Surface treated copper foil, copper-clad laminate, and print circuit board

The surface-treated copper foil with controlled nickel layer properties addresses magnetization issues, ensuring reduced transmission loss and improved heat resistance, suitable for high-frequency printed wiring boards.

JP2024145588AInactive Publication Date: 2024-10-15FURUKAWA ELECTRIC CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023058012
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing surface-treated copper foils used in printed wiring boards face issues with nickel layers becoming magnetized during heat treatment, leading to deteriorated transmission characteristics and compromised heat resistance due to the trade-off relationship between the two.

Method used

A surface-treated copper foil with a nickel-containing surface treatment layer that maintains saturation magnetic flux density and residual magnetic flux density at specific low levels, along with controlled crystal grain size and surface roughness, to suppress magnetization and enhance transmission characteristics and heat resistance.

Benefits of technology

The copper foil effectively reduces magnetization and transmission loss while maintaining excellent heat resistance, suitable for high-frequency applications and printed wiring boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145588000001
    Figure 2024145588000001
  • Figure 2024145588000002
    Figure 2024145588000002
Patent Text Reader

Abstract

To provide a surface-treated copper foil, a copper-clad laminate, and a printed circuit board that can suppress magnetization of a nickel layer even after prescribed heat treatment and exhibit excellent transmission characteristics and heat resistance.SOLUTION: A surface treatment copper foil having a surface treatment film including a nickel-containing surface treatment layer on at least one side of a copper foil substrate, where a saturation magnetic flux density (Bs300) is 5.0×10-3T or less after heat treatment at 300°C for 2 hours.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a surface-treated copper foil, a copper-clad laminate, and a printed wiring board. [Background technology]

[0002] Surface-treated copper foils are used in a variety of applications, such as copper foils for circuits in printed wiring boards and negative electrode current collectors in lithium-ion secondary batteries.

[0003] In particular, in the field of printed wiring boards, the increasing need for smaller electronic devices and higher performance in recent years has led to higher density mounting of mounted components and higher frequency signals, requiring printed wiring boards to be able to handle high frequencies.

[0004] In the case of copper foil for circuits used in such printed wiring boards, the surface condition of the circuit conductor, that is, the dissimilar metal treated on the surface, becomes important as the frequency increases due to the influence of the skin effect. In particular, nickel (Ni), which is widely used as a dissimilar metal, is a metal that exhibits ferromagnetic properties at room temperature. Therefore, when nickel is present on the surface of copper foil for circuits, the current distribution and magnetic field distribution in the conductor are affected by the effect of magnetism, resulting in a problem of deterioration of the transmission characteristics of the surface-treated copper foil.

[0005] On the other hand, when producing a printed wiring board, it is necessary to laminate a copper foil for circuits and a resin substrate, and in this case, good adhesion is required between the copper foil and the resin substrate, and in particular, heat-resistant adhesion (hereinafter sometimes simply referred to as "heat resistance"). Nickel on the surface of the copper foil for circuits plays an important role in providing such heat resistance. In other words, the presence of nickel on the surface of the copper foil for circuits is in a trade-off relationship between the transmission characteristics and the heat resistance.

[0006] Known examples aimed at improving both of the above characteristics include the techniques of Patent Documents 1 and 2. Patent Document 1 proposes controlling the total amount of Co, Ni, and Mo deposited in the surface treatment layer of the copper foil to a predetermined amount or less and forming particles of a predetermined shape in the surface treatment layer in order to suppress the influence of ferromagnetic metals on the transmission characteristics. Patent Document 2 also proposes a surface-treated copper foil in which the magnetism is controlled to a predetermined condition (demagnetized) by controlling the manufacturing process of the base foil (copper foil substrate) of the surface-treated copper foil. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent No. 7055049 [Patent Document 2] Patent No. 7174869 Summary of the Invention [Problem to be solved by the invention]

[0008] However, in both Patent Documents 1 and 2, only the magnetism of the surface-treated copper foil without thermal history after production was considered, and no consideration was given to the effects of thermal compression bonding with a resin substrate or thermal load during solder reflow in the manufacturing process of a printed wiring board.

[0009] In response to this, the present inventors conducted extensive research and found that even if a surface-treated copper foil having a surface treatment film containing a nickel-containing surface treatment layer (hereinafter simply referred to as a "nickel layer (Ni layer)") is demagnetized without having a thermal history after production, when the surface-treated copper foil as a circuit conductor is subjected to a heat treatment in the process of producing a printed wiring board as described above, the nickel layer in the surface treatment film of the surface-treated copper foil may subsequently exhibit magnetism (become magnetized). As described above, when the nickel layer in the surface treatment film of the surface-treated copper foil serving as a circuit conductor is magnetized due to the heat treatment that is performed during the manufacturing process of the printed wiring board, this leads to a problem of deterioration in transmission characteristics. Therefore, there is a demand for a surface-treated copper foil that can suppress magnetization of the nickel layer even after a specified heat treatment and can exhibit excellent transmission characteristics and heat resistance.

[0010] Therefore, an object of the present invention is to provide a surface-treated copper foil, a copper-clad laminate, and a printed wiring board that can suppress magnetization of the nickel layer even after a specified heat treatment and exhibit excellent transmission characteristics and heat resistance. [Means for solving the problem]

[0011] That is, the gist of the present invention is as follows. [1] A surface-treated copper foil having a surface treatment film including a nickel-containing surface treatment layer on at least one surface of a copper foil substrate, Saturation magnetic flux density (Bs) after heat treatment at 300℃ for 2 hours 300 ) is 5.0 × 10 -3 Surface-treated copper foil with a resistance of 0.1 to 1000 MPa. [2] Residual magnetic flux density (Br 300 ) is 5.0 × 10 -4 The surface-treated copper foil according to the above-mentioned [1], wherein the surface roughness (T) is T or less. [3] The surface-treated copper foil according to the above [1] or [2], which satisfies the following requirements (I) and (II): Requirement (I): The rate of increase in saturation magnetic flux density Bs after heat treatment at 300°C for 2 hours [{(Bs 300 -Bs0) / Bs0}×100] is 300% or less. Requirement (II): The increase rate of residual magnetic flux density Br after heat treatment at 300°C for 2 hours [{(Br 300 -Br0) / Br0}×100] is 300% or less. In the above requirements (I) and (II), Bs 300 is the saturation magnetic flux density after heat treatment at 300°C for 2 hours, Bs0 is the saturation magnetic flux density before the heat treatment, Br 300 is the residual magnetic flux density after heat treatment at 300° C. for 2 hours, and Br0 is the residual magnetic flux density before the heat treatment. [4] On the surface having the surface treatment film, the nickel adhesion amount is 0.02 mg / dm 2 or more and 3.0 mg / dm 2 or less. The surface-treated copper foil according to any one of [1] to [3] above. [5] The surface treatment film includes, in order from the copper foil substrate side, a roughened treatment layer and a surface treatment layer containing the nickel, On the surface of the surface treatment film, the arithmetic mean height Sa measured optically in accordance with ISO25178 is 0.02 μm or more and 0.35 μm or less. The surface-treated copper foil according to any one of [1] to [4] above. [6] The surface treatment layer containing the nickel is composed of a nickel alloy containing one or more elements selected from the group consisting of zinc, phosphorus, molybdenum, tungsten, chromium, iron, cobalt, and niobium. The surface-treated copper foil according to any one of [1] to [5] above. [7] A copper-clad laminate including the surface-treated copper foil according to any one of [1] to [6] above. [8] A printed wiring board including the copper-clad laminate according to [7] above. [Advantages of the Invention]

[0012] According to the present invention, even after a predetermined heat treatment, it is possible to suppress magnetization of the nickel layer, and it is possible to provide a surface-treated copper foil, a copper-clad laminate, and a printed wiring board that can exhibit excellent transmission characteristics and heat resistance. [Embodiments for Carrying Out the Invention]

[0013] Embodiments of the surface-treated copper foil, copper-clad laminate, and printed wiring board according to the present invention will be described in detail below. In this specification, the term "A to B" regarding the description of numerical values means "A or more and B or less" (when A < B) or "A or less and B or more" (when A > B). Also, in the present invention, a combination of preferred embodiments is a more preferred embodiment.

