Electret film roll and manufacturing method thereof
By laminating a conductor on a porous electret film and winding it around a core, the method addresses excessive surface potential issues in continuous electret film production, maintaining safe and controlled surface potentials.
Patent Information
- Application Number
- JP2023058052
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
The continuous manufacturing of electret films leads to an excessive rise in surface potential, causing discharge to the human body or manufacturing equipment.
An electret film-wound body is created by laminating a conductor on at least one side of a porous electret film, which is then wound around a core, with controlled charging and winding processes to manage surface potential.
The method effectively suppresses excessive surface potential, ensuring safe and continuous production of electret films with surface potentials of 15 kV or less.
Abstract
Description
[Technical field]
[0001] The present invention relates to an electret film roll and a manufacturing method thereof, and more particularly to an electret film roll that can be suitably used for actuators, oscillators, sonars, vibration power generation, sensors, and the like, and a manufacturing method thereof. [Background technology]
[0002] An electret is a material in which a part of a polymeric material or an inorganic material that does not easily conduct electricity is semi-permanently polarized by thermally or electrically treating the material. For example, porous electrets using porous resin films are known to exhibit excellent piezoelectric effects and are widely used in actuators, oscillators, sonars, vibration power generators, sensors, etc. In order to obtain an electret with excellent piezoelectricity, it is necessary to polarize the film at a higher voltage during charge injection and to inject a larger amount of charge. As an example of a porous electret, Patent Document 1 proposes a compressible polyolefin film using a microporous membrane that utilizes β crystals of a polypropylene-based resin.
[0003] In order to turn a resin film into an electret, a high voltage must be applied to the resin film, so a batch-type charging process (poling process) was the mainstream method used in the past. However, in order to mass-produce electret films, it is necessary to produce large-area electret films continuously. For example, Patent Document 2 proposes a technique for continuously producing electret films through a charging process, a static elimination process, and a winding process. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-055114 A [Patent Document 2] JP 2022-133991 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the surface potential of a wound electret film obtained by continuously producing the electret film tends to increase as the wound length increases, and discharge (spark) may occur from the electret film wound body to the human body or production equipment.
[0006] Therefore, an object of the present invention is to provide an electret film roll capable of suppressing an excessive increase in surface potential even when produced continuously, and a method for producing the same. [Means for solving the problem]
[0007] The present inventors have conducted extensive research to achieve the above object, and as a result, have focused on solving the above object and have completed the present invention. In one aspect, the present invention is summarized as follows: [1] to
[12] .
[0008] [1] An electret film roll, comprising an electret film and a laminate having a conductor on at least one side of the electret film, wound around a core. [2] The electret film roll according to the above [1], wherein the electret film is a porous film. [3] The electret film roll according to [1] or [2] above, wherein the electret film has a porosity of more than 0% and not more than 50%. [4] The electret film roll according to any one of the above [1] to [3], wherein the electret film contains a polyolefin resin as a main component. [5] The electret film roll according to the above [4], wherein the polyolefin resin is a polypropylene resin having a β-crystal generating ability of 80% or more. [6] The electret film roll according to any one of the above [1] to [5], wherein the conductor is a metal foil. [7] The electret film roll according to any one of the above [1] to [6], wherein the absolute value of a surface potential of the electret film roll is 15 kV or less. [8] A charging treatment step (A) of charging the film to obtain an electret film; A conductor lamination step (B) of laminating a conductor on at least one surface of the electret film to obtain a laminate; a winding step (C) of winding the laminate around a core to obtain a wound body; The method for producing an electret film roll has at least the above features. [9] The method for producing an electret film roll according to the above [8], wherein the length of the film wound into a roll obtained in the winding step (C) is 5 m or more.
[10] The method for producing an electret film roll according to the above [8] or [9], wherein the absolute value of the applied voltage in the charging treatment step (A) is 6 kV or more and 20 kV or less.
[11] The method for producing an electret film roll according to any one of the above [8] to
[10] , wherein the charging step (A), the conductor laminating step (B), and the winding step (C) are performed while transporting the film.
[12] The method for producing an electret film roll according to any one of the above [8] to
[11] , wherein the film transport speed is 1 m / min or more and 10 m / min or less. Effect of the Invention
[0009] According to the present invention, even when electret film rolls are continuously produced, an excessive increase in surface potential can be suppressed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present invention will be described in detail. However, the content of the present invention is not limited to the embodiment described below.
[0011] <Electret film roll> The electret film wound body of the present invention (hereinafter also referred to as "the present wound body") is formed by winding an electret film and a laminate including a conductor on at least one surface of the electret film, around a core. In this wound body, excess charge accumulated in the electret film is transferred to the earth through the conductor, so that even if the winding length is increased, an excessive rise in the surface potential can be suppressed. The absolute value of the surface potential of the present wound body is preferably 15 kV or less, more preferably 12 kV or less, even more preferably 10 kV or less, and even more preferably 5 kV or less.
