Electronic component

A glass ceramic sintered body with cordierite or indialite phases coated with forsterite or willemite phases addresses the challenge of achieving low dielectric constant, high strength, and high Q value in electronic components, enhancing performance in high-frequency applications.

JP2024145848APending Publication Date: 2024-10-15TDK CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023058383
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing electronic components face challenges in achieving both low dielectric constant, high strength, and high Q value, particularly in high-frequency applications, due to issues with stray capacitance and material properties.

Method used

The use of a glass ceramic sintered body with main phase particles composed of cordierite or indialite phases, coated with a forsterite or willemite phase coating layer, which applies compressive stress to maintain strength and reduce dielectric constant, while enhancing the Q value.

Benefits of technology

This configuration achieves a low dielectric constant, high strength, and high Q value, suitable for high-frequency applications, by managing thermal expansion and stress distribution within the electronic component.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145848000001_ABST
    Figure 2024145848000001_ABST
Patent Text Reader

Abstract

To provide an electronic component capable of achieving low dielectric constant, high strength, and high Q-value.SOLUTION: An electronic component includes a glass-ceramic sintered body. The glass-ceramic sintered body has: main phase particles including at least one of a cordierite phase and an indialite phase; and a coating layer including a forsterite phase present to cover the main phase particles.SELECTED DRAWING: Figure 2A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electronic component including, for example, a glass ceramic sintered body. [Background technology]

[0002] In ceramics used in electronic components such as capacitors, inductors, and circuit boards, it is common to use materials with a low dielectric constant (ε) (e.g., the composition described in Patent Document 1) in order to reduce stray capacitance that occurs between the internal conductor and the terminals.

[0003] In recent years, electronic components are required to have high-frequency characteristics due to the development of 5th generation mobile communication systems. Electronic components that require high-frequency characteristics are required to have even lower dielectric constants due to concerns about noise caused by stray capacitance. Furthermore, in recent years, the development of electric vehicles has required not only lower dielectric constants but also improved component strength. However, although progress has been made in the development of core material compositions to improve the above characteristics, it remains difficult to achieve low dielectric constants, high strength, and high Q values ​​at the same time when used as sintered ceramics, and the reality is that production has not yet been achieved. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2004-168557 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide an electronic component that can achieve a low dielectric constant, high strength, and a high Q value all at once. [Means for solving the problem]

[0006] In order to achieve the above object, an electronic component according to a preferred embodiment of the present invention comprises: An electronic component including a glass ceramic sintered body, The glass ceramic sintered body is Main phase particles including at least one of a cordierite phase and an indialite phase; and a coating layer including a forsterite phase that is present so as to cover the main phase particles.

[0007] In the electronic component according to this embodiment, it is possible to achieve both a low dielectric constant, high strength, and a high Q value. The reason is not necessarily clear, but it is presumed, for example, as follows. In general, the cordierite phase and the indialite phase, especially the indialite phase, have a relatively low thermal expansion coefficient compared to the forsterite phase. Therefore, by covering the main phase particles having a relatively low thermal expansion coefficient with a coating layer having a relatively high thermal expansion coefficient, stress is continuously applied to the main phase particles, and cracks are less likely to progress when stress is applied from the outside, so it is possible to achieve both a low dielectric constant and high strength, and to maintain a high Q value.

[0008] Moreover, an electronic component according to another preferred embodiment of the present invention comprises: An electronic component including a glass ceramic sintered body, The glass ceramic sintered body is Main phase particles including a composite oxide including Si, Mg, and Al as main components; and a coating layer which is present so as to cover the main phase particles and which contains a composite oxide containing Mg, Si and Zn as main components.

[0009] For example, a composite oxide containing Si, Mg, and Al as the main components to form a cordierite or indialite phase has a relatively low thermal expansion coefficient compared to a composite oxide containing Mg, Si, and Zn as the main components to form a forsterite phase. Therefore, by covering the main phase particles, which have a relatively low thermal expansion coefficient, with a coating layer, which has a relatively high thermal expansion coefficient, stress is continuously applied to the main phase particles, and cracks are less likely to develop when stress is applied from the outside. This makes it possible to achieve both a low dielectric constant and high strength, and to maintain a high Q value.

[0010] Preferably, the main phase particles are an indialite phase. Since indialite has a higher Q value than cordierite, it is possible to achieve both a low dielectric constant and high strength, and the Q value is further improved.

[0011] Preferably, the particle size of the main phase particles is 0.35 μm or more. As the particle size increases, the strength of the electronic component tends to improve. However, if the particle size is too large, the Q value tends to decrease and the dielectric constant tends to increase.

[0012] Preferably, the coating layer has a thickness of 0.02 μm or more.

[0013] By keeping the thickness of the coating layer (e.g., corresponding to the amount of forsterite / or the amount of complex oxide containing Mg, Si, and Zn as main components) within an appropriate range, the stress from the coating layer to the main phase particles is kept within an appropriate range, which is believed to prevent the occurrence of cracks. Furthermore, by keeping the thickness of the coating layer within an appropriate range, the strength of the electronic component is improved. This is believed to be because the compressive stress applied to the main phase particles is kept appropriate, improving the strength.

[0014] Preferably, the coating layer may contain a willemite phase (or a composite oxide containing Mg, Si and Zn as main components with more Mg than Zn / similar below) together with a forsterite phase (or a composite oxide containing Mg, Si and Zn as main components with more Zn than Mg / similar below). By forming a part of the coating layer from the willemite phase, it is possible to lower the dielectric constant and increase the Q value.

