Clothing laminate and infection prevention clothing
A laminate of polyamide fiber knitted fabrics and a polyurethane microporous membrane addresses the issues of stretchability, lightness, and moisture permeability in infection prevention clothing, ensuring comfort and effective protection against blood and viruses, including resistance to disinfectants.
Patent Information
- Application Number
- JP2023058302
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing infection prevention clothing lacks sufficient stretchability, lightness, and moisture permeability, leading to discomfort and stuffiness, especially in summer, and does not adequately address chemical resistance against disinfectants like ethanol.
A laminate structure composed of polyamide fiber knitted fabrics for the outer and lining layers, combined with a polyurethane microporous membrane, and an adhesive layer, providing excellent stretchability, lightness, moisture permeability, and durability against alcohol, while maintaining virus and blood barrier properties.
The laminate ensures comfort and ease of movement by preventing stuffiness, maintaining lightweight properties, and offering robust protection against blood and viruses, even after repeated washing and disinfection.
Smart Images

Figure 2024145798000001 
Figure 2024145798000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a clothing laminate and an infection-preventing clothing that have barrier properties against blood and viruses, and are also excellent in moisture permeability, stretchability, and light weight. [Background technology]
[0002] In recent years, in the medical field, infection protection clothing is used in medical settings to protect the body from viruses and the like. In addition to having high virus barrier properties and blood barrier properties, infection protection clothing is also required to have high moisture permeability that can efficiently release heat and moisture generated by sweating to the outside of the fabric from the viewpoint of wearing comfort. Here, in order to have high virus barrier properties and blood barrier properties, it is required to have high waterproof performance that is commensurate with them. If the desired waterproofness is not achieved, blood, body fluids, etc. will easily penetrate, and the opportunity to come into contact with bacteria, viruses, etc. will increase. And, as a clothing material that has both waterproofness to achieve virus barrier properties and blood barrier properties and moisture permeability, a blood / virus barrier laminate in which a substrate, a resin film, and an adhesive layer are laminated has been conventionally known. For example, Patent Document 1 describes a laminate in which a woven fabric made of polyester-based fibers is used as a surface fiber fabric, a knitted fabric made of polyester-based fibers is used as a lining fiber fabric, and the surface fiber fabric, a microporous membrane and adhesive layer made of polycarbonate-based polyurethane resin, and the lining fiber fabric are laminated in this order. Patent Document 2 describes a laminate usable for medical applications in which a tricot knitted fabric made of polyester filaments is laminated on both sides of a film mainly composed of polycarbonate-based polyurethane resin via an adhesive resin. Patent Document 3 describes a blood barrier laminate having excellent washing durability, which is a laminate in which a surface fabric, a first adhesive layer, a microporous polytetrafluoroethylene (PTFE) film having moisture permeability, a second adhesive layer, and a lining are laminated together in this order, and both the surface fabric and the lining are woven or knitted fabrics using polyester fibers. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2014-46576 A [Patent Document 2] JP 2012-076273 A [Patent Document 3] JP 2014-121858 A
[0004] Conventionally, infection prevention clothing such as infection protection clothing includes disposable types that are assumed to be used once and reusable types that are assumed to be used multiple times while being disinfected and washed after each use. These infection prevention clothing are required to have excellent virus barrier properties and blood barrier properties in particular, and therefore, in particular, reusable infection protection clothing is required to have washing durability against disinfection, etc., so the fabric is thick and has poor stretchability. Such infection protection clothing is easy to feel fatigued due to the weight of the infection protection clothing and low stretchability when worn, and is prone to becoming stuffy when worn in the summer, so it is poor in comfort and workability. In recent years, as temperatures have risen due to global warming, there has been a growing demand for infection protection clothing that prevents stuffiness when worn in the summer, allows ease of movement even when worn for long periods of time, and is less uncomfortable and more comfortable to wear.
[0005] The laminate disclosed in Patent Document 1 is designed to provide comfort by imparting moisture permeability, but this is not sufficient, and the garment is prone to becoming stuffy when worn in the summer. In addition, since a woven fabric is used as the outer fiber fabric, the laminate has poor stretchability and is also poor in comfort. In addition, the laminate disclosed in Patent Document 2 has excellent stretchability because a tricot knit is used on both sides of the film, but is not lightweight because the tricot knit is made of polyester filaments. In addition, the moisture permeability of the film was not taken into consideration, so the laminate is prone to becoming stuffy when worn in summer, and is uncomfortable to wear. In addition, the blood barrier laminate disclosed in Patent Document 3 uses a PTFE film as the microporous film, and therefore has poor stretchability and light weight. Therefore, when worn in summer, the laminate is prone to becoming stuffy, and is poor in ease of movement and comfort. To prevent stuffiness when worn in summer and to improve comfort, it is necessary to give the constituent fabric sufficient stretchability and light weight, but no infection prevention clothing has yet been proposed that satisfies all of the performance requirements of sufficient stretchability, light weight, and moisture permeability and waterproofness.