[0012] 1. Electret film The electret film of the present wound body can be suitably made of a resin film that has been charged. The resin film is not particularly limited as long as it exhibits piezoelectric properties by being charged, but is preferably a porous film in order to further enhance the piezoelectric properties. When the electret film is a porous film, the method of making it porous is not particularly limited, but examples of the porous film include chemical or physical foaming and porous film made by stretching. Among them, a film made porous by stretching is preferred in that a dense porous structure is obtained and the shape of the pores is easily controlled. In the following description, the film before being subjected to charging treatment may be referred to as a "film", and the film after being subjected to charging treatment and static elimination treatment may be referred to as an "electret film".
[0013] Examples of materials for the film include polyolefin resins, fluororesins, vinyl chloride resins, polystyrene resins, butadiene resins, polyester resins, and acrylic resins. Polyolefin resins are preferred because they have a small environmental impact and are easy to charge.
[0014] (1) Polyolefin resin The film of the present invention preferably contains a polyolefin resin as a main component, and more preferably contains a polypropylene resin as a main component. When the film contains a polyolefin resin as a main component, the content of the polyolefin resin in the film is 50% by mass or more, preferably 70% by mass or more and 99.9999% by mass or less, more preferably 80% by mass or more and 99.999% by mass or less, and even more preferably 90% by mass or more and 99.99% by mass or less.
[0015] Furthermore, when the film is primarily composed of a polypropylene resin, the content of the polypropylene resin in the film is 50% by mass or more, preferably 70% by mass or more and 99.9999% by mass or less, more preferably 80% by mass or more and 99.999% by mass or less, and even more preferably 90% by mass or more and 99.99% by mass or less. Examples of polypropylene resins include homopolypropylene (propylene homopolymer), and random or block copolymers of propylene and α-olefins such as ethylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, or 1-decene. Among these, homopolypropylene is more preferably used from the viewpoint of mechanical strength.
[0016] Furthermore, the polypropylene resin preferably has an isotactic pentad fraction, which indicates stereoregularity, of 80% or more and 99% or less, more preferably 83% or more and 98% or less, and further preferably 85% or more and 97% or less. If the isotactic pentad fraction is 80% or more, the mechanical strength is good. On the other hand, the upper limit of the isotactic pentad fraction is set at the upper limit that can be obtained industrially at present, but this will not apply in the future if a resin with higher regularity is developed at the industrial level. The isotactic pentad fraction means a three-dimensional structure or a ratio thereof in which all five methyl groups, which are side chains, are located in the same direction relative to the main chain formed by carbon-carbon bonds composed of any five consecutive propylene units. The assignment of signals in the methyl group region is in accordance with A. Zambelli et al. (Macromol. 8, 687 (1975)).
[0017] Moreover, the polypropylene resin preferably has a Mw / Mn, which is a parameter indicating the molecular weight distribution, of 1.5 or more and 10.0 or less, more preferably 2.0 or more and 8.0 or less, and further preferably 2.0 or more and 6.0 or less. A smaller Mw / Mn ratio means a narrower molecular weight distribution, but by making the Mw / Mn ratio 1.5 or more, sufficient extrusion moldability is obtained and industrial mass production is possible, while by making the Mw / Mn ratio 10.0 or less, sufficient mechanical strength can be ensured. Mw / Mn is measured by GPC (gel per emission chromatography) method and expressed as a polystyrene equivalent value.
[0018] The melt flow rate (MFR) of the polypropylene resin is not particularly limited, but in general, the MFR is preferably 0.5 g / 10 min or more and 15 g / 10 min or less, and more preferably 1.0 g / 10 min or more and 10 g / 10 min or less. By setting the MFR to 0.5 g / 10 min or more, sufficient melt viscosity can be obtained during molding and high productivity can be ensured, while by setting the MFR to 15 g / 10 min or less, sufficient strength can be ensured. The MFR is measured in accordance with JIS K7210-1 (2014) at a temperature of 230°C and a load of 2.16 kg.
[0019] The method for producing the polypropylene resin is not particularly limited, and examples thereof include known polymerization methods using known polymerization catalysts, such as a polymerization method using a multi-site catalyst represented by a Ziegler-Natta catalyst or a single-site catalyst represented by a metallocene catalyst.
[0020] Examples of polypropylene-based resins that can be suitably used in the present invention include commercially available products such as those sold under the trade names "Novatec PP," "WINTEC," and "WAYMAX" (manufactured by Japan Polypropylene Corporation), "Versify," "Notio," and "Tafmer XR" (manufactured by Mitsui Chemicals, Inc.), "Zelas" and "Thermorun" (manufactured by Mitsubishi Chemical Corporation), "Sumitomo Noblen" and "Tafthren" (manufactured by Sumitomo Chemical Co., Ltd.), "Prime Polypro" and "Prime TPO" (manufactured by Prime Polymer Co., Ltd.), "Adflex," "Adsyl," and "HMS-PP (PF814)" (manufactured by SunAllomer Co., Ltd.), and "Inspire" (Dow Chemical Co., Ltd.).
