Polyvinyl alcohol-based resin composition and molded article using the same
A dual-melting-point PVA resin composition addresses cold crystallization issues by optimizing the extruder temperature profile, enhancing pellet feedability and moldability in low-temperature melt molding processes.
Patent Information
- Application Number
- JP2023058370
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
PVA resins with low melting points exhibit slow crystallization rates and cold crystallization during heating, leading to poor pellet feeding and molding issues in low-temperature melt molding processes.
A polyvinyl alcohol-based resin composition containing two types of PVA resins with different melting points, where the difference is 30 to 70°C, is used to suppress crystallization rates and optimize the extruder temperature profile, improving feedability and moldability.
The composition achieves improved melt moldability with reduced cold crystallization, enabling efficient low-temperature molding and stable pellet formation.
Smart Images

Figure 2024145840000001 
Figure 2024145840000002 
Figure 2024145840000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyvinyl alcohol-based resin composition (hereinafter, polyvinyl alcohol may be referred to as "PVA") having excellent melt moldability, and a laminate using the resin composition. [Background technology]
[0002] Plastics are widely used as packaging materials because of their excellent moldability, strength, water resistance, transparency, etc. Examples of plastics used in such packaging materials include polyolefin resins such as polyethylene and polypropylene, vinyl resins such as polystyrene and polyvinyl chloride, and aromatic polyester resins such as polyethylene terephthalate. However, these plastics are poorly biodegradable, and if dumped in the natural environment after use, they may remain for a long time, damaging the scenery and causing environmental destruction.
[0003] In response to this, in recent years, biodegradable resins that are biodegraded or hydrolyzed in soil or water and are useful for preventing environmental pollution have attracted attention and are being put to practical use. Examples of such biodegradable resins include aliphatic polyester resins, cellulose acetate, and modified starch. As packaging materials, polylactic acid, condensation polymers of adipic acid / terephthalic acid / 1,4-butanediol, and condensation polymers of succinic acid / 1,4-butanediol / lactic acid are used because of their excellent transparency, heat resistance, and strength.
[0004] However, since aliphatic polyester resins such as polylactic acid have insufficient oxygen gas barrier properties, they cannot be used alone as packaging materials for contents that may be subject to oxidative deterioration, such as food, medicines, etc. Therefore, aliphatic polyester resins such as polylactic acid and PVA resins are laminated by co-extrusion molding or the like to form a laminate.
[0005] Generally, biodegradable polyesters are molded in a temperature range of 140 to 170° C., while PVA resins are molded in a temperature range of 185 to 220° C. (For example, this is described in Patent Document 1, Patent Document 2, etc.). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2006-312313 A [Patent Document 2] JP 2009-196287 A Summary of the Invention [Problem to be solved by the invention]
[0007] Low-temperature melt molding is possible if a low-melting PVA resin is used. However, low-melting PVA resins have a slow crystallization rate during the cooling process, resulting in a low degree of crystallization, which causes cold crystallization during the heating process. Cold crystallization is a phenomenon in which crystals form from a supercooled liquid state above the glass transition temperature during heating. The occurrence of cold crystallization makes it difficult to optimize the extruder temperature profile during melt molding, which can lead to issues such as poor pellet feeding and molding defects.
[0008] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a PVA resin composition having excellent melt moldability. [Means for solving the problem]
[0009] The inventors of the present invention have found that by adding a polyvinyl alcohol resin having a higher melting point than a low-melting polyvinyl alcohol resin to the low-melting polyvinyl alcohol resin, the melting point rise can be suppressed, the crystallization rate during the cooling process can be increased, and cold crystallization during the heating process can be suppressed.The inventors have also found that such a polyvinyl alcohol resin composition can easily optimize the temperature profile of an extruder during low-temperature melt molding, and can improve the feedability and moldability of pellets.
[0010] That is, the present inventors have discovered that a polyvinyl alcohol-based resin composition containing two or more polyvinyl alcohol-based resins having different melting points, in which the melting point difference between a low-melting point polyvinyl alcohol-based resin (A) and a high-melting point polyvinyl alcohol-based resin (B) among the two or more polyvinyl alcohol-based resins is 30 to 70°C and the polyvinyl alcohol-based resin composition has a melting point of 160 to 200°C, can improve melt moldability, and have completed the present invention.
