Polystyrenic resin foam sheet and method for producing the same
A polystyrene resin foam sheet with a specific foam layer and optional non-foam layers addresses appearance defects and brittleness by improving resin compatibility, enhancing impact resistance and strength.
Patent Information
- Application Number
- JP2023057660
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Conventional polystyrene resin foam sheets suffer from appearance defects such as resin lumps and streaks, brittleness, and poor impact strength due to low compatibility between polypropylene resin and polystyrene resin and styrene-(meth)acrylic acid copolymers.
A polystyrene resin foam sheet with a specific foam layer containing 100 parts by mass of polystyrene resin, 0.5 to 15 parts by mass of hydrogenated styrene thermoplastic elastomer, and 1 to 20 parts by mass of polypropylene resin, forming a sea-island structure with improved resin compatibility, and optionally including a non-foam layer on both sides.
The solution suppresses appearance defects and enhances impact resistance, resulting in a polystyrene resin foam sheet with improved strength and appearance.
Smart Images

Figure 2024145350000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a polystyrene resin foamed sheet and a method for producing the same. [Background technology]
[0002] Containers having a foamed layer of polystyrene resin (foamed containers) are known as containers for food, etc. A method for manufacturing the containers includes a method of subjecting a polystyrene resin foamed sheet having a foamed layer of polystyrene resin to thermoforming. When manufacturing the containers, trimming after thermoforming generates scraps. In order to protect the environment and make effective use of resources, it is desirable to reuse scrap materials as described above.
[0003] For the purpose of improving the heat resistance of foamed containers, a polystyrene-based resin foam sheet (sometimes called a "laminated foam sheet") is known, which has a foam layer of heat-resistant polystyrene resin and a non-foam layer of a non-foamed resin such as a polyolefin-based resin on one or both sides of the foam layer. When the remnants of the laminated foam sheet are used for the foam layer, the strength of the resulting container is not sufficient for practical use. In response to these problems, a polystyrene-based resin foam sheet has been proposed that is composed of a mixture containing less than 50% by mass of recycled raw materials derived from polystyrene-based resin foam sheets containing methacrylic acid, the mixture being mainly composed of styrene, and having a foam layer that is foamed containing methacrylic acid and a rubber component (for example, Patent Document 1). According to the invention described in Patent Document 1, the strength of a polystyrene-based resin foam sheet formed from recycled raw materials containing methacrylic acid is improved. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2021-046466 Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the conventional techniques, a beautiful polystyrene-based resin foamed sheet cannot be obtained because the surface of the obtained raw sheet has poor appearance such as resin lumps and streaks, etc. In addition, the molded article molded from the obtained polystyrene-based resin foamed sheet has a problem of being brittle and having poor impact resistance. Therefore, an object of the present invention is to provide a polystyrene-based resin foamed sheet which can suppress poor appearance and has excellent impact resistance. [Means for solving the problem]
[0006] According to the study by the present inventors, the polypropylene resin contained in the scrap material has low compatibility with polystyrene resin and styrene-(meth)acrylic acid copolymer, and thus it has low impact resistance and causes poor appearance. That is, when the scrap material is melt-kneaded and extruded, the polypropylene resin has low compatibility with polystyrene resin and styrene-(meth)acrylic acid copolymer, so that the unmelted polypropylene resin aggregates in the melt-kneaded scrap material and forms lumps, and these lumps are generated on the surface of the foamed sheet, causing poor appearance. It was also found that the lumps of polypropylene resin are accumulated on the lip of the extruder die, causing streaks on the surface of the foamed sheet, causing poor appearance of the foamed sheet. Based on the above findings, the present inventors improved the compatibility of resins and completed the present invention.
[0007] The present invention has the following aspects. <1> A foam layer is formed of one or more unit foam layers, At least one of the unit foam layers is a specific foam layer containing a resin including 100 parts by mass of a polystyrene resin, 0.5 to 15 parts by mass of a hydrogenated styrene thermoplastic elastomer, and 1 to 20 parts by mass of a polypropylene resin; The polystyrene resin contains a rubber component and a styrene-(meth)acrylic acid copolymer, The polystyrene-based resin foam sheet has a rubber content of 1 to 7% by mass based on the total mass of the resin. <2> the specific foam layer has a sea-island structure in which the polypropylene-based resin is dispersed in a matrix structure of the polystyrene-based resin and the hydrogenated styrene-based thermoplastic elastomer; <1> The polystyrene resin foam sheet according to claim 1, <3> The hydrogenated styrene-based thermoplastic elastomer contains at least one selected from a styrene-butadiene-butylene-styrene block copolymer and a styrene-ethylene-butylene-styrene block copolymer. <1> or <2> The polystyrene resin foam sheet according to claim 1, <4> The specific foam layer further contains carbon. <1> ~ <3> 2. The polystyrene resin foam sheet according to claim 1 , <5> The resin comprises recycled materials. <1> ~ <4> 2. The polystyrene resin foam sheet according to claim 1 , <6> A non-foamed layer is provided on one or both sides of the foamed layer. <1> ~ <5> 2. The polystyrene resin foam sheet according to claim 1 ,
[0008] <7> <1> ~ <6> A method for producing a polystyrene-based resin foamed sheet according to any one of the above, A method for producing a polystyrene-based resin foamed sheet, comprising a step of extruding a kneaded mixture of the resin and the foaming agent into a sheet shape and foaming the sheet to form the specific foamed layer. <8> The resin comprises recycled materials. <7> A method for producing the polystyrene resin foam sheet according to claim 1. Effect of the Invention
[0009] The polystyrene-based resin foamed sheet of the present invention can suppress defects in appearance and has excellent impact resistance. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a cross-sectional view of a polystyrene-based resin foam sheet according to a first embodiment. [Diagram 2] FIG. 4 is a cross-sectional view of a polystyrene-based resin foam sheet according to a second embodiment. [Diagram 3] FIG. 2 is a cross-sectional view of a polystyrene-based resin foam sheet according to another embodiment. [Figure 4] FIG. 2 is a cross-sectional view of a polystyrene-based resin foam sheet according to another embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The polystyrene resin foamed sheet of the present invention (hereinafter, may be simply referred to as "foamed sheet") has a foamed layer. The foamed sheet may be a single-layer foamed sheet consisting of only a foamed layer, or a laminated foamed sheet having a foamed layer and a non-foamed layer located on one or both sides of the foamed layer. The foamed sheet of the present invention will be described below by taking the foamed sheet according to an embodiment of the present invention as an example.
[0012] First Embodiment The foamed sheet according to the first embodiment of the present invention will be described with reference to FIG. 1 has a foamed layer 10, a first non-foamed layer 20 located on one side of the foamed layer 10, and a second foamed layer 30 located on the other side of the foamed layer 10. That is, the foamed sheet 1 is a laminated foamed sheet having non-foamed layers on both sides of the foamed layer 10.
[0013] The thickness t1 of the foamed sheet 1 is appropriately determined taking into consideration the application and the like. For example, the thickness t1 is preferably 0.5 to 3.0 mm, more preferably 0.7 to 2.5 mm, and more preferably 1.0 to 2.0 mm. When the thickness t1 is equal to or greater than the above lower limit, the impact resistance and rigidity can be further improved. When the thickness t1 is equal to or less than the above upper limit, the reproducibility of the shape can be improved (i.e., the moldability can be improved) when a molded product is formed by thermoforming. The thickness is measured, for example, using a dial thickness gauge at 10 points in an arbitrary direction (for example, the TD direction), and the average value is calculated.
