High-chromium cast iron

High chromium cast iron with a controlled microstructure and composition addresses the wear resistance issue by reducing wear rates and maintaining hardness, enhancing durability in demanding applications.

JP2024145542APending Publication Date: 2024-10-15FURUKAWA COMPANY

Patent Information

Application Number
JP2023057939
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing high chromium cast iron materials do not provide sufficient wear resistance for applications requiring stringent durability, particularly in equipment and machinery that come into contact with raw materials, leading to rapid wear and failure.

Method used

The development of high chromium cast iron with a specific composition and microstructure, including a carbide phase with an average diameter of 30 μm or less, a primary crystal structure area ratio of 30% or more, and a eutectic structure surrounding the primary crystal structure, achieved through controlled casting and quenching processes.

Benefits of technology

The improved microstructure enhances wear resistance, reducing wear rates to 3.5% or less and maintaining a Rockwell hardness of 55 or more, thereby extending the lifespan of components in harsh operating conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145542000001_ABST
    Figure 2024145542000001_ABST
Patent Text Reader

Abstract

To provide high-chromium cast iron with improved abrasion resistance.SOLUTION: High-chromium cast iron comprises C, Cr, and Fe, wherein a content of C is 4.0 mass% or more and 7.0 mass% or less, a content of Cr is 15.0 mass% or more and 40.0 mass% or less, and a content of Fe is 48.0 mass% or more and 81.0 mass% or less. The high-chromium cast iron comprises a eutectic structure and a primary crystal structure containing a carbide phase, wherein an average diameter of the primary crystal structure is 30 μm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to high chromium cast iron. [Background technology]

[0002] High chromium cast iron is a material whose main constituent elements are iron (Fe), carbon (C), and chromium (Cr), and which consists of high-hardness carbides surrounded by a matrix structure, and which has excellent wear resistance. Examples of techniques relating to such high chromium cast iron include those described in the following Patent Documents 1 to 5.

[0003] Patent Document 1 (JP Patent Publication 2001-49381A) describes a wear-resistant alloy cast iron material that is made of high Cr cast iron containing 3.8-4.5% C, 1.0% or less Si, 1.5% or less Mn, 10.0-20.0% Cr, 3.0-4.5% Mo, 3.0-4.0% W, 3.0-5.0% Nb (all by weight %) and unavoidable impurities, with the balance being essentially Fe, and that is heated and held at an optimum heat treatment temperature, and then quenched to have a high hardness of at least Rockwell hardness C (HRC) 69 or at least Shore hardness (Hs) 100, and that is always within the hypoeutectic range on the low C side of the Fe-Cr-C carbide eutectic line in the relationship between C weight % and Cr weight %, corrected by the carbide forming action of W and Nb. Patent Document 1 also describes that the wear-resistant alloy cast iron material has the effect of providing an ideal wear-resistant member that has the effect of forming extremely hard W and Nb carbides while maintaining substantially the same toughness as the hypoeutectic range in which toughness is not lost, while falling within the hypereutectic range that is well-known for improving inherent wear resistance, and that has the effect of providing an ideal wear-resistant member in which fine Cr carbides are dispersed and precipitated, while simultaneously achieving the effect of forming extremely hard W and Nb carbides while maintaining the matrix strength in the relatively stable hypoeutectic range.

[0004] Patent Document 2 (JP 2003-286537 A) describes that a large high chromium cast iron casting characterized by having 2.4 to 3.5 wt% C, 0.5 to 1.5 wt% Si, 0.5 to 2.5 wt% Mn, 14 to 21 wt% Cr, 2 to 4 wt% Mo, 0.5 to 2.5 wt% Ni, with the balance being Fe and unavoidable impurities, and having a hardness of 62 to 67 HRC and a residual stress of -200 to 200 MPa, can extend the service life and prevent breakage during use.

[0005] Patent Document 3 (JP 2008-75108 A) describes that a casting for a wear-resistant part, which has a composition, by mass%, of 1.6-3% C, 0.3-2% Si, 0.3-2% Mn, 6-15% Cr, 2-8% Mo, 4-8% V, 0.5-4.0% Nb, with the balance being Fe and unavoidable impurities, and which has been quenched and tempered, has significantly superior wear resistance compared to conventional high chromium cast iron and high manganese cast steel, and further has higher strength and superior toughness compared to high chromium cast iron, and is suitable for use in a wear-resistant part, and can be produced easily and at low cost, providing significant industrial benefits.

[0006] Patent Document 4 (JP 2012-219346 A) describes that high chromium cast iron with a manganese content of 2.15% by weight to 3.5% by weight can improve wear resistance.

[0007] Patent Document 5 (JP 2013-237904 A) describes a high chromium wear-resistant cast iron that is characterized by containing, by mass%, 3.0-3.4% C, 0.3-1.0% Si, 0.5-1.2% Mn, 16-20% Cr, 0.3-1.0% Mo, 5×Mo%≧Ni%≧2×Mo%, and the remainder being Fe and unavoidable impurities, and has a product thickness of 1-6 inches, which saves Mo resources and reduces costs, and also makes it possible to harden the cast product to a uniform hardness all the way to its inside, thereby improving the durability of the cast product. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2001-49381 A [Patent Document 2] JP 2003-286537 A [Patent Document 3] JP 2008-75108 A [Patent Document 4] JP 2012-219346 A [Patent Document 5] JP 2013-237904 A Summary of the Invention [Problem to be solved by the invention]

[0009] The present invention provides a high chromium cast iron with improved wear resistance. [Means for solving the problem]

[0010] The present inventors conducted extensive research to achieve the above object, and as a result, found that the wear resistance of high chromium cast iron can be improved by providing a high chromium cast iron containing C, Cr, and Fe in a specific ratio, and having a primary crystal structure containing a carbide phase with an average diameter in a specific range, thereby completing the present invention.

