AI Technical Summary
【0016】 本発明によれば、原料の濃度を高濃度とした混合液を利用した場合においても反応生成物中のエステル基含有化合物や重質物の残存率を低減させることが可能であり、エステル基含有化合物や重質物の残存率を低減させた脂環式テトラカルボン酸二無水物を効率よく製造することが可能な脂環式テトラカルボン酸二無水物の製造方法及びその方法を利用したポリイミドの製造方法を提供することが可能となる。
Smart Images

Figure 2024145574000001 
Figure 2024145574000002 
Figure 2024145574000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an alicyclic tetracarboxylic dianhydride and a method for producing a polyimide. [Background technology]
[0002] Polyimides have traditionally been attracting attention as a material that is highly heat-resistant, lightweight, and flexible. In recent years, alicyclic tetracarboxylic dianhydrides have been attracting attention as raw materials used in the production of such polyimides from the viewpoint of transparency and the like. In general, a method for producing such alicyclic tetracarboxylic dianhydrides involves heating an alicyclic tetraester compound (a tetraester compound having an alicyclic structure) in a lower carboxylic acid (for example, WO 2011 / 099518 (Patent Document 1) also employs a method for heating a specific alicyclic tetraester compound in a lower carboxylic acid). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2011 / 099518 Summary of the Invention [Problem to be solved by the invention]
[0004] However, when an alicyclic tetracarboxylic acid dianhydride is produced by employing a conventional method of heating an alicyclic tetraester compound (raw material compound) in a lower carboxylic acid, in order to reduce the ratio (residual rate: residual amount) of ester group-containing compounds (compounds having ester groups, including unreacted raw material compounds and reaction intermediates) and heavy materials remaining in the reaction product, it is necessary to lower the concentration of the raw materials in a mixed liquid containing a solvent (lower carboxylic acid) and the raw materials, and it has not been possible to efficiently produce an alicyclic tetracarboxylic acid dianhydride in which the residual rate (residual amount) of ester group-containing compounds and heavy materials in the reaction product is reduced.
[0005] The present invention has been made in consideration of the problems associated with the prior art, and an object of the present invention is to provide a method for producing an alicyclic tetracarboxylic acid dianhydride that can reduce the residual rate of ester group-containing compounds and heavy substances in a reaction product even when a mixed liquid containing high concentrations of raw materials is used, and that can efficiently produce an alicyclic tetracarboxylic acid dianhydride in which the residual rate of ester group-containing compounds and heavy substances is reduced, and a method for producing a polyimide using the method. [Means for solving the problem]
[0006] As a result of intensive research to achieve the above-mentioned object, the present inventors have found that by heating a mixed liquid containing a solvent consisting of a carboxylic acid having 1 to 5 carbon atoms and γ-butyrolactone, where the content of the γ-butyrolactone is 20 to 92 mass% based on the total amount of the γ-butyrolactone and the carboxylic acid, and an alicyclic tetraester compound, it is possible to reduce the residual rate of an ester group-containing compound (a compound having an ester group, including an unreacted raw material compound and a reaction intermediate) and heavy matters in a reaction product even when the concentration of the raw material (alicyclic tetraester compound) in the mixed liquid is high, and it is possible to efficiently produce an alicyclic tetracarboxylic acid dianhydride in which the residual rate of the ester group-containing compound and heavy matters in the reaction product is reduced, thereby completing the present invention.
[0007] That is, the present invention provides the following aspects.
[0008] [1] A solvent consisting of a carboxylic acid having 1 to 5 carbon atoms and γ-butyrolactone, and the content of the γ-butyrolactone is 20 to 92 mass% based on the total amount of the γ-butyrolactone and the carboxylic acid; an alicyclic tetraester compound; The method for producing an alicyclic tetracarboxylic acid dianhydride comprises heating a mixed liquid containing the following:
[0009] [2] The method for producing an alicyclic tetracarboxylic dianhydride according to [1], further comprising adding an acid catalyst to the mixed solution.
[0010] [3] The method for producing an alicyclic tetracarboxylic dianhydride according to [1] or [2], further comprising adding acetic anhydride to the mixed solution.
[0011] [4] The alicyclic tetraester compound is represented by the following formula (1):
[0012] [ka]
[0013] (In the formula, X 1 represents a tetravalent organic group having a six-membered alicyclic structure, and a plurality of R 1 each independently represents one selected from the group consisting of hydrocarbon groups having 1 to 10 carbon atoms.) The method for producing an alicyclic tetracarboxylic dianhydride according to any one of [1] to [3], wherein the alicyclic tetracarboxylic dianhydride is a compound represented by the following formula:
[0014] [5] The method for producing an alicyclic tetracarboxylic dianhydride according to any one of [1] to [4], wherein the content of the alicyclic tetraester compound in the mixed liquid is 10 to 30 mass %.
[0015] [6] A step of obtaining an alicyclic tetracarboxylic dianhydride by employing the method for producing an alicyclic tetracarboxylic dianhydride according to any one of [1] to [5]; a step of reacting the alicyclic tetracarboxylic dianhydride with a diamine to obtain a polyimide; A method for producing a polyimide, comprising: Effect of the Invention
[0016] According to the present invention, even when a mixed solution containing high concentrations of raw materials is used, it is possible to reduce the residual rate of ester group-containing compounds and heavy substances in the reaction product, and it is possible to provide a method for producing an alicyclic tetracarboxylic acid dianhydride capable of efficiently producing an alicyclic tetracarboxylic acid dianhydride in which the residual rate of ester group-containing compounds and heavy substances is reduced, and a method for producing a polyimide using the method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The present invention will be described in detail below with reference to preferred embodiments. In this specification, unless otherwise specified, the expression "X to Y" for numerical values X and Y means "X or more and Y or less." In such an expression, when a unit is added only to the numerical value Y, the unit is also applied to the numerical value X.
[0018] [Method for producing alicyclic tetracarboxylic dianhydride] The method for producing an alicyclic tetracarboxylic dianhydride of the present invention includes the steps of: a solvent consisting of a carboxylic acid having 1 to 5 carbon atoms and γ-butyrolactone, the content of said γ-butyrolactone being 20 to 92 mass% based on the total amount of said γ-butyrolactone and said carboxylic acid; an alicyclic tetraester compound; The method is characterized in that an alicyclic tetracarboxylic dianhydride is obtained by heating a mixed liquid containing
[0019] The solvent according to the present invention is a solvent consisting of a carboxylic acid having 1 to 5 carbon atoms and γ-butyrolactone. Thus, in the present invention, a mixed solvent of a carboxylic acid having 1 to 5 carbon atoms and γ-butyrolactone is used as the solvent for the mixed solution. By using such a mixed solvent, it is possible to reduce the remaining rate (remaining amount) of ester group-containing compounds and heavy substances in the reaction product. The reason why the remaining amount of ester group-containing compounds and heavy substances in the reaction product can be reduced by using the solvent is not necessarily clear, but the present inventors speculate that this is because by using γ-butyrolactone in combination with a carboxylic acid having 1 to 5 carbon atoms, γ-butyrolactone becomes a solvent with high solubility for ester group-containing compounds and heavy substances, and therefore it is possible to obtain a reaction product in which the remaining amount of these compounds is reduced.
[0020] The number of carbon atoms of the carboxylic acid used in such a solvent is 1 to 5 (more preferably 1 to 3, and even more preferably 1 to 2). If the number of carbon atoms of such a carboxylic acid exceeds the upper limit, it becomes difficult to efficiently produce an alicyclic tetracarboxylic dianhydride. Examples of such a carboxylic acid having 1 to 5 carbon atoms include formic acid, acetic acid, propionic acid, and butyric acid, and among them, from the viewpoint of ease of production and purification, formic acid, acetic acid, and propionic acid are preferable, and formic acid and acetic acid are more preferable. Such a carboxylic acid having 1 to 5 carbon atoms may be used alone or in combination of two or more.
[0021] The solvent according to the present invention contains γ-butyrolactone as an essential component together with the carboxylic acid having 1 to 5 carbon atoms. In such a solvent, the content of γ-butyrolactone must be 20 to 92 mass% (more preferably 20 to 90 mass%, and even more preferably 30 to 90 mass%) based on the total amount of the carboxylic acid having 1 to 5 carbon atoms and the γ-butyrolactone. If the content of γ-butyrolactone is less than the lower limit, the effect obtained by using γ-butyrolactone cannot be sufficiently obtained, whereas if the content of γ-butyrolactone exceeds the upper limit, the yield decreases and an alicyclic tetracarboxylic dianhydride cannot be efficiently obtained.