[0015] Preferably, the area ratio of the willemite phase to the total area of ​​the forsterite phase and the willemite phase in the coating layer is 0 to 73%, 1 to 73%, or 7 to 70%. If the willemite phase is too much, the strength decreases and the thermal expansion coefficient decreases, which tends to make it difficult to co-fire with an electrode (e.g., Ag).

[0016] Preferably, the coating layer contains Ce or Cu. The strength of the coating layer is increased by including Ce or Cu in a part of the coating layer. It is considered that these elements are not included in the sintered body as filler particles, but are diffused on the surface of the coating layer or the main phase particles. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a cross-sectional view of a chip coil as an electronic component according to one embodiment of the present invention. [Figure 2A] FIG. 2A is an image of a part of a cross section of a glass ceramic sintered body according to an embodiment of the present invention analyzed by STEM-EDS. [Figure 2B] FIG. 2B is an image obtained by analyzing a part of a cross section of a glass ceramic sintered body according to a comparative example of the present invention by STEM-EDS. [Figure 3A] FIG. 3A is an image obtained by analyzing a part of a cross section of a glass ceramic sintered body according to an embodiment of the present invention by XRD. [Figure 3B] FIG. 3B is an image obtained by analyzing a part of a cross section of a glass ceramic sintered body according to a comparative example of the present invention by XRD. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, an embodiment of the present invention will be described. However, the present invention is not limited to the embodiment described below. In addition, the components described below include modifications or similar objects that can be easily imagined by a person skilled in the art. Furthermore, the components described below can be appropriately combined.

[0019] (Coil electronic parts) As shown in FIG. 1, as an electronic component according to one embodiment of the present invention, a chip coil 1 has a chip element 4 in which ceramic layers 2 and internal electrode layers 3 are alternately laminated in the Z-axis direction.

[0020] The internal electrode layers 3 of each layer have a ring shape (circular, elliptical or polygonal) or C-shape when viewed from the Z-axis direction, and are connected in a spiral shape by internal electrode connection through-hole electrodes (not shown) or stepped electrodes that penetrate adjacent ceramic layers 2, forming a coil conductor 30.

[0021] Terminal electrodes 5 are formed on both ends in the Y-axis direction of the chip element 4. Ends of extraction electrodes 3a, 3b that are extracted to opposite sides along the Y-axis from a spirally continuous coil conductor 30 are connected to each terminal electrode 5. That is, each terminal electrode 5 is connected to both ends of the coil conductor 30 that constitutes a closed magnetic circuit coil (winding pattern).

[0022] In this embodiment, the lamination direction of the ceramic layers 2 and the internal electrode layers 3 coincides with the Z axis, the top and bottom surfaces of the element body 4 are parallel to the XY plane, and the end faces facing each other along the Y axis on which the terminal electrodes 5 are formed are parallel to the XZ plane. The X, Y, and Z axes are perpendicular to each other. In the multilayer chip coil 1 shown in FIG. 1, the winding axis of the coil conductor 30 approximately coincides with the Z axis.

[0023] There are no particular limitations on the external shape or dimensions of the chip element 4 and these can be set appropriately depending on the application. Typically, the external shape is approximately a rectangular parallelepiped with, for example, an X-axis dimension of 0.1 to 0.8 mm, a Y-axis dimension of 0.2 to 1.6 mm, and a Z-axis dimension of 0.1 to 1.0 mm.

[0024] In addition, there are no particular restrictions on the inter-electrode thickness and base thickness of the ceramic layer 2, and the inter-electrode thickness (the distance between the internal electrode layers 3 and 3) can be set to 2 to 50 μm, and the base thickness (the distance from the Z-axis end of the coil conductor 30 to the top and bottom surfaces of the chip element 4) can be set to approximately 5 to 300 μm.

[0025] In this embodiment, the terminal electrodes 5 are not particularly limited, and are formed by adhering a conductive paste containing Ag, Pd, or the like as a main component to the outer surface of the element body 4, baking the paste, and then electroplating the paste. Cu, Ni, Sn, or the like can be used for the electroplating.

[0026] The coil conductor 30 preferably contains Ag (including Ag alloys) and is made of, for example, simple Ag, an Ag-Pd alloy, etc. The coil conductor may also contain, as secondary components, Cu, Zr, Si, Al, Ti, Mg, and oxides thereof.

[0027] The ceramic layer 2 is made of a glass ceramic sintered body according to one embodiment of the present invention. The glass ceramic sintered body will be described in detail below.

[0028] (Glass ceramics sintered body) 2A, the glass ceramic sintered body according to this embodiment constituting the ceramic layer 2 has main phase particles 2a1, which are crystal particles, and a coating layer 2b1 and an auxiliary coating layer 2c1 present so as to cover the main phase particles 2a1. Note that "present so as to cover the main phase particles 2a1" does not necessarily mean that the layers are present so as to completely cover the main phase particles 2a1 in the cross-sectional image, but may be present so as to cover 50% or more of the circumference of the main phase particles 2a1, or may be present so as to cover 80% or more.

[0029] In this embodiment, the main phase particles 2a1 are composed of a composite oxide containing Si, Mg, and Al as main components, and may contain other components such as oxides of Zn, Zr, Ce, Cu, B, Ca, Sr, Ba, Li, Na, and K. In this embodiment, "elements contained as main components" refers to elements whose content, calculated as an oxide, of each element contained as a main component is 10 mass % (or mol %, the same applies below) or more.

[0030] In this embodiment, the main phase grains 2a1 are composed of a cordierite phase or an indialite phase, and preferably composed of an indialite phase. Whether the main phase grains 2a1 are composed of a cordierite phase or an indialite phase can be determined, for example, from the results of STEM-EDS (e.g., FIG. 2A or FIG. 2B) and XRD analysis (e.g., FIG. 3A or FIG. 3B).

