Sintered composite material, bonded body, member for semiconductor manufacturing apparatus, and method for manufacturing sintered composite material
A silicon carbide, tungsten silicide, and tungsten carbide composite material addresses thermal expansion issues with aluminum nitride electrostatic chucks, ensuring durability and efficient heat dissipation in semiconductor manufacturing equipment.
Patent Information
- Application Number
- JP2023057826
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Existing composite materials for cooling plates in semiconductor processing, such as those composed of silicon carbide, titanium silicon carbide, and titanium carbide, have a linear thermal expansion coefficient that is outside the preferred range, leading to decreased compactness and unsuitability for use with aluminum nitride electrostatic chucks.
A composite material sintered body composed of silicon carbide, tungsten silicide, and tungsten carbide, with specific weight percentages and porosity, achieving a thermal expansion coefficient matching that of aluminum nitride and maintaining high density and strength.
The composite material ensures durability and efficient heat dissipation by minimizing thermal expansion mismatch and peeling, extending the lifespan of semiconductor manufacturing equipment components.
Smart Images

Figure 2024145464000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a sintered composite material. [Background technology]
[0002] A cooling plate is attached to an electrostatic chuck that becomes hot during a semiconductor process in order to dissipate heat. For example, a dense sintered body of a composite material made of silicon carbide, titanium silicide, titanium silicon carbide, and titanium carbide, which is suitable as a constituent material of a cooling plate when the material of the electrostatic chuck is alumina, is already known (see, for example, Patent Document 1). Such a composite sintered body has a small difference in linear thermal expansion coefficient with alumina, and is characterized by being dense and high strength.
[0003] Also, a dense sintered body of a composite material consisting of silicon carbide, titanium silicon carbide, and titanium carbide, which is suitable as a constituent material of a cooling plate when the material of an electrostatic chuck is aluminum nitride, is already known (see, for example, Patent Document 2). Such a composite material sintered body has a small difference in linear thermal expansion coefficient from aluminum nitride, and is characterized by being dense and high strength. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2014-198662 A [Patent Document 2] JP 2014-208567 A Summary of the Invention [Problem to be solved by the invention]
[0005] The linear thermal expansion coefficient of aluminum nitride at 40° C. to 570° C. is 5.1 ppm / K, whereas the suitable range of the linear thermal expansion coefficient of the composite material disclosed in Patent Document 2 at 40° C. to 570° C. is 5.4 ppm / K to 6.0 ppm / K. In order to realize a linear thermal expansion coefficient of 5.1 ppm / K in the Ti-Si-C-based composite sintered body as disclosed in Patent Document 2, it is necessary to increase the amount of silicon carbide. However, in this case, the density of the composite sintered body decreases, and it becomes unsuitable for the cooling plate of an electrostatic chuck.
[0006] The present invention has been made in view of the above problems, and has an object to provide a dense composite sintered body which is composed of constituent phases different from those of the prior art, has a linear thermal expansion coefficient difference with aluminum nitride that is equal to or smaller than that of the prior art, and has a high density. [Means for solving the problem]
[0007] In order to solve the above problems, a first aspect of the present invention is a composite material sintered body, characterized in that it is composed of silicon carbide, tungsten silicide, and tungsten carbide, contains 14.4 wt% or more and 48.6 wt% or less of silicon carbide, and has an open porosity of 1% or less.
[0008] A second aspect of the present invention is a sintered composite material according to the first aspect, characterized in that the difference between the thermal expansion coefficient at 40°C to 550°C and the thermal expansion coefficient of aluminum nitride at 40°C to 550°C is 0.5 ppm / K or less.
[0009] A third aspect of the present invention is the sintered composite material according to the second aspect, characterized in that the open porosity is 0.1% or less.
[0010] A fourth aspect of the present invention is a sintered composite material according to any one of the first to third aspects, characterized in that the surfaces of individual crystal particles of silicon carbide are covered with at least one of tungsten silicide and tungsten carbide, and thus at least one of tungsten silicide and tungsten carbide crystal particles are present in the gaps between the silicon carbide crystal particles.
[0011] A fifth aspect of the present invention is a composite material sintered body according to any one of the first to fourth aspects, characterized in that the content of tungsten silicide is greater than the content of silicon carbide.
[0012] A sixth aspect of the present invention is a sintered composite material according to any one of the first to fifth aspects, characterized in that the four-point bending strength is 200 MPa or more.
[0013] A seventh aspect of the present invention is the sintered composite material according to the sixth aspect, characterized in that the four-point bending strength is 350 MPa or more.
[0014] An eighth aspect of the present invention is a sintered composite material according to any one of the first to seventh aspects, characterized in that the thermal conductivity is 90 W / m·K or more.
[0015] A ninth aspect of the present invention is a sintered composite material according to any one of the first to eighth aspects, having a fracture toughness value of 6.0 MPa m 1 / 2 ~8.8MPa m 1 / 2 The present invention is characterized in that:
[0016] A tenth aspect of the present invention is a sintered composite material according to any one of the first to ninth aspects, characterized in that the Young's modulus is 273 GPa to 594 GPa.
[0017] An eleventh aspect of the present invention is the sintered composite material according to the tenth aspect, characterized in that the Young's modulus is 460 GPa to 594 GPa.
[0018] A twelfth aspect of the present invention is a bonded body formed by bonding a first member and a second member, characterized in that the first member is a sintered composite material composed of silicon carbide, tungsten silicide, and tungsten carbide, containing 14.4 wt% or more and 48.6 wt% or less of silicon carbide and having an open porosity of 1% or less, and the second member is made of aluminum nitride.
[0019] A thirteenth aspect of the present invention is a joined body according to the twelfth aspect, characterized in that a difference between a thermal expansion coefficient of the first member at 40°C to 550°C and a thermal expansion coefficient of the second member at 40°C to 550°C is 0.5 ppm / K or less.
[0020] A fourteenth aspect of the present invention is the joined body according to the thirteenth aspect, characterized in that the first member has an open porosity of 0.1% or less.
[0021] A fifteenth aspect of the present invention is a joined body according to any one of the twelfth to fourteenth aspects, characterized in that the first member and the second member are joined by metal joining.
[0022] A sixteenth aspect of the present invention is a member for semiconductor manufacturing equipment comprising a bonded body formed by bonding a first member and a second member, characterized in that the first member is a cooling member for cooling the second member, and is made of a composite material sintered body composed of silicon carbide, tungsten silicide and tungsten carbide, containing 14.4 wt% or more and 48.6 wt% or less of silicon carbide and having an open porosity of 1% or less, and the second member is made of aluminum nitride.
