Laminated film and method for producing laminated film

The laminated film with specific optical and mechanical properties minimizes interference during optical inspection, enabling accurate detection of adherends by reducing defects and peeling force.

JP2024145562AInactive Publication Date: 2024-10-15NITTO DENKO CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023057969
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Laminated films attached to adherends can cause erroneous optical inspections, leading to inaccurate detection of the adherend.

Method used

A laminated film with a base film made of a resin material having an in-plane retardation of 10 nm or less and a defect count of 8 or less per 10 cm², and an adhesive layer with a peeling force of 3.0 N/25 mm or less, ensuring accurate optical inspection by minimizing interference.

Benefits of technology

Suppresses false detections during optical inspection and allows for accurate inspection of adherends by reducing optical interference and ensuring smooth peeling of the laminated film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145562000001_ABST
    Figure 2024145562000001_ABST
Patent Text Reader

Abstract

To provide a laminated film that can reduce erroneous detection caused by the laminated film, allowing for precise examination of an adherend, even when subjected to optical inspection while being bonded to the adherend, and a production method of the same laminated film.SOLUTION: A laminated film according to an embodiment includes a base film composed of a resin material and an adhesive layer. The adhesive layer is laminated on the base film. The base film has an in-plane phase difference Re(550) of 10 nm or less. The number of defects with a maximum Feret diameter of 30 μm or more is 8 or fewer in a unit area of 10 cm2 of the base film.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate film and a method for producing the laminate film. [Background technology]

[0002] It is known that a laminate film having a base film and a pressure-sensitive adhesive layer is attached to the surface of various industrial products for various purposes. One purpose of attaching a laminate film is to protect the surface of an adherend. As such a laminate film, for example, a surface protection film for a polarizing plate having a support film and a pressure-sensitive adhesive layer formed on one or both sides of the support film has been proposed (see Patent Document 1).

[0003] It has been considered to inspect the adherend with such a laminate film attached to the adherend. However, when the adherend with the laminate film attached is subjected to optical inspection, erroneous detection due to the laminate film may occur, and the adherend may not be inspected accurately. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2017-32768 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention has been made to solve the above-mentioned conventional problems, and its main object is to provide a laminate film and a method for manufacturing a laminate film that can suppress erroneous detections caused by the laminate film even when attached to an adherend and subjected to optical inspection, and can accurately inspect the adherend. [Means for solving the problem]

[0006] [1] A laminated film according to one embodiment of the present invention includes a base film and a pressure-sensitive adhesive layer. The base film is made of a resin material. The pressure-sensitive adhesive layer is laminated on the base film. The base film has an in-plane retardation Re(550) of 10 nm or less. The unit area of ​​the base film is 10 cm. 2 The number of defects having a maximum Feret's diameter of 30 μm or more is eight or less. [2] In the laminated film described in [1] above, the peel force of the laminated film from the acrylic plate may be 3.0 N / 25 mm or less at a pulling speed of 30 m / min and a peel angle of 180°. [3] In the laminate film according to the above [1] or [2], the resin material may contain a polycarbonate-based resin and / or a cycloolefin-based resin. [4] A method for producing a laminated film according to another aspect of the present invention includes the steps of forming a base film made of a resin material and forming a pressure-sensitive adhesive layer on the base film, the step of forming the base film including the steps of melting the resin material, passing the molten resin material through a filter, and extruding the resin material after passing through the filter. [5] In the method for producing a laminated film according to the above item [4], the filter may be a screen mesh, in which case the opening of the screen mesh may be 0.035 mm to 0.070 mm. Effect of the Invention

[0007] According to the embodiments of the present invention, even when the laminate film is attached to an adherend and subjected to optical inspection, erroneous detection due to the laminate film can be suppressed, and the adherend can be inspected with high accuracy. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a schematic cross-sectional view of a laminated film according to one embodiment of the present invention. [Diagram 2]FIG. 2 is a schematic cross-sectional view of an optical member with a laminate film including the laminate film of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Representative embodiments of the present invention will be described below, but the present invention is not limited to these embodiments. In addition, in order to clarify the description, the width, thickness, shape, etc. of each part may be shown in a schematic manner compared to the embodiment, but these are merely examples and do not limit the interpretation of the present invention.

[0010] (Definition of terms and symbols) The definitions of terms and symbols used in this specification are as follows. (1) Refractive index (nx, ny, nz) "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the direction perpendicular to the slow axis in the plane (i.e., the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-plane phase difference (Re) "Re(λ)" is the in-plane retardation measured with light of wavelength λ nm at 23° C. For example, "Re(550)" is the in-plane retardation measured with light of wavelength 550 nm at 23° C. Re(λ) is calculated by the formula: Re(λ)=(nx-ny)×d, where d(nm) is the thickness of the layer (film). (3) Retardation in the thickness direction (Rth) "Rth(λ)" is the retardation in the thickness direction measured with light of wavelength λ nm at 23° C. For example, "Rth(550)" is the retardation in the thickness direction measured with light of wavelength 550 nm at 23° C. Rth(λ) is calculated by the formula: Rth(λ)=(nx-nz)×d, where d(nm) is the thickness of the layer (film).

[0011] A. Overall structure of laminated film FIG. 1 is a schematic cross-sectional view of a laminated film according to one embodiment of the present invention. The laminated film 100 in the illustrated example includes a base film 1 and a pressure-sensitive adhesive layer 2. The base film 1 is made of a resin material. The pressure-sensitive adhesive layer 2 is laminated on the base film 1. The in-plane retardation Re(550) of the base film 1 is 10 nm or less. The unit area of ​​the base film 1 is 10 cm 2 The number of defects with a maximum Feret diameter of 30 μm or more (hereinafter, D30 / 10 cm of the base film) 2 The number of defects is 8 or less. The method for measuring the number of defects will be described in the examples below. In-plane retardation Re(550) of the substrate film and D30 / 10cm of the substrate film 2 With such a combination, even if the laminate film is attached to an adherend and subjected to optical inspection, false detections due to the laminate film can be suppressed, and the adherend can be inspected with high accuracy. In other words, the result of inspecting the adherend with the laminate film attached can be matched with the result of inspecting the adherend alone.