[0006] Furthermore, due to recent social circumstances, there is a strong demand for infection prevention clothing to be resistant to chemicals, and in particular, to ethanol preparations (alcohol) used for sterilization and disinfection. Summary of the Invention [Problem to be solved by the invention]
[0007] Therefore, the object of the present invention is to provide a laminate for clothing that is a suitable material for reusable infection prevention clothing, and that not only has excellent waterproof properties as a virus barrier and blood barrier required for infection prevention clothing, but also has moisture permeability that does not easily cause stuffiness when worn in summer, is lighter than conventional products, and has sufficient stretchability.Furthermore, the present invention is to provide infection prevention clothing that uses the laminate, which has excellent waterproof properties as a barrier against blood and viruses, excellent durability against alcohol, reduces the feeling of stuffiness when worn, is lightweight and has sufficient stretchability to make it easy to move around when moving, and is excellent in wearing comfort. [Means for solving the problem]
[0008] The present inventors conducted extensive research to solve the above problems and arrived at the present invention. That is, the present invention relates to the following (i) to (f). (A) A laminated knitted fabric comprising a front knitted fabric, a microporous membrane, and a back knitted fabric laminated in this order, the front knitted fabric and the back knitted fabric being mainly composed of polyamide fibers, and the microporous membrane being mainly composed of polyurethane resin; Weight is 100g / m 2 or less, and the moisture permeability measured by JIS L 1099 A-1 method (calcium chloride method) is 8000g / m 2 / 24h or more for clothing laminates. (ii) The clothing laminate according to (i), wherein the outer knitted fabric and the lining knitted fabric are tricot knitted fabrics. (C) The laminate for clothing according to (A), having a longitudinal elongation percentage of 5 to 15% and a transverse elongation percentage of 10 to 30%, as measured according to JIS L 1096 B method. (D) The clothing laminate according to (A), which has a water pressure resistance of 100 kPa or more when measured according to JIS L 1092 (2009) Method B (high water pressure method) after being immersed in an 80% aqueous ethanol solution for 25 hours and dried. (E) The laminate for clothing according to (A), having adhesive layers mainly composed of a polycarbonate-based polyurethane resin between the outer knitted fabric and the microporous membrane, and between the microporous membrane and the lining knitted fabric. (f) Infection-preventing clothing using the clothing laminate described in (a). Effect of the Invention
[0009] The clothing laminate of the present invention has excellent waterproofing properties such as virus barrier properties and blood barrier properties, moisture permeability that does not easily cause stuffiness when worn in summer, and is also lightweight and has excellent stretchability. Furthermore, these properties are also durable against alcohol used as a disinfectant, making it a particularly suitable material for reusable infection prevention clothing. Furthermore, infection-preventive clothing obtained by using the clothing laminate of the present invention is less likely to become stuffy even when worn in the summer, and is excellent in terms of comfort and ease of use. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described in detail below.
[0011] The laminate for clothing of the present invention is a laminate comprising a knitted outer fabric, a microporous membrane mainly composed of a polyurethane resin, and a knitted inner fabric laminated in this order. In the present invention, the laminate for clothing may be referred to as the "laminate of the present invention."
[0012] The present inventors have considered that it is important to use knitted fabrics mainly composed of polyamide fibers on both sides of the front and back layers of the clothing laminate in order to obtain a clothing laminate having sufficient lightness and stretchability in addition to moisture permeability and waterproofness. That is, as will be described later, by using polyamide-based fibers with a low polymer specific gravity, the basis weight is within a specific range and the clothing laminate has excellent lightness, and by forming both sides of the front and back layers from a specific knitted fabric, the clothing laminate can also have excellent stretchability. Therefore, by using the laminate of the present invention to make infection prevention clothing, for example, medical personnel can move easily and reduce heat when wearing it to perform emergency activities. In addition, the clothing can be made to be comfortable to wear, such as being easy to put on and take off. In order to make the laminate of the present invention excellent in moisture permeability, waterproofness, light weight and stretchability, it is important that the outer knitted fabric and the lining knitted fabric, which are mainly composed of polyamide fibers, have the configuration described specifically below.
[0013] The knitted fabric for outer layer and the knitted fabric for inner layer in the present invention will be described below. [Outer fabric / Lining fabric] In the present invention, the outer knitted fabric and the inner knitted fabric are mainly composed of polyamide fibers. As the polyamide-based fibers, homopolymers such as nylon 6, nylon 66, nylon 11, nylon 12, nylon 56, nylon MXD (polymetaxylylene adipamide), and copolymers or mixtures mainly composed of these are preferably used. Among them, fibers made of nylon 6 are preferable. Compared with polyester-based polymers, polyamide-based polymers have a specific gravity that is about 20% lighter as a polymer characteristic, and are suitable from the viewpoint of light weight, which is one of the appealing points of the present invention. Therefore, in the present invention, polyamide-based fibers are used as the fibers constituting the outer knitted fabric and the inner knitted fabric.
[0014] As long as the effects of light weight and moisture permeability and waterproofness are not impaired, the knitted fabric may contain fibers other than polyamide fibers, for example, synthetic fibers such as polyester fibers typified by polyethylene terephthalate, polyacrylonitrile fibers, and polyvinyl alcohol fibers, semi-synthetic fibers such as triacetate, and cellulosic fibers such as cotton, hemp, rayon, polynosic, cupra, lyocell, and acetate. Furthermore, the outer knitted fabric and the lining knitted fabric may contain fibers such as conductive threads as necessary. However, the polyamide fiber content of the fibers constituting the outer knitted fabric and the lining knitted fabric is preferably 90% by mass or more, and particularly preferably 100% by mass.
[0015] The polyamide fiber may be any of long fiber, short fiber, and staple yarn, and may be any of multifilament and monofilament. As the filament, flat yarn (raw silk), false twisted yarn, air entangled yarn, and other yarn-processed yarns may be used. From the viewpoint of making the laminate of the present invention thin and providing excellent surface smoothness, it is preferable to use raw silk, and from the viewpoint of further improving the stretchability of the laminate of the present invention, it is more preferable to use false twisted yarn.
[0016] The single yarn fineness of the polyamide fiber is preferably 0.7 to 10 dtex, more preferably 1.0 to 6 dtex. If the single yarn fineness is less than 0.7 dtex, the single yarn fineness may be too thin, resulting in a decrease in moisture permeability. On the other hand, if the single yarn fineness exceeds 10 dtex, the single yarn fineness may be too thick, resulting in a coarse knitted fabric, resulting in a decrease in the feel to the touch, or the microporous membrane may be exposed from the knitted fabric surface, resulting in a decrease in the durability of the laminate.
[0017] The total fineness of the polyamide fiber is preferably 10 to 80 dtex, more preferably 20 to 60 dtex. If the total fineness is less than 10 dtex, the adhesiveness between the outer or inner lining knitted fabric and the microporous membrane may decrease, or the resin used as an adhesive during lamination may leak from the surface of the knitted fabric, while if it exceeds 80 dtex, the knitted fabric becomes heavy and less lightweight.
[0018] The knitted fabrics used for the outer fabric and the inner fabric may have the same structure and characteristic values as those described below, or may be different.