[0014] The basis weight of the foam sheet 1 is 100 to 500 g / m 2 is preferable, and 150 to 350 g / m 2 When the basis weight is equal to or more than the lower limit, the impact resistance and rigidity can be further increased, whereas when the basis weight is equal to or less than the upper limit, the moldability can be improved. The basis weight can be measured by the following method. The foam sheet 1 is cut into 10 pieces of 10 cm x 10 cm at equal intervals in the width direction (TD direction), excluding 20 mm at both ends, and the mass (g) of each piece is measured to the nearest 0.001 g. The average mass (g) of each piece is calculated as 1 m. 2 The converted value is the basis weight (g / m2) of the foam sheet 1. 2 )
[0015] The apparent density of the foamed sheet 1 is, for example, 0.060 to 0.716 g / cm 3 is preferable, and 0.086 to 0.540 g / cm 3 More preferably, 0.130 to 0.363 g / cm 3 When the apparent density of the foamed sheet 1 is equal to or higher than the above lower limit, the impact resistance can be further improved. When the apparent density of the foamed sheet 1 is equal to or lower than the above upper limit, the molded product can be made lighter and the heat insulating property can be further improved.
[0016] The apparent density of the foamed sheet 1 is determined by measurement in accordance with JIS K7222:2005 "Foamed plastics and rubber - Determination of apparent density". Specifically, the mass and apparent volume of a test piece of the foamed sheet 1 cut without changing the original cell structure are measured, and the mass and apparent volume are calculated according to the following formula (1). Apparent density of foam sheet 1 (g / cm 3 ) = mass of test piece (g) / apparent volume of test piece (cm 3 ) · · · (1)
[0017] To further exert the effects of the present invention, the maximum point load in the MD direction of the foamed sheet 1 is preferably 4.0 to 10.0 N, more preferably 4.0 to 9.0 N, and even more preferably 4.0 to 8.0 N. The maximum point load is determined in accordance with the three-point bending test method described in JIS K7221:1997 "Bending test method for rigid foamed plastics".
[0018] <Foam layer> The foamed layer 10 of this embodiment has a two-layer structure having a first unit foamed layer 12 and a second unit foamed layer 14. In this embodiment, the first unit foamed layer 12 is a specific foamed layer. The thickness t10 of the foam layer 10 is appropriately determined taking into consideration the application and the like. For example, the thickness t10 is preferably 0.5 to 3.0 mm, more preferably 1.0 to 2.5 mm, and more preferably 1.0 to 2.0 mm. When the thickness t10 is equal to or greater than the above lower limit, the impact resistance and rigidity can be further improved. When the thickness t10 is equal to or less than the above upper limit, the moldability can be improved.
[0019] The basis weight of the foam layer 10 is 50 to 250 g / m 2 is preferable, and 100 to 200 g / m 2 When the basis weight is equal to or more than the lower limit, the impact resistance and rigidity can be further increased, whereas when the basis weight is equal to or less than the upper limit, the moldability can be improved. The basis weight of the foam layer 10 can be measured in the same manner as the basis weight of the foam sheet 1.
[0020] The apparent density of the foam layer 10 is, for example, 0.055 to 0.716 g / cm 3 is preferable, and 0.086 to 0.540 g / cm 3 More preferably, 0.130 to 0.363 g / cm 3 When the apparent density of the foamed layer 10 is equal to or higher than the above lower limit, the impact resistance can be further improved. When the apparent density of the foamed layer 10 is equal to or lower than the above upper limit, the molded body can be made lighter and the heat insulating property can be further improved. The apparent density of the foamed layer 10 can be measured in the same manner as the apparent density of the foamed sheet 1.
[0021] The expansion ratio of the foamed layer 10 is, for example, preferably 2 to 18 times, more preferably 5 to 15 times, and further preferably 3 to 10 times. When the expansion ratio of the foamed layer 10 is equal to or higher than the above lower limit, the impact resistance can be further improved. When the expansion ratio of the foamed layer 10 is equal to or lower than the above upper limit, the molded body can be made lighter and the heat insulating property can be further improved. Generally, when the expansion ratio is increased, the strength is reduced, and the foamed sheet may lack suitability as a molded product (for example, a thermoformed container, etc.). In the present invention, even if the expansion ratio of the foamed layer 10 is set to the above lower limit or more, the molded product has sufficient strength. The expansion ratio is calculated by dividing 1 by the apparent density.
[0022] <First unit foam layer> The first unit foam layer 12 contains a resin (first foam layer resin), and the first foam layer resin contains a polystyrene-based resin (component (A1)), a hydrogenated styrene-based thermoplastic elastomer (component (B1)), and a polypropylene-based resin (component (C1)). The first unit foam layer 12 is a layer formed by foaming a first foamable resin composition containing a first foam layer resin, and has air bubbles formed in the layer.
[0023] The component (A1) is a polystyrene-based resin containing a styrene-(meth)acrylic acid copolymer. That is, the component (A1) is a polystyrene-based resin, a part or the whole of which is a styrene-(meth)acrylic acid copolymer. (Meth)acrylic acid is a general term for methacrylic acid and acrylic acid.
[0024] Examples of polystyrene-based resins include homopolymers of styrene-based monomers such as styrene, α-methylstyrene, vinyltoluene, chlorostyrene, ethylstyrene, i-propylstyrene, dimethylstyrene, and bromostyrene, or copolymers thereof. Examples of polystyrene-based resins include so-called high impact polystyrene (HIPS), which is a copolymer of a styrene-based monomer and a vinyl monomer polymerizable therewith, a copolymer of a styrene-based monomer and a rubber component such as butadiene, a homopolymer of a styrene-based monomer, or a copolymer thereof, or a mixture or polymer of a copolymer of a styrene-based monomer and a vinyl monomer and a diene-based rubber-like polymer, with a styrene-based monomer as the main component.
[0025] Examples of the vinyl monomer that can be polymerized with the styrene-based monomer and that constitutes the styrene-(meth)acrylic acid copolymer include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, and cetyl (meth)acrylate, and (meth)acrylonitrile. Examples of other vinyl monomers that can be polymerized with the styrene-based monomer include dimethyl maleate, dimethyl fumarate, diethyl fumarate, ethyl fumarate, divinylbenzene, and alkylene glycol dimethacrylate. These vinyl monomers may be used alone or in combination of two or more. Here, "(meth)acrylate" refers to either or both of "acrylate" and "methacrylate", and "(meth)acrylonitrile" refers to either or both of "acrylonitrile" and "methacrylonitrile".
[0026] The content of units derived from (meth)acrylic acid ((meth)acrylic acid units) in the styrene-(meth)acrylic acid copolymer is preferably 2 to 10 mass %, more preferably 3 to 8 mass %, and even more preferably 4 to 8 mass %, based on the total mass of the styrene-(meth)acrylic acid copolymer. When the content of the (meth)acrylic acid units is equal to or greater than the above lower limit, heat resistance can be improved. When the content of the (meth)acrylic acid units is equal to or less than the upper limit, appearance defects can be further suppressed.
[0027] The content of the styrene-(meth)acrylic acid copolymer in the first foamed layer resin is preferably 50 to 90 mass%, more preferably 60 to 80 mass%, and even more preferably 70 to 80 mass%, based on the total mass of the first foamed layer resin. When the content of the styrene-(meth)acrylic acid copolymer is equal to or more than the lower limit, the heat resistance can be further improved. When the content of the styrene-(meth)acrylic acid copolymer is equal to or less than the upper limit, the flexibility can be further improved.
[0028] In addition, the component (A1) contains a rubber component, that is, a part or the whole of the component (A1) is the above-mentioned rubber-like polymer. Examples of diene rubber polymers include polybutadiene, styrene-butadiene copolymers, and ethylene-propylene-non-conjugated diene three-dimensional copolymers. These polystyrene resins may be used alone or in combination of two or more.
[0029] The rubber content is preferably 1 to 7 mass%, more preferably 2 to 6 mass%, and even more preferably 3 to 5 mass%, based on the total mass of the resin of the first foamed layer. When the rubber content is equal to or more than the lower limit, the impact resistance and moldability can be further improved. When the rubber content is equal to or less than the upper limit, the rigidity can be further improved.