[0012] Defects in the base film 1 include, for example, foreign matter such as fibers mixed in the resin material, gel-like matter formed by thermal crosslinking of the resin material, and air bubbles caused by moisture in the resin.

[0013] The in-plane retardation Re(550) of the base film 1 is preferably 5 nm or less, more preferably 3 nm or less. The lower limit of the in-plane retardation Re(550) of the base film 1 is typically 0 nm. When the in-plane retardation Re(550) of the base film is in this range, rainbow unevenness of the base film in optical inspection can be effectively suppressed, and as a result, the adherend can be inspected more accurately.

[0014] Base film D30 / 10cm 2 is preferably 5 or less, more preferably 3 or less, and even more preferably 1 or less. 2 The lower limit of is typically 0. D30 / 10cm of the base film 2If is in such a range, erroneous detection of defects in the base film in the optical inspection of the adherend can be suppressed, and as a result, the adherend can be inspected with even greater accuracy.

[0015] In addition, the unit area of ​​the base film 1 is 10 cm 2 The number of defects having a maximum Feret's diameter of less than 30 μm is not particularly limited. Unit area 10cm 2 The number of defects having a maximum Feret's diameter of 10 μm or more and less than 30 μm is, for example, 15 or less, preferably 10 or less. 2 The lower limit of the number of defects having a maximum Feret diameter of less than 30 μm and 10 μm or more is typically 0.

[0016] The peel force of the laminated film 100 from the acrylic plate is, for example, 3.5 N / 25 mm or less, preferably 3.0 N / 25 mm or less, more preferably 2.5 N / 25 mm or less, and even more preferably 2.0 N / 25 mm or less, at a pulling speed of 30 m / min and a peel angle of 180°. If the laminated film has such a peel force, the laminated film can be smoothly peeled from the adherend after optical inspection. On the other hand, the peel strength of the laminated film 100 from the acrylic plate is, for example, 0.5 N / 25 mm or more, preferably 1.0 N / 25 mm or more, and preferably 1.2 N / 25 mm or more. If the laminated film has such a peel strength, the laminated film can stably follow the surface of the adherend when the laminated film is attached to the adherend. The peel strength can be measured in accordance with JIS Z0237, and more specifically, can be measured by the following peel strength test. (peel strength test) A sample is prepared by cutting the laminated film into a strip of 25 mm x 100 mm; the sample is roll-pressed onto the surface of an acrylic plate via the adhesive layer at a pressure of 0.25 MPa and a feed rate of 0.3 m / min; the sample attached to the acrylic plate is left to stand in an environment with a temperature of 23°C and a relative humidity of 50% for 30 minutes, and then peeled at a peel angle of 180° and a tensile speed of 30 m / min in the same environment to measure the peel force.

[0017] The components of the laminated film will be described below.

[0018] B. Base film The base film 1 contains a resin material as a main component. Specific examples of the resin material include transparent resins such as cycloolefin (COP) resins such as polynorbornene resins, polyester resins such as polyethylene terephthalate (PET) resins, cellulose resins such as triacetyl cellulose (TAC), polycarbonate (PC) resins, (meth)acrylic resins, polyvinyl alcohol resins, polyamide resins, polyimide resins, polyethersulfone resins, polysulfone resins, polystyrene resins, polyolefin resins, and acetate resins. In addition, the base film 1 may include thermosetting resins or ultraviolet curing resins such as (meth)acrylic resins, urethane resins, (meth)acrylic urethane resins, epoxy resins, and silicone resins. The term "(meth)acrylic resin" refers to acrylic resins and / or methacrylic resins. In addition, glassy polymers such as siloxane polymers may also be used. In addition, the polymer films described in JP 2001-343529 A (WO01 / 37007) may also be used. The material of this film may be, for example, a resin composition containing a thermoplastic resin having a substituted or unsubstituted imide group in the side chain, and a thermoplastic resin having a substituted or unsubstituted phenyl group and a nitrile group in the side chain, such as a resin composition having an alternating copolymer of isobutene and N-methylmaleimide, and an acrylonitrile-styrene copolymer. The polymer film may be, for example, an extrusion product of the above resin composition. The materials of the resin film may be used alone or in combination.

[0019] In one embodiment, the resin material of the base film 1 is amorphous. When the base film is made of an amorphous resin material, excellent transparency can be imparted to the laminate film.

[0020] Of these resin materials, preferably, PC-based resin and COP-based resin are used, and more preferably, PC-based resin is used.

[0021] The PC resin contains at least a structural unit derived from a dihydroxy compound having a bond structure represented by the following structural formula (1), and has at least one bond structure -CH 2 PC resins are produced by reacting a dihydroxy compound containing at least a dihydroxy compound having -O- with a carbonic acid diester in the presence of a polymerization catalyst. In other words, PC resins contain structural units derived from the dihydroxy compound and carbonate groups derived from the carbonic acid diester. [ka]

[0022] Here, the dihydroxy compound having the bond structure represented by structural formula (1) is a compound having two alcoholic hydroxyl groups and a linking group -CH 2 Any compound having any structure can be used as long as it contains a structure having --O-- and can react with a carbonate diester in the presence of a polymerization catalyst to produce a polycarbonate, and two or more types of compounds may be used in combination.

[0023] In addition, a dihydroxy compound not having the bond structure represented by the above structural formula (1) may be used in combination as a dihydroxy compound for use in a PC resin. Hereinafter, a dihydroxy compound having the bond structure represented by structural formula (1) may be abbreviated as dihydroxy compound (A), and a dihydroxy compound not having the bond structure represented by structural formula (1) may be abbreviated as dihydroxy compound (B).