[0019] The knitting density of the outer knitted fabric is preferably 40-150 courses / 2.54 cm and 25-100 wales / 2.54 cm, and more preferably 45-150 courses / 2.54 cm and 28-100 wales / 2.54 cm. On the other hand, the knitting density of the lining knitted fabric is preferably 40-100 courses / 2.54 cm and 25-80 wales / 2.54 cm, and more preferably 45-150 courses / 2.54 cm and 28-100 wales / 2.54 cm. If the course density and wale density are below the above ranges, the knitted fabric will have coarse weaving points and will tend to have more voids in the knitted fabric, which will result in the microporous membrane being exposed to the knitted fabric surface through the voids, and the waterproofing that acts as a barrier against blood and viruses will be easily reduced. On the other hand, if the course density and wale density exceed the above ranges, the constraint by the weaving points will be strengthened, and the tear strength and burst strength of the knitted fabric will decrease, the weight of the knitted fabric will increase, making it less lightweight, and the moisture permeability of the laminate will tend to decrease.
[0020] The weight of the outer and lining fabrics is 20 to 80 g / m 2 It is preferable that the thickness is 20 to 50 g / m 2 It is more preferable that the weight of the outer knit fabric and the lining knit fabric is 20 g / m 2 By setting the thickness to 80 g / m or more, the laminate of the present invention is not too thin and has excellent tensile strength, burst strength, and water pressure resistance. 2 By setting the above, when the laminate of the present invention is used for infection preventive clothing or the like, the infection preventive clothing becomes lighter and more comfortable to wear. In the present invention, the total weight of the outer knit fabric and the lining knit fabric is 40 to 95 g / m 2 It is preferable that the thickness is 40 to 90 g / m 2 More preferably, 45 to 90 g / m 2 When the total weight of the outer knitted fabric and the lining knitted fabric falls within the above range, the laminate of the present invention has a sufficiently light weight, and when used as infection prevention clothing, it allows ease of movement and reduces heat.
[0021] The knitted fabric in the present invention may be either a warp knitted fabric or a weft knitted fabric. Examples of warp knitted fabrics include denby knitted fabrics, cord knitted fabrics, and atlas knitted fabrics, and examples of weft knitted fabrics include flat knitted fabrics, rib knitted fabrics, pearl knitted fabrics, and smooth knitted fabrics. In particular, tricot knitted fabrics are preferred because they have less stretchability than knitted fabrics having other structures and do not have too large stitch gaps. In addition, tricot knitted fabrics are preferred in that they can provide a long green fabric in the knitted fabric length direction during knitting and can reduce seams, allowing the knitted fabric to be uniformly laminated on the microporous membrane when forming the laminate of the present invention. Among these, half tricot knitted fabrics are preferred from the viewpoints of light weight, durability, and shape stability.
[0022] [Microporous membrane] Next, the microporous membrane of the present invention will be described.
[0023] In the present invention, in order to impart excellent stretchability, the microporous membrane is mainly composed of a polyurethane resin. Among them, a polycarbonate-based polyurethane resin is preferably used because it has excellent heat resistance, hydrolysis resistance, and the like and is durable against washing. The microporous membrane may be a planar material having micropores, such as a wet-coagulated membrane, a dry membrane, or a foam, but in the present invention, a dry polyurethane membrane in the form of a film is preferably used from the viewpoints of waterproofness and durability, and the dry polyurethane membrane in the form of a film is preferably laminated with the outer knitted fabric and the inner knitted fabric by a lamination method described later.
[0024] As the polyurethane resin, a conventionally known one obtained by reacting a polyisocyanate component with a polyol component can be used. As the polyisocyanate component, aromatic diisocyanates, aliphatic diisocyanates, alicyclic diisocyanates, etc. are used alone or in mixture. Specifically, tolylene-2,4-diisocyanate, 4,4'-diphenylmethane diisocyanate, 1,6-hexane diisocyanate, 1,4-cyclohexane diisocyanate, etc. are used as the main component, and trifunctional or higher polyisocyanates may be used as necessary. On the other hand, as the polyol component, polyether polyols, polyester polyols, etc. are used. As the polyether polyols, polyethylene glycol, polypropylene glycol, polytetraethylene glycol, etc. are used. As the polyester polyols, reaction products of diols such as ethylene glycol or propylene glycol with dibasic acids such as adipic acid or sebacic acid, or ring-opening polymers such as caprolactone can be used, and polymers of oxyacid monomers or prepolymers thereof can also be used. In order to obtain a high level of moisture permeability from the polyurethane resin alone, it is preferable to use, as the polyol component, one having a relatively large amount of polyoxyethylene groups, such as polyethylene glycol or a polyoxypropylene polyoxyethylene copolymer.
[0025] The microporous membrane of the present invention preferably has only micropores with a pore size of 1 μm or less. If the pore size is 1 μm or less, it is possible to suppress the penetration of blood and the like from the surface of the laminate of the present invention, thereby making it possible to improve the barrier properties against viruses and bacteria transmitted by blood.
[0026] Since the laminate of the present invention is expected to be repeatedly washed and disinfected, it is preferable that the microporous membrane contain a fluorine-based water repellent and an oil-soluble fluorine-based surfactant to prevent a decrease in water pressure resistance due to detergent or the like remaining in the microporous membrane.
[0027] The fluorine-based water repellent to be contained may be a conventionally known one, but it is preferable to use one obtained by polymerizing an acrylate compound having a perfluoroalkyl group with 1 to 6 carbon atoms in the side chain. Specific examples include "Asahiguard AG-E061" manufactured by Asahi Glass Co., Ltd., "Unidyne TG-5521" manufactured by Daikin Industries, Ltd., "NK Guard SCH-02" manufactured by Nicca Chemical Co., Ltd., and "NUVA N2114 LIQ" manufactured by Clariant Japan Co., Ltd.
[0028] The fluorine-based water repellent is preferably contained in an amount of 1 to 9 mass % based on the solid content of the polyurethane resin (composition) forming the microporous membrane. When the content of the fluorine-based water repellent is within the above range, a uniform microporous membrane is easily formed, and detergent is less likely to be adsorbed on the microporous membrane even after repeated washing, thereby improving the washing durability of water pressure resistance.
