Resin film, laminated film and method for producing resin film
The resin film with a controlled anti-blocking agent content and properties addresses blocking and optical deterioration issues, ensuring high transmittance and low haze, suitable for optical applications.
Patent Information
- Application Number
- JP2023057971
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Resin films without a release liner suffer from blocking due to adhesion and deteriorated optical properties when anti-blocking agents are added, necessitating a solution that maintains both anti-blocking and optical qualities.
A resin film with an anti-blocking agent dispersed at 350 ppm to 3000 ppm, refractive index difference of 0.10 or less, and average primary particle diameter of 0.1 μm to 1.3 μm, along with specific optical and mechanical properties, is produced using a method involving mixing, filtering, and extrusion.
The resin film achieves excellent anti-blocking properties, maintaining high total light transmittance and low haze, suitable for optical applications without forming dents during winding and reducing false detections in optical inspections.
Smart Images

Figure 2024145564000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin film, a laminated film, and a method for producing a resin film. [Background technology]
[0002] Resin films are widely used in various industrial products. For example, it is known that resin films are used as surface protection films for protecting the surface of an adherend (see, for example, Patent Document 1).
[0003] Such a resin film is generally collected by winding it up into a roll with a release liner attached to its surface. However, when the resin film with the release liner attached is wound up into a roll, the unevenness of the release liner may be transferred to the resin film, forming dents in the resin film.
[0004] For this reason, winding up the resin film without attaching a release liner has been considered. However, when a resin film is wound into a roll without a release liner (release linerless), there is a risk of blocking, in which the resin films stick to each other. In this regard, although it is possible to impart antiblocking properties to the resin film by incorporating an antiblocking agent (hereinafter referred to as an AB agent) into the resin film, the optical properties of the resin film may deteriorate. For this reason, it is desirable for the resin film to have both excellent antiblocking properties and optical properties. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2017-32768 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made to solve the above-mentioned conventional problems, and its main object is to provide a resin film, a laminate film, and a method for producing a resin film that can simultaneously achieve excellent anti-blocking properties and optical properties. [Means for solving the problem]
[0007] [1] A resin film according to one embodiment includes a resin material as a matrix and an antiblocking agent dispersed in the resin material. The content of the antiblocking agent in the resin film is 350 ppm to 3000 ppm. The absolute value of the refractive index difference between the resin material and the antiblocking agent is 0.10 or less. [2] In the resin film described in the above [1], the refractive index of the antiblocking agent may be equal to or lower than the refractive index of the resin material. [3] In the resin film according to the above [1] or [2], the average primary particle size of the antiblocking agent may be 0.1 μm to 1.3 μm. [4] The resin film according to any one of the above [1] to [3] may have an indentation modulus at 25° C. of 2.0 N to 6.5 N. [5] In the resin film according to any one of the above [1] to [4], the dynamic friction coefficient may be 1.0 or less. [6] In the resin film according to any one of the above [1] to [5], the total light transmittance may be 90% or more and the haze value may be 1.0% or less. [7] In the resin film according to any one of the above [1] to [6], an in-plane retardation Re(550) may be 10 nm or less. [8] In the resin film according to any one of [1] to [7] above, the resin material may contain a polycarbonate-based resin. [9] A laminate film in another aspect of the present invention includes the resin film according to any one of [1] to [8] above, and a pressure-sensitive adhesive layer laminated on the resin film.
[10] In still another aspect of the present invention, a method for producing a resin film includes the steps of: mixing a molten resin material with an antiblocking agent to prepare a resin composition; passing the resin composition through a filter; and extrusion molding the resin composition after passing through the filter. The content of the antiblocking agent in the resin composition is 350 ppm to 3000 ppm. The difference in refractive index between the resin material and the antiblocking agent is 0.10 or less.
[11] In the method for producing a resin film according to the above
[10] , the filter may be a screen mesh, and the opening of the screen mesh may be 0.035 mm to 0.070 mm.
[12] The method for producing a resin film according to
[10] or
[11] above may further include a step of winding up the resin film using a winding member. Effect of the Invention
[0008] According to the embodiments of the present invention, it is possible to realize a resin film and a laminate film that can simultaneously achieve excellent antiblocking properties and optical properties. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a schematic cross-sectional view of a resin film according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view of a laminated film according to another embodiment of the present invention. [Diagram 3] FIG. 3 is a schematic cross-sectional view of an optical member with a laminate film including the laminate film of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Representative embodiments of the present invention will be described below, but the present invention is not limited to these embodiments. In addition, in order to clarify the description, the width, thickness, shape, etc. of each part may be shown in a schematic manner compared to the embodiment, but these are merely examples and do not limit the interpretation of the present invention.
[0011] (Definition of terms and symbols) The definitions of terms and symbols used in this specification are as follows. (1) Refractive index (nx, ny, nz) "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the direction perpendicular to the slow axis in the plane (i.e., the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-plane phase difference (Re) "Re(λ)" is the in-plane retardation measured with light of wavelength λ nm at 23° C. For example, "Re(550)" is the in-plane retardation measured with light of wavelength 550 nm at 23° C. Re(λ) is calculated by the formula: Re(λ)=(nx-ny)×d, where d(nm) is the thickness of the layer (film). (3) Retardation in the thickness direction (Rth) "Rth(λ)" is the retardation in the thickness direction measured with light of wavelength λ nm at 23° C. For example, "Rth(550)" is the retardation in the thickness direction measured with light of wavelength 550 nm at 23° C. Rth(λ) is calculated by the formula: Rth(λ)=(nx-nz)×d, where d(nm) is the thickness of the layer (film).
[0012] A. Overall composition of resin film FIG. 1 is a schematic cross-sectional view of a resin film according to one embodiment of the present invention. The resin film 1 in the illustrated example contains a resin material as a matrix and an antiblocking agent (hereinafter, referred to as AB agent) dispersed in the resin material. The content (by mass) of the AB agent in the resin film 1 is 350 ppm to 3000 ppm. The absolute value of the refractive index difference between the resin material and the AB agent is 0.10 or less. When the content ratio of the AB agent and the absolute value of the refractive index difference between the resin material and the AB agent are within such ranges, the resin film can be given excellent anti-blocking properties and the light diffusion caused by the AB agent can be suppressed. Therefore, the total light transmittance of the resin film can be improved and the haze can be reduced. In other words, a resin film that has both excellent anti-blocking properties and optical properties can be realized.
[0013] The content (by mass) of the AB agent in the resin film 1 is preferably 500 ppm to 3000 ppm, more preferably 500 ppm to 2000 ppm, and further preferably 500 ppm to 1500 ppm. When the content of the AB agent is within this range, sufficient anti-blocking properties can be imparted to the resin film.
