Manufacturing method of rolling roll

The method enhances bondability and reduces cracks in rolling rolls by pre-sintering the outer ring before main sintering, stabilizing the bond and reducing manufacturing complexity and costs.

JP2024145342AInactive Publication Date: 2024-10-15MMC RYOTEC CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023057648
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing rolling rolls face issues with bondability between inner and outer layer rings, leading to cracks and require large-scale, complex manufacturing equipment, with potential for damage and high costs due to insufficient bonding strength and tensile stress.

Method used

A method involving pre-sintering the outer ring at a lower temperature than the main sintering temperature, followed by fitting and main sintering to join the inner and outer rings, ensuring stable bonding and reducing thermal deformation, with compressive stress enhancing the strength of the outer ring.

Benefits of technology

Improves bondability, reduces cracks, simplifies manufacturing equipment, and lowers costs by reusing worn rolls, while ensuring high bonding strength and precision alignment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145342000001_ABST
    Figure 2024145342000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method of a rolling roll, capable of enhancing bondability between an inner layer ring and an outer layer ring, reducing generation of crack or fracture on a fitting face of the rings, and suppressing a manufacturing facility of a rolling roll from becoming a large scale and complicated.SOLUTION: A manufacturing method of a rolling roll includes: a temporary sintering step of temporarily sintering an outer layer ring molding made by subjecting a base powder to pressed powder molding so as to obtain an outer layer ring temporary sintered body; and a regular sintering step of sintering a rolling ring intermediate sintered body obtained by fitting an inner peripheral surface of the outer layer ring temporary sintered body and an external peripheral surface of a regularly sintered inner layer ring 11, at a regular sintering temperature higher than a temporary sintering temperature in the temporary sintering step so as to regularly sinter the outer layer ring temporary sintered body and obtain an outer layer ring 12, and bonding the outer layer ring 12 with the inner layer ring 11 so as to obtain a rolling roll 2. The temporary sintering temperature in the temporary sintering step is -100°C or more and -10°C or less relative to the regular sintering temperature in the regular sintering step.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a rolling roll. [Background technology]

[0002] A rolling roll is used to roll various metal materials such as wire rods and steel bars by hot rolling, etc. As a conventional rolling roll, one in which an inner layer ring and an outer layer ring are each made of a cemented carbide is known (for example, Patent Documents 1 to 5).

[0003] In Patent Document 1, an outer ring and an inner ring, each made of a cemented carbide, are fitted together by shrink fitting or cold fitting, and then heated at a temperature at which the cemented carbide that constitutes the outer ring and the inner ring does not generate a liquid phase, causing the metal joining material made of copper, nickel, silver brazing material, or the like provided between the rings to become a liquid phase or a softened solid phase, and the temperature is then lowered to join the outer ring and the inner ring.

[0004] In addition, in Patent Document 2, the inner roll portion and the outer roll portion, which are made of the same cemented carbide, are integrated by engaging and combining their deformed circular outer and inner circumferences, making the outer roll portion replaceable.

[0005] In Patent Document 3, an outer ring and an inner ring, both of which are made of cemented carbide, are joined to each other by brazing, shrink fitting or other mechanical methods, making it possible to replace only the outer ring.

[0006] In Patent Document 4, an outer ring member compact and an inner ring member compact are each press-molded, and then these are fitted together and sintered at a predetermined temperature within the range of 1360 to 1400°C.

[0007] In addition, in Patent Document 5, a base material for a core (inner layer ring) is formed from powder of a first cemented carbide and sintered, a base material for a sleeve (outer layer ring) is formed from powder of a second cemented carbide and sintered, the sintered core is shrunk by placing it in liquid nitrogen, the shrunk sintered core is pressed into the opening of the sintered sleeve, the sintered core is thermally expanded to mechanically join with the sintered sleeve, and the assembled sintered core and sintered sleeve are then heated to a fusion temperature higher than the eutectic temperature of WC-Co and lower than the sintering temperature. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Japanese Patent Application Publication No. 49-105749 [Patent Document 2] Japanese Utility Model Application Publication No. 53-74447 [Patent Document 3] Japanese Utility Model Application Publication No. 59-135806 [Patent Document 4] JP 2004-255401 A [Patent Document 5] Patent No. 6794416 Summary of the Invention [Problem to be solved by the invention]

[0009] In this type of rolling roll, it is required to further improve the bonding between the inner layer ring and the outer layer ring, and to reduce the occurrence of cracks, breaks, etc. on the fitting surfaces between these rings, etc. There is also room for improvement in preventing the equipment for manufacturing the rolling roll from becoming large-scale and complicated.

[0010] One of the objects of the present invention is to provide a method for manufacturing a rolling roll that can improve the bonding strength between an inner layer ring and an outer layer ring, reduce the occurrence of cracks and breaks on the mating surfaces between these rings, and prevent the manufacturing equipment for the rolling roll from becoming large-scale and complicated. [Means for solving the problem]

[0011] In order to solve the above problems, the present invention provides the following means.

[0012] [First aspect of the present invention] A method for manufacturing a rolling roll having a rolling ring formed by bonding the outer peripheral surface of an inner layer ring made of cemented carbide to the inner peripheral surface of an outer layer ring made of cemented carbide, the method comprising: a preliminary sintering step in which an outer layer ring molded body formed by compacting a raw material powder is preliminary sintered to form a preliminary sintered outer layer ring body; and a main sintering step in which the inner peripheral surface of the preliminary sintered outer layer ring body is fitted with the outer peripheral surface of the sintered inner layer ring, and the intermediate sintered rolled ring body is sintered at a main sintering temperature higher than the preliminary sintering temperature in the preliminary sintering step to main sinter the preliminary sintered outer layer ring body to form the outer layer ring, and the outer layer ring and the inner layer ring are bonded to form the rolling ring, wherein the preliminary sintering temperature in the preliminary sintering step is -100°C or more and -10°C or less than the main sintering temperature in the main sintering step.

[0013] In the manufacturing method of the rolling roll of the present invention, the outer peripheral surface of the inner layer ring that has been sintered is fitted to the inner peripheral surface of the outer layer ring pre-sintered body that has been pre-sintered at a temperature lower than the main sintering temperature of the rolling ring, and the intermediate sintered rolled ring body is then sintered. During the main sintering, the pre-sintered outer layer ring body shrinks as its volume decreases. This allows the outer layer ring and the inner layer ring to be firmly bonded to each other after sintering. In addition, the occurrence of cracks or breaks on the fitting surfaces between these rings is suppressed.

[0014] Furthermore, when the rings are fitted together, the inner layer ring will not deform because it has already been fully sintered. On the other hand, the pre-sintered outer layer ring contains more pores inside than the inner layer ring, making it deformable. This allows these rings to be fitted together easily, improving workability during roll manufacturing. Furthermore, by deforming the pre-sintered outer layer ring to match the shape (standard shape) of the inner layer ring, which is not deformable, the accuracy of the coaxiality (concentricity) and roundness of the manufactured rolled ring is also improved.

[0015] For example, there is a risk that sufficient joint strength may not be obtained when the outer layer ring and the inner layer ring are joined by a metal joining material such as a brazing material as in the above Patent Document 1. Also, when the outer layer ring and the inner layer ring are joined by mechanical engagement as in the above Patent Documents 2 and 3, sufficient joint strength may not be obtained. On the other hand, in the present invention, the outer layer ring and the inner layer ring are bonded together by main sintering, so that the bonding strength between these rings can be stably increased.