[0029] As the fluorosurfactant contained in the polyurethane resin (composition) forming the microporous membrane, it is preferable to use an oil-soluble one, and it is preferable to use one having a hydrophobic group consisting of a perfluoroalkyl group and a hydrophilic group such as a polyoxyalkylene group, a sulfonic acid group, or a carboxylic acid group, and having surface activity. Here, oil-soluble means that it is soluble or compatible with toluene at 50% by mass or more. That is, when 50 parts by mass of the fluorosurfactant are mixed and stirred with 100 parts by mass of toluene, phase separation does not occur even after 1 hour has passed. In the present invention, by using an oil-soluble fluorosurfactant, the fluorowater repellent can be uniformly present in the microporous membrane. As the oil-soluble fluorosurfactant, "SURFLON S-651", "SURFLON S-611", "SURFLON S-386" and "SURFLON S-243" manufactured by AGC Seimi Chemical Co., Ltd. are used.
[0030] The fluorosurfactant is preferably contained in an amount of 0.1 to 2 mass % based on the solid content of the polyurethane resin (composition) forming the microporous membrane. When the content of the fluorosurfactant is within the above range, the coatability of the polyurethane resin forming the microporous membrane can be improved, and the water pressure resistance and washing durability of the water pressure resistance can be improved.
[0031] The ratio of fluorine-based water repellent to fluorine-based surfactant used is preferably about 3 / 1 to 30 / 1 parts by mass, more preferably 5 / 1 to 20 / 1 parts by mass, in terms of solid content ratio. When the ratio is within the above range, the coatability of the polyurethane resin forming the microporous membrane can be improved, and the water pressure resistance and washing durability of the water pressure resistance can be improved.
[0032] In the present invention, in order to obtain a microporous film having further excellent moisture permeability and waterproofing performance, it is preferable to blend silica fine powder together with a fluorine-based water repellent and a fluorine-based surfactant in the polyurethane resin (composition) forming the microporous film. As the silica fine powder, any conventionally known silicon dioxide fine powder can be used. In general, a fine powder made of silicon dioxide having a primary particle diameter of about 7 to 40 nm is used. If the primary particle diameter is within the above range, the diameter of the micropores in the microporous film does not become too large, and the decrease in the water pressure resistance of the laminate can be suppressed. In the present invention, it is preferable to use fumed silica fine powder having a particle diameter of 7 to 40 nm, which is made of amorphous glass-like spherical primary particles without pores. Specifically, hydrophilic fumed silica fine powder or hydrophobic fumed silica fine powder is used, and in the present invention, it is particularly preferable to use hydrophobic fumed silica fine powder. Such silica fine powders are commercially available, and examples of such fine powders include hydrophilic fumed silica fine powders such as "AEROSIL 90", "AEROSIL 130", "AEROSIL 200" and "AEROSIL 300" manufactured by Nippon Aerosil Co., Ltd., and hydrophobic fumed silica fine powders such as "AEROSIL NX90G", "AEROSIL RX200", "AEROSIL RX300", "AEROSIL R972", "AEROSIL R974" and "AEROSIL R976". In addition, "AEROSIL COK84", a fine powder made by mixing fumed silica and fumed aluminum oxide, can also be used.
[0033] The content of the silica fine powder may be about 3 to 45% by mass, preferably 15 to 45% by mass, and particularly preferably 20 to 40% by mass, in the solid content of the polyurethane resin (composition) forming the microporous film. In particular, if the content of the silica fine powder is in the range of 15 to 45% by mass, a large number of nano-order pores with a pore size of 1 μm or less can be formed in the microporous film, and the formation of long holes specific to polyurethane can be suppressed. As a result, it is possible to make the laminate of the present invention have significantly improved moisture permeability and waterproof performance. The silica fine powder is preferably contained in a state of being uniformly dispersed in the polyurethane resin (composition), and in order to uniformly disperse it, it is sufficient to mix it with the polyurethane resin in advance using a mixer such as a three-roll mill, a kneader, or a sand mill to prepare it.
[0034] The polyurethane resin (composition) forming the microporous membrane preferably further contains a crosslinkable isocyanate compound. By containing the crosslinkable isocyanate compound, the polyurethane resin is crosslinked, and the strength of the microporous membrane and the adhesive strength between the microporous membrane and the knitted fabric for the outer material and / or the knitted fabric for the inner material can be improved. The crosslinkable isocyanate compound is preferably contained in an amount of about 1 to 10% by mass in the solid content of the polyurethane resin (composition).
[0035] Examples of the crosslinkable isocyanate compound include tolylene 2,4-diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, and hexamethylene diisocyanate. In addition, triisocyanates obtained by an addition reaction between 3 moles of these diisocyanates and 1 mole of a compound containing active hydrogen can also be used. Examples of the compound containing active hydrogen include trimethylolpropane and glycerin. Among the crosslinkable isocyanate compounds, the use of blocked isocyanates is particularly advantageous in terms of the stability and pot life of the polyurethane resin (composition). As the blocked isocyanate, a type that dissociates by heat treatment is preferable, and specifically, an addition block formed with phenol, lactam, methyl ketoxime, or the like is preferable.
[0036] In the present invention, the microporous membrane may contain a small amount of resin other than polyurethane resin, for example, about 20 mass% or less in the solid content, as long as the effect of moisture permeability and waterproofing is not impaired. For example, polymers or copolymers such as polyacrylic acid, polyvinyl chloride, polystyrene, polybutadiene, polyamino acids, and polycarbonate are used as such resins. These polymers or copolymers may also be modified with fluorine, silicon, or the like. In addition, various additives such as pigments and fillers, and various functional materials such as antibacterial agents, deodorants, and flame retardants may be contained as a third component.
[0037] As a solvent for the polyurethane resin (composition) forming the microporous membrane, it is preferable to mainly use N,N-dimethylformamide, which is a compatible solvent for polyurethane resin, and the solid content of the polyurethane resin (composition) is preferably about 15 to 35 mass %. If it is less than 15 mass %, a large amount of solution is required for a release cloth having a large fineness of 200 dtex or more and strong unevenness, and it becomes difficult to completely cover the surface of the release cloth, and if it exceeds 35 mass %, it is not preferable because there are problems such as a decrease in leveling properties, making it difficult to control the coating thickness when obtaining a microporous membrane.
