more in an electron backscatter diffraction pattern obtained from a cross section parallel to the rolling direction and the sheet thickness direction.
[0008] Aspect 2 of the present invention is The copper alloy sheet according to embodiment 1, further comprising at least one selected from the group consisting of Al, Mn, Cr, Ti, Zr, P, Ag, and Mg in an amount of more than 0 mass% and 0.50 mass% or less in total, each of which is 0.10 mass% or less.
[0009] Aspect 3 of the present invention is preparing a copper alloy ingot having a composition consisting of 2.00 to 5.00 mass% Ni, 0.50 to 1.50 mass% Si, and the balance being Cu and unavoidable impurities; heating the copper alloy ingot to 800 to 1050°C; hot rolling the heated copper alloy ingot at a total rolling reduction of 55% or more to obtain a copper alloy plate; A step of performing a first cold rolling on the hot-rolled copper alloy sheet; A step of subjecting the copper alloy sheet that has been subjected to the first cold rolling to a solution treatment; A step of subjecting the solution-treated copper alloy sheet to aging treatment at a temperature of 400 to 500°C for 30 minutes to 10 hours; A step of subjecting the aging-treated copper alloy sheet to a second cold rolling at a total reduction ratio of 50% or more and less than 90%; The method for producing the copper alloy sheet according to embodiment 1 includes the steps of:
[0010] A fourth aspect of the present invention is preparing a copper alloy ingot having a chemical composition containing 2.00 to 5.00 mass% Ni, 0.50 to 1.50 mass% Si, and at least one selected from the group consisting of Al, Mn, Cr, Ti, Zr, P, Ag, and Mg in an amount of 0.10 mass% or less each, in total more than 0 mass% and 0.50 mass% or less, with the balance being Cu and unavoidable impurities; heating the copper alloy ingot to 800 to 1050°C; hot rolling the heated copper alloy ingot at a total rolling reduction of 55% or more to obtain a copper alloy plate; A step of performing a first cold rolling on the hot-rolled copper alloy sheet; A step of subjecting the copper alloy sheet that has been subjected to the first cold rolling to a solution treatment; A step of subjecting the solution-treated copper alloy sheet to aging treatment at a temperature of 400 to 500°C for 30 minutes to 10 hours; A step of subjecting the aging-treated copper alloy sheet to a second cold rolling at a total reduction ratio of 50% or more and less than 90%; The method for producing the copper alloy sheet according to embodiment 2 includes the steps of: Effect of the Invention
[0011] According to an embodiment of the present invention, it is possible to provide a copper alloy sheet and a method for producing the same, which can obtain sufficient strength while limiting the total amount of Ni and Si added to 6.50 mass % or less. [Brief description of the drawings]
[0012] [Figure 1A] FIG. 1A is a transmission electron microscope image showing an example of precipitate particles such as Ni—Si compounds after aging treatment. [Figure 1B]FIG. 1B is a transmission electron microscope image showing an example of precipitate particles such as Ni—Si compounds after the second cold rolling. [Figure 2A] FIG. 2A is the EBSD pattern of sample No. 1. [Figure 2B] Figure 2B is the EBSD pattern of sample No. 2. [Figure 2C] Figure 2C is the EBSD pattern of sample No. 3. [Figure 2D] FIG. 2D is the EBSD pattern of sample No. 4. [Figure 2E] Figure 2E is the EBSD pattern of sample No. 5. [Figure 2F] Figure 2F is the EBSD pattern of sample No. 6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present inventors have investigated from various angles to realize a copper alloy sheet that can obtain sufficient strength while the total amount of Ni and Si added is 6.50 mass% or less. As a result, they have found that a specific metal structure (hereinafter also referred to as "deformation twins") in which the (111) plane is oriented in a specific direction in an electron backscatter diffraction (EBSD) pattern is very effective for improving strength. Then, by setting the total amount of Ni and Si added to 6.50 mass% or less, setting the average particle diameter of precipitate particles measured by small angle X-ray scattering within a predetermined range, and setting the area ratio of the (111) plane to 3% or more in an EBSD pattern obtained from a cross section parallel to the rolling direction and the sheet thickness direction, a copper alloy sheet that can obtain sufficient strength has been realized.
[0014] The following provides details of each requirement stipulated by the embodiment of the present invention.