[0011] According to the present invention, there is provided a high chromium cast iron as follows:

[0012] [1] A high chromium cast iron containing C, Cr and Fe, The C content is 4.0% by mass or more and 7.0% by mass or less, The Cr content is 15.0 mass% or more and 40.0 mass% or less, The Fe content is 48.0% by mass or more and 81.0% by mass or less, The steel sheet includes a eutectic structure and a primary crystal structure including a carbide phase, High chromium cast iron, wherein the primary crystal structure has an average diameter of 30 μm or less, according to the following method 1: (Method 1) The high chromium cast iron is polished to prepare a test piece for microstructural observation, and then the polished surface of the test piece for microstructural observation is observed by a scanning electron microscope (SEM). The obtained SEM photograph is then analyzed by image processing software to determine the average diameter of the primary crystal structure. [2] The high chromium cast iron according to [1], wherein the eutectic structure surrounds the primary crystal structure. [3] The high chromium cast iron according to the above [1] or [2], wherein the area ratio X1 of the primary crystal structure is 30% or more, according to the following method 2. (Method 2) The high chromium cast iron is polished to prepare a test piece for microstructural observation, and then the polished surface of the test piece for microstructural observation is observed by an electron microscope (SEM). The SEM photograph obtained is then analyzed by image processing software to determine the area ratio X1 of the primary crystal structure. [4] The high chromium cast iron according to any one of the above [1] to [3], wherein the C content is 4.1 mass% or more and 5.5 mass% or less, and the Cr content is 20.0 mass% or more and 35.0 mass% or less. [5] The high chromium cast iron according to any one of the above [1] to [4], wherein the C content is 4.2 mass% or more and 5.0 mass% or less, and the Cr content is 23.0 mass% or more and 32.0 mass% or less. [6] The high chromium cast iron according to any one of the above [1] to [5], wherein the C content is 4.3 mass% or more and 4.8 mass% or less, and the Cr content is 25.0 mass% or more and 30.0 mass% or less. [7] The high chromium cast iron according to any one of [1] to [6] above, wherein the Fe content is 55.0% by mass or more and 76.0% by mass or less. [8] The high chromium cast iron according to any one of [1] to [7] above, further containing one or two elements selected from the group consisting of Si and Mn. [9] The high chromium cast iron according to [8], wherein the Si content is more than 0% by mass and not more than 2.0% by mass.

[10] The high chromium cast iron according to [8] or [9], wherein the Mn content is more than 0 mass% and not more than 5.0 mass%.

[11] The high chromium cast iron according to any one of the above [1] to

[10] , further containing one or more elements selected from the group consisting of Mo, W, Nb, V, Co, Ni, Cu, Ti, B and rare earth elements.

[12] The high chromium cast iron according to any one of the above [1] to

[11] , having a Rockwell hardness HRC of 55 or more.

[13] The high chromium cast iron according to any one of the above [1] to

[12] , which has an abrasion rate of 3.5 mass % or less according to the following method 3. (Method 3) A test piece of 40 mm length x 22 mm width x 6 mm height (with Φ8 mm bolt hole) made of the high chromium cast iron is prepared. Next, a mixture of SiO2 and water with a mass ratio of SiO2 to water of 1:2 is made into a slurry, the test piece is set in the slurry, the temperature of the slurry is set to 20°C, the test piece is rotated at a speed of 2000 rpm, and a wear test is performed at a peripheral speed of 10.5 m / s. Next, the slurry is replaced every hour during the test, and the wear rate is calculated by dividing the change in mass from the initial mass of the test piece after 12 hours by the initial mass of the test piece.

[14] Impact value according to method 4 below is 1.0 J / cm 2 The high chromium cast iron according to any one of the above [1] to

[13] . (Method 4) A test piece with a notch of 50 mm length × 10 mm width × 10 mm height (notch shape: U notch, notch size: depth 2 mm, tip R1.0 mm, notch position: center in the vertical direction) made of the high chromium cast iron is prepared. Next, an impact test is carried out at 20°C, and in accordance with JIS Z2242:2018, an impact load is applied to the test piece with a pendulum hammer, and the energy E (J) at the time of destruction is calculated as the impact value C (=E / A: A is the cross-sectional area (cm) of the notch part of the test piece).2 )) is required. Effect of the Invention

[0013] According to the present invention, it is possible to provide a high chromium cast iron having improved wear resistance. [Brief description of the drawings]

[0014] [Figure 1] FIG. 2 is a diagram for explaining the diameter of a primary crystal structure. [Diagram 2] FIG. 2 is a diagram showing the structure of the high chromium cast iron obtained in Examples 1 to 3. [Diagram 3] FIG. 2 is a diagram showing the structure of the high chromium cast iron obtained in Comparative Examples 1 to 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, an embodiment of the present invention will be described. Unless otherwise specified, the symbol "to" indicating a range of values ​​means "greater than or equal to" to "less than or equal to".

[0016] [High chromium cast iron] The high chromium cast iron of the present invention contains C, Cr and Fe, the C content is 4.0 mass% or more and 7.0 mass% or less, the Cr content is 15.0 mass% or more and 40.0 mass% or less, and the Fe content is 48.0 mass% or more and 81.0 mass% or less, and contains a eutectic structure and a primary crystal structure containing a carbide phase, and the average diameter of the primary crystal structure according to the following method 1 is 30 μm or less. (Method 1) The high chromium cast iron is polished to prepare a test piece for microstructural observation, and then the polished surface of the test piece for microstructural observation is observed by a scanning electron microscope (SEM). The obtained SEM photograph is then analyzed by image processing software to determine the average diameter of the primary crystal structure. Here, Fig. 1 is a diagram for explaining the diameter (l) of the primary crystal structure. In this specification, as shown in Fig. 1, the diameter of the primary crystal structure indicates the maximum distance between planes perpendicular to the minor axis direction of the primary crystal structure, that is, the maximum distance in the minor axis direction. The average diameter of the primary crystal structure is determined by randomly selecting 50 primary crystal structures and measuring the diameter of each of them. The average diameter is calculated by accumulating all the diameters of the primary crystal structures and dividing by the number of structures. The primary crystal structures to be randomly selected here are those whose short and long axes can be clearly determined, as shown in Figure 1.

[0017] For example, in facilities and industrial machinery such as construction machinery, ceramics, crushing, mining, power, and dredging, the components that come into contact with or rub against the raw materials and materials handled are subject to significant wear, and therefore there is a demand for further improvement in the wear resistance of materials used for such components. Known techniques are unable to ensure wear resistance sufficient to satisfy recent stringent requirements for wear-resistant members, resulting in rapid wear of the members.