[0016] Furthermore, for example, as in Patent Document 5 mentioned above, when an outer layer ring and an inner layer ring that have already been sintered are prepared, the inner layer ring is cooled to shrink it and fitted into the outer layer ring, and then the inner layer ring is thermally expanded to mechanically join them, tensile stress may be generated in the outer layer ring, which may cause cracks or the like to occur in the outer layer ring. On the other hand, in the present invention, the outer layer ring and the inner layer ring are joined by the main sintering, so that no tensile stress is generated in the outer layer ring, and the occurrence of cracks, etc. can be prevented. Furthermore, in the present invention, since the outer layer ring tends to have a compressive stress generated by the main sintering, the strength of the outer layer ring is further increased. In addition, in the present invention, cooling equipment for shrinking the inner layer ring by cooling is not required, and the manufacturing equipment can be simplified. In addition, the manufacturing process is shortened and the production efficiency is improved.

[0017] Furthermore, in the present invention, for example, a used rolling roll (rolling ring) that has been used in rolling and whose outer diameter has reached a predetermined discard diameter due to wear, regrinding, etc., can be reused as an inner layer ring. That is, unlike the manufacturing method of a rolling roll in which an outer layer ring and an inner layer ring that have been powder-pressed are fitted together and sintered as in the above-mentioned Patent Document 4, for example, according to the present invention, a used rolling roll that was conventionally discarded is used to make an inner layer ring by adjusting the outer shape, and only the outer layer ring is newly pressed and sintered (after temporary sintering, main sintering), thereby manufacturing a rolling roll. Therefore, the amount of expensive cemented carbide material used can be kept small, and manufacturing costs can be reduced. In addition, it is also possible to shorten the sintering time of the rolling ring, improving production efficiency.

[0018] The reason why the pre-sintering temperature in the pre-sintering step is set to be −100° C. or higher and −10° C. or lower with respect to the main sintering temperature in the main sintering step is as follows. If the pre-sintering temperature is -100°C or higher than the main sintering temperature, the pre-sintered outer ring body shrinks by a certain amount during pre-sintering, which can prevent uneven thermal deformation, gaps, and localized distortion from occurring on the mating surface between the outer ring and the inner ring during main sintering. This allows the strength of the manufactured rolling roll to be stably increased and prevents roll breakage, etc.

[0019] In addition, if the preliminary sintering temperature is -10°C or lower than the main sintering temperature, the outer layer ring molded body is prevented from being sintered accidentally (unintentionally), and the pores remain stable inside the preliminary sintered outer layer ring body after the preliminary sintering process, so that the preliminary sintered outer layer ring body can be maintained in a state in which it is easy to deform. In other words, the amount of deformation of the preliminary sintered outer layer ring body is ensured to be greater than a predetermined amount, so that the preliminary sintered outer layer ring body and the inner layer ring can be easily combined and fitted together.

[0020] As described above, according to the present invention, it is possible to improve the bonding strength between the inner layer ring and the outer layer ring, reduce the occurrence of cracks and fractures on the mating surfaces between these rings, and prevent the manufacturing equipment for the rolling roll from becoming large-scale and complicated. Furthermore, it is possible to reduce the manufacturing cost of the rolling roll.

[0021] [Aspect 2 of the present invention] 2. The method for producing a reduction roll according to aspect 1, wherein the main sintering temperature in the main sintering step is 1300° C. or higher and 1400° C. or lower.

[0022] In this case, regardless of the type of cemented carbide constituting the outer layer ring, the intermediate sintered rolled ring body obtained by fitting the provisionally sintered outer layer ring and the inner layer ring together can be sintered stably.

[0023] [Embodiment 3 of the present invention] In the sintering process, the central axes of the outer layer ring pre-sintered body and the inner layer ring are arranged to extend in the vertical direction, and the rolled ring intermediate sintered body is sintered by fitting an outer layer tapered surface provided on the inner surface of the outer layer ring pre-sintered body with an inner layer tapered surface provided on the outer surface of the inner layer ring.This is a method for manufacturing a rolling roll described in embodiment 1 or 2.

[0024] In this case, the outer layer ring pre-sintered body and the inner layer ring are fitted with a taper and arranged so that the central axis of each ring extends vertically, so that during the main sintering, a pressing force (load) acts on these fitting surfaces (outer layer tapered surface and inner layer tapered surface) in a direction perpendicular to the fitting surfaces due to the weight of the rings, etc. In other words, the outer layer tapered surface of the outer layer ring pre-sintered body and the inner layer tapered surface of the inner layer ring can be sintered while being pressed against each other. Therefore, the outer layer ring and the inner layer ring are more firmly joined to each other.

[0025] [Embodiment 4 of the present invention] A method for manufacturing a rolling roll as described in aspect 3, in which the minimum value of the inner diameter dimension of the outer layer tapered surface is smaller than the minimum value of the outer diameter dimension of the inner layer tapered surface, and the maximum value of the inner diameter dimension of the outer layer tapered surface is smaller than the maximum value of the outer diameter dimension of the inner layer tapered surface, and in the sintering process, a weight is placed on one of the outer layer ring pre-sintered body and the inner layer ring, which is positioned higher than the other, and the outer layer tapered surface and the inner layer tapered surface are slid by the weight of the other and the weight of the weight.

[0026] In this case, a larger pressing force (load) can be applied to the outer layer tapered surface and the inner layer tapered surface during the main sintering. This allows the outer layer ring and the inner layer ring to be more firmly bonded to each other. In addition, the outer layer tapered surface and the inner layer tapered surface slide and fit together, allowing the outer layer ring and the inner layer ring to be more precisely aligned coaxially (concentrically).

[0027] [Embodiment 5 of the present invention] A method for manufacturing a rolling roll according to aspect 3 or 4, wherein, in a cross section along the ring central axis, a first inclination angle at which the inner layer tapered surface is inclined with respect to the ring central axis and a second inclination angle at which the outer layer tapered surface is inclined with respect to the ring central axis are the same.

[0028] In this case, since the first inclination angle and the second inclination angle are the same, the inner layer tapered surface and the outer layer tapered surface can be closely attached to each other over a wide area. The outer layer ring pre-sintered body and the inner layer ring can be stably tapered and fitted, and the bonding strength between the outer layer ring and the inner layer ring after sintering can be stably increased.

[0029] [Aspect 6 of the present invention] A method for manufacturing a rolling roll according to any one of aspects 3 to 5, wherein, in a cross section along the ring central axis, a first inclination angle at which the inner layer tapered surface is inclined with respect to the ring central axis, and a second inclination angle at which the outer layer tapered surface is inclined with respect to the ring central axis, are each greater than 0° and less than 5°.

[0030] When the first inclination angle and the second inclination angle are each greater than 0°, the inner layer tapered surface and the outer layer tapered surface are reliably inclined with respect to the ring central axis, so that a pressing force (load) can be applied stably to the outer layer tapered surface and the inner layer tapered surface. Therefore, the bonding strength between the outer layer ring and the inner layer ring is more stably increased. It is more preferable that the first inclination angle and the second inclination angle are each greater than 0°30′.