[0014] [Surface-Treated Copper Foil] The surface-treated copper foil of the present invention has a surface treatment film including a nickel-containing surface treatment layer on at least one surface of a copper foil substrate, and has a saturation magnetic flux density (Bs 300 ) is 5.0 × 10 -3 It is less than T.

[0015] The surface-treated copper foil of the present invention has the above-mentioned structure, and therefore can suppress magnetization of the nickel layer even after a specified heat treatment, and can exhibit excellent transmission characteristics and heat resistance. Although the detailed reason why such an effect is obtained is not clear, one of the possible reasons is as follows.

[0016] First, in order to solve the above problems, the present inventors focused on suppressing magnetization in the nickel layer after heat treatment and conducted extensive research. As a result of research, the inventors have found that in surface-treated copper foil having a conventional surface treatment film containing a nickel layer, (1) the magnetic flux density increases by undergoing a specified heat treatment, and (2) in copper foil types in which the increase is large, the transmission loss in the high frequency band becomes significantly large. The reason why the magnetic flux density increases in the surface-treated copper foil after a specified heat treatment is not clear, but one reason is thought to be that the heat treatment causes crystallization and / or an increase in crystal grain size in the nickel layer, which magnetizes the nickel layer after the heat treatment.

[0017] Therefore, the inventors of the present invention conducted further research and improved the nickel layer, which made it possible to suppress the nickel layer from being magnetized by heat treatment, and the saturation magnetic flux density (Bs 300 ) is 5.0 × 10 -3 It has been found that a surface-treated copper foil having a thickness of 0.1 mm or less can be obtained, and that such a surface-treated copper foil can reduce transmission loss and also exhibit excellent heat resistance. Here, the relationship between saturation magnetic flux density and transmission loss is not entirely clear. However, it is thought that the influence of the surface condition of the circuit conductor becomes greater as the frequency increases, and that the adhesion of ferromagnetic metal to the circuit conductor increases the transmission loss of high-frequency signals due to losses caused by the generation of eddy currents (losses caused by an increase in the electrical resistance of the circuit conductor due to the generation of eddy currents) and magnetic hysteresis losses. Therefore, in the present invention, by controlling the saturation magnetic flux density of the nickel layer to a predetermined value or less, the magnetism of the circuit conductor can be made to a level that does not affect transmission loss in the high frequency band, and it is believed that this can significantly reduce transmission loss. Moreover, it is believed that the surface-treated copper foil of the present invention can also exhibit excellent heat resistance by including a nickel layer as a surface treatment film. The surface-treated copper foil of the present invention is preferably used for printed wiring board applications, for example. When the surface-treated copper foil of the present invention is used, both reduced transmission loss and excellent heat resistance can be achieved.

[0018] The surface-treated copper foil of the present invention will be described in detail below.

[0019] The surface-treated copper foil of the present invention has a surface treatment film including a nickel-containing surface treatment layer on at least one surface of a copper foil substrate.

[0020] <Copper foil base> The copper foil substrate serves as a base layer for the surface-treated copper foil. The copper foil substrate may be an electrolytic copper foil or a rolled copper foil, preferably an electrolytic copper foil. The thickness of the copper foil substrate is, for example, 5 to 210 μm, preferably 5 to 100 μm, and more preferably 5 to 40 μm. In addition, when the copper foil substrate is an electrolytic copper foil, the surface treatment film may be the surface (hereinafter referred to as the "drum surface") derived from the peeled surface of the electrolytic copper foil from a rotating drum-shaped cathode (hereinafter simply referred to as the "drum-shaped cathode"), or the surface opposite to the drum surface (hereinafter referred to as the "non-drum surface"), but is preferably the non-drum surface. In general, the drum surface is sometimes called the glossy surface (S surface), and the non-drum surface is sometimes called the deposition surface or matte surface (M surface).

[0021] <Surface treatment film> The surface treatment film is a layer formed on at least one surface of a copper foil substrate, and serves to impart a desired function to the surface-treated copper foil. The surface treatment film may be formed on either the front or back surface of the copper foil substrate, or on both surfaces. The surface treatment film also includes a nickel layer. Specifically, the surface treatment film may be composed of only a nickel layer, or may include one or more other surface treatment layers. Other surface treatment layers include, for example, a roughening treatment layer formed on a copper foil substrate, an intermediate layer such as a surface treatment layer containing zinc (Zn) (hereinafter sometimes referred to as a "zinc layer (Zn layer)") formed on a nickel layer and a surface treatment layer containing chromium (Cr) (hereinafter sometimes referred to as a "chromium layer (Cr layer)"), and a chemical adhesion layer formed using a silane coupling agent or the like.

[0022] The surface of the surface treatment film is at least one of the front and back surfaces of the surface-treated copper foil, and is the surface of the copper foil substrate having a surface treatment film containing a nickel layer. The surface of such a surface treatment film may be the surface of a nickel layer formed on a copper foil substrate, or it may be the surface of another surface treatment layer (e.g., a chemical adhesion layer formed by a silane coupling agent) formed directly or indirectly on the nickel layer. Furthermore, when the surface-treated copper foil of the present invention is used for the conductor circuit of a printed wiring board, the surface of the above-mentioned surface treatment film, preferably the surface of the above-mentioned surface treatment film further including a roughening treatment layer, becomes the surface (adhesion surface) for adhering and laminating a resin substrate.

[0023] (Surface treatment layer containing nickel) The surface treatment film includes a surface treatment layer (nickel layer) containing nickel. The nickel layer serves as a base layer for the surface-treated copper foil.

[0024] The nickel layer may be any layer containing nickel, and may be a single layer or a multilayer having two or more layers of different compositions laminated together. From the viewpoint of ease of production, however, a single layer is preferable.

[0025] The nickel layer may be composed of nickel alone or an alloy of nickel and other elements (hereinafter also referred to as "nickel alloy"), but from the viewpoint of being able to exhibit excellent heat resistance while reducing transmission loss, it is preferable that the nickel layer be composed of a nickel alloy. The nickel alloy is preferably a nickel alloy containing one or more elements selected from the group consisting of zinc (Zn), phosphorus (P), molybdenum (Mo), tungsten (W), chromium (Cr), iron (Fe), cobalt (Co) and niobium (Nb), and more preferably a nickel alloy containing one or more elements selected from the group consisting of Zn, P, Mo, W, Cr and Co. More specifically, the nickel alloy is preferably one or more selected from the group consisting of Ni-P, Ni-Zn, Ni-Mo, Ni-W, Ni-Cr, Ni-Co, Ni-Zn-P, Ni-Zn-Mo and Ni-Zn-Cr. The metal or alloy composition constituting the nickel layer can be confirmed by the method described in the Examples.