[0030] The (A1) component may be a part or the whole of a recycled material. Examples of recycled materials include used polystyrene resin foam molded products, such as fish boxes, cushioning materials for home appliances, and food packaging trays, which are collected and regenerated by a limonene dissolution method or a heat volume reduction method. Another example of recycled materials is scraps generated after punching food packaging containers from a foam sheet, which are crushed, melt-kneaded, and repelletized. Examples of recyclable raw materials that can be used include those obtained by recycling molded bodies such as used foamed containers, as well as non-foamed polystyrene resins separated and recovered from home appliances (e.g., televisions, refrigerators, washing machines, air conditioners, etc.) and office equipment (e.g., copiers, facsimiles, printers, etc.). The component (A1) may be a virgin material other than a recycled material. Examples of the virgin material include general-purpose polystyrene resin (GPPS), commercially available polystyrene-based resins, and polystyrene-based resins newly prepared by a method such as suspension polymerization.
[0031] The weight average molecular weight Mw of the component (A1) is, for example, preferably 120,000 to 450,000, and more preferably 150,000 to 400,000. The weight average molecular weight Mw is a value measured by gel permeation chromatography (GPC) and converted based on a calibration curve using standard polystyrene.
[0032] The melt flow rate (MFR) of the (A1) component is preferably 0.5 to 6.0 g / 10 min, and more preferably 0.7 to 3.0 g / 10 min. When the (A1) component has an MFR equal to or higher than the lower limit, the impact resistance can be further improved. When the (A1) component has an MFR equal to or lower than the upper limit, the moldability can be further improved. In this specification, MFR refers to a value measured in accordance with Method B described in JIS K7210:1999 "Test method for melt mass-flow rate (MFR) and melt volume-flow rate (MVR) of plastics - thermoplastics" under conditions of a test temperature of 200°C, a test load of 49.03 N, and a preheating time of 5 minutes.
[0033] The content of the (A1) component in the first foamed layer resin is preferably 50 to 90 mass %, more preferably 60 to 80 mass %, and even more preferably 70 to 80 mass %, based on the total mass of the first foamed layer resin. When the content of the (A1) component is equal to or more than the lower limit, the heat resistance can be further improved and the rigidity of the molded article can be further improved. When the content of the (A1) component is equal to or less than the upper limit, the flexibility can be further improved.
[0034] The component (B1) is a hydrogenated styrene-based thermoplastic elastomer. The content of units derived from a styrene-based monomer (styrene units) in the (B1) component is preferably 50 to 85 mass %, more preferably 60 to 75 mass %, based on the total mass of the (B1) component. When the content of the styrene units is within the above range, the compatibility of the (A1) and (B1) components with the (C1) component can be further improved, appearance defects can be further suppressed, and impact resistance can be further improved. The content of units derived from conjugated diene monomers (conjugated diene units) in the component (B1) is preferably 15 to 50 mass %, more preferably 25 to 40 mass %, based on the total mass of the component (B1). When the conjugated diene units are within the above range, the compatibility of the components (A1) and (B1) with the component (C1) is further improved, appearance defects can be further suppressed, and impact resistance can be further improved. In the (B1) component, the double bonds of the conjugated diene units are partially or completely saturated by hydrogenation. The hydrogenation rate of the double bonds in the (B1) component is preferably 30% or more, more preferably 40 to 100%, and particularly preferably 50 to 100%. When the hydrogenation rate is within the above range, the compatibility of the (A1) and (B1) components with the (C1) component can be further improved.
[0035] The hydrogenation ratio of the double bond portion of the conjugated diene unit in the component (B1) means the ratio of the hydrogenated double bond portion to the double bond portion before hydrogenation. The hydrogenation ratio can be analyzed by instrumental analysis using a nuclear magnetic resonance (NMR) apparatus.
[0036] Examples of the (B1) component include styrene-butadiene-butylene-styrene block copolymer (SBBS), styrene-ethylene-butylene-styrene block copolymer (SEBS), styrene-ethylene-propylene-styrene block copolymer (SEPS), and styrene-ethylene-propylene-styrene block copolymer (SEEPS). Among them, the (B1) component is preferably styrene-butadiene-butylene-styrene block copolymer (SBBS) and styrene-ethylene-butylene-styrene block copolymer (SEBS), and more preferably styrene-ethylene-butylene-styrene block copolymer (SEBS). These (B1) components can further increase the compatibility of the (C1) component with the (A1) component and the (B1) component. These (B1) components may be used alone or in combination of two or more.
[0037] The content of the (B1) component in the first foamed layer resin is 0.5 to 15 parts by mass, preferably 1.0 to 8.0 parts by mass, and more preferably 2.0 to 5.0 parts by mass, based on 100 parts by mass of the (A1) component. When the content of the (B1) component is equal to or greater than the lower limit, the compatibility of the (C1) component with the (A1) and (B1) components can be further improved. When the content of the (B1) component is equal to or less than the upper limit, the rigidity of the foamed sheet 1 can be increased.
[0038] The component (C1) is a polypropylene resin. The component (C1) is preferably dispersed in a matrix structure containing the components (A1) and (B1). That is, the first foamed layer resin preferably has an islands-in-a-sea structure in which the component (C1) is an island. Whether or not the resin has an islands-in-a-sea structure can be confirmed by a transmission electron microscope (TEM).
[0039] In the first foam layer resin, the presence of the component (B1) increases the compatibility of the component (C1) with the components (A1) and (B1), so that even if the foam layer 10 of the foam sheet 1 contains the component (B1), the component (C1) is finely dispersed without agglomeration, providing a beautiful appearance.
[0040] The content of the (C1) component in the first foamed layer resin is 1 to 20 parts by mass, preferably 2 to 10 parts by mass, and more preferably 2 to 8 parts by mass, based on 100 parts by weight of the (A1) component. If the content of the (C1) component is equal to or greater than the lower limit, poor appearance occurs when the (B1) component is not included. If the content of the (C1) component is equal to or less than the upper limit, the (C1) component can be dispersed more effectively, and poor appearance can be more effectively prevented.
[0041] The total amount of the (A1), (B1) and (C1) components is preferably 80 to 100% by mass, more preferably 85 to 100% by mass, and even more preferably 90 to 100% by mass, based on the total mass of the resin of the first foamed layer. When the content of the (A1) to (C1) components is equal to or greater than the lower limit, the impact resistance can be further improved and appearance defects can be more effectively suppressed.
[0042] The mass ratio of the (B) component to the (C) component, expressed as the (B) component / (C) component (B / C ratio) is preferably 0.5 to 4.0, more preferably 1.0 to 3.0, and even more preferably 1.2 to 2.5. When the B / C ratio is equal to or greater than the lower limit, the appearance defect can be suppressed more effectively. When the B / C ratio is equal to or less than the upper limit, the moldability can be improved more.
[0043] The first expandable resin composition contains a foaming agent. Examples of the blowing agent include hydrocarbons such as propane, butane, and pentane; halogenated hydrocarbons such as tetrafluoroethane, chlorodifluoroethane, and difluoroethane; and among these, hydrocarbons are preferred, and butane is preferred. As butane, normal butane or isobutane may be used alone, or normal butane and isobutane may be used in any ratio. These blowing agents may be used alone or in combination of two or more.
[0044] The content of the foaming agent in the first foamable resin composition is, for example, preferably 0.1 to 10 parts by mass, more preferably 1 to 7 parts by mass, and even more preferably 1 to 5 parts by mass, relative to 100 parts by mass of the first foam layer resin.
[0045] The first foamable resin composition may contain other components (hereinafter, also referred to as "optional components of the first foam layer") other than the first foam layer resin and the foaming agent. Examples of the optional components of the first foam layer include a cell regulator, a stabilizer, an ultraviolet absorber, an antioxidant, a colorant, a deodorant, a lubricant, a flame retardant, an antistatic agent, and carbon. The type of the optional component of the first foamed layer is determined in consideration of the physical properties required for the first unit foamed layer 12. The optional component of the first foamed layer may be one type alone or two or more types in combination.