[0021] [β crystal activity] The film of the present invention is preferably made of a resin composition mainly composed of a polypropylene resin containing a large amount of β-crystals, which is one of the crystalline forms. The non-porous membrane made of a resin composition mainly composed of a polypropylene resin containing a large amount of β-crystals shows excellent piezoelectricity after charging treatment, but even better piezoelectricity can be obtained by stretching to form a porous structure. The formation of a porous structure using β-crystals is advantageous for preparing a porous structure because pores are formed during the process in which the β-crystals in the polypropylene resin are transformed into α-crystals during the stretching process, and the porous structure is dense, and does not depend on particle size or dispersion diameter compared to the pores formed by the addition of inorganic fillers or incompatible organic substances, which are known in the art. A film made porous by using β crystals has a dense porous structure and a large surface area of the pores, so that more charges are easily trapped during the charging process. Since a porous electret film exhibits piezoelectricity due to charges trapped at the interface between the pores and the matrix, a dense porous structure of the film tends to improve the piezoelectric properties. In addition, a dense porous structure makes the distance between the pores very short, and the trapped charges are easily fixed by the mutual Coulomb force. This makes it difficult for the trapped charges to be discharged, and the properties of the electret film are also less likely to deteriorate.
[0022] The β-crystal activity of the film of the present invention can be regarded as an index showing that the polypropylene resin in the nonporous membrane material before stretching has generated β-crystals. If the polypropylene resin in the nonporous membrane material before stretching has generated β-crystals, many fine and uniform pores are formed by subsequent stretching, so that excellent mechanical properties can be obtained, and excellent voltage resistance can be obtained by the formation of fine and uniform pores.
[0023] The presence or absence of β-crystal activity in the film is determined by performing differential thermal analysis of the obtained electret film using a differential scanning calorimeter and determining whether or not a crystal melting peak temperature derived from the β-crystal of the polypropylene-based resin is detected. Specifically, when an electret film is heated in a differential scanning calorimeter from 40°C to 200°C at a heating rate of 10°C / min and held for 1 minute, then cooled from 200°C to 40°C at a cooling rate of 10°C / min and held for 1 minute, and then heated again from 40°C to 200°C at a heating rate of 10°C / min, if a crystal melting peak temperature (Tmβ) derived from the β crystals of the polypropylene resin is detected during reheating, it is determined to have β crystal activity.
[0024] The presence or absence of the β-crystal activity can also be determined by the diffraction profile obtained by X-ray diffraction measurement of an electret film that has been subjected to a specific heat treatment. In detail, the film is subjected to heat treatment at 170 to 190°C, which is a temperature exceeding the crystal melting peak temperature of the polypropylene resin, and then slowly cooled to generate and grow β-crystals. When X-ray diffraction measurement is performed on the film, and a diffraction peak derived from the (300) plane of the β-crystal of the polypropylene resin is detected in the range of 2θ = 16.0° to 16.5°, it is determined that the film has β-crystal activity. For details on the β-crystal structure and X-ray diffraction measurement of the polypropylene resin, Macromol.Chem.187,643-652(1986), Prog.Polym.Sci.Vol.16,361-404(1991), Macromol.Symp.89,499-511(1995), Macromol.Chem.75,134(1964), and references cited in these documents can be referred to.
[0025] The above-mentioned method for obtaining β-crystal activity of polypropylene resin includes a method of not adding a substance that promotes the formation of α-crystal of polypropylene resin, a method of adding polypropylene resin that has been treated to generate peroxide radicals as described in Japanese Patent No. 3739481, and a method of adding a β-crystal nucleating agent, but in the present invention, it is particularly preferable to obtain β-crystal activity by adding a β-crystal nucleating agent. By adding a β-crystal nucleating agent, it is possible to promote the formation of β-crystal of polypropylene resin more uniformly and efficiently, and to obtain a film having β-crystal activity.
[0026] The degree of β-crystal activity of the polypropylene resin contained in the film can be quantified by measuring the β-crystal formation ability. The β-crystal formation ability may be measured, for example, in an electret film. The β-crystal formation ability of the specific polypropylene resin is preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more. When the β-crystal generating ability is 80% or more, the film can exhibit suitable piezoelectricity when made into an electret film. There is no particular upper limit to the β-crystal generating ability, but it is preferably 100% or less. The β-crystal forming ability is calculated by the method described below.
[0027] (2) β-crystal nucleating agent The film of the present invention preferably contains a β-crystal nucleating agent in order to obtain an electret film with excellent piezoelectricity. By containing a β-crystal nucleating agent, it is possible to have β-crystal activity. Examples of the β-crystal nucleating agent used in the present invention include the following. If necessary, two or more types of β-crystal nucleating agents may be mixed and used.
[0028] Examples of the β-crystal nucleating agent include amide compounds; tetraoxaspiro compounds; quinacridones; iron oxides having a nanoscale size; alkali or alkaline earth metal salts of carboxylic acids, such as potassium 1,2-hydroxystearate, magnesium benzoate or magnesium succinate, and magnesium phthalate; aromatic sulfonic acid compounds, such as sodium benzenesulfonate or sodium naphthalenesulfonate; di- or triesters of di- or tribasic carboxylic acids; phthalocyanine pigments, such as phthalocyanine blue; two-component compounds consisting of component A which is an organic dibasic acid and component B which is an oxide, hydroxide, or salt of a metal in Group 2 of the periodic table; and compositions consisting of a cyclic phosphorus compound and a magnesium compound.