[0038] The polyurethane resin (composition) is applied to the release surface of the release agent by a known means such as a comma coater or a knife coater, and then immersed in a wet coagulation liquid to form a microporous film. As the wet coagulation bath, an aqueous solution containing 30% by mass or less of N,N-dimethylformamide is used. The temperature of the coagulation liquid is preferably about 5 to 35°C, and the coagulation time is about 30 seconds to 5 minutes. After the polyurethane resin (composition) is coagulated in the wet coagulation liquid to obtain a microporous film, the film is washed with hot water at a temperature of 35 to 80°C for 1 to 10 minutes to remove the N,N-dimethylformamide. After washing with hot water, the film is dried at a temperature of 50 to 150°C for 1 to 10 minutes to form a microporous film on one side of the release agent. The release agent is then peeled off to obtain a microporous film to be used in the laminate of the present invention.
[0039] The thickness of the microporous membrane is preferably in the range of 5 to 45 μm, more preferably 15 to 35 μm. If the thickness is less than 5 μm, the waterproof performance tends to decrease, while if it exceeds 45 μm, the weight of the laminate becomes heavy, resulting in poor lightness and poor moisture permeability, both of which are undesirable.
[0040] In the laminate of the present invention, the outer knitted fabric and the inner knitted fabric may be laminated directly to the microporous membrane or may be laminated via an adhesive layer. In particular, when the lamination method described below is used, it is preferable to provide an adhesive layer on the knitted fabric, that is, to laminate the knitted fabric and the microporous membrane via an adhesive layer.
[0041] In the laminate of the present invention, when the knitted fabric and the microporous membrane are laminated via an adhesive layer, a coating method in which a resin solution serving as an adhesive is directly applied to the knitted fabric, and a lamination method in which the microporous membrane is pressed or heated to be bonded to the knitted fabric can be mentioned. In the present invention, from the viewpoint of improving the waterproofness and durability of the polyurethane resin and the peel strength between the knitted fabric and the microporous membrane, it is preferable to laminate the microporous membrane to the knitted fabric by a lamination method. As a lamination method, it is preferable to laminate the microporous membrane on the knitted fabric by dry lamination in which an adhesive layer described below is provided by applying and drying on the knitted fabric, and then a microporous membrane made of a polyurethane resin previously formed into a film shape is laminated on the adhesive layer while pressing it with a heated roll, from the viewpoint of improving the peel strength between the knitted fabric and the microporous membrane and providing excellent moisture permeability.
[0042] In addition, lamination should be performed while minimizing tension on the knitted fabric and the microporous membrane, since excessive tension causes distortion in the knitted fabric and the microporous membrane, making the laminate of the present invention prone to subsequent shrinkage in washing.
[0043] The type of adhesive used in the adhesive layer is not particularly limited, and examples include polyurethane resin, polyester resin, polyamide resin, polytetrafluoroethylene resin, polyethylene resin, polypropylene resin, polyacrylic resin, polyvinyl chloride resin, ethylene-vinyl alcohol copolymer resin, etc. Among these, it is preferable to use an adhesive that has excellent compatibility with the microporous membrane, and therefore it is preferable to employ an adhesive layer made of a polyurethane-based adhesive, like the polyurethane resin that constitutes the microporous membrane.
[0044] The adhesive layer may be formed over the entire surface of the microporous membrane, or may be formed in a pattern from the viewpoint of moisture permeability, texture, etc. of the laminate for clothing. The shape of the pattern is not particularly limited, but examples include dots, lines, a lattice, a checkered pattern, and a tortoiseshell pattern, and it is basically preferable that the adhesive layer be uniformly arranged over the entire surface.
[0045] The area of the adhesive layer relative to the microporous membrane or knitted fabric is preferably about 25 to 90%, more preferably 40 to 70%, of the total area. If the coating area of the adhesive layer is significantly small, peel resistance tends to decrease and moisture permeability tends to increase, whereas if the coating area of the adhesive layer is significantly large, peel resistance tends to increase and moisture permeability tends to decrease, so it is preferable to keep it within the above range in order to balance the two.
[0046] The thickness of the adhesive layer is generally preferably 5 to 100 μm, more preferably 10 to 70 μm, and particularly preferably 20 to 50 μm. If the thickness is less than 5 μm, it is difficult to obtain a durable laminate even if the area occupied by the adhesive is increased, while if it exceeds 100 μm, the manufacturing cost increases and the moisture permeability decreases or the texture becomes hard, both of which are undesirable.
[0047] [Characteristics of laminates for clothing] Next, the characteristics of the laminate for clothing of the present invention will be described.
[0048] From the viewpoint of light weight, the laminate of the present invention is preferably as thin as possible.2 It is necessary that the thickness is less than 90 g / m2, especially when used for infection prevention clothing. 2 Preferably, it is 85 g / m or less. 2 It is more preferable that the basis weight is 100 g / m or less. 2 If the basis weight is larger than 40 g / m, when the laminate of the present invention is used in infection preventive clothing, the infection preventive clothing will not be sufficiently lightweight, and the wearer will feel fatigued and will have a poor wearing comfort. On the other hand, if the basis weight is too small, the tensile strength, burst strength, and water pressure resistance will be easily reduced, so the basis weight should be 40 g / m 2 More preferably, it is equal to or greater than this.
[0049] The laminate of the present invention has a moisture permeability of 8000 / m as measured according to JIS L 1099 A-1 method (calcium chloride method). 2 / 24h or more, and among them, 8000~12000g / m 2 / 24h. The laminate of the present invention preferably has a moisture permeability of 15,000 to 50,000 g / m2 as measured according to JIS L 1099 B-1 method (potassium acetate method). 2 / 24h is preferable, and 20000 to 40000g / m 2 / 24h is more preferable. Regardless of the measurement method, if the moisture permeability range is below the above range, the moisture permeability is insufficient, so that the microporous membrane surface is prone to condensation, and when the laminate of the present invention is used as infection prevention clothing, etc., a stuffy feeling occurs, reducing wearing comfort. On the other hand, if the moisture permeability range is above the above range, there is a risk that the desired waterproofness related to the barrier properties against blood and viruses cannot be obtained.