[0014] The absolute value of the refractive index difference between the resin material and the AB agent is preferably 0.08 or less, more preferably 0.06 or less, and further preferably 0.04 or less. The lower limit of the absolute value of the refractive index difference between the resin material and the AB agent is typically 0. When the absolute value of the refractive index difference between the resin material and the AB agent is within such a range, the total light transmittance can be further improved and the haze can be further reduced in the resin film.
[0015] In one embodiment, the refractive index of the AB agent is equal to or lower than the refractive index of the resin material. When the refractive index of the AB agent is equal to or lower than the refractive index of the resin material and the refractive index difference between the resin material and the AB agent is within the above range, the total light transmittance of the resin film can be further improved and the haze can be further reduced.
[0016] The refractive index of the AB agent is, for example, 1.35 or more, preferably 1.40 or more, more preferably 1.45 or more. On the other hand, the refractive index of the AB agent is, for example, 1.65 or less, preferably 1.60 or less, more preferably 1.55 or less. The refractive index of the AB agent can be measured at 25°C using light with a wavelength of 590 nm, for example, in accordance with JIS K7142. The refractive index of the resin material is, for example, 1.40 or more, preferably 1.45 or more, more preferably 1.48 or more. On the other hand, the refractive index of the resin material is, for example, 1.70 or less, preferably 1.65 or less, more preferably 1.60 or less. The refractive index of the resin material can be measured at 25° C. using light with a wavelength of 590 nm, for example, in accordance with JIS K7142.
[0017] The dynamic friction coefficient of the resin film 1 is, for example, 1.2 or less, and preferably 1.0 or less. On the other hand, the lower limit of the dynamic friction coefficient of the resin film 1 is typically 0.2. The dynamic friction coefficient of the resin film is measured, for example, in accordance with JIS K7142. If the dynamic friction coefficient of the resin film is within this range, excellent anti-blocking properties can be stably imparted to the resin film.
[0018] As described above, the resin film 1 has excellent anti-blocking properties. Therefore, the resin film 1 can be typically wound into a roll without a release liner. This can prevent dents from being formed on the resin film even when the resin film is wound into a roll.
[0019] The indentation elastic modulus of the resin film 1 at 25° C. is, for example, 2.0 N to 6.5 N, or for example, 2.5 N to 6.0 N. The indentation elastic modulus of the resin film can be measured by a nanoindentation method. Even if the resin film has an indentation modulus in this range, dents in the resin film can be sufficiently suppressed by winding the resin film without a release liner.
[0020] The total light transmittance of the resin film 1 is, for example, 90.0% or more, more preferably 91.0% or more, and even more preferably 92.0% or more. The upper limit of the total light transmittance of the resin film 1 is typically 100%. The total light transmittance of the resin film can be measured in accordance with JIS R3106-2019. The haze value of the resin film 1 is, for example, 1.0% or less, preferably 0.90% or less, more preferably 0.80% or less, and further preferably 0.70% or less. The lower limit of the haze value of the resin film 1 is typically 0%. The haze value of the resin film can be measured in accordance with JIS K7136.
[0021] The resin film 1 can be used in any suitable application, and can be particularly suitably employed as an optical film that requires excellent optical properties. Examples of optical films include a protective layer attached to a polarizer, a raw film used in the manufacture of a retardation film, and a base film of a laminated film that requires optical properties.
[0022] B. Overall structure of laminated film 2, in one embodiment, the resin film 1 is provided as a base film in a laminate film 100. The laminate film 100 in the illustrated example is a film with an adhesive layer, and includes an adhesive layer 2 in addition to the resin film 1. The adhesive layer 2 is laminated on the resin film 1.
[0023] The laminated film 100 may further include a release liner 3 in addition to the resin film 1 and the pressure-sensitive adhesive layer 2. The release liner 3 is typically temporarily attached to the pressure-sensitive adhesive layer 2 until the laminated film is attached to an adherend, and is peeled off from the pressure-sensitive adhesive layer 2 when the laminated film is attached. The release liner 3 is formed of any appropriate resin film that can be used as a release liner. A release treatment layer may be provided on the surface of the release liner 3 that comes into contact with the pressure-sensitive adhesive layer 2.
[0024] Typically, the laminated film 100 including the release liner 3 can be wound into a roll. Since the resin film has excellent anti-blocking properties, when the laminated film including the release liner is wound into a roll, even if the resin film and the release liner come into contact with each other, the occurrence of blocking, in which they stick to each other, can be suppressed.
[0025] As shown in Fig. 3, the laminate film 100 can be suitably used as a surface protection film. In this case, the laminate film 100 is attached to the surface of various adherends 5, and can protect the surface of the adherend during inspection, processing, and / or transportation of the adherend. The laminate film 100 is typically attached to the surface of the adherend 5 by the pressure-sensitive adhesive layer 2. As will be described in detail later, there are cases where the adherend is subjected to optical inspection with the laminate film attached to the adherend. In this case, since the resin film has excellent optical properties as described above, even if the laminate film is attached to the adherend and subjected to optical inspection, erroneous detection due to the resin film can be suppressed, and as a result, the adherend can be inspected with high accuracy. In other words, the result of inspecting the adherend with the laminate film attached can be matched with the result of inspecting only the adherend.
[0026] The resin film and the pressure-sensitive adhesive layer will be described in detail below.
[0027] C. Resin film The resin film 1 typically has optical isotropy. In this specification, the term "optically isotropic" means that the in-plane retardation Re(550) and the retardation Rth(550) in the thickness direction are within the following ranges. The in-plane retardation Re(550) of the resin film 1 is, for example, 10 nm or less, preferably 5 nm or less, and more preferably 3 nm or less. On the other hand, the lower limit of the in-plane retardation Re(550) of the resin film 1 is typically 0 nm. If the in-plane retardation Re(550) of the resin film is within this range, rainbow unevenness of the resin film during optical inspection can be effectively suppressed, and as a result, the inspection accuracy of the adherend can be improved. The resin film 1 has a thickness direction retardation Rth(550) of, for example, −10 nm to +10 nm, and preferably −5 nm to +5 nm.
[0028] Unit area of resin film 1: 10cm 2 The number of defects with a maximum Feret diameter of 30 μm or more (hereinafter, D30 / 10 cm of the resin film) 2The number of the resin film particles is, for example, 5 or less, and preferably 3 or less. 2 The lower limit is typically 0. The number of defects can be measured using an optical microscope. Resin film D30 / 10cm 2 If is within such a range, false detections caused by the resin film can be stably suppressed in optical inspection of the adherend, and as a result, the inspection accuracy of the adherend can be improved. The unit area of resin film 1 is 10 cm 2 The number of defects having a maximum Feret's diameter of less than 30 μm is not particularly limited.