[0031] Furthermore, when the first inclination angle and the second inclination angle are each 5° or less, for example, when a used inner layer ring is reused, the amount of processing (i.e., the amount of waste) of the cemented carbide cut to form the inner layer tapered surface can be reduced. In addition, the radial thickness of the manufactured rolled ring is prevented from becoming too large, resulting in bulky dimensions. It is more preferable that the first inclination angle and the second inclination angle are each 4° or less.

[0032] [Seventh aspect of the present invention] 7. The method for producing a rolling roll according to any one of aspects 1 to 6, further comprising a shaft fitted to an inner peripheral surface of the rolling ring, the rolling ring having an outer diameter of 300 mm or more and 450 mm or less.

[0033] The rolling roll having the above configuration is a composite roll equipped with a rolling ring and a shaft, and is called a clamp roll, etc. For example, compared with a rolling roll having a small diameter (outer diameter of 210 mm or less) called a Morgan roll, etc., the outer diameter of the rolling ring in the above composite roll is made large, so that the effect of reducing the manufacturing cost by reusing the above-mentioned inner layer ring is more remarkable. Effect of the Invention

[0034] According to the manufacturing method for a rolling roll of the above-mentioned aspect of the present invention, the bonding strength between the inner layer ring and the outer layer ring can be further improved, the occurrence of cracks and breaks on the mating surfaces between these rings can be reduced, and the manufacturing equipment for the rolling roll can be prevented from becoming large-scale and complicated. [Brief description of the drawings]

[0035] [Figure 1] FIG. 1 is a half cross-sectional view showing a roll manufactured by the method for manufacturing a roll of the present embodiment. [Diagram 2] FIG. 2 is a perspective view showing a rolling ring of a rolling roll. [Diagram 3] FIG. 3 is a diagram for explaining the method for manufacturing a roll, specifically, showing a cross-sectional view of a roll ring. [Figure 4] FIG. 4 is a diagram for explaining the method for manufacturing a rolling roll, specifically, showing a cross-sectional view of a rolling ring. [Diagram 5] FIG. 5 is a flow diagram showing a method for producing a reduction roll. [Figure 6] FIG. 6 is a diagram for explaining a modified example of the method for producing a rolling roll, specifically, showing a cross-sectional view of a rolling ring. [Figure 7]FIG. 7 is a diagram for explaining a modified example of the method for producing a rolling roll, specifically, showing a cross-sectional view of a rolling ring. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0036] A reduction roll 10 according to one embodiment of the present invention and a manufacturing method thereof will be described with reference to Fig. 1 to Fig. 5. The reduction roll 10 according to this embodiment is used for rolling various metal materials such as wire rods and steel bars by hot rolling or the like.

[0037] As shown in FIG. 1, the rolling roll 10 includes a shaft 1 centered on a central axis C, a rolling ring 2, a support portion 3, and a lateral pressure applying portion 4. The rolling roll 10 of this embodiment is a composite roll including the rolling ring 2 and the shaft 1, and is called a clamp roll or the like. The shaft 1, the rolling ring 2, the support portion 3, and the lateral pressure applying portion 4 are arranged coaxially with the central axis C as a common axis. The support portion 3 and the lateral pressure applying portion 4 are arranged at different positions from each other in the direction in which the central axis C extends. The central axis C may be referred to as the shaft central axis C, the ring central axis C, the roll central axis C, or the like.

[0038] [Direction definition] In this embodiment, the direction in which the central axis C extends is called the axial direction. In each drawing, the axial direction corresponds to the X-axis direction. In the axial direction, the direction from the lateral pressure imparting portion 4 to the support portion 3 (+X side) is called one axial side, and the direction from the support portion 3 to the lateral pressure imparting portion 4 (-X side) is called the other axial side.

[0039] The direction perpendicular to the central axis C is called the radial direction. Within the radial direction, the direction approaching the central axis C is called the radially inner direction, and the direction away from the central axis C is called the radially outer direction. Moreover, the direction going around the central axis C is called the circumferential direction.

[0040] 〔shaft〕 The shaft 1 is made of steel, iron, or the like. The shaft 1 extends along an axial direction. Both axial ends 1f, 1g of the shaft 1 are rotatably supported by a rolling mill (not shown). During rolling, the shaft 1 is rotationally driven by the rolling mill in a predetermined rotation direction among the circumferential directions, i.e., the rolling rotation direction.

[0041] An intermediate portion 1a of the shaft 1 located between both end portions 1f, 1g in the axial direction has a larger outer diameter than both end portions 1f, 1g of the shaft 1. The intermediate portion 1a has a first male thread portion 1b, a step portion 1c, a second male thread portion 1d, and a ring fitting portion 1e. In other words, the shaft 1 has the first male thread portion 1b, the step portion 1c, the second male thread portion 1d, and the ring fitting portion 1e.

[0042] The first male thread portion 1b is disposed at one axial end of the middle portion 1a of the shaft 1. The first male thread portion 1b is provided by machining a spiral male thread centered on the central axis C at one axial end of the outer circumferential surface of the middle portion 1a.

[0043] The step 1c and the second male thread 1d are disposed at the end of the intermediate portion 1a of the shaft 1 on the other axial side. At the end of the intermediate portion 1a on the other axial side, the step 1c is located on one axial side of the second male thread 1d. The end of the intermediate portion 1a on the other axial side has a smaller outer diameter than the other portion of the intermediate portion 1a on the other axial side. That is, the outer diameters of the step 1c and the second male thread 1d are smaller than the outer diameters of the first male thread 1b and the ring fitting portion 1e. The second male thread 1d is provided by machining the outer peripheral surface of the intermediate portion 1a on the end on the other axial side to form a helical male thread centered on the central axis C.

[0044] The ring fitting portion 1e is located between both axial ends of the intermediate portion 1a. The ring fitting portion 1e is disposed between the first male thread portion 1b and the step portion 1c in the axial direction. The ring fitting portion 1e has a cylindrical shape centered on the central axis C.

[0045] [Rolled ring] The rolled ring 2 is made of cemented carbide. The rolled ring 2 is, for example, mainly composed of WC and contains binder (binding phase) components such as Ni and Co. The rolled ring 2 is cylindrical or annular about a central axis C. In this embodiment, the rolled ring 2 is cylindrical and extends in the axial direction. The inner peripheral surface of the rolled ring 2 is fitted with the outer peripheral surface of the ring fitting portion 1e. That is, the shaft 1 is fitted with the inner peripheral surface of the rolled ring 2. In this embodiment, the axial dimension of the rolled ring 2 is approximately the same as the axial dimension of the ring fitting portion 1e. The outer diameter of the rolled ring 2 is, for example, 300 mm or more and 450 mm or less.

[0046] The rolled ring 2 has a caliber 2a. The caliber 2a is recessed radially inward from the outer circumferential surface of the rolled ring 2 and is groove-shaped extending in the circumferential direction. The caliber 2a is an annular groove centered on the central axis C. The caliber 2a is a forming groove for performing rolling processing on a metal material, which is a rolling material (work). In this embodiment, a plurality of calibers 2a are provided on the outer circumferential surface of the rolled ring 2 at intervals from each other in the axial direction. Note that in the rolled ring 2 shown in the drawings other than FIG. 1, the calibers 2a are omitted from the illustration.