[0022] The amount of the carboxylic acid having 1 to 5 carbon atoms used in the solvent according to the present invention is not particularly limited, but is preferably 4 to 90 times (more preferably 6 to 82 times) the molar amount of the alicyclic tetraester compound (raw material compound) contained in the mixed liquid. If the amount of the carboxylic acid used is less than the lower limit, the reaction rate tends to decrease, whereas if the amount exceeds the upper limit, the yield decreases and it becomes difficult to efficiently obtain the alicyclic tetracarboxylic dianhydride.
[0023] The solvent of the mixed solution according to the present invention may contain other solvent components in addition to the carboxylic acid having 1 to 5 carbon atoms and γ-butyrolactone, as long as the effects of the present invention are not impaired. As such other solvent components, for example, known solvents that can be used in acid anhydride reactions (for example, solvents exemplified in paragraph
[0146] of WO 2015 / 163314 (for example, ester solvents such as ethyl acetate, aromatic solvents such as benzene and toluene, etc.)) can be appropriately used.
[0024] In the present invention, the alicyclic tetraester compound is used as a raw material compound for an alicyclic tetracarboxylic dianhydride. As such an alicyclic tetraester compound (alicyclic tetracarboxylic tetraester), any tetraester compound having an alicyclic structure may be used, and known compounds (for example, alicyclic tetracarboxylic tetraesters described in WO 2011 / 099518, WO 2017 / 030019, etc.) may be appropriately used without any particular limitation. Among them, from the viewpoint of obtaining a higher degree of heat resistance when producing a polyimide, a compound represented by the following formula (1):
[0025] [ka]
[0026] (In the formula, X 1 represents a tetravalent organic group having a six-membered alicyclic structure, and multiple R 1 each independently represents one selected from the group consisting of hydrocarbon groups having 1 to 10 carbon atoms.) It is preferable that the compound is represented by the following formula:
[0027] In this formula (1), X 1 is a tetravalent organic group having a 6-membered alicyclic structure. Regarding such a "tetravalent organic group having a 6-membered alicyclic structure", the "6-membered ring" is not particularly limited as long as it is a ring having 6 atoms forming a cyclic structure (note that, in the case of forming a polycyclic structure such as a bicyclic structure including a bridged structure (for example, in the case of a norbornane ring structure or a bicyclooctane ring structure), any of the rings may be a ring having 6 atoms).
[0028] In addition, X in formula (1) 1 The "six-membered alicyclic structure" of the tetravalent organic group as the aryl group is not particularly limited, and examples thereof include those represented by the following general formulas (i) to (iii):
[0029] [ka]
[0030] As such a six-membered alicyclic structure, a structure consisting of an aliphatic six-membered ring (norbornane ring) represented by the above formula (ii) is more preferable, from the viewpoint of obtaining higher heat resistance and higher resistance to tensile stress, and thus obtaining higher mechanical strength.
[0031] Also, X 1 The "tetravalent organic group having a six-membered alicyclic structure" that can be selected as X may have the six-membered alicyclic structure, and the carbon atom forming the six-membered alicyclic structure may be bonded to various atoms such as hydrogen atoms and atoms other than hydrogen atoms, or other substituents (including other organic groups). 1 The "tetravalent organic group having a six-membered alicyclic structure" selected as is preferably a tetravalent organic group having two norbornane rings.
[0032] Also, X 1 As the "tetravalent organic group having a 6-membered alicyclic structure" that can be selected as above, from the viewpoints of transparency, heat resistance, and high dimensional stability, it is preferable to have two or more of the 6-membered alicyclic structures (more preferably a structure consisting of norbornene rings). Among these, when a polyimide is produced using the finally obtained alicyclic tetracarboxylic acid dianhydride, the transparency, heat resistance, and high dimensional stability are further improved, and therefore it is preferable to use the following general formulas (iv) to (vi):
[0033] [ka]
[0034] [In formula (iv), m represents an integer of 0 to 2; in formula (v), n represents an integer of 1 to 2; in formula (vi), A represents one selected from the group consisting of a single bond; and a divalent aromatic group which may have a substituent and which has 6 to 30 carbon atoms forming an aromatic ring; and the symbols *1 to *4 in formulas (iv) to (vi) each represent a bond to which the symbol is attached, and 1 This indicates that the bond is one of the four bonds attached to the atom. A tetravalent organic group represented by the following formula is more preferred.
[0035] With respect to the tetravalent organic groups represented by such general formulas (iv) to (vi), m in formula (iv) is an integer of 0 to 2 (more preferably 1 to 2, and even more preferably 1). If the value of m exceeds the upper limit, production and purification tend to become difficult.
[0036] Furthermore, n in the formula (v) is an integer of 1 to 2 (more preferably 1). If the value of n exceeds the upper limit, production and purification tend to become difficult.
[0037] Furthermore, A in the above general formula (vi) is one member selected from the group consisting of a single bond; and a divalent aromatic group which may have a substituent and which has 6 to 30 carbon atoms forming an aromatic ring.
[0038] The divalent aromatic group that can be selected as A is a divalent aromatic group that may have a substituent, and the number of carbon atoms forming the aromatic ring contained in the aromatic group (note that, when the aromatic group has a carbon-containing substituent (such as a hydrocarbon group), the number of carbon atoms in the substituent is not included, and only the number of carbon atoms in the aromatic ring in the aromatic group is referred to. For example, in the case of a 2-ethyl-1,4-phenylene group, the number of carbon atoms forming the aromatic ring is 6.) is 6 to 30. Thus, the divalent aromatic group that can be selected as A in the above formula is a divalent group (divalent aromatic group) that may have a substituent and has an aromatic ring having 6 to 30 carbon atoms. If the number of carbon atoms forming such an aromatic ring exceeds the upper limit, when a resin having such a repeating unit is used to prepare a resin, it tends to be difficult to sufficiently suppress coloration of the resin. From the viewpoints of transparency and ease of purification, the aromatic ring of the divalent aromatic group more preferably has 6 to 18 carbon atoms, and further preferably has 6 to 12 carbon atoms.
[0039] The divalent aromatic group that can be selected as A is not particularly limited as long as it satisfies the above-mentioned condition regarding the number of carbon atoms. For example, a residue in which two hydrogen atoms have been eliminated from an aromatic compound such as benzene, naphthalene, terphenyl, anthracene, phenanthrene, triphenylene, pyrene, chrysene, biphenyl, terphenyl, quaterphenyl, or quinquephenyl (note that, as for such a residue, the position of the eliminated hydrogen atom is not particularly limited, but examples thereof include a 1,4-phenylene group, a 2,6-naphthylene group, a 2,7-naphthylene group, a 4,4'-biphenylene group, and a 9,10-anthracenylene group); and a group in which at least one hydrogen atom in the residue has been substituted with a substituent (for example, a 2,5-dimethyl-1,4-phenylene group, a 2,3,5,6-tetramethyl-1,4-phenylene group), etc., can be appropriately used. In such a residue, as described above, the position of the eliminated hydrogen atom is not particularly limited. For example, when the residue is a phenylene group, the hydrogen atom may be at any of the ortho, meta, and para positions.
[0040] As the divalent aromatic group that can be selected as A, from the viewpoint that the transparency of the polyimide is more excellent when the polyimide is prepared, a phenylene group that may have a substituent, a biphenylene group that may have a substituent, a naphthylene group that may have a substituent, an anthracenylene group that may have a substituent, and a terphenylene group that may have a substituent are preferred. Furthermore, among such divalent aromatic groups, a phenylene group, a biphenylene group, and a naphthylene group, each of which may have a substituent, are more preferred, a phenylene group and a biphenylene group, each of which may have a substituent, are even more preferred, and a phenylene group that may have a substituent is the most preferred, since a higher effect can be obtained from the above viewpoint.
[0041] In addition, the substituent that the divalent aromatic group that can be selected as A may have is not particularly limited, and examples thereof include an alkyl group, an alkoxy group, and a halogen atom. Among the substituents that the divalent aromatic group may have, from the viewpoint of obtaining a resin with better transparency when produced, an alkyl group having 1 to 10 carbon atoms and an alkoxy group having 1 to 10 carbon atoms are more preferred. If the carbon number of the alkyl group and alkoxy group suitable as such a substituent exceeds 10, the heat resistance of the obtained resin tends to decrease. In addition, the carbon number of the alkyl group and alkoxy group suitable as such a substituent is preferably 1 to 6, more preferably 1 to 5, even more preferably 1 to 4, and particularly preferably 1 to 3, from the viewpoint of obtaining a higher heat resistance when produced. In addition, the alkyl group and alkoxy group that can be selected as such a substituent may each be linear or branched.