[0046] The cell regulator may be, for example, a mixture of inorganic powder such as talc or silica. These cell regulators can increase the closed cell ratio of the first unit foam layer 12. Examples of the stabilizer include calcium zinc-based heat stabilizers, tin-based heat stabilizers, and lead-based heat stabilizers. Examples of the ultraviolet ray absorbent include cesium oxide-based ultraviolet ray absorbents and titanium oxide-based ultraviolet ray absorbents. Examples of the antioxidant include cerium oxide, cerium oxide / zirconia solid solution, cerium hydroxide, titanium oxide, and fullerene. Examples of colorants (excluding carbon) include titanium oxide, carbon black, titanium yellow, iron oxide, ultramarine, cobalt blue, calcined pigments, metallic pigments, mica, pearl pigments, zinc oxide, precipitated silica, and cadmium red. Examples of deodorants include silica, zeolite, zirconium phosphate, and calcined hydrotalcite. Examples of carbon include carbon, carbon nanotubes, carbon black, etc. By including carbon, the design properties can be further improved.
[0047] The content of the optional component for the first foam layer in the first foamable resin composition is, for example, preferably 0.05 to 20 parts by mass, more preferably 0.1 to 10 parts by mass, and even more preferably 0.3 to 5.0 parts by mass, based on 100 parts by mass of the resin for the first foam layer. When the content of the optional component for the first foam layer is equal to or more than the lower limit, the effects derived from the optional component for the first foam layer can be exhibited. When the content of the optional component for the first foam layer is equal to or less than the upper limit, clogging of the die or the like can be more effectively prevented, and the appearance of the foam sheet 1 can be more improved.
[0048] The thickness of the first unit foam layer 12 can be determined in consideration of the application, and is, for example, preferably 250 to 1500 μm, more preferably 500 to 1000 μm.
[0049] The basis weight of the first unit foam layer 12 is 25 to 150 g / m 2 is preferable, and 35 to 100 g / m 2 When the basis weight is equal to or more than the lower limit, the impact resistance and rigidity can be further increased, whereas when the basis weight is equal to or less than the upper limit, the moldability can be improved when a molded article is formed by thermoforming. The basis weight of the first unit foamed layer 12 can be measured in the same manner as the basis weight of the foamed sheet 1.
[0050] The apparent density of the first unit foam layer 12 is, for example, 0.055 to 0.716 g / cm 3 is preferable, and 0.086 to 0.540 g / cm 3 More preferably, 0.130 to 0.363 g / cm 3 is more preferable. When the apparent density of the first unit foamed layer 12 is equal to or higher than the lower limit, the impact resistance can be further improved. When the apparent density of the first unit foamed layer 12 is equal to or lower than the upper limit, the molded body can be made lighter and the heat insulating property can be further improved. The apparent density of the first unit foamed layer 12 can be measured in the same manner as the apparent density of the foamed sheet 1.
[0051] The expansion ratio of the first unit foamed layer 12 is, for example, preferably 2 to 18 times, more preferably 5 to 15 times, and further preferably 3 to 10 times. When the expansion ratio of the first unit foamed layer 12 is equal to or higher than the above lower limit, the impact resistance can be further improved. When the expansion ratio of the first unit foamed layer 12 is equal to or lower than the above upper limit, the molded body can be made lighter and the heat insulating property can be further improved.
[0052] Any appropriate temperature may be adopted as the glass transition temperature Tg1 of the first unit foam layer 12 as long as it does not impair the effects of the present invention. In terms of further exerting the effects of the present invention, the glass transition temperature Tg1 is preferably 110°C to 150°C, more preferably 113°C to 140°C, further preferably 115°C to 130°C, and particularly preferably 117°C to 125°C.
[0053] The method for measuring the glass transition temperature will be described. [Preprocessing] A sample of 5 to 6 g is weighed out from the first unit foam layer 12, sandwiched between two polytetrafluoroethylene sheets, and pressed in the following manner to defoam (pretreatment). Press equipment: Small press equipment "Lab Press 10T" manufactured by Toyo Seiki Co., Ltd. Temperature: Upper heater 180℃, lower heater 180℃. Pressing process: Pressing is performed at 0.54 MPa for 3 minutes, followed by 5 cycles of pressing, with one cycle being 0.54 MPa for 2 seconds and pressure release for 2 seconds. Next, pressing is performed at 15.5 MPa for 2 minutes.
[0054] [Measurement of glass transition temperature (Tg)] The glass transition temperature (midpoint glass transition temperature) of the pretreated sample is measured by the method described in JIS K7121:1987 "Method of measuring glass transition temperature of plastics." However, the sampling method and temperature conditions will be as follows: Using a differential scanning calorimeter "DSC6220" (manufactured by SII NanoTechnology), fill the bottom of an aluminum measurement container with approximately 6 mg of sample so that there are no gaps. Under a nitrogen gas flow rate of 20 mL / min, the sample is heated from 30°C to 220°C at a heating rate of 20°C / min. After heating, the sample is held for 10 minutes, then quickly removed and allowed to cool in an environment of 25±10°C. For the cooled sample, the midpoint glass transition temperature is calculated from the DSC curve obtained when the sample is heated from 30°C to 220°C at a heating rate of 20°C / min. In this case, alumina is used as the reference material. The midpoint glass transition temperature is determined according to the standard (9.3 "Determination of glass transition temperature").
[0055] The average cell diameter of the first unit foamed layer 12 is preferably 100 to 500 μm, more preferably 150 to 400 μm, and even more preferably 200 to 350 μm. When the average cell diameter of the first unit foamed layer 12 is equal to or more than the lower limit, moldability can be improved. When the average cell diameter of the first unit foamed layer 12 is equal to or less than the upper limit, aesthetics can be improved.
[0056] <Second unit foam layer> The second unit foam layer 14 is a layer formed by foaming a second foamable resin composition containing a foaming agent and a second foam layer resin containing a polystyrene-based resin. The second foam layer resin may contain a polystyrene-based resin (component (A2)). The second foam layer resin may contain only component (A2), or may contain component (A2) and at least one of a hydrogenated styrene-based thermoplastic elastomer (component (B2)) and a polypropylene-based resin (component (C2)).
[0057] The amount of the component (A2) is determined taking into consideration the application of the foamed sheet 1 and other factors. For example, the (A2) component may be composed of a homopolymer of a styrene-based monomer or a copolymer thereof, or may contain other polystyrene-based resins (rubber-like polymers, styrene-(meth)acrylic acid copolymers, etc.). The types of the (A2) component may be the same as those of the (A1) component. The styrene-styrene-(meth)acrylic acid copolymer (A2) component may be the same as or different from the (A1) component.
[0058] When the second foam layer resin contains the (B2) component, the type or content of the (B2) component is the same as the type or content of the (B1) component. At least one of the type or content of the (B2) component and the type or content of the (B1) component may be the same, or both may be different.
[0059] When the second foam layer resin contains the (C2) component, the type or content of the (C2) component is the same as the type or content of the (C1) component. At least one of the type or content of the (C2) component and the type or content of the (C1) component may be the same, or both may be different.
[0060] The type and amount of the foaming agent of the second foamable resin composition are the same as those of the first foamable resin composition. At least one of the type and amount of the foaming agent of the second foamable resin composition may be the same as those of the first foamable resin composition, or both may be different.
[0061] The second foamable resin composition may contain other components (hereinafter also referred to as "second foam layer optional components") other than the second foam layer resin and the foaming agent. The type and amount of the optional ingredient of the second foam layer is the same as the type and amount of the optional ingredient of the first foam layer. The type and amount of the optional ingredient of the second foam layer may be at least one of the same as the type and amount of the optional ingredient of the first foam layer, or may be both different.
[0062] The thickness of the second unit foam layer 14 is similar to that of the first unit foam layer 12. The thickness of the second unit foam layer 14 may be the same as or different from that of the first unit foam layer 12.
[0063] The apparent density of the second unit foamed layer 14 is similar to the apparent density of the first unit foamed layer 12. The apparent density of the second unit foamed layer 14 may be the same as or different from the apparent density of the first unit foamed layer 12.