[0011] A first aspect of the present invention is a polyvinyl alcohol-based resin composition comprising two or more polyvinyl alcohol-based resins having different melting points, wherein the difference in melting point between a low-melting point polyvinyl alcohol-based resin (A) and a high-melting point polyvinyl alcohol-based resin (B) among the two or more polyvinyl alcohol-based resins is 30 to 70°C, and the melting point of the polyvinyl alcohol-based resin composition is 160 to 200°C.
[0012] A second aspect of the present invention is the polyvinyl alcohol-based resin composition of the first aspect, wherein the low melting point polyvinyl alcohol-based resin (A) has a melting point of 160 to 195°C, and the high melting point polyvinyl alcohol-based resin (B) has a melting point of 200 to 230°C.
[0013] A third aspect of the present invention is the polyvinyl alcohol-based resin composition according to the first or second aspect, wherein the polyvinyl alcohol-based resin composition is cooled from 250° C. to −50° C. at 40° C. / min, and then heated at 5° C. / min, and the amount of heat of cold crystallization generated is 14 J / g or less.
[0014] A fourth aspect of the present invention is the polyvinyl alcohol-based resin composition according to any one of the first to third aspects, wherein the low-melting point polyvinyl alcohol-based resin (A) is a polyvinyl alcohol-based resin containing a primary hydroxyl group in a side chain.
[0015] A fifth aspect of the present invention is a film or sheet made of the polyvinyl alcohol-based resin composition according to any one of the first to fourth aspects.
[0016] A sixth aspect of the present invention is a multilayer structure comprising at least one layer of the film or sheet of the fifth aspect. Effect of the Invention
[0017] The polyvinyl alcohol-based resin composition of the present invention has improved melt moldability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] [Polyvinyl alcohol resin composition] The polyvinyl alcohol (PVA) resin composition of the present invention contains two or more polyvinyl alcohol resins having different melting points, and the melting point difference between the low-melting polyvinyl alcohol resin (A) (hereinafter also referred to as low-melting PVA resin (A)) having a lower melting point among the two or more PVA resins and the high-melting polyvinyl alcohol resin (B) (hereinafter also referred to as high-melting PVA resin (B)) having a higher melting point than the low-melting polyvinyl alcohol resin (A) is 30 to 70° C., and the melting point of the PVA resin composition is 160 to 200° C. Hereinafter, each component of the PVA resin composition of the present invention will be described in order.
[0019] <Low melting point PVA resin (A) and high melting point PVA resin (B)> The low-melting-point PVA-based resin (A) and the high-melting-point PVA-based resin (B) used in the PVA-based resin composition of the present invention are PVA-based resins to be subjected to melt molding, and include not only unmodified PVA-based resins, but also copolymer-modified PVA-based resins obtained by saponifying a copolymer obtained by copolymerizing a modifying monomer in order to impart desired properties (e.g., high barrier properties) to the PVA-based resins, and post-modified PVA-based resins obtained by post-modifying a PVA-based resin.
[0020] In this specification, unless otherwise specified, the term "PVA-based resin" is a general term for unmodified PVA-based resin, copolymer-modified PVA-based resin, and post-modified PVA-based resin. When copolymer-modified PVA-based resin and post-modified PVA-based resin are collectively referred to, they are called "modified PVA-based resin".
[0021] 1. Unmodified PVA resin The unmodified PVA resin is a polyvinyl alcohol obtained by saponifying a polyvinyl ester obtained by polymerizing a vinyl ester monomer, and contains vinyl alcohol units represented by the following formula (1) and vinyl ester units (the following formula (2)) which are unsaponified portions. The vinyl ester units are included when the degree of saponification is less than 100%.
[0022] [ka]
[0023] [ka]
[0024] (2) In the formula, R a depends on the type of vinyl ester monomer used, and for example, when vinyl acetate monomer is used, it becomes a methyl group.
[0025] Examples of the vinyl ester monomer include vinyl formate, vinyl acetate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl benzoate, and vinyl versatate, with vinyl acetate being economically preferred.
[0026] The number average degree of polymerization of the unmodified PVA resin (measured in accordance with JIS K6726) is preferably 150-4,000, more preferably 200-2,000, further preferably 250-800, and particularly preferably 300-600.