[0050] As characteristic values showing that the laminate of the present invention has excellent stretchability, the longitudinal elongation rate measured according to JIS L 1096 B method is preferably 5 to 20% and the transverse elongation rate is preferably 10 to 35%. The longitudinal elongation rate is preferably 8 to 15%, and the transverse elongation rate is preferably 15 to 25%. When the longitudinal and transverse elongation rates of the laminate of the present invention satisfy the above ranges, when the laminate is used to make infection prevention clothing, the laminate can be sufficiently stretched in accordance with the movement of the wearer's body, making it easier to move and providing excellent wearing comfort. When the longitudinal elongation rate of the laminate is 20% or less and the transverse elongation rate is 35% or less, even if a force is applied to the laminate during the movement of the wearer of the infection prevention clothing, causing the microporous membrane to stretch, the pores of the microporous membrane can be suppressed from being excessively enlarged, and blood and viruses can be prevented from penetrating the microporous membrane.
[0051] Furthermore, as a characteristic value showing that the laminate of the present invention has excellent stretchability, the elongation recovery rate in the longitudinal direction and the transverse direction after one hour of unloading measured according to JIS L 1096 B-1 method is 70% or more, and from the viewpoint of wearing comfort, it is preferably 80% or more. If the elongation recovery rate is 70% or more, it can be said that the laminate has sufficient stretchability for practical use. Details of the measurement method will be described later.
[0052] As an index of durability against alcohol, the laminate of the present invention has a water pressure resistance of 100 kPa or more, preferably 120 kPa or more, measured according to JIS L 1092 (2009) B method (high water pressure method) after immersion in an 80% ethanol aqueous solution for 25 hours and drying. If the water pressure resistance after immersion in an ethanol aqueous solution is within the above range, the laminate of the present invention exhibits excellent durability against alcohol. Therefore, when the laminate of the present invention is used as infection prevention clothing, etc., even if the surface of the clothing is wiped multiple times with alcohol for the purpose of sterilization, etc., it can maintain excellent barrier properties against blood and viruses. The reason why the laminate of the present invention has excellent durability against alcohol is unclear, but it is presumed to be due to the characteristics of the polyurethane resin used as the microporous membrane.
[0053] The laminate of the present invention has an initial water pressure resistance of 100 kPa or more, preferably 120 kPa or more, as an index of waterproofness, measured by JIS L 1092 (2009) B method (high water pressure method). By setting the initial water pressure resistance within the above range, the laminate of the present invention exhibits excellent waterproofness and has excellent barrier properties against blood and viruses. In addition, since an appropriate number of through holes can be provided in the microporous membrane, the laminate can also have excellent moisture permeability. In the present invention, the initial water pressure resistance means the water pressure resistance before immersion in the above 80% ethanol aqueous solution for 25 hours.
[0054] The blood barrier property of the laminate of the present invention preferably passes the test described in the ASTM F1670-08B method. If the laminate passes the test, the laminate has sufficient blood barrier property for practical use and can be evaluated as preferable.
[0055] The virus barrier property of the laminate of the present invention preferably passes the test described in the ASTM F1671-07B method. If the laminate passes the test, it has sufficient virus barrier property for practical use and can be evaluated as preferable.
[0056] [Method of manufacturing laminate for clothing] Next, a method for producing the laminate for clothing of the present invention will be described by taking as an example a method for producing a laminate in which a lamination method is used to form a microporous membrane on one surface of a knitted fabric.
[0057] In the lamination method, first, a resin composition for forming a microporous membrane (for example, a resin composition containing a resin that forms a microporous membrane and an organic solvent) is applied to the surface of a release material (such as release paper, release cloth, or release film) with a clearance provided, a microporous membrane is formed while adjusting the thickness, and then heat-treated to completely react to obtain a film. The release material can be appropriately removed after lamination or aging.
[0058] Next, an adhesive layer is formed on the knitted fabric for the outer material or the microporous membrane. The adhesive layer can be formed by a method using a resin solution or a hot melt method. For example, in the method using a resin solution, a two-component curing polyurethane resin solution with a viscosity of 500 to 5000 mPa·s is applied to the entire surface or in a pattern. The adhesive layer is then formed by drying, and the knitted fabric and the microporous membrane are bonded together via the adhesive layer, and the two are pressure-bonded or heat-pressed to obtain a laminate of the knitted fabric for the outer material and the microporous membrane.
[0059] On the other hand, in the case of hot melt, it is preferable to use a moisture-curing resin that reacts with moisture in the air, and it is more preferable for practical use to use one that melts at a temperature range of about 80 to 150°C. In this case, the hot melt resin is first melted while taking into consideration the melting point of the resin and the viscosity when melted. Then, the molten resin is applied onto the knitted fabric or the microporous membrane and matured while cooling at room temperature to form an adhesive layer. Then, the knitted fabric and the microporous membrane are bonded together via the adhesive layer and pressed to obtain a laminate of the outer knitted fabric and the microporous membrane.
[0060] Thereafter, the lining knitted fabric can be laminated to the microporous membrane using a technique similar to that used for the outer knitted fabric.
[0061] As described above, the clothing laminate of the present invention has a microporous membrane and a lining knitted fabric laminated in this order on top of the outer knitted fabric. That is, in the present invention, the microporous membrane is sandwiched between the knitted fabrics. The reason for using two knitted fabrics, one for the outer knitted fabric and the other for the lining, in the laminate of the present invention is to protect the microporous membrane, since when one side of the microporous membrane is exposed, the exposed microporous membrane is likely to deteriorate due to friction such as peeling when it comes into contact with an object, and to prevent discomfort due to direct contact between the microporous membrane and the skin surface or insufficient moisture permeability, which may occur when the laminate of the present invention is worn as clothing.