[0015] <1. Ingredient composition> The copper alloy sheet according to the embodiment of the present invention preferably has a composition containing Ni: 2.00 to 5.00 mass %, Si: 0.50 to 1.50 mass %, with the balance being Cu and unavoidable impurities. Each element will be described in detail below.
[0016] (Ni:2.00~5.00% by mass) Ni, when added together with Si, forms Ni-Si compounds (e.g., Ni 2 Ni is an element that can precipitate silicon compounds (Si compounds) and improve strength. It is also an element that easily induces deformation twins. To effectively exert these effects, the Ni content is set to 2.00 mass% or more. On the other hand, if excessive Ni is added, the precipitates tend to become coarse and deformation twins become less likely to appear. Therefore, the Ni content is set to 5.00 mass% or less.
[0017] (Si:0.50~1.50% by mass) When Si is added together with Ni, it forms Ni-Si compounds (e.g., Ni 2 Si is an element that can precipitate Si compounds and improve strength. It is also an element that easily induces deformation twins. To effectively exert these effects, the Si content is set to 0.50 mass% or more. On the other hand, if excessive Si is added, the precipitates tend to become coarse and deformation twins become less likely to appear. Therefore, the Si content is set to 1.50 mass% or less.
[0018] The copper alloy sheet according to the embodiment of the present invention contains the above-mentioned composition, and in one embodiment of the present invention, the balance is preferably copper and inevitable impurities. As inevitable impurities, the inclusion of elements brought in due to the conditions of raw materials, materials, manufacturing facilities, etc. is permitted.
[0019] Furthermore, the copper alloy sheet according to the embodiment of the present invention may selectively contain the following arbitrary elements as necessary, and the properties of the copper alloy sheet are further improved depending on the components contained.
[0020] (At least one selected from the group consisting of Al, Mn, Cr, Ti, Zr, P, Ag, and Mg is 0.10 mass% or less, and the total amount is more than 0 mass% and 0.50 mass% or less) Al, Mn, Cr, Ti, Zr, P, Ag, and Mg have the effect of further improving strength and / or heat resistance and also improving workability (press punching ability) when coexisting with Ni-Si based compounds. In order to effectively exhibit these effects, it is preferable to contain at least one selected from the group consisting of Al, Mn, Cr, Ti, Zr, P, Ag, and Mg in a total amount of more than 0 mass%. However, if the above elements are added in excess, deformation twins are less likely to appear, the strength improving effect of the Ni-Si based compounds may decrease, and coarse precipitates may occur, causing a decrease in workability (bendability). Therefore, it is preferable to set at most 0.10 mass% of at least one selected from the group consisting of Al, Mn, Cr, Ti, Zr, P, Ag, and Mg, and set their total content at most 0.50 mass%.
[0021] <2. Average particle diameter of precipitate particles> In the copper alloy sheet according to the embodiment of the present invention, the average particle diameter of the precipitate particles measured by small angle X-ray scattering is 1.0 nm to 4.5 nm. If the average particle diameter of the precipitate particles is less than 1.0 μm, sufficient precipitation strengthening by the precipitates cannot be obtained. The average particle diameter of the precipitate particles is preferably 3.0 nm or more, more preferably 3.5 nm or more. On the other hand, if the average particle diameter of the precipitate particles exceeds 4.5 nm, the number of large precipitate particles is large and / or the interaction with dislocations is weakened, and the appearance amount of deformation twins is reduced, and the strength is reduced. In addition, the precipitate particles may be Ni-Si compound particles in consideration of the above-mentioned component composition.
[0022] The average particle diameter of the above precipitate particles is measured by small angle X-ray scattering. As described later, the presence of precipitate particles such as Ni-Si compound particles can be confirmed by TEM observation, for example, but in the case of cold-rolled material, their size cannot be accurately measured due to the influence of dislocation contrast. Small angle X-ray scattering is a typical method for investigating structural information on the nanometer order. When a material is irradiated with X-rays, the incident X-rays reflect the information of the electron density distribution inside the material, and scattered X-rays are generated around the incident X-rays. For example, if there are particles or regions with non-uniform electron density in the material, the X-rays interfere with each other and scattering due to density fluctuations occurs. If this is a metal such as a copper alloy, scattering due to the particles is observed if minute precipitate particles such as Ni-Si compounds on the nanometer order are present in the copper alloy structure. The region where this scattered X-ray occurs is a measurement angle (2θ) of 0.1 to 10 degrees or less when X-rays with a wavelength of 1.54 Å using a Cu target are incident perpendicularly to the measurement region. In the small-angle X-ray scattering method, information such as the size and distribution of minute precipitate particles on the nanometer order can be obtained by analyzing this scattered X-ray.