[0018] Known high chromium cast irons are classified into two types based on the solidification structure: hypoeutectic alloys with austenite as the primary crystal structure, and hypereutectic alloys with carbide as the primary crystal structure. High chromium cast irons are generally used as wear-resistant parts by transforming the austenite phase into martensite by quenching heat treatment, and are often used in a martensite and carbide phase configuration. This is because both the martensite and carbide phases are hard and have strong wear resistance. In hypoeutectic alloy high chromium cast iron, the austenite phase in the primary crystal structure and the austenite phase in the eutectic structure transform into martensite phase through quenching heat treatment, while the phase structure of the carbide phase in the eutectic structure does not change, so that the structure after quenching heat treatment consists of a martensite phase formed from the primary crystal austenite phase, a martensite phase formed from the austenite phase in the eutectic structure, and a carbide phase in the eutectic structure. On the other hand, in the case of high chromium cast iron which is a hypereutectic alloy, the austenite phase in the eutectic structure transforms into a martensite phase by quenching heat treatment, while the phase structures of the carbide phase in the primary crystal structure and the carbide phase in the eutectic structure do not change, and the structure after quenching heat treatment consists of a martensite phase formed from the austenite phase in the eutectic structure, the carbide phase in the eutectic structure, and the carbide phase in the primary crystal structure. Here, the present inventors have found that in hypereutectic high chromium cast iron, there is a correlation between the average diameter of the primary crystal structure containing a carbide phase and the wear resistance. That is, according to the high chromium cast iron of this embodiment, since it contains C, Cr and Fe in the above ratio and the average diameter of the primary crystal structure containing the carbide phase is within the above range, the wear resistance can be improved.

[0019] Here, a general explanation regarding the eutectic structure, hypoeutectic structure, and hypereutectic structure will be supplemented. A eutectic structure is one of the solidification forms (crystalline structures) that occur when an alloy or the like solidifies; it is a crystal that is formed when the liquid phase L decomposes and solid phases α and β are formed simultaneously. The reaction that forms a eutectic structure, i.e., L → α + β, is called a eutectic reaction. The composition and temperature of the eutectic reaction are called the eutectic point. Since the solid phases α and β in the eutectic reaction form next to each other, the eutectic structure is characterized by the two phases, α and β, surrounding each other, intertwining, and dispersing uniformly. As an example of a eutectic structure, the eutectic point of a binary alloy system of Fe and C has a composition of 95.8% Fe by mass and 4.2% C by mass, and a temperature of 1153°C. The liquid phase L with the eutectic composition of 95.8% Fe by mass and 4.2% C by mass decomposes at temperatures below 1153°C, forming the austenite phase and carbide phase of the eutectic structure. As a result, the austenite phase and the carbide phase surround each other, intertwine, and are uniformly dispersed. A hypoeutectic structure is one of the solidification forms (crystalline structures) that occur when an alloy or the like solidifies. The hypoeutectic composition is to the left of the eutectic point. First, a solid α phase called the primary crystal crystallizes out of the liquid phase L of the hypoeutectic composition, and as the primary α phase crystallizes out, the composition of the liquid phase L changes to that of the eutectic point. When the composition of the liquid phase L reaches the composition of the eutectic point, the liquid phase L of the eutectic point composition decomposes, simultaneously forming the solid α and solid β phases of the eutectic structure. A structure consisting of the primary α phase and a eutectic structure is defined as a hypoeutectic structure. A hypereutectic structure is one of the solidification forms (crystalline structures) that occur when an alloy or the like solidifies. The hypereutectic composition is to the right of the eutectic point. First, a solid β phase called the primary crystal crystallizes out of the liquid phase L of the hypereutectic composition, and as the primary β phase crystallizes out, the composition of the liquid phase L changes to that of the eutectic point. When the composition of the liquid phase L reaches the composition of the eutectic point, the liquid phase L of the eutectic point composition decomposes, simultaneously forming the solid α and solid β phases of the eutectic structure. A structure consisting of the primary β phase and a eutectic structure is defined as a hypereutectic structure. Hypoeutectic and hypereutectic structures are the opposite of eutectic structures, and a composition to the left of the eutectic point, i.e., a hypoeutectic composition, has a primary α phase in addition to the eutectic structure, while a composition to the right of the eutectic point, i.e., a hypereutectic composition, has a primary β phase in addition to the eutectic structure. Taking an Fe and C binary alloy system as an example, the composition at the eutectic point, i.e., the eutectic composition, is Fe 95.8% by mass and C 4.2% by mass, and a hypoeutectic composition with C < 4.2% by mass is composed of a primary austenite phase and a eutectic structure, and has a hypoeutectic structure. On the other hand, a hypereutectic composition with C > 4.2% by mass is composed of a primary carbide phase and a eutectic structure, and has a hypereutectic structure.

[0020] In the high chromium cast iron of this embodiment, the average diameter of the primary crystal structure is 30 μm or less, but from the viewpoint of further improving the balance of the wear resistance and corrosion resistance of the high chromium cast iron of this embodiment, it is preferably 28 μm or less, more preferably 25 μm or less, and even more preferably 23 μm or less. Since the smaller the average diameter of the primary crystal structure, the more preferable it is, the lower limit of the average diameter of the primary crystal structure is not particularly limited, but may be, for example, 0.1 μm or more, 1 μm or more, 3 μm or more, 5 μm or more, or 10 μm or more. Here, in order to adjust the average diameter of the primary crystal structures in the high chromium cast iron of this embodiment to fall within the above range, it is important to, for example, add a refiner together with each raw material in the casting process, to appropriately adjust the content ratio of each component of the high chromium cast iron of this embodiment, and to adjust the pouring temperature in the casting process to a specific temperature, which will be described later.

[0021] In the high chromium cast iron of the present embodiment, the area ratio X1 of the primary crystal structure by the following method 2 is preferably 30% or more, more preferably 35% or more, and further preferably 40% or more, from the viewpoint of further improving the wear resistance and corrosion resistance of the high chromium cast iron of the present embodiment. The upper limit of the area ratio X1 of the primary crystal structure is not particularly limited, but may be, for example, 80% or less, 70% or less, 60% or less, or 50% or less. (Method 2) The high chromium cast iron is polished to prepare a test piece for microstructural observation, and then the polished surface of the test piece for microstructural observation is observed by an electron microscope (SEM). The SEM photograph obtained is then analyzed by image processing software to determine the area ratio X1 of the primary crystal structure.