[0027] The viscosity of an aqueous solution of the unmodified PVA resin may be used as an index of the average degree of polymerization. The viscosity of a 4% by mass aqueous solution at 20°C measured in accordance with JIS K6726 is preferably 1.5 to 20 mPa s, more preferably 2 to 12 mPa s, and particularly preferably 2.5 to 8 mPa s.
[0028] The degree of saponification of the unmodified PVA resin is preferably 68 to 99.9 mol%, more preferably 70 to 99.7 mol%, and particularly preferably 72 to 99.5 mol%. If the degree of saponification is too low, the flexibility becomes too high, and the shape stability during lamination tends to decrease. The saponification degree is an average saponification degree measured in accordance with JIS K6726.
[0029] The melting point of the unmodified PVA resin is preferably 160 to 230°C, and the decomposition temperature is preferably 250 to 350°C, although this depends on the degree of polymerization and the degree of saponification.
[0030] In the case of a typical PVA resin, the main chain bond is mainly 1,3-diol bond, and the content of 1,2-diol bond is about 1.5 to 1.7 mol %. However, the content of 1,2-diol bond can be increased by increasing the polymerization temperature when polymerizing the vinyl ester monomer.
[0031] 2. Modified PVA resin Examples of copolymerization monomers used in the copolymerized modified PVA resin include olefins such as ethylene, propylene, isobutylene, α-octene, α-dodecene, and α-octadecene; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, maleic anhydride, and itaconic acid, or their salts or mono- or dialkyl esters; nitriles such as acrylonitrile and methacrylonitrile; amides such as acrylamide and methacrylamide; olefin sulfonic acids such as ethylene sulfonic acid, allyl sulfonic acid, and methallyl sulfonic acid, or their salts; alkyl vinyl ethers, N-acrylamidomethyltrimethylammonium chloride, allyltrimethylammonium chloride, dimethylallyl vinyl ketone, N-vinylpyrrolidone, vinyl chloride, vinylidene chloride, polyoxyethylene (meth)allyl ether, and polyoxypropylene. Examples of the polyoxyalkylene (meth)allyl ether include polyoxyalkylene (meth)acrylates such as polyoxyethylene (meth)acrylate and polyoxypropylene (meth)acrylate; polyoxyalkylene (meth)acrylamides such as polyoxyethylene (meth)acrylamide and polyoxypropylene (meth)acrylamide; hydroxyl group-containing α-olefins such as polyoxyethylene (1-(meth)acrylamide-1,1-dimethylpropyl) ester, polyoxyethylene vinyl ether, polyoxypropylene vinyl ether, polyoxyethylene allylamine, polyoxypropylene allylamine, polyoxyethylene vinylamine, polyoxypropylene vinylamine, 3-buten-1-ol, 4-penten-1-ol, and 5-hexen-1-ol, and derivatives thereof such as acylated products.
[0032] Examples of post-modified PVA-based resins include those having an acetoacetyl group by reaction with diketene, those having a polyalkylene oxide group by reaction with ethylene oxide, those having a hydroxyalkyl group by reaction with an epoxy compound or the like, and those obtained by reacting an aldehyde compound having various functional groups with a PVA-based resin.
[0033] The amount of modification in the modified PVA-based resin, i.e., the content of structural units derived from various monomers in the copolymer or functional groups introduced by a post-reaction, cannot be generally determined because the characteristics vary greatly depending on the type of modification, but is preferably in the range of 0.1 to 20 mol %, and particularly preferably in the range of 0.5 to 15 mol %.
[0034] Among these various modified PVA resins, in the present embodiment, a PVA resin having a hydrophilic modified group is preferably used. Examples of the hydrophilic modified group include a hydroxyl group, a carboxyl group, and an amino group. In particular, from the viewpoint of water solubility, a PVA resin containing a structural unit having a 1,2 diol modified group is preferred.
[0035] The modified PVA resin containing a structural unit having a 1,2-diol modifying group contains a structural unit having a 1,2-diol modifying group in a side chain in addition to the vinyl alcohol unit represented by the following formula (1) constituting polyvinyl alcohol and the vinyl ester unit (the following formula (2)) which is an unsaponified portion. The vinyl ester unit is included when the saponification degree is less than 100%.