[0029] Among these β-crystal nucleating agents, amide compounds are preferred. The use of amide compounds can enhance the piezoelectric properties of the electret film. Examples of amide compounds include N,N'-dicyclohexyl-2,6-naphthalenedicarboxyamide, N,N'-dicyclohexylterephthalamide, and N,N'-diphenylhexanediamide, among which N,N'-dicyclohexyl-2,6-naphthalenedicarboxyamide is preferred. Since amide compounds have highly polar amide groups, they can localize charges in the crystal structure, and are considered to have high piezoelectric properties. On the other hand, compounds with high polarity such as amide compounds have poor dispersibility in polypropylene resins with low polarity due to electrostatic interactions, and are prone to aggregation. However, general β crystal nucleating agents have the property of dissolving in polypropylene resins at a certain temperature range. Due to this property, the β crystal nucleating agent is uniformly dispersed in the polypropylene resin, and crystals derived from the β crystal nucleating agent are easily precipitated uniformly. Therefore, it is believed that crystals of the amide compound with high polarity are uniformly dispersed in the polypropylene resin with low polarity, and high piezoelectric properties can be obtained.
[0030] Specific examples of commercially available β-crystal nucleating agents include the β-crystal nucleating agent "N-Jester NU-100" manufactured by New Japan Chemical Co., Ltd., and specific examples of propylene-based resins to which a β-crystal nucleating agent has been added include the polypropylene "Bepol B-022SP" manufactured by Aristech, the polypropylene "Beta(β)-PP BE60-7032" manufactured by Borealis, and the polypropylene "BNX BETAPP-LN" manufactured by Mayzo.
[0031] The content of the β-crystal nucleating agent in the film can be appropriately adjusted depending on the type of β-crystal nucleating agent or the composition of the polypropylene resin, but is preferably 0.0001 to 5.0 parts by mass relative to 100 parts by mass of the polypropylene resin, more preferably 0.001 to 3.0 parts by mass, and even more preferably 0.01 to 1.0 parts by mass. If it is 0.0001 parts by mass or more, the β-crystals of the polypropylene resin can be sufficiently generated and grown during production, sufficient β-crystal activity can be ensured, and sufficient β-crystal activity can be ensured even when the film is made into a porous film. Therefore, a porous electret film having the desired piezoelectricity can be obtained by charging the porous film. On the other hand, if it is added in an amount of 5.0 parts by mass or less, it is economically advantageous and there is no bleeding of the β-crystal nucleating agent onto the film surface, which is preferable.
[0032] (3) Other ingredients When the film of the present invention is a porous film, it may contain a foaming agent, a filler, or the like instead of or in addition to the β-crystal nucleating agent. For example, when a film made porous by chemical or physical foaming is used as the film of the present invention, it is preferable to add a chemical foaming agent, a physical foaming agent, a supercritical fluid, a thermally expandable microcapsule, etc. to the resin that is the main component. These may be used alone or in combination of two or more kinds. In addition, when a film made porous by stretching is used as the film of the present invention, it is also preferable to add a resin that is incompatible with the main resin or an inorganic filler, such as calcium carbonate, calcium sulfate, barium carbonate, barium sulfate, titanium oxide, talc, clay, kaolinite, and montmorillonite.
[0033] In addition, the film of the present invention may contain various additives, such as heat stabilizers, antioxidants, ultraviolet absorbers, light stabilizers, crystal nucleating agents, colorants, antistatic agents, hydrolysis inhibitors, lubricants, flame retardants, conductive agents, and elastomers, to the extent that the properties of the film are not impaired.
[0034] (4) Physical properties of electret film The porosity of the electret film of the present invention is preferably more than 0% and not more than 50%, more preferably 5% to 40%, even more preferably 10% to 35%, and even more preferably 10% to 30%. By setting the porosity of the electret film within the above range, the pressure resistance of the electret film becomes good.
[0035] The thickness of the electret film of the present invention is preferably from 10 μm to 200 μm, more preferably from 15 μm to 150 μm, and further preferably from 20 μm to 120 μm. By setting the thickness of the electret film within the above range, the piezoelectric properties can be improved, and roll-to-roll transportation and winding can be facilitated.
[0036] (5) Film manufacturing method The method for producing the film before the charging treatment is not particularly limited, but it is preferably produced through a film-forming step (a) and a stretching step (b), although the stretching step (b) may be omitted. The film obtained in the above-mentioned film-forming step (a), or the film obtained in the film-forming step (a) and the stretching step (b), may be transported to a winding step (c) and wound up into a roll. The film-forming step (a), the stretching step (b), and the winding step (c) will be described in order below.
[0037] (5-1) Film forming process (a) In the film-forming step (a), a non-porous film-like material is formed from the material that constitutes the film. The film-forming method is not particularly limited, but for example, a method of heating and melting the resin (material resin) that constitutes the film to form a film can be mentioned. Specifically, the T-die method and the inflation method can be mentioned, and among them, the T-die method is preferably used. For practical purposes, it is preferable to melt-extrude the material resin from the T-die and cast it with a cast roll (chill roll, cast drum, etc.). Furthermore, the material resin may be appropriately mixed with additives, or two or more resin components may be mixed together to form a film as a resin composition containing two or more components.