[0042] From the viewpoint of obtaining a higher level of heat resistance, A in such formula (vi) is more preferably a single bond, an optionally substituted phenylene group, an optionally substituted biphenylene group, an optionally substituted naphthylene group or an optionally substituted terphenylene group, still more preferably a single bond, an optionally substituted phenylene group, an optionally substituted biphenylene group or an optionally substituted naphthylene group, particularly preferably a single bond, an optionally substituted phenylene group or an optionally substituted biphenylene group, and most preferably a single bond or an optionally substituted phenylene group.
[0043] In addition, multiple R 1 Each independently represents one selected from the group consisting of hydrocarbon groups having 1 to 10 carbon atoms. 1 The hydrocarbon group that can be selected as R may have 1 to 10 carbon atoms (more preferably 1 to 5, and particularly preferably 1 to 3). When the number of carbon atoms is equal to or less than the upper limit, synthesis and purification can be facilitated compared with the case where the number of carbon atoms exceeds the upper limit. Moreover, such a hydrocarbon group may be a saturated hydrocarbon group or an unsaturated hydrocarbon group. Furthermore, the hydrocarbon group may be any of linear, branched, and cyclic. Such R 1 Examples of the hydrocarbon group that can be selected as R include linear alkyl groups such as methyl, ethyl, propyl, and butyl groups; branched alkyl groups such as isopropyl and isobutyl groups; cyclic alkyl groups such as cyclohexyl groups; and aromatic hydrocarbon groups such as benzyl groups. 1 From the viewpoint of ease of purification, the hydrocarbon group that can be selected as is preferably an alkyl group, and particularly preferably a methyl group or an ethyl group.
[0044] In addition, R in the formula (1) 1 From the viewpoint of ease of synthesis and purification, it is particularly preferable that each of the ester groups is independently a methyl group or an ethyl group. The structure of such an ester group can be identified by NMR measurement.
[0045] The method for preparing the alicyclic tetraester compound of the present invention is not particularly limited, and known methods (e.g., methods described in WO 2011 / 099518, WO 2015 / 163314, WO 2017 / 030019, etc.) can be appropriately adopted.
[0046] The content of the alicyclic tetraester compound in the mixed solution according to the present invention is not particularly limited, but the content of the alicyclic tetraester compound is preferably 10 to 30% by mass (more preferably 20 to 30% by mass) based on the total amount of the mixed solution. Even when the alicyclic tetraester compound is used at such a content, the content of the ester group-containing compound and heavy substances can be reduced in the present invention, and an alicyclic tetracarboxylic acid dianhydride having a reduced residual rate (remaining amount) of the ester group-containing compound and heavy substances in the reaction product can be efficiently produced. Note that, when a solvent consisting of a carboxylic acid having 1 to 5 carbon atoms and γ-butyrolactone is not used, and only a carboxylic acid having 1 to 5 carbon atoms is used as a solvent, the reduction in the content of the ester group-containing compound and the reduction in the content of the heavy substances cannot be achieved at the same time (in some cases, both cannot be reduced), and an alicyclic tetracarboxylic acid dianhydride having a reduced residual rate (remaining amount) of the ester group-containing compound and heavy substances in the reaction product cannot necessarily be efficiently produced. In this way, by setting the content of the alicyclic tetraester compound to 10% by mass or more, it tends to be possible to more efficiently produce an alicyclic tetracarboxylic acid dianhydride in which the residual rate of ester group-containing compounds and the residual rate of heavy substances are reduced. On the other hand, by setting the content of the alicyclic tetraester compound to 30% by mass or less, it tends to be possible to more efficiently produce an alicyclic tetracarboxylic acid dianhydride in which the residual rate of ester group-containing compounds and the residual rate of heavy substances are reduced, as compared with the case where the content exceeds 30% by mass.
[0047] In the present invention, it is preferable that the mixed solution further contains an acid catalyst. Such an acid catalyst is not particularly limited, and a known one that can be used in the reaction of converting a tetraester into an acid dianhydride (hereinafter, sometimes simply referred to as "acid anhydride reaction") (for example, the acid catalysts exemplified in paragraph
[0140] of International Publication No. 2015 / 163314 (for example, trifluoromethanesulfonic acid (TfOH) etc.) and other known acid catalysts (for example, hydrochloric acid, sulfuric acid etc.)) can be appropriately used. In addition, as such an acid catalyst, trifluoromethanesulfonic acid and tetrafluoroethanesulfonic acid are more preferable, and trifluoromethanesulfonic acid is particularly preferable, from the viewpoint of improving the reaction yield. Note that such an acid catalyst may be used alone or in combination of two or more kinds.
[0048] The amount of the acid catalyst used is not particularly limited, but is preferably about 1 mole of the alicyclic tetraester compound used and about 1 mole of the hydrogen ion (H + It is preferable that the amount of the acid catalyst used is 0.005 to 0.2 moles (more preferably 0.01 to 0.1 moles). If the amount of the acid catalyst used is less than the lower limit, the reaction rate tends to decrease, whereas if the amount of the acid catalyst used exceeds the upper limit, it becomes difficult to further improve the effect obtained by using the catalyst, and the economic efficiency tends to decrease. It is preferable that the concentration of the acid catalyst is in the range of 0.50 to 5.0 mole % of the total mole amount of the alicyclic tetraester compound.
[0049] In the present invention, it is preferable that the mixed solution further contains acetic anhydride. This allows efficient removal of water generated during the reaction. The content of such acetic anhydride is not particularly limited, but it is preferable that the molar amount of acetic anhydride is 2 to 10 moles (more preferably 2 to 5 moles) per mole of the amount of the alicyclic tetraester compound used. If the content (amount used) of acetic anhydride is less than the lower limit, the effect obtained by using acetic anhydride tends not to be sufficiently obtained, while if it exceeds the upper limit, the yield tends to decrease, making it difficult to efficiently obtain alicyclic tetracarboxylic dianhydride.
[0050] The method for preparing the mixed solution according to the present invention is not particularly limited, and it may be prepared appropriately depending on the apparatus used for heating, etc. For example, the mixed solution may be prepared by adding (introducing) the components to be used into the same container. When the acid catalyst or acetic anhydride is added, the alicyclic tetraester compound is heated and dissolved in a solvent containing a carboxylic acid having 1 to 5 carbon atoms before adding the acid catalyst or acetic anhydride (before preparing the mixture) (preferably, heating is continued even after dissolution to dissolve the R 1 with a hydrogen atom), and then adding an acid catalyst or acetic anhydride (these may be added simultaneously or separately in sequence), thereby resulting in the addition of an acid catalyst or acetic anhydride to the mixed solution.
[0051] In the present invention, the mixed solution is heated (heating step). By heating the mixed solution in this manner, an ester exchange reaction occurs between the alicyclic tetraester compound and the carboxylic acid having 1 to 5 carbon atoms, and the ester group (the compound represented by the formula: -COOR in the case of the compound represented by the formula (1)) in the alicyclic tetraester compound (raw material compound) is converted to an ester group represented by the formula: -COOR 1(a group represented by the formula: —COOH) becomes a carboxy group, and then the carboxy groups in the same molecule react with each other to cause dehydration and ring closure, making it possible to obtain an alicyclic tetracarboxylic dianhydride. The conditions (heating conditions, etc.) employed during such heating are not particularly limited, and heating conditions employed in a known method of obtaining a tetracarboxylic dianhydride by heating a tetraester compound in a carboxylic acid having 1 to 5 carbon atoms can be appropriately employed, except for using the mixed liquid.
[0052] In the heating step according to the present invention, the heating temperature is preferably lower than the boiling point of γ-butyrolactone (204° C.), more preferably 80 to 180° C., even more preferably 80 to 150° C., particularly preferably 100 to 140° C., and most preferably 110 to 130° C. In addition, when the acid catalyst is used, the heating temperature is preferably set to a temperature lower than the boiling point of the acid catalyst within the above temperature condition range. The heating time during the heating is not particularly limited, but is preferably 0.5 to 100 hours, more preferably 1 to 50 hours. By setting the heating temperature and heating time to satisfy such conditions, the alicyclic tetracarboxylic dianhydride can be obtained more efficiently.