[0047] 1, 2, and 4, the rolled ring 2 of this embodiment has a two-layer structure. The rolled ring 2 includes an inner layer ring 11 made of cemented carbide, and an outer layer ring 12 made of cemented carbide arranged adjacent to the radial outside of the inner layer ring 11. The cemented carbide materials (constituent components, composition, etc.) constituting the inner layer ring 11 and the outer layer ring 12 may be different from each other or may be the same as each other.

[0048] The inner layer ring 11 has a cylindrical or annular plate shape centered on the central axis C. In this embodiment, the inner layer ring 11 is cylindrical extending in the axial direction. The inner layer ring 11 is located at the radially inner portion of the rolled ring 2. The inner layer ring 11 constitutes the inner layer portion of the rolled ring 2. The inner peripheral surface of the inner layer ring 11 fits with the outer peripheral surface of the ring fitting portion 1e of the shaft 1.

[0049] The inner layer ring 11 has an inner layer tapered surface 11a arranged on the outer circumferential surface of the inner layer ring 11. The inner layer tapered surface 11a is a tapered surface centered on the central axis C, and the outer diameter dimension gradually changes as it approaches the axial direction. Specifically, in this embodiment, the inner layer tapered surface 11a is a tapered surface whose diameter increases as it approaches one axial side (+X side). Also, in this embodiment, the inner layer tapered surface 11a is arranged on the outer circumferential surface of the inner layer ring 11 over the entire axial length.

[0050] As shown in Figure 3, in a cross section along the central axis C of the rolled ring 2 (a cross section including the central axis C; a longitudinal cross section), the first inclination angle θ1 at which the inner layer tapered surface 11a is inclined with respect to the central axis C is, for example, greater than 0° and not more than 5°.

[0051] As shown in Figures 1, 2 and 4, the outer layer ring 12 has a cylindrical or annular plate shape centered on the central axis C. In this embodiment, the outer layer ring 12 has a cylindrical shape extending in the axial direction. The outer layer ring 12 is located at the radially outer portion of the rolled ring 2. The outer layer ring 12 constitutes the outer layer portion of the rolled ring 2. A caliber 2a is formed on the outer peripheral surface of the outer layer ring 12.

[0052] The outer layer ring 12 has an outer layer tapered surface 12a arranged on the inner peripheral surface of the outer layer ring 12. The outer layer tapered surface 12a is a tapered surface centered on the central axis C, and the inner diameter dimension gradually changes as it approaches the axial direction. Specifically, in this embodiment, the outer layer tapered surface 12a is a tapered surface whose diameter increases as it approaches one axial side (+X side). Also, in this embodiment, the outer layer tapered surface 12a is arranged on the inner peripheral surface of the outer layer ring 12 over the entire axial length.

[0053] As shown in FIG. 3, in a cross section along the central axis C of the rolled ring 2, a second inclination angle θ2 at which the outer layer tapered surface 12a is inclined with respect to the central axis C is, for example, greater than 0° and not more than 5°. In this embodiment, the first inclination angle θ1 and the second inclination angle θ2 are the same.

[0054] The outer peripheral surface of the inner layer ring 11 and the inner peripheral surface of the outer layer ring 12 are joined to each other by sintering. Specifically, the inner layer tapered surface 11a and the outer layer tapered surface 12a are joined to each other by sintering.

[0055] [Support part] As shown in Fig. 1, the support part 3 is attached to an end part on one axial side (+X side) of the middle part 1a of the shaft 1. The support part 3 is disposed radially outward from the end part on one axial side of the middle part 1a. In this embodiment, the support part 3 is cylindrical with the central axis C as its center.

[0056] The support portion 3 has a first female screw portion 3a on its inner peripheral surface. The support portion 3 is shaped like a nut. Therefore, the support portion 3 may be referred to as a support ring nut 3 or the like. The first female screw portion 3a of the support portion 3 is screwed into the first male screw portion 1b. In other words, the support portion 3 is detachably screwed onto the outer peripheral surface of the shaft 1. An end face of the support portion 3 facing the other axial side (-X side) comes into contact with an end face of the rolled ring 2 facing one axial side. As a result, the support portion 3 supports the rolled ring 2 from one axial side.

[0057] [Lateral pressure applying section] The lateral pressure applying portion 4 has a function of applying a pressing force, i.e., lateral pressure, from the axial direction to the rolled ring 2. The lateral pressure applying portion 4 is disposed on the other axial side of the rolled ring 2, and presses the rolled ring 2 towards one axial side. The lateral pressure applying portion 4 has a lateral pressure ring nut 6, an intermediate ring 7, and a male thread member 8.

[0058] The lateral pressure ring nut 6 is disposed on the other axial side of the rolled ring 2. The lateral pressure ring nut 6 is attached to the other axial end of the intermediate portion 1a of the shaft 1. The lateral pressure ring nut 6 is disposed radially outward from the other axial end of the intermediate portion 1a. The lateral pressure ring nut 6 is cylindrical and centered on the central axis C.

[0059] The lateral pressure ring nut 6 has a second female screw portion 6a on its inner circumferential surface. The second female screw portion 6a of the lateral pressure ring nut 6 is screwed into the second male screw portion 1d. That is, the lateral pressure ring nut 6 is detachably screwed onto the outer circumferential surface of the shaft 1.

[0060] The lateral pressure ring nut 6 has a nut body 6b, a protruding cylindrical portion 6c, and a female screw hole 6d. The nut body 6b has a cylindrical shape centered on the central axis C. The second female thread portion 6a is disposed on the inner circumferential surface of the nut body 6b.

[0061] The protruding tubular portion 6c protrudes from the outer periphery of the end face of the nut body 6b facing one axial direction side to the axial direction. The protruding tubular portion 6c is cylindrical and centered on the central axis C. The inner diameter of the protruding tubular portion 6c is larger than the inner diameter of the nut body 6b. The outer diameter of the protruding tubular portion 6c is the same as the outer diameter of the nut body 6b.

[0062] The female screw hole 6d penetrates the nut body 6b in the axial direction. The female screw hole 6d is located radially inward from the protruding tubular portion 6c. The female screw hole 6d opens on an end face of the nut body 6b facing one axial side and an end face facing the other axial side. That is, the female screw hole 6d penetrates the lateral pressure ring nut 6 in the axial direction. A plurality of female screw holes 6d are provided at intervals from each other in the circumferential direction. In this embodiment, for example, three or more female screw holes 6d are provided at equal pitches in the circumferential direction. The female screw hole 6d overlaps with the inner peripheral portion of the rolled ring 2 when viewed from the axial direction.

[0063] The interposition ring 7 is attached to the other axial end of the intermediate portion 1a of the shaft 1. The interposition ring 7 is disposed radially outward from the other axial end of the intermediate portion 1a. The interposition ring 7 is disposed axially between the lateral pressure ring nut 6 and the rolling ring 2. The interposition ring 7 is cylindrical and centered on the central axis C. The interposing ring 7 has a fitting cylindrical portion 7a and a pressing cylindrical portion 7b.