[0023] In order to measure the average particle diameter of the precipitate particles, first, an X-ray scattering intensity profile measured by a small-angle X-ray scattering method is obtained. This X-ray scattering intensity profile is obtained, for example, with the vertical axis representing the X-ray scattering intensity and the horizontal axis representing the scattering vector q (nm-1) depending on the measurement angle 2θ and the wavelength λ. The average particle diameter of the precipitate particles can be obtained by fitting the measured X-ray scattering intensity to the X-ray scattering intensity calculated from a theoretical formula represented by a function of particle diameter and size distribution by a nonlinear least squares method so that they are close to each other. At this time, the X-ray scattering intensity profile may also include the influence of scattering due to dislocations introduced by cold rolling. That is, in the embodiment of the present invention, the "average particle diameter of the precipitate particles" may be the particle size of the precipitate particles including the influence of scattering due to dislocations.
[0024] The copper alloy sheet according to the embodiment of the present invention may contain precipitate particles such as Ni-Si based compounds as described above. In this specification, the term "Ni-Si compound" refers to a compound that mainly contains Ni and Si, such as Ni 2 It may be, but is not limited to, a Si compound, and may contain impurities other than Ni and Si (such as S). The presence or absence of precipitate particles such as Ni-Si based compounds may be confirmed as follows. First, a disk-shaped specimen with a diameter of 3 mm was punched in the thickness direction (hereinafter also referred to as "ND"), and then a wedge-shaped thin film specimen with a thickness of 150 to 250 nm was obtained near the center of the thickness of the plate by electrolytic polishing. Using a transmission electron microscope (TEM), an accelerating voltage of 200 kV and an observation magnification of 50,000 times or more were used to observe the copper alloy crystal grains (recrystallized grains) in a field of view of 250 nm x 250 nm. <110> By observing the copper alloy sheet as a specimen, the presence or absence of precipitate particles such as Ni-Si compounds can be confirmed. Examples of the observation are shown in FIG. 1A and FIG. 1B. FIG. 1A shows a TEM image of the copper alloy sheet after aging treatment in Test No. 1 of the embodiment described later, and FIG. 1B shows a TEM image of the copper alloy sheet after the second cold rolling in Test No. 1. As shown in FIG. 1A and FIG. 1B, the presence of precipitate particles 1 such as Ni-Si compounds can be confirmed in the circled area. In addition, when the copper alloy sheet has the above-mentioned composition, a person skilled in the art can understand that the precipitate is a Ni-Si compound by the above-mentioned TEM observation, but the precipitate may be directly confirmed to be a Ni-Si compound by analyzing the precipitate by, for example, TEM-EDX.
[0025] Precipitate particles such as Ni-Si compounds may be generated after aging treatment at a temperature of 400 to 500° C. for 30 minutes or more in the manufacturing method of the copper alloy sheet described later, and will not disappear or change significantly in size unless there is a subsequent heating step, for example, at a temperature of more than 350° C. Therefore, the presence or absence of precipitate particles such as Ni-Si compounds may be confirmed in the final product, or may be confirmed after aging treatment, for example.