[0038] The material constituting the film may be kneaded in a kneading device before being formed into a film. The kneading device used for kneading is not particularly limited. For example, a known extruder such as a single screw extruder, a twin screw extruder, or a multi-screw extruder can be used. Depending on the equipment structure and necessity, a pressure reducer may be connected to the vent port of the extruder to remove moisture and low molecular weight substances from the material constituting the film.
[0039] As a specific method for forming a film, when the T-die method is used, a sheet-like molten resin is extruded from a T-die onto a casting roll, and then pulled up while being in close contact with the rotating casting roll to form a film-like material. In order to bring the film-like material into close contact with the casting roll, a touch roll, an air knife, an electric contacting device, or the like may be attached to the casting roll.
[0040] In addition, when the molten resin (resin composition) is cooled and molded into a film, the temperature of the cast roll is preferably 100° C. or higher, more preferably 110° C. or higher, and even more preferably 120° C. or higher. In the present invention, since the porosity can also be increased by opening holes in the crystalline and amorphous parts of the polypropylene resin during the stretching process, it is preferable to set the temperature of the cast roll to 100° C. or higher to obtain a nonporous membrane with a high degree of crystallinity. The upper limit of the casting roll temperature is preferably 140° C. or lower, more preferably 135° C. or lower, and even more preferably 130° C. or lower. By setting the casting roll temperature to 140° C. or lower, peeling from the casting roll during film formation becomes easy.
[0041] In the obtained nonporous membrane, the thickness of the effective portion excluding both ends is preferably 30 μm to 500 μm, more preferably 40 μm to 300 μm, and even more preferably 50 μm to 200 μm. If the thickness of the nonporous membrane is 30 μm or more, breakage during stretching can be prevented, and if the thickness of the nonporous membrane is 500 μm or less, stretching of the nonporous membrane can be facilitated. The layer structure of the non-porous film is not limited to the single layer structure described above, and may be a combination of other layers.
[0042] (5-2) Stretching process (b) The obtained nonporous membrane-like material may be directly charged or wound up, or may be stretched. By stretching the nonporous membrane-like material, the nonporous membrane-like material can be easily made into a porous film. In the stretching step, the nonporous membrane may be stretched uniaxially or biaxially, but from the viewpoint of increasing the pressure resistance of the film by setting the porosity of the film to more than 0% and not more than 50%, uniaxial stretching is preferable. The uniaxial stretching may be longitudinal uniaxial stretching or transverse uniaxial stretching. The biaxial stretching may be simultaneous biaxial stretching or sequential biaxial stretching. The stretching of the film in the machine direction (MD) is called "longitudinal stretching", and the stretching in the direction perpendicular to the machine direction (TD) is called "transverse stretching".
[0043] The stretching temperature must be appropriately selected depending on the composition of the resin composition used, the crystalline melting peak temperature, the crystallinity, etc., but the longitudinal stretching temperature is preferably 60°C or higher and 140°C or lower, more preferably 80°C or higher and 120°C or lower. A longitudinal stretching temperature of 140° C. or less is preferable because stretching can be performed without breakage at a temperature below the melting point of the polypropylene resin, which is a suitable main component, whereas a longitudinal stretching temperature of 60° C. or more is preferable because breakage during stretching can be suppressed. The transverse stretching temperature is preferably 90° C. or more and 160° C. or less, more preferably 100° C. or more and 150° C. or less. When the transverse stretching temperature is within the specified range, stretching can be performed without breakage. In addition, when transverse stretching is performed after longitudinal stretching, the pores generated during longitudinal stretching are enlarged, increasing the porosity, and sufficient piezoelectric properties can be obtained. The temperatures described above are for uniaxial stretching or sequential biaxial stretching, but the stretching temperature for simultaneous biaxial stretching may be adjusted within the range of preferably 90°C or more and 140°C or less, more preferably 100°C or more and 120°C or less, from the above-mentioned viewpoints.
[0044] The stretching ratio may be selected arbitrarily according to the desired porosity, but the stretching ratio per uniaxial stretching is preferably 1.1 to 10 times, more preferably 1.5 to 9.0 times, and even more preferably 1.5 to 8.0 times. By setting the stretching ratio per uniaxial stretching to 1.1 times or more, whitening progresses and the stretching-induced porosity becomes sufficient, while by setting the stretching ratio per uniaxial stretching to 10 times or less, the porosity does not become too high and a film with excellent pressure resistance can be obtained. In the case of successive biaxial stretching, by stretching at the stretch ratio specified above for each axis, voids generated during the previous stretching are not deformed during the subsequent stretching.
[0045] (5-3) Winding process (c) The film obtained by the film-forming step (a) and the stretching step (b) may be wound around a core to be wound into a roll. The length of the film is not particularly limited, but from the viewpoint of facilitating continuous charging treatment and conductor lamination described later, it is preferably 5 m or more, more preferably 10 m or more, even more preferably 20 m or more, and even more preferably 50 m or more. The length of the film is preferably 10,000 m or less.
[0046] 2. Conductor The conductor of the present wound body may be any conductive material, for example, a metal foil, a carbon sheet, or a sheet made of conductive particles and a resin. Examples of the metal foil include aluminum foil, copper foil, silver foil, gold foil, nickel foil, and tin foil. Examples of the conductive particles include carbon particles, silver particles, gold particles, copper particles, nickel particles, aluminum particles, tin particles, and zinc particles. Examples of the resin that can be used in combination with the conductive particles include silicone resin, urethane resin, urea resin, epoxy resin, polyolefin resin, and polyester resin.