[0029] Defects in the resin film 1 include, for example, aggregates of the AB agent described above; foreign matter such as fibers mixed into the resin material; gel-like matter formed by thermal crosslinking of the resin material; and air bubbles caused by moisture in the resin.
[0030] The thickness of the resin film 1 is, for example, 30 μm or more, preferably 40 μm or more. On the other hand, the thickness of the resin film 1 is, for example, 130 μm or less, preferably 120 μm or less. If the thickness of the resin film is in such a range, the resin film can be given stiffness (elasticity) suitable for peeling off the laminated film. Therefore, the resin film can be smoothly peeled off from the adherend. In addition, the in-plane retardation of the resin film can be stably adjusted to the above range.
[0031] The trouser tear strength of the resin film 1 is, for example, 0.09 N or more, preferably 0.10 N or more. The trouser tear strength of the resin film 1 is, for example, 0.4 N or less, preferably 0.3 N or less. If the trouser tear strength of the resin film is within such a range, the laminate film can be smoothly peeled off from the adherend, and the occurrence of tearing (cracking) in the laminate film when the laminate film is peeled off from the adherend can be suppressed. The trouser tear strength can be measured, for example, in accordance with JIS K7128-1.
[0032] C-1.Resin material The resin film 1 contains a resin material as a main component. Specific examples of the resin material include transparent resins such as cycloolefin (COP) resins such as polynorbornene resins, polyester resins such as polyethylene terephthalate (PET) resins, cellulose resins such as triacetyl cellulose (TAC), polycarbonate (PC) resins, (meth)acrylic resins, polyvinyl alcohol resins, polyamide resins, polyimide resins, polyethersulfone resins, polysulfone resins, polystyrene resins, polyolefin resins, and acetate resins. In addition, the resins may include thermosetting resins or ultraviolet curing resins such as (meth)acrylic resins, urethane resins, (meth)acrylic urethane resins, epoxy resins, and silicone resins. The term "(meth)acrylic resin" refers to acrylic resins and / or methacrylic resins. In addition, glassy polymers such as siloxane polymers may also be used. Polymers described in JP 2001-343529 A (WO01 / 37007) may also be used. As the material of this polymer, for example, a resin composition containing a thermoplastic resin having a substituted or unsubstituted imide group in the side chain and a thermoplastic resin having a substituted or unsubstituted phenyl group and a nitrile group in the side chain can be used, for example, a resin composition containing an alternating copolymer of isobutene and N-methylmaleimide and an acrylonitrile-styrene copolymer. The materials of the resin film can be used alone or in combination.
[0033] In one embodiment, the resin material of the resin film 1 is amorphous. When the resin film is made of an amorphous resin material, excellent transparency can be imparted to the resin film.
[0034] Of these resin materials, preferably, PC-based resin and COP-based resin are used, and more preferably, PC-based resin is used.
[0035] In one embodiment, the PC resin contains at least a structural unit derived from a dihydroxy compound having a bond structure represented by the following structural formula (1), and is produced by reacting a dihydroxy compound containing at least a dihydroxy compound having at least one bond structure -CH2-O- in the molecule with a carbonate diester in the presence of a polymerization catalyst. In other words, the PC resin contains a structural unit derived from a dihydroxy compound and a carbonate group derived from a carbonate diester. [ka]
[0036] Here, as the dihydroxy compound having a bond structure represented by structural formula (1), any compound can be used as long as it has two alcoholic hydroxyl groups, contains a structure having a linking group -CH2-O- in the molecule, and can react with a carbonate diester in the presence of a polymerization catalyst to produce a polycarbonate, and multiple types of compounds can be used in combination.
[0037] In addition, a dihydroxy compound not having the bond structure represented by the above structural formula (1) may be used in combination as a dihydroxy compound for use in a PC resin. Hereinafter, a dihydroxy compound having the bond structure represented by structural formula (1) may be abbreviated as dihydroxy compound (A), and a dihydroxy compound not having the bond structure represented by structural formula (1) may be abbreviated as dihydroxy compound (B).
[0038] (Dihydroxy compound (A)) The "linking group -CH2-O-" in the dihydroxy compound (A) means a structure that bonds with atoms other than hydrogen atoms to form a molecule. In this linking group, the atom to which at least an oxygen atom can be bonded or the atom to which a carbon atom and an oxygen atom can be bonded simultaneously is preferably a carbon atom. The number of "linking groups -CH2-O-" in the dihydroxy compound (A) is preferably 1 or more, more preferably 2 to 4.
[0039] Specific examples of the dihydroxy compound (A) include 9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isopropylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isobutylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butylphenyl)fluorene, and 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butylphenyl)fluorene. )-3-cyclohexylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3,5-dimethylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butyl-6-methylphenyl)fluorene, and 9,9-bis(4-(3-hydroxy-2,2-dimethylpropoxy)phenyl)fluorene;Bis[4-(2-hydroxyethoxy)phenyl]methane, bis[4-(2-hydroxyethoxy)phenyl]diphenylmethane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]ethane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]-1-phenylethane, 2,2-bis[4-(2-hydroxyethoxy)phenyl]propane, 2,2-bis[4-(2-hydroxyethoxy)-3-methylphenyl]propane, 2,2-bis[3,5-dimethyl-4-(2-hydroxyethoxy)phenyl] 1,1-bis[4-(2-hydroxyethoxy)phenyl]propane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]-3,3,5-trimethylcyclohexane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 1,4-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 1,3-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 2,2-bis[4-(2-hydroxyethoxy)-3-phenylphenyl]propane, 2,2-bis[(2-hydroxyethoxy)-3-phenylphenyl]propane, isopropylphenyl]propane, 2,2-bis[3-tert-butyl-4-(2-hydroxyethoxy)phenyl]propane, 2,2-bis[4-(2-hydroxyethoxy)phenyl]butane, 2,2-bis[4-(2-hydroxyethoxy)phenyl]-4-methylpentane, 2,2-bis[4-(2-hydroxyethoxy)phenyl]octane, 1,1-bis[4-(2-hydroxyethoxy)phenyl]decane, 2,2-bis[3-bromo-4-(2-hydroxyethoxy)phenyl]propane bis(hydroxyalkoxyaryl)alkanes, such as 2,2-bis[3-cyclohexyl-4-(2-hydroxyethoxy)phenyl]propane; bis(hydroxyalkoxyaryl)cycloalkanes, such as 1,1-bis[4-(2-hydroxyethoxy)phenyl]cyclohexane, 1,1-bis[3-cyclohexyl-4-(2-hydroxyethoxy)phenyl]cyclohexane, and 1,1-bis[4-(2-hydroxyethoxy)phenyl]cyclopentane;Dihydroxyalkoxy diaryl ethers, such as 4,4'-bis(2-hydroxyethoxy)diphenyl ether and 4,4'-bis(2-hydroxyethoxy)-3,3'-dimethyldiphenyl ether; bishydroxyalkoxy aryl sulfides, such as 4,4'-bis(2-hydroxyethoxyphenyl) sulfide and 4,4'-bis[4-(2-dihydroxyethoxy)-3-methylphenyl] sulfide; bishydroxyalkoxy aryl sulfoxides, such as 4,4'-bis(2-hydroxyethoxyphenyl) sulfone and 4,4'-bis[4-(2- bishydroxyalkoxyarylsulfones, such as 1,4-bishydroxyethoxybenzene, bishydroxyalkoxybenzenes, such as 1,3-bis[2-[4-(2-hydroxyethoxy)phenyl]propyl]benzene, 1,4-bis[2-[4-(2-hydroxyethoxy)phenyl]propyl]benzene, 4,4'-bis(2-hydroxyethoxy)biphenyl, 1,3-bis[4-(2-hydroxyethoxy)phenyl]-5,7-dimethyladamantane, anhydrous sugar alcohols, such as dihydroxy compounds represented by the following formula (2), and compounds having a cyclic ether structure, such as spiro glycols, such as those represented by the following general formula (3). The dihydroxy compounds (A) may be used alone or in combination.