[0024] (Dihydroxy compound (A)) The linking group -CH in the dihydroxy compound (A) 2 "-O-" means a structure in which the linking group is bonded to an atom other than a hydrogen atom to form a molecule. In this linking group, the atom to which at least an oxygen atom can be bonded or the atom to which both a carbon atom and an oxygen atom can be bonded at the same time is preferably a carbon atom. 2 The number of "-O-" is preferably 1 or more, and more preferably 2 to 4.

[0025] Specific examples of the dihydroxy compound (A) include 9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isopropylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isobutylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butylphenyl)fluorene, and 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butylphenyl)fluorene. )-3-cyclohexylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3,5-dimethylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butyl-6-methylphenyl)fluorene, and 9,9-bis(4-(3-hydroxy-2,2-dimethylpropoxy)phenyl)fluorene;Bis[4-(2-hydroxyethoxy)phenyl]methane, bis[4-(2-hydroxyethoxy)phenyl]diphenylmethane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]ethane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]-1-phenylethane, 2,2-bis[4-(2-hydroxyethoxy)phenyl]propane, 2,2-bis[4-(2-hydroxyethoxy)-3-methylphenyl]propane, 2,2-bis[3,5-dimethyl-4-(2-hydroxyethoxy)phenyl] 1,1-bis[4-(2-hydroxyethoxy)phenyl]propane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]-3,3,5-trimethylcyclohexane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 1,4-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 1,3-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 2,2-bis[4-(2-hydroxyethoxy)-3-phenylphenyl]propane, 2,2-bis[(2-hydroxyethoxy)-3-phenylphenyl]propane, isopropylphenyl]propane, 2,2-bis[3-tert-butyl-4-(2-hydroxyethoxy)phenyl]propane, 2,2-bis[4-(2-hydroxyethoxy)phenyl]butane, 2,2-bis[4-(2-hydroxyethoxy)phenyl]-4-methylpentane, 2,2-bis[4-(2-hydroxyethoxy)phenyl]octane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]decane, 2,2-bis[3-bromo-4-(2-hydroxyethoxy)phenyl]propane bis(hydroxyalkoxyaryl)alkanes, such as 2,2-bis[3-cyclohexyl-4-(2-hydroxyethoxy)phenyl]propane; bis(hydroxyalkoxyaryl)cycloalkanes, such as 1,1-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 1,1-bis[3-cyclohexyl-4-(2-hydroxyethoxy)phenyl]cyclohexane, and 1,1-bis[4-(2-hydroxyethoxy)phenyl]cyclopentane;Dihydroxyalkoxy diaryl ethers, such as 4,4'-bis(2-hydroxyethoxy)diphenyl ether and 4,4'-bis(2-hydroxyethoxy)-3,3'-dimethyldiphenyl ether; bishydroxyalkoxy aryl sulfides, such as 4,4'-bis(2-hydroxyethoxyphenyl) sulfide and 4,4'-bis[4-(2-dihydroxyethoxy)-3-methylphenyl] sulfide; bishydroxyalkoxy aryl sulfoxides, such as 4,4'-bis(2-hydroxyethoxyphenyl) sulfone and 4,4'-bis[4-(2- bishydroxyalkoxyarylsulfones, such as 1,4-bishydroxyethoxybenzene, bishydroxyalkoxybenzenes, such as 1,3-bis[2-[4-(2-hydroxyethoxy)phenyl]propyl]benzene, 1,4-bis[2-[4-(2-hydroxyethoxy)phenyl]propyl]benzene, 4,4'-bis(2-hydroxyethoxy)biphenyl, 1,3-bis[4-(2-hydroxyethoxy)phenyl]-5,7-dimethyladamantane, anhydrous sugar alcohols, such as dihydroxy compounds represented by the following formula (2), and compounds having a cyclic ether structure, such as spiro glycols, such as those represented by the following general formula (3). The dihydroxy compounds (A) may be used alone or in combination.

[0026] [ka]

[0027] [ka]

[0028] Of these dihydroxy compounds (A), preferred is the dihydroxy compound represented by the above formula (2). Examples of the dihydroxy compound represented by the above formula (2) include isosorbide, isomannide, and isoidite, which are stereoisomeric, and these may be used alone or in combination of two or more. Among the dihydroxy compounds (A), isosorbide obtained by dehydration condensation of sorbitol produced from various starches, which are abundant and easily available as resources, is most preferred in terms of availability, ease of production, optical properties, and moldability.

[0029] The ratio of the structural units derived from the dihydroxy compound (A) to the total structural units derived from the dihydroxy compounds contained in the PC resin is, for example, 10 mol% or more, preferably 40 mol% or more, and more preferably 60 mol% or more. On the other hand, the ratio of the structural units derived from the dihydroxy compound (A) is, for example, 100 mol% or less, preferably 90 mol% or less, more preferably 80 mol% or less, and even more preferably 70 mol% or less. When the ratio of the dihydroxy compound (A) is within the above range, rainbow unevenness of the base film during optical inspection can be stably suppressed.

[0030] (Dihydroxy Compound (B)) As the dihydroxy compound that is the structural unit of the PC resin, dihydroxy compound (A) and dihydroxy compound (B) can be used together. By using dihydroxy compounds (A) and (B) in combination, rainbow unevenness of the base film during optical inspection can be more stably suppressed.

[0031] The dihydroxy compound (B) is typically a dihydroxy compound other than the dihydroxy compound (A). Examples of the dihydroxy compound (B) include alicyclic dihydroxy compounds, aliphatic dihydroxy compounds, oxyalkylene glycols, aromatic dihydroxy compounds, and diols having a cyclic ether structure. The dihydroxy compounds (B) may be used alone or in combination. Of the dihydroxy compounds (B), preferably, alicyclic dihydroxy compounds are used.