[0062] The clothing laminate of the present invention is also suitable for clothing used in medical applications, and can provide clothing that has excellent waterproof properties that provide a barrier against blood and viruses, reduces stuffiness when worn, and has sufficient stretchability to facilitate movement during movement, resulting in excellent comfort when worn. Note that the medical applications referred to in the present invention are not limited to the medical field targeting hospitals, but also include the surrounding fields of care, nursing, and pharmaceuticals. EXAMPLES
[0063] The present invention will now be described in more detail with reference to examples. The methods for measuring and evaluating various property values are as follows.
[0064] (a) Elongation rate The obtained clothing laminate was cut into a size of 60 mm x 300 mm and used as a test piece to measure the elongation percentage according to the method specified in JIS L1096 (2010) 8.16.1, Method B. The elongation percentage was determined in both the warp and weft directions when the specimen was elongated to a tensile load of 14.7 N under conditions of a gripping distance of 200 mm and a pulling speed of 20 cm / min. (b) Elongation recovery rate The obtained clothing laminate was cut into 60 mm x 300 mm pieces and used as test pieces to measure the elongation recovery rate according to the method specified in the B-1 method (constant load method) described in 8.16.2 of JIS L1096 (2010). The test piece was fixed to the upper clamp and an initial load was applied, and then the lower clamp was fixed. Marks were then made at intervals of 200 mm (L0), a load of 14.7 N was applied, and after leaving it for 1 hour, the length between the marks (L1) was measured. The weight was then removed, and after 1 hour, the initial load was applied, and the length between the marks (L2) was measured again, and the elongation recovery rate was calculated using the following formula. Elongation recovery rate (%)=[(L1-L2) / (L1-L0)]×100 (c) Moisture permeability The obtained laminate for clothing was used as a test piece to measure the moisture permeability according to the methods specified in JIS L1099 A-1 method (calcium chloride method) and B-1 method (potassium acetate method), and the moisture permeability was evaluated. (d)Waterproof The obtained clothing laminate was used as a test piece to measure water pressure resistance according to the method specified in JIS L 1092 (2009) Method B (high water pressure method), and waterproofness was evaluated. (e) Alcohol resistance The obtained clothing laminate was used as a test piece, which was immersed in an 80% aqueous ethanol solution for 25 hours and dried. The water pressure resistance was then measured according to the method specified in JIS L 1092 (2009) Method B (high water pressure method) to evaluate the waterproofness. (f) Blood barrier properties The blood barrier properties of the obtained clothing laminate were evaluated by pass / fail judgment according to the method specified in ASTM F1670-08B. (g) Virus Barrier Property The virus barrier properties of the obtained clothing laminate were evaluated by pass / fail evaluation according to the method specified in ASTM F1671-07B. (h) Observation of the thickness and cross-sectional shape of the microporous membrane Using a Hitachi S-4000 field emission scanning electron microscope, a cross-sectional photograph was taken at a magnification of 2000 times to measure the thickness of the microporous membrane and to observe the cross-sectional shape. (i) Wearing comfort The clothing laminate was used to create infection prevention clothing consisting of a long-sleeved top and pants, which were then worn by medical workers. The clothing was then evaluated in terms of comfort (not feeling stuffy) and ease of movement while performing the same tasks as normal medical work for a day in a midsummer environment (temperature above 30°C), and the following two-level rating was used: ○: Both comfort and ease of operation are good. ×: Both comfort and ease of operation are poor.
[0065] Example 1 [Preparation of outer knit fabric] Using a 28 gauge tricot knitting machine, nylon 6 multifilament raw silk 22 dtex / 7f was used to knit a half tricot fabric with a knitting structure of front reed: 1-2 / 1-0, back reed: 1-0 / 2-3. The obtained grey fabric was dyed under known conditions to obtain a knitted fabric having a knit density of 46 courses / 2.54 cm×30 wales / 2.54 cm.
[0066] [Preparation of lining fabric] The knit fabric used was the same as the outer knit fabric described above, but had a knit density of 46 courses / 2.54 cm×30 wale / 2.54 cm.
[0067] [Preparation of resin composition for forming microporous membrane] 30 parts by mass of an ester-type polyurethane resin solution using N,N-dimethylformamide as a solvent ("Luxkin UJ8517" manufactured by Seiko Chemical Co., Ltd., solid content 25% by mass), 10 parts by mass of fumed silica fine powder ("AEROSIL R974" manufactured by Nippon Aerosil Co., Ltd., average primary particle diameter 12 nm), and 10 parts by mass of N,N-dimethylformamide were mixed and roughly kneaded, and then uniformly kneaded using a three-roll mill to prepare 50 parts by mass of resin solution A. Next, 0.1 parts by mass of an oil-soluble and water-soluble fluorosurfactant ("SURFLON S-386" manufactured by AGC Seimi Chemical Co., Ltd.) was dissolved in 35 parts by mass of N,N-dimethylformamide, and then 5 parts by mass of a fluororesin water repellent emulsion ("NUVA N2114 LIQ" manufactured by Clariant Japan Co., Ltd.) was mixed and dispersed to prepare 40.1 parts by mass of resin solution B. Next, the ingredients were mixed in the following <Formulation 1>, and then stirred with a Disper-type stirrer while vacuum degassing to prepare a polyurethane resin composition for forming a microporous membrane. This polyurethane resin composition had a solid content of 23 mass%, a viscosity of 10,000 mPa s / 25°C, and a fluorine-based water repellent content of 5 mass%, an oil-soluble and water-soluble fluorine-based surfactant content of 0.3 mass%, and a silica fine powder content of 30 mass%. <Prescription 1> Ester-type polyurethane resin solution 50 parts by weight (Seiko Chemicals Corporation's "Luckskin UJ8517", solid content 25% by mass) Resin solution A 50 parts by mass Resin solution B 40.1 parts by mass Isocyanate compound 1.5 parts by mass ("Rezamin X Crosslinking Agent" manufactured by Dainichi Seika Color & Chemicals Co., Ltd.)
[0068] [Production of microporous membranes] Next, the calendar side of the release cloth is used as the coating surface, and a comma coater is used to apply 100 g / m 2 After applying the polyurethane resin composition of <Formulation 1>, the polyurethane resin composition was coagulated by immersing it in a coagulation bath of a 15% by mass aqueous solution of N,N-dimethylformamide (20°C) for 2 minutes, and then washed with hot water at 50°C for 5 minutes. After that, the water was removed by squeezing it with a mangle, and then it was dried at 130°C for 2 minutes to form a microporous film on the surface of the release cloth. Then, it was set at 170°C for 1 minute, and after it became normal, the release cloth was peeled off to obtain a microporous film.