[0040] [ka]
[0041] [ka]
[0042] Of these dihydroxy compounds (A), preferred is the dihydroxy compound represented by the above formula (2). Examples of the dihydroxy compound represented by the above formula (2) include isosorbide, isomannide, and isoidite, which are stereoisomeric, and these may be used alone or in combination of two or more. Among the dihydroxy compounds (A), isosorbide obtained by dehydration condensation of sorbitol produced from various starches, which are abundant and easily available as resources, is most preferred in terms of availability, ease of production, optical properties, and moldability.
[0043] The ratio of the structural units derived from the dihydroxy compound (A) to the total structural units derived from the dihydroxy compounds contained in the PC resin is, for example, 10 mol% or more, preferably 40 mol% or more, and more preferably 60 mol% or more. On the other hand, the ratio of the structural units derived from the dihydroxy compound (A) is, for example, 100 mol% or less, preferably 90 mol% or less, more preferably 80 mol% or less, and even more preferably 70 mol% or less. When the ratio of the dihydroxy compound (A) is within the above range, rainbow unevenness of the resin film during optical inspection can be stably suppressed.
[0044] (Dihydroxy Compound (B)) As the dihydroxy compound that is the structural unit of the PC resin, dihydroxy compound (A) and dihydroxy compound (B) can be used together. By using dihydroxy compounds (A) and (B) in combination, rainbow unevenness of the resin film during optical inspection can be more stably suppressed.
[0045] The dihydroxy compound (B) is typically a dihydroxy compound other than the dihydroxy compound (A). Examples of the dihydroxy compound (B) include alicyclic dihydroxy compounds, aliphatic dihydroxy compounds, oxyalkylene glycols, aromatic dihydroxy compounds, and diols having a cyclic ether structure. The dihydroxy compounds (B) may be used alone or in combination. Of the dihydroxy compounds (B), preferably, alicyclic dihydroxy compounds are used.
[0046] The alicyclic dihydroxy compound is not particularly limited, but preferably includes a compound having a 5-membered ring structure or a 6-membered ring structure. The 6-membered ring structure may be fixed to a chair or boat shape by a covalent bond. When the alicyclic dihydroxy compound has a 5-membered ring or a 6-membered ring structure, the heat resistance of the resulting PC resin can be improved. The number of carbon atoms contained in the alicyclic dihydroxy compound is, for example, 70 or less, preferably 50 or less, more preferably 30 or less.
[0047] Specific examples of the alicyclic dihydroxy compound containing a 5-membered ring structure or a 6-membered ring structure include alicyclic dihydroxy compounds represented by the following general formula (I) or (II). HOCH2-R 1 -CHOH (I) H.O.R. 2 -OH (II) (In formulas (I) and (II), R 1 and R 2 Each of represents a cycloalkylene group having 4 to 20 carbon atoms.
[0048] Cyclohexanedimethanol, which is an alicyclic dihydroxy compound represented by the above general formula (I), is 1 is represented by the following general formula (Ia) (wherein R 3 represents an alkyl group having 1 to 12 carbon atoms or a hydrogen atom. Specific examples of such isomers include 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, and 1,4-cyclohexanedimethanol.
[0049] [ka]
[0050] The alicyclic dihydroxy compound represented by the above general formula (I), tricyclodecane dimethanol or pentacyclopentadecanedimethanol, is represented by the general formula (I), 1 is represented by the following general formula (Ib) (wherein n is 0 or 1):
[0051] [ka]
[0052] Decalin dimethanol or tricyclotetradecane dimethanol, which is an alicyclic dihydroxy compound represented by the above general formula (I), is a compound represented by the general formula (I) 1 is represented by the following general formula (Ic) (wherein m is 0 or 1). Specific examples of such isomers include 2,6-decalin dimethanol, 1,5-decalin dimethanol, and 2,3-decalin dimethanol.
[0053] [ka]
[0054] Norbornane dimethanol, which is an alicyclic dihydroxy compound represented by the above general formula (I), is 1 The isomers include various isomers represented by the following general formula (Id): Specific examples of such isomers include 2,3-norbornane dimethanol and 2,5-norbornane dimethanol.
[0055] [ka]
[0056] Adamantane dimethanol, which is an alicyclic dihydroxy compound represented by general formula (I), is 1The isomers include various isomers represented by the following general formula (Ie): A specific example of such isomers is 1,3-adamantanedimethanol.
[0057] [ka]
[0058] Cyclohexanediol, which is an alicyclic dihydroxy compound represented by the above general formula (II), is 2 is represented by the following general formula (IIa) (wherein R 3 represents an alkyl group having 1 to 12 carbon atoms or a hydrogen atom. Specific examples of such isomers include 1,2-cyclohexanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, and 2-methyl-1,4-cyclohexanediol.
[0059] [ka]
[0060] The alicyclic dihydroxy compound represented by the above general formula (II), tricyclodecanediol or pentacyclopentadecanediol, is a compound represented by the general formula (II), 2 is represented by the following general formula (IIb) (wherein n is 0 or 1):
[0061] [ka]
[0062] Decalindiol or tricyclotetradecanediol, which is an alicyclic dihydroxy compound represented by the above general formula (II), is a compound represented by the general formula (II) in which R 2is represented by the following general formula (IIc) (wherein m is 0 or 1). Specific examples of such isomers include 2,6-decalindiol, 1,5-decalindiol, and 2,3-decalindiol.