[0022] In the high chromium cast iron of the present embodiment, from the viewpoint of further improving the balance of the wear resistance and corrosion resistance of the high chromium cast iron, it is preferable that the eutectic structure surrounds the primary crystal structure.

[0023] In the high chromium cast iron of this embodiment, from the viewpoint of further improving the performance balance of the wear resistance and corrosion resistance of the high chromium cast iron, it is preferable that the eutectic structure is composed of the martensite phase formed by cooling the austenite phase and the carbide phase.

[0024] The Rockwell hardness HRC of the high chromium cast iron of this embodiment is preferably 55 or more, more preferably 57 or more, even more preferably 60 or more, still more preferably 63 or more, still more preferably 64 or more, and even more preferably 66 or more, from the viewpoint of further improving the performance balance of the high chromium cast iron in terms of wear resistance and corrosion resistance. Further, the upper limit of the Rockwell hardness HRC is not particularly limited, but may be, for example, 100 or less, 90 or less, 80 or less, 75 or less, or 70 or less.

[0025] The wear rate of the high chromium cast iron of this embodiment, measured by the following method 3, is preferably 3.5 mass% or less, more preferably 3.3 mass% or less, even more preferably 3.2 mass% or less, even more preferably 3.0 mass% or less, and even more preferably 2.9 mass% or less, from the viewpoint of further improving the wear resistance of the high chromium cast iron. Furthermore, the upper limit of the wear rate is not particularly limited, but may be, for example, 0.1 mass% or more, optionally 0.5 mass% or more, optionally 1.0 mass% or more, optionally 1.5 mass% or more, optionally 2.0 mass% or more, or optionally 2.5 mass% or more. (Method 3) A test piece of 40 mm length x 22 mm width x 6 mm height (with Φ8 mm bolt hole) made of the high chromium cast iron is prepared. Next, a mixture of SiO2 and water with a mass ratio of SiO2 to water of 1:2 is made into a slurry, the test piece is set in the slurry, the temperature of the slurry is set to 20°C, the test piece is rotated at a speed of 2000 rpm, and a wear test is performed at a peripheral speed of 10.5 m / s. Next, the slurry is replaced every hour during the test, and the wear rate is calculated by dividing the change in mass from the initial mass of the test piece after 12 hours by the initial mass of the test piece.

[0026] The impact value of the high chromium cast iron of this embodiment, as measured by the following method 4, is preferably 1.0 J / cm from the viewpoint of further improving the balance of the wear resistance and impact resistance of the high chromium cast iron. 2 More preferably, 1.3 J / cm 2 More preferably, 1.5 J / cm 2 More preferably, 1.8 J / cm 2 That's all. The upper limit of the impact value is not particularly limited, but is, for example, 10.0 J / cm 2 Less than 5.0 J / cm 2 It may be less than 3.0 J / cm 2 It may be less than 2.5 J / cm 2 It may be less than 2.3 J / cm 2 It may be the following. (Method 4) A test piece with a notch of 50 mm length × 10 mm width × 10 mm height (notch shape: U notch, notch size: depth 2 mm, tip R1.0 mm, notch position: center in the vertical direction) made of the high chromium cast iron is prepared. Next, an impact test is carried out at 20°C, and in accordance with JIS Z2242:2018, an impact load is applied to the test piece with a pendulum hammer, and the energy E (J) at the time of destruction is calculated as the impact value C (=E / A: A is the cross-sectional area (cm) of the notch part of the test piece). 2 )) is required.

[0027] Each component will be described in detail below.

[0028] From the viewpoint of further improving the performance balance of the wear resistance and corrosion resistance of the high chromium cast iron, the C content in the high chromium cast iron of this embodiment is 4.0 mass% or more, preferably 4.1 mass% or more, more preferably 4.2 mass% or more, even more preferably 4.3 mass% or more, and even more preferably 4.4 mass% or more, and is 7.0 mass% or less, preferably 6.0 mass% or less, more preferably 5.5 mass% or less, even more preferably 5.0 mass% or less, even more preferably 4.8 mass% or less, and even more preferably 4.6 mass% or less.

[0029] From the viewpoint of further improving the performance balance of the wear resistance and corrosion resistance of the high chromium cast iron, the Cr content in the high chromium cast iron of this embodiment is 15.0 mass% or more, preferably 18.0 mass% or more, more preferably 20.0 mass% or more, even more preferably 23.0 mass% or more, even more preferably 25.0 mass% or more, even more preferably 27.0 mass% or more, and is 40.0 mass% or less, preferably 38.0 mass% or less, more preferably 35.0 mass% or less, even more preferably 33.0 mass% or less, even more preferably 32.0 mass% or less, and even more preferably 30.0 mass% or less.

[0030] In addition, from the viewpoint of further improving the performance balance of the wear resistance and corrosion resistance of the high chromium cast iron of this embodiment, the C content in the high chromium cast iron of this embodiment is preferably 4.1 mass% or more and 5.5 mass% or less, and the Cr content is preferably 20.0 mass% or more and 35.0 mass% or less, the C content in the high chromium cast iron of this embodiment is more preferably 4.2 mass% or more and 5.0 mass% or less, and the Cr content is more preferably 23.0 mass% or more and 32.0 mass% or less, the C content in the high chromium cast iron of this embodiment is more preferably 4.3 mass% or more and 4.8 mass% or less, and the Cr content is more preferably 25.0 mass% or more and 30.0 mass% or less, and the C content in the high chromium cast iron of this embodiment is more preferably 4.4 mass% or more and 4.6 mass% or less, and the Cr content is more preferably 27.0 mass% or more and 30.0 mass% or less.

[0031] The content of Fe in the high chromium cast iron of this embodiment is 48.0 mass% or more, preferably 50.0 mass% or more, more preferably 53.0 mass% or more, even more preferably 55.0 mass% or more, even more preferably 58.0 mass% or more, even more preferably 60.0 mass% or more, even more preferably 61.0 mass% or more, and 81.0 mass% or less, preferably 78.0 mass% or less, more preferably 76.0 mass% or less, even more preferably 74.0 mass% or less, even more preferably 72.0 mass% or less, even more preferably 70.0 mass% or less, even more preferably 68.0 mass% or less, even more preferably 67.0 mass% or less, and even more preferably 66.0 mass% or less.