[0026] On the surface having the surface treatment film, the nickel coating amount is preferably 0.02 mg / dm 2 More than 3.5mg / dm 2 Less than or equal to 0.02 mg / dm 2 More than 3.0 mg / dm 2 Less than 0.02 mg / dm 2 More than 2.0 mg / dm 2 Less than 0.02 mg / dm2 More than 1.0 mg / dm 2 By setting the thickness within the above range, it is possible to reduce transmission loss and exhibit excellent heat resistance. The amount of nickel deposited on the surface having the surface treatment film can be measured by the method described in the Examples.

[0027] (Other surface treatment layers) The surface treatment film may further include other surface treatment layers in addition to the nickel layer, as necessary. Other surface treatment layers include, for example, a roughening treatment layer formed on a copper foil substrate, an intermediate layer such as a Zn layer and a Cr layer formed on a Ni layer, and a chemical adhesion layer formed by a silane coupling agent.

[0028] <Magnetic properties of surface-treated copper foil> The surface-treated copper foil of the present invention has a saturation magnetic flux density (Bs 300 ) is 5.0×10 -3 T or less, preferably 2.0×10 -3 T or less, preferably 7.0×10 -4 T or less. By setting the temperature within the above range, the occurrence of magnetism due to heating can be reduced, transmission loss can be reduced, and excellent heat resistance can also be exhibited. 300 ) is preferably 1.0×10 -6 T or more, preferably 5.0×10 -6 T or more, more preferably 2.0×10 -5 T or greater.

[0029] The surface-treated copper foil of the present invention has a residual magnetic flux density (Br 300 ), but preferably 6.0 × 10 -4 T or less, preferably 5.0×10 -4 T or less, more preferably 4.0×10 -4T or less. By keeping it within the above range, it is possible to effectively reduce the magnetism caused by the heat treatment, and to further reduce the transmission loss. In particular, it is considered that the higher the residual magnetic flux density, the greater the loss due to the generation of eddy currents and the magnetic hysteresis loss, and the greater the transmission loss of high frequency signals. Therefore, it is considered that the transmission loss can be further reduced significantly by reducing the above-mentioned predetermined residual magnetic flux density. Note that the residual magnetic flux density (Br 300 ) is preferably 1.0×10 -7 T or more, preferably 5.0×10 -7 T or more, more preferably 3.0×10 -6 T or greater.

[0030] The surface-treated copper foil of the present invention preferably satisfies the following requirements (I) and (II). Requirement (I): The rate of increase in saturation magnetic flux density Bs after heat treatment at 300°C for 2 hours [{(Bs 300 −Bs0) / Bs0}×100] is preferably 310% or less, more preferably 300% or less, even more preferably 200% or less, and still more preferably 100% or less. Requirement (II): The increase rate of residual magnetic flux density Br after heat treatment at 300°C for 2 hours [{(Br 300 -Br0) / Br0}×100] is preferably 310% or less, more preferably 300% or less, even more preferably 200% or less, and still more preferably 100% or less. In the above requirements (I) and (II), Bs 300 is the saturation magnetic flux density after heat treatment at 300°C for 2 hours, Bs0 is the saturation magnetic flux density before the heat treatment, Br 300 is the residual magnetic flux density after heat treatment at 300° C. for 2 hours, and Br0 is the residual magnetic flux density before the heat treatment. By satisfying the above requirements, the surface-treated copper foil of the present invention can keep the increase in each magnetic flux density after heat treatment within a predetermined range, thereby further reducing the transmission loss. In particular, in a surface-treated copper foil with a large increase rate of magnetic flux density after heat treatment, the waveform of the high-frequency signal when measuring the transmission loss tends to become unstable. It is presumed that the cause of this phenomenon is that when the thermal load is distributed in the plane during the manufacturing process of the printed wiring board, a change in the distribution of magnetization in the plane of the printed wiring board occurs. Therefore, it is considered that the quality of the high-frequency signal can be improved by controlling the increase rate of magnetic flux density after heat treatment within a certain range.

[0031] The saturation magnetic flux density Bs and the residual magnetic flux density Br before and after the above-mentioned predetermined heat treatment can be measured by the following method. First, the surface-treated copper foil after a predetermined heat treatment is obtained by heating the surface-treated copper foil at 300° C. for 2 hours. The surface-treated copper foil before and after the heat treatment is cut into a size of 10 mm x 10 mm to be used as a measurement subject, and the saturation magnetic flux density Bs and the residual magnetic flux density Br are measured using a vibrating sample magnetometer (VSM) under the following conditions. Applied magnetic field range: ±10000[Oe] Sweep speed: 50[Oe / s] More specifically, the magnetic properties can be measured by the method described in the Examples.

[0032] <Surface roughness of surface-treated copper foil> In the surface-treated copper foil of the present invention, when the surface treatment film includes, in order from the copper foil substrate side, a roughening treatment layer and the nickel layer, the arithmetic mean height Sa of the surface of the surface treatment film measured optically in accordance with ISO25178 is preferably 0.02 μm or more and 0.50 μm or less, more preferably 0.02 μm or more and 0.35 μm or less, even more preferably 0.02 μm or more and 0.30 μm or less, and even more preferably 0.02 μm or more and 0.20 μm or less. By adopting the above-mentioned configuration, excellent heat resistance can be exhibited while reducing transmission loss. In particular, in the surface-treated copper foil, the surface treatment film includes a roughening treatment layer below the nickel layer (copper foil substrate side), thereby improving adhesion to the resin substrate. At that time, by having the uneven shape on the surface of the surface treatment film within the above-mentioned predetermined range, adhesion to the resin substrate can be improved without adversely affecting transmission loss. The arithmetic mean height Sa can be measured by the method described in the Examples.

[0033] <Method of manufacturing surface-treated copper foil> Next, an example of a preferred method for producing the surface-treated copper foil of the present invention will be described. A preferred method for producing the surface-treated copper foil of the present invention includes a step of forming a surface treatment film containing a nickel layer on at least one surface of a copper foil substrate, and more specifically, includes a step of forming a nickel layer directly or indirectly on at least one surface of the copper foil substrate.

[0034] (Copper foil base) As the copper foil substrate, it is preferable to use electrolytic copper foil or rolled copper foil, which has a smooth and glossy surface without large irregularities. Among them, electrolytic copper foil is preferable from the viewpoint of productivity and cost, and it is particularly preferable to use the non-drum side of electrolytic copper foil as the side on which the surface treatment film is formed. In addition, it is preferable that the surface of the drum-shaped cathode used in the production of electrolytic copper foil is polished with a buff of #1000 to #2500.

[0035] The copper foil substrate has a ten-point average roughness Rzjis of preferably 2 μm or less, more preferably 1 μm or less, and even more preferably 0.8 μm or less, at least on the surface on which the surface treatment film is formed. By keeping the roughness within the above range, the adhesion to the resin substrate can be improved, and the transmission loss is not deteriorated. The copper foil substrate preferably has a ten-point average roughness Rzjis of 2 μm or less, more preferably 1 μm or less, and further preferably 0.8 μm or less on both sides. The lower limit of the ten-point average roughness Rzjis on each surface of the copper foil substrate is, for example, 0.1 μm or more from the viewpoint of ease of production or availability. The ten-point average roughness Rzjis can be measured using a contact surface roughness measuring device in accordance with the method specified in JIS B0601: 2001. Specifically, it can be measured by the method described in the examples.

[0036] The thickness of the copper foil substrate is, for example, 5 to 210 μm, preferably 5 to 100 μm, and more preferably 5 to 40 μm.