[0031] The particle size of the main phase particles 2a1 is preferably 0.35 μm or more, 0.4 μm or more, 0.5 μm or more, or 0.55 μm or more, and is preferably 2.2 μm or less, 2.15 μm or less, 2.0 μm or less, or 1.9 μm or less. The larger the particle size, the stronger the chip coil 1 as an electronic component tends to be, but if the particle size is too large, the Q value tends to decrease and the dielectric constant tends to increase. For a chip coil 1 that is compatible with high frequencies, a low dielectric constant is preferable.

[0032] The particle size of the main phase particles 2a1 can be determined, for example, by determining the area of ​​each main phase particle 2a1 from a cross-sectional image of an SEM, defining the diameter of a virtual circle having that area as the particle size, and calculating the average of 300 or more randomly selected main phase particles 2a1. The observation magnification of the SEM cross-sectional image is appropriately adjusted to 2,000 to 10,000 times so that 300 or more main phase particles are included in one field of view.

[0033] In this embodiment, the coating layer 2b1 is composed of a forsterite phase, but may include an auxiliary coating layer 2c1 composed of a willemite phase. The coating layer 2b1 may be said to be composed of a composite oxide containing Mg, Si, and Zn as main components, with more Mg than Zn. The coating layer 2b1 may also contain oxides of Al, Zr, Ce, Cu, B, Ca, Sr, Ba, Li, Na, K, etc. as other components.

[0034] The auxiliary coating layer 2c1 can also be said to be composed of a composite oxide containing Mg, Si, and Zn as main components, with Zn being more abundant than Mg. The auxiliary coating layer 2c1 may contain oxides of other components similar to those of the coating layer 2b1 as other components. The strength of the electronic component is increased by including Ce or Cu in a portion of the coating layer 2b1 (2c1). These elements are not contained in the sintered body as filler particles, but are thought to be diffused on the surfaces of the coating layer 2b1 (2c1) or the main phase particles 2a1.

[0035] The coating layer 2b1 made of the forsterite phase includes the auxiliary coating layer 2c1 made of the willemite phase, so that the dielectric constant can be lowered and the Q value can be increased.

[0036] The thickness of the coating layer 2b1 (including the auxiliary coating layer 2c1 / the same applies below) is preferably 0.02 μm or more, 0.025 μm or more, or 0.05 μm or more, and is preferably 0.6 μm or less, 0.55 μm or less, or 0.5 μm or less.

[0037] By keeping the thickness of the coating layer 2b1 (e.g., corresponding to the amount of forsterite / or the amount of complex oxide containing Mg, Si, and Zn as main components) within an appropriate range, the thermal expansion coefficient of the coating layer 2b1 is kept within an appropriate range, and it is believed that the occurrence of cracks can be suppressed. In addition, it also becomes easier to simultaneously fire the coating layer 2b1 with the internal electrode phase (e.g., Ag) 3. Furthermore, by keeping the thickness of the coating layer 2b1 within an appropriate range, the strength of the chip coil 1 is improved. This is believed to be because the compressive stress applied to the main phase particles 2a1 is kept appropriate, improving the strength.

[0038] The thickness of the coating layer 2b1 can be determined by measuring the thickness of 50 or more points of the portion that has a different contrast from the main phase particle 2a1 and extends so as to surround the main phase particle 2a1 in the image obtained by STEM-EDS shown in FIG. 2A, and averaging the measured values ​​to obtain the thickness of the coating layer 2b1 and the auxiliary coating layer 2c1. At this time, the observation magnification is set to 5,000 to 20,000 times, and appropriately adjusted so that 30 or more main phase particles are included in one field of view. In this embodiment, the main phase particles 2a1 that are 50% or more surrounded by the coating layer 2b1 and the auxiliary coating layer 2c1 are present in a cross-sectional image of the ceramic sintered body within a range of 7.5 μm × 7.5 μm, preferably 30 or more, or 20 or more.

[0039] Alternatively, for example, from the element distribution of Mg measured by STEM-EDS in the same manner as in FIG. 2A, the thickness of the Mg layer covering the main phase particle 2a1 may be measured at 50 or more points, and the average value may be used as the thickness of the coating layer 2b1. Note that Mg is the most abundant element among the main component elements constituting the coating layer 2b1 made of the forsterite phase. In addition, regarding the thickness of the auxiliary coating layer 2c1 made of the willemite phase, the thickness of the Zn layer covering the main phase particle 2a1 may be measured at 50 or more points from the element distribution of Zn measured by STEM-EDS in the same manner as in FIG. 2A, and the average value may be used as the thickness of the auxiliary coating layer 2c1. Note that Zn is the most abundant element among the main component elements constituting the auxiliary coating layer 2c1 made of the willemite phase.

[0040] 2A, the ceramic sintered body constituting the ceramic layer may contain first subphase particles 2d1 and second subphase particles 2e1 as other particles. The first subphase particles 2d1 are preferably mainly composed of Ce oxide and / or Cu oxide and are present as part of the coating layer 2b1 or the auxiliary coating layer 2c1. The content of Ce and / or Cu in the first subphase particles 2d1 is, for example, 95 mass % or more, or 97 mass % or more, calculated as oxides, and may contain, for example, oxides of Si, Zn, Al, etc., in amounts of less than 5 mass % or less than 3 mass % as other components.