[0064] The expansion ratio of the second unit foaming layer 14 is the same as that of the first unit foaming layer 12. The expansion ratio of the second unit foaming layer 14 may be the same as or different from that of the first unit foaming layer 12.
[0065] The glass transition point Tg2 of the second unit foam layer 14 is the same as the glass transition temperature Tg1. The glass transition temperature Tg2 may be the same as or different from the glass transition temperature Tg1.
[0066] The average cell diameter of the second unit foamed layer 14 is the same as that of the first unit foamed layer 12. The average cell diameter of the second unit foamed layer 14 may be the same as that of the first unit foamed layer 12 or may be different.
[0067] <First non-foamed layer> The first non-foamed layer 20 of this embodiment is located on the first unit foamed layer 12 of the foamed layer 10. The first non-foamed layer 20 has a three-layer structure including a first unit non-foamed layer 22, a second unit non-foamed layer 24, and a third unit non-foamed layer 26. In this embodiment, the third unit non-foamed layer 26, the second unit non-foamed layer 24, and the first unit non-foamed layer 22 are laminated in this order from the foamed layer 10 side. By including the first non-foamed layer 20, the foamed sheet 1 can further improve aesthetics and moldability.
[0068] The thickness t20 of the first non-foamed layer 20 is appropriately determined taking into consideration the application and the like. For example, the thickness t20 is preferably 80 to 180 μm, more preferably 80 to 170 μm, further preferably 80 to 150 μm, and particularly preferably 100 to 145 μm. When the thickness t20 is equal to or greater than the above lower limit, the strength can be increased. When the thickness t20 is equal to or less than the above upper limit, the moldability can be increased and the environmental load can be reduced.
[0069] The basis weight of the first non-foamed layer 20 is 80 to 200 g / m 2 is preferable, and 80 to 150 g / m 2 When the basis weight is equal to or more than the lower limit, the impact resistance and rigidity can be further increased, whereas when the basis weight is equal to or less than the upper limit, the moldability can be improved. The basis weight of the first non-foamed layer 20 can be measured in the same manner as the basis weight of the foamed sheet 1.
[0070] <First unit non-foamed layer> The first unit non-foamed layer 22 is a layer formed by curing a first non-foamable resin composition containing a first non-foamed layer resin. The first unit non-foamed layer 22 may be a non-stretched film or a stretched film.
[0071] Examples of the resin for the first non-foamed layer include polyolefin resins, polystyrene resins, and polyester resins. Examples of the polyolefin resin include polypropylene resin and polyethylene resin. The polystyrene resin may be the same as that of the component (A1). The polystyrene resin of the first non-foamed layer resin may be the same as or different from that of the component (A1). An example of the polyester resin is a polyethylene terephthalate resin. The above-mentioned first non-foamed layer resin may be used alone or in combination of two or more kinds.
[0072] The first non-foamable resin composition may contain optional components (optional components for the first non-foamed layer) other than the first non-foamable resin. Examples of optional components of the first non-foamed layer include stabilizers, ultraviolet absorbers, antioxidants, colorants, deodorants, lubricants, flame retardants, antistatic agents, and carbon. The type of the optional component of the first non-foamed layer is determined in consideration of the physical properties required for the first unit non-foamed layer 22. The optional component of the first non-foamed layer may be one type alone or a combination of two or more types.
[0073] The thickness of the first unit non-foamed layer 22 is appropriately determined taking into consideration the application and the like. The thickness of the first unit non-foamed layer 22 is, for example, preferably 10 to 150 μm, more preferably 10 to 100 μm. When the thickness of the first unit non-foamed layer 22 is equal to or greater than the above lower limit, it becomes easier to stretch and formability can be improved. When the thickness of the first unit non-foamed layer 22 is equal to or less than the above upper limit, the environmental load can be reduced and productivity and glossiness can be improved.
[0074] <<Second Unit Non-foamed Layer>> The second unit non-foamed layer 24 is a layer formed by curing a second non-foamable resin composition containing a second non-foamed layer resin. The second unit non-foamed layer 24 may be a non-stretched film or a stretched film.
[0075] The second non-foamed layer resin is similar to the first non-foamed layer resin. The second non-foamed layer resin may be the same as or different from the first non-foamed layer resin.
[0076] The second non-foamable resin composition may contain optional components (second non-foamed layer optional components) other than the second non-foamable resin. The second non-foamed layer optional ingredients are similar to the first non-foamed layer optional ingredients. The second non-foamed layer optional ingredients may be the same as or different from the first non-foamed layer optional ingredients.
[0077] The thickness of the second unit non-foamed layer 24 is similar to the thickness of the first unit non-foamed layer 22. The thickness of the second unit non-foamed layer 24 may be the same as the thickness of the first unit non-foamed layer 22 or may be different.
[0078] There is no particular limitation on the combination of the first unit non-foamed layer 22 and the second unit non-foamed layer 24. For example, a combination of a non-stretched polypropylene-based resin film as the first unit non-foamed layer 22 and a non-stretched polystyrene-based resin film as the second unit non-foamed layer 24 may be used. A print layer may be located between the first unit non-foamed layer 22 and the second unit non-foamed layer 24 .
[0079] <Third unit non-foamed layer> The third unit non-foamed layer 26 is a layer formed by curing a third non-foamable resin composition containing a third non-foamed layer resin. The third unit non-foamed layer 26 may be a stretched film.
[0080] The third non-foamed layer resin is similar to the first non-foamed layer resin. The third non-foamed layer resin may be the same as or different from the first non-foamed layer resin or the second non-foamed layer resin.
[0081] The third non-foamable resin composition may contain optional components (third non-foamed layer optional components) other than the third non-foamable resin. The third non-foamed layer optional ingredients are similar to the first non-foamed layer optional ingredients. The third non-foamed layer optional ingredients may be the same as or different from the first non-foamed layer optional ingredients or the second non-foamed layer optional ingredients.
[0082] The thickness of the third unit non-foamed layer 26 is similar to the thickness of the first unit non-foamed layer 22. The thickness of the third unit non-foamed layer 26 may be the same as or different from the thickness of the first unit non-foamed layer 22 or the thickness of the second unit non-foamed layer 24.
[0083] The basis weight of the third unit non-foamed layer 26 is similar to the basis weight of the first unit non-foamed layer 22. The basis weight of the third unit non-foamed layer 26 may be the same as or different from the basis weight of the first unit non-foamed layer 22 or the basis weight of the second unit non-foamed layer 24.
[0084] There is no particular limitation on the combination of the first unit non-foamed layer 22, the second unit non-foamed layer 24, and the third unit non-foamed layer 26. For example, a combination of a non-stretched polypropylene-based resin film as the first unit non-foamed layer 22, a non-stretched polystyrene-based resin film as the second unit non-foamed layer 24, and a polystyrene-based resin film as the third unit non-foamed layer 126 may be used. In this case, from the viewpoint of increasing strength and glossiness, the resin of the third unit non-foamed layer is preferably HIPS.
[0085] <Second non-foamed layer> The second non-foamed layer 30 of this embodiment is located on the second unit foamed layer 14 of the foamed layer 10. By having the second non-foamed layer 30, the strength of the foamed sheet 1 can be further improved.
[0086] The second non-foamed layer 30 has the same composition as the first unit non-foamed layer 22. That is, the non-foamed resin composition constituting the second non-foamed layer 30 is the same as the first non-foamed resin composition constituting the first unit non-foamed layer 22. The non-foamed resin composition constituting the second non-foamed layer 30 may be the same as or different from the first non-foamed resin composition constituting the first unit non-foamed layer 22.
[0087] The second non-foamed layer 30 may be a non-stretched film or a stretched film. The thickness t30 of the second non-foamed layer 30 is similar to the thickness of the first unit non-foamed layer 22. The thickness t30 may be the same as the thickness of the first unit non-foamed layer 22, or may be different. The second non-foamed layer 30 is preferably a film of a polystyrene-based resin thermally laminated onto the foamed layer 10 .