[0064] The fitting tubular portion 7a constitutes the other axial side portion of the intermediate ring 7. The fitting tubular portion 7a is disposed radially inside the protruding tubular portion 6c. The outer peripheral surface of the fitting tubular portion 7a contacts the inner peripheral surface of the protruding tubular portion 6c. The fitting tubular portion 7a fits into the inner peripheral surface of the protruding tubular portion 6c. The inner peripheral surface of the fitting tubular portion 7a contacts the outer peripheral surface of the step portion 1c. The fitting tubular portion 7a fits into the outer peripheral surface of the step portion 1c. That is, the intermediate ring 7 fits into the outer peripheral surface of the shaft 1. The end face of the fitting tubular portion 7a facing the other axial side faces or contacts the end face of the nut body 6b facing one axial side with a gap therebetween.

[0065] The pressing cylindrical portion 7b constitutes a portion of the intermediate ring 7 on one axial side. The pressing cylindrical portion 7b is disposed on one axial side of the protruding cylindrical portion 6c. The end face of the pressing cylindrical portion 7b facing one axial side contacts the end face of the rolled ring 2 facing the other axial side. The inner diameter of the end face of the pressing cylindrical portion 7b facing one axial side is equal to or larger than the inner diameter of the rolled ring 2. The outer diameter of the end face of the pressing cylindrical portion 7b facing one axial side is the same as the outer diameter of the rolled ring 2.

[0066] The male screw member 8 is columnar and extends in the axial direction. The male screw member 8 is, for example, a hexagonal socket bolt. A plurality of male screw members 8 are provided at intervals in the circumferential direction. Each male screw member 8 is screwed into each female screw hole 6d. An end portion of the male screw member 8 on one axial side can protrude toward one axial side from an end face of the nut body 6b facing the one axial side. An end portion of the male screw member 8 on one axial side contacts an end face of the fitting tubular portion 7a facing the other axial side. That is, the male screw member 8 contacts the intermediate ring 7 from the other axial side. By adjusting the amount of screwing of the male screw member 8 into the female screw hole 6d, the pressing force, i.e., the lateral pressure, that presses the rolled ring 2 toward one axial side via the intermediate ring 7 is adjusted.

[0067] [Procedure for attaching and detaching the rolling ring] In the roll 10 of this embodiment, the roll ring 2 is attached to and detached from the shaft 1, for example, in the following procedure.

[0068] With the support portion 3 attached to the middle portion 1a of the shaft 1, the rolled ring 2 is fitted to the middle portion 1a. After the rolled ring 2 is attached to the middle portion 1a, the intermediate ring 7 and the lateral pressure ring nut 6 are attached to the middle portion 1a.

[0069] The male screw member 8 provided on the lateral pressure ring nut 6 is operated with a work tool such as a hexagonal wrench, and the male screw member 8 is screwed into the female screw hole 6d toward one axial side, and the intermediate ring 7 is pressed toward one axial side by the male screw member 8. By performing this operation on each male screw member 8, a pressing force (lateral pressure) toward one axial side is applied to the rolled ring 2 via the intermediate ring 7. As a result, the rolled ring 2 is fixed to the shaft 1.

[0070] When removing the rolled ring 2 from the shaft 1, the above-described procedure is reversed. That is, the male screw member 8 is loosened to reduce the lateral pressure on the rolled ring 2, and the fixed state of the rolled ring 2 is released. Then, the lateral pressure ring nut 6, the intermediate ring 7, and the rolled ring 2 are removed from the shaft 1 in this order.

[0071] [Method of manufacturing rolling roll] Next, a method for manufacturing the roll 10 of this embodiment will be described. Specifically, the method for manufacturing the rolled ring 2 will be mainly described below.

[0072] As shown in FIG. 5, the manufacturing method of the rolling roll 10 (the manufacturing method of the rolled ring 2) includes an inner layer ring processing step S1, an outer layer ring forming step S2, a preliminary sintering step S3, an outer layer ring processing step S4, a main sintering step S5, an end face processing step S6, and an isostatic sintering step S7.

[0073] [Inner layer ring processing process] In the inner layer ring processing step S1, an inner layer ring 11 sintered (main sintering) at a temperature of 1300° C. to 1400° C. is prepared, and an inner layer tapered surface 11a is processed on the outer circumferential surface of this inner layer ring 11 by cutting, grinding, or the like.

[0074] In this embodiment, for example, a used rolled ring that has been used in rolling processing and whose outer diameter has reached a predetermined discard diameter (become equal to or smaller than the predetermined discard diameter) due to wear, regrinding, etc. is reused as the sintered inner layer ring 11. That is, the outer circumferential surface of the used rolled ring is processed by cutting, grinding, etc. to form the inner layer ring 11 having the inner layer tapered surface 11a.

[0075] However, without being limited to this, for example, an inner layer ring compact (not shown) may be obtained by compacting a raw powder of cemented carbide containing WC as the main component and binder (bonding phase) components such as Ni and Co, and then sintering the compact at a temperature of 1300°C or higher and 1400°C or lower. The outer peripheral surface of the obtained unused inner layer ring 11 may be processed by cutting or grinding to form the inner layer tapered surface 11a.

[0076] [Outer layer ring molding process] In the outer layer ring forming process S2, for example, a raw material powder of a cemented carbide containing WC as a main component and binder components such as Ni and Co is compacted to form an outer layer ring compact (not shown). The outer layer ring compact is annular about a central axis C, and specifically, is cylindrical or annular plate-like.

[0077] [Pre-sintering process] In the preliminary sintering step S3, the outer layer ring compact is subjected to preliminary sintering at a temperature lower than the main sintering temperature to obtain a preliminary sintered outer layer ring compact. Specifically, the preliminary sintering temperature in the preliminary sintering step S3 is set to be −100° C. or higher and −10° C. or lower than the main sintering temperature in the main sintering step S5 described later. A more preferable range of the preliminary sintering temperature is, for example, −60° C. or higher and −10° C. or lower than the main sintering temperature. The sintering time of the preliminary sintering is, for example, about 1 hour.

[0078] Due to this presintering, the volume of the presintered outer layer ring compact is reduced and shrinks more than the outer layer ring compact. More specifically, by presintering the outer layer ring compact, a bonding phase such as Ni, Co is melted and diffused between hard phases such as WC and bonded. There are many pores inside the outer layer ring compact, and the bonding phase melted by presintering fills these pores. Therefore, the volume of the presintered outer layer ring compact is reduced more than the outer layer ring compact, that is, it shrinks. In the preliminary sintering step S3, the outer layer ring is heated until this shrinkage occurs sufficiently (that is, until the preliminary sintered body of the outer layer ring shrinks from the outer layer ring compact by a predetermined amount or more), and this heated state is maintained.

[0079] [Outer layer ring processing process] In the outer layer ring processing step S4, the inner peripheral surface of the outer layer ring pre-sintered body is machined to have an outer layer tapered surface 12a by cutting, grinding, etc. Also, the outer peripheral surface of the outer layer ring pre-sintered body is machined to have a caliber 2a by cutting, grinding, etc. Note that the caliber 2a may be machined in a separate step other than the outer layer ring processing step S4.