[0041] The second subphase particles 2e1 are mainly composed of Si oxides and may be present as a part of the coating layer 2b1 or the auxiliary coating layer 2c1. The content of Si in the second subphase particles 2e1 is, for example, 95 mass% or more, or 97 mass% or more, calculated as oxide, and other components such as oxides of Mg, Zn, Al, Ce, etc. may be contained in amounts of less than 5 mass% or less than 3 mass%. The second subphase particles 2e1 may be contained as a filler made of SiO2 alone, a filler made of Al2O3 alone, or a filler made of a composite oxide thereof.

[0042] In this embodiment, when 30 or more main phase grains 2a1 are included in one field of view of STEM-EDS, the area ratio of the main phase grains 2a1 in one field of view is preferably 30 to 70%, or 40 to 60%.

[0043] Under similar conditions, the total area ratio of the coating layer 2b1 and the auxiliary coating layer 2c1 (one field of view being 100%) is not particularly limited, but is smaller than the area ratio of the main phase particles 2a1, and is preferably about 15 to 45%, or 20 to 40%. The area ratio of the auxiliary coating layer 2c1 to the total area of ​​the coating layer 2b1 and the auxiliary coating layer 2c1 is preferably 0 to 73%, 1 to 73%, or 7 to 70%. If the auxiliary coating layer 2c1 made of the willemite phase is too much, the strength decreases and the thermal expansion coefficient decreases, which tends to make it difficult to co-fire with an electrode (for example, Ag).

[0044] Under similar conditions, the area ratio of the first subphase particles 2d1 within one visual field is preferably 1% or less, or 0.5% or less, or 0.3% or less. Under similar conditions, the area ratio of the second subphase particles 2e1 within one visual field is preferably 15% or less, or 13% or less.

[0045] (Manufacturing method) Next, a method for manufacturing the chip coil 1 shown in Fig. 1 will be described. First, a conductive paste containing Ag or the like that will become the internal electrode layers 3 shown in Fig. 1 is prepared. The conductive paste can be produced by a known method.

[0046] Separately from the conductor paste, a ceramic paste containing raw materials for the glass ceramic sintered body constituting the ceramic layer 2 shown in FIG. 1 is prepared. The ceramic paste contains raw materials that will become a glass ceramic sintered body having the above-mentioned composition and crystal structure after firing. The raw materials for the glass ceramic sintered body are not particularly limited, but examples thereof include various oxides, various compounds, or single or multiple glass compositions containing metal elements contained in the main phase particles 2a1 and the coating layer 2b1 shown in FIG. 2A and, if necessary, metal elements contained in the auxiliary coating layer 2c1 and / or the subphase particles 2d1 and 2e1.

[0047] For example, a ceramic paste can be obtained by pulverizing a single type or multiple types of glass composition as a raw material, adding other oxide powders, sintering aids, fillers, etc., and kneading the mixture with a binder and a solvent.

[0048] In this embodiment, the area ratio of the auxiliary coating layer 2c1 to the total area of ​​the coating layer 2b1 and the auxiliary coating layer 2c1 shown in Fig. 2A can be controlled by controlling the amount of Zn contained in the glass composition, etc. For example, the area ratio of the auxiliary coating layer 2c1 can be increased by increasing the amount of Zn.

[0049] In addition, as a filler, for example, it has a large specific surface area (for example, SSA is 5m 2 / g or more), a small amount of CeO2 and / or CuO can be added to the coating layer 2b1 and / or the auxiliary coating layer 2c1 to allow the coating layer 2b1 and / or the auxiliary coating layer 2c1 to contain Ce and / or Cu. Note that a part of the filler may generate subphase particles 2d1. Also, silicon oxide as a filler will generate subphase particles 2e1, and a part of it is thought to diffuse into the coating layer 2b1 and / or the auxiliary coating layer 2c1.

[0050] Next, the above-mentioned ceramic paste and conductor paste are printed, for example, alternately, and the patterns of the conductor paste between different layers are connected with through holes or steps, forming a spiral conductor pattern inside the laminate of ceramic paste layers. Next, if necessary, the laminate is pressed and cut to a predetermined size to obtain a green chip, and the green chip is fired to form the chip element 4 shown in Figure 1 (printing method).

[0051] Alternatively, green sheets may be made using ceramic paste, the internal electrode paste may be printed on the surfaces of the green sheets, and these may be stacked and fired to form the chip element 4 (sheet method). In either case, after the chip element 4 is formed, the terminal electrodes 5 may be formed by baking or plating.

[0052] There is no limit to the content of the binder and the solvent in the ceramic paste, and for example, the binder content can be set in the range of about 5 to 25 mass% and the solvent content can be set in the range of about 30 to 80 mass% with the total of the entire ceramic paste being 100 mass%. In addition, the paste can contain a dispersant, a plasticizer, etc., in the range of 20 mass% or less, as necessary.

[0053] A conductive paste containing Ag or the like can be prepared in the same manner. In addition, the firing conditions are not particularly limited, but when the internal electrode layer contains Ag or the like, the firing temperature is preferably 960° C. or less, 920° C. or less, or 900° C. or less, and preferably 870° C. or more. By controlling the maximum temperature during firing, it is possible to control the thickness of the covering layer 2b1 and the auxiliary covering layer 2c1 shown in FIG. 2A, for example.

[0054] The firing time is not particularly limited, but is preferably about 0.5 to 10 hours. The particle size of the main phase particles 2a1 can be controlled by the firing time, and the longer the firing time, the larger the particle size tends to be. The temperature rise rate during firing is not particularly limited, but by increasing the temperature rise rate (for example, 3 to 10 times the normal rate), the particle size of the main phase particles 2a1 shown in FIG. 2A can be increased.