[0032] From the viewpoint of further improving the wear resistance, the high chromium cast iron of the present embodiment preferably further contains one or two elements selected from the group consisting of Si and Mn.

[0033] Si is an element that improves the fluidity of the molten high chromium cast iron and acts as a deoxidizer during melting. From the viewpoint of further increasing the strength of the martensite phase generated when the high chromium cast iron is quenched, the content of Si in the high chromium cast iron of this embodiment is preferably 0 mass% or more, more preferably more than 0 mass%, even more preferably 0.1 mass% or more, even more preferably 0.2 mass% or more, even more preferably 0.4 mass% or more, even more preferably 0.5 mass% or more, even more preferably 0.6 mass% or more, and preferably 2.0 mass% or less, more preferably 1.5 mass% or less, even more preferably 1.2 mass% or less, and even more preferably 1.0 mass% or less.

[0034] From the viewpoint of further increasing the strength of the martensite phase generated when the high chromium cast iron is quenched and further improving the corrosion resistance of the quenched molded product, the Mn content in the high chromium cast iron of this embodiment is preferably 0 mass% or more, more preferably more than 0 mass%, even more preferably 0.1 mass% or more, even more preferably 0.3 mass% or more, even more preferably 0.5 mass% or more, even more preferably 0.8 mass% or more, even more preferably 1.0 mass% or more, even more preferably 1.2 mass% or more, and is preferably 5.0 mass% or less, more preferably 4.0 mass% or less, even more preferably 3.0 mass% or less, even more preferably 2.0 mass% or less, and even more preferably 1.8 mass% or less.

[0035] In order to further strengthen the austenite phase or martensite phase and the carbide phase and to further improve the wear resistance, the high chromium cast iron of this embodiment preferably further contains one or more elements selected from the group consisting of Mo, W, Nb, V, Co, Ni, Cu, Ti, B and rare earth elements, and more preferably further contains one or more elements selected from the group consisting of Mo, Nb and Ni. By containing the above elements in the high chromium cast iron of this embodiment, the corrosion resistance and toughness of the hardened product using the high chromium cast iron of this embodiment can be further improved, and cracks during hardening can be further prevented. The contents of these elements can be appropriately determined depending on the application of the high chromium cast iron according to this embodiment, but the total content of the above elements in the high chromium cast iron according to this embodiment is preferably 0 mass% or more, more preferably 0.1 mass% or more, even more preferably 0.5 mass% or more, even more preferably 0.8 mass% or more, even more preferably 1.0 mass% or more, and preferably 5.0 mass% or less, more preferably 3.0 mass% or less, and even more preferably 2.5 mass% or less.

[0036] The high chromium cast iron of this embodiment may contain unavoidable impurities. Inevitable impurities refer to elements that cannot be completely removed from the raw materials used in the production of high chromium cast iron. Examples of such unavoidable impurities include P, S, Al, Pb, and Zn. The content of unavoidable impurities in the high chromium cast iron of this embodiment is preferably 0 mass% or more and 0.1 mass% or less, more preferably 0 mass% or more and 0.08 mass% or less, more preferably 0 mass% or more and 0.05 mass% or less, and even more preferably 0 mass% or more and 0.01 mass% or less, from the viewpoint of further preventing deterioration in performance, including embrittlement and deterioration in corrosion resistance, of the high chromium cast iron.

[0037] Various elements have been exemplified above, but elements other than the above exemplified elements may be added within a range that does not impair the effects of this embodiment. The composition of the various elements may be the raw material blending ratio during production, or may be a composition measured by component analysis after production. For the component analysis, known analytical methods can be used, such as energy dispersive X-ray spectrometry (SEM-EDS), optical emission spectrometry (OES), inductively coupled plasma analysis (ICP), and X-ray fluorescence analysis (XRF).

[0038] Due to its characteristics, the high chromium cast iron of the present embodiment is preferably used for parts that operate while coming into contact with other parts or substances such as liquids, solids, and liquid-solid mixtures, etc. In particular, it is preferably used for pump parts or crusher parts.

[0039] [Manufacturing method of high chromium cast iron] The manufacturing method of high chromium cast iron in this embodiment includes, for example, a casting process in which a molten metal obtained by melting raw materials of high chromium cast iron is poured into a mold and the high chromium cast iron is cast at a specific temperature, and a quenching process in which the high chromium cast iron is heated and held at that temperature, and then cooled to quench it.

[0040] (Casting process) In the manufacturing method of the high chromium cast iron of the present embodiment, in the casting process, the raw materials such as Fe, C, and Cr are mixed in a desired composition ratio, and then, for example, the mixture is filled in a magnesia crucible and heated and melted under an argon atmosphere or a nitrogen atmosphere to obtain a molten metal (molten liquid). Next, the obtained molten liquid is cast into a mold (sand mold), and the high chromium cast iron is cast at a temperature preferably between (liquidus temperature of high chromium cast iron) ° C. and (liquidus temperature of high chromium cast iron + 25) ° C., more preferably between (liquidus temperature of high chromium cast iron + 3) ° C. and (liquidus temperature of high chromium cast iron + 20) ° C., even more preferably between (liquidus temperature of high chromium cast iron + 5) ° C. and (liquidus temperature of high chromium cast iron + 18) ° C., and even more preferably between (liquidus temperature of high chromium cast iron + 8) ° C. and (liquidus temperature of high chromium cast iron + 15) ° C. to obtain the high chromium cast iron. Here, the liquidus temperature of high chromium cast iron refers to the lowest temperature at which the high chromium cast iron is completely liquid, and can be calculated by measuring the solid / liquid phase transformation temperature of the high chromium cast iron using the thermal analysis method of differential thermal analysis (DTA) or differential scanning calorimetry (DSC), and specifically, can be measured by the method described in the examples.