[0080] In this embodiment, as described above, the inner layer tapered surface 11a is provided on the outer peripheral surface of the inner layer ring 11, and the outer layer tapered surface 12a is provided on the inner peripheral surface of the outer layer ring pre-sintered body, and the outer diameter dimension of the inner layer tapered surface 11a is made larger than the inner diameter dimension of the outer layer tapered surface 12a. More specifically, as shown in Fig. 3, the minimum value of the inner diameter dimension of the outer layer tapered surface 12a is made smaller than the minimum value of the outer diameter dimension of the inner layer tapered surface 11a, and the maximum value of the inner diameter dimension of the outer layer tapered surface 12a is made smaller than the maximum value of the outer diameter dimension of the inner layer tapered surface 11a.

[0081] In other words, the inner diameter dimension at the end of the outer layer tapered surface 12a on the other axial side (-X side) is smaller than the outer diameter dimension at the end of the inner layer tapered surface 11a on the other axial side. Also, the inner diameter dimension at the end of the outer layer tapered surface 12a on one axial side (+X side) is smaller than the outer diameter dimension at the end of the inner layer tapered surface 11a on one axial side. In addition, the first inclination angle θ1 of the inner layer tapered surface 11a and the second inclination angle θ2 of the outer layer tapered surface 12a are set to be equal to each other. In the following description, the first inclination angle θ1 or the second inclination angle θ2 may be simply referred to as the inclination angle θ.

[0082] [Main sintering process] In the main sintering step S5, the rolled ring intermediate sintered body, in which the inner surface of the outer layer ring pre-sintered body is fitted with the outer surface of the sintered inner layer ring 11, is sintered at a main sintering temperature higher than the pre-sintering temperature in the pre-sintering step S3, thereby sintering the outer layer ring pre-sintered body to form the outer layer ring 12, and joining the outer layer ring 12 and the inner layer ring 11 to form the rolled ring 2.

[0083] Specifically, in the main sintering step S5, the rolled ring intermediate sintered body is subjected to main sintering at a temperature of 1300° C. or more and 1400° C. or less to obtain a rolled ring 2. Note that a more preferable range of the main sintering temperature is, for example, 1340° C. or more and 1400° C. or less. Various settings for the main sintering in this embodiment are, for example, as follows: <Various settings for sintering> Sintering temperature: 1360℃ Sintering time: 1 hour

[0084] Due to this final sintering, the rolled ring 2 has a smaller volume and shrinks than the intermediate sintered rolled ring body. In detail, the inner layer ring 11 of the intermediate sintered rolled ring body does not deform because it has already been final sintered, but the provisionally sintered outer layer ring body contains more pores inside than the inner layer ring 11, and as the binder phase fills these pores, it reduces in volume and shrinks.

[0085] 3, in the main sintering step S5, the outer layer ring pre-sintered body and the inner layer ring 11 are arranged so that their respective ring central axes C extend in the vertical direction (up-down direction), and a rolled ring intermediate sintered body is sintered in which the outer layer tapered surface 12a provided on the inner peripheral surface of the outer layer ring pre-sintered body and the inner layer tapered surface 11a provided on the outer peripheral surface of the inner layer ring 11 are fitted together. That is, the inclination directions of the tapered surfaces 11a, 12a are set to be the same, and the main sintering is performed in a state in which they are fitted together.

[0086] More specifically, as shown in Figures 3 and 4, in the sintering step S5, a weight (not shown) is placed on one of the outer layer ring pre-sintered body and the inner layer ring 11 (the inner layer ring 11 in this embodiment), which is located above the other (the outer layer ring pre-sintered body in this embodiment), and the outer layer tapered surface 12a and the inner layer tapered surface 11a are slid by the weight of the other and the weight of the weight. That is, while the rolled ring intermediate sintered body in which the two rings are fitted is sintered, the other is slid downward relative to the one by the weight. As a result, the two rings are aligned coaxially while remaining fitted together.

[0087] In the main sintering step S5, a pressing force (load) F acts on each of the tapered surfaces 11a and 12a in a direction perpendicular to the tapered surfaces, as shown in Fig. 3. The load F can be calculated, for example, by the following formula. F=m×g×sinθ In the above formula, F is the load (vertical load acting on the contact surface), m is the sum of the weight of the other (inner layer ring 11) and the weight of the weight, g is the gravitational acceleration, and θ is the inclination angle (θ1, θ2).

[0088] The load F divided by the contact area of ​​the mating surfaces (tapered surfaces 11a, 12a) is the surface pressure acting on the mating surfaces. By carrying out the main sintering (second sintering for the outer layer ring 12) with the load F (surface pressure) applied, the bonding of the mating surfaces is improved and defects such as cracks and breaks on the mating surfaces are reduced.

[0089] [End face processing process] In the end face processing step S6, the end face facing the axial direction of the rolled ring 2 after the sintering is subjected to processing such as cutting or grinding to smooth out any step that occurs between the inner layer ring 11 and the outer layer ring 12. Note that if no step occurs on the end face of the rolled ring 2 integrated by the sintering, the end face processing step S6 does not need to be performed.

[0090] [Isostatic sintering process] In the isostatic sintering step S7, finish isostatic sintering (Sinter-HIP) is performed on the rolled ring 2. This improves the flexural strength (strength) of the rolled ring 2 as a whole.

[0091] The rolling ring 2 is manufactured in this manner, and the rolling roll 10 of this embodiment is manufactured by assembling the rolling ring 2, the support portion 3 and the lateral pressure imparting portion 4 to the shaft 1 in accordance with the above-mentioned “Rolling ring attachment / detachment procedure.”

[0092] [Effects of this embodiment] In the manufacturing method of the rolling roll 10 of this embodiment described above, the outer peripheral surface of the inner layer ring 11 that has been sintered is fitted to the inner peripheral surface of the outer layer ring pre-sintered body that has been pre-sintered at a temperature lower than the main sintering temperature of the rolling ring 2, and then the intermediate sintered rolled ring body is sintered. During the main sintering, the pre-sintered outer layer ring body shrinks as its volume decreases. This allows the outer layer ring 12 and the inner layer ring 11 to be firmly bonded to each other after sintering. In addition, the occurrence of cracks, breaks, etc. on the fitting surfaces between these rings 11, 12 is also suppressed.

[0093] Furthermore, when the rings 11, 12 are fitted together, the inner layer ring 11 will not deform because it has already been fully sintered. On the other hand, the provisionally sintered outer layer ring contains more pores inside than the inner layer ring 11 and is deformable. This allows these rings 11, 12 to be easily fitted together, improving workability during roll manufacturing. Furthermore, by deforming the provisionally sintered outer layer ring according to the shape (reference shape) of the undeformable inner layer ring 11, the precision of the coaxiality (concentricity) and roundness of the manufactured rolled ring 2 is also improved.

[0094] For example, when the outer layer ring and the inner layer ring are joined by a metal joining material such as a brazing material as in the above Patent Document 1 (JP Patent Publication 105749 / 1974), sufficient joining strength may not be obtained. Also, when the outer layer ring and the inner layer ring are joined by mechanical engagement as in the above Patent Document 2 (JP Utility Model Publication 74447 / 1978) and the above Patent Document 3 (JP Utility Model Publication 135806 / 1984), sufficient joining strength cannot be obtained. On the other hand, in this embodiment, the outer layer ring 12 and the inner layer ring 11 are joined by main sintering, so that the joining strength between these rings 11, 12 can be stably increased.