[0037] (nickel treatment) The surface-treated copper foil of the present invention is subjected to a nickel treatment to form a nickel layer on at least one surface of a copper foil substrate directly or indirectly. An object of the present invention is to provide a surface-treated copper foil capable of suppressing magnetization of the nickel layer even after a specified heat treatment. In response to this, the present inventors conducted extensive research and came to the conclusion that the increase in magnetic flux density in surface-treated copper foil after a specified heat treatment is due to the progress of crystallization of the nickel layer and / or an increase in crystal grain size caused by the heat treatment. Focusing on this phenomenon, the inventors investigated nickel treatments that can suppress this. The following nickel treatment (A) and nickel treatment (B) will be described in detail below as suitable examples of nickel treatments investigated by the present inventors.

[0038] Nickel treatment (A) The nickel treatment (A) is an example of a nickel treatment that can suppress an increase in the crystal grain size in the nickel layer after a predetermined heat treatment, and is performed by pulse electrolysis with flow rate control.

[0039] In general, pulse electrolysis allows for instantaneous application of a higher current density than normal DC electrolysis, making it possible to form a plating film with a dense microcrystalline structure. On the other hand, because reactive species near the electrode are lost due to the instantaneous application of high electric density, pulse electrolysis requires alternating periods of current application and rest, and in order to obtain a dense crystal structure, the duty ratio (current application time / [current application time + current rest time]) must be reduced. However, if the duty ratio is reduced, the time during which no current is applied will occupy a large portion of the process, raising concerns about a decline in productivity. In addition, because discontinuous multi-step plating is used, impurities are more likely to be incorporated into the nickel layer, raising concerns about a decline in heat resistance, which poses challenges in terms of manufacturing.

[0040] Therefore, the inventors of the present invention conducted extensive research and found that the above problem could be solved by controlling the liquid flow rate in the tank to increase the stirring speed in the liquid and supply sufficient reactive species to the vicinity of the electrodes, which serve as the reaction field. In other words, by performing pulse electrolysis in a reaction field where the liquid flow rate is controlled, reactive species can be immediately supplied to the vicinity of the electrodes immediately after current application, making it possible to efficiently deposit nickel under conditions with a higher duty ratio than in the past. This makes it possible to reduce the amount of impurities taken in between the nickel layers and to electrolytically plate a nickel layer with a fine crystal grain size.

[0041] In such pulse electrolysis, the duty ratio is preferably 0.1 to 0.9, more preferably 0.1 to 0.8, and the liquid flow rate is preferably 15 to 110 L / min, more preferably 20 to 100 L / min. By setting the duty ratio and the liquid flow rate within the above ranges, it is possible to efficiently attach microcrystallized nickel, and the resulting nickel layer is microcrystallized. Therefore, even after a predetermined heat treatment, it is considered that the crystal grain size does not increase completely, and the nickel layer can be suppressed from being magnetized. On the other hand, if the duty ratio is too small, the productivity tends to deteriorate, and if the duty ratio is too large, reactive species are not sufficiently supplied to the electrode surface, and poor plating appearance on the electrode surface tends to occur. In addition, if the flow rate is too small, reactive species are not sufficiently supplied to the electrode surface, and if the flow rate is too large, poor plating appearance on the electrode surface tends to occur due to reasons such as the inclusion of air bubbles in the liquid.

[0042] An example of the plating bath composition and electrolysis conditions suitable for nickel treatment (A) is shown below. Note that the following conditions are preferred examples, and the types and amounts of additives, electrolysis conditions, etc. can be appropriately changed and adjusted as necessary within the scope that does not impair the effects of the present invention. <Plating bath composition> Nickel sulfate hexahydrate: 10-80g / L in terms of nickel (atom) Boric acid: 5~40g / L pH: 3.0~5.0 <Conditions for pulse electrolysis> Bath temperature: 10~60℃ Current density: 1~15A / dm 2 Current application time: 5 to 100 milliseconds Duty ratio:0.1~0.9 Total charge: 0.5~30A·S / dm 2 Liquid flow rate: 15~110L / min

[0043] Nickel treatment (B) The nickel treatment (B) is an example of a nickel treatment that can suppress the increase in crystal grain size in the nickel layer after a specific heat treatment, and is carried out by an electrochemical reduction reaction of nickel hydroxide. Specifically, it is as follows.

[0044] First, a nickel layer is formed on the surface of a copper foil substrate. Nickel hydroxide is then attached to the surface of the copper foil substrate by a method such as alkaline immersion, oxidation at an anode, or nickel plating in an alkaline pH state (hereinafter sometimes referred to as "hydroxide treatment"). The nickel hydroxide is then reduced to nickel by an electrochemical reduction reaction (hereinafter sometimes referred to as "reduction treatment") to re-form the nickel layer. At this time, by performing the reduction treatment under appropriate conditions, it is believed that a state like a mixture of nickel hydroxide and metallic nickel can be formed in the nickel layer, the crystallinity becomes random, and the nickel layer can be made amorphous. Furthermore, it is believed that the presence of some of the oxygen atoms incorporated in the hydroxide at the grain boundaries also has the effect of suppressing the increase in crystal grain size during heating.

[0045] In such an electrochemical reduction reaction of nickel hydroxide, the current density is preferably 0.1 to 2.7 A / dm 2 , more preferably 0.2 to 2.5 A / dm 2 It is believed that the above-mentioned effects can be obtained by keeping the current density within the above range. On the other hand, if the current density is too small, the reduction of nickel hydroxide tends to be insufficient, and if the current density is too large, the crystal grain size tends to increase, and magnetism tends to be exhibited.

[0046] Below, examples of electrolytic plating conditions, hydroxide treatment conditions, and reduction treatment conditions suitable for nickel treatment (B) are shown. Note that the following conditions are preferred examples, and the type and amount of additives, electrolytic conditions, etc. can be appropriately changed and adjusted as necessary within the range that does not impair the effects of the present invention. (1) First, it is preferable to carry out electroplating under the following conditions: <Composition of plating solution> Nickel sulfate hexahydrate: 20-60g / L in terms of nickel (atom) Boric acid: 5~40g / L pH: 3.0~5.0 <Electrolysis conditions> Bath temperature: 20~60℃ Current density: 0.1~2.7A / dm 2 Current application time: 1.5 to 30 seconds

[0047] (2) Next, it is preferable to sequentially carry out a hydroxide treatment and a reduction treatment on the surface of the nickel layer obtained in the above (1) under the following conditions. <Conditions for Hydroxide Treatment> Sodium hydroxide solution: Sodium hydroxide concentration 5-50g / L Immersion time: 10 to 60 seconds <Conditions for reduction treatment> Current density: 0.1~2.7A / dm 2 Current application time: 10 to 60 seconds

[0048] In addition, by alloying the nickel layer with a different metal such as Zn, P, Mo, W, Cr, Fe, Co, or Nb, it is possible to further suppress the increase in magnetization and improve heat resistance. The reaction mechanism for suppressing the magnetism of nickel as described above has a similar effect in plating baths containing different metals. For example, in nickel treatment (A), a finely crystallized nickel layer can be formed by adding elements such as a Zn source or a P source to the nickel plating bath used in pulse electrolysis.

[0049] In this embodiment, it is considered that the cause of the increase in magnetic flux density in the surface-treated copper foil after the specified heat treatment is the progress of crystallization of the nickel layer and / or an increase in the crystal grain size due to the heat treatment, and the above nickel treatments (A) and (B) are preferably exemplified as a means for improving this. However, the increase in magnetic flux density in the surface-treated copper foil after the specified heat treatment may be suppressed by a means other than the above.