[0055] In addition, by controlling the heat treatment after firing at the maximum firing temperature, the crystal structure of the main phase particles 2a1 can also be controlled. For example, by extending the time for annealing at a temperature lower than the maximum firing temperature after firing at the maximum firing temperature, the main phase particles 2a1 made of cordierite are easily generated. In addition, by shortening the annealing time after firing at the maximum firing temperature or by lowering the temperature without annealing, the main phase particles 2a1 made of indialite are easily generated.

[0056] (Summary of the embodiment) In the chip coil 1 as an electronic component according to the present embodiment, it is possible to achieve both a low dielectric constant, high strength, and a high Q value. The reason for this is not necessarily clear, but it is presumed, for example, as follows. In general, the cordierite phase and the indialite phase, especially the indialite phase, have a relatively low thermal expansion coefficient compared to the forsterite phase. Therefore, by covering the main phase particles with a relatively low thermal expansion coefficient with a coating layer with a relatively high thermal expansion coefficient, stress is continuously applied to the main phase particles, and cracks are less likely to progress when stress is applied from the outside, so it is thought that it is possible to achieve both a low dielectric constant and high strength, and to maintain a high Q value.

[0057] Alternatively, a composite oxide containing Si, Mg, and Al as main components to form a cordierite phase or an indialite phase has a relatively low thermal expansion coefficient compared to a composite oxide containing Mg, Si, and Zn as main components to form a forsterite phase. Therefore, it is considered that by covering the main phase particles, which have a relatively low thermal expansion coefficient, with a coating layer, which has a relatively high thermal expansion coefficient, a compressive stress is applied to the main phase particles, making it possible to achieve both a low dielectric constant and high strength, and to maintain a high Q value.

[0058] In this embodiment, the main phase particles 2a1 are preferably an indialite phase. Since indialite has a higher Q value than cordierite, it is possible to achieve both a low dielectric constant and high strength, and the Q value is further improved.

[0059] In this embodiment, the coating layers 2b1 and 2c1 contain a forsterite phase (or a composite oxide containing Mg, Si, and Zn as main components, with more Mg than Zn; the same applies below) and a willemite phase (or a composite oxide containing Mg, Si, and Zn as main components, with more Zn than Mg; the same applies below). By forming a part of the coating layer from the willemite phase, it is possible to lower the dielectric constant and increase the Q value.

[0060] In this embodiment, the coating layers 2b1 and 2c1 contain Ce or Cu. The strength of the coating layers 2b1 and 2c1 is increased by including Ce or Cu in a portion of the coating layers 2b1 and 2c1. It is considered that these elements are not included in the sintered body as filler particles, but are diffused on the surface of the coating layers or the main phase particles. Note that Ce or Cu included in the raw material may be present in the form of oxide particles (first subphase particles 2d1 shown in FIG. 2A) in a form in which a portion of the Ce or Cu is incorporated into the coating layers 2b1 and 2c1.

[0061] The present invention is not limited to the above-described embodiment, and various modifications can be made within the scope of the present invention.

[0062] For example, the glass ceramic sintered body according to the present embodiment can be used as an element of a coil element incorporated in a semiconductor device. For example, the glass ceramic sintered body according to the present embodiment can be made into a thin film and incorporated into a substrate on which a semiconductor device is formed.

[0063] Moreover, the glass ceramic sintered body according to this embodiment can be suitably used as an interlayer material for high frequency coils.

[0064] The glass ceramic sintered body according to this embodiment has a low dielectric constant and sufficient strength, and therefore can be suitably used, in particular, as an interlayer material constituting the ceramic layer 2 between the internal electrode layers 3 and 3.

[0065] The ceramic sintered body according to the present embodiment can improve the dielectric constant, strength, and sinterability in a well-balanced manner, and can achieve a high Q value in the high frequency range as an electronic component. The ceramic sintered body is particularly suitable for use in high frequency coils used in the frequency range of 1 GHz or more.

[0066] In the above embodiment, the ceramic layers 2 of the chip coil 1 are formed of the same material, but they do not necessarily have to be formed of the same material. As described above, the glass ceramic sintered body according to the embodiment is particularly suitable as an interlayer material constituting the ceramic layers 2 between the internal electrode layers 3, 3, and the ceramic layers 2 not in contact with the coil conductor 30 may be composed of other ceramic materials. EXAMPLES

[0067] The present invention will be described below with reference to more detailed examples, but the present invention is not limited to these examples.

[0068] (Sample No. 1a) The raw materials consist of 83 parts by mass or more of glass powder (silica magnesium aluminum glass frit) containing Mg, Al, Zn, and Si, and a glass substrate with a specific surface area (SSA) of 6.4 m 2A glass ceramic paste was prepared by preparing 0.5 parts by mass or less of cordierite powder having a molecular weight of 1000 to 1000 g / g or more, 2.0 parts by mass or less of cerium oxide (CeO2), 15 parts by mass or less of silica (SiO2) filler, and 1 part by mass or less of a sintering aid containing B, in a total amount of 100 parts by mass, and mixing them in a ball mill.

[0069] The obtained glass ceramic paste was applied to a PET film by a coater to form a green sheet. In addition, an Ag electrode pattern was formed on the dried green sheet by screen printing. After peeling off the PET film, the sheets were stacked and pressed so that the electrode patterns on each sheet were connected in a spiral shape, and the obtained laminate was cut to prepare a green chip.