[0036] [ka]
[0037] [ka]
[0038] (2) In the formula, R adepends on the type of vinyl ester monomer used, and for example, when vinyl acetate monomer is used, it becomes a methyl group.
[0039] As the structural unit having a 1,2-diol modifying group in the side chain, a 1,2-diol-containing unit in the side chain represented by the following formula (3) is preferred.
[0040] [ka]
[0041] In formula (3), R 1 ~R 6 each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and X represents a single bond or a bonding chain.
[0042] In the general formula (3), R 1 ~R 6 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms (e.g., methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, etc., which may have a substituent such as a halogen group, a hydroxyl group, an ester group, a carboxylic acid group, or a sulfonic acid group). A hydrogen atom is more preferable. R 1 ~R 6 may be all the same or different, but are preferably all hydrogen atoms. When all are hydrogen atoms, the terminals of the side chains become primary hydroxyl groups, which is preferable in that the reactivity with adhesive resins such as acid-modified polyolefin resins is improved and the formation of a laminate is facilitated.
[0043] In formula (3), X is a single bond or a bonding chain. Examples of the bonding chain (X) include hydrocarbon groups such as alkylene groups, alkenylene groups, alkynylene groups, phenylene groups, and naphthylene groups (these hydrocarbon groups may be substituted with halogen atoms such as fluorine atoms, chlorine atoms, and bromine atoms), -O-, -(CHO) m -, -(OCH2) m -, -(CH2O) mCH2-, -CO-, -COCO-, -CO(CH2) m Examples thereof include CO-, -CO(CH)CO-, -S-, -CS-, -SO-, -SO-, -NR-, -CONR-, -NRCO-, -CSNR-, -NRCS-, -NRNR-, -HPO-, -Si(OR)-, -OSi(OR)-, -OSi(OR)O-, -Ti(OR)-, -OTi(OR)-, -OTi(OR)O-, -Al(OR)-, -OAl(OR)-, -OAl(OR)O-, and the like (each R is independently any substituent, preferably a hydrogen atom or an alkyl group, and m is an integer of 1 to 5). From the viewpoint of stability during production or use, X is preferably a single bond, an alkylene group having 6 or less carbon atoms (particularly a methylene group), or -CH2OCH2-, and among these, a single bond is most preferable from the viewpoint of thermal stability and stability under high temperatures or acidic conditions.
[0044] The structural unit represented by the above formula (3) is R 5 and R 6 A structural unit having a primary hydroxyl group in a side chain in which R is a hydrogen atom is particularly preferred, and the most preferred structural unit is 1 ~R 6 are all hydrogen atoms and X is a single bond,
[0045] [ka]
[0046] The degree of modification (content) of the modified PVA resin is preferably 0.1 to 20 mol%, more preferably 0.5 to 15 mol%, further preferably 1 to 10 mol%, and particularly preferably 2 to 8 mol%. If the modification rate is too low, the reactivity with adhesive resins such as acid-modified polyolefin resins tends to decrease, while if it is too high, the crystallization rate becomes too slow, and when a laminate is formed with another resin, the laminate tends to deform, and the appearance tends to deteriorate.
[0047] The number average degree of polymerization of the modified PVA resin (measured in accordance with JIS K6726) is preferably 150 to 4000, more preferably 200 to 2000, further preferably 250 to 800, and particularly preferably 300 to 600. If the average degree of polymerization is too low, it tends to be difficult to form a stable shape during melt molding, whereas if it is too high, the viscosity of the resin composition tends to become too high, making molding difficult.
[0048] The viscosity of a 4% by mass aqueous solution of the modified PVA resin at 20°C, measured in accordance with JIS K6726, is preferably 1.5 to 20 mPa s, more preferably 2 to 12 mPa s, and particularly preferably 2.5 to 8 mPa s. If the viscosity is too low, it tends to be difficult to form a stable shape during melt molding, and if it is too high, molding tends to be difficult.
[0049] The saponification degree of the modified PVA resin (average saponification degree measured in accordance with JIS K6726) is preferably 70 to 100 mol%, more preferably 80 to 99.9 mol%, and particularly preferably 85 to 99.7 mol%. If the saponification degree is too low, the gas barrier property tends to decrease.