[0050] (Roughening treatment) The surface-treated copper foil of the present invention may be provided with a roughening treatment on the surface of the copper foil substrate before the nickel treatment, to form a roughening layer on the surface of the copper foil substrate. In this case, examples of the roughening treatment include forming the roughening layer by electrodeposition of copper particles, and forming the roughening layer by etching using hydrogen peroxide or the like.

[0051] In addition, when forming a roughened layer, it is desirable to control the treatment conditions so that the arithmetic mean height Sa of the surface of the surface treatment film including the roughened layer and the nickel layer, measured optically in accordance with ISO 25178, is preferably 0.02 μm or more and 0.50 μm or less, more preferably 0.02 μm or more and 0.35 μm or less, even more preferably 0.02 μm or more and 0.30 μm or less, and even more preferably 0.02 μm or more and 0.20 μm or less. By controlling the surface state of the obtained surface-treated copper foil as described above, it is possible to further improve the adhesion to the surface of the resin substrate while reducing the transmission loss. The method of controlling the treatment conditions may be, for example, a method of adjusting the current flow time or current flow amount in the case of forming roughening particles by copper electrodeposition, or a method of adjusting the treatment time in the case of forming roughening particles by etching.

[0052] As the roughening treatment, it is preferable to subject the copper foil substrate surface before nickel treatment to the roughening plating treatment (1) described below. If necessary, it may be combined with the fixed plating treatment (2). · Roughening plating process (1) <Plating bath composition> Copper sulfate pentahydrate: 3~20g / L in terms of copper (atoms) Sulfuric acid: 100~250g / L Ammonium molybdate: 400-1200mg / L in molybdenum (atom) equivalent <Conditions for electroplating treatment> Bath temperature: 5~20℃ Current density: 5~55A / dm 2 Current application time: 0.5 to 15 seconds Fixed plating process (2) <Plating bath composition> Copper sulfate pentahydrate: 40~70g / L in terms of copper (atoms) Sulfuric acid: 100~250g / L <Conditions for electroplating treatment> Bath temperature: 15~30℃ Current density: 2~10A / dm 2 Current application time: 0.5 to 5 seconds

[0053] (Other processing) In addition, the surface-treated copper foil of the present invention may further have a chemical adhesion layer such as a silane coupling agent layer formed on the nickel layer directly or via an intermediate layer such as a heat-resistant layer containing zinc (Zn) and an anti-rust layer containing chromium (Cr). Note that the intermediate layer and the chemical adhesion layer are very thin, so they do not affect the roughness of the surface treatment surface and have little effect on the magnetism.

[0054] The heat-resistant layer is preferably formed when it is necessary to further improve the heat resistance of the surface treatment film. The heat-resistant layer is preferably formed of, for example, zinc or an alloy containing zinc. Examples of alloys containing zinc include zinc-tin (Sn) alloy, zinc-cobalt (Co) alloy, zinc-copper (Cu) alloy, zinc-molybdenum (Mo) alloy, zinc-chromium (Cr) alloy, and zinc-vanadium (V) alloy.

[0055] The rust-proofing layer is preferably formed when it is necessary to further improve the corrosion resistance of the surface treatment film. Examples of the rust-proofing layer include a chrome layer formed by chrome plating and a chromate layer formed by chromate treatment.

[0056] When both the heat-resistant layer and the rust-proofing layer are formed, it is preferable to form them on the surface treatment layer in this order. That is, when all of them are provided, the order is copper foil substrate-roughening layer-nickel layer-heat-resistant layer-rust-proofing layer. Also, only one or two of the heat-resistant layer and the rust-proofing layer may be formed depending on the application and the desired characteristics.

[0057] The chemical adhesion layer can be formed, for example, by applying a silane coupling agent solution directly or via an intermediate layer onto the surface of the nickel layer of the surface-treated copper foil, followed by air drying (natural drying) or heat drying. When the water in the applied coupling agent solution evaporates, a silane coupling agent layer is formed. In particular, from the viewpoint of further promoting the dehydration reaction of the silane coupling agent, it is preferable to perform the drying by heating at 100 to 220°C.

[0058] In addition, the silane coupling agent layer preferably contains one or more selected from the group consisting of epoxy-based silane coupling agents, amino-based silane coupling agents, vinyl-based silane coupling agents, methacryl-based silane coupling agents, acrylic-based silane coupling agents, azole-based silane coupling agents, styryl-based silane coupling agents, ureido-based silane coupling agents, mercapto-based silane coupling agents, sulfide-based silane coupling agents, and isocyanate-based silane coupling agents.

[0059] [Application] The surface-treated copper foil of the present invention is suitably used for the manufacture of a copper-clad laminate, and further for the manufacture of a printed wiring board. That is, the copper-clad laminate of the present invention comprises the surface-treated copper foil of the present invention, and preferably further comprises a resin substrate laminated on the surface treatment layer of the surface-treated copper foil. Also, the printed wiring board of the present invention comprises the copper-clad laminate of the present invention. When such a surface-treated copper foil is used to manufacture a copper-clad laminate or a printed wiring board, the nickel layer can be prevented from being magnetized even after a specified heat treatment. Therefore, the resulting copper-clad laminate or printed wiring board can reduce transmission loss and also exhibit good heat resistance due to the nickel layer.

[0060] Incidentally, in next-generation wireless transmission applications, the fact that the circuit board has magnetism can itself become a major problem. For example, remote medical care is one of the technologies expected to be used with the next generation 5G and 6G. However, when considering the use of printed wiring boards in magnetic testing equipment such as MRI, there is a possibility that problems may arise, such as inaccurate test results being obtained, due to the printed wiring board itself being magnetized. Other examples of technology include wearable devices such as smart watches. However, as these devices become more sophisticated, it is possible that they may also experience problems such as not functioning properly due to magnetic failure. As the frequency of high-frequency signals increases in the future, it is expected that the effect of magnetic metals on magnetic fields will become greater. Therefore, in addition to reducing transmission loss, there is a demand for using non-magnetic surface-treated copper foil as a circuit conductor for printed wiring boards. From this viewpoint as well, the surface-treated copper foil of the present invention is extremely useful.

[0061] That is, the printed wiring board having the surface-treated copper foil of the present invention is suitable as a printed wiring board for use in a high frequency band (particularly a high frequency band of 1 to 100 GHz) and as a printed wiring board where the influence of a magnetic field is a concern.

[0062] The copper-clad laminate comprising the surface-treated copper foil of the present invention can be formed by a known method. Specifically, the copper-clad laminate is generally produced by laminating and adhering the surface-treated copper foil and the resin substrate (insulating substrate) so that the roughened surface (adhering surface) of the surface-treated copper foil faces the resin substrate. In particular, when producing a copper-clad laminate using the surface-treated copper foil of the present invention, it is preferable to use the surface having a predetermined surface treatment film as the adhering surface to the resin substrate. This can reduce transmission loss and also exhibit good heat resistance due to the nickel layer.

[0063] Examples of resin substrates include flexible resin substrates and rigid resin substrates, and the surface-treated copper foil of the present invention is particularly suitable for use in combination with rigid resin substrates, which require high transmission characteristics and adhesion in the high frequency band. Examples of resins that form the resin substrate include epoxy resins, polyphenylene ethers, phenolic resins, bis(phenoxyphenoxy)benzene, polyimides, liquid crystal polymers, and fluororesins (eg, polytetrafluoroethylene).