[0095] Furthermore, for example, as in the above-mentioned Patent Document 5 (Patent Publication No. 6794416), when an outer layer ring and an inner layer ring which have each been sintered are prepared, the inner layer ring is cooled to shrink it and fitted into the outer layer ring, and then the inner layer ring is thermally expanded to mechanically join them, tensile stress may be generated in the outer layer ring, which may cause cracks or the like to occur in the outer layer ring. On the other hand, in this embodiment, the outer layer ring 12 and the inner layer ring 11 are joined by the sintering, so that no tensile stress is generated in the outer layer ring 12, and the occurrence of cracks and the like can be prevented. Furthermore, in this embodiment, the outer layer ring 12 tends to have compressive stress generated by the sintering, so the strength of the outer layer ring 12 is further increased. Also, in this embodiment, cooling equipment for shrinking the inner layer ring 11 by cooling is not required, and the manufacturing equipment can be simplified. In addition, the manufacturing process is shortened and production efficiency is improved.

[0096] Furthermore, in this embodiment, for example, a used rolling roll (rolling ring) that has been used in rolling and whose outer diameter has reached a predetermined discard diameter due to wear, re-polishing, etc., can be reused as the inner layer ring 11. That is, unlike the manufacturing method of a rolling roll in which an outer layer ring and an inner layer ring that have been powder-pressed are fitted together and sintered, as in the above-mentioned Patent Document 4 (JP Patent Publication 2004-255401), according to this embodiment, a used rolling roll that has conventionally been discarded is used to make the inner layer ring 11 by adjusting the outer shape, and only the outer layer ring 12 is newly pressed and sintered (preliminary sintering followed by main sintering), thereby manufacturing the rolling roll 10. Therefore, the amount of expensive cemented carbide material used can be kept small, and manufacturing costs can be reduced. In addition, it is also possible to shorten the sintering time of the rolling ring 2, improving production efficiency.

[0097] The reason why the preliminary sintering temperature in the preliminary sintering step S3 is set to be −100° C. or higher and −10° C. or lower with respect to the main sintering temperature in the main sintering step S5 is as follows. If the preliminary sintering temperature is −100° C. or higher with respect to the main sintering temperature, the preliminary sintering causes the outer layer ring pre-sintered body to shrink to a certain degree or more, and this makes it possible to suppress the occurrence of non-uniform thermal deformation, gaps, and localized distortion on the mating surface between the outer layer ring 12 and the inner layer ring 11 during main sintering. This makes it possible to stably increase the strength of the manufactured rolling roll 10 and prevent roll breakage, etc.

[0098] In addition, if the preliminary sintering temperature is -10°C or lower than the main sintering temperature, the outer layer ring compact is prevented from being sintered erroneously (unintentionally), and pores remain stable inside the preliminary sintered outer layer ring compact that has undergone the preliminary sintering step S3, so that the preliminary sintered outer layer ring compact can be maintained in a state in which it is easily deformed. In other words, the amount of deformation of the preliminary sintered outer layer ring compact is ensured to be greater than or equal to a predetermined amount, so that the preliminary sintered outer layer ring compact and the inner layer ring 11 can be easily combined and fitted together.

[0099] As described above, according to this embodiment, the bonding strength between the inner layer ring 11 and the outer layer ring 12 can be improved, the occurrence of cracks and fractures on the mating surfaces between these rings 11, 12 can be reduced, and the manufacturing equipment for the rolling roll 10 can be prevented from becoming large-scale and complicated. Furthermore, the manufacturing cost of the rolling roll 10 can be reduced.

[0100] Furthermore, as in this embodiment, when the sintering temperature in the sintering step S5 is 1300°C or higher and 1400°C or lower, the rolled ring intermediate sintered body in which the outer layer ring pre-sintered body and the inner layer ring 11 are fitted together can be sintered stably, regardless of the type of cemented carbide constituting the outer layer ring 12.

[0101] In this embodiment, in the sintering process S5, the central axes C of the outer layer ring pre-sintered body and the inner layer ring 11 are arranged to extend in the vertical direction, and a rolled ring intermediate sintered body is sintered in which the outer layer tapered surface 12a provided on the inner surface of the outer layer ring pre-sintered body and the inner layer tapered surface 11a provided on the outer surface of the inner layer ring 11 are fitted together. In this case, the outer layer ring pre-sintered body and the inner layer ring 11 are tapered and fitted together, and the central axis C of each ring is arranged to extend vertically. During the main sintering, a pressing force (load F) acts on these fitting surfaces (the outer layer tapered surface 12a and the inner layer tapered surface 11a) due to the weight of the rings, etc., in a direction perpendicular to the fitting surfaces. In other words, the outer layer tapered surface 12a of the outer layer ring pre-sintered body and the inner layer tapered surface 11a of the inner layer ring 11 can be sintered while being pressed against each other. This allows the outer layer ring 12 and the inner layer ring 11 to be more firmly joined to each other.

[0102] In addition, in this embodiment, in the sintering process S5, a weight is placed on one of the outer layer ring pre-sintered body and the inner layer ring 11, which is located higher than the other (the outer layer ring pre-sintered body), and the outer layer tapered surface 12a and the inner layer tapered surface 11a are slid by the weight of the other ring and the weight of the weight. In this case, a larger pressing force (load F) can be applied to the outer layer tapered surface 12a and the inner layer tapered surface 11a during the main sintering. This allows the outer layer ring 12 and the inner layer ring 11 to be more firmly bonded to each other. In addition, the outer layer tapered surface 12a and the inner layer tapered surface 11a are fitted together while sliding, allowing the outer layer ring 12 and the inner layer ring 11 to be more precisely aligned coaxially (concentrically).

[0103] In this embodiment, in a cross section along the ring central axis C, the first inclination angle θ1 at which the inner layer tapered surface 11a is inclined relative to the ring central axis C and the second inclination angle θ2 at which the outer layer tapered surface 12a is inclined relative to the ring central axis C are the same as each other. In this case, since the first inclination angle θ1 and the second inclination angle θ2 are the same, the inner layer tapered surface 11a and the outer layer tapered surface 12a can be brought into close contact over a wide range. The outer layer ring pre-sintered body and the inner layer ring 11 can be stably tapered-fitted, and the bonding strength between the outer layer ring 12 and the inner layer ring 11 after main sintering can be stably increased.

[0104] In this embodiment, in a cross section along the ring central axis C, the first inclination angle θ1 at which the inner layer tapered surface 11a is inclined relative to the ring central axis C, and the second inclination angle θ2 at which the outer layer tapered surface 12a is inclined relative to the ring central axis C are each greater than 0° and not greater than 5°.

[0105] When the first inclination angle θ1 and the second inclination angle θ2 are each greater than 0°, the inner layer tapered surface 11a and the outer layer tapered surface 12a are reliably inclined with respect to the ring central axis C, so that a pressing force (load F) can be applied stably to the outer layer tapered surface 12a and the inner layer tapered surface 11a. This makes it possible to more stably increase the bonding strength between the outer layer ring 12 and the inner layer ring 11. It is more preferable that the first inclination angle θ1 and the second inclination angle θ2 are each greater than 0°30′.