[0070] The green chip was sintered according to the following procedure. The temperature was raised from room temperature to 400°C, and a de-bismuth treatment was performed. The temperature was raised to 800°C at a rate of 1000°C / hour, and then raised to 900°C at a rate of 200°C / hour. Then, the chip was sintered in air at 900°C for 1 hour, and cooled to room temperature at a rate of 200°C / hour without annealing treatment, to obtain a sample of the chip element 4 shown in FIG. 1. The sample of the chip element 4 was cut to obtain a ceramic sintered sample constituting the ceramic layer 2. The obtained ceramic sintered sample and the chip element sample were evaluated as follows.

[0071] <Cross-sectional analysis> A cross-sectional analysis of the sintered body sample was performed using STEM-EDS, and the image shown in FIG. 2A was obtained. It was confirmed that many main phase particles 2a1 were surrounded by a coating layer 2b1 (and in some cases, an auxiliary coating layer 2c1). Subphase particles 2d1 and 2e1 were also observed. A composition analysis of the main phase particle 2a1 revealed that the main phase particle 2a1 contained 45 to 70 mass% Si in oxide equivalent, 15 to 20 mass% Mg in oxide equivalent, 15 to 20 mass% Al in oxide equivalent, 4 mass% or less Zn in oxide equivalent, 0.1 mass% or less Ce in oxide equivalent, and 0.2 mass% or less Zr in oxide equivalent.

[0072] The coating layer 2b1 contained 30 to 40 mass% Si in terms of oxide, 30 to 40 mass% Mg in terms of oxide, 3 mass% or less Al in terms of oxide, 20 to 30 mass% Zn in terms of oxide, 0.1 to 0.2 mass% Ce in terms of oxide, and 0.3 to 0.7 mol Zr in terms of oxide.

[0073] Furthermore, when an XRD analysis was performed on a sintered body sample including the main phase particles 2a1 and the coating layer 2b1, an indialite peak (black circle) and a forsterite peak (X) were observed, as shown in Fig. 3A. From the results of STEM-EDS and XRD, it was considered that the main phase particles included an indialite phase, and the coating layer 2b1 included a forsterite phase.

[0074] Furthermore, by using a similar analysis method, it was found that coating layer 2c1, which has a different image contrast from coating layer 2b1, contains 20 to 30 mass% Si in oxide equivalent, 3 to 10 mass% Mg in oxide equivalent, 1 mass% or less Al in oxide equivalent, 60 to 70 mass% Zn in oxide equivalent, 0.1 to 0.2 mass% Ce in oxide equivalent, and 0.2 or less Zr in oxide equivalent. Judging comprehensively including other observation results, coating layer 2c1 was considered to contain a willemite phase.

[0075] Furthermore, by the same analysis method, it was confirmed that the subphase particle 2d1 contains Ce at 99 mass % or more in terms of oxide, and the subphase particle 2e1 contains Si at 99 mass % or more in terms of oxide. It was also confirmed that Ce is diffused into the coating layers 2b1 and 2c1.

[0076] <Size of main phase particles> A cross-sectional analysis of the sintered body sample was performed using an SEM to obtain an image as shown in FIG. 2A. The observation magnification was set to 2,000 to 10,000 times, and 300 or more main phase particles were included in one field of view. The circle equivalent diameters of the 300 or more main phase particles 2a1 were calculated from the cross-sectional areas, and the average value was taken as the particle size of the main phase particles. The results are shown in Table 1.

[0077] <Coating thickness> Cross-sectional analysis of the sintered body sample was performed by STEM-EDS, and an image as shown in Fig. 2A was obtained. At this time, the observation magnification was set to 5,000 to 20,000 times, and 30 or more primary phase particles were included in one field of view. The thickness of the coating layer 2b1 covering the primary phase particle 2a1 was randomly measured for 50 or more coating layers 2b1 of the primary phase particle 2a1, and the average value was taken as the thickness of the coating layer. The results are shown in Table 1.

[0078] <Relative permittivity> The relative permittivity (unitless) was measured by the resonance method (JIS R 1627) using a network analyzer (PNA N5222A manufactured by Agilent Technologies). In this example, a relative permittivity of 5.8 or less, preferably 5.7 or less, or 5.6 or less was considered good. In the table, it is described as the dielectric constant. The results are shown in Table 1.

[0079] <Strength> For the prismatic sample (outer diameter 20 mm × 5 mm × 2 mm) of the chip body, the flexural strength of the sintered body was measured by a three-point bending test (span distance 15 mm) using a universal material testing machine 5543 manufactured by INSTRON. In this example, 185 MPa or more, preferably 200 MPa or more was considered good. The results are shown in Table 1.

[0080] <Q value> The Q value was measured according to the Japanese Industrial Standard "Test Method for Dielectric Properties of Fine Ceramics for Microwaves (JIS R1627 1996 Edition)". Specifically, a cylinder (pellet) of 15 mmφ × 5 mm made of a glass-ceramic sintered body was prepared, and the dielectric loss tangent tanδ was calculated by the two-terminal short-circuited dielectric resonator method. Further, 1 / tanδ = Q was used. The Q value is 630 or more, and preferably 700 or more, 800 or more, 900 or more, 1000 or more, and the larger the better. The results are shown in Table 1.

[0081] (Sample No. 1b) A chip element and a sintered body sample were prepared in the same manner as in sample 1a, except that a glass composition containing less Zn than the glass composition used in sample 1a was used and no cerium oxide was added as an additive. The results are shown in Table 1.

[0082] In the cross section of the sintered glass ceramic body of sample number 1b, no subphase particles made of Ce oxide were observed, and the coating layer 2b1 was observed, but the auxiliary coating layer 2c1 was not observed.