[0064] In addition, when manufacturing a copper-clad laminate for printed wiring boards, it is sufficient to manufacture by bonding a surface-treated copper foil having a silane coupling agent layer and a resin substrate by hot pressing. Note that the copper-clad laminate for printed wiring boards manufactured by applying a silane coupling agent onto a resin substrate, bonding the resin substrate coated with the silane coupling agent and a surface-treated copper foil having a rust-proofing layer on the outermost surface by hot pressing also has the same effect as when using the surface-treated copper foil having the above-mentioned silane coupling agent layer.

[0065] The printed wiring board including the surface-treated copper foil of the present invention can be formed by a known method. Specifically, it may be formed using the above-mentioned copper-clad laminate for printed wiring board. Such a printed wiring board preferably includes the above-mentioned copper-clad laminate for printed wiring board.

[0066] The printed wiring board according to the present embodiment can be obtained by, for example, forming a circuit by etching the surface-treated copper foil of a copper-clad laminate, and then laminating another resin base material so as to cover the circuit. The resin base material to be laminated so as to cover the circuit may be the same type as the resin base material of the copper-clad laminate, or may be a different type.

[0067] The surface-treated copper foil of the present invention can also be suitably used as a negative electrode current collector for lithium ion secondary batteries and the like. The negative electrode current collector including the surface-treated copper foil of the present invention can be formed by a known method. Specifically, the negative electrode current collector is formed by coating the surface of the copper foil with carbon particles or the like as a negative electrode active material layer, drying the coated surface, and pressing the coated surface.

[0068] Although the embodiment of the present invention has been described above, the above embodiment is merely an example of the present invention. The present invention includes all aspects included in the concept of the present invention and the scope of the claims, and can be modified in various ways within the scope of the present invention. EXAMPLES

[0069] The present invention will be described in more detail below with reference to examples, which are merely examples of the present invention.

[0070] (Manufacturing Example 1: Preparation of copper foil substrate) A roll of electrolytic copper foil (double-sided glossy foil) having a ten-point average roughness Rzjis of 0.8 μm on the M side and a thickness of 18 μm was produced using the following cathode and anode as a copper foil substrate serving as a base material for forming a surface treatment film, and a copper sulfate electrolyte of the following composition under the following electrolysis conditions. The ten-point average roughness Rzjis on the M side is a value measured under the following measurement conditions.

[0071] <Cathode and anode> Cathode: Titanium rotating drum with surface roughness adjusted by buffing with #1000~#2000 Anode: Dimensionally Stable Anode DSA® <Electrolyte composition> Copper sulfate pentahydrate: 75g / L in terms of copper (atoms) Sulfuric acid: 65g / L Chlorine concentration: 20mg / L (Additives) Sodium 3-mercapto-1-propanesulfonate: 2mg / L Hydroxyethylcellulose: 10mg / L ·Low molecular weight glue (molecular weight 3000): 50mg / L <Electrolysis conditions> Liquid temperature: 55℃ Current density: 45A / dm 2

[0072] <Ten-point average roughness Rzjis> On the M side of the electrodeposited copper foil, a contact surface roughness tester (manufactured by Kosaka Laboratory, Ltd., "Surfcorder SE1700") was used to measure the ten-point average roughness Rzjis (μm) defined in JIS B 0601:2001 in the direction perpendicular to the longitudinal direction (transport direction, MD) of the electrodeposited copper foil (TD direction), i.e., the ten-point average roughness Rzjis (μm) of the TD.

[0073] (Examples 1 to 10 and 48 to 51 and Comparative Examples 4 and 5) In Examples 1 to 10 and 48 to 51 and Comparative Examples 4 and 5, the electrolytic copper foil produced in Production Example 1 was used as the copper foil substrate, and the copper foil substrate was subjected to the following steps [1] to [3] to obtain surface-treated copper foils. The details are explained below.

[0074] [1] Nickel layer formation A nickel layer was formed on the M side of the electrolytic copper foil by electroplating (nickel treatment (A)) using a pulse electrolysis device. At this time, a bath capable of circulating the plating solution was used, and plating was performed while controlling the flow rate. The plating bath composition and pulse electrolysis conditions were as follows: <Plating bath composition> Nickel sulfate hexahydrate: 50g / L in terms of nickel (atom) Boric acid: 20g / L pH: 4.3 <Conditions for pulse electrolysis> Bath temperature: 20℃ Current density: 10A / dm 2 Current application time: 10 ms Duty ratio: Shown in Tables 1 and 2. Total charge: 4A·S / dm 2 Liquid flow rate: shown in Tables 1 and 2.

[0075] [2] Formation of the intermediate layer Next, the surface of the nickel layer formed in [1] above was subjected to zinc plating and chrome plating in the following order under the following conditions to form an intermediate layer. The compositions of the plating baths and the electrolysis conditions for the zinc plating and chrome plating were as follows:

[0076] Zinc plating treatment <Plating bath composition> Zinc sulfate heptahydrate: 2.5g / L in terms of zinc (atom) Sodium hydroxide): 25g / L pH: 10~12 <Electrolysis conditions> Bath temperature: 20℃ Current density: 0.7A / dm 2 Processing time: 4 seconds

[0077] Chrome plating <Plating bath composition> Chromium(VI) oxide: 8g / L in terms of chromium (atom) pH: 2.4 <Electrolysis conditions> Bath temperature: 30℃ Current density: 5A / dm 2 Processing time: 4 seconds

[0078] [3] Formation of chemical adhesion layer Finally, a 0.8% by mass aqueous solution of 3-aminopropyltrimethoxysilane was applied onto the intermediate layer (particularly the outermost chrome plating layer) formed in [2] above, and dried at 200°C to form a chemical adhesion layer using a silane coupling agent.

[0079] (Examples 11 to 17 and Comparative Example 6) In Examples 11 to 17 and Comparative Example 6, surface-treated copper foils were obtained in the same manner as in Example 1, except that in the above [1], instead of the nickel treatment (A), an electrochemical reduction reaction of nickel hydroxide (nickel treatment (B)) was carried out under the conditions shown below. Specifically, the following steps were taken.

[0080] (1) First, a nickel layer was formed on the M side of the above-mentioned electrolytic copper foil by electrolytic plating as follows. The composition of the plating bath and the electrolytic conditions were as follows. <Plating bath composition> Nickel sulfate hexahydrate: 40g / L in terms of nickel (atom) Boric acid: 20g / L pH: 4.2 <Electrolysis conditions> Bath temperature: 30℃ Current density: 0.5A / dm 2 Power-on time: 5 seconds

[0081] (2) Next, the surface of the nickel layer obtained in (1) above was immersed in an aqueous sodium hydroxide solution (sodium hydroxide concentration: 30 g / L) for 30 seconds to carry out a hydroxide treatment of the nickel layer. Thereafter, an electrochemical reduction reaction of nickel hydroxide was carried out in an aqueous sodium hydroxide solution under the following conditions to obtain a nickel layer. <Conditions for reduction treatment> Current density: shown in Tables 1 and 2. Current application time: 30 seconds