[0050] The melting point of the modified PVA resin is preferably 160 to 230°C, and the decomposition temperature is preferably 250 to 350°C, although this depends on the degree of polymerization and the degree of saponification.
[0051] 3. Low melting point PVA resin (A) and high melting point PVA resin (B) The PVA resin composition of the present invention contains two or more kinds of PVA resins. Examples of the two or more kinds of PVA resins include the combination of the above-mentioned unmodified PVA resins, the combination of an unmodified PVA resin and various modified PVA resins, and the combination of different kinds of modified PVA resins. Examples of the combination of the same kind of modified PVA resins but different in saponification degree, polymerization degree, modification rate, etc. are also included.
[0052] At least two of the PVA resins contained in the PVA resin composition are a low-melting-point PVA resin (A) and a high-melting-point PVA resin (B) having a melting point higher than that of the low-melting-point PVA resin (A), and the difference in melting point between them is 30 to 70° C. If the difference in melting point between the low-melting-point PVA resin (A) and the high-melting-point PVA resin (B) is within the above range, the crystallization rate during the cooling process is increased, and cold crystallization during the heating process can be suppressed. The difference in melting point between the low melting point PVA resin (A) and the high melting point PVA resin (B) is preferably 32 to 66°C, and more preferably 35 to 63°C.
[0053] In the present invention, the melting point of the low melting point PVA resin (A) is preferably 160 to 195° C., more preferably 163 to 194° C., and further preferably 165 to 193° C. When the melting point of the low melting point PVA resin (A) is within the above range, melt molding can be performed in a low temperature range, specifically, in a temperature range from 160° C. to 195° C.
[0054] The melting point of the high melting point PVA resin (B) is preferably 200 to 230° C., more preferably 205 to 229° C., and further preferably 210 to 228° C. When the melting point of the high melting point PVA resin (B) is within the above range, the processability during low-temperature molding can be improved.
[0055] The melt flow rate (MFR) (210°C, load 2160g) of the low melting point PVA resin (A) and the high melting point PVA resin (B) is preferably 1 to 100g / 10min, more preferably 2 to 50g / 10min, and particularly preferably 3 to 30g / 10min. If the MFR is too high, the mechanical strength of the molded product tends to decrease, and if it is too low, the extrusion processability tends to decrease.
[0056] In addition, in order to ensure that the resin flow properties during melt molding are comparable between the low-melting-point PVA-based resin (A) and the high-melting-point PVA-based resin (B), it is preferable to adjust the difference in MFR (210°C, load 2160 g) (ΔMFR) to 5 g / 10 min or less, and more preferably 3 g / 10 min or less.
[0057] The PVA resin composition of the present invention preferably contains a low melting point PVA resin (A) as a main component. That is, the content of the low melting point PVA resin (A) in the PVA resin composition is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more. When the content of the low melting point PVA resin (A) is 70% by mass or more, low temperature melt molding is possible. From the viewpoint of processability during low-temperature molding, the content of the low-melting-point PVA resin (A) is preferably 99.995% by mass or less, more preferably 99.99% by mass or less, and even more preferably 99.95% by mass or less.
[0058] On the other hand, the high melting point PVA resin (B) is a minor component in the PVA resin composition, and the content of the high melting point PVA resin (B) in the PVA resin composition is preferably 0.004 to 9% by mass, more preferably 0.01 to 7% by mass, and even more preferably 0.05 to 5% by mass. When the content of the high melting point PVA resin (B) is within the above range, the processability during low-temperature molding can be improved.
[0059] The mass blending ratio of the low melting point PVA resin (A) to the high melting point PVA resin (B) contained in the PVA resin composition [low melting point PVA resin (A) / high melting point PVA resin (B)] is preferably in the range of 99.995 / 0.005 to 91 / 9, more preferably 99.99 / 0.01 to 93 / 7, and even more preferably 99.95 / 0.05 to 95 / 5. If the ratio of the high melting point PVA resin (B) is too small, pellet feeding failure and molding failure tend to occur, while if it is too large, the melting point becomes high, so that unmelted matter is generated during low-temperature melt molding, and molding failure tends to occur.