[0069] The average thickness of the obtained microporous membrane was 30 μm and the basis weight was 25 g / m 2 A large number of micropores with a diameter of 1 μm or less were formed throughout the film.
[0070] Next, the outer knitted fabric and the microporous membrane were attached to each other. A moisture-curing polyurethane hot melt adhesive (Takemelt MA3229, manufactured by Mitsui Takeda Chemical Co., Ltd.) melted at 120°C was applied to the above-mentioned outer knitted fabric at a rate of 10 g / m using a gravure roll (20 mesh) engraved with a dot pattern. 2 The above-mentioned moisture-permeable waterproof membrane was then laminated on the coated surface, pressed at a pressure of 300 kPa, and then aged for 3 days in an environment of 40°C x 80% RH to obtain a laminate of "surface knit / adhesive / microporous membrane." A lining knitted fabric was laminated on the microporous membrane surface of this "outer knitted fabric / adhesive / microporous membrane" in the same manner to obtain a clothing laminate of the present invention having a laminated structure of "outer knitted fabric / adhesive / microporous membrane / adhesive / lining knitted fabric."
[0071] Comparative Example 1 [Fabric Production] A ripstop fabric was woven on a water jet loom (WJL) loom using nylon 6 multifilament false twist textured yarns of 22 dtex / 14 f for the warp and weft. The obtained grey fabric was scoured with a scouring agent at 80°C for 20 minutes, and dyed with a disperse dye at 130°C for 30 minutes. Then, it was final set at 170°C for 1 minute to obtain a woven fabric with a warp density of 227 threads / 2.54 cm and a weft density of 167 threads / 2.54 cm. Except for using the obtained woven fabric instead of the outer knitted fabric of Example 1, the same procedures as in Example 1 were carried out to produce a microporous membrane and to laminate the outer woven fabric, lining knitted fabric, and microporous membrane, thereby obtaining a laminate for clothing.
[0072] Comparative Example 2 Instead of the microporous membrane of Example 1, a membrane with a thickness of 35 μm and a basis weight of 37 g / m 2 Except for using the above polytetrafluoroethylene (PTFE) film, the outer knitted fabric, the lining knitted fabric and the PTFE film were laminated in the same manner as in Example 1 to obtain a laminate for clothing.
[0073] Comparative Example 3 [Preparation of outer knit fabric] Using a 28 gauge tricot knitting machine, a half tricot knit fabric with a knitting structure of front reed: 1-0 / 2-3, back reed: 1-2 / 1-0 was knitted using nylon 6 multifilament raw silk of 33 dtex / 6f. The obtained grey fabric was dyed under known conditions to obtain a knitted fabric having a knit density of 50 courses / 2.54 cm×30 wales / 2.54 cm. Except for using the obtained knitted fabric instead of the outer knitted fabric and the inner knitted fabric of Example 1, lamination processing of the outer knitted fabric, the inner knitted fabric and the PTFE film was carried out in the same manner as in Example 1 to obtain a laminate for clothing.
[0074] Table 1 shows the configurations of the outer fabric, inner fabric, and moisture-permeable membrane used in Example 1 and Comparative Examples 1 to 3, and Table 2 shows the property values and evaluation results of the obtained laminates for clothing.
[0075] [Table 1]
[0076] [Table 2]
[0077] As is clear from Table 2, the clothing laminate of Example 1 had excellent blood barrier properties and virus barrier properties, and also had sufficient moisture permeability, stretchability, and light weight. Therefore, it was excellent in ease of movement when worn, and the feeling of stuffiness was reduced. Furthermore, it had excellent durability against alcohol, making it a suitable material for reusable infection prevention clothing.
[0078] On the other hand, in Comparative Example 1, a woven fabric was used as the outer fabric, so the elongation rate of the clothing laminate was too small, the stretchability was poor, and it was difficult to move when worn. In Comparative Example 2, a PTFE film was used instead of a polyurethane microporous membrane, so the clothing laminate did not return to its stretched state when stretched, and was insufficient for use as infection prevention clothing. In Comparative Example 3, the knitted fabric for the outer fabric and the knitted fabric for the lining had a large basis weight, so the weight of the obtained clothing laminate was heavy, and the weight made the wearer feel fatigued when worn, resulting in a poor wearing comfort.
Claims
1. A laminated knitted fabric comprising an outer knitted fabric, a microporous membrane, and a lining knitted fabric laminated in this order, the outer knitted fabric and the lining knitted fabric being mainly made of polyamide fibers, and the microporous membrane being mainly made of polyurethane resin; Weight is 100g / m 2 or less, and the moisture permeability measured by JIS L 1099 A-1 method (calcium chloride method) is 8000 g / m 2 / 24 hours or more.
2. 2. The laminate for clothing according to claim 1, wherein the outer knitted fabric and the inner knitted fabric are tricot knitted fabrics.
3. 2. The laminate for clothing according to claim 1, which has a longitudinal elongation rate of 5 to 15% and a transverse elongation rate of 10 to 30%, as measured by JIS L 1096 B method.
4. The laminate for clothing according to claim 1, which has a water pressure resistance of 100 kPa or more when measured according to JIS L 1092 (2009) Method B (high water pressure method) after being immersed in an 80% aqueous ethanol solution for 25 hours and dried.
5. 2. The laminate for clothing according to claim 1, further comprising an adhesive layer mainly composed of a polycarbonate-based polyurethane resin between the outer knitted fabric and the microporous membrane, and between the microporous membrane and the inner knitted fabric.
6. An infection-preventing garment comprising the clothing laminate according to claim 1.
Citation Information
Patent Citations
Laminated cloth, medical clothing formed of the cloth, and medical material
JP2012076273A
Moisture permeation waterproofness fabric for medical care
JP2014046576A
Blood-barriering laminate cloth having excellent laundry durability
JP2014121858A