[0082] (Examples 18 to 35) In Examples 18 to 35, surface-treated copper foils were obtained in the same manner as in Example 3, except that each component was added to the plating bath in [1] above at the following concentrations so that the composition of the Ni-containing surface treatment layer would be the alloy composition shown in Table 1. In the case of Ni-P Sodium hypophosphite monohydrate: 15g / L in phosphorus (atom) equivalent In the case of Ni-Zn Zinc sulfate heptahydrate: 5g / L in terms of zinc (atom) For Ni-Mo Sodium molybdate dihydrate: 5g / L in molybdenum (atom) equivalent For Ni-W Sodium tungstate dihydrate: 5g / L in terms of tungsten (atom) In the case of Ni-Cr Chromium(VI) oxide: 4g / L in terms of chromium (atom) In the case of Ni-Co Cobalt chloride hexahydrate: 4g / L in terms of cobalt (atom) In the case of Ni-Zn-P Zinc sulfate heptahydrate: 5g / L in terms of zinc (atom) Sodium hypophosphite monohydrate: 15g / L in phosphorus (atom) equivalent In the case of Ni-Zn-Mo Zinc sulfate heptahydrate: 5g / L in terms of zinc (atom) Sodium molybdate dihydrate: 5g / L in molybdenum (atom) equivalent In the case of Ni-Zn-Cr Zinc sulfate heptahydrate: 5g / L in terms of zinc (atom) Chromium(VI) oxide: 4g / L in terms of chromium (atom)

[0083] (Examples 36 to 40) In Examples 36 to 40, surface-treated copper foils were obtained in the same manner as in Example 3, except that a roughened layer was first formed on a copper foil substrate under the following conditions, and then a surface treatment layer containing Ni was formed on the roughened layer.

[0084] [Formation of roughened layer] Before the nickel treatment in [1] above, a roughening treatment layer was formed on the M side of the electrolytic copper foil by roughening plating treatment. At this time, by changing the current application time, roughening particles of different shapes were formed on the surface of the copper foil substrate. The plating bath composition and plating conditions were as follows. <Plating bath composition> Copper sulfate pentahydrate: 10g / L in terms of copper (atoms) Sulfuric acid: 150g / L Ammonium molybdate: 600 mg / L in molybdenum (atom) equivalent <Conditions for electroplating treatment> Bath temperature: 12℃ Current density: 20A / dm 2 Current application time: 2 to 8 seconds

[0085] (Examples 41 to 47) In Examples 41 to 47, the total charge of Ni plating was set to 1 to 20 A·S / dm so as to obtain the Ni coating weight shown in Table 2. 2 A surface-treated copper foil was obtained in the same manner as in Example 3, except that the range was changed as follows.

[0086] (Comparative Examples 1 to 3) In Comparative Examples 1 to 3, surface-treated copper foils were obtained in the same manner as in Example 1, except that in the above [1], nickel treatment (A) was replaced by nickel treatment under the following conditions as a general nickel plating method. The plating bath composition and electrolysis conditions were as follows. <Plating bath composition> Nickel sulfate hexahydrate: 45g / L in terms of nickel (atom) Boric acid: 20g / L pH: 3.5 <Electrolysis conditions> Bath temperature: 20℃ Current density: 0.5A / dm 2 Power-on time: 9 seconds

[0087] Comparative Example 7 In Comparative Example 7, a surface-treated copper foil was obtained in the same manner as in Example 1, except that Ni plating was not performed.

[0088] Comparative Example 8 In Comparative Example 8, a surface-treated copper foil was obtained in the same manner as in Example 1, except that a surface treatment layer containing Ni was formed under the same Ni-Co treatment conditions as in Example 4 of Patent Document 1.

[0089] Comparative Example 9 In Comparative Example 9, a surface-treated copper foil was obtained in the same manner as in Example 1 of Patent Document 2.

[0090] (evaluation) The surface-treated copper foils according to the above examples and comparative examples were used to carry out the following characteristic evaluations. The evaluation conditions for each characteristic were as follows, and unless otherwise specified, each measurement was carried out at room temperature (20°C ± 5°C). The results are shown in Tables 1 and 2.

[0091] [Composition of surface treatment layer containing Ni] The composition of the nickel layer of the surface-treated copper foil was analyzed by X-ray photoelectron spectroscopy (XPS) using an X-ray photoelectron spectrometer (ULVAC-PHI, Inc., "PHI Quants"). The incident X-ray was a monochromated Al-Kα ray (hν=1486.6 eV) with an escape angle of 45°. The surface of the surface treatment film including the nickel layer of the surface-treated copper foil was measured in an analysis area of ​​100 μmφ, and a depth direction analysis was performed by Ar sputtering. When one or more elements selected from the group consisting of Zn, P, Mo, W, Cr, and Co were detected in the same depth region as the depth region where nickel was detected, it was determined that nickel was alloyed, and the alloy composition was estimated to be an alloy of nickel and the detected elements.

[0092] [Ni adhesion amount] The surface of the surface-treated copper foil having a surface treatment film containing a nickel layer was analyzed by fluorescent X-ray analysis using a scanning fluorescent X-ray analyzer (Rigaku Corporation, ZSX Primus IV) to determine the Ni adhesion amount (mg / dm 2 The amount of Ni attached was quantified using a calibration curve obtained using a known standard sample.

[0093] [Magnetic properties] The magnetic properties of the surface-treated copper foil were measured by the following method before and after the following prescribed heat treatment. (Heat treatment) The surface-treated copper foil was cut into a size of 40 mm x 80 mm, and the cut foil was heat-treated in an oven at 300°C for 2 hours in an inert atmosphere to prepare a heat-treated surface-treated copper foil.

[0094] (Measurement of magnetic properties) The magnetic properties of the surface-treated copper foil before and after the heat treatment were measured by the following method. (1) First, the surface-treated copper foil to be measured was cut into ten measurement samples measuring 10 mm x 10 mm. (2) The magnetic properties of the measurement samples obtained in (1) above were measured under the following conditions. The measurements were performed using a vibrating sample magnetometer (manufactured by Tamagawa Seisakusho Co., Ltd., "TM-VSM211483-HGC type"). First, the measurement sample was set in a sample holder, and while vibrating the measurement sample, a magnetic field was applied up to +10,000 Oe at a sweep speed of 50 Oe / s, then the magnetic field was swept down to -10,000 Oe at a sweep speed of 50 Oe / s, and then up to +10,000 Oe at a sweep speed of 50 Oe / s, thereby obtaining a BH curve with the vertical axis being magnetic flux density and the horizontal axis being magnetic field. (3) Based on the BH curve obtained in (2) above, the magnetic flux density when the magnetic field was +10,000 Oe and the magnetic flux density when the magnetic field was 0 Oe were read, and these were determined as the saturation magnetic flux density Bs [T] and the residual magnetic flux density Br [T]. In this method, two values ​​of magnetic flux density are obtained for the magnetic field. Normally, if the magnetic property measurement is performed normally, the BH curve is a vertically symmetrical graph, so the absolute values ​​of the two values ​​calculated for the magnetic field are almost the same. In this example, it was confirmed that the BH curve was vertically symmetrical, and the value calculated first was used. (4) The above measurement was performed once for each measurement sample, and the measured values ​​of the 10 measurement samples were averaged to obtain the magnetic flux density of each of the surface-treated copper foils to be measured. The saturation magnetic flux density Bs and residual magnetic flux density Br of the surface-treated copper foil before the heat treatment are "Bs0" and "Br0", and the saturation magnetic flux density Bs and residual magnetic flux density Br of the surface-treated copper foil after the heat treatment are "Bs 300 " and "Br 300 " will be displayed respectively. In addition, "A×10^-B" in the table means "A×10 -B " means " (5) Furthermore, the saturation magnetic flux density Bs0 and residual magnetic flux density Br0 of the surface-treated copper foil before the heat treatment, and the saturation magnetic flux density Bs 300 and residual magnetic flux density Br 300Based on the values, the increase rate of the saturation magnetic flux density Bs and the increase rate of the residual magnetic flux density Br after the heat treatment were calculated by the following formulas (I) and (II), respectively. Increase rate of saturation magnetic flux density Bs after heat treatment (%) = [{(Bs 300 -Bs0) / Bs0}×100] (I) Increase rate of residual magnetic flux density Br after heat treatment (%) = [{(Br 300 -Br0) / Br0}×100] (II)