[0047] The thickness of the conductor is preferably 2 μm or more and 100 μm or less, more preferably 3 μm or more and 50 μm or less, and even more preferably 5 μm or more and 30 μm or less.
[0048] 3. Core The core refers to a cylindrical core used for winding up a film. The material of the core is not particularly limited, but examples thereof include paper, resin-impregnated paper, acrylonitrile-butadiene-styrene copolymer (ABS resin), FRP, phenol resin, and inorganic substance-containing resin. Among them, from the viewpoints of a small thermal expansion coefficient, high rigidity, low swelling due to humidity, and excellent winding properties, it is preferable to use a resin such as acrylonitrile-butadiene-styrene copolymer (ABS resin), FRP, phenol resin, or inorganic substance-containing resin. When the core material is paper, the desired characteristics can be easily obtained by coating the surface with a resin, etc. Furthermore, from the viewpoint of surface smoothness, it is also preferable that the core is a tube made of resin-impregnated paper.
[0049] <Manufacturing method of electret film roll> The manufacturing method for an electret film wound body of the present invention (hereinafter also referred to as "the present manufacturing method") includes at least an electrification treatment step (A) of charging a film to obtain an electret film, a conductor lamination step (B) of laminating a conductor on at least one side of the electret film to obtain a laminate, and a winding step (C) of winding the laminate around a core to obtain a wound body. This manufacturing method is highly efficient because it allows the continuous production of electret films by continuously conducting the charging process (A) and the conductor lamination process (B) while transporting the film with multiple guide rolls and winding it up into a roll. In the present production method, the film transport speed is preferably 1 m / min or more and 10 m / min or less. By setting the conveying speed within the above range, the productivity can be improved and the film can be sufficiently electretized in the charging treatment step (A). A preferred embodiment of the present production method will now be described.
[0050] 1. Manufacturing method according to the first embodiment The manufacturing method according to the first embodiment of the present invention (hereinafter also referred to as the "first manufacturing method") is applied when the film before charging is wound into a roll, and the process from unwinding the film to manufacturing the rolled body is carried out continuously. The first manufacturing method includes an unwinding step (X) of unwinding the film wound into a roll, an electrification treatment step (A) of electrifying the film to obtain an electret film, a conductor lamination step (B) of laminating a conductor on at least one side of the electret film to obtain a laminate, and a winding step (C) of winding the laminate around a core to obtain a wound body. In this manufacturing method, the surface potential can be further reduced by winding the conductor while connecting it to earth, or by connecting the conductor to earth after obtaining the wound body. The unwinding step (X), the electrification treatment step (A), the conductor lamination step (B) and the winding step (C) will be described below.
[0051] (1) Unwinding process (X) In the unwinding process (X), the film wound in a roll is unwound. The unwound film may be transported and directly subjected to the charging process (A), or may be slit to a width suitable for the subsequent process, or may be shortened in length. When the length of the film is shortened, from the viewpoint of facilitating continuous charging treatment and conductor lamination described below, the length is preferably from 5 m to 1000 m, more preferably from 10 m to 500 m, and even more preferably 50 m or more.
[0052] (2) Charging process (A) In the charging treatment step (A), the film unwound from the roll in the unwinding step (X) is converted into an electret by applying a voltage to the film while being transported by a guide roll.
[0053] The charging process may be carried out by passing the film between electrodes such as needle electrodes, wire electrodes, roll electrodes, or plate electrodes (e.g., flat electrodes) and applying an electric field between the electrodes, or by forming electrodes directly on the front and back of the film by coating or vapor deposition and then applying an electric field. The absolute value of the applied voltage in the charging process (A) is preferably 6 kV or more and 20 kV or less. By setting the absolute value of the applied voltage to 6 kV or more, the film can be sufficiently electretized and the piezoelectric properties can be improved. In addition, by setting the absolute value of the applied voltage to 20 kV or less, insulation breakdown and spark discharge are unlikely to occur, and the deterioration of the piezoelectric properties and the deterioration of the appearance of the film can be prevented. In addition, the voltage applied in the charging treatment step (A) preferably has a negative polarity. By making the polarity negative, discharge is less likely to occur, and the electret film is more likely to retain charge, resulting in good piezoelectric properties.
[0054] The environmental temperature in the charging treatment step (A) is preferably 10° C. or higher and 100° C. or lower. When the temperature is 10° C. or higher, temperature control becomes easy and productivity becomes good. Also, when the temperature is 100° C. or lower, dielectric breakdown is unlikely to occur. In addition, the environmental humidity in the charging treatment step (A) is preferably 20% or more and 100% or less, more preferably 40% or more and 80% or less. When the humidity is 20% or more, discharge is less likely to occur, and it is possible to prevent the deterioration of the piezoelectric properties and the deterioration of the appearance of the film. In addition, when the humidity is 80% or less, humidity control is easy and productivity is good. In this specification, humidity means relative humidity.