[0041] In the casting process, refiners can be further added together with the raw materials such as Fe, C, Cr, etc. The grain refiner includes, for example, a carbide containing one or more elements selected from the group consisting of Cr, Mo, W, V, Nb, Ta, Ti, Zr, Hf, B and rare earth elements, more preferably includes a chromium carbide, further preferably includes one or more elements selected from the group consisting of Cr7C3, Cr3C2 and high carbon ferrochrome (HC-FeCr), and further preferably includes HC-FeCr. The amount of the refiner added is, when the amount of the obtained high chromium cast iron is taken as 100 mass%, preferably 0.1 mass% or more, more preferably 0.2 mass% or more, even more preferably 0.3 mass% or more, even more preferably 0.5 mass% or more, even more preferably 0.8 mass% or more, and is preferably 5.0 mass% or less, more preferably 3.0 mass% or less, even more preferably 2.0 mass% or less, and even more preferably 1.5 mass% or less.

[0042] (Quenching process) In the manufacturing method of the high chromium cast iron of the present embodiment, the quenching step is a step of hardening the high chromium cast iron by further heating and cooling the high chromium cast iron. The temperature conditions in the quenching step are preferably such that the high chromium cast iron is heated and held at a furnace temperature of 880°C to 1200°C for a holding time of 1 hour to 12 hours, and then cooled at a cooling rate of 50°C / min or more.

[0043] In the manufacturing method of the high chromium cast iron of this embodiment, the temperature in the furnace in the quenching step is preferably 880° C. to 1200° C., more preferably 900° C. to 1100° C., and further preferably 920° C. to 1000° C. By setting the temperature in the furnace within the above range, the hardness can be further improved without deteriorating the balance of the wear resistance and corrosion resistance of the quenched high chromium cast iron product.

[0044] In the manufacturing method of the high chromium cast iron of this embodiment, the lower limit of the holding time in the quenching step is preferably 1 hour or more, more preferably 2 hours or more, and further preferably 3 hours or more. By setting the lower limit of the holding time to the above lower limit or more, the hardness of the quenched product of the high chromium cast iron can be improved without deteriorating the balance of the wear resistance and corrosion resistance of the product. The upper limit of the holding time is preferably 12 hours or less, more preferably 10 hours or less, even more preferably 8 hours or less, and even more preferably 6 hours or less. By keeping the upper limit of the holding time below the above upper limit, the performance balance of the wear resistance and corrosion resistance of the quenched formed product of high chromium cast iron can be further improved.

[0045] In the quenching heat treatment method of the high chromium cast iron of this embodiment, the lower limit of the cooling rate of the high chromium cast iron in the quenching step is preferably 50°C / min or more, more preferably 60°C / min or more, and further preferably 70°C / min or more. By setting the lower limit of the cooling rate to the above lower limit or more, the hardness of the quenched product of the high chromium cast iron can be improved without deteriorating the wear resistance and corrosion resistance. The upper limit of the cooling rate is preferably 150° C. / min or less, more preferably 140° C. / min or less, and even more preferably 130° C. / min or less. By keeping the upper limit of the cooling rate below the above upper limit, the wear resistance and corrosion resistance of the quench-formed product of high chromium cast iron can be made more suitable. The cooling method at this time is not particularly limited, and any known cooling method can be used, but forced air cooling is preferred.

[0046] The manufacturing method of the high chromium cast iron of this embodiment can further include, between the casting step and the quenching step, an annealing heat treatment step of heating and holding the high chromium cast iron at a temperature of, for example, 700°C or higher and lower than 880°C to anneal it, and a processing step of machining the high chromium cast iron after the annealing heat treatment step.

[0047] (Annealing heat treatment process) In the manufacturing method of the high chromium cast iron of this embodiment, the annealing heat treatment step is a step for improving the machinability of the high chromium cast iron by annealing the cast iron by heating and holding the temperature at, for example, 700° C. or more and less than 880° C. The temperature conditions in the annealing heat treatment step are preferably a furnace temperature of 700° C. or more and less than 880° C., and a holding time of 1 hour or more and 12 hours or less.

[0048] In the manufacturing method of the high chromium cast iron of the present embodiment, the temperature in the furnace in the annealing heat treatment step is more preferably 700° C. or more and less than 880° C., even more preferably 750° C. or more and 870° C. or less, and even more preferably 800° C. or more and 870° C. or less. By setting the temperature in the furnace within the above numerical range, the machinability of the high chromium cast iron can be further improved.

[0049] In the manufacturing method of the high chromium cast iron of the present embodiment, the lower limit of the holding time in the annealing heat treatment step is preferably 1 hour or more, more preferably 2 hours or more, and further preferably 3 hours or more. By setting the lower limit of the holding time to the above lower limit or more, the machinability of the high chromium cast iron can be improved. Moreover, the upper limit of the holding time is preferably 12 hours or less, more preferably 10 hours or less, further preferably 8 hours or less, and further preferably 6 hours or less. By setting the upper limit of the holding time to the above upper limit or less, the productivity of high chromium cast iron can be more suitably improved.

[0050] In the manufacturing method of the high chromium cast iron of this embodiment, the cooling rate of the high chromium cast iron in the annealing heat treatment step is preferably 100° C. / hour or less, more preferably 50° C. / hour or less, and further preferably 30° C. / hour or less. By setting the upper limit of the cooling rate to the above upper limit or less, the machinability of the high chromium cast iron can be made more suitable. The lower limit of the cooling rate is not particularly limited, but may be, for example, 5° C. / hour or more, 10° C. / hour or more, or 20° C. / hour or more. The cooling method at this time is not particularly limited, and any known cooling method can be used, but slow cooling in a furnace is preferable.

[0051] (Processing process) In the manufacturing method of the high chromium cast iron of the present embodiment, the high chromium cast iron is machined into a final target shape in the processing step. The machining method can be a conventionally known method, for example, lathe processing, milling, drilling, grinding, polishing, electric discharge machining, etc.

[0052] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted as long as they do not impair the effects of the present invention.

[0053] The present invention is not limited to the above-described embodiment, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention. EXAMPLES

[0054] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to the descriptions of these examples and comparative examples.

[0055] The methods for confirming the effects of this embodiment, including melting of high chromium cast iron, casting, annealing heat treatment, quenching heat treatment, hardness measurement method, impact value measurement method, structure observation of high chromium cast iron, measurement method of average diameter of primary crystal structures, measurement method of area ratio X1 of primary crystal structures, measurement method of liquidus temperature, and measurement method of wear rate and wear resistance, will be described in detail below.