[0032] The alicyclic dihydroxy compound is not particularly limited, but preferably includes a compound having a 5-membered ring structure or a 6-membered ring structure. The 6-membered ring structure may be fixed to a chair or boat shape by a covalent bond. When the alicyclic dihydroxy compound has a 5-membered ring or a 6-membered ring structure, the heat resistance of the resulting PC resin can be improved. The number of carbon atoms contained in the alicyclic dihydroxy compound is, for example, 70 or less, preferably 50 or less, more preferably 30 or less.

[0033] Specific examples of the alicyclic dihydroxy compound containing a 5-membered ring structure or a 6-membered ring structure include alicyclic dihydroxy compounds represented by the following general formula (I) or (II). HOCH 2 -R 1 -CH 2 OH (I) H.O.R. 2 -OH (II) (In formulas (I) and (II), R 1 and R 2 Each of represents a cycloalkylene group having 4 to 20 carbon atoms.

[0034] Cyclohexanedimethanol, which is an alicyclic dihydroxy compound represented by the above general formula (I), is 1 is represented by the following general formula (Ia) (wherein R 3 represents an alkyl group having 1 to 12 carbon atoms or a hydrogen atom. Specific examples of such isomers include 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, and 1,4-cyclohexanedimethanol.

[0035] [ka]

[0036] The alicyclic dihydroxy compound represented by the above general formula (I), tricyclodecane dimethanol or pentacyclopentadecanedimethanol, is represented by the general formula (I), 1 is represented by the following general formula (Ib) (wherein n is 0 or 1):

[0037] [ka]

[0038] Decalin dimethanol or tricyclotetradecane dimethanol, which is an alicyclic dihydroxy compound represented by the above general formula (I), is a compound represented by the general formula (I) 1 is represented by the following general formula (Ic) (wherein m is 0 or 1). Specific examples of such isomers include 2,6-decalin dimethanol, 1,5-decalin dimethanol, and 2,3-decalin dimethanol.

[0039] [ka]

[0040] Norbornane dimethanol, which is an alicyclic dihydroxy compound represented by the above general formula (I), is 1 The isomers include various isomers represented by the following general formula (Id): Specific examples of such isomers include 2,3-norbornane dimethanol and 2,5-norbornane dimethanol.

[0041] [ka]

[0042] Adamantane dimethanol, which is an alicyclic dihydroxy compound represented by general formula (I), is 1The isomers include various isomers represented by the following general formula (Ie): A specific example of such isomers is 1,3-adamantanedimethanol.

[0043] [ka]

[0044] Cyclohexanediol, which is an alicyclic dihydroxy compound represented by the above general formula (II), is 2 is represented by the following general formula (IIa) (wherein R 3 represents an alkyl group having 1 to 12 carbon atoms or a hydrogen atom. Specific examples of such isomers include 1,2-cyclohexanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, and 2-methyl-1,4-cyclohexanediol.

[0045] [ka]

[0046] The alicyclic dihydroxy compound represented by the above general formula (II), tricyclodecanediol or pentacyclopentadecanediol, is a compound represented by the general formula (II), 2 is represented by the following general formula (IIb) (wherein n is 0 or 1):

[0047] [ka]

[0048] Decalindiol or tricyclotetradecanediol, which is an alicyclic dihydroxy compound represented by the above general formula (II), is a compound represented by the general formula (II) in which R 2is represented by the following general formula (IIc) (wherein m is 0 or 1). Specific examples of such isomers include 2,6-decalindiol, 1,5-decalindiol, and 2,3-decalindiol.

[0049] [ka]

[0050] Norbornanediol, which is an alicyclic dihydroxy compound represented by the above general formula (II), is 2 The isomers include various isomers represented by the following general formula (IId): Specific examples of such isomers include 2,3-norbornanediol and 2,5-norbornanediol.

[0051] [ka]

[0052] The adamantanediol, which is an alicyclic dihydroxy compound represented by the above general formula (II), is represented by the following general formula (II): 2 is represented by the following general formula (IIe): A specific example of such an isomer is 1,3-adamantanediol.

[0053] [ka]

[0054] Among the specific examples of the alicyclic dihydroxy compound described above, preferred are cyclohexanedimethanols, tricyclodecane dimethanols, adamantanediols, and pentacyclopentadecanedimethanols. From the viewpoints of availability and ease of handling, more preferred are 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,2-cyclohexanedimethanol, and tricyclodecane dimethanol, and even more preferred is tricyclodecane dimethanol.

[0055] The ratio of the structural units derived from the dihydroxy compound (B) to the total structural units derived from the dihydroxy compounds contained in the PC resin is, for example, 0 mol% or more, preferably 10 mol% or more, more preferably 20 mol% or more, and even more preferably 30 mol% or more. On the other hand, the ratio of the structural units derived from the dihydroxy compound (B) is, for example, 90 mol% or less, preferably 60 mol% or less, and more preferably 40 mol% or less.

[0056] Details of these PC resins are described, for example, in JP 2012-31370 A (Patent No. 5448264), the disclosure of which is incorporated herein by reference.

[0057] In one embodiment, the PC resin contains a structural unit derived from the dihydroxy compound (A) represented by the above formula (2), a structural unit derived from the alicyclic dihydroxy compound (B) represented by the above general formula (I), and a carbonate group linking them together. When the PC resin containing these structural units is applied to a base film, rainbow unevenness of the base film during optical inspection can be more stably suppressed. In such a PC resin, the molar ratio (A:B) of the structural unit derived from the dihydroxy compound (A) represented by the above formula (2) to the structural unit derived from the alicyclic dihydroxy compound (B) represented by the above general formula (I) is, for example, 5:5 to 9:1, and preferably 6:4 to 8:2. In such a PC resin, the combination of the dihydroxy compound (A) represented by the above formula (2) and the alicyclic dihydroxy compound (B) represented by the above general formula (I) is preferably a combination of isosorbide and tricyclodecane dimethanol.