[0026] <3. The area ratio of the (111) plane in the electron backscatter diffraction pattern obtained from a cross section parallel to the rolling direction and plate thickness direction is 3% or more> In the copper alloy sheet according to the embodiment of the present invention, the area ratio of the (111) plane in the electron backscatter diffraction (EBSD) pattern obtained from a cross section parallel to the rolling direction (hereinafter also referred to as "RD") and the sheet thickness direction (when the direction perpendicular to RD and ND is TD, the cross section perpendicular to TD) is 3% or more. Here, as the definition of the EBSD pattern in this specification, those with an orientation deviation of ±5° or less from the crystal plane belong to the same crystal plane (orientation factor), and the boundary between crystal grains with an orientation difference of 5° or more between adjacent crystal grains is defined as a crystal grain boundary. In other words, "the area ratio of the (111) plane in the EBSD pattern obtained from the cross section parallel to the rolling direction and the sheet thickness direction is 3% or more" means "the total area ratio of the planes with an orientation difference of ±5° or less from the (111) plane in the EBSD pattern obtained from the cross section parallel to the rolling direction and the sheet thickness direction is 3% or more". The copper alloy sheet according to the embodiment of the present invention has sufficient strength by adjusting the composition to the above, setting the average particle diameter of the precipitate particles to the above, and setting the area ratio of the (111) plane to 3% or more. If the area ratio of the (111) plane is less than 3%, sufficient strength cannot be obtained.
[0027] In the embodiment of the present invention, the area ratio of the (111) plane is confirmed as follows. First, a cross section parallel to the rolling direction and the sheet thickness direction is exposed by machining. Then, an electron backscatter diffraction (EBSD) pattern is obtained from a field of view of 40 μm×40 μm at a magnification of 1000 to 2000 times from the cross section using a scanning electron microscope with an electron backscatter diffraction device (SEM-EBSD device). Since the analysis results may vary between the surface and the center in the sheet thickness direction, the position of the field of view in the sheet thickness direction is within the range of the center in the sheet thickness direction of the copper alloy sheet ± sheet thickness × 25%. The rolling direction of the field of view does not particularly affect the analysis results, so it may be any position. In addition, the position of the TD of the exposed cross section may be any position since it does not particularly affect the analysis results. The present inventors also discovered that deformation twins, which are effective in improving strength, have the following two patterns (Pattern A and Pattern B) in EBSD patterns obtained from cross sections parallel to the rolling direction and plate thickness direction. "Pattern A TD / / <211> ; RD / / <110> ; and ND / / <111> [Pattern B] TD / / <110> ; RD / / <211> ; and ND / / <111> The area ratio of the (111) plane is defined as the ratio of the total area of the regions satisfying either the above pattern A or pattern B.
[0028] The area ratio of the (111) plane increases after the second cold rolling performed at a total rolling reduction of 50% or more and less than 90% in the manufacturing method of the copper alloy sheet described later, and will not decrease at least unless there is a subsequent heating step at a temperature of more than 350° C. Therefore, the area ratio of the (111) plane may be confirmed in the final product or after the second cold rolling.
[0029] The thickness of the copper alloy sheet according to the embodiment of the present invention is not particularly limited, but may be, for example, 100 μm (i.e., 0.100 mm) or more and 20 mm or less.
[0030] The copper alloy sheet according to the embodiment of the present invention can obtain sufficient strength by satisfying the above requirements. Specifically, even when the Ni content and the Si content are low (for example, Ni: 2.00 mass% and Si: 0.50 mass%), the Vickers hardness HV (load 49.0 N) can be at least 250 or more. When the Ni content and the Si content are relatively high (for example, Ni: 4.0 mass% or more and Si: 1.1 mass% or more), the Vickers hardness HV (load 49.0 N) can be 300 or more.
[0031] <4. Manufacturing method> An example of a method for producing a copper alloy sheet according to an embodiment of the present invention is (A) preparing a copper alloy ingot having the above-mentioned composition; (B) heating the copper alloy ingot to 800 to 1050°C; (C) hot rolling the heated copper alloy ingot at a total rolling reduction of 55% or more to obtain a copper alloy plate; (D) performing a first cold rolling on the hot rolled copper alloy sheet; (E) subjecting the copper alloy sheet that has been subjected to the first cold rolling to a solution treatment; (F) subjecting the solution-treated copper alloy sheet to aging treatment at a temperature of 400 to 500°C for 30 minutes to 10 hours; (G) subjecting the aging-treated copper alloy sheet to a second cold rolling at a total rolling reduction of 50% or more and less than 90%. By the above-mentioned manufacturing method, a copper alloy sheet having sufficient strength can be manufactured. Each step will be described in detail below.
[0032] (A) The process of preparing a copper alloy ingot First, the copper alloy having the above-mentioned composition is melted and cast by a known method to prepare a copper alloy ingot. For example, the copper alloy having the above-mentioned composition can be melted in air under a charcoal cover in a crypt furnace, and then an ingot can be cast.