[0056] [Melting and casting of high chromium cast iron] The raw materials Fe, C, Cr, Si and Mn, all with a purity of 99.9% (mass%), were mixed so that the composition ratio of each element was as shown in Table 1. The mixture was then filled into a magnesia crucible and heated and melted under an argon atmosphere. After melting, HC-FeCr (High Carbon Ferro Chrome), a refiner, was added in the ratio shown in Table 1. The molten liquid was poured into a mold (sand mold), and high chromium cast iron was cast at the casting temperature shown in Table 1, producing high chromium cast iron pieces measuring 140 mm long x 49 mm wide x 12 mm high.

[0057] [Annealing heat treatment of high chromium cast iron] The high chromium cast iron produced in the above [Melting and casting of high chromium cast iron] was subjected to annealing heat treatment by heating and holding at a temperature of 850°C for 4 hours. The high chromium cast iron after annealing heat treatment had low hardness and was easy to machine.

[0058] [Quenching heat treatment of high chromium cast iron] The annealed and heat-treated high chromium cast iron produced in the above [Annealing heat treatment of high chromium cast iron] was processed by electrical discharge machining and machining to a size of 20 mm length x 20 mm width x 6 mm height. After that, using an electric furnace in an air atmosphere, the processed high chromium cast iron was heated and held at a temperature of 950°C for 4.5 hours, and then cooled at a cooling rate of 75°C / min to perform a quenching heat treatment, thereby obtaining high chromium cast iron after quenching heat treatment.

[0059] [Hardness measurement of high chromium cast iron] The high chromium cast iron after quenching heat treatment prepared in the above [Heat treatment of quenching high chromium cast iron] was processed by grinding into test pieces of 20 mm length x 20 mm width x 5.5 mm height. The hardness of the test pieces was measured at nine points using a Rockwell (HRC) hardness tester under the conditions of a load of 150 kgf and a load holding time of 15 s. Of the nine measurement data points, the average value of seven points excluding the maximum and minimum hardness data was used as the hardness data for each test piece.

[0060] [Impact value measurement of high chromium cast iron] The annealed and heat-treated high chromium cast iron produced in the above [Annealing heat treatment of high chromium cast iron] was machined by wire electric discharge machining into 50 mm length x 10 mm width x 10 mm height (with a notch in the vertical center).Then, using an electric furnace, the machined high chromium cast iron was heated and held at 950°C for 4.5 hours in an air atmosphere, and then cooled at a cooling rate of 75°C / min to perform quenching heat treatment, thereby obtaining notched test pieces for impact value measurement with dimensions of 50 mm length x 10 mm width x 10 mm height (notch shape: U notch, notch size: depth 2 mm, tip R1.0 mm, notch position: vertical center). The impact test was carried out at 20°C in accordance with JIS Z2242:2018, and the impact value C (=E / A) was calculated from the energy E (J) at the time when the test piece was broken by applying an impact load to the test piece with a pendulum hammer, where A is the cross-sectional area of ​​the notch part of the test piece.

[0061] [Observation of the structure of high chromium cast iron] The high chromium cast iron after quenching heat treatment prepared in the above [Heat treatment of high chromium cast iron] was processed by polishing into a test piece for microstructure observation of length 20 mm x width 20 mm x height 6 mm. For the microstructure observation, the observation surface of the test piece was polished with waterproof abrasive paper silicon carbide (SiC) #100 → #220 → #400 → #800 → #1000 → #2000 in that order, then buffed with diamond polishing liquid (abrasive grain: 1 μm), and the entire polished surface was immersed in the etchant at 23 ° C for 20 seconds using Murakami's reagent and nital etchant (5%). The obtained observation surface was then observed using an electron microscope (SEM).

[0062] [Measurement of the average diameter of primary crystal structure] The image processing software ImageJ was used to analyze the structure (SEM photograph) of the high chromium cast iron taken at 100 times magnification in the above [Structural observation of high chromium cast iron], and the average diameter of the primary crystal structure consisting of carbide phase was obtained. Here, as shown in Figure 1, the diameter of the primary crystal structure was the maximum distance between the planes perpendicular to the minor axis direction of the primary crystal structure, that is, the maximum distance in the minor axis direction. The average diameter of the primary crystal structure was determined by randomly selecting 50 primary crystal structures, measuring the diameter of each of the primary crystal structures, accumulating all the diameters of the primary crystal structures, and dividing the total by the number of structures. Here, the primary crystal structures selected at random were those in which the minor and major axes could be clearly determined, as shown in Figure 1.

[0063] [Measurement of area ratio X1 of primary crystal structure] Using the image processing software ImageJ, the structure of the high chromium cast iron (SEM photograph) taken at 100x magnification in the above [Structural observation of high chromium cast iron] was analyzed to determine the area ratio (X1) of the primary crystal structure consisting of carbide phase. Here, the area ratio was measured at any five points on the observation surface of the test piece for structural observation, and the average of the obtained values ​​was taken as the area ratio (X1) of the primary crystal structure.

[0064] [Measurement of the liquidus temperature of high chromium cast iron] The liquidus is the lowest temperature at which an alloy is completely liquid, and can be calculated by measuring the solid / liquid phase transformation temperature of the alloy using the thermal analysis methods differential thermal analysis (DTA) or differential scanning calorimetry (DSC). DSC measurements were performed on high chromium cast irons of the same composition as in the examples and comparative examples, as follows. First, 300 mg of high chromium cast iron was weighed into an aluminum pan in an argon atmosphere to prepare a sample. Next, differential scanning calorimetry was performed on the sample using a differential scanning calorimeter (STA449 F3, manufactured by Netzsch Japan Co., Ltd.) under the following conditions: starting temperature 25°C, measurement temperature range 25°C to 1500°C, heating rate 5°C / min, and argon atmosphere of 20 ml per minute. From the DSC curve obtained in the temperature range of 1340°C to 1500°C, the higher of the two intersections between the tangent of the inflection point of the endothermic peak during heating and the baseline was determined as the liquidus temperature of the high chromium cast iron.