[0023] A 17th aspect of the present invention is a semiconductor manufacturing equipment member related to the 16th aspect, characterized in that a difference between a thermal expansion coefficient of the first member at 40°C to 550°C and a thermal expansion coefficient of the second member at 40°C to 550°C is 0.5 ppm / K or less.
[0024] An eighteenth aspect of the present invention is the semiconductor manufacturing equipment member according to the seventeenth aspect, characterized in that the first member has an open porosity of 0.1% or less.
[0025] A nineteenth aspect of the present invention is a semiconductor manufacturing equipment member according to any one of the sixteenth to seventeenth aspects, characterized in that the first member and the second member are metal-jointed.
[0026] A twentieth aspect of the present invention is a method for producing a sintered composite material, comprising: a mixing step of mixing SiC powder, WSi2 powder, and WC powder or W powder to obtain a powder mixture; a molding step of molding the powder mixture into a predetermined shape to obtain a molded body; and a sintering step of hot-pressing and sintering the molded body in an inert atmosphere; in the mixing step, 5.7 wt% to 27.7 wt% of SiC powder, 12.5 wt% to 55.3 wt% of WSi2 powder, and 49.5 wt% to 81.3 wt% of WC powder or 17.0 wt% to 55.7 wt% of W powder are mixed together to give a total weight ratio of 100 wt%; and in the sintering step, a maximum temperature is set to 1700°C to 1850°C, and a pressing pressure is set to 225 kgf / cm. 2 ~300kgf / cm 2 The present invention is characterized in that:
[0027] A 21st aspect of the present invention is a method for producing a composite material sintered body according to the 20th aspect, characterized in that in the mixing step, 5.7 wt% to 13.1 wt% SiC powder, 12.5 wt% to 39.1 wt% WSi2 powder, and 49.5 wt% to 81.3 wt% WC powder are mixed so that the total weight ratio is 100 wt%. Effect of the Invention
[0028] According to the first to eleventh, twentieth and twenty-first aspects of the present invention, a dense composite sintered body can be obtained which is unlikely to peel off even when bonded to aluminum nitride and used under thermal cycles.
[0029] Furthermore, according to the twelfth to nineteenth aspects of the present invention, even if the bonded body is used under thermal cycles, peeling of the members is unlikely to occur, so that the service life of semiconductor manufacturing equipment members including such bonded bodies can be improved. [Brief description of the drawings]
[0030] [Figure 1] 1 is an example of a cross-sectional SEM image of a sintered composite material. [Diagram 2] 1 is a graph showing the relationship between the silicon carbide content and the open porosity in a composite material sintered body. [Diagram 3] 1 is an example of a temperature and pressure profile in hot press firing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0031] <Sintered composite material> The composite sintered body according to the present embodiment is a composite sintered body containing silicon carbide (SiC), tungsten silicide, and tungsten carbide (WC) as crystal phases. The composite sintered body according to the present embodiment contains silicon carbide (SiC) in an amount of 14.4 wt% or more and 48.6 wt% or less when the total weight ratio of these crystal phases is 100 wt%. Preferably, the content of tungsten silicide is greater than the content of silicon carbide. Specifically, the tungsten silicide is WSi2 and W5Si3.
[0032] The fact that the composite sintered body according to the present embodiment contains SiC, tungsten silicide, and tungsten carbide as crystal phases is confirmed by X-ray diffraction measurement of the powder obtained by pulverizing the sintered body. The content of each substance is a value (simple quantitative value) calculated based on the diffraction peak of the X-ray diffraction measurement profile.
[0033] The composite sintered body according to the present embodiment is dense (a dense composite sintered body) with an open porosity of 1% or less. The open porosity is a value measured by Archimedes' method using pure water as a medium.
[0034] More specifically, in the composite sintered body according to the present embodiment, the surfaces of the individual silicon carbide crystal grains are covered with at least one of tungsten silicide and tungsten carbide, so that at least one of tungsten silicide and tungsten carbide crystal grains is present in the gaps between the silicon carbide crystal grains.
[0035] Fig. 1 is an example of a cross-sectional SEM image of a composite sintered body according to the present embodiment. In Fig. 1, images of four crystal phases, SiC, WSi2, WC, and W5Si3, are visible in order of decreasing brightness (darkness). More specifically, it can be seen that the individual SiC crystal grains, which are almost black, are separated from each other, and that the WSi2, WC, and W5Si3 crystal grains surround each crystal grain without any gaps.
[0036] In a sintered body having a high content of silicon carbide and in which silicon carbide particles are dispersed at a high frequency, many pores may occur between the particles, but in the case of the composite material sintered body according to the present embodiment, the surfaces of the silicon carbide particles are covered with particles of other crystal phases, so that such pores are hardly formed. As a result, the composite material sintered body according to the present embodiment is dense and has high strength.
[0037] Preferably, the open porosity of the composite sintered body according to the present embodiment is 0.1% or less. The composite sintered body satisfying this open porosity has extremely excellent density and extremely high strength.
[0038] FIG. 2 is a graph showing the relationship between the silicon carbide content and the open porosity in various composite sintered bodies produced under different production conditions. Specifically, the conditions of the maximum temperature and the press pressure during hot pressing, which will be described later, are different, and in FIG. 2, data is plotted according to the maximum temperature during hot pressing. In FIG. 2, it is confirmed that the open porosity tends to increase as the silicon carbide content in the composite sintered body increases. In particular, it can be seen that when the silicon carbide content is approximately 50 wt% or less, a composite sintered body having an open porosity of 1% or less can be produced by suitably setting the production conditions. Furthermore, it can be seen that when the silicon carbide content is approximately 30 wt% or less, a composite sintered body having an open porosity of 0.1% or less can also be produced. On the other hand, when the silicon carbide content exceeds 50 wt%, it is difficult to obtain a composite sintered body having a small open porosity, which is not preferable.
[0039] The linear thermal expansion coefficient of the composite sintered body according to the present embodiment is approximately the same as that of aluminum nitride (AlN). Note that, hereinafter, the linear thermal expansion coefficient is also simply referred to as the thermal expansion coefficient.