[0063] [ka]
[0064] Norbornanediol, which is an alicyclic dihydroxy compound represented by the above general formula (II), is 2 The isomers include various isomers represented by the following general formula (IId): Specific examples of such isomers include 2,3-norbornanediol and 2,5-norbornanediol.
[0065] [ka]
[0066] The adamantanediol, which is an alicyclic dihydroxy compound represented by the above general formula (II), is represented by the following general formula (II): 2 is represented by the following general formula (IIe): A specific example of such an isomer is 1,3-adamantanediol.
[0067] [ka]
[0068] Among the specific examples of the alicyclic dihydroxy compound described above, preferred are cyclohexanedimethanols, tricyclodecane dimethanols, adamantanediols, and pentacyclopentadecanedimethanols. From the viewpoints of availability and ease of handling, more preferred are 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,2-cyclohexanedimethanol, and tricyclodecane dimethanol, and even more preferred is tricyclodecane dimethanol.
[0069] The ratio of the structural units derived from the dihydroxy compound (B) to the total structural units derived from the dihydroxy compounds contained in the PC resin is, for example, 0 mol% or more, preferably 10 mol% or more, more preferably 20 mol% or more, and even more preferably 30 mol% or more. On the other hand, the ratio of the structural units derived from the dihydroxy compound (B) is, for example, 90 mol% or less, preferably 60 mol% or less, and more preferably 40 mol% or less.
[0070] Details of these PC resins are described, for example, in JP 2012-31370 A (Patent No. 5448264), the disclosure of which is incorporated herein by reference.
[0071] In one embodiment, the PC resin contains a structural unit derived from the dihydroxy compound (A) represented by the above formula (2), a structural unit derived from the alicyclic dihydroxy compound (B) represented by the above general formula (I), and a carbonate group linking them together. When the PC resin containing these structural units is applied to a resin film, rainbow unevenness of the resin film during optical inspection can be more stably suppressed. In such a PC resin, the molar ratio (A:B) of the structural unit derived from the dihydroxy compound (A) represented by the above formula (2) to the structural unit derived from the alicyclic dihydroxy compound (B) represented by the above general formula (I) is, for example, 5:5 to 9:1, and preferably 6:4 to 8:2. In such a PC resin, the combination of the dihydroxy compound (A) represented by the above formula (2) and the alicyclic dihydroxy compound (B) represented by the above general formula (I) is preferably a combination of isosorbide and tricyclodecane dimethanol.
[0072] C-2. Anti-blocking agents The resin film 1 contains an AB agent in addition to a resin material. The AB agent typically has a particulate form, and is dispersed in the resin material as aggregates in which a plurality of particles of the AB agent are aggregated together.
[0073] The average primary particle size of the AB agent is, for example, 0.1 μm to 1.3 μm, and preferably 0.1 μm to 1.0 μm. The average primary particle size of the AB agent can be measured by a laser diffraction method. When the average primary particle size of the AB agent is within this range, erroneous detection of the AB agent (particularly aggregates of the AB agent) can be stably suppressed in optical inspection of an adherend.
[0074] The AB agent is preferably transparent. Examples of materials constituting the AB agent include metal oxides and resins. Examples of metal oxides include silica, alumina, titania, zirconia, and calcium oxide. Examples of resins include polymethyl methacrylate, polystyrene, polyurethane, (meth)acrylic resins, (meth)acrylic-styrene copolymers, benzoguanamine, melamine, polycarbonate, and silicone. The surface of the AB agent may be subjected to any suitable surface modification, for example, chemical modification, preferably alkyl group modification. The AB agents may be used alone or in combination of two or more. Of these AB agents, preferred are resins and metal oxides, more preferred are resins, and even more preferred are (meth)acrylic-styrene copolymers.
[0075] The resin film 1 may contain any suitable additive in addition to the above-mentioned resin material and AB agent. Examples of the additive include antioxidants, UV absorbers, light stabilizers, nucleating agents, fillers, pigments, surfactants, and antistatic agents. Any suitable surface treatment layer may be provided on the surface of the resin film 1 (the surface opposite to the pressure-sensitive adhesive layer 2). Examples of the surface treatment layer include an easy-adhesion layer, an easy-slip layer, an antistatic layer, an antireflection layer, and an oligomer prevention layer.
[0076] D. Manufacturing method of resin film The above-mentioned resin film 1 can be produced by any appropriate method. In one embodiment, the method for producing the resin film includes a step of preparing a resin composition (preparation step), a step of passing the resin composition through a filter (filter passing step), and a step of extruding the resin composition after passing through the filter (extrusion molding step).
[0077] In the preparation step, typically, the above-mentioned resin material is melted, and then the molten resin material is mixed with the above-mentioned AB agent to prepare a resin composition.
[0078] The resin material before melting may have any suitable shape. In one embodiment, the resin material is pelletized in advance. The method of pelletizing the resin material is not particularly limited, and may be a strand cut method or a hot cut method. Details of the pellet preparation process are described in, for example, JP 2013-181105 A. The description of this patent document is incorporated herein by reference.
[0079] Next, the resin material (typically pellets) is heated to melt. The heating temperature may be any appropriate value depending on the resin material. The molten resin material is mixed with the AB agent. This prepares a molten resin composition. The range of the content ratio of the AB agent in the resin composition is, for example, the same as the range of the content ratio of the AB agent in the resin film 1 described above.
[0080] In the filter passing step, the molten resin composition is passed through a filter, whereby foreign matter and / or aggregates of the AB agent contained in the resin composition can be removed from the resin composition.
[0081] The filter may have any suitable configuration, and examples of the filter include a screen mesh and a disk filter, and preferably a screen mesh. The opening of the screen mesh is, for example, 0.080 mm or less, preferably 0.070 mm or less, and more preferably 0.055 mm or less. When the screen mesh has such an opening, it is possible to suppress the inclusion of foreign matter and / or AB agent aggregates having a maximum Feret's diameter of 30 μm or more in the resin film to be formed. Therefore, defects in the resin film (specifically, foreign matter and / or AB agent aggregates) can be reduced, and the D30 / 10 cm of the resin film can be improved. 2 can be stably adjusted to be within the above range. On the other hand, the opening of the screen mesh is, for example, 0.025 mm or more, preferably 0.035 mm or more. When the screen mesh has such openings, the resin composition can smoothly pass through the screen mesh. Therefore, the resin composition can be prevented from being retained, and the resin composition can be prevented from being excessively heated. This can prevent the generation of gel-like matter due to thermal crosslinking of the resin material. As a result, defects in the resin film (specifically, gel-like matter) can be reduced, and the D30 / 10cm of the resin film can be improved. 2 can be adjusted more stably within the above range.