[0053] In addition, the pressure conditions (pressure conditions during the reaction) employed in such a heating step are not particularly limited, and any of normal pressure, pressurized conditions, and reduced pressure conditions may be employed. Regardless of the pressure conditions, the reaction of converting the acid anhydride can be sufficiently advanced. When the reaction is carried out in a vessel (for example, refluxing), the reaction may be carried out under pressurized conditions using the vapor of the solvent in the mixed liquid (for example, vapor of a carboxylic acid having 1 to 5 carbon atoms, etc.). In addition, the atmospheric gas during the heating step is not particularly limited, and may be, for example, air or an inert gas (nitrogen, argon, etc.).
[0054] In addition, the heating step is preferably a step of heating to reflux the reaction. When the reaction is heated to reflux, the reflux step may be a step of heating to reflux the reaction to a certain extent, and then distilling (removing) water generated during the reaction (water generated during ring-closing dehydration when converting to an acid anhydride) and an ester compound of a carboxylic acid having 1 to 5 carbon atoms (a compound generated in the system by the transesterification reaction) out of the system to allow the reaction to proceed. When adopting a step of allowing the reaction to proceed while discharging (removing) components such as water and an ester compound of a carboxylic acid having 1 to 5 carbon atoms out of the system, it is preferable to perform reflux while appropriately adding a carboxylic acid having 1 to 5 carbon atoms to the mixture so that the amount of the mixture is approximately constant. By performing the reaction while appropriately adding a carboxylic acid having 1 to 5 carbon atoms to the mixture, it is possible to allow the reaction to proceed while replenishing the carboxylic acid having 1 to 5 carbon atoms that has been reduced by distillation, and it is possible to allow the reaction to proceed more efficiently.
[0055] In addition, when the heating step is a step of heating to reflux to cause the reaction to proceed, it is more preferable that the reflux step is a step of adding acetic anhydride to the mixed solution and heating to reflux in the presence of acetic anhydride to cause the reaction to proceed. By heating to reflux in the presence of acetic anhydride in this way, the step of distilling off water can be omitted, making the process more simple.
[0056] By heating the mixture in this manner, an alicyclic tetracarboxylic acid dianhydride can be obtained. The alicyclic tetracarboxylic acid dianhydride thus obtained is not particularly limited, but for example, when the compound represented by the formula (1) is used as the raw material compound, it is possible to obtain an alicyclic tetracarboxylic acid dianhydride represented by the following formula (2):
[0057] [ka]
[0058] (X in the formula1 and multiple R 1 are the X in formula (1), 1 and multiple R 1 (Similarly, the preferred ones are the same.) Among the alicyclic tetracarboxylic dianhydrides thus obtained, from the viewpoint of improving the transparency, heat resistance, and high dimensional stability of the resulting polyimide when used as a raw material for polyimide, a compound represented by the following formula:
[0059] [ka]
[0060] (Note that these compounds are preferably selected from the group consisting of the raw material compounds represented by formula (1) (particularly X 1 The compound represented by formula (11) may be referred to as "CpODA" and the compound represented by formula (14) may be referred to as "BNBDA" for the sake of convenience.
[0061] When such a method for producing an alicyclic tetracarboxylic dianhydride according to the present invention is employed, the resulting alicyclic tetracarboxylic dianhydride has a sufficiently low residual rate (content) of ester group-containing compounds and a sufficiently low residual rate (content) of heavy substances. The reaction intermediate that can be included in the "ester group-containing compound" referred to here means a compound in which the ester group in the raw material compound has not reacted completely and the ester group remains in its structure. For example, when the raw material compound (alicyclic tetraester compound) is a compound represented by the above formula (1), the reaction intermediate can be represented by the following formulas (a) to (b):
[0062] [ka]
[0063] (In the formula, X 1represents a tetravalent organic group having a six-membered alicyclic structure, and a plurality of R 1 each independently represents one selected from the group consisting of hydrocarbon groups having 1 to 10 carbon atoms.) Examples of the compound include a compound having a structure represented by the formula (a). Each elementary reaction when converting an ester group into an acid anhydride is composed of an intermolecular reaction (ester exchange reaction) between a carboxylic acid and a raw material compound, and an intramolecular reaction (ring-closing dehydration reaction) between hydroxyl groups formed in the raw material compound. Considering that the reaction rate of an intermolecular reaction is generally much slower than that of an intramolecular reaction, the reaction intermediate is basically considered to be a compound represented by the formula (a). Here, such a reaction intermediate and an unreacted raw material compound (tetraester) all have an ester group, and even if an NMR measurement is performed to examine the content ratio of them based on the signal derived from the hydrocarbon group in the ester group, it is not possible to examine the content by separating the reaction intermediate from the unreacted raw material compound. Therefore, in this specification, when measuring the content of an ester group-containing compound (a compound having an ester group, including the unreacted raw material compound and the reaction intermediate), the content of the ester group-containing compound (ester body) is obtained by regarding all ester group-containing compounds as raw alicyclic tetraester compounds as shown below.
[0064] Hereinafter, a method for measuring the content of such ester group-containing compounds (compounds having ester groups, including unreacted raw material compounds and reaction intermediates) will be described. First, an alicyclic tetracarboxylic acid dianhydride is dissolved in deuterated DMSO (deuterated dimethyl sulfoxide) and measured by 600 MHz NMR. 1The analysis is carried out by H-NMR measurement. Next, the integral value A of the signal of the hydrocarbon group (e.g., methyl group) in the ester group is obtained from the NMR chart, and this is used as the integral value of the signal derived from the ester group-containing compound. Here, all the signals of the hydrocarbon group in the ester group are considered to be derived from the tetraester (raw material compound) (for example, when the hydrocarbon group in the ester group is a methyl group, the signal is a signal of 12 protons (because 4 methyl groups are contained in the tetraester)). Then, based on the integral value A of the signal derived from such a tetraester (raw material compound) and the integral value B of the signal (reference signal) derived from a structural part commonly contained in all compounds in the product analyzed by NMR (integral value of the signal of the common structural part contained in all compounds in the product measured), the content ratio of the ester group-containing compound is calculated taking into account the number of protons of each signal, and the residual rate (content) of the ester group-containing compound can be calculated. In this specification, the content (residual rate) of the ester group-containing compound is determined by using the area ratio value analyzed by NMR and calculating (converting) a value (mol %) assuming that all of the ester groups measured are derived from tetraesters (raw material compounds) (assuming that all of the compounds having ester groups incorporated in the reaction product are tetraesters).
[0065] Here, the residual ratio of ester group-containing compounds in the alicyclic tetracarboxylic dianhydride finally obtained by the method for producing an alicyclic tetracarboxylic dianhydride of the present invention is preferably 0.7 mol % or less (more preferably 0.6 mol % or less, and even more preferably 0.3 mol % or less). By making the residual ratio of such ester group-containing compounds equal to or less than the upper limit, when a polyimide is produced using such an alicyclic tetracarboxylic dianhydride, the tensile properties (tensile strength and elongation at break) are improved. When the method for producing an alicyclic tetracarboxylic dianhydride of the present invention is adopted, it is possible to easily make the residual ratio of ester group-containing compounds in the obtained alicyclic tetracarboxylic dianhydride (the ratio calculated from the area ratio) within the above range.
[0066] The heavy materials are presumed to be mainly derived from components contained in the alicyclic tetraester compound as a raw material compound (basically components that are mixed into the ester compound as a result of two or more compounds to be esterified being reacted (polymerized) in the production process (esterification process) of the alicyclic tetraester compound), and are contained in the finally obtained alicyclic tetracarboxylic acid dianhydride. For example, when the raw material compound (alicyclic tetraester compound) is a compound represented by the above formula (1), heavy materials are presumed to be contained in the finally obtained alicyclic tetracarboxylic acid dianhydride as a result of the following formula (c):
[0067] [ka]
[0068] (Note that in formula (c), X 1 is X in formula (1). 1 (Same meaning as above). In the present specification, the alicyclic tetracarboxylic dianhydride is subjected to GPC (gel permeation chromatography) measurement, and the content of the heavy matter (content ratio calculated from the area ratio of the peaks) is determined by assuming that all peaks detected at a time position before the peak of the alicyclic tetracarboxylic dianhydride (earlier time in the graph of time and detection intensity) are derived from the heavy matter. In the present invention, the residual rate (area ratio) of the heavy matter in the finally obtained alicyclic tetracarboxylic dianhydride is preferably 0.21% (area %) or less (more preferably 0.1% or less). By setting such a residual rate to the upper limit or less, when a polyimide is produced using the alicyclic tetracarboxylic dianhydride, the tensile properties (tensile strength and elongation at break) are improved. In addition, when the method for producing an alicyclic tetracarboxylic dianhydride of the present invention is adopted, it is possible to easily set the residual rate (area ratio) of the heavy matter in the obtained alicyclic tetracarboxylic dianhydride within the above range.