[0060] <Other ingredients>
[0061] 1. Plasticizers The PVA resin composition of the present invention may contain a plasticizer within a range that does not impair the effect of the present invention (melt moldability). Examples of the plasticizer include aliphatic polyhydric alcohols (e.g., ethylene glycol, hexanediol, glycerin, trimethylolpropane, diglycerin, etc.), compounds obtained by adding ethylene oxide to polyhydric alcohols, various alkylene oxides (e.g., ethylene oxide, propylene oxide, mixed adducts of ethylene oxide and propylene oxide, etc.), saccharides (e.g., sorbitol, mannitol, pentaerythritol, xylitol, arabinose, ribulose, etc.), phenol derivatives such as bisphenol A and bisphenol S, amide compounds such as N-methylpyrrolidone, glucosides such as α-methyl-D-glucoside, and the like.
[0062] 2. Other Resins The PVA-based resin composition of the present invention may contain other polymers within a range that does not inhibit the effects of the present invention (for example, less than 30% by mass of the composition). Examples of the polymers that can be contained include various thermoplastic resins such as polyamide, polyester, polyethylene, polypropylene, and polystyrene.
[0063] 3. Other Additives Also, within a range that does not inhibit the effects of the present invention (10% by mass or less of the composition), if necessary, a reinforcing agent, a filler, a pigment, a dye, a lubricant, an antioxidant, an antistatic agent, an ultraviolet absorber, a heat stabilizer, a light stabilizer, a surfactant, an antibacterial agent, an antistatic agent, a desiccant, an antiblocking agent, a flame retardant, a crosslinking agent, a curing agent, a foaming agent, a crystal nucleating agent, etc. may be contained.
[0064] The PVA-based resin composition of the present invention having the above composition improves the melt moldability without impairing the improved properties of the PVA-based resin.
[0065] <Method for Producing PVA-Based Resin Composition> The PVA resin composition of the present invention is produced using the essential components, low melting point PVA resin (A) and high melting point PVA resin (B), and the optional components described above, which are blended as necessary. Methods for producing a PVA resin composition having the above composition include (i) a method of kneading with a twin-screw extruder, and (ii) a method of kneading with a batch kneader. Method (i) is preferred, as it allows stable and efficient production of a pellet-shaped resin composition.
[0066] The PVA resin composition of the present invention has a melting point of 160 to 200° C. When the melting point of the PVA resin composition is 160° C. or higher, the crystallization rate during the cooling process is increased and cold crystallization during the heating process can be suppressed, and when the melting point is 200° C. or lower, low-temperature melt molding is possible. The melting point of the PVA resin composition is preferably 163 to 194°C, and more preferably 165 to 193°C.
[0067] In addition, the PVA resin composition of the present invention preferably has a heat of cold crystallization of 14 J / g or less when cooled from 250°C to -50°C at a cooling rate of 40°C / min and then heated at 5°C / min in a differential scanning calorimeter (DSC) measurement. If the heat is 14 J / g or less, the temperature profile of the extruder can be easily optimized during low-temperature melt molding, and the feedability and moldability of the pellets can be improved. The heat of cold crystallization is more preferably 12 J / g or less, and even more preferably 10 J / g or less. The smaller the heat of cold crystallization, the better, so there is no particular lower limit.
[0068] [Melt-molded product of PVA-based resin composition and its manufacturing method] The PVA resin composition of the present invention is melt moldable, and a melt extrusion molding method generally used for thermoplastic resins can be adopted. Therefore, the PVA-based resin composition of the present invention can be used for melt-molded products requiring gas barrier properties, particularly for applications such as melt-molded films, stretched films, and sheets, as well as containers and lids such as cups, trays, tubes, and bottles. The film or container may be a film or container made of the PVA-based resin composition of the present invention alone (single layer), but may also be used as a multilayer structure of two or more layers containing at least one film or sheet made of the PVA-based resin composition of the present invention and laminated with other thermoplastic resins, papers, etc. In the multilayer structure, the layer of the PVA-based resin composition of the present invention serves as a gas barrier layer.