[0088] <Manufacturing method> An example of a method for producing the foamed sheet 1 will be described. The first foamable resin composition is melt-kneaded, and the kneaded product is extruded into a sheet and foamed to obtain the first unit foam layer 12 . The second foamable resin composition is melt-kneaded, and the kneaded product is extruded into a sheet and foamed to obtain the second unit foam layer 14 . Next, the first unit foam layer 12 and the second unit foam layer 14 are bonded together to form the foam layer 10. Examples of a method for bonding the first unit foam layer 12 and the second unit foam layer 14 include a method of heat fusing the first unit foam layer 12 and the second unit foam layer 14 together. Alternatively, a method of co-extruding the first foamable resin composition and the second resin composition to form the first unit foam layer 12 and the second unit foam layer 14 and bonding the two layers together may be used.
[0089] Next, a first non-foamed layer 20 is provided on one surface of the foamed layer 10 (the surface of the first unit foamed layer 12 in this embodiment). The first non-foamed layer 20 may be formed by extruding the third non-foamable resin composition onto the first unit foamed layer 12 using a T-die, placing a laminate film on the extruded third non-foamable resin composition, and curing the third non-foamable resin composition. The laminate film is a laminate film of the first unit non-foamed layer 22 and the second unit non-foamed layer 24. Alternatively, the first unit non-foamed layer 22, the second unit non-foamed layer 24, and the third unit non-foamed layer 26 are laminated by coextrusion to form the first non-foamed layer 20 as a three-layer laminate film. Next, the three-layer laminate film is fused to the foamed layer 10 by heat fusion or the like to form the first non-foamed layer 20.
[0090] As described above, according to the foamed sheet of the present embodiment, since the foamed layer contains a hydrogenated styrene-based thermoplastic elastomer, the compatibility with polypropylene is improved and the appearance defect can be suppressed. In addition, since the foamed layer resin contains a specific amount of rubber, the impact resistance can be improved. According to the foamed sheet of the present embodiment, since the foamed layer has non-foamed layers on both sides thereof, the impact resistance can be further improved.
[0091] Second Embodiment The foamed sheet of the present embodiment will be described with reference to Fig. 2. Mainly, configurations different from those of the first embodiment will be described, and the same configurations will be denoted by the same reference numerals and description thereof will be omitted. The foamed sheet 100 of FIG. 2 has a foamed layer 110, a first non-foamed layer 20, and a second non-foamed layer 30.
[0092] The thickness t100 of the foamed sheet 100 is, for example, preferably 0.5 to 3.0 mm, more preferably 0.7 to 2.5 mm, and even more preferably 1.0 to 2.0 mm. When the thickness t100 is equal to or greater than the lower limit, the impact resistance and rigidity can be further improved. When the thickness t100 is equal to or less than the upper limit, the reproducibility of the shape can be improved (i.e., moldability can be improved) when a molded product is formed by thermoforming.
[0093] The basis weight of the foamed sheet 100 is, for example, 100 to 500 g / m 2 is preferable, and 150 to 350 g / m 2 More preferably, 200 to 300 g / m 2 When the basis weight is equal to or more than the lower limit, the impact resistance and rigidity can be further improved, and when the basis weight is equal to or less than the upper limit, the moldability can be improved.
[0094] The apparent density of the foamed sheet 100 is, for example, 0.06 to 0.716 g / cm 3 is preferable, and 0.086 to 0.54 g / cm 3 More preferably, 0.13 to 0.363 g / cm 3 is more preferred.
[0095] The foamed layer 110 of this embodiment has a single-layer structure. The foamed layer 110 has the same composition as the first unit foamed layer 12 in the first embodiment. That is, the foamable resin composition constituting the foamed layer 110 is the same as the first foamable resin composition constituting the first unit foamed layer 12.
[0096] The thickness t110 of the foam layer 110 is similar to the thickness of the first unit foam layer 12 of the first embodiment. The basis weight of the foam layer 110 is similar to that of the first unit foam layer 12 of the first embodiment. The apparent density of the foam layer 110 is similar to the apparent density of the first unit foam layer 12 of the first embodiment. The expansion ratio of the foam layer 110 is similar to that of the first unit foam layer 12 of the first embodiment.
[0097] According to this embodiment, since the foam layer has a single-layer structure, the foam sheet can be further lightened and thinned.
[0098] (Molded body) The molded article of the present invention is obtained by thermoforming the foamed sheet of the present invention. Examples of the molded article include food containers, packaging materials, bedding materials, core materials, etc. Among them, the molded article is preferably a heat-resistant container. Methods for producing molded bodies include, for example, vacuum forming, compressed air forming, and applications of these, such as free drawing forming, plug and ridge forming, ridge forming, matched mold forming, straight forming, drape forming, reverse draw forming, air slip forming, plug assist forming, and plug assist reverse load forming, as well as conventionally known thermoforming methods.
[0099] (Other embodiments) In the first and second embodiments, the first non-foamed layer has a three-layer structure, but the present invention is not limited thereto, and the layer structure of the first non-foamed layer may be one or two layers, or four or more layers. However, from the viewpoints of cost and strength, the layer structure of the first non-foamed layer is preferably two or three layers. FIG. 3 shows an example of a foamed sheet having a two-layer structure with a first non-foamed layer. The foamed sheet 200 of FIG. 3 has a foamed layer 10, a first non-foamed layer 220 located on one side of the foamed layer 10, and a second non-foamed layer 30 located on the other side of the foamed layer 10. This embodiment differs from the foamed sheet 1 of the first embodiment in that the first non-foamed layer 210 has a two-layer structure consisting of a first unit non-foamed layer 22 and a second unit non-foamed layer 24. The foamed sheet 200 has an advantage in terms of cost and reduction of environmental load since the first non-foamed layer 220 has a two-layer structure. The foam layer 10 of the foam sheet 200 may be a foam layer having a single-layer structure (for example, the foam layer 110 of the second embodiment).
[0100] In the first and second embodiments, the non-foamed layers are located on both sides of the foamed layer. However, the present invention is not limited thereto, and the foamed sheet may have a non-foamed layer on only one side of the foamed layer, or may not have a non-foamed layer. However, from the viewpoint of further increasing the strength of the foamed sheet, it is preferable to have a non-foamed layer, and it is more preferable to have a non-foamed layer on both sides of the foamed layer. FIG. 4 shows a foamed sheet having a non-foamed layer on only one side of the foamed layer. The foamed sheet 300 in FIG. 4 has a foamed layer 10 and a first non-foamed layer 20 located on one side of the foamed layer 10, and has no non-foamed layer on the other side of the foamed layer 10. The foamed sheet 300 of this embodiment differs from the first embodiment in that a non-foamed layer is provided on only one side of the foamed layer 10. The foam layer 10 of the foam sheet 300 may be a foam layer having a single-layer structure (for example, the foam layer 110 of the second embodiment).