[0040] Specifically, the difference between the thermal expansion coefficient of the composite material sintered body according to this embodiment at 40° C. to 550° C. and the average thermal expansion coefficient (5.1 ppm / K) of aluminum nitride at 40° C. to 550° C. is 0.5 ppm / K or less. Specifically, the thermal expansion coefficient of the composite material sintered body according to this embodiment at 40° C. to 550° C. is 4.6 ppm / K to 5.6 ppm / K, and preferably 4.8 to 5.3 ppm / K.
[0041] Moreover, the composite sintered body according to the present embodiment has excellent thermal conductivity, with a thermal conductivity of 90 W / m·K or more, and preferably 100 W / m·K or more.
[0042] The composite sintered body according to the present embodiment is also excellent in strength, specifically, the four-point bending strength is 200 MPa or more, preferably 350 MPa or more, and more preferably 420 MPa or more.
[0043] In addition, the fracture toughness value (K1c) of the composite sintered body according to this embodiment is 6.0 MPa m 1 / 2 ~8.8MPa m 1 / 2 and preferably 6.2 MPa m 1 / 2 ~8.8MPa m 1 / 2 It is.
[0044] Furthermore, the Young's modulus of the composite sintered body according to the present embodiment may be from 273 GPa to 594 GPa, preferably from 330 GPa to 594 GPa, and more preferably from 460 GPa to 594 GPa.
[0045] <zygote> As described above, the composite sintered body according to the present embodiment has a thermal expansion coefficient similar to that of aluminum nitride. Therefore, even if a joined body in which a member (first member) made of the composite sintered body according to the present embodiment is joined (for example, by metal joining) to a member (second member) made of aluminum nitride is used under a thermal cycle in which low and high temperatures are repeated, separation between the two members is unlikely to occur.
[0046] The bonded body can be applied to, for example, a semiconductor manufacturing equipment member, for example, a semiconductor manufacturing equipment member in which a cooling plate (first member) made of the composite material sintered body according to the present embodiment and an electrostatic chuck (second member) made of aluminum nitride are bonded together with a bonding material mainly composed of aluminum or its alloy.
[0047] In such a bonded body or semiconductor manufacturing equipment member, the difference in linear thermal expansion coefficient between the first member and the second member is extremely small, so that the first member is unlikely to peel off from the second member even when used under thermal cycles.
[0048] Moreover, the first member made of the composite material sintered body according to this embodiment has sufficiently high thermal conductivity to efficiently dissipate heat contained in the second member made of aluminum nitride, thereby enabling the second member to be efficiently cooled.
[0049] Furthermore, the first member made of the sintered composite material according to the present embodiment has a sufficiently high density and can be structured to allow a coolant to pass through it, which further improves the cooling efficiency of the second member.
[0050] In addition, the first member made of the composite material sintered body according to this embodiment has sufficient strength to withstand stresses that arise during processing and joining to manufacture semiconductor manufacturing equipment components, as well as stresses that arise due to temperature differences when the completed component is used.
[0051] That is, by using the composite material sintered body according to the present embodiment as a cooling plate for an electrostatic chuck, the useful life of the semiconductor manufacturing equipment member can be improved.
[0052] <Method of manufacturing sintered composite material> Next, a method for producing a composite sintered body according to the present embodiment will be described. In the present embodiment, the raw material powders are mixed at a predetermined weight ratio, the mixed powder thus obtained is molded into a predetermined shape, and the molded body thus obtained is hot-pressed and sintered to obtain a desired composite sintered body.
[0053] The raw powder is prepared so that the total weight ratio of the following is 100wt%: 5.7wt% to 27.7wt% SiC, 12.5wt% to 55.3wt% WSi2, 17.0wt% to 55.7wt% tungsten (W) or 49.5wt% to 81.3wt% WC. The weight ratio of SiC is preferably 6.0wt% to 13.1wt%.
[0054] The particle size of the SiC raw material powder is not particularly limited, but the average particle size is preferably 2 μm to 35 μm. In addition, only coarse particles (e.g., average particle size 15 μm to 35 μm) may be used, only fine particles (e.g., average particle size 2 μm to 10 μm) may be used, or a mixture of coarse and fine particles may be used.
[0055] When using SiC powder with an average particle size smaller than 2 μm, if the SiC ratio in the mixed powder is large, the surface area of the SiC particles increases, which reduces sinterability and makes it difficult to obtain a dense sintered body. On the other hand, when using SiC powder with an average particle size larger than 35 μm, even if there is no problem with sinterability, there is a possibility that sufficient strength cannot be obtained.
[0056] The raw material powders can be mixed by dry mixing using a high-speed fluid mixer. For example, if the total weight of the raw material powders is about 300 g to 500 g, it is preferable to set the rotation speed of the stirring blades of the high-speed fluid mixer to about 1000 rpm to 1500 rpm and mix for 10 to 15 minutes.
[0057] Alternatively, wet mixing may be performed using a nylon pot and nylon balls with iron cores, with isopropyl alcohol as the solvent. In this case, the slurry obtained by mixing is dried for 16 hours at 110° C. in a nitrogen stream, for example, and then passed through a sieve to obtain a mixed powder.
[0058] The hot press sintering of the compact obtained by molding the mixed powder is carried out in an inert atmosphere, such as a vacuum atmosphere, a nitrogen gas atmosphere, or an argon gas atmosphere.
[0059] The pressure during hot pressing (pressing pressure) is 225kgf / cm 2 ~300kgf / cm 2 is preferable, and 250 kgf / cm 2 ~300kgf / cm 2 It is more preferable to set the pressure at 200 kgf / cm 2 It is not preferable to set the sintered body to less than 1%, since the sintered body will not be densified and the open porosity will exceed 1%.
[0060] The maximum temperature during hot pressing is preferably 1700°C to 1850°C, and more preferably 1770°C to 1830°C. Note that a maximum temperature of 1900°C or higher is not preferred because the material melts and a sintered body of the desired shape cannot be obtained. On the other hand, a maximum temperature of less than 1700°C is not preferred because sintering does not proceed sufficiently.
[0061] The specific pressure and temperature profile during hot pressing (hereinafter, hot pressing conditions) may be appropriately set within the above-mentioned preferred ranges depending on the composition of the powder mixture (weight ratio of each raw material powder), the particle size of the raw material powder, the size and shape of the compact, etc. Note that the smaller the weight ratio of silicon carbide in the mixed powder, the easier it is for sintering to proceed, and therefore the allowable range of hot pressing conditions under which densification can be achieved tends to be relatively wide. Also, compared with the case where only coarse particles are used for silicon carbide, the allowable range of hot pressing conditions under which densification can be achieved tends to be relatively wide when a mixture of coarse and fine particles is used.