[0095] [Surface roughness (arithmetic mean height Sa)] The arithmetic mean height Sa was measured on the surface of the surface-treated copper foil having a surface treatment film including a nickel layer using a confocal laser microscope (manufactured by Keyence Corporation, "VK-X1050" and "VK-X1000") in accordance with ISO25178. The objective lens magnification of the confocal laser microscope is 100x, the scan mode is laser confocal, the measurement size is 2048 × 1536, the measurement quality is High Precision, and the pitch is 0.08 μm. Moreover, calculations of Vvc and Sa were performed under the following filter processing and calculation conditions. <Filter processing and calculation conditions> Image processing: averaging, 3x3, median S filter: None F-operation: Plane tilt correction L filter: 0.025μm Calculation area: 100μm×100μm

[0096] [Transmission characteristics] To evaluate the high frequency characteristics, the transmission loss in the high frequency band was measured, as described in detail below. A copper-clad laminate was produced by laminating surface-treated copper foil on both sides of two overlapping low-dielectric polyphenylene ether resin films (MEGTRON7, a multilayer board material manufactured by Panasonic Corporation, 60 μm thick). At this time, the surface of the resin film and the surface of the surface-treated film containing the nickel layer of the surface-treated copper foil were arranged to face each other, and the two were laminated by pressing under conditions of a surface pressure of 3.5 MPa and 210°C for 2 hours to produce a double-sided copper-clad laminate. The obtained copper-clad laminate was subjected to circuit processing to produce a printed wiring board in which a strip line with a transmission path width of 140 μm and a circuit length of 1000 mm was formed. A high-frequency signal was transmitted to the transmission path of this printed wiring board using a network analyzer (Keysight Technologies, "N5291A"), and the transmission loss was measured. The characteristic impedance was set to 50 Ω. The above measurement was performed three times for one copper-clad laminate, and the average value was taken as the measured value. The smaller the absolute value of the measured transmission loss, the smaller the transmission loss and the better the high-frequency characteristics. Using the obtained measured value as an index, the high-frequency characteristics were evaluated according to the following evaluation criteria. S: Absolute value of transmission loss at 40GHz is less than 41.5dB A: The absolute value of the transmission loss at 40 GHz is 41.5 dB or more and less than 43.0 dB. B: The absolute value of the transmission loss at 40 GHz is 43.0 dB or more and less than 45.0 dB. C: Absolute value of transmission loss at 40GHz is 45.0dB or more

[0097] [Heat resistance] A double-sided copper-clad laminate was produced in the same manner as described in the above [Evaluation of high-frequency characteristics]. The resulting double-sided copper-clad laminate was cut into pieces measuring 5 cm x 5 cm to prepare 10 test pieces. The resulting 10 test pieces were subjected to a heat treatment in an oven at 290° C. in an air atmosphere for 1 hour. After that, the test pieces after the heat treatment were taken out, and each test piece was visually judged whether or not peeling occurred between the copper foil and the resin. Based on the judgment results of the 10 test pieces, the heat-resistant adhesion was evaluated according to the following evaluation criteria. <Evaluation criteria for heat-resistant adhesion> A: 0 or 1 test piece has peeled off B: Two or three test pieces have peeled off. C: Four or more test pieces have peeled off.

[0098] [Table 1]

[0099] [Table 2]

[0100] As shown in Tables 1 and 2, the saturation magnetic flux density (Bs 300 ) is 5.0 × 10 -3 It was confirmed that the surface-treated copper foil having a hardness of 0.1M or less can suppress the nickel layer from being magnetized even after heat treatment, and therefore has excellent transmission characteristics and heat resistance (Examples 1 to 51).

[0101] In contrast, the saturation magnetic flux density (Bs 300 ) is 5.0 × 10 -3 It was confirmed that the surface-treated copper foils having a resistance exceeding T (Comparative Examples 1 to 6, 8 and 9) had inferior transmission characteristics compared to the surface-treated copper foils of Examples 1 to 51 because the nickel layer was magnetized after the heat treatment. Furthermore, it was confirmed that the surface-treated copper foil (Comparative Example 7), which does not have a surface treatment film including a nickel-containing surface treatment layer on at least one side of the copper foil substrate, has good transmission characteristics but inferior heat resistance compared to the surface-treated copper foils of Examples 1 to 51.

Claims

1. A surface-treated copper foil having a surface treatment film including a nickel-containing surface treatment layer on at least one surface of a copper foil substrate, The saturation magnetic flux density (Bs 300 ) is 5.0 x 10 -3 T or less.

2. Residual magnetic flux density (Br 300 ) is 5.0 x 10 -4 The surface-treated copper foil according to claim 1, wherein the surface tension is T or less.

3. 3. The surface-treated copper foil according to claim 1 or 2, which satisfies the following requirements (I) and (II): Requirement (I): The increase rate of saturation magnetic flux density Bs after heat treatment at 300° C. for 2 hours [{(Bs 300 -Bs 0 ) / Bs 0 }×100] is 300% or less. Requirement (II): The increase rate of residual magnetic flux density Br after heat treatment at 300° C. for 2 hours [{(Br 300 -Br 0 ) / Br 0 }×100] is 300% or less. In the above requirements (I) and (II), Bs 300 is the saturation magnetic flux density after heat treatment at 300° C. for 2 hours, Bs 0 is the saturation magnetic flux density before the heat treatment, Br 300 is the residual magnetic flux density after heat treatment at 300° C. for 2 hours, and B 0 is the residual magnetic flux density before the heat treatment.

4. On the surface having the surface treatment film, the amount of nickel deposited was 0.02 mg / dm 2 More than 3.0 mg / dm 2 The surface-treated copper foil according to any one of claims 1 to 3, wherein:

5. the surface treatment film includes, in order from the copper foil substrate side, a roughening treatment layer and the nickel-containing surface treatment layer, The surface-treated copper foil according to any one of claims 1 to 4, wherein the surface of the surface treatment film has an arithmetic mean height Sa of 0.02 µm or more and 0.35 µm or less, as measured optically in accordance with ISO 25178.

6. The surface-treated copper foil according to any one of claims 1 to 5, wherein the nickel-containing surface treatment layer is composed of a nickel alloy containing one or more elements selected from the group consisting of zinc, phosphorus, molybdenum, tungsten, chromium, iron, cobalt and niobium.

7. A copper-clad laminate comprising the surface-treated copper foil according to any one of claims 1 to 6.

8. A printed wiring board comprising the copper clad laminate of claim 7.

Citation Information

Patent Citations

  • Nickel-plated copper material and preparation method and application thereof

    CN105063699A

  • Composite copper member

    WO2020226160A1

  • Surface-treated copper foil, laminate using the same, carrier-attached copper foil, printed wiring board, electronic device, and method for manufacturing printed wiring board

    JP7055049B2

  • Surface-treated copper foil and copper clad laminate

    JP7174869B1