[0101] In the first and second embodiments, the foam layer has one or two unit foam layers. However, the present invention is not limited thereto, and the layer structure of the foam layer may have three or more layers. However, from the viewpoint of moldability and productivity of the foam sheet, the layer structure of the foam layer is preferably one to three layers, more preferably one to two layers. When the layer structure of the foam layer is two or more layers, it is sufficient that one or more of the unit foam layers are the specific foam layers, and all of the unit foam layers may be the specific foam layers. EXAMPLES
[0102] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the tables, "-" indicates that the component was not blended. (Raw materials used) <Component (A1): Polystyrene resin> A1-1: Heat-resistant polystyrene (heat-resistant PS), product name "T080", manufactured by Toyo Styrene Co., Ltd., styrene-methacrylic acid copolymer resin, styrene monomer content = 92 mass%, methacrylic acid monomer content = 8 mass%. A1-2: Polystyrene (PS), product name "HRM12", manufactured by Toyo Styrene Co., Ltd. A1-3: HIPS, rubber content = 60 mass%, styrene-butadiene block copolymer resin (SBS: styrene block copolymer), product name "Tufprene 125", manufactured by Asahi Kasei Chemicals Corporation. A1-4: Recycled raw material whose main component is polystyrene resin. <Component (A2): Polystyrene resin> A2-1: PS, HRM12 (product name), manufactured by Toyo Styrene Co., Ltd. A2-2: HIPS, rubber content = 6 mass%, E641N (product name), manufactured by Toyo Styrene Co., Ltd. <Component (B1): Additive styrene-based thermoplastic elastomer> B1-1: Hydrogenated styrene-based thermoplastic elastomer 1 (styrene-butadiene-butylene-styrene block copolymer (SBBS), styrene-based monomer component 67% by mass, butadiene monomer component 33% by mass, hydrogenation rate 60% by mass, manufactured by Asahi Kasei, product name "Tuftec P2000"). B1-2: Hydrogenated styrene-based thermoplastic elastomer 2 (styrene-ethylene-butylene-styrene block copolymer (SEBS), styrene-based monomer component 67% by mass, hydrogenation rate 100% by mass, manufactured by Asahi Kasei Corporation, product name "Tuftec H1043"). <Component (C1): Polypropylene resin> · C1-1: Recycled raw material for polypropylene resin moldings (recovered products from the market). <Rubber> Styrene-butadiene block copolymer resin (SBS: styrene block copolymer) (product name "Tufprene 125", manufactured by Asahi Kasei Chemicals Corporation). <Carbon> Carbon-containing masterbatch (Polycool Kogyo Co., Ltd., product name "Polycool Master ESH-K4799LB"). <Talc> Talc MB: Kneaded masterbatch (product name "DSM1401M"). <Foaming agent> A mixture of isobutane:normal butane = 70:30 (mass ratio).
[0103] (Examples 1 to 5, Comparative Examples 1 to 5) A foamed sheet similar to foamed sheet 100 in FIG. 2 was obtained by the following procedure. The amount of talc MB was set to obtain the amount of talc shown in Table 1, and the (A1), (B1), and (C1) components, talc MB, and carbon were mixed together. These were charged into a batch-type continuous mixer, and then fed into the hopper of the upstream extruder (screw diameter 90 mm) of a tandem extruder (having a screw diameter of 90 mm and a screw diameter of 115 mm). In the upstream extruder, the maximum cylinder temperature was set to 280° C., a foaming agent was added to the resin to form a foamable resin composition, and the foamable resin composition was supplied to the downstream extruder. In the downstream extruder, the foamable resin composition was fed to the die at a rate of 120 kg / h. The foamable resin composition fed into the mold was fed into a circular die with a diameter of 175 mm and a slit clearance of 0.5 mm, and passed through the slit of the die to form a cylindrical foamed sheet. Immediately afterwards, the cylindrical foamed sheet was cooled by blowing air onto it, taken along the outer surface of a cooling device (mandrel) with a diameter of 675 mm, and then cut into two pieces along the extrusion direction to obtain a foamed sheet with a width of 1050 mm. The air temperature was 31°C, and the amount of air blown was 0.053 m on the inside. 3 / m 2 , 0.032m on the outer first foam layer side 3 / m 2 It was decided. To replace the foaming gas, the foamed sheet was stored for 14 days after production. HIPS (same as A2-2) was melted in an extruder (diameter 120 mm) set at a maximum temperature of 240°C, and this was extruded from a T-die onto one side of the foamed sheet, and laminated to a thickness of 100 μm. Immediately after that, a film (CPP / CPS 45 μm plain (product name)) in which CPP (unoriented polypropylene) 25 μm and CPS 20 μm (Oishi Sangyo SPH) were dry laminated onto the HIPS layer. A CPS (unoriented polystyrene) film (thickness 20 μm, Oishi Sangyo SPH) was hot laminated onto the other side of the foamed sheet to obtain a foamed sheet.
[0104] (Measurement method) <Average bubble diameter> The average cell diameter of the foamed sheet was determined as follows. The foamed sheet was cut perpendicularly to the surface from the center in the width direction along the MD direction (extrusion direction) and TD direction (direction perpendicular to the extrusion direction). The cut surface was photographed at a magnification of 50x using a scanning electron microscope (SU1510, Hitachi High-Technologies Corporation). The microscope images were taken so that the specified magnification would be achieved when two images (four images in total) were printed side by side on a single sheet of A4 paper in landscape orientation. Specifically, on the image, 60 mm arbitrary straight lines parallel to each of the MD and TD directions and 60 mm arbitrary straight lines in the direction perpendicular to each direction (VD direction) were drawn. For each of the cross sections cut along the MD direction (MD cross section) and the cross sections cut along the TD direction (TD cross section), two microscopic images of four fields of view were taken and printed on A4 paper. Three arbitrary straight lines (60 mm long) parallel to the MD direction were drawn on each of the two images of the MD cross section, and three arbitrary straight lines (60 mm long) parallel to the TD direction were drawn on each of the two images of the TD cross section. In addition, three straight lines (60 mm long) parallel to the VD direction were drawn on one image of the MD cross section and one image of the TD cross section, and six arbitrary straight lines of 60 mm long parallel to the MD, TD, and VD directions were drawn in each direction. Note that the arbitrary straight lines were made as far as possible so that bubbles would not come into contact only at the contact points, and if there was contact, the bubbles were also counted. The number of bubbles D counted for six arbitrary straight lines in each of the MD, TD, and VD directions was calculated as the arithmetic average, which was used as the number of bubbles in each direction. The average chord length t of the bubbles was calculated from the image magnification at which the number of bubbles was counted and this number of bubbles using formula (s1).
[0105] Average chord length t (mm) = 60 / (number of bubbles × image magnification) (s1)
[0106] The image magnification was calculated by measuring the scale bar on the image to the nearest 1 / 100 mm using a Digimatic Caliper (manufactured by Mitutoyo Corporation) and using the following formula: Image magnification = Actual scale bar value (mm) / Displayed scale bar value (mm).
[0107] The bubble diameter in each direction was calculated using equation (s2). Bubble diameter D (mm) = t / 0.616 (s2)
[0108] Furthermore, the cube root of the product was determined as the average bubble diameter (equation (s3)). Average bubble diameter (mm) = (DMD x DTD x DVD) 1 / 3 (s3) DMD: bubble diameter in MD direction (mm). DTD: bubble diameter in TD direction (mm). DVD: Bubble diameter in the VD direction (mm).
[0109] <Impact resistance> The impact resistance was evaluated comprehensively based on the required punching energy and the results of the three-point bending test, according to the following evaluation criteria.
[0110] Evaluation Criteria 〇: Three-point bending strength is 4 to 10 N, and the energy required for punching is 0.2 to 1.0 J (both sides). △: Three-point bending strength is less than 4N or more than 10N, and the required punching energy is 0.2 to 1.0J (both sides). Or, three-point bending strength is 2 to 5N, and the required punching energy is less than 0.2J or more than 1.0J (one side or both sides). ×: Three-point bending strength is less than 4 N or more than 10 N, and the energy required for punching is less than 0.2 J or more than 1.0 J (one side or both sides).
[0111] <Energy required for punching> The energy required for punching was measured using a film impact tester (manufactured by Yasuda Seiki Seisakusho, product name "No. 181 Film Impact Tester"). A 100mm x 90mm sample was taken from the foam sheet. The energy required to punch the sample (unit: J) was determined in an environment controlled to a temperature of 22°C and a relative humidity of 40% using an impact ball size of 12.7mmR and a pendulum angle of 90°. Specifically, the sample for which the required punching energy was to be calculated was set between the sample plate and the sample presser, the pointer was placed on the 3.0 J line, and the pendulum stopper handle was tilted to drop the pendulum. This caused the sample to break, and the pendulum pushed the pointer, and the scale indicated was read. The above operation was performed five times on each side of the foamed sheet, and the average value was calculated.