[0062] The firing time may also be appropriately set depending on the hot press conditions and the size and shape of the molded body, etc. For example, when a disk-shaped molded body having a diameter of about 50 mm and a thickness of about 15 mm is hot press fired, it is preferable to set the holding time at the maximum temperature in the range of 4 to 8 hours.
[0063] <Method of manufacturing the bonded body> A method (joining method) for obtaining a joint body by joining a first member made of a composite material sintered body according to the present embodiment and a second member made of aluminum nitride will be described. There are two types of joining methods: metal joining, in which both members are joined via a metal joining layer, and direct joining, in which both members are directly joined.
[0064] In the case of metal bonding, a laminate obtained by laminating an aluminum foil and a dense aluminum nitride sintered body in this order on the composite material sintered body according to the present embodiment processed into a predetermined shape such as a disk shape, is placed in a graphite mold for firing, and hot press fired under an inert gas atmosphere, for example a vacuum atmosphere, a nitrogen gas atmosphere, an argon gas atmosphere, etc.
[0065] The thickness of the metal foil may be about 180 μm to 220 μm. It is preferable that the lamination surfaces of the composite sintered body, the metal foil, and the aluminum nitride have the same shape.
[0066] The hot press firing is performed at a maximum temperature of 1770℃ to 1830℃ and a pressing pressure of 250kgf / cm. 2 ~300kgf / cm 2 The temperature may be set to a value within a certain range and the holding time at the highest temperature may be set to 4 to 8 hours, thereby obtaining a bonded body (metal bonded body) that is free of peeling or voids at the interface.
[0067] In the case of direct bonding, a powder mixture having a composition ratio capable of obtaining the composite material sintered body according to the present embodiment is first uniaxially pressed under a predetermined pressure condition to obtain, for example, a disk-shaped compact. Then, a laminate obtained by laminating a dense aluminum nitride sintered body on the powder mixture is placed in a graphite mold for firing and hot-press fired under an inert gas atmosphere. Examples of the inert atmosphere include a vacuum atmosphere, a nitrogen gas atmosphere, and an argon gas atmosphere.
[0068] In such a case, it is preferable that the lamination surfaces of the compact and aluminum nitride have the same shape.
[0069] The hot press firing is performed at a maximum temperature of 1770℃ to 1830℃ and a pressing pressure of 250kgf / cm. 2 ~300kgf / cm 2 The temperature can be set to a value within a certain range and the holding time at the highest temperature can be set to 4 to 8 hours, thereby obtaining a bonded body (directly bonded body) that is free of peeling or voids at the interface. EXAMPLES
[0070] We attempted to fabricate and evaluate sintered composite bodies in 26 experimental examples with different combinations of raw powder compositions and hot pressing conditions. In the following, powder mixtures, compacts, and sintered bodies from the same experimental example may be referred to as samples without distinguishing between their states.
[0071] <Raw material powder> The raw material powders prepared were SiC, WSi2, W, and WC.
[0072] Three commercially available SiC powders with different particle sizes were prepared as raw powders. Specifically, three powders with average particle sizes of 36 μm (hereinafter referred to as #500), 15 μm (hereinafter referred to as #1000), and 3 μm (hereinafter referred to as #6000) were prepared. The purity of each was 99% or higher.
[0073] The raw powder for WSi2 was a commercially available product with a purity of 99% or more and an average particle size of 6 μm. The raw powder for WC was a commercially available product with a purity of 99% or more and an average particle size of 2 μm. The raw powder for W was a commercially available product with a purity of 99% or more and an average particle size of 2.3 μm.
[0074] <Preparation of sintered body> The raw material compositions and hot pressing conditions for all experimental examples are listed in Table 1. Table 1 also shows whether the samples melted when hot pressing was performed.
[0075] [Table 1]
[0076] In each experimental example, in preparing the composite sintered body, a total of 300 g of SiC raw material powder, WSi2 raw material powder, and WC raw material powder or W raw material powder were weighed out so as to have the composition ratio (weight ratio) shown in Table 1. The weighed three types of powder were put into a high-speed fluid mixer with a powder input capacity of 1.8 L, and stirred and mixed at 1500 rpm for 10 minutes to obtain a powder mixture.
[0077] The powder mixtures obtained for each experimental example were subjected to a pressure of 200 kgf / cm 2 The mixture was uniaxially pressed at a pressure of 1000 MPa to produce a disk-shaped compact with a diameter of 50 mm and a thickness of about 15 mm. The produced compact was placed in a graphite mold for firing.
[0078] The compact was then hot-pressed and sintered to obtain a composite sintered body. In the hot-press sintering, the maximum temperature was varied to seven levels: 1650°C, 1700°C, 1770°C, 1800°C, 1830°C, 1850°C, and 1900°C. The holding time at the maximum temperature was four hours. The pressure was 200 kgf / cm. 2 , 225kgf / cm 2 , 250kgf / cm 2 , and 300 kgf / cm 2 The pressure was applied at four different levels. The pressure was started when the firing temperature reached 900°C. Figure 3 shows the results of the hot press firing with the maximum temperature set to 1800°C and the pressure set to 250 kgf / cm. 2 4 is an example of a temperature and pressure profile when
[0079] <Composition and properties of sintered composite materials> For the composite sintered bodies of each experimental example, the constituent phases were identified and their composition ratios (contents) were calculated (simple quantification).In addition, the open porosity, bulk density, bending strength, and thermal expansion coefficient were measured to evaluate the properties.
[0080] Table 2 shows the composition ratio of the constituent phases and the measurement results of the open porosity, bulk density, bending strength, thermal expansion coefficient, fracture toughness value, Young's modulus, and thermal conductivity for the sintered bodies of each experimental example.
[0081] [Table 2]
[0082] As shown in Table 2, Experimental Examples 1, 3 to 8, 10 to 12, 14 to 15, 17 to 19, and 21 to 25 correspond to embodiments, and the other experiments correspond to comparative examples.
[0083] The composite sintered bodies corresponding to the examples were also measured for fracture toughness (K1c value), Young's modulus, and thermal conductivity, with some exceptions. The results of these measurements are also shown in Table 2.