[0082] In the extrusion molding step, the molten resin after passing through the filter is typically extruded into a film shape using a die, thereby preparing the resin film 1. The above-mentioned preparation step, filter passing step, and extrusion molding step can be performed by any appropriate film forming device.
[0083] The method for producing the resin film 1 may include, in addition to the above-mentioned preparation step and the above-mentioned film-forming step, a step (winding step) in which a winding member winds up the resin film. In the winding step, the winding member winds up the resin film 1 into a roll. The winding member typically has a cylindrical shape and is rotatable about its axis. Since the resin film 1 has excellent anti-blocking properties, even when the resin film 1 is wound into a roll, the resin films 1 can be sufficiently prevented from sticking to each other. In this manner, the resin film 1 is manufactured.
[0084] E. Adhesive layer The adhesive layer 2 is provided on the surface of the resin film 1 in order to attach the laminate film 100 to the surface of an adherend. The adhesive layer 2 is made of an adhesive (pressure-sensitive adhesive).
[0085] Examples of adhesives constituting the adhesive layer 2 include (meth)acrylic adhesives, rubber adhesives, silicone adhesives, polyester adhesives, urethane adhesives, epoxy adhesives, and polyether adhesives. By adjusting the type, number, combination, and compounding ratio of monomers forming the base resin of the adhesive, as well as the compounding amount of the crosslinking agent, reaction temperature, reaction time, etc., an adhesive having desired properties according to the purpose can be prepared. The base resin of the adhesive may be used alone or in combination of two or more types.
[0086] In one embodiment, the pressure-sensitive adhesive layer 2 is composed of a (meth)acrylic pressure-sensitive adhesive (a (meth)acrylic pressure-sensitive adhesive composition). When the pressure-sensitive adhesive layer is composed of a (meth)acrylic pressure-sensitive adhesive, the peel force of the laminated film can be suitably adjusted.
[0087] The (meth)acrylic pressure-sensitive adhesive composition typically contains a (meth)acrylic polymer as a main component. The content of the (meth)acrylic polymer in the solid content of the pressure-sensitive adhesive composition is, for example, 50% by mass or more, preferably 70% by mass or more, and more preferably 90% by mass or more. On the other hand, the upper limit of the content of the (meth)acrylic polymer is typically 100% by mass.
[0088] The (meth)acrylic polymer contains a structural unit derived from an alkyl (meth)acrylate. In the (meth)acrylic polymer, the content of the structural unit derived from an alkyl (meth)acrylate is, for example, 70% by mass or more, preferably 80% by mass or more. On the other hand, the upper limit of the content of the structural unit derived from an alkyl (meth)acrylate is typically 90% by mass. Examples of the alkyl group of the alkyl (meth)acrylate include linear or branched alkyl groups having 1 to 18 carbon atoms. The average number of carbon atoms in the alkyl group is preferably 3 to 12, and more preferably 3 to 8. Among the alkyl (meth)acrylates, preferred are butyl acrylate and 2-ethylhexyl acrylate, and more preferably 2-ethylhexyl acrylate.
[0089] The (meth)acrylic polymer may contain a structural unit derived from a copolymerizable monomer polymerizable with the alkyl (meth)acrylate, in addition to the structural unit derived from the alkyl (meth)acrylate. Examples of the copolymerizable monomer include a carboxyl group-containing monomer, a hydroxyl group-containing monomer, an amide group-containing monomer, an aromatic ring-containing (meth)acrylate, and a heterocyclic ring-containing vinyl monomer. The copolymerizable monomer may be used alone or in combination. Of the copolymerizable monomers, preferred are carboxyl group-containing monomers and hydroxyl group-containing monomers. In one embodiment, the (meth)acrylic polymer contains structural units derived from an alkyl (meth)acrylate, structural units derived from a carboxyl group-containing monomer, and structural units derived from a hydroxyl group-containing monomer.
[0090] The carboxyl group-containing monomer is a compound that contains a carboxyl group in its structure and a polymerizable unsaturated double bond such as a (meth)acryloyl group or a vinyl group. Examples of the carboxyl group-containing monomer include (meth)acrylic acid, carboxyethyl (meth)acrylate, maleic acid, fumaric acid, and crotonic acid, and preferably (meth)acrylic acid. When the (meth)acrylic polymer contains a structural unit derived from the carboxyl group-containing monomer, the adhesive properties of the adhesive layer can be improved.
[0091] When the (meth)acrylic polymer contains a structural unit derived from a carboxyl group-containing monomer, the content of the structural unit derived from the carboxyl group-containing monomer is, for example, 0.01% by mass or more, preferably 0.10% by mass or more. On the other hand, the content of the structural unit derived from the carboxyl group-containing monomer is, for example, 10% by mass or less, preferably 5.0% by mass or less, more preferably 1.0% by mass or less, and even more preferably 0.5% by mass or less.
[0092] The hydroxyl group-containing monomer is a compound that contains a hydroxyl group in its structure and a polymerizable unsaturated double bond such as a (meth)acryloyl group or a vinyl group. Examples of the hydroxyl group-containing monomer include 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)-methylacrylate, preferably 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate, more preferably 4-hydroxybutyl (meth)acrylate. When the (meth)acrylic polymer contains a structural unit derived from a hydroxyl group-containing monomer, the durability of the adhesive layer can be improved.
[0093] When the (meth)acrylic polymer contains a structural unit derived from a hydroxyl group-containing monomer, the content of the structural unit derived from the hydroxyl group-containing monomer is, for example, 0.01 mass% or more, preferably 1.0 mass% or more, more preferably 5.0 mass% or more, and even more preferably 8.0 mass% or more. The upper limit of the content of the structural unit derived from the hydroxyl group-containing monomer is typically 10 mass%.
[0094] The weight average molecular weight Mw of the (meth)acrylic polymer is, for example, from 100,000 to 2,000,000, and preferably from 200,000 to 1,000,000. The weight average molecular weight Mw can be calculated, for example, from the results of GPC measurement in terms of styrene.
[0095] In addition, the (meth)acrylic adhesive may contain a crosslinking agent. As the crosslinking agent, representative examples include organic crosslinking agents and polyfunctional metal chelates, and preferably organic crosslinking agents. As the organic crosslinking agent, for example, isocyanate crosslinking agents, peroxide crosslinking agents, epoxy crosslinking agents, and imine crosslinking agents are included, and more preferably, isocyanate crosslinking agents are included.