[0065] [Wear rate and wear resistance measurement of high chromium cast iron] The annealed and heat-treated high chromium cast irons prepared in the above [Annealing heat treatment of high chromium cast iron] were machined by cutting and wire electric discharge machining into 40 mm length x 22 mm width x 6 mm height (with Φ8 mm bolt holes).Then, using an electric furnace, the machined high chromium cast irons were heated and held at 950°C for 4.5 hours in an air atmosphere, and then cooled at a cooling rate of 75°C / min to perform quenching heat treatment, thereby obtaining test pieces for wear resistance measurement measuring 40 mm length x 22 mm width x 6 mm height (with Φ8 mm bolt holes). Next, a mixture of quartz gravel (SiO2, manufactured by Toyo Kosan Co., Ltd. Fukushima Factory, product name: artificial Iwaki silica sand No. 3, particle size: 1 to 2 mm) and water with a mass ratio of SiO2 to water of 1:2 was made into a slurry, and four test pieces for measuring wear resistance were set in the slurry, the temperature of the slurry was set to 20°C, and the test pieces were rotated at a speed of 2000 rpm using an erosion tester, and a wear test was performed at a peripheral speed of 10.5 m / s. The slurry was replaced every hour during the test, and the wear rate (mass reduction rate) was calculated by dividing the mass change of the test piece by the initial mass each time, and the wear test was performed for a total of 12 hours. The wear rate was calculated by dividing the amount of change from the initial mass of the test piece after 12 hours by the initial mass of the test piece. The smaller the wear rate, the better the wear resistance. The average value of the four pieces was used as the wear rate. Here, for Examples 1 and 2 and Comparative Examples 1 and 2, the improvement rates of the wear rate relative to Comparative Example 1 were calculated, and for Example 3 and Comparative Example 3, the improvement rates of the wear rate relative to Comparative Example 3 were calculated.

[0066] The above results are shown in Table 1.

[0067] [Table 1]

Claims

1. A high chromium cast iron containing C, Cr and Fe, The C content is 4.0% by mass or more and 7.0% by mass or less, The Cr content is 15.0 mass% or more and 40.0 mass% or less, The Fe content is 48.0 mass% or more and 81.0 mass% or less, The steel sheet includes a eutectic structure and a primary crystal structure including a carbide phase, A high chromium cast iron, wherein the primary crystal structure has an average diameter of 30 μm or less, by the following method 1. (Method 1) The high chromium cast iron is polished to prepare a test piece for microstructural observation, and then the polished surface of the test piece for microstructural observation is observed by a scanning electron microscope (SEM). The obtained SEM photograph is then analyzed by image processing software to determine the average diameter of the primary crystal structure.

2. The high chromium cast iron according to claim 1 , wherein the eutectic structure surrounds the primary structure.

3. The area ratio X of the primary crystal structure according to the following method 2 1 The high chromium cast iron according to claim 1 or 2, wherein the content of Cr is 30% or more. (Method 2) The high chromium cast iron was polished to prepare a test piece for microstructural observation, and then the polished surface of the test piece for microstructural observation was observed by an electron microscope (SEM). The SEM photograph obtained was then analyzed by image processing software to determine the area ratio X of the primary crystal structure. 1 Request.

4. The high chromium cast iron according to claim 1 or 2, wherein the C content is 4.1 mass% or more and 5.5 mass% or less, and the Cr content is 20.0 mass% or more and 35.0 mass% or less.

5. The high chromium cast iron according to claim 1 or 2, wherein the C content is 4.2 mass% or more and 5.0 mass% or less, and the Cr content is 23.0 mass% or more and 32.0 mass% or less.

6. The high chromium cast iron according to claim 1 or 2, wherein the C content is 4.3 mass% or more and 4.8 mass% or less, and the Cr content is 25.0 mass% or more and 30.0 mass% or less.

7. The high chromium cast iron according to claim 1 or 2, wherein the Fe content is 55.0 mass% or more and 76.0 mass% or less.

8. The high chromium cast iron according to claim 1 or 2, further comprising one or two elements selected from the group consisting of Si and Mn.

9. The high chromium cast iron according to claim 8, wherein the Si content is more than 0 mass% and not more than 2.0 mass%.

10. The high chromium cast iron according to claim 8, wherein the Mn content is more than 0 mass% and not more than 5.0 mass%.

11. 3. The high chromium cast iron according to claim 1 or 2, further comprising one or more elements selected from the group consisting of Mo, W, Nb, V, Co, Ni, Cu, Ti, B and rare earth elements.

12. 3. The high chromium cast iron according to claim 1 or 2, having a Rockwell hardness HRC of 55 or more.

13. The high chromium cast iron according to claim 1 or 2, having a wear rate of 3.5 mass% or less according to the following method 3. (Method 3) A test piece of the high chromium cast iron with a length of 40 mm, a width of 22 mm, and a height of 6 mm (with a Φ8 mm bolt hole) is prepared. 2 and water in a mass ratio of 1:

2. 2 A mixture of water and ethanol is made into a slurry, the test piece is placed in the slurry, the temperature of the slurry is set to 20° C., the test piece is rotated at a speed of 2000 rpm, and a wear test is performed at a peripheral speed of the test piece of 10.5 m / s. Next, the slurry is replaced with a new one every hour during the test, and the wear rate is calculated by dividing the amount of change from the initial mass of the test piece after 12 hours by the initial mass of the test piece.

14. The impact value according to the following method 4 is 1.0 J / cm 2 The high chromium cast iron according to claim 1 or 2. (Method 4) A notched test piece (notch shape: U notch, notch size: depth 2 mm, tip R 1.0 mm, notch position: center in the vertical direction) made of the high chromium cast iron is prepared. Then, an impact test is carried out at 20°C in accordance with JIS Z2242:2018, and the impact value C (=E / A: A is the cross-sectional area (cm) of the notched part of the test piece) is calculated from the energy E (J) when the test piece is broken by applying an impact load to the test piece with a pendulum hammer. 2 )).

Citation Information

Patent Citations

  • Wear resistant alloy cast iron material

    JP2001049381A

  • High-chromium iron casting for large object and its manufacturing process

    JP2003286537A

  • Casting for wear-resistant member, and manufacturing method therefor

    JP2008075108A

  • High chromium cast iron

    JP2012219346A

  • High chromium wear resistant cast iron

    JP2013237904A

Cited By

  • Cast iron with excellent abrasion resistance

    JP7931535B1