[0033] (B) Heating process After step (A), the copper alloy ingot is heated to 800 to 1050° C. By setting the heating temperature to 800 to 1050° C., it is possible to obtain a desired metal structure in the final product. If necessary, the temperature may be held for a certain period of time (for example, 10 minutes or more).
[0034] (C) Hot rolling process After step (B), the copper alloy ingot is hot-rolled at a total rolling reduction of 55% or more. If the total rolling reduction is less than 55%, deformation twins do not grow sufficiently in the final product, and specifically, the area ratio of the (111) plane in the electron backscatter diffraction pattern obtained from a cross section parallel to the rolling direction and the plate thickness direction is less than 3%. The number of passes of the hot rolling is not particularly limited.
[0035] The cooling after rolling may be allowed to stand, but is preferably rapid cooling by water cooling or the like. When rapid cooling by water cooling or the like is performed, the cooling start temperature is preferably 750 to 850°C, and the average cooling rate to the temperature of the first cold rolling is preferably 50 to 100°C / sec. By adjusting the cooling in this way, Ni and Si are easily dissolved, and the formation of unnecessary compounds is easily suppressed. After cooling, the surface in the plate thickness direction may be cut to remove oxide scale.
[0036] (D) A step of performing a first cold rolling After step (C), the first cold rolling is performed. By performing the first cold rolling, the recrystallized grain structure of the copper alloy by the solution treatment described later can be formed to a uniform size, and the plastic deformation accompanying the second cold rolling described later can be made uniform. The first cold rolling can be performed, for example, at 10°C or more and 200°C or less. The number of passes and the total rolling reduction of the first cold rolling can be appropriately determined in relation to the target plate thickness and the total rolling reduction in the above-mentioned hot rolling and the second cold rolling described later, but the total rolling reduction of the first cold rolling is preferably 80% or more, more preferably 90% or more.
[0037] (E) Solution treatment process After step (D), a solution treatment is performed. The solution treatment is performed under conditions that precipitates such as Ni-Si compounds by aging treatment described later and that Ni-Si compounds that may precipitate by melt casting and / or hot rolling are redissolved in order to set the average particle diameter of the precipitate particles to a predetermined value. If the crystal grains (recrystallized grains) of the copper alloy after the solution treatment become coarse, the strength improvement effect of the subsequent second cold rolling cannot be obtained, so the solution treatment is performed under conditions that do not cause the crystal grains to become too coarse (for example, the size of the crystal grains of the copper alloy by the cutting method becomes 150 μm or less). Therefore, the solution treatment may be performed, for example, by holding at 850 to 1050 ° C for 10 to 60 minutes. After heating and holding, the copper alloy may be cooled to room temperature at an average cooling rate of 50 to 150 ° C / s. The size of the crystal grains (recrystallized grains) of the copper alloy can be measured, for example, by polishing the surface by a mechanical method, chemically etching it to reveal the metal structure, and then taking a photograph taken with an optical microscope near the center of the plate thickness. The size of the crystal grains (recrystallized grains) of the copper alloy can be measured by counting the number of crystal grains that are completely cut by a line of a known length (for example, 650 μm) in the plate thickness direction along three points on a photograph taken with an optical microscope with reference to JIS H 0501, and averaging the cut lengths.
[0038] (F) Aging treatment at a temperature of 400 to 500°C for 30 minutes to 10 hours After step (E), aging treatment is performed at a temperature of 400 to 500°C for 30 minutes to 10 hours. If the temperature is less than 400°C or the time is less than 30 minutes, the average particle diameter of the precipitate particles may become small (e.g., less than 1.0 nm), or precipitate particles such as Ni-Si compounds may not precipitate. On the other hand, if the temperature is more than 500°C or the time is more than 10 hours, the workability may decrease, and the average particle diameter of the precipitate particles may become large (e.g., more than 4.5 nm). There are no particular limitations on the cooling after heating, and the product may be allowed to cool or may be rapidly cooled by water cooling or the like.