[0069] According to the method for producing an alicyclic tetracarboxylic dianhydride of the present invention, when the alicyclic tetracarboxylic dianhydride is BNBDA, the maximum particle size (long side of needle-like crystals) can be 120 μm, and when the alicyclic tetracarboxylic dianhydride is CpODA, the maximum particle size can be 1000 μm. Here, the maximum particle size is the particle size of the largest particle in the powder observed by measuring 1 g of a powder sample of the compound (1 g of powder randomly sampled) using a digital microscope (manufactured by KEYENCE Corporation, product name: VHX DIGITAL MICROSCOPE) as a measuring device.
[0070] The method for producing the alicyclic tetracarboxylic dianhydride of the present invention has been described above. Next, the method for producing the polyimide of the present invention will be described.
[0071] [Polyimide manufacturing method] The method for producing a polyimide of the present invention comprises the steps of: A step of obtaining an alicyclic tetracarboxylic dianhydride by employing the above-mentioned method for producing an alicyclic tetracarboxylic dianhydride of the present invention (hereinafter sometimes simply referred to as the "first step"); a step of reacting the alicyclic tetracarboxylic dianhydride with a diamine to obtain a polyimide (hereinafter sometimes simply referred to as the "second step"); The polyimide production method of the present invention is thus a method of obtaining a polyimide by utilizing the alicyclic tetracarboxylic acid dianhydride obtained by the above-mentioned method for producing an alicyclic tetracarboxylic acid dianhydride of the present invention and reacting the alicyclic tetracarboxylic acid dianhydride with a diamine. The polyimide production method of the present invention thus utilizes the alicyclic tetracarboxylic acid dianhydride obtained by the above-mentioned method for producing an alicyclic tetracarboxylic acid dianhydride of the present invention, and since the alicyclic tetracarboxylic acid dianhydride has a sufficiently low amount of ester group-containing compounds and heavy substances remaining in the compound, it is possible to obtain a polyimide having high tensile properties.
[0072] The first step is a step of obtaining an alicyclic tetracarboxylic dianhydride by employing the above-mentioned method for producing an alicyclic tetracarboxylic dianhydride of the present invention, i.e., a step of obtaining an alicyclic tetracarboxylic dianhydride by carrying out the above-mentioned method for producing an alicyclic tetracarboxylic dianhydride of the present invention. The preferred conditions for such a step are the same as those described in the above-mentioned method for producing an alicyclic tetracarboxylic dianhydride of the present invention. Therefore, the alicyclic tetracarboxylic dianhydride obtained in the first step is the same as the alicyclic tetracarboxylic dianhydride described in the above-mentioned method for producing an alicyclic tetracarboxylic dianhydride of the present invention (the preferred conditions are also the same).
[0073] The second step is a step of obtaining a polyimide by reacting the alicyclic tetracarboxylic dianhydride with a diamine. The diamine is not particularly limited as long as it can be used for producing a polyimide, and may be an aliphatic diamine or an aromatic diamine.
[0074] As such a diamine, from the viewpoints of heat resistance and simplicity of the polymerization method, aromatic diamines are preferable, and among them, diamines represented by the following general formula (3): HY a NR 10 -NY b H (3) [In formula (3), R 10 represents an arylene group having 6 to 50 carbon atoms; Y a and Y b each independently represents one selected from the group consisting of a hydrogen atom and an alkylsilyl group having 3 to 9 carbon atoms.] In addition, aromatic diamines represented by the following general formula (3) are more preferable. a and Y b As the alkylsilyl group which can be selected for, a trimethylsilyl group or a t-butyldimethylsilyl group is more preferable.
[0075] In addition, Y in such formula (3) a and Y bFrom the viewpoint of ease of synthesis of polyimide, it is more preferable that each of the is a hydrogen atom. 10 An aromatic diamine represented by -NH2 is more preferred.
[0076] In addition, R in the formula (3) 10 The arylene group that can be selected as has a carbon number of 6 to 50, and the carbon number of such an arylene group is preferably 6 to 40, more preferably 6 to 30, and further preferably 12 to 20. If the carbon number is less than the lower limit, the heat resistance of the finally formed polyimide tends to decrease, while if the carbon number exceeds the upper limit, the solubility of the polyimide in a solvent when it is prepared tends to decrease.
[0077] The aromatic diamine represented by formula (3) suitable as the diamine is not particularly limited, and may be any of the following: 10 A known compound containing an arylene group having 6 to 50 carbon atoms at the position (for example, aromatic diamines described in WO 2019 / 163703) can be appropriately used, and a commercially available product may also be appropriately used (in this case, 10 is a residue (divalent group: arylene group) obtained by removing two amino groups from a known aromatic diamine.
[0078] In addition, R in such formula (3) 10From the viewpoint of being able to improve the heat resistance when producing polyimide, the following compounds are used: 4,4'-diaminobenzanilide (DABAN), p-diaminobenzene (PPD), 2,2'-bis(trifluoromethyl)benzidine (TFMB), 4,4'-bis(4-aminophenoxy)biphenyl (BODA), 2,7-diaminofluorene, o-tolidine, m-tolidine, 3,3',5,5'-tetramethylbenzidine, benzidine, o-dianisidine, m-dianisidine, 3,7-diamino-2,8-dimethyl It is more preferably a divalent group (arylene group) obtained by removing two amino groups from at least one aromatic diamine selected from the group consisting of diphenylene sulfone, 4,4″-diamino-p-terphenyl, 4-aminophenyl 4-aminobenzoate, 1,4-diaminonaphthalene, 1,5-diaminonaphthalene, and 2,6-diaminonaphthalene, and even more preferably a divalent group (arylene group) obtained by removing two amino groups from at least one aromatic diamine selected from the group consisting of DABAN, TFMB, PPD, and BODA. Such aromatic diamines may be used alone or in combination of two or more.
[0079] In addition, Y in the formula (3) a and Y b As an aromatic diamine in which at least one of the groups is other than a hydrogen atom, there is an aromatic diamine having the formula: 10 Examples of the silylated diamine include those obtained by reacting an aromatic diamine represented by -NH2 with a silylating agent, such as bis(4-trimethylsilylaminophenyl)ether, 1,4-bis(trimethylsilylamino)benzene, etc. Examples of the silylating agent include N,O-bis(trimethylsilyl)trifluoroacetamide, N,O-bis(trimethylsilyl)acetamide, hexamethyldisilazane, etc.
[0080] The method for producing such a diamine is not particularly limited, and any known method can be appropriately adopted. In addition, a commercially available product may be appropriately used as such a diamine.
[0081] Furthermore, the method of synthesizing a polyimide by reacting the alicyclic tetracarboxylic dianhydride with the diamine is not particularly limited, and a method similar to that described in known polyimide synthesis methods (for example, methods described in International Publication No. WO 2011 / 099518, WO 2015 / 163314, WO 2017 / 030019, WO 2019 / 005814, etc.) (reaction conditions, etc.) can be appropriately adopted, except that the alicyclic tetracarboxylic dianhydride obtained by adopting the above-mentioned method for producing an alicyclic tetracarboxylic dianhydride of the present invention is used as the alicyclic tetracarboxylic dianhydride. In addition, a method of producing a polyimide using the varnish of the polyamic acid by adopting such a known method, for example, by reacting an alicyclic tetracarboxylic dianhydride with a diamine in a solvent to obtain a solution (varnish) of a polyamic acid may be adopted. In addition, when a polyimide is produced after obtaining a polyamic acid solution (varnish) in this way, it is preferable to make the polyamic acid varnish (resin solution) contain an imidazole compound (more preferably, 2-ethylimidazole, 1-propylimidazole, 2-aminobenzimidazole, etc.). By using an imidazole compound in this way, the heat resistance of the finally obtained polyimide tends to be higher.
[0082] The polyimide thus obtained can be, for example, a compound represented by the following general formula (4) when the alicyclic tetracarboxylic dianhydride is a compound represented by the formula (2) and the diamine is an aromatic diamine represented by the formula (3):
[0083] [ka]
[0084] [where, X 1 is X in the formula (1) 1 is synonymous with (and preferred with) R 10 is R in the above formula (3). 10 (Similarly preferred). The polyimide obtained by the present invention is produced by utilizing the alicyclic tetracarboxylic acid dianhydride obtained by employing the above-mentioned method for producing an alicyclic tetracarboxylic acid dianhydride of the present invention, and therefore can have high tensile properties. EXAMPLES
[0085] The present invention will be described in more detail below based on examples and comparative examples, but the present invention is not limited to the following examples.