[0058] The base film 1 may contain any suitable additive in addition to the above-mentioned resin material. Examples of the additive include antioxidants, UV absorbers, light stabilizers, nucleating agents, fillers, pigments, surfactants, and antistatic agents. Any suitable surface treatment layer may be provided on the surface of the base film 1 (the surface opposite to the pressure-sensitive adhesive layer 2). Examples of the surface treatment layer include an easy-adhesion layer, an easy-slip layer, an antiblocking layer, an antistatic layer, an antireflection layer, and an oligomer prevention layer.

[0059] The thickness of the substrate film 1 is, for example, 30 μm or more, preferably 40 μm or more. On the other hand, the thickness of the substrate film 1 is, for example, 130 μm or less, preferably 120 μm or less. If the thickness of the substrate film is in such a range, the substrate film can be given stiffness (elasticity) suitable for peeling off the laminated film. Therefore, the substrate film can be smoothly peeled off from the adherend. In addition, the in-plane retardation of the substrate film can be stably adjusted to the above range.

[0060] The trouser tear strength of the base film 1 is, for example, 0.09 N or more, preferably 0.10 N or more. The trouser tear strength of the base film 1 is, for example, 0.4 N or less, preferably 0.3 N or less. If the trouser tear strength of the base film is within such a range, the laminate film can be smoothly peeled off from the adherend, and the occurrence of tearing (cracking) in the laminate film can be suppressed when the laminate film is peeled off from the adherend. The trouser tear strength can be measured, for example, in accordance with JIS K7128-1.

[0061] Typically, the base film 1 is optically isotropic. In this specification, "optically isotropic" means that the in-plane retardation Re(550) of the base film 1 is in the above-mentioned range, and the retardation Rth(550) in the thickness direction of the base film 1 is in the range of, for example, -10 nm to +10 nm, or in the range of, for example, -5 nm to +5 nm.

[0062] The total light transmittance of the substrate film 1 is, for example, 80% or more, preferably 85% or more, more preferably 90% or more, and even more preferably 95% or more. The haze value of the base film 1 is, for example, 2.0% or less, preferably 1.5% or less, more preferably 1.0% or less, even more preferably 0.7% or less, particularly preferably 0.5% or less, and particularly preferably 0.3% or less. The lower limit of the haze value of the base film 1 is typically 0.05%. If the total light transmittance and / or haze value of the base film is within such range, the base film can be imparted with extremely excellent transparency, and as a result, the influence of the laminate film on optical inspection of the adherend can be reduced.

[0063] C.Adhesive layer The adhesive layer 2 is provided on the surface of the base film 1 in order to attach the laminate film 100 to the surface of an adherend. The adhesive layer 2 is made of an adhesive (pressure-sensitive adhesive).

[0064] Examples of adhesives constituting the adhesive layer 2 include (meth)acrylic adhesives, rubber adhesives, silicone adhesives, polyester adhesives, urethane adhesives, epoxy adhesives, and polyether adhesives. By adjusting the type, number, combination, and compounding ratio of monomers forming the base resin of the adhesive, as well as the compounding amount of the crosslinking agent, reaction temperature, reaction time, etc., an adhesive having desired properties according to the purpose can be prepared. The base resin of the adhesive may be used alone or in combination of two or more types.

[0065] In one embodiment, the pressure-sensitive adhesive layer 2 is composed of a (meth)acrylic pressure-sensitive adhesive (a (meth)acrylic pressure-sensitive adhesive composition). When the pressure-sensitive adhesive layer is composed of a (meth)acrylic pressure-sensitive adhesive, the peel force of the laminated film can be stably adjusted to within the above-mentioned range.

[0066] The (meth)acrylic pressure-sensitive adhesive composition typically contains a (meth)acrylic polymer as a main component. The content of the (meth)acrylic polymer in the solid content of the pressure-sensitive adhesive composition is, for example, 50% by mass or more, preferably 70% by mass or more, and more preferably 90% by mass or more. On the other hand, the upper limit of the content of the (meth)acrylic polymer is typically 100% by mass.

[0067] The (meth)acrylic polymer contains a structural unit derived from an alkyl (meth)acrylate. In the (meth)acrylic polymer, the content of the structural unit derived from an alkyl (meth)acrylate is, for example, 70% by mass or more, preferably 80% by mass or more. On the other hand, the upper limit of the content of the structural unit derived from an alkyl (meth)acrylate is typically 90% by mass. Examples of the alkyl group of the alkyl (meth)acrylate include linear or branched alkyl groups having 1 to 18 carbon atoms. The average number of carbon atoms in the alkyl group is preferably 3 to 12, and more preferably 3 to 8. Among the alkyl (meth)acrylates, preferred are butyl acrylate and 2-ethylhexyl acrylate, and more preferably 2-ethylhexyl acrylate.

[0068] The (meth)acrylic polymer may contain a structural unit derived from a copolymerizable monomer polymerizable with the alkyl (meth)acrylate, in addition to the structural unit derived from the alkyl (meth)acrylate. Examples of the copolymerizable monomer include a carboxyl group-containing monomer, a hydroxyl group-containing monomer, an amide group-containing monomer, an aromatic ring-containing (meth)acrylate, and a heterocyclic ring-containing vinyl monomer. The copolymerizable monomer may be used alone or in combination. Of the copolymerizable monomers, preferred are carboxyl group-containing monomers and hydroxyl group-containing monomers. In one embodiment, the (meth)acrylic polymer contains structural units derived from an alkyl (meth)acrylate, structural units derived from a carboxyl group-containing monomer, and structural units derived from a hydroxyl group-containing monomer.