[0039] (G) performing a second cold rolling process at a total reduction of 50% or more but less than 90%; After step (F), the second cold rolling is performed with a total reduction of 50% or more but less than 90%. If the total reduction is less than 50% or more than 90%, deformation twins do not grow sufficiently, and specifically, the area ratio of the (111) plane in the electron backscatter diffraction pattern obtained from a cross section parallel to the rolling direction and the sheet thickness direction is less than 3%. In addition, if the total reduction is 90% or more, the influence of scattering due to processing structures such as dislocations and / or atomic vacancies also increases, and as a result, the calculation accuracy of the average particle diameter of the precipitate particles decreases, and the average particle diameter may be measured as being large. The second cold rolling can be performed, for example, at a temperature of 10°C or more and 200°C or less.
[0040] The manufacturing method of the copper alloy sheet according to the embodiment of the present invention may include other steps as long as they do not deviate from the purpose of the embodiment of the present invention, but for example, when another step is included after the second cold rolling and the other step includes heating, the heating temperature needs to be 350° C. or less in order to obtain a desired metal structure. For example, after the second cold rolling, stress relief annealing may be performed under conditions that do not cause formation of precipitates and / or recrystallization and do not reduce strength.
[0041] Although an example of the manufacturing method of the copper alloy sheet according to the embodiment of the present invention has been described, a person skilled in the art who understands the desired properties of the copper alloy sheet according to the embodiment of the present invention may find a method for manufacturing a copper alloy sheet having the desired properties according to the embodiment of the present invention through trial and error, other than the above manufacturing method. EXAMPLES
[0042] The following examples are provided to more specifically describe the embodiments of the present invention. The embodiments of the present invention are not limited to the following examples, and may be modified as appropriate within the scope of the above and below-described aims, and all of these are included in the technical scope of the embodiments of the present invention.
[0043] A copper alloy containing 4.0 mass% Ni and 1.1 mass% Si, with the balance being Cu and inevitable impurities, was melted in a crucible furnace under a charcoal coating in the atmosphere to produce an ingot of 180 mm (RD) × 80 mm (TD) × 45 mm (ND). This ingot was heated in the temperature range of 900 - 970 °C for 30 minutes or more and then hot-rolled to a plate thickness of 20 mm (i.e., after hot-rolling with a total reduction ratio of 55.6%), and then water-cooled from 750 - 850 °C to room temperature at an average cooling rate of 50 - 100 °C / s to obtain a copper alloy plate (hot-rolled material) with a thickness of 20 mm. To remove the oxide scale on the surface of this hot-rolled material, the surface was cut. Then, as the first cold rolling, it was rolled to a plate thickness of 2 mm at room temperature, and then solution treatment (held at 850 - 1050 °C for 10 - 60 minutes and then cooled to room temperature at an average cooling rate of 50 - 150 °C / s) was performed. Note that this condition is an example of the condition for redissolving the Ni-Si-based compounds that can precipitate during melting casting and / or hot rolling. The size of the crystal grains of the copper alloy by the cutting method after solution treatment was 10 - 100 μm. After solution treatment, aging treatment was performed under the conditions shown in Table 1 described later. After aging treatment, the second cold rolling was performed at room temperature under the conditions shown in Table 1 described later to obtain copper alloy plates (plate thickness 0.14 - 1.0 mm) of Sample Nos. 1 - 6. Note that Samples Nos. 4 - 6 were not subjected to aging treatment for comparison.
[0044] For Sample Nos. 1 - 6, in the following manner, the presence or absence of precipitate particles such as Ni-Si-based compounds was confirmed, the average particle diameter of the precipitate particles was measured, the area ratio of deformation twins was measured, and hardness measurement was performed to confirm whether the copper alloy plate had sufficient strength. Note that the confirmation of the presence or absence of precipitate particles such as Ni-Si-based compounds was performed after aging treatment. However, since the subsequent process was only the second cold rolling and did not include a process of heating above 350 °C, for example, the precipitate confirmed after aging treatment was considered to be confirmed in the same manner in the final form (i.e., after the second cold rolling). Also, the confirmation of the area ratio of deformation twins and the confirmation of whether it had sufficient strength were performed after the second cold rolling.