[0086] (I) Synthesis of CpODA and synthesis of polyimide using CpODA I-1. Synthesis of CpODA (Synthesis Example 1) The same method as that used in Example 1 of WO 2011 / 099518 was used to obtain a compound represented by the following formula (10):
[0087] [ka]
[0088] In the following, for the sake of convenience, the compound represented by the formula (10) is referred to as "alicyclic tetraester (A)."
[0089] Example 1 First, the gas in a 300 mL three-neck flask (reaction vessel) equipped with a reflux condenser was replaced with nitrogen, and a mixture was obtained by charging the alicyclic tetraester (A) (50.0 g, 105 mmol), acetic acid (60.5 g), and γ-butyrolactone (64.1 g) at room temperature (about 25° C.) (mixture preparation step). Then, nitrogen was circulated in the reaction vessel at a flow rate of 50 to 60 mL / min to create a microflow state in the reaction vessel, and the reaction vessel was immersed in an oil bath set at a temperature of 124° C. to heat and stir the mixture in the vessel. A half-moon blade was used to stir the mixture, and the rotation speed was set to 200 rpm. The mixture was a white suspension at room temperature, but when the temperature in the vessel (temperature of the mixture) exceeded 90° C., the entire amount was dissolved and became a transparent solution. After that, after the temperature inside the container (temperature of the mixed liquid) reached 118°C, a solution containing 394 mg of trifluoromethanesulfonic acid as an acid catalyst (a solution diluted with 3.6 g of acetic acid) was dropped over 2 minutes. Next, acetic anhydride (21.4 g, 210 mmol) was dropped into the mixed liquid over 1 minute. By dropping the acid catalyst and acetic anhydride in this way, the amount of acetic anhydride per mole of the alicyclic tetraester (A) became 2 moles, and the amount of the acid catalyst per mole of the alicyclic tetraester (A) became 0.025 moles, and the ratio of the alicyclic tetraester (A) to the total amount of the solvent, acetic anhydride, acid catalyst, and alicyclic tetraester (A) (the concentration of the alicyclic tetraester (A) in the mixed liquid) became 25 mass%.
[0090] After that (after dropping acetic anhydride into the mixed solution as described above), the mixed solution in the container was heated and stirred in an oil bath. It is clear that in the reaction (acid anhydride reaction) that proceeds by continuing to heat and stir the mixed solution, methyl acetate is produced as the reaction progresses. When methyl acetate is produced as the reaction progresses, the boiling point of the mixed solution drops. Therefore, when the temperature in the container (temperature of the mixed solution) reaches 119°C by heating and stirring the mixed solution in the container, reflux begins and the reaction progresses, but the temperature in the container (temperature of the mixed solution) eventually drops to 103°C (it is clear that the drop in temperature is due to methyl acetate produced as the reaction progresses). It is confirmed that a white precipitate was produced in the liquid (mixed solution) in the flask 20 minutes after the acid catalyst was added by such a heating and stirring process (heating in an oil bath). Then, 5 hours after the addition of the acid catalyst, the flask was removed from the oil bath (the heating time from the addition of the acid catalyst to the removal of the flask from the oil bath is sometimes referred to simply as the "time required for the heating reaction step" for the sake of convenience), and the mixture in the flask (the reaction solution in which the white precipitate was generated) was left at room temperature for a whole day (24 hours), and then the white solid was filtered under reduced pressure using filter paper to separate the white solid from the reaction solution. The white solid thus obtained was then washed with ethyl acetate, and then subjected to a step of drying under reduced pressure to obtain 35.6 g (yield 88.2%) of a product consisting of a white powder.
[0091] The product thus obtained was found to be a compound represented by the following formula (11):
[0092] [ka]
[0093] It was confirmed that the compound was CpODA. 1 g of the powder was randomly sampled from the product (white powder) obtained in this manner and observed with a digital microscope (Keyence Corporation, product name: VHX DIGITAL MICROSCOPE) to measure the particle size of the largest particle contained in the powder. It was found that the maximum particle size of the particles in the powder was 1000 μm, and that the powder was composed of relatively large particles.
[0094] Example 2 Except for using a solvent consisting of 34.9 g of acetic acid and 89.7 g of γ-butyrolactone instead of the above solvent, the same procedure as in Example 1 was repeated to obtain 35.4 g (yield 85.1%) of a product (CpODA) consisting of a white powder.
[0095] Comparative Example 1 Instead of the solvent, a solvent consisting of 128.1 g of acetic acid was used (γ-butyrolactone was not used as the solvent, and only acetic acid was used as the solvent) and the duration of the heating reaction step was changed to 7 hours, and 37.9 g (yield 93.9%) of a product consisting of a white powder (CpODA) was obtained in the same manner as in Example 1. The maximum particle size of the product (white powder) obtained in Comparative Example 1 was measured in the same manner as in Example 1, and it was found that the maximum particle size of the particles in the powder was 200 μm.
[0096] <Measurement of the content (residual rate) of ester group-containing compounds and heavy substances contained in the product CpODA> Measurement of the residual ratio of ester group-containing compounds in CpODA The products (CpODA) obtained in Examples 1 and 2 and Comparative Example 1 were used to measure the residual rate of the ester group-containing compound as follows. Although various forms of such ester group-containing compounds (compounds with unreacted ester groups remaining) are conceivable, for convenience, the residual rate of the ester group-containing compound was determined assuming that all ester group-containing compounds were unreacted raw material compounds (tetraesters: compounds represented by the above formula (1)). That is, first, CpODA was dissolved in deuterated DMSO (deuterated dimethyl sulfoxide) and analyzed by 600 MHz NMR. 1 H-NMR measurement was performed, and from the obtained NMR chart, the integral value (peak area) A of the signal (3.52 ppm) of the methyl group (equivalent to three protons) in the methyl ester and the integral value (peak area) B (integral value serving as a reference for the amount of all compounds in the product) of the signal (reference signal: 1.14 ppm) of the common structural portion contained in the product (all compounds including the ester group-containing compound) were calculated. Next, based on the integral value A and the integral value B, the remaining amount of the ester group-containing compound was calculated according to the following formula (X): [Remaining amount of ester group-containing compound (mol%)] = ([Converted value of integral value A when integral value B is set to 100] ÷ 600) × 100 (X) It should be noted that such calculation formula (X) is obtained by calculating the following: the integral value (peak area value) B is the integral value of the signals of two of the four protons at the norbornane bridgehead position that can be used as an index of the content of all compounds in the product (note that such signals are signals measured from both the CpODA and tetraester compounds), and the integral value (peak area value) A is the integrated amount of 12 protons (protons in four tetramethyl groups) if it is assumed that all ester groups are derived from unreacted tetraesters. Therefore, the value of [integral value B] / 2 is the area that is an index of the amount of all compounds, and the value of [integral value A] / 12 is the area that is an index of the amount of tetraester. Therefore, the calculation formula (X) can be obtained by calculating the following formula: {([Integral value A] / 12)÷([Integral value B] / 2)}×100 This formula was derived based on the fact that the calculated value of (which can be transformed into the calculated value of the formula: ([integral value A] / [integral value B])×(1 / 6)×100) corresponds to the content (mol%) of tetraester (ester group-containing compound). The obtained results are shown in Table 1.
[0097] <Measurement of the residual rate of heavy substances in CpODA> Using the products (CpODA) obtained in Examples 1 and 2 and Comparative Example 1, GPC measurement was performed for each CpODA, and a graph of the relationship between time and detection intensity was obtained. It was assumed that all peaks measured at a time before the time when the CpODA peak was confirmed were derived from heavy substances, and the residual rate of heavy substances (area ratio: area %) was calculated. Note that examples of such heavy substances include those represented by the following formula (12):
[0098] [ka]
[0099] In this specification, any peak observed before the peak of the product (CpODA) is considered to be a peak derived from a heavy matter.
[0100] The GPC measurement for determining the residual rate of the heavy substances was performed using a measuring device "TOSOH HLC-8220GPC" manufactured by Tosoh Corporation, and further using one "TOSOH TSKguardcolumn SuperMP(HZ)-M" manufactured by Tosoh Corporation and three "TOSOH TSKgelSuperMultiporeHZ-M" manufactured by Tosoh Corporation connected together as columns. In addition, in such GPC measurement, a differential refractometer (RI detector) was used as a detector, and tetrahydrofuran (THF) was used as a solvent. Furthermore, 2 mg of each product was used as a sample in the measurement. Furthermore, in the GPC measurement, a measurement sample was prepared by dissolving 2 mg of the sample in 1.5 mL of THF, and the GPC measurement was performed under the conditions of a flow rate of 0.35 ml / min and an injection amount of 25 μl. The obtained results are shown in Table 1.