[0084] On the other hand, in the case of Experimental Example 16 and Experimental Example 20, in which the maximum temperature in the hot-press sintering was set to 1900°C, the samples melted during the sintering as shown in Table 1, and a sintered body of the desired shape was not obtained, so it was not possible to identify the constituent phases or measure any of the above-mentioned characteristics.
[0085] (Identification and simple quantification of constituent phases) Except for Experimental Examples 16 and 20, the composite sintered body obtained by the above procedure was ground in a mortar and subjected to X-ray diffraction measurement (θ-2θ measurement) using a sealed tube type X-ray diffractometer (D8 ADVANCE manufactured by Bruker AXS). The constituent phases (crystal phases) of the composite sintered body were identified based on the peak patterns that appeared in the obtained X-ray diffraction profile. CuKα rays were used as characteristic X-rays, the tube output was 40 kV, 40 mA, and the measurement range was 2θ = 5° to 70°.
[0086] In addition, the composition ratio (content) of the crystalline phase contained in the sintered composite material was determined by simple quantification based on the intensity of the peaks that appeared in the X-ray diffraction profile. For simple quantification, the simple profile fitting function (FPM Eval.) of the powder diffraction data analysis software "EVA" from Bruker AXS was used. This function calculates the weight ratio of the constituent phases using the I / Icor (intensity ratio to the diffraction intensity of corundum) on the ICDD PDF card of the identified crystalline phase.
[0087] (Measurement of open porosity and bulk density) The measurement was performed by the Archimedes method using pure water as a medium.
[0088] (4-point bending strength measurement) Measurements were performed in accordance with JIS-R1601.
[0089] (Measurement of thermal expansion coefficient) The average linear thermal expansion coefficient at 40°C to 550°C was calculated using a TD5020S (horizontal differential expansion measurement method) manufactured by Bruker AXS Co., Ltd.
[0090] Specifically, the temperature was raised twice to 650°C at a heating rate of 20°C / min in an argon atmosphere, and the average linear thermal expansion coefficient was calculated from the data from the second measurement. The standard sample was an alumina standard sample (purity 99.7%, bulk density 3.9 g / cm) provided with the device. 3 , length 20 mm) was used.
[0091] (Measurement of fracture toughness value) The fracture toughness was evaluated by the SEPB method according to JIS-R1607.
[0092] (Young's modulus measurement) The Young's modulus was measured in accordance with JIS R1602 (Testing method for elastic modulus of fine ceramics).
[0093] (Measurement of thermal conductivity) The measurement was performed by the laser flash method.
[0094] <Details of each experiment> (Experimental Examples 1 to 5) In Experimental Examples 1 to 5, composite sintered bodies were produced using powders of SiC, WSi2, and W. #500 and #6000 SiC powders were used.
[0095] As shown in Table 1, the raw material composition is common to Experimental Example 1 and Experimental Example 2. SiC (#500 products): 18.0wt%; SiC (#6000 products): 9.7wt%; WSi2: 55.3wt%; W: 17.0wt%; It was decided.
[0096] In common with Experimental Examples 3 to 5, SiC (#500 products): 15.8wt%; SiC (#6000 products): 8.5wt%; WSi2: 20.0wt%; W: 55.7wt%; It was decided.
[0097] That is, in Experimental Examples 3 to 5, compared with Experimental Examples 1 and 2, the ratio of W was significantly increased, the ratio of WSi2 was significantly decreased, and the ratio of SiC was also slightly decreased.
[0098] The hot pressing conditions were a maximum temperature of 1700° C. for Experimental Examples 2 and 4, and a maximum temperature of 1800° C. for Experimental Examples 1, 3, and 5. The pressing pressure was 250 kgf / cm 2 It was decided.
[0099] In all of Experimental Examples 1 to 5, sintered bodies were obtained, and only SiC, WSi2, W5Si3, and WC were identified as constituent phases. The SiC content in the sintered bodies was 48.6 wt% or less.
[0100] However, while the open porosity was 1% or less in the sintered bodies of Experimental Examples 1 and 3 to 5, the open porosity was significantly greater than 1% in the sintered body of Experimental Example 2. That is, while dense composite sintered bodies were obtained in Experimental Examples 1 and 3 to 5, a dense composite sintered body was not obtained in Experimental Example 2.
[0101] More specifically, in Experimental Examples 1, 3, and 5, in which the maximum temperature during hot-press sintering was 1800°C, the open porosity was 1% or less, whereas in Experimental Examples 2 and 4, in which the maximum temperature during hot-press sintering was 1700°C, only the latter had an open porosity of 1% or less. Since the only difference between Experimental Examples 2 and 4 is the raw material composition, when W is used as a raw material, it can be said that at least the maximum temperature during hot-press sintering needs to be set according to the raw material composition.
[0102] Except for Experimental Example 2, the thermal expansion coefficient was in the range of 4.6 ppm / K to 5.6 ppm / K. On the other hand, the bending strength exceeded 200 MPa in all of the Experimental Examples, but was below 350 MPa. In Experimental Examples 1, 4, and 5, the fracture toughness value (K1c) was 6.0 MPa m 1 / 2 ~6.5MPa m 1 / 2 The Young's modulus was 448 GPa to 484 GPa, and the thermal conductivity was 100 W / m K or more.
[0103] The results of Experimental Examples 1 to 5 show that when the weight ratio of SiC in the raw material powder is within the range of 5.7 wt% to 27.7 wt%, the weight ratio of WSi2 is within the range of 12.5 wt% to 55.3 wt%, and the weight ratio of W is within the range of 17.0 wt% to 55.7 wt%, by appropriately setting the hot pressing conditions according to the raw material composition, a composite material sintered body can be obtained that contains 14.4 wt% to 48.6 wt% silicon carbide, is dense with an open porosity of 1% or less, and has a thermal expansion coefficient close to that of aluminum nitride.
[0104] (Experimental Examples 6 to 14) In Experimental Examples 6 to 14, composite sintered bodies were produced using powders of SiC, WSi2, and WC as raw materials. Only #1000 SiC powder was used.
[0105] The raw material composition is common to Experimental Examples 6 to 9 as shown in Table 1. SiC (#1000 products): 13.1wt%; WSi2: 22.2wt%; WC: 64.7wt%; It was decided.
[0106] In Experimental Example 10, SiC (#1000 products): 11.4wt%; WSi2: 39.1wt%; WC: 49.5wt%; It was decided.