[0112] ≪Maximum point load≫ The maximum point load was determined according to the three-point bending test method described in JIS K7221:1997 "Bending test method for rigid foamed plastics." Test pieces with a width of 50 mm and a length of 150 mm were cut out from three arbitrary points of the foam sheet. The maximum point load (N) was measured for these three test pieces using a Tensilon universal testing machine (manufactured by A&D, model: RTG-1310) under the following conditions: distance between supports: 100 mm, compression speed: 50 mm / min, and tip curvature radius of the support jig and pressure jig: 3.2 mm.
[0113] <Appearance> The foamed sheet of each example was visually observed and the appearance was evaluated according to the following evaluation criteria. Evaluation Criteria ◯: No resin lumps or streaks are formed on the surface, and the appearance is beautiful. ×: Resin lumps and streaks were observed on the surface, and the appearance was beautiful.
[0114] <Heat resistance test> Using the foamed sheet of each example, a bowl-shaped container having an opening inner diameter of 160 mm, a bottom inner diameter of 110 mm, a depth of 50 mm, and a drawing ratio of 0.31 was produced. A foamed container was produced by continuously supplying a foamed sheet to a press molding device having a cavity (concave mold) with 5 x 5 = 25 concave portions corresponding to the outer shape of the foamed container and a plug (convex mold) with the same number of convex portions corresponding to the inner shape of the container. The molding conditions were as follows: molding cycle for one shot (=25 pieces) was 10.0 seconds, the heater temperature on the cavity side was set to 320°C, and the heater temperature on the plug side was set to 350°C. The timing of molding was set so that the cavity and the plug came into contact with the laminated polystyrene resin foam sheet at almost the same time and molding was started. When heated with a heater, those that were smooth and in good condition were rated as "◯" (good), and those that developed blisters and were unnecessarily bad were rated as "×".
[0115] [Table 1]
[0116] As shown in Table 1, in all of Examples 1 to 5 in which the present invention was applied, the impact resistance and appearance were rated "good." Comparative Example 1, which did not contain a hydrogenated styrene-based thermoplastic elastomer, had an appearance of "x". In Comparative Example 2, in which the content of the hydrogenated styrene-based thermoplastic resin elastomer was 0.4 parts by mass relative to 100 parts by mass of the polystyrene-based resin, the appearance was rated as "x". In Comparative Example 3, in which the polypropylene resin content was 28% by mass, the appearance was rated as "X". Comparative Example 4, which does not contain rubber content, was rated as "Δ" in impact resistance. Comparative Example 5, which did not contain a hydrogenated styrene-based thermoplastic elastomer and had an expansion ratio of 17.9, was rated "x" for impact resistance and appearance. From these results, it was confirmed that application of the present invention can improve impact resistance and suppress defects in appearance.
[0117] (Examples 11 to 12) A foamed sheet similar to foamed sheet 1 in FIG. 1 was obtained by the following procedure. The amount of talc MB was set to the amount of talc shown in Table 2, and the raw materials for the first unit foam layer, Component (A1), Component (B1), Component (C1), talc MB, and carbon, were mixed. These were charged into a batch-type continuous mixer, and then fed into the hopper of the upstream extruder (screw diameter 90 mm) of a tandem extruder (having a screw diameter of 90 mm and a screw diameter of 115 mm). In the upstream extruder, the maximum cylinder temperature was set to 280° C., a foaming agent was added to the resin to prepare a first foamable resin composition, and the first foamable resin composition was supplied to the downstream extruder. In the downstream extruder, the first expandable resin composition was fed to the joining die at a rate of 120 kg / h. The amount of talc MB was set to the amount of talc shown in Table 2, and the (A2) component, which is the raw material of the second unit foam layer, talc MB, and carbon were mixed. These were charged into a batch-type continuous mixer, and then fed into the hopper of the upstream extruder (screw diameter 90 mm) of another tandem extruder (having a screw diameter of 90 mm and a screw diameter of 115 mm). In the upstream extruder, the maximum cylinder temperature was set to 260° C., a foaming agent was added to prepare a second foamable resin composition, and the second foamable resin composition was supplied to the downstream extruder. In the downstream extruder, the second foamable resin composition was fed to the joining die at a rate of 120 kg / h. The first and second foamable resin compositions fed into the joining die were joined and laminated in the joining die, and the laminate was fed into an annular die (diameter 175 mm, slit clearance 0.5 mm) and passed through the slits of the die to form a cylindrical foam sheet. Immediately after that, the cylindrical foam was cooled by blowing air into it, and taken along the outer surface of a cooling device (mandrel) with a diameter of 675 mm, and then cut into two pieces along the extrusion direction to obtain a foam sheet with a width of 1050 mm. The air temperature was 31°C, and the amount of air blown was 0.053 m on the inside first unit foam layer side. 3 / m 2 , 0.032m on the outer first foam layer side 3 / m 2 It was decided. To replace the foaming gas, the foamed sheet was stored for 14 days after production. HIPS (same as A2-2) was melted in an extruder (diameter 120 mm) set at a maximum temperature of 240°C, extruded from a T-die onto one side of the foamed sheet, and laminated in the form of a film with a thickness of 100 μm. Immediately after that, a film (CPP / CPS 45 μm plain (product name)) in which CPP (unoriented polypropylene) 25 μm and CPS 20 μm (Oishi Sangyo SPH) were dry-laminated onto the HIPS layer. A CPS (unoriented polystyrene) film (thickness 20 μm, Oishi Sangyo SPH) was hot-laminated onto the other side of the foamed sheet to obtain a foamed sheet. The heat resistance, impact resistance and appearance of the resulting foamed sheet were evaluated, and the results are shown in the table.
[0118] [Table 2]
[0119] As shown in Table 2, Examples 11 and 12 in which the present invention was applied were all rated as "good" for heat resistance, impact resistance and appearance. [Explanation of symbols]
[0120] 1, 100, 200, 300 Polystyrene resin foam sheet 10, 110 Foam layer 12 First unit foam layer 14 Second unit foam layer 20, 220 First non-foamed layer 22 First unit non-foamed layer 24 Second unit non-foamed layer 26 Third unit non-foamed layer 30 Second non-foamed layer
Claims
1. A foam layer is formed of one or more unit foam layers, At least one of the unit foam layers is a specific foam layer containing a resin including 100 parts by mass of a polystyrene-based resin, 0.5 to 15 parts by mass of a hydrogenated styrene-based thermoplastic elastomer, and 1 to 20 parts by mass of a polypropylene-based resin; The polystyrene resin contains a rubber component and a styrene-(meth)acrylic acid copolymer, The polystyrene-based resin foam sheet, wherein the rubber content is 1 to 7 mass% based on the total mass of the resin.
2. 2. The polystyrene-based resin foamed sheet according to claim 1, wherein the specific foamed layer has a sea-island structure in which the polypropylene-based resin is dispersed in a matrix structure of the polystyrene-based resin and the hydrogenated styrene-based thermoplastic elastomer.
3. The polystyrene-based resin foam sheet according to claim 1 or 2, wherein the hydrogenated styrene-based thermoplastic elastomer comprises at least one selected from a styrene-butadiene-butylene-styrene block copolymer and a styrene-ethylene-butylene-styrene block copolymer.
4. The polystyrene-based resin foamed sheet according to claim 1 or 2, wherein the specific foamed layer further contains carbon.
5. The polystyrene-based resin foam sheet according to claim 1 or 2, wherein the resin contains recycled materials.
6. The polystyrene-based resin foamed sheet according to claim 1 or 2, which has a non-foamed layer on one or both sides of the foamed layer.
7. A method for producing the polystyrene-based resin foamed sheet according to claim 1, A method for producing a polystyrene-based resin foamed sheet, comprising a step of extruding a kneaded mixture of the resin and the foaming agent into a sheet shape and foaming the sheet to form the specific foamed layer.
8. The method for producing a polystyrene-based resin foam sheet according to claim 7 , wherein the resin contains recycled materials.
Citation Information
Patent Citations
Synthetic resin foamed sheet and method for producing the same, laminated sheet, and food container
JP2021046466A