[0083] (Sample No. 2) A chip element and a sintered body sample were produced in the same manner as sample No. 1b, and evaluated in the same manner as sample No. 1b, except that cordierite powder, cerium oxide (CeO2), and silica (SiO2) filler were not included in the raw material powder, and the powder was sintered at 900°C for 1 hour, cooled to 850°C over 15 minutes, annealed at 850°C for 60 minutes in air, and then cooled to room temperature at a rate of 200°C / hour. The results are shown in Table 1.

[0084] FIG. 2B shows a STEM-EDS image of the glass ceramic sintered body taken in the same manner as in Example 1a.

[0085] As shown in FIG. 2B, it was confirmed that the main phase particles 2a2 were cordierite phase, but the main phase surface layer 2b2 covering the surface thereof contained 45-50 mass% Si in oxide equivalent, 15-20 mass% Mg in oxide equivalent, 5-8 mass% Al in oxide equivalent, and 25-30 mass% Zn in oxide equivalent, and was confirmed to be a Zn-rich main phase surface layer compared to the main phase particles 2a2, and was neither forsterite nor willemite. That is, the coating layers 2b1 and 2c1 shown in the sample numbers 1a and 1b of the embodiment were not observed in the sample of sample number 2, which is a comparative example. In the table, the fact that it was not observed is indicated by "-" in the column of the coating layer thickness.

[0086] In the sample of sample number 2, which is a comparative example, third subphase particles 2c2, fourth subphase particles 2d2, and amorphous phase 2e2 were observed. In the example, the amorphous phase 2e2 was not observed. It was confirmed that the third subphase particles 2c2 were composed of a willemite phase, and the fourth subphase particles 2d2 were composed of a forsterite phase or an enstatite phase.

[0087] (Sample No. 3) After sintering at 900°C for 1 hour, this was cooled to 850°C over 15 minutes, annealed in air at 850°C for 60 minutes, and then cooled to room temperature at a rate of 200°C / hour. Except for this, a chip element sample and a sintered body sample were produced in the same manner as sample number 1b, and evaluated in the same manner as sample number 1b. The results are shown in Table 1. It was confirmed that the main phase particles were cordierite phase.

[0088] (Sample No. 4) A chip element sample and a sintered body sample were produced in the same manner as sample No. 2, except that the annealing treatment was not performed, and were evaluated in the same manner as sample No. 2. The results are shown in Table 1. It was confirmed that the main phase particles were cordierite phase.

[0089] (Rating 1) As shown in Table 1, it was confirmed that the examples of sample numbers 1a, 1b, and 3 in which a coating layer of a forsterite phase was formed could achieve high strength and a high Q value, compared to the comparative examples of sample numbers 2 and 4. In particular, it was confirmed that the examples in which the main phase particles consisted of an indialite phase had improved Q values ​​and strengths, compared to the examples in which the main phase particles consisted of a cordierite phase.

[0090] (Sample Nos. 5 to 8) A chip element sample and a sintered body sample were prepared in the same manner as sample number 3, and evaluated in the same manner as sample number 3, except that the firing time and temperature rise time were controlled to adjust the size of the main phase particles to the values ​​shown in Table 2. The results are shown in Table 2. In Table 2, a coating layer is recorded as "present" when the coating layer thickness was recognized to be 0.02 μm or more. Furthermore, it was confirmed that the longer the firing time, the larger the particle size tends to be, and that the particle size can also be increased by increasing the heating rate.

[0091] (Sample Nos. 9-12) A chip element sample and a sintered body sample were prepared in the same manner as sample number 1b, and evaluated in the same manner as sample number 1b, except that the size of the main phase particles was adjusted to the values ​​shown in Table 2 by controlling the firing time and the temperature rise time in the same manner as sample numbers 5 to 8. In Table 2, a coating layer was recorded as "present" when the thickness of the coating layer was recognized to be 0.02 μm or more. The results are shown in Table 2.

[0092] (Rating 2) As shown in Table 2, it was confirmed that a coating layer was formed in each example with a different main phase grain size, and a ceramic sintered body with a low dielectric constant, high strength, and high Q value was obtained. It was also confirmed that as the main phase grain size increases, the dielectric constant increases, the strength increases, and the Q value decreases. In particular, it was confirmed that the Q value was particularly improved in the example in which the main phase grains were made of an indialite phase, compared to the example in which the main phase grains were made of a cordierite phase.

[0093] (Sample Nos. 13-16)

[0094] Compared to sample No. 3, the thickness of the coating layer was changed by controlling the maximum temperature and holding time during firing. Except for this, sintered body samples were prepared in the same manner as sample No. 3 and evaluated in the same manner as sample No. 3. The results are shown in Table 3. It was confirmed that the higher the maximum temperature during firing, the thicker the coating layer tends to be, and that the longer the holding time of the maximum temperature during firing, the thicker the coating layer becomes.

[0095] A crack test was conducted according to the procedure shown below. The results of the crack test are also shown in Table 3.

[0096] <Crack test> 50 chip element samples were prepared and subjected to a crack test using the test method described below.

[0097] A chip element sample of each sample number was soldered to the center of a substrate (glass epoxy substrate, size 100 mm x 40 mm, thickness 0.08 mm), and then a load was applied to the other side (back of the substrate) from the side to which the sample was soldered for 5 seconds with a deflection of 1.2 mm. After the load was applied, the appearance of the sample and the presence or absence of internal cracks were evaluated.

[0098] The fewer the number of cracks observed, the more preferable.

[0099] (Sample Nos. 17-20) Compared to sample number 1b, the thickness of the coating layer was changed by controlling the maximum temperature during firing, but other than that, sintered samples were prepared in the same manner as sample number 1b, and evaluations were performed in the same manner as sample numbers 13 to 16. The results are shown in Table 3.