[0107] In Experimental Examples 11 to 13, SiC (#1000 products): 9.1wt%; WSi2: 31.5wt%; WC: 59.4wt%; It was decided.
[0108] In Experimental Example 14, SiC (#1000 products): 8.5wt%; WSi2: 19.6wt%; WC: 71.9wt%; It was decided.
[0109] That is, Experimental Examples 6 to 9, Experimental Example 10, Experimental Examples 11 to 13, and Experimental Example 14 have a relationship in which the weight ratios of SiC and WSi2 in the raw materials decrease and the weight ratio of WC increases in this order.
[0110] On the other hand, the hot pressing conditions were a maximum temperature of 1770°C for Experimental Example 7, a maximum temperature of 1830°C for Experimental Example 8, and a maximum temperature of 1800°C for all other examples. The pressing pressure was 200 kgf / cm in Experimental Examples 9 and 13. 2 The rest are 250kgf / cm 2 It was decided.
[0111] That is, only the maximum temperature during hot-press sintering is different between Experimental Examples 6 to 8. Also, only the pressure during hot-press sintering is different between Experimental Examples 6 and 9. Similarly, only the pressure during hot-press sintering is different between Experimental Examples 11 and 13 and between Experimental Examples 12 and 13.
[0112] On the other hand, the hot pressing conditions of Experimental Example 6, Experimental Example 10, Experimental Example 11, Experimental Example 12, and Experimental Example 14 are the same, and only the raw material composition is different.
[0113] Experimental Examples 11 and 12 have the same raw material composition and hot pressing conditions.
[0114] In all of Experimental Examples 6 to 14, sintered bodies were obtained, and only SiC, WSi2, W5Si3, and WC were identified as constituent phases. The SiC content in the sintered bodies was within the range of 14.4 wt% to 48.6 wt% in all of the Experimental Examples.
[0115] In addition, the pressing pressure during hot press firing was set at 200 kgf / cm 2 In Experimental Examples 9 and 13, where the pressing pressure was 250 kgf / cm, the open porosity was much higher than 1%. In other words, a dense composite sintered body was not obtained. 2 In Experimental Examples 6 to 8, 10 to 12, and 14, in which the open porosity was set at 0.1% or less, an extremely excellent dense sintered composite material was obtained.
[0116] In addition, in Experimental Examples 6 to 8, 10 to 12, and 14, in which dense composite sintered bodies were obtained, the content of tungsten silicide (WSi2 and W5Si3) was greater than the content of silicon carbide (SiC), except for Experimental Example 7.
[0117] The thermal expansion coefficient in all experimental examples was within the range of 4.9 ppm / K to 5.3 ppm / K, which is within the range of 4.6 ppm / K to 5.6 ppm / K. In other words, the difference with the thermal expansion coefficient of aluminum nitride was 0.2 ppm / K or less.
[0118] In addition, the sintered composite bodies of Experimental Examples 6 to 8, 10 to 12, and 14, which have an open porosity of 0.1% or less and are judged to have extremely excellent denseness, achieved bending strengths of over 350 MPa. Furthermore, in these sintered composite bodies, the fracture toughness value (K1c) was 6.3 MPa m 1 / 2 ~7.9MPa m 1 / 2 The Young's modulus was 448 GPa to 520 GPa, except for Experimental Example 12, which was not measured. The thermal conductivity was 98 W / m K in Experimental Example 11, and was 100 W / m K or higher in all other cases.
[0119] (Experimental Examples 15 to 21) In Experimental Examples 15 to 21, composite sintered bodies were produced using SiC, WSi2, and WC powders as raw materials. As the SiC powder, #500 and #6000 were used in Experimental Examples 15 to 17, and only #1000 was used in Experimental Examples 18 to 21.
[0120] The raw material composition was the same in Experimental Examples 15 to 17 as shown in Table 1. SiC (#500 products): 5.0wt%; SiC (#6000 products): 1.2wt%; WSi2: 12.5wt%; WC: 81.3wt%; It was decided.
[0121] In addition, in common to Experimental Examples 18 to 21, SiC (#1000 products): 6.2wt%; WSi2: 12.5wt%; WC: 81.3wt%; It was decided.
[0122] That is, in Experimental Examples 15 to 21, the weight ratios of SiC and WSi2 were smaller, and the weight ratio of WC was larger than those in Experimental Examples 6 to 14. Also, in Experimental Examples 15 to 17 and Experimental Examples 18 to 21, the overall weight ratio of SiC was the same, but the particle size of the powder used was different.
[0123] On the other hand, the hot pressing conditions were as follows: the maximum temperature was 1800°C for Experimental Examples 15 and 18, 1900°C for Experimental Examples 16 and 20, and 1830°C for Experimental Examples 17, 19, and 21. The pressing pressure was 250 kgf / cm 2 It was decided.
[0124] As a result, in Experimental Examples 16 and 20 in which the maximum temperature during hot-press sintering was set to 1900° C. as described above, the samples melted during sintering, and no sintered bodies were obtained.
[0125] In Experimental Example 15, Experimental Example 17 to Experimental Example 19, and Experimental Example 21, in which the maximum temperature during hot press sintering was 1800°C or 1830°C, sintered bodies were obtained, and only SiC, WSi2, W5Si3, and WC were identified as constituent phases. In addition, the SiC content in the sintered bodies was within the range of 14.4wt% or more and 48.6wt% or less in all of these Experimental Examples.
[0126] Furthermore, the open porosity of the sintered body was 0.1% or less in all of Experimental Examples 15, 17 to 19, and 21. That is, an extremely excellent dense sintered composite material body was obtained.
[0127] Moreover, the thermal expansion coefficients of these sintered bodies were all values of 4.8 ppm / K to 4.9 ppm / K, which fell within the range of 4.6 ppm / K to 5.6 ppm / K. In other words, the values obtained were slightly smaller than the thermal expansion coefficient of aluminum nitride.
[0128] In addition, in Experimental Example 15, Experimental Example 17 to Experimental Example 19, and Experimental Example 21 in which dense composite sintered bodies were obtained, the content of tungsten silicide (WSi2 and W5Si3) was greater than the content of silicon carbide (SiC).