[0101] [Table 1]
[0102] As is clear from the results shown in Table 1, in all cases where γ-butyrolactone was used together with acetic acid as a solvent (Examples 1 and 2), the residual rate of ester group-containing compounds was 0.7 mol % or less, and the residual rate of heavy substances was 0.21 area % or less (specifically, 0.044 area % or less). Comparing the results of Examples 1 and 2 with the results of the residual rates of ester group-containing compounds and heavy substances in CpODA obtained in Comparative Example 1, it was confirmed that the residual rates of ester group-containing compounds and heavy substances were both sufficiently reduced according to the method adopted in Examples 1 and 2. In addition, considering that the content (concentration) of alicyclic tetraester (A) in the mixed liquid used for reflux in Examples 1 and 2 and Comparative Example 1 was 25 mass %, it was also found that the method adopted in Examples 1 and 2 could efficiently produce CpODA in which the residual rates of ester group-containing compounds and heavy substances were sufficiently reduced. In Example 1, large particles with a maximum particle size of 1000 μm were confirmed, and it was found that the present invention also makes it possible to obtain a compound (CpODA) with a large particle size.
[0103] (Comparative Examples 2 to 7) The production of CpODA was attempted in the same manner as in Example 2, except that dimethyl sulfoxide (used in Comparative Example 2), N,N-dimethylformamide (used in Comparative Example 3), 1,3-dimethyl-2-imidazolidinone (used in Comparative Example 4), acetylacetone (used in Comparative Example 5), propylene glycol monomethyl ether acetate (used in Comparative Example 6) or N-methyl-2-pyrrolidone (used in Comparative Example 7) was used instead of γ-butyrolactone. However, CpODA was not produced, and only the raw material was recovered. Considering the results of Comparative Examples 2 to 7 in which other organic solvents were used instead of γ-butyrolactone, together with the results of Examples 1 and 2, it became clear that the method adopted in Examples 1 and 2 made it possible to efficiently produce CpODA while sufficiently reducing the residual rate of both ester group-containing compounds and heavy substances.
[0104] I-2. Synthesis of polyimide Example 3 In a nitrogen atmosphere, 3.84 g (10 mmol) of 4,4'-diaminobenzanilide (DABAN) was introduced into a 30 mL screw tube, and 2.27 g (10 mmol) of CpODA obtained in Example 1 was introduced. Next, 24.5 g of N-methyl-2-pyrrolidone (NMP) as a solvent was added to the screw tube to obtain a mixture having a ratio (content) of the total amount of diamine and tetracarboxylic dianhydride (total amount of monomers) of 20 mass%. Next, the obtained mixture was stirred at 80°C under a nitrogen atmosphere to confirm dissolution of crystals, and then further stirred at room temperature (about 25°C) for 4 days to form polyamic acid in the solution, thereby obtaining a reaction solution containing polyamic acid. Next, 2-ethylimidazole in an amount (0.61 g) equivalent to 10 mass % of the total amount of diamine and CpODA used in the production of the polyamic acid (total amount of monomers: 6.12 g) was added to the reaction solution, and the mixture was stirred at room temperature for 1 hour to obtain a varnish (resin solution) for producing polyimide, which contains a solvent (NMP), 2-ethylimidazole, and polyamic acid.
[0105] Next, the varnish was applied to a glass substrate having a size of 76 mm in length and 52 mm in width using a spin coater to form a coating film on the glass substrate. Then, the glass substrate on which the coating film was formed was set in a vacuum hot chamber, and a process of heating at 70°C for 60 minutes under reduced pressure conditions (pressure: 150 Pa) was carried out to remove the solvent from the coating film. Then, the glass substrate on which the coating film was laminated after the solvent removal was set in the heating chamber of an inert oven, and nitrogen purging was carried out in the heating chamber. Next, the temperature of the inert oven was raised to 380°C and held for 1 hour (the conditions of the heating temperature and holding time are sometimes referred to as "film-forming heating conditions" below), and then the inert oven was operated so as to cool to room temperature (about 25°C), thereby forming polyimide on the glass substrate, and a glass substrate coated with a film made of polyimide was obtained. Next, the film made of polyimide was peeled off from the glass substrate to obtain a colorless and transparent film made of polyimide. Table 2 shows the film thickness of the obtained polyimide and the type of monomer used.
[0106] (Example 4 and Comparative Example 8) A colorless and transparent polyimide film was obtained in the same manner as in Example 3, except that the CpODA obtained in Example 2 (used in Example 4) or the CpODA obtained in Comparative Example 1 (used in Comparative Example 8) was used instead of the CpODA obtained in Example 1. The film thickness of the obtained polyimide and the type of monomer used in each Example are shown in Table 2.
[0107] <Evaluation of polyimide properties> The tensile strength (unit: MPa) and breaking elongation (unit: %) of the polyimide film obtained in each of Examples 3 to 4 and Comparative Example 8 were measured as follows. That is, first, a "Super Dumbbell Cutter (type: SDMK-1000-D, conforming to the A22 standard of JIS K7139 (issued in 2009))" made by Dumbbell Co., Ltd. was attached to an SD type lever type sample cutter (a cutter (model SDL-200) made by Dumbbell Co., Ltd.) to cut the polyimide film to the following dimensions: total length: 75 mm, distance between tabs: 57 mm, length of parallel part: 30 mm, radius of shoulder: 30 mm, width of end: 10 mm, width of parallel part in the center: 5 mm, thickness: 13 μm. Dumbbell-shaped test pieces (thickness of the test piece was the thickness of the film obtained in each Example, but conforming to the standard of JIS K7139 type A22 (scale test piece)) were prepared as measurement samples. Next, using a Tensilon type universal testing machine (for example, model number "UCT-10T" manufactured by A&D Co., Ltd.), the measurement sample was arranged so that the width between the grips was 57 mm and the width of the gripped portion was 10 mm (full width of the end), and then the measurement sample was pulled under the conditions of a full scale load of 0.05 kN and a test speed of 5.00 mm / min to perform a tensile test to determine the tensile strength and breaking elongation values. Note that such a test was a test in accordance with JIS K7162 (published in 1994). The breaking elongation value (%) was calculated by the following formula, where L0 is the distance between the tabs of the sample before the start of the tensile test (= width between the grips: 57 mm) and L is the distance between the tabs of the sample until it breaks in the tensile test (width between the grips at the time of breakage: 57 mm + α): [Elongation at break (%)] = {(L-L0) / L0} x 100 The results are shown in Table 2.
[0108] [Table 2]
[0109] As is clear from the results shown in Table 2, it was confirmed that when polyimides were produced using the CpODA obtained in Examples 1 and 2 (Examples 3 and 4), the tensile properties based on the tensile strength and elongation at break were superior to those when polyimides were produced using the CpODA obtained in Comparative Example 1 (Comparative Example 8). These results demonstrated that when tetracarboxylic dianhydrides with reduced contents of ester group-containing compounds and heavy substances were used (Examples 3 to 5), it was possible to further improve the tensile properties of the resulting polyimides.
[0110] [(II) Synthesis of BNBDA and synthesis of polyimide using BNBDA] II-1. Synthesis of BNBDA (Synthesis Example 2) The same method as that used in Example 1 of WO 2017 / 030019 was used to obtain a compound represented by the following formula (13):
[0111] [ka]
[0112] In the following, for the sake of convenience, the compound represented by the formula (13) is referred to as "alicyclic tetraester (B)".
[0113] Example 5 A 1 L flask equipped with a reflux condenser was used instead of a 300 mL flask equipped with a reflux condenser, the mixed solution preparation step was changed to a step of obtaining a mixed solution by charging 30 g of the alicyclic tetraester (B), 102.6 g of acetic acid, and 102.6 g of γ-butyrolactone into a 1 L flask equipped with a reflux condenser, the amount of trifluoromethanesulfonic acid as an acid catalyst added to the mixed solution was changed to 0.266 g, the amount of acetic anhydride added to the mixed solution was changed to 14.5 g, and the implementation time of the heating reaction step was changed to 6.5 hours. Except for this, 21.3 g (yield 90.7%) of a product (BNBDA) consisting of a white powder was obtained in the same manner as in Example 1. In Example 5, the amount of acetic anhydride relative to 1 mole of the alicyclic tetraester (B) was 2 moles, the amount of the acid catalyst relative to 1 mole of the alicyclic tetraester (B) was 0.025 moles, and the ratio of the alicyclic tetraester (B) to the total amount of the solvent, acetic anhydride, acid catalyst, and alicyclic tetraester (A) (the concentration of the alicyclic tetraester (A) in the mixed liquid) was 12 mass%.