[0069] Examples of multilayer structures containing a PVA-based resin composition layer of the present invention as a gas barrier layer include food packaging materials such as coffee capsules and shrink films, medicine packaging materials, cosmetic packaging materials such as lotion and foundation cases, packaging materials for metal parts, packaging materials for electronic parts, packaging materials for items in which deterioration of properties due to oxidation or moisture absorption should be suppressed, packaging materials for substances in which odor transfer or odor leakage is a concern, and multilayer structures used for various agricultural sheets and agricultural materials such as mulch sheets, fumigation sheets, seedling trays, and covering sheets.
[0070] Applicable melt molding methods include injection molding and extrusion molding. Extrusion molding is particularly suitable as a molding method for films and sheets, and examples thereof include T-die molding and inflation molding (tubular film method). Not only single-layer extrusion but also multi-layer extrusion may be used. Multi-layer extrusion (co-extrusion molding) is suitable for producing a multi-layer structure in which films are laminated.
[0071] The obtained film or sheet may be subjected to secondary processing such as uniaxial or biaxial stretching. Since the PVA-based resin composition of the present invention has excellent stretchability, it is preferable to perform a stretching treatment in order to increase the film strength and further improve the gas barrier property. EXAMPLES
[0072] The present invention will be further described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0073] [Measurement and evaluation method] 1. Saponification degree (mol%) Measurements were performed in accordance with JIS K6726.
[0074] 2.Number average degree of polymerization Measurements were performed in accordance with JIS K6726.
[0075] 3. Degree of modification (mol%) It was calculated from the amount of copolymerization monomer charged during synthesis of the PVA-based resin.
[0076] 4. Melting Point Measurement The melting points of the low melting point PVA resin (A), the high melting point PVA resin (B), and the PVA resin composition are values measured by a differential scanning calorimeter (DSC, Q2000, manufactured by TA Instruments). The measurement conditions are as follows. 1st run: -50℃~250℃, 5℃ / min, temperature modulation amplitude ±0.796℃, cycle 60sec, Cooling:250℃~-50℃, 40℃ / min, 2nd run: -50℃~250℃, 5℃ / min, temperature modulation amplitude ±0.796℃, cycle 60sec, The melting point was measured from the endothermic peak occurring in the range of 140 to 230°C in the reversing heat flow of the second run.
[0077] 5.Cold crystallization calorimetry The cold crystallization heat of the low melting point PVA resin (A), the high melting point PVA resin (B), and the PVA resin composition is a value measured by a differential scanning calorimeter (DSC) under the following measurement conditions. 1st run: -50℃~250℃, 5℃ / min, temperature modulation amplitude ±0.796℃, cycle 60sec, Cooling:250℃~-50℃, 40℃ / min, 2nd run: -50℃~250℃, 5℃ / min, temperature modulation amplitude ±0.796℃, cycle 60sec, The heat of cold crystallization was measured from the exothermic peak that occurred in the temperature range between the glass transition temperature and the melting temperature of the non-reversing heat flow in the second run.
[0078] 6. Melt molding evaluation The pellets were fed into a φ40 mm single screw extruder equipped with a strand die for 30 minutes and melt molded at the following molding temperatures. At that time, the feedability of the pellets, the molten resin temperature, and the processability were evaluated. Molding temperature: C1 / C2 / C3 / C4 / Head / Adapter / Die=170 / 190 / 190 / 180 / 180 / 180 / 180(℃)
[0079] <Feedability> The amount of material discharged for 1 minute was measured (N=5), and the feedability was evaluated. A (Good): Standard deviation σ of discharge amount is 3 or less B (bad): No resin is discharged from the strand die, or the standard deviation σ of the discharge amount is greater than 3.
[0080] <Molten resin temperature> The resin temperature was measured by a thermocouple thermometer installed in the extruder head.
[0081] <Workability> The strand discharged for 1 minute was evaluated for the presence of unmelted material. A (Good): 5 or less unmelted pieces B (bad): 6 or more unmelted pieces
[0082] [Preparation and Evaluation of Resin Composition] Example 1 As the low melting point PVA resin (A), a PVA resin containing 1,2-diol in the side chain having the structural unit shown in formula (3a) was used. The PVA resin containing 1,2-diol in the side chain used had a degree of modification (content of 1,2-diol unit in the side chain) of 8 mol%, a degree of saponification measured according to JIS K6726 of 99 mol%, a degree of polymerization measured according to JIS K6726 of 450, and a melting point measured by the above-mentioned measurement method of 169°C.