[0129] In addition, the sintered composite materials of Experimental Examples 15, 17 to 19, and 21, which are judged to have an extremely excellent dense quality, had bending strengths exceeding 350 MPa. Furthermore, in these sintered composite materials, the fracture toughness value (K1c) was 7.5 MPa m 1 / 2 ~8.5MPa m 1 / 2 and the Young's modulus was 523 GPa to 561 GPa. All of these values were generally higher than those of Experimental Examples 6 to 14. In addition, the thermal conductivity was 134 W / m·K or higher, which was also higher than those of Experimental Examples 6 to 14.
[0130] (Experimental Examples 22 to 23) In Experimental Examples 22 and 23, composite sintered bodies were produced using powders of SiC, WSi2, and WC as raw materials. Only #1000 SiC powder was used.
[0131] As shown in Table 1, the raw material composition in Experimental Example 22 was as follows: SiC (#1000 products): 12.8wt%; WSi2: 13.5wt%; WC: 73.7wt%; It was decided.
[0132] In addition, in Experimental Example 23, SiC (#1000 products): 5.7wt%; WSi2: 26.7wt%; WC: 67.6wt%; It was decided.
[0133] The hot pressing conditions were the same: maximum temperature 1800°C, pressing pressure 250kgf / cm 2 It was decided.
[0134] In other words, Experimental Example 22 and Experimental Example 23 are different from Experimental Examples 6, 10, 11, 12, 14, and 18, which have common hot pressing conditions, in that the weight ratio combinations of the raw materials SiC powder (#1000 product), WSi2 powder, and WC powder are different.
[0135] In all the experimental examples, sintered bodies were obtained, and the only constituent phases identified were SiC, WSi2, W5Si3, and WC. The SiC content in the sintered bodies was in the range of 14.4wt% to 48.6wt% in all the experimental examples.
[0136] However, in Example 23, the content of tungsten silicide (WSi2 and W5Si3) was greater than the content of silicon carbide (SiC), while in Example 22, the opposite was true.
[0137] The open porosity of the sintered body was 0.1% or less in both Experimental Example 22 and Experimental Example 23. That is, in all Experimental Examples, an extremely excellent dense sintered composite material body was obtained.
[0138] On the other hand, the thermal expansion coefficient of the sintered body was in the range of 4.6 ppm / K to 5.6 ppm / K in all the experimental examples, but was at the lower limit of the range, 4.6 ppm / K, in experimental example 22. And at the upper limit of the range, 5.6 ppm / K, in experimental example 23.
[0139] The bending strength was 423 MPa in Experimental Example 22 and 424 MPa in Experimental Example 23. That is, the bending strength exceeded 350 MPa in both Experimental Examples, but there was almost no difference between the two.
[0140] On the other hand, the fracture toughness (K1c), Young's modulus, and thermal conductivity of Example 23 were 8.2 MPa m 1 / 2 , 548GPa, and 134W / m K, while in Example 22, the values were 6.0MPa m 1 / 2 , 332 GPa, and 104 W / m K.
[0141] In comparison with other experimental examples, the tungsten silicide (WSi2 and W5Si3) content of 12.7 wt%, which is less than the silicon carbide (SiC) content of 28.1 wt%, may have affected the properties of the sintered body in experimental example 22. Also, in experimental example 23, the weight ratio of SiC in the raw material powder was as low as 5.7 wt%, which may have affected the properties of the sintered body.
[0142] (Experimental Examples 24 to 26) In Experimental Examples 24 to 26, composite sintered bodies were produced using powders of SiC, WSi2, and W. #500 and #6000 SiC powders were used.
[0143] The raw material composition was the same as in Experimental Example 1 and Experimental Example 2, as shown in Table 1. SiC (#500 products): 18.0wt%; SiC (#6000 products): 9.7wt%; WSi2: 55.3wt%; W: 17.0wt%; It was decided.
[0144] As for the hot pressing conditions, the combination of maximum temperature and pressing pressure in each of Experimental Examples 24 to 26 was different from that in Experimental Examples 1 to 5. In Experimental Example 24, the maximum temperature was 1850°C, and the pressing pressure was 225 kgf / cm 2 In Experimental Example 25, the maximum temperature was 1700°C and the pressing pressure was 300 kgf / cm 2 In Experimental Example 26, the maximum temperature was 1650°C and the pressing pressure was 300 kgf / cm 2 It was decided.
[0145] That is, in Experimental Example 24, the maximum temperature is higher than that in Experimental Example 1, but the pressing pressure is lower. Also, in Experimental Example 25, the pressing pressure is higher than that in Comparative Example Experimental Example 2. Furthermore, in Experimental Example 26, the maximum temperature is lower than that in Comparative Example Experimental Example 2, but the pressing pressure is higher.
[0146] In each of Experimental Examples 24 to 26, sintered bodies were obtained, and only SiC, WSi2, W5Si3, and WC were identified as constituent phases. However, the content of SiC in the sintered body was 48.6 wt% or less in Experimental Examples 24 and 25, but it was 50.1 wt% in Experimental Example 26, exceeding 48.6 wt%.
[0147] The open porosity of the sintered body was below 1% in Experimental Examples 24 and 25, but exceeded 1% in Experimental Example 26.
[0148] The thermal expansion coefficient was 5.4 ppm / K, which was within the range of 4.6 ppm / K to 5.6 ppm / K, in all of Experimental Examples 24 to 26. On the other hand, the bending strength was 252 MPa in Experimental Examples 24 and 25, which was similar to Experimental Examples 1 and 2, but remained at 116 MPa in Experimental Example 26. The fracture toughness value (K1c) and Young's modulus in Experimental Examples 24 and 25 were similar to Experimental Example 1, but the thermal conductivity was slightly higher than that of Experimental Example 1.
[0149] (Summary of Experimental Examples 1 to 26) The results of Experimental Examples 1 to 26 show that when the weight ratio of SiC in the raw material powder is within the range of 5.7 wt% to 27.7 wt%, the weight ratio of WSi2 is within the range of 12.5 wt% to 55.3 wt%, and the weight ratio of WC is within the range of 49.5 wt% to 81.3 wt% or the weight ratio of W is within the range of 17.0 wt% to 55.7 wt%, by appropriately setting the hot pressing conditions, a composite material sintered body can be obtained that contains 14.4 wt% to 48.6 wt% silicon carbide, is dense with an open porosity of 1% or less, and has a thermal expansion coefficient close to that of aluminum nitride.