[0069] The carboxyl group-containing monomer is a compound that contains a carboxyl group in its structure and a polymerizable unsaturated double bond such as a (meth)acryloyl group or a vinyl group. Examples of the carboxyl group-containing monomer include (meth)acrylic acid, carboxyethyl (meth)acrylate, maleic acid, fumaric acid, and crotonic acid, and preferably (meth)acrylic acid. When the (meth)acrylic polymer contains a structural unit derived from the carboxyl group-containing monomer, the adhesive properties of the adhesive layer can be improved.

[0070] When the (meth)acrylic polymer contains a structural unit derived from a carboxyl group-containing monomer, the content of the structural unit derived from the carboxyl group-containing monomer is, for example, 0.01% by mass or more, preferably 0.10% by mass or more. On the other hand, the content of the structural unit derived from the carboxyl group-containing monomer is, for example, 10% by mass or less, preferably 5.0% by mass or less, more preferably 1.0% by mass or less, and even more preferably 0.5% by mass or less.

[0071] The hydroxyl group-containing monomer is a compound that contains a hydroxyl group in its structure and a polymerizable unsaturated double bond such as a (meth)acryloyl group or a vinyl group. Examples of the hydroxyl group-containing monomer include 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)-methylacrylate, preferably 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate, more preferably 4-hydroxybutyl (meth)acrylate. When the (meth)acrylic polymer contains a structural unit derived from a hydroxyl group-containing monomer, the durability of the adhesive layer can be improved.

[0072] When the (meth)acrylic polymer contains a structural unit derived from a hydroxyl group-containing monomer, the content of the structural unit derived from the hydroxyl group-containing monomer is, for example, 0.01 mass% or more, preferably 1.0 mass% or more, more preferably 5.0 mass% or more, and even more preferably 8.0 mass% or more. The upper limit of the content of the structural unit derived from the hydroxyl group-containing monomer is typically 10 mass%.

[0073] The weight average molecular weight Mw of the (meth)acrylic polymer is, for example, from 100,000 to 2,000,000, and preferably from 200,000 to 1,000,000. The weight average molecular weight Mw can be calculated, for example, from the results of GPC measurement in terms of styrene.

[0074] In addition, the (meth)acrylic adhesive may contain a crosslinking agent. As the crosslinking agent, representative examples include organic crosslinking agents and polyfunctional metal chelates, and preferably organic crosslinking agents. As the organic crosslinking agent, for example, isocyanate crosslinking agents, peroxide crosslinking agents, epoxy crosslinking agents, and imine crosslinking agents are included, and more preferably, isocyanate crosslinking agents are included.

[0075] The content of the crosslinking agent is, for example, 0.01 parts by mass or more, preferably 0.5 parts by mass or more, more preferably 0.8 parts by mass or more, and even more preferably 1.2 parts by mass or more, relative to 100 parts by mass of the (meth)acrylic polymer. On the other hand, the content of the crosslinking agent is, for example, 10 parts by mass or less, preferably 5 parts by mass or less, more preferably 2.5 parts by mass or less, and even more preferably 2.0 parts by mass or less. When the content of the crosslinking agent is in this range, the peel force of the laminated film can be stably adjusted to the above range.

[0076] Furthermore, the (meth)acrylic pressure sensitive adhesive may contain various additives (for example, a silane coupling agent, a polymerization initiator, a solvent, a crosslinking catalyst) in an appropriate ratio. Details of these adhesives are described, for example, in JP 2006-183022 A, JP 2015-199942 A, JP 2018-053114 A, JP 2016-190996 A, and WO 2018 / 008712, the disclosures of which are incorporated herein by reference.

[0077] The thickness of the pressure-sensitive adhesive layer 2 is typically 1 μm or more, and preferably 5 μm or more. On the other hand, the thickness of the pressure-sensitive adhesive layer 2 is, for example, 30 μm or less, and preferably 15 μm or less.

[0078] The storage modulus of the pressure-sensitive adhesive layer 2 at 25° C. is, for example, 5.0×10 4 Pa~5.0×10 6 Pa, preferably 7.5×10 4 Pa~2.5×10 6 When the storage modulus of the pressure-sensitive adhesive layer is within such a range, the pressure-sensitive adhesive layer can have good wettability to an adherend and sufficient adhesive strength.

[0079] D. Release Liner The laminated film 100 may further include a release liner 3 in addition to the base film 1 and the pressure-sensitive adhesive layer 2. The release liner 3 is typically temporarily attached to the pressure-sensitive adhesive layer 2 until the laminated film is attached to an adherend, and is peeled off from the pressure-sensitive adhesive layer 2 when the laminated film is attached. The release liner 3 is formed of any appropriate resin film that can be used as a release liner. A release treatment layer may be provided on the surface of the release liner 3 that comes into contact with the pressure-sensitive adhesive layer 2.

[0080] E. Manufacturing method of laminated film The laminated film 100 described above can be produced by any appropriate method. In one embodiment, the method for producing the laminated film includes a step of forming a base film 1 (film formation step) and a step of forming a pressure-sensitive adhesive layer 2 on the base film 1 (pressure-sensitive adhesive layer formation step).

[0081] The film-forming process typically includes a step of melting the above-mentioned resin material (melting step); a step of passing the molten resin material (hereinafter referred to as molten resin) through a filter (filtering step); and a step of extruding the molten resin after passing through the filter (extrusion step).

[0082] The resin material subjected to the melting step may have any suitable shape. In one embodiment, the resin material is pelletized in advance. The method of pelletizing the resin material is not particularly limited, and may be a strand cut method or a hot cut method. Details of the pellet preparation step are described in, for example, JP 2013-181105 A. The description of this patent document is incorporated herein by reference.

[0083] In the melting step, the resin material (typically pellets) is heated and melted. Any appropriate heating temperature may be adopted depending on the resin material. As a result, a molten resin is obtained by melting the resin material.