[0045] <Confirmation of the presence or absence of precipitate particles such as Ni-Si-based compounds> Each sample was punched out in the thickness direction to a disk shape with a diameter of 3 mm. Then, a wedge-shaped thin film specimen with a thickness of 150 to 250 nm was obtained near the center of the thickness direction using a Tenupol-5 manufactured by Struers by the electrolytic thin film method. Then, using a JEOL field emission transmission electron microscope JEM-2010F with an accelerating voltage of 200 kV and an observation magnification of 50,000 times or more, the crystal grains (recrystallized grains) in a field of view of 250 nm × 250 nm were observed in the electrolytically polished observation surface (surface perpendicular to the ND) with an incident azimuth. <110> The presence or absence of precipitate particles such as Ni-Si compounds was confirmed by observing the specimen under these conditions.
[0046] <Measurement of the average particle diameter of precipitate particles> The average particle diameter of the precipitate particles of each sample was measured by the X-ray small angle scattering method using a horizontal X-ray diffractometer (Rigaku Corporation, SmartLab). The test piece size was 10 mm (TD) × 20 mm (RD) × 22 μm (ND). The test piece was prepared by polishing the outermost surface of one side of the copper alloy plate to produce a flat surface, and then adjusting the thickness from the back side and performing a thinning process to about 22 μm. X-rays with a wavelength of 0.154186 nm were vertically incident on the center of the flat surface in a slit shape of 0.5 mm × 10 mm, and X-rays scattered backward from the test piece at angles of 0.1 to 10 degrees with respect to the incident X-rays were detected to obtain a scattering intensity profile. At this time, the sampling width was 0.02° step, and the target and target output were Cu and 45 kV, 200 mA, respectively. The average particle diameter of the precipitate particles was calculated by fitting the measured X-ray scattering intensity with the X-ray scattering intensity value obtained using the particle size and pore analysis software NANO-Solver (Ver.3.7.3.1) made by Rigaku Corp. using the nonlinear least squares method so as to be close to each other. Note that the analytical model assumes that the precipitate particles are perfectly spherical, calculates the scattering intensity using a theoretical formula, and fits the experimental values and analytical results to obtain the average particle diameter of the precipitate particles.
[0047] <Measurement of area ratio of deformation twins> A cross section parallel to the rolling direction and the sheet thickness direction (cross section perpendicular to TD) was exposed by machining. Then, an electron backscatter diffraction (EBSD) pattern was obtained from a field of view of 40 μm×40 μm at a magnification of 1000 to 2000 times using a scanning electron microscope equipped with an electron backscatter diffraction device manufactured by JEOL Ltd. The position of the field of view in the sheet thickness direction was within the range of the center in the sheet thickness direction of the copper alloy sheet ± sheet thickness × 25%. In the above EBSD pattern, the ratio of the total area of the following patterns A and B was defined as the area ratio of deformation twins (i.e., the area ratio of the (111) plane in the EBSD pattern obtained from a cross section parallel to the rolling direction and the sheet thickness direction). "Pattern A TD / / <211> ; RD / / <110> ; and ND / / <111> [Pattern B] TD / / <110> ; RD / / <211> ; and ND / / <111>
[0048] FIG. 2A shows the EBSD pattern for Test No. 1, FIG. 2B shows the EBSD pattern for Test No. 2, FIG. 2C shows the EBSD pattern for Test No. 3, FIG. 2D shows the EBSD pattern for Test No. 4, FIG. 2E shows the EBSD pattern for Test No. 5, and FIG. 2F shows the EBSD pattern for Test No. 6. In addition, for Figures 2A to 2F, original drawings in which the difference in crystal planes can be identified by color have been submitted as a document to enable understanding of the parts corresponding to the (111) plane and the difference between Pattern A and Pattern B within the (111) plane. Please refer to these original drawings as necessary. In the original drawings, the colored parts correspond to the (111) plane, the pink parts indicate Pattern A, and the green parts indicate Pattern B.
[0049] <Hardness measurement> For specimens with a thickness of 0.4 mm or more, the Vickers hardness was measured on a surface perpendicular to the rolling direction, and for specimens with a thickness of less than 0.4 mm, the micro Vickers hardness was measured. The Vickers hardness was measured in accordance with the micro hardness test method specified in JIS-Z2248, with a test load of 49.0 N (i.e. 5 kgf).
[0050] The measurement results are shown in Table 1. In Table 1, the "average particle diameter of precipitate particles" shows only the results of Tests 1 to 3 in which the presence or absence of precipitate particles such as Ni-Si compounds was confirmed as described above.