[0150] In addition, the dense composite sintered body has a four-point bending strength of 200 MPa or more and a compressive strength of 6.0 MPa m 1 / 2 ~8.8MPa m 1 / 2 It has also been shown that the alloy satisfies a fracture toughness value within a range of 273 GPa to 594 GPa, a Young's modulus within a range of 273 GPa to 594 GPa, and a thermal conductivity of 90 W / m·K or more.
[0151] In particular, the results of Experimental Examples 6 to 23 show that when the weight ratio of SiC in the raw material powder is within the range of 5.7 wt% to 13.1 wt%, the weight ratio of WSi2 is within the range of 12.5 wt% to 39.1 wt%, and the weight ratio of WC is within the range of 49.5 wt% to 81.3 wt%, an extremely excellent dense composite sintered body with an open porosity of 0.1% or less can be obtained, and further, the composite sintered body has an excellent four-point bending strength of 350 MPa or more.
Claims
1. It is composed of silicon carbide, tungsten silicide, and tungsten carbide, Contains 14.4 wt % or more and 48.6 wt % or less of silicon carbide, The open porosity is 1% or less. A sintered composite material comprising:
2. 2. The composite material sintered body according to claim 1, The difference between the thermal expansion coefficient at 40°C to 550°C and the thermal expansion coefficient of aluminum nitride at 40°C to 550°C is 0.5 ppm / K or less. A sintered composite material comprising:
3. The composite material sintered body according to claim 2, The open porosity is 0.1% or less. A sintered composite material comprising:
4. The composite material sintered body according to any one of claims 1 to 3, a surface of each crystal particle of silicon carbide is covered with at least one of tungsten silicide and tungsten carbide, so that at least one of crystal particles of tungsten silicide and tungsten carbide is present in gaps between the silicon carbide crystal particles; A sintered composite material comprising:
5. The composite material sintered body according to any one of claims 1 to 3, The content of tungsten silicide is greater than the content of silicon carbide. A sintered composite material comprising:
6. The composite material sintered body according to any one of claims 1 to 3, The four-point bending strength is 200 MPa or more. A sintered composite material comprising:
7. 7. The composite material sintered body according to claim 6, The four-point bending strength is 350 MPa or more. A sintered composite material comprising:
8. The composite material sintered body according to any one of claims 1 to 3, The thermal conductivity is 90 W / m·K or more. A sintered composite material comprising:
9. The composite material sintered body according to any one of claims 1 to 3, Fracture toughness value is 6.0 MPa m 1/2 ~8.8MPa m 1/2 That is, A sintered composite material comprising:
10. The composite material sintered body according to any one of claims 1 to 3, Young's modulus is 273 GPa to 594 GPa; A sintered composite material comprising:
11. The composite material sintered body according to claim 10, Young's modulus is 460 GPa to 594 GPa; A sintered composite material comprising:
12. A joined body formed by joining a first member and a second member, The first member is It is composed of silicon carbide, tungsten silicide, and tungsten carbide, Contains 14.4 wt % or more and 48.6 wt % or less of silicon carbide, The open porosity is 1% or less. It is made of a sintered composite material, The second member is made of aluminum nitride. A conjugate characterized in that
13. The joint body according to claim 12, The difference between the thermal expansion coefficient of the first member at 40°C to 550°C and the thermal expansion coefficient of the second member at 40°C to 550°C is 0.5 ppm / K or less. A conjugate characterized in that
14. The joint according to claim 13, The open porosity of the first member is 0.1% or less. A conjugate characterized in that
15. The bonded body according to any one of claims 12 to 14, The first member and the second member are metal-jointed. A conjugate characterized in that
16. A semiconductor manufacturing equipment member including a bonded body formed by bonding a first member and a second member, The first member is a cooling member for cooling the second member, It is composed of silicon carbide, tungsten silicide, and tungsten carbide, Contains 14.4 wt % or more and 48.6 wt % or less of silicon carbide, The open porosity is 1% or less. It is made of a sintered composite material, The second member is made of aluminum nitride. A semiconductor manufacturing equipment member characterized in that:
17. The semiconductor manufacturing equipment member according to claim 16, The difference between the thermal expansion coefficient of the first member at 40°C to 550°C and the thermal expansion coefficient of the second member at 40°C to 550°C is 0.5 ppm / K or less. A semiconductor manufacturing equipment member characterized in that:
18. 18. The semiconductor manufacturing equipment member according to claim 17, The open porosity of the first member is 0.1% or less. A semiconductor manufacturing equipment member characterized in that:
19. A semiconductor manufacturing equipment member according to any one of claims 16 to 18, The first member and the second member are metal-jointed. A semiconductor manufacturing equipment member characterized in that:
20. A method for producing a composite material sintered body, comprising the steps of: SiC powder and WSi 2 a mixing step of mixing the powder with WC powder or W powder to obtain a powder mixture; a molding step of molding the powder mixture into a predetermined shape to obtain a molded body; A sintering step of hot-pressing the molded body under an inert atmosphere; Equipped with In the mixing step, 5.7 wt% to 27.7 wt% of SiC powder and 12.5 wt% to 55.3 wt% of WSi 2 The powder is mixed with 49.5 wt % to 81.3 wt % of WC powder or 17.0 wt % to 55.7 wt % of W powder so that the total weight ratio is 100 wt %; In the firing process, the maximum temperature is 1700°C to 1850°C, and the pressing pressure is 225 kgf / cm 2 ~300kgf / cm 2 Let us say, 4. A method for producing a sintered composite material comprising the steps of:
21. A method for producing a composite material sintered body according to claim 20, comprising the steps of: In the mixing step, 5.7 wt% to 13.1 wt% of SiC powder and 12.5 wt% to 39.1 wt% of WSi 2 The powder is mixed with 49.5 wt % to 81.3 wt % of WC powder so that the total weight ratio is 100 wt %.
4. A method for producing a sintered composite material comprising the steps of:
Citation Information
Patent Citations
Silicon carbide base sintered body and manufacture
JP1986227965A
Composite material and its manufacturing method, and wafer holding member
JP2005154832A
WC-SiC-BASED COMPOSITE WITH HIGH HARDNESS, HIGH YOUNG'S MODULUS AND HIGH FRACTURE TOUGHNESS VALUE, AND ITS MANUFACTURING METHOD
JP2006089351A
Substrate loading table
JP2008103713A
WC-SiC-Mo2C-BASED SINTERED BODY AND ITS MANUFACTURING METHOD
JP2009209022A