[0084] In the filter passing step, the molten resin is passed through a filter, whereby foreign matter contained in the molten resin can be removed from the molten resin.

[0085] The filter may have any suitable configuration, and examples of the filter include a screen mesh and a disk filter, and preferably a screen mesh. The mesh size of the screen mesh is, for example, 0.080 mm or less, preferably 0.070 mm or less, and more preferably 0.055 mm or less. When the screen mesh has such mesh size, it is possible to prevent foreign matter having a maximum Feret's diameter of 30 μm or more from being mixed into the substrate film to be formed. Therefore, defects in the substrate film (specifically, foreign matter) can be reduced, and the D30 / 10 cm of the substrate film can be reduced. 2 can be stably adjusted to the above range. On the other hand, the opening of the screen mesh is, for example, 0.025 mm or more, preferably 0.035 mm or more. When the screen mesh has such openings, the molten resin can smoothly pass through the screen mesh. Therefore, the molten resin can be prevented from being retained and from being excessively heated. This can prevent the generation of gel-like matter due to thermal crosslinking of the molten resin. As a result, defects in the base film (specifically, gel-like matter) can be reduced, and the D30 / 10cm of the base film can be improved. 2 can be adjusted more stably within the above range.

[0086] In the extrusion molding step, the molten resin that has passed through the filter is typically extruded into a film shape using a die. This prepares the substrate film 1. Such a film-forming process can be carried out by any appropriate film-forming device.

[0087] Next, in the pressure-sensitive adhesive layer forming step, a pressure-sensitive adhesive layer 2 is formed on the obtained base film 1. Any appropriate means may be adopted as a method for forming the pressure-sensitive adhesive layer. To form the pressure-sensitive adhesive layer 2 on the base film 1, for example, the above-mentioned pressure-sensitive adhesive may be directly applied to the base film 1, or a pressure-sensitive adhesive may be applied to another base material to form a pressure-sensitive adhesive layer, which is then transferred to the base film 1. In this manner, the laminated film 100 is manufactured.

[0088] F. Applications of laminated film The laminated films described in the above items A to E are used by being attached to the surface of various adherends. Examples of the adherends include optical members and electronic members, and preferably optical members. Representative examples of the optical members include polarizing plates, retardation films, optical laminates containing polarizing plates and / or retardation films, displays, imaging devices, lenses, and (half) mirrors.

[0089] In one embodiment, the laminate film 100 is a film with an adhesive layer and can be suitably used as a surface protection film. In this case, the laminate film 100 is attached to the surface of an adherend and can protect the surface of the adherend during inspection, processing, and / or transportation of the adherend.

[0090] Fig. 2 is a schematic cross-sectional view of an optical member with a laminate film including the laminate film of Fig. 1. The illustrated example of the optical member with a laminate film 200 includes an optical member 5 as an adherend and a laminate film 100 as a surface protective film. The laminate film 100 is attached to the surface of the optical member 5 by a pressure-sensitive adhesive layer 2.

[0091] In one embodiment, the optical member 5 included in the laminate film-attached optical member 200 is a polarizing plate. The polarizing plate has a thickness of, for example, 5 μm to 200 μm. The thickness of the base film 1 of the laminate film 100 is, for example, 0.1 to 1.05, and preferably 0.15 to 1.0, relative to the thickness of the adherend (optical member). If the thickness ratio of the base film to the adherend is within this range, the adherend (optical member) can be inspected with even greater accuracy even when the laminate film is attached to the adherend and subjected to optical inspection.

[0092] Such an optical member 200 with a laminated film is typically subjected to optical inspection. The optical inspection is not particularly limited, and may be, for example, an automated optical inspection (AOI). Examples of the automated optical inspection include a foreign body inspection for inspecting foreign bodies contained in an optical member, and an air bubble inspection for inspecting air bubbles contained in an optical member. In such optical inspection, false detections caused by the laminated film are sufficiently suppressed, so that the optical member can be inspected with high accuracy even in a state where the laminated film is attached to the optical member.

[0093] Thereafter, the laminated film 100 can be peeled off and removed from the surface of the optical member 5 at a desired timing. EXAMPLES

[0094] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring the various properties are as follows.

[0095] (1) Measuring the number of defects on the base film The substrate films used in the examples and comparative examples were measured using an optical microscope to determine the area of ​​the film. 2 The number of defects with a maximum Feret's diameter of 30 μm or more was measured. The results are shown in Table 1.

[0096] (2) Rainbow unevenness on the base film The substrate film used in the examples and comparative examples was placed between two polarizing plates in a crossed Nicol state. The substrate film was placed so that the length direction of the substrate film was parallel to the transmission axis direction of one of the polarizing plates. In this state, fluorescent light was irradiated from below the lower polarizing plate, and the presence or absence of rainbow unevenness was visually observed. The results are shown in Table 1. Furthermore, when a laminate film having a base film on which rainbow unevenness may occur is attached to an adherend and subjected to automated optical inspection (AOI), the accuracy of the optical inspection of the adherend may decrease.

[0097] (3) Automatic foreign body inspection The number of foreign objects contained in an area of ​​10 cm x 10 cm in the laminated films obtained in the examples and comparative examples was counted based on the method described in JP 2021-135219 A. The results of the automatic foreign matter inspection were then evaluated according to the following criteria. The results are shown in Table 1. 〇: 5 foreign objects over 30μm / 10cm 2 below ×: 6 foreign objects over 30μm / 10cm 2 End

[0098] <<Preparation Example 1: Adhesive Composition>> In a reaction vessel equipped with a thermometer, a stirrer, a cooler and a nitrogen gas inlet tube, 100 parts by mass of 2-ethylhexyl acrylate (2EHA), 10 parts by mass of 4-hydroxybutyl acrylate (4HBA), 0.02 parts by mass of acrylic acid (AA), and 0.2 parts by mass of 2,2'-azobisisobutyronitrile (AIBN) as a polymerization initiator were charged together with 157 parts by mass of ethyl acetate, and nitrogen gas was introduced while gently stirring at 23°C to perform nitrogen substitution. Thereafter, the liquid temperature was kept at around 65°C and a polymerization reaction was carried out for 6 hours to prepare a solution of (meth)acrylic polymer A (concentration 40% by mass). The weight average molecular weight of acrylic polymer A was 540,000.