[0055] The distance (gap) between the electrode and the guide roll that transports the film in the charging process (A) is preferably 15 mm or more and 25 mm or less. When the gap is 15 mm or more, a high electric field is not applied to the film, making it difficult for dielectric breakdown and spark discharge to occur. Also, when the gap is 25 mm or less, a sufficient electric field can be applied to the film, and the film can be sufficiently electretized. Note that the guide roll here constitutes the earth roll as described above. That is, in the charging process (A), when the film is passed between a pair of electrodes, the gap between the electrodes is preferably 15 mm or more and 25 mm or less.
[0056] (3) Conductor lamination process (B) In the conductor laminating step (B), a conductor is laminated on at least one surface of the electret film obtained in the charging treatment step (A) to obtain a laminate. The method for laminating the conductor is not particularly limited, and the conductor may be laminated directly onto the electret film or via an adhesive layer or the like. From the viewpoint of preventing a decrease in the piezoelectric properties of the electret film, it is preferable to laminate the conductor directly without using an adhesive layer.
[0057] (4) Winding process (C) In the winding step (C), the laminate obtained in the conductor laminating step (B) is wound around a core to obtain an electret film wound body. The length of the film wound into a roll is not particularly limited, but is preferably 5 m or more, more preferably 10 m or more, even more preferably 20 m or more, and even more preferably 50 m or more. The length of the film is preferably 10,000 m or less. When the length of the film is 5 m or more, the above-mentioned charging process and conductor lamination can be easily performed continuously.
[0058] 2. Manufacturing method according to the second embodiment The production method according to the second embodiment of the present invention (hereinafter also referred to as the "second production method") is a method in which the steps from film formation to production of a wound body are carried out continuously. That is, the second manufacturing method includes a film-forming step (a) of forming a film, a charging step (A) of charging the film to obtain an electret film, a conductor laminating step (B) of laminating a conductor on at least one side of the electret film to obtain a laminate, and a winding step (C) of winding the laminate around a core. Since the piezoelectric properties can be further improved by stretching the film to make it porous, it is preferable to have a stretching step (b) of stretching the formed film between the film-forming step (a) and the charging step (A).
[0059] The film-forming step (a) and the stretching step (b) are the same as the film-forming step (a) and the stretching step (b) described in 1.(5) of <Electret film roll> above. The charging step (A), the conductor lamination step (B) and the winding step (C) are the same as the charging step (A), the conductor lamination step (B) and the winding step (C) described in the first manufacturing method. However, the charging step (A) in the second manufacturing method is performed by transporting the film after the film-forming step (a) (after the stretching step (b) in the case of stretching) with a guide roll, without winding.
[0060] 3.Other The manufacturing method of the present invention may include a functional layer lamination step (Y) of laminating a functional layer such as a protective layer on the electret film. In that case, the functional layer lamination step (Y) may be performed after the conductor lamination step (B) or after the winding step (C) in the first manufacturing method and the second manufacturing method. More specifically, the functional layer may be laminated after the conductor lamination step (B) is performed, and the electret film on which the functional layer is laminated (laminated electret film) may be wound in the winding step (C). In addition, after the conductor lamination step (B) is performed, an electret film roll may be obtained once in the winding step (C), and then the electret film may be unwound again to laminate a functional layer on the electret film.
[0061] Examples of the functional layer include a protective layer and a printed layer. The material of the protective layer is not particularly limited as long as it can protect the electret film, and examples thereof include resin films made of polyester-based resins, polyolefin-based resins, acrylic-based resins, polystyrene-based resins, polycarbonate-based resins, fluorine-based resins, etc. The material of the printing layer may be any of paper, film, cloth, and the like.
[0062] These functional layers may be laminated by overlapping with the electret film, may be laminated via an adhesive layer, or may be laminated by a method such as thermal lamination.
[0063] <Applications of electret film> The electret film of the present invention can be used, for example, as an actuator, an oscillator, a sonar, a vibration power generation, a sensor, etc. The electret film is not particularly limited, but for example, by mounting a lead wire or forming an insulating film to form a piezoelectric element, the pressure acting on the electret film can be converted into a voltage, and the pressure acting on the electret film can be detected or electricity can be generated. EXAMPLES
[0064] The piezoelectric film of the present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited in any way.
[0065] The electret film rolls obtained in the examples and comparative examples were evaluated for thickness, porosity, β-crystal formation ability, and surface potential by the following methods.
[0066] (1) Thickness The thickness of the electret film was measured at 10 random points using a 1 / 1000 mm dial gauge, and the average value was calculated.
[0067] (2) Porosity The electret film was cut into a size of 100 mm width x 100 mm length to prepare a measurement sample. The actual mass W1 of the measurement sample was measured, and the mass W0 when the porosity was 0% was calculated based on the density of the resin composition. The porosity was calculated from these values based on the following formula. Porosity (%)={(W0-W1) / W0}×100
[0068] (3) β crystal formation ability The DSC measurement of the electret film was carried out by the method shown below. First, the temperature was raised from 40 ° C. to 200 ° C. at 10 ° C. / min under a nitrogen atmosphere, and then held for 1 minute, and then cooled to 40 ° C. at 10 ° C. / min. Regarding the melting peak observed when the temperature was raised again at 10 ° C. / min after holding for 1 minute, the melting peaks present in the temperature range of 145 to 157 ° C. were considered to be the melting peaks of β crystals, and the melting peaks observed at 158 ° C. or higher were considered to be the melting peaks of α crystals. The heat of fusion of each was calculated from the area of the region surrounded by the baseline and the peaks drawn based on the flat part on the high temperature side, and the heat of fusion of the α crystals was ΔHα, and the heat of fusion of the β crystals was ΔHβ, and calculated by the following formula. β crystal formation ability (%) = [ΔHβ / (ΔHα+ΔHβ)]×100
[0069] (4) Surface potential The surface potential of the electret film roll was measured using a non-contact electrostatic potential meter (Keyence Corporation, static electricity measuring instrument SK-H050) in accordance with JIS C 61340-2-2.