[0096] The content of the crosslinking agent is, for example, 0.01 parts by mass or more, preferably 0.5 parts by mass or more, more preferably 0.8 parts by mass or more, and even more preferably 1.2 parts by mass or more, relative to 100 parts by mass of the (meth)acrylic polymer. On the other hand, the content of the crosslinking agent is, for example, 10 parts by mass or less, preferably 5 parts by mass or less, more preferably 2.5 parts by mass or less, and even more preferably 2.0 parts by mass or less. When the content of the crosslinking agent is within such a range, the peel force of the laminated film can be suitably adjusted.
[0097] Furthermore, the (meth)acrylic pressure sensitive adhesive may contain various additives (for example, a silane coupling agent, a polymerization initiator, a solvent, a crosslinking catalyst) in an appropriate ratio. Details of these adhesives are described, for example, in JP 2006-183022 A, JP 2015-199942 A, JP 2018-053114 A, JP 2016-190996 A, and WO 2018 / 008712, the disclosures of which are incorporated herein by reference.
[0098] The thickness of the pressure-sensitive adhesive layer 2 is typically 1 μm or more, and preferably 5 μm or more. On the other hand, the thickness of the pressure-sensitive adhesive layer 2 is, for example, 30 μm or less, and preferably 15 μm or less.
[0099] The storage modulus of the pressure-sensitive adhesive layer 2 at 25° C. is, for example, 5.0×10 4 Pa~5.0×10 6 Pa, preferably 7.5×10 4 Pa~2.5×10 6 When the storage modulus of the pressure-sensitive adhesive layer is within such a range, the pressure-sensitive adhesive layer can have good wettability to an adherend and sufficient adhesive strength.
[0100] Such a pressure-sensitive adhesive layer 2 is formed by any appropriate means on the resin film 1. To form the pressure-sensitive adhesive layer 2 on the resin film 1, for example, the above-mentioned pressure-sensitive adhesive may be directly applied to the resin film 1, or the pressure-sensitive adhesive may be applied to a separate substrate to form a pressure-sensitive adhesive layer, which is then transferred to the resin film 1.
[0101] F. Applications of laminated film As shown in Figures 2 and 3, in one embodiment, the above-mentioned laminate film 100 is attached to the surface of an adherend 5 by the adhesive layer 2 after the release liner 3 is peeled off from the adhesive layer 2. Examples of the adherend 5 include optical members and electronic members, and preferably optical members. Representative examples of the optical members include a polarizing plate, a retardation film, an optical laminate including a polarizing plate and / or a retardation film, a display, an imaging device, a lens, and a (half) mirror.
[0102] Fig. 3 is a schematic cross-sectional view of an optical member with a laminate film including the laminate film of Fig. 2. The illustrated example of the optical member with a laminate film 200 includes an optical member 5a as an adherend and a laminate film 100 as a surface protective film. The laminate film 100 is attached to the surface of the optical member 5a by a pressure-sensitive adhesive layer 2.
[0103] In one embodiment, the optical member 5a included in the laminated film-attached optical member 200 is a polarizing plate. The polarizing plate has a thickness of, for example, 5 μm to 200 μm. The thickness of the resin film 1 in the laminate film 100 is, for example, 0.1 to 1.05 relative to the thickness of the adherend (optical member), and preferably 0.15 to 1.0. If the thickness ratio of the resin film to the adherend is within this range, the adherend (optical member) can be inspected with even greater accuracy even when the laminate film is attached to the adherend and subjected to optical inspection.
[0104] Such an optical member 200 with a laminated film is typically subjected to optical inspection. The optical inspection is not particularly limited, and may be, for example, an automated optical inspection (AOI). Examples of the automated optical inspection include a foreign body inspection for inspecting foreign bodies contained in an optical member, and an air bubble inspection for inspecting air bubbles contained in an optical member. In such optical inspection, false detections caused by the resin film are sufficiently suppressed, so that the optical member can be inspected with high accuracy even in a state where the laminated film is attached to the optical member.
[0105] Thereafter, the laminated film 100 can be peeled off from the surface of the optical member 5a (adherend) at a desired timing.
[0106] The peel force of the laminated film 100 from the acrylic plate is, for example, 3.5 N / 25 mm or less, preferably 3.0 N / 25 mm or less, more preferably 2.5 N / 25 mm or less, and even more preferably 2.0 N / 25 mm or less, at a pulling speed of 30 m / min and a peel angle of 180°. If the laminated film has such a peel force, the laminated film can be smoothly peeled from the adherend after optical inspection. On the other hand, the peel strength of the laminated film 100 from the acrylic plate is, for example, 0.5 N / 25 mm or more, preferably 1.0 N / 25 mm or more, and preferably 1.2 N / 25 mm or more. If the laminated film has such a peel strength, the laminated film can stably follow the surface of the adherend when the laminated film is attached to the adherend. The peel strength can be measured in accordance with JIS Z0237, and more specifically, can be measured by the following peel strength test. (peel strength test) A sample is prepared by cutting the laminated film into a strip of 25 mm x 100 mm; the sample is roll-pressed onto the surface of an acrylic plate via the adhesive layer at a pressure of 0.25 MPa and a feed rate of 0.3 m / min; the sample attached to the acrylic plate is left to stand in an environment with a temperature of 23°C and a relative humidity of 50% for 30 minutes, and then peeled at a peel angle of 180° and a tensile speed of 30 m / min in the same environment to measure the peel force. EXAMPLES
[0107] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring the various properties are as follows.
[0108] (1) Optical properties (1-1) Total light transmittance The total light transmittance of the resin films of the examples and comparative examples was measured in accordance with JIS R3106-2019 using a spectrophotometer (product name: U-4100, manufactured by Hitachi High-Tech Science Corporation). (1-2) Haze value The haze values of the resin films of the examples and comparative examples were measured in accordance with JIS K7136 using a haze meter (product name: HAZE METER HM-150, manufactured by Murakami Color Research Laboratory). The optical properties of the resin film were evaluated according to the following criteria. The results are shown in Table 1. Good: The resin film has a total light transmittance of 90% or more and a haze value of 1.0% or less. ×: The total light transmittance of the resin film is less than 90% and / or the haze value exceeds 1.0%.
[0109] (2) Slipperiness (anti-blocking properties) The resin films obtained in the Examples and Comparative Examples were rubbed against each other to evaluate the slipperiness (anti-blocking property) according to the following criteria. The results are shown in Table 1. If the slipperiness is sufficient, blocking between the resin films can be sufficiently suppressed even when the resin film alone is wound into a roll. ◎: The base films slide easily and do not stick to each other. ◯: The base films do not stick to each other, but they are slightly slippery compared to ◎ ×: The base films stick together and do not slide.