[0114] [ka]
[0115] It was confirmed that the compound was BNBDA.
[0116] Example 6 A 200 L reaction vessel capable of refluxing was used instead of the 1 L flask equipped with a reflux condenser, a solvent consisting of 10.3 kg of acetic acid and 92.4 kg of γ-butyrolactone was used instead of the solvent, the amount of the alicyclic tetraester (B) used was changed to 15 kg, the amount of trifluoromethanesulfonic acid as an acid catalyst added to the mixture was changed to 0.133 kg, the amount of acetic anhydride added to the mixture was changed to 7.25 kg, and the duration of the heating reaction step was changed to 6 hours. Except for this, 10.97 kg (yield 93.5%) of a product (BNBDA) consisting of a white powder was obtained in the same manner as in Example 5.
[0117] Comparative Example 9 A solvent consisting of 205.2 g of acetic acid was used instead of the above solvent (γ-butyrolactone was not used as a solvent, and only acetic acid was used as a solvent) and the duration of the heating reaction step was changed to 7 hours. In the same manner as in Example 5, 23.0 g (yield 98.2%) of a product consisting of a white powder (BNBDA) was obtained.
[0118] <Measurement of the content (residual rate) of ester group-containing compounds and heavy substances contained in the product BNBDA> Measurement of the Residual Rate of Ester Group-Containing Compounds in BNBDA The residual ratio of the ester group-containing compound in the product (BNBDA) obtained in Examples 5 to 6 and Comparative Example 9 was determined as follows. That is, the measurement target was changed from CpODA to BNBDA, and all of the ester group-containing compounds were considered to be compounds represented by the above formula (13) (unreacted raw material compound: tetraester) when determining the residual ratio, but the same method as that employed in the above-mentioned "Measurement of the residual ratio of the ester group-containing compound in CpODA" was employed to determine the residual ratio of the ester group-containing compound. The residual ratio (mol%) was calculated using the integral value (peak area) A of the signal (3.52 ppm) of the methyl group in the methyl ester and the integral value (peak area) B of the reference signal (1.2 ppm: the signal of the proton at one of the two norbornane bridgehead positions, which is a structural part commonly contained in all the compounds) of all the compounds (BNBDA and the ester group-containing compound) (the calculation formula was the same as the above formula (X)). The results obtained are shown in Table 3.
[0119] <Measurement of the residual rate of heavy substances in BNBDA> Using the products (BNBDA) obtained in Examples 5 to 6 and Comparative Example 9, GPC measurement was performed for each BNBDA, a graph of the relationship between time and detection intensity was obtained, and the residual rate of heavy substances (area ratio: area %) was obtained by assuming that all peaks measured at a time before the time when the BNBDA peak was confirmed were derived from heavy substances. Note that, as a specific measurement method, the same method as that adopted in the above-mentioned "Measurement of the residual rate of heavy substances in CpODA" was adopted, except that BNBDA was used instead of CpODA. The obtained results are shown in Table 3.
[0120] [Table 3]
[0121] As is clear from the results shown in Table 3, in all cases where γ-butyrolactone was used together with acetic acid as a solvent (Examples 5 to 6), the residual rate of ester group-containing compounds was 0.7 mol % or less, and the residual rate of heavy substances was 0.21 area % or less. Comparing the results of Examples 5 to 6 with the results of the residual rates of ester group-containing compounds and heavy substances in BNBDA obtained in Comparative Example 9, it was confirmed that the residual rates of ester group-containing compounds and heavy substances were both sufficiently reduced according to the method adopted in Examples 5 to 6. In addition, considering that the content of alicyclic tetraester (B) in the mixed liquid was 12 mass % in both Examples 5 to 6 and Comparative Example 9, it was also found that the method adopted in Examples 5 to 6 could efficiently produce BNBDA in which the residual rates of ester group-containing compounds and heavy substances were sufficiently reduced.
[0122] <II-2> Synthesis of Polyimide (Examples 7 to 8 and Comparative Example 10) Polyimide (polyimide film) was obtained in the same manner as in Example 3, except that BNBDA obtained in Example 5 (used in Example 7), BNBDA obtained in Example 6 (used in Example 8), or BNBDA obtained in Comparative Example 9 (used in Comparative Example 10) was used instead of CpODA obtained in Example 1, and the amount of BNBDA used was 3.3033 g (10.0 mmol) in each case. The film thickness of the obtained polyimide and the type of monomer used in each Example are shown in Table 4.
[0123] The tensile strength (unit: MPa) and breaking elongation (unit: %) of the polyimide films obtained in Examples 7-8 and Comparative Example 10 were measured using the same method as that used in the above "Evaluation of polyimide properties" except that the polyimide films obtained in Examples 7-8 and Comparative Example 10 were used instead of the polyimide films obtained in Examples 3-4 and Comparative Example 8. The results are shown in Table 4.
[0124] [Table 4]
[0125] As is clear from the results shown in Table 4, it was confirmed that when polyimides were produced using the BNBDA obtained in Examples 5 and 6 (Examples 7 and 8), the tensile properties based on the tensile strength and elongation at break were superior to those when polyimides were produced using the BNBDA obtained in Comparative Example 9 (Comparative Example 10). From these results, it was found that when ester group-containing compounds (compounds having ester groups including unreacted raw materials and reaction intermediates) and tetracarboxylic dianhydrides with reduced contents of heavy substances were used (Examples 7 and 8), it was possible to further improve the tensile properties of the resulting polyimides. [Industrial Applicability]
[0126] As described above, according to the present invention, even when a mixed solution containing high concentrations of raw materials is used, it is possible to reduce the residual rate of ester group-containing compounds and heavy substances in the reaction product, and it is possible to provide a method for producing an alicyclic tetracarboxylic acid dianhydride capable of efficiently producing an alicyclic tetracarboxylic acid dianhydride having a reduced residual rate of ester group-containing compounds and heavy substances, and a method for producing a polyimide using the method. Therefore, the method for producing an alicyclic tetracarboxylic acid dianhydride of the present invention is particularly useful as a method for producing an alicyclic tetracarboxylic acid dianhydride to be used as a polyimide monomer, for example.
Claims
1. a solvent consisting of a carboxylic acid having 1 to 5 carbon atoms and γ-butyrolactone, the content of said γ-butyrolactone being 20 to 92 mass% based on the total amount of said γ-butyrolactone and said carboxylic acid; an alicyclic tetraester compound; A method for producing an alicyclic tetracarboxylic dianhydride, comprising heating a mixed liquid containing:
2. 2. The method for producing an alicyclic tetracarboxylic dianhydride according to claim 1, wherein the mixed solution further contains an acid catalyst.
3. 2. The method for producing an alicyclic tetracarboxylic dianhydride according to claim 1, wherein the mixed solution further contains acetic anhydride.
4. The alicyclic tetraester compound is represented by the following formula (1): 【Chemistry 1】 (In the formula, X 1 represents a tetravalent organic group having a 6-membered alicyclic structure, and a plurality of R 1 Each independently represents one selected from the group consisting of hydrocarbon groups having 1 to 10 carbon atoms. The method for producing an alicyclic tetracarboxylic dianhydride according to claim 1, wherein the compound is represented by the formula:
5. 2. The method for producing an alicyclic tetracarboxylic dianhydride according to claim 1, wherein the content of the alicyclic tetraester compound in the mixed solution is 10 to 30% by mass.
6. A step of obtaining an alicyclic tetracarboxylic dianhydride by employing the method for producing an alicyclic tetracarboxylic dianhydride according to any one of claims 1 to 5; a step of reacting the alicyclic tetracarboxylic dianhydride with a diamine to obtain a polyimide; A method for producing a polyimide, comprising:
Citation Information
Patent Citations
Norbornane-2-spiro-?-cycloalkanone-?'-spiro-2''-norbornane-5,5'',6,6''-tetracarboxylic dianhydride, norbornane-2-spiro-?-cycloalkanone-?'-spiro-2''-norbornane-5,5'',6,6''-tetracarboxylic acid and ester thereof, method for producing norbornane-2-spiro
WO2011099518A1