[0051] [Table 1]
[0052] The results in Table 1 can be considered as follows: Test Nos. 1 and 2 in Table 1 all satisfied the requirements defined in the embodiment of the present invention, and had sufficient strength (Vickers hardness of 300 or more) when containing 4.0 mass% Ni and 1.1 mass% Si. On the other hand, Test Nos. 3 to 6 in Table 2 all did not satisfy the requirements defined in the embodiment of the present invention, and did not obtain sufficient strength.
[0053] In Test No. 3, since the total reduction rate during the second cold rolling was 90% or more, the average particle diameter of the precipitate particles measured by small-angle X-ray scattering exceeded 4.5 nm. As a result, the area ratio of deformation twins was less than 3%, and the Vickers hardness was less than 300.
[0054] In Test Nos. 4 to 6, since aging treatment was not performed, no precipitate particles such as Ni-Si compounds were observed, and it is considered that the average particle diameter of the precipitate particles could not be measured (or was small) by small-angle X-ray scattering method. As a result, the Vickers hardness was less than 300. [Explanation of symbols]
[0055] 1 Precipitate particles
Claims
1. The composition of the components is Ni: 2.00 to 5.00% by mass, Si: 0.50 to 1.50 mass%; and The balance is composed of Cu and inevitable impurities. The average particle diameter of the precipitate particles is 1.0 nm to 4.5 nm as measured by small angle X-ray scattering; A copper alloy sheet, in which an area ratio of (111) planes in an electron backscatter diffraction pattern obtained from a cross section parallel to the rolling direction and thickness direction is 3% or more.
2. The copper alloy sheet according to claim 1, further comprising at least one selected from the group consisting of Al, Mn, Cr, Ti, Zr, P, Ag and Mg, each of which is 0.10 mass% or less, and a total of more than 0 mass% and 0.50 mass% or less.
3. preparing a copper alloy ingot having a composition consisting of 2.00 to 5.00 mass% Ni, 0.50 to 1.50 mass% Si, and the balance being Cu and unavoidable impurities; heating the copper alloy ingot to 800 to 1050°C; hot rolling the heated copper alloy ingot at a total rolling reduction of 55% or more to obtain a copper alloy plate; A step of performing a first cold rolling on the hot-rolled copper alloy sheet; A step of subjecting the copper alloy sheet that has been subjected to the first cold rolling to a solution treatment; A step of subjecting the solution-treated copper alloy sheet to an aging treatment at a temperature of 400 to 500° C. for 30 minutes to 10 hours; A step of subjecting the aging-treated copper alloy sheet to a second cold rolling at a total reduction ratio of 50% or more and less than 90%; The method for producing a copper alloy sheet according to claim 1, comprising:
4. preparing a copper alloy ingot having a component composition containing Ni: 2.00 to 5.00 mass%, Si: 0.50 to 1.50 mass%, and at least one selected from the group consisting of Al, Mn, Cr, Ti, Zr, P, Ag, and Mg in an amount of 0.10 mass% or less, with a total amount of more than 0 mass% and 0.50 mass% or less, with the balance being Cu and unavoidable impurities; heating the copper alloy ingot to 800 to 1050°C; hot rolling the heated copper alloy ingot at a total rolling reduction of 55% or more to obtain a copper alloy plate; A step of performing a first cold rolling on the hot-rolled copper alloy sheet; A step of subjecting the copper alloy sheet that has been subjected to the first cold rolling to a solution treatment; A step of subjecting the solution-treated copper alloy sheet to an aging treatment at a temperature of 400 to 500° C. for 30 minutes to 10 hours; A step of subjecting the aging-treated copper alloy sheet to a second cold rolling at a total reduction ratio of 50% or more and less than 90%; The method for producing a copper alloy sheet according to claim 2, comprising:
Citation Information
Patent Citations
High strength copper alloy material, and method of manufacturing the same
JP2012162782A
Cu-Ni-Si BASED ALLOY AND Cu-Co-Si BASED ALLOY FOR ELECTRONIC MATERIAL, AND METHOD OF MANUFACTURING THE SAME
JP2012224898A
Cu-Ni-Si BASED COPPER ALLOY
JP2014173167A
Copper alloy sheet material and production method thereof
JP2015034336A
High strength copper alloy thin sheet material and production method thereof
JP2015161009A