[0110] <<Preparation Example 1: PC Resin Film>> 81.98 parts by mass of isosorbide (ISB), 47.19 parts by mass of tricyclodecane dimethanol (TCDDM), 175.1 parts by mass of diphenyl carbonate (DPC), and 0.979 parts by mass of cesium carbonate 0.2% by mass aqueous solution as a catalyst were charged into a reaction vessel, and in a nitrogen atmosphere, the temperature of the heating vessel was heated to 150°C as the first step of the reaction, and the raw materials were dissolved (about 15 minutes) while stirring as necessary. Next, the pressure was changed from normal pressure to 13.3 kPa, and the temperature of the heating vessel was raised to 190°C in one hour, while the generated phenol was extracted outside the reaction vessel. After the entire reaction vessel was kept at 190°C for 15 minutes, the pressure in the reaction vessel was changed to 6.67 kPa, the temperature of the heating vessel was raised to 230°C in 15 minutes, and the generated phenol was extracted outside the reaction vessel as the second step. As the stirring torque of the stirrer increased, the temperature was raised to 250°C in 8 minutes, and the pressure inside the reaction vessel was lowered to 0.200 kPa or less in order to remove the phenol that was generated. After the predetermined stirring torque was reached, the reaction was terminated and the reaction product was extruded into water to obtain pellets of PC resin.
[0111] [Example 1, Comparative Examples 1 and 3] The PC resin pellets obtained in Preparation Example 1 were vacuum dried at 100°C for 12 hours. Thereafter, the PC resin pellets and an AB agent (polymer particles, average primary particle size: 0.5 μm, refractive index: 1.5, manufactured by Sekisui Chemical Co., Ltd., product name: Techpolymer) were supplied to a film forming device. The addition ratio of the AB agent to the total amount of the pellets and the AB agent, and the average primary particle size of the AB agent are shown in Table 1. The film-forming equipment was equipped with a single-screw extruder (manufactured by Toshiba Machine Co., Ltd., cylinder set temperature: 250°C), a screen mesh with an opening of 0.045 mm, a T-die (width 1700 mm, set temperature: 250°C), a casting roll (set temperature: 60°C), and a winding member. More specifically, the pellets and the AB agent were supplied to a single-screw extruder and heated. As a result, the pellets were melted, and the molten PC resin and the AB agent were kneaded to prepare a resin composition. Thereafter, the resin composition was extruded from the single-screw extruder and passed through a screen mesh and a T-die in this order. As a result, a PC resin film having a thickness of 40 μm was produced. After passing through a cast roll, the PC resin film was taken up by a take-up member. In this manner, a PC resin film (resin film) was obtained.
[0112] [Example 2] A PC resin film (resin film) was obtained in the same manner as in Example 1, except that the AB agent (polymer particles, average primary particle size: 0.5 μm, refractive index: 1.5, manufactured by Sekisui Chemical Co., Ltd., product name: Techpolymer) was changed to an AB agent (average primary particle size: 1.0 μm, refractive index: 1.5, manufactured by Sekisui Chemical Co., Ltd., product name: Techpolymer) and the addition ratio of the AB agent to the total amount of pellets and AB agent was changed to 500 ppm.
[0113] [Example 3] A PC-based resin film (resin film) was obtained in the same manner as in Example 1, except that the AB agent (polymer particles, average primary particle size: 0.5 μm, refractive index: 1.5, manufactured by Sekisui Chemical Co., Ltd., product name: Techpolymer) was changed to fine particles in which silica was methyl-modified (average primary particle size: 0.5 μm, refractive index: 1.43, manufactured by Nippon Shokubai Co., Ltd., product name: Seahoster KE).
[0114] [Comparative Example 2] A PC-based resin film (resin film) was obtained in the same manner as in Example 1, except that the AB agent (polymer particles, average primary particle size: 0.5 μm, refractive index: 1.5, manufactured by Sekisui Chemical Co., Ltd., product name: Techpolymer) was changed to magnesium fluoride nanoparticles (average primary particle size: 0.5 μm, refractive index: 1.38, manufactured by Stella Chemifa Corporation).
[0115] [Table 1]
[0116] [evaluation] As is clear from Table 1, when the content of the AB agent in the resin film is 350 ppm or more, the resin film has excellent antiblocking properties. In addition, when the content of the AB agent in the resin film is 3000 ppm or less and the absolute value of the refractive index difference between the resin material and the AB agent is 0.10 or less, the resin film can improve the total light transmittance and reduce the haze value. [Industrial Applicability]
[0117] The resin film of the present invention can be applied to various industrial products, and can be suitably used in particular as an optical film (for example, a protective layer for a polarizer, a raw material for a retardation film, or a base film for a surface protection film). [Explanation of symbols]
[0118] 1 Resin film 2 Adhesive layer 100 Laminated Film
Claims
1. A resin material as a matrix; an antiblocking agent dispersed in the resin material; The content of the antiblocking agent is 350 ppm to 3000 ppm, A resin film, wherein an absolute value of a refractive index difference between the resin material and the antiblocking agent is 0.10 or less.
2. The resin film according to claim 1 , wherein the refractive index of the antiblocking agent is equal to or lower than the refractive index of the resin material.
3. The resin film according to claim 1, wherein the average primary particle diameter of the antiblocking agent is 0.1 μm to 1.3 μm.
4. The resin film according to claim 1, having an indentation modulus at 25°C of 2.0 N to 6.5 N.
5. The resin film according to claim 1 , which has a dynamic friction coefficient of 1.0 or less.
6. 2. The resin film according to claim 1, which has a total light transmittance of 90% or more and a haze value of 1.0% or less.
7. The resin film according to claim 1 , having an in-plane retardation Re(550) of 10 nm or less.
8. The resin film according to claim 1 , wherein the resin material includes a polycarbonate-based resin.
9. A resin film according to any one of claims 1 to 8, A laminate film comprising: a pressure-sensitive adhesive layer laminated on the resin film.
10. A step of mixing a molten resin material and an antiblocking agent to prepare a resin composition; Passing the resin composition through a filter; and extrusion molding the resin composition after passing through the filter. The content of the antiblocking agent in the resin composition is 350 ppm to 3000 ppm, A method for producing a resin film, wherein a refractive index difference between the resin material and the antiblocking agent is 0.10 or less.
11. The filter is a screen mesh, The method for producing a resin film according to claim 10, wherein the opening of the screen mesh is 0.035 mm to 0.070 mm.
12. The method for producing a resin film according to claim 10 or 11, further comprising a step of winding up the resin film with a winding member.
Citation Information
Patent Citations
Polycarbonate-based resin film, material for optical recording medium given by using the same, and material for liquid crystal display
JP2006182879A
Cycloolefin resin film and its production method, polarizing plate and liquid crystal display
JP2007112967A
Film, multilayer body, and transparent conductive film
JP2022182086A
Film, multilayer body, and transparent conductive film
JP2022182907A
Method for producing polycarbonate resin composition
WO2019026671A1