[0106] Furthermore, when the first inclination angle θ1 and the second inclination angle θ2 are each 5° or less, for example, when reusing a used inner layer ring 11, the amount of processing (i.e., the amount of waste) of the cemented carbide cut to form the inner layer tapered surface 11a can be reduced. Also, the radial thickness of the manufactured rolled ring 2 is prevented from becoming too large, resulting in bulky dimensions. It is more preferable that the first inclination angle θ1 and the second inclination angle θ2 are each 4° or less.

[0107] The rolling roll 10 of this embodiment is a composite roll, known as a clamp roll or the like, that includes a rolling ring 2 and a shaft 1. Therefore, the outer diameter of the rolling ring 2 is 300 mm or more and 450 mm or less. For example, compared with a small-diameter rolling roll (outer diameter of 210 mm or less) called a Morgan roll or the like, the outer diameter of the rolling ring 2 of the above composite roll is large, so that the effect of reducing manufacturing costs by reusing the above-mentioned inner layer ring 11 becomes more significant.

[0108] [Other configurations included in the present invention] The present invention is not limited to the above-described embodiment, and the configuration may be modified within the scope of the present invention, as described below. In the illustration of the modified example, the same components as those in the above-described embodiment are given the same reference numerals, and the following mainly describes the differences.

[0109] 6 and 7 show a modified example of the manufacturing method of the rolling roll 10 described in the above embodiment. In this modified example, the vertical (up-down) positional relationship between the outer layer ring pre-sintered body and the inner layer ring 11 in the main sintering step S5 is different from that in the above embodiment. Specifically, in this modified example, a weight (not shown) is placed on one of the outer layer ring pre-sintered body and the inner layer ring 11 (the outer layer ring pre-sintered body) that is located above the other (the inner layer ring 11) in the main sintering step S5, and the outer layer tapered surface 12a and the inner layer tapered surface 11a are slid by the weight of the other and the weight of the weight. This modification also provides the same effects as those of the above-described embodiment.

[0110] In the above embodiment, the manufacturing method of the rolling roll 10 includes the inner layer ring processing step S1, the outer layer ring forming step S2, the preliminary sintering step S3, the outer layer ring processing step S4, the main sintering step S5, the end face processing step S6, and the isostatic sintering step S7 in this order, but is not limited thereto. For example, the inner layer ring processing step S1 only needs to be performed before the main sintering step S5, and therefore may be performed between any of the steps S2 to S5.

[0111] In the above embodiment, the inner layer tapered surface 11a of the inner layer ring 11 and the outer layer tapered surface 12a of the outer layer ring 12 are tapered surfaces that increase in diameter toward one axial side (+X side), but this is not limited to the above. The inner layer tapered surface 11a of the inner layer ring 11 and the outer layer tapered surface 12a of the outer layer ring 12 may also be tapered surfaces that decrease in diameter toward one axial side (+X side).

[0112] Although not particularly shown, the rolling roll 10 may have a plurality of rolling rings 2 arranged side by side in the axial direction. In this case, a cylindrical or annular spacer may be provided between the rolling rings 2 adjacent to each other in the axial direction.

[0113] The present invention may be combined with the various configurations described in the above-mentioned embodiments and modifications, and may include additions, omissions, substitutions, and other modifications, without departing from the spirit of the present invention. The present invention is not limited to the above-mentioned embodiments, but is limited only by the claims. [Industrial Applicability]

[0114] According to the manufacturing method of the rolling roll of the present invention, it is possible to further improve the bonding strength between the inner layer ring and the outer layer ring, reduce the occurrence of cracks and fractures on the fitting surfaces between these rings, and prevent the manufacturing equipment for the rolling roll from becoming large-scale and complicated. Therefore, the method has industrial applicability. [Explanation of symbols]

[0115] 1...Shaft 2…Rolled ring 10...Roller 11…Inner layer ring 11a…Inner layer tapered surface 12...Outer layer ring (outer layer ring pre-sintered body) 12a…Outer layer tapered surface C...Center axis (center axis of ring) S3: Pre-sintering process S5…Main sintering process θ1…first inclination angle θ2…Second inclination angle

Claims

1. A method for manufacturing a rolling roll including a rolling ring in which an outer peripheral surface of an inner layer ring made of a cemented carbide alloy and an inner peripheral surface of an outer layer ring made of a cemented carbide alloy are joined together, comprising: a preliminary sintering step of preliminary sintering an outer layer ring compact obtained by compacting the raw material powder into an outer layer ring preliminary sintered body; a final sintering step in which the inner peripheral surface of the outer layer ring pre-sintered body is fitted with the outer peripheral surface of the sintered inner layer ring, and the intermediate sintered body is sintered at a final sintering temperature higher than the preliminary sintering temperature in the preliminary sintering step to final sinter the outer layer ring pre-sintered body to form the outer layer ring, and the outer layer ring and the inner layer ring are joined to form the rolled ring, The preliminary sintering temperature in the preliminary sintering step is set to be −100° C. or more and −10° C. or less with respect to the main sintering temperature in the main sintering step; A method for manufacturing a rolling roll.

2. The sintering temperature in the sintering step is 1300° C. or higher and 1400° C. or lower. The method for producing a reduction roll according to claim 1 .

3. In the sintering process, the outer layer ring pre-sintered body and the inner layer ring are arranged so that their central axes extend in the vertical direction, and the rolled ring intermediate sintered body is sintered by fitting an outer layer tapered surface provided on the inner peripheral surface of the outer layer ring pre-sintered body with an inner layer tapered surface provided on the outer peripheral surface of the inner layer ring. The method for producing a rolling roll according to claim 1 or 2.

4. a minimum value of an inner diameter dimension of the outer layer tapered surface is smaller than a minimum value of an outer diameter dimension of the inner layer tapered surface, and a maximum value of an inner diameter dimension of the outer layer tapered surface is smaller than a maximum value of an outer diameter dimension of the inner layer tapered surface, In the sintering process, a weight is placed on one of the outer layer ring pre-sintered body and the inner layer ring, which is located above the other, and the outer layer tapered surface and the inner layer tapered surface are slid by the weight of the other and the weight of the weight. The method for producing a rolling roll according to claim 3 .

5. In a cross section along the ring central axis, a first inclination angle at which the inner layer tapered surface is inclined with respect to the ring central axis and a second inclination angle at which the outer layer tapered surface is inclined with respect to the ring central axis are equal to each other. The method for producing a rolling roll according to claim 3 .

6. In a cross section along the ring central axis, a first inclination angle at which the inner layer tapered surface is inclined with respect to the ring central axis, and a second inclination angle at which the outer layer tapered surface is inclined with respect to the ring central axis are each greater than 0° and equal to or less than 5°. The method for producing a rolling roll according to claim 3 .

7. The rolling mill further includes a shaft fitted to an inner peripheral surface of the rolling ring, The outer diameter of the rolled ring is 300 mm or more and 450 mm or less. The method for producing a rolling roll according to claim 1 or 2.

Citation Information

Patent Citations

  • JP1974105749A

  • JP1978074447U

  • The rolling roll seal -

    JP1984135806U

  • Cemented carbide double layer hot rolling roll having outer ring member made of wear-resistant cemented carbide exhibiting excellent high temperature hardness and strength

    JP2004255401A

  • Composite Roles

    JP6794416B2