[0099] Ethyl acetate was added to the solution of acrylic polymer A to dilute it to a concentration of 20% by mass. 1.5 parts by mass of an isocyanurate of hexamethylene diisocyanate ("Coronate HX" manufactured by Tosoh Corporation) as a crosslinking agent and 3 parts by mass (solid content 0.03 parts by mass) of dibutyltin dilaurate (1% by mass solution in ethyl acetate) as a crosslinking catalyst were added to 500 parts by mass of this solution (solid content 100 parts by mass) and stirred to prepare a pressure-sensitive adhesive composition.

[0100] <<Preparation Example 2: PC Resin Film>> 81.98 parts by mass of isosorbide (ISB), 47.19 parts by mass of tricyclodecane dimethanol (TCDDM), 175.1 parts by mass of diphenyl carbonate (DPC), and 0.979 parts by mass of cesium carbonate 0.2% by mass aqueous solution as a catalyst were charged into a reaction vessel, and in a nitrogen atmosphere, the temperature of the heating vessel was heated to 150°C as the first step of the reaction, and the raw materials were dissolved (about 15 minutes) while stirring as necessary. Next, the pressure was changed from normal pressure to 13.3 kPa, and the temperature of the heating vessel was raised to 190°C in one hour, while the generated phenol was extracted outside the reaction vessel. After the entire reaction vessel was kept at 190°C for 15 minutes, the pressure in the reaction vessel was changed to 6.67 kPa, the temperature of the heating vessel was raised to 230°C in 15 minutes, and the generated phenol was extracted outside the reaction vessel as the second step. As the stirring torque of the stirrer increased, the temperature was raised to 250°C in 8 minutes, and the pressure inside the reaction vessel was lowered to 0.200 kPa or less in order to remove the phenol that was generated. After the predetermined stirring torque was reached, the reaction was terminated and the reaction product was extruded into water to obtain pellets of PC resin.

[0101] [Example 1, Comparative Examples 2 and 3] The PC resin pellets obtained in Preparation Example 2 were vacuum-dried at 100°C for 12 hours and then fed to a film-forming device. The film-forming device was equipped with a single-screw extruder (manufactured by Toshiba Machine Co., Ltd., cylinder temperature setting: 250°C), a filter shown in Table 1, a T-die (width 1700 mm, temperature setting: 250°C), a cast roll (temperature setting: 60°C), and a winder. More specifically, the pellets were fed to a single-screw extruder and heated to melt. The molten PC resin was then extruded from the single-screw extruder and passed through a filter and a T-die in this order. This produced a PC resin film with a thickness of 40 μm. The PC resin film passed through a cast roll and was then wound up by a winder. Next, the adhesive composition of Preparation Example 1 was applied to the release-treated surface of a release liner (a 25 μm-thick biaxially oriented polyethylene terephthalate film with one side treated with silicone release) and heated at 130° C. for 20 seconds to form an adhesive layer with a thickness of 10 μm. This adhesive layer was bonded to the corona-treated surface of a PC resin film with one side corona-treated to obtain a laminated film.

[0102] [Example 2] A laminated film was obtained in the same manner as in Example 1, except that the pellets of the PC resin obtained in Preparation Example 2 were changed to pellets of a COP resin.

[0103] [Comparative Example 1] A laminated film was obtained in the same manner as in Example 1, except that the pellets of the PC resin obtained in Preparation Example 2 were changed to pellets of PET.

[0104] [Table 1]

[0105] [evaluation] As is clear from Table 1, when the in-plane retardation Re(550) of the base film and the number of defects of 30 μm or more in the base film are adjusted as described above, even if the laminate film is attached to an adherend and subjected to optical inspection, erroneous detection due to the laminate film can be suppressed, and the adherend can be inspected accurately. [Industrial Applicability]

[0106] The laminated film of the present invention can be applied to various industrial products, and can be particularly suitably used for optical products that are subjected to optical inspection. [Explanation of symbols]

[0107] 1. Base film 2 Adhesive layer 100 Laminated Film

Claims

1. A base film made of a resin material; A pressure-sensitive adhesive layer laminated on the base film, The in-plane retardation Re(550) of the base film is 10 nm or less, The unit area of ​​the base film is 10 cm 2 The laminated film has eight or less defects having a maximum Feret's diameter of 30 μm or more.

2. 2. The laminated film according to claim 1, which has a peel force from an acrylic plate of 3.0 N / 25 mm or less at a tensile speed of 30 m / min and a peel angle of 180°.

3. The laminated film according to claim 1 , wherein the resin material contains a polycarbonate-based resin and / or a cycloolefin-based resin.

4. A step of forming a substrate film made of a resin material; forming a pressure-sensitive adhesive layer on the base film; The step of forming the base film includes: Melting the resin material; Passing the molten resin material through a filter; and extrusion molding the resin material after passing through the filter.

5. The filter is a screen mesh, The method for producing a laminated film according to claim 4, wherein the opening of the screen mesh is 0.035 mm to 0.070 mm.

Citation Information

Patent Citations

  • Optical film

    JP2008225286A

  • Surface protection film and its production process

    JP2009113481A

  • Production method of optical film

    JP2016203384A

  • Surface protective film and optical member having protective film

    JP2019099751A

  • Method for manufacturing film

    JP2019202482A