[0083] An unmodified PVA resin was used as the high melting point PVA resin (B). The unmodified PVA resin used had a saponification degree of 99 mol% measured according to JIS K6726, a polymerization degree of 450 measured according to JIS K6726, and a melting point of 227°C measured by the above measurement method.
[0084] PVA resin composition pellets were prepared by melt-kneading 99.9% by mass of low-melting-point PVA resin (A) and 0.1% by mass of high-melting-point PVA resin (B) under the following conditions using a twin-screw extruder TEM-18DS (manufactured by Shibaura Machine Co., Ltd.) The melting point of the PVA resin composition was 169°C.
[0085] Diameter (D)20mm L / D=48 Screw rotation speed: 300 rpm Set temperature: C1 / C2 / C3 / C4 / C5 / C6 / D=160 / 200 / 200 / 210 / 210 / 200 / 200(℃) Screw pattern: 2-way mixing screw Screen mesh: 90 / 120 / 90mesh
[0086] The prepared resin composition pellets were subjected to cold crystallization calorimetry and melt molding evaluation according to the above-mentioned measurement and evaluation methods. The results are shown in Table 2.
[0087] (Examples 2 to 6, Comparative Examples 1 to 5) A PVA-based resin composition was prepared according to the composition in Table 1, and cold crystallization calorimetry and melt molding evaluation were carried out in the same manner as in Example 1. The results are shown in Table 2.
[0088] [Table 1]
[0089] [Table 2]
[0090] As shown in Table 2, in Comparative Examples 1, 3, 4, and 5, the PVA resin composition had a large amount of heat of cold crystallization, and poor feeding occurred during melt molding, indicating that the melt moldability was poor. In Comparative Example 2, the melting point of the PVA resin composition was high, and unmelted matter occurred during melt molding, indicating that the melt moldability was poor. On the other hand, in Examples 1 to 6, in which the PVA resin composition of the present invention was used, the PVA resin composition had a small amount of heat of cold crystallization, and there was almost no increase in the melting point, so that the feedability during extrusion molding was good, and no unmelted matter was observed. From these results, it is understood that the PVA resin composition of the present invention has good melt moldability.
[0091] In the above embodiment, specific embodiments of the present invention are shown, but the above embodiment is merely illustrative and should not be interpreted as being limiting. Various modifications that are obvious to those skilled in the art are intended to be within the scope of the present invention. [Industrial Applicability]
[0092] The PVA resin composition of the present invention has sufficient melt moldability and can therefore be suitably used for various packaging materials, particularly food packaging materials such as coffee capsules.
Claims
1. A polyvinyl alcohol-based resin composition comprising two or more polyvinyl alcohol-based resins having different melting points, A polyvinyl alcohol-based resin composition, in which the melting point difference between the low melting point polyvinyl alcohol-based resin (A) and the high melting point polyvinyl alcohol-based resin (B) among the two or more polyvinyl alcohol-based resins is 30 to 70°C, and the melting point of the polyvinyl alcohol-based resin composition is 160 to 200°C.
2. The polyvinyl alcohol-based resin composition according to claim 1, wherein the low melting point polyvinyl alcohol-based resin (A) has a melting point of 160 to 195 ° C., and the high melting point polyvinyl alcohol-based resin (B) has a melting point of 200 to 230 ° C.
3. The polyvinyl alcohol-based resin composition according to claim 1, wherein the amount of heat of cold crystallization generated when the polyvinyl alcohol-based resin composition is cooled from 250°C to -50°C at 40°C / min and then heated at 5°C / min is 14 J / g or less.
4. 2. The polyvinyl alcohol-based resin composition according to claim 1, wherein the low melting point polyvinyl alcohol-based resin (A) is a polyvinyl alcohol-based resin containing a primary hydroxyl group in a side chain.
5. A film or sheet comprising the polyvinyl alcohol-based resin composition according to any one of claims 1 to 4.
6. A multilayer structure comprising at least one layer of the film or sheet of claim 5.
Citation Information
Patent Citations
Laminated structure
JP2006312313A
Biodegradable laminate
JP2009196287A