[0070] The materials used in the examples and comparative examples are as follows. (Polypropylene resin) A-1: Homopolypropylene (Novatec PP FY6HA, MFR: 2.4g / 10min [230℃, 2.16kg load], Mw / Mn=3.2, Japan Polypropylene Corporation) (β crystal nucleating agent) B-1: N,N'-dicyclohexyl-2,6-naphthalenedicarboxamide (NU-100, manufactured by New Japan Chemical Co., Ltd.) (Antioxidants) C-1: A 1:1 mixture of tris(2,4-di-t-butylphenyl)phosphite and tetrakis[3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionic acid]pentaerythritol (IRGANOX-B225, manufactured by BASF)
[0071] Example 1 100 parts by mass of polypropylene resin (A-1), 0.2 parts by mass of β-crystal nucleating agent (B-1), and 0.1 parts by mass of antioxidant (C-1) were mixed and melt-extruded at 280°C using a twin-screw extruder to obtain resin composition 1. Resin composition 1 was charged into the extruder connected to a T-die with a lip opening of 1 mm and molded, and was guided to a cast roll to obtain a non-porous membrane 1 with a thickness (thickness of the effective part excluding both ends) of 60 μm. Thereafter, the film was stretched 5 times in the transverse direction at a stretching temperature of 100°C in a film tenter facility (manufactured by Kyoto Machinery Co., Ltd.) to obtain a porous film 1 having a thickness of 60 μm, a width of 25 cm, and a length of 20 m. The porous film 1 was wound around a core and wound into a roll. The porosity of the obtained porous film was 18%, and the β crystal activity was 70%. The obtained porous film 1 was transported by a roll-to-roll type film transport device set to a transport speed of 2 m / min. At that time, a high voltage application device equipped with a wire electrode (Φ0.15 mm, made of tungsten) was used during the transport process to apply a voltage of -15 kV to perform charging treatment. At this time, the gap between the wire electrode and the earth roll was 30 mm. Then, an aluminum foil with a thickness of 12 μm connected to the earth was laminated, and the film was wound around a core to obtain an electret film roll. The environmental temperature during the experiment was 27°C, the humidity was 60%, and the surface temperature of the earth roll was 20°C. The surface potential of the obtained electret film roll was 3.5 kV.
[0072] Comparative Example 1 After the porous film 1 was charged, an electret film roll was obtained in the same manner as in Example 1, except that the aluminum foil was not laminated thereon. The surface potential of the obtained electret film roll was 25 kV.
[0073] Example 1 and Comparative Example 1 show that the wound body of the present invention can suppress an excessive increase in the surface potential after winding by laminating the electret film and the conductor and winding them around a core.
Claims
1. The electret film roll is formed by winding an electret film and a laminate having a conductor on at least one surface of the electret film around a core.
2. The electret film roll according to claim 1 , wherein the electret film is a porous film.
3. The electret film roll according to claim 1 , wherein the electret film has a porosity of more than 0% and not more than 50%.
4. The electret film roll according to claim 1 , wherein the electret film contains a polyolefin resin as a main component.
5. The electret film roll according to claim 4 , wherein the polyolefin resin is a polypropylene resin having a β-crystal generating ability of 80% or more.
6. The electret film roll according to claim 1 , wherein the conductor is a metal foil.
7. The electret film roll according to claim 1 , wherein an absolute value of a surface potential of the electret film roll is 15 kV or less.
8. A charging treatment step (A) of charging the film to obtain an electret film; A conductor lamination step (B) of laminating a conductor on at least one surface of the electret film to obtain a laminate; a winding step (C) of winding the laminate around a core to obtain a wound body; The method for producing an electret film roll has at least the above features.
9. The method for producing an electret film roll according to claim 8 , wherein the electret film obtained in the winding step (C) has a length of 5 m or more.
10. The method for producing an electret film roll according to claim 8 , wherein an absolute value of the applied voltage in the charging treatment step (A) is 6 kV or more and 20 kV or less.
11. The method for producing an electret film roll according to claim 8 , wherein the charging step (A), the conductor laminating step (B), and the winding step (C) are performed while the film is being transported.
12. The method for producing an electret film roll according to claim 11, wherein the film transport speed is 1 m / min or more and 10 m / min or less.
Citation Information
Patent Citations
Electret film manufacturing method and manufacturing device
JP2022133991A
Multilayered film, method for producing same, and use thereof
WO2021200790A1
Compressible polyolefin film, piezoelectric element, vibration element, and sensor
JP2017055114A