[0100] (Rating 3) As shown in Table 3, it was confirmed that in each example in which the thickness of the coating layer was changed, a ceramic sintered body that realized a low dielectric constant, high strength, and high Q value could be obtained. Furthermore, it was confirmed that the dielectric constant increases and the Q value decreases as the coating layer becomes thicker. It was also confirmed that the strength increases and the internal cracks decrease as the coating layer becomes thicker, but that the strength decreases and the internal cracks increase when the coating layer becomes too thick.

[0101] (Sample Nos. 21-25) Sintered samples were prepared in the same manner as sample number 3, and evaluated in the same manner as sample numbers 13 to 16, except that the amount of Zn contained in the glass composition was controlled and the sintering temperature (maximum temperature during firing) was controlled to adjust the abundance ratio (area ratio) of the willemite phase in the coating layer to the values ​​shown in Table 4. The results are shown in Table 4. In Table 4, forsterite was recorded as "present" when the area ratio of forsterite in the field of view was recognized to be 3.5% or more.

[0102] (Sample Nos. 26-30) Sintered samples were prepared in the same manner as sample number 1b, and evaluated in the same manner as sample numbers 17 to 20, except that the amount of Zn contained in the glass composition was controlled so that the proportion (area proportion) of the willemite phase in the coating layer became the values ​​shown in Table 4. The results are shown in Table 4. In Table 4, forsterite was recorded as "present" when the area proportion of forsterite in the field of view was recognized to be 3.5% or more.

[0103] (Rating 4) As shown in Table 4, it was confirmed that in each example in which willemite was contained in the coating layer, a ceramic sintered body with low dielectric constant, high strength, and high Q value was obtained. It was also confirmed that by increasing the proportion of willemite in the coating layer, the dielectric constant decreased, the strength decreased, and the Q value increased. The reason for the decrease in strength and increase in cracks is thought to be that the amount of willemite increased, resulting in a decrease in the thermal expansion coefficient. It was also confirmed that by increasing the amount of Zn contained in the glass composition, the proportion of the willemite phase in the coating layer increased. It was also confirmed that the sintering temperature could be decreased by increasing the amount of Zn contained in the glass composition.

[0104] (Sample Nos. 31-37) A chip element sample and a sintered body sample were prepared in the same manner as sample No. 3, except that the amount of Ce and / or Cu oxide contained in the raw material was adjusted to adjust the proportions of CeO2 and CuO in the coating layer to the values ​​(mass%) shown in Table 5, and evaluations were performed in the same manner as for sample No. 3. The results are shown in Table 5. In Table 5, forsterite was recorded as "present" when the area proportion of forsterite in the field of view was recognized to be 3.5% or more.

[0105] (Sample Nos. 38-44) A chip element sample and a sintered body sample were prepared in the same manner as sample number 1b, except that the amount of Ce and / or Cu oxide contained in the raw material was adjusted to adjust the mass percentage of CeO2 and CuO in the coating layer to the values ​​(mass percentages) shown in Table 5, and evaluations were performed in the same manner as for sample number 1b. The results are shown in Table 5. In Table 5, forsterite was recorded as "present" when the area percentage of forsterite in the field of view was found to be 3.5% or more.

[0106] (Rating 5) As shown in Table 5, it was confirmed that in each Example in which the coating layer contained Ce or Cu, a ceramic sintered body realizing a low dielectric constant, high strength, and high Q value was obtained. Furthermore, it was confirmed that, compared with Example 3 in which the coating layer did not contain Ce or Cu, Examples 31 to 37 were able to achieve higher strength and Q value. Furthermore, it was confirmed that, compared with Example 1b in which the coating layer did not contain Ce or Cu, Examples 38 to 44 were able to achieve higher strength and Q value.

[0107] [Table 1]

[0108] [Table 2]

[0109] [Table 3]

[0110] [Table 4]

[0111] [Table 5] [Explanation of symbols]

[0112] 1...Chip coil 2…Ceramic layer 2a1...Main phase particles (cordierite / indialite) 2b1…Coating layer (forsterite) 2c1...Auxiliary covering layer (Willemite) 2d1…First subphase particle (cerium oxide) 2e1: Second subphase particles (silicon oxide) 2a2…Main phase particles (cordierite) 2b2: Main phase surface layer (zinc-rich) 2c2…Third subphase particles (willemite) 2d2…fourth subphase particles (forsterite / enstatite) 2e2...amorphous phase (silicon oxide) 3...Internal electrode layer 3a, 3b...Extraction electrode 30…Coil conductor 4…Chip element 5...Terminal electrode

Claims

1. An electronic component including a glass ceramic sintered body, The glass ceramic sintered body is Main phase particles including at least one of a cordierite phase and an indialite phase; and a coating layer containing a forsterite phase present so as to cover the main phase particles.

2. The electronic component according to claim 1 , wherein the main phase grains are the indialite phase.

3. 3. The electronic component according to claim 1, wherein the main phase grains have a grain size of 0.35 μm or more.

4. 3. The electronic component according to claim 1, wherein the coating layer has a thickness of 0.02 [mu]m or more.

5. 3. The electronic component according to claim 1, wherein the coating layer contains a willemite phase.

6. 6. The electronic component according to claim 5, wherein the area ratio of the willemite phase to the total area of ​​the forsterite phase and the willemite phase in the coating layer is 1 to 73%.

7. The electronic component according to claim 1 or 2, wherein the coating layer contains Ce or Cu.

8. An electronic component including a glass ceramic sintered body, The glass ceramic sintered body is Main phase particles including a composite oxide including Si, Mg, and Al as main components; a coating layer present so as to cover the main phase particles, the coating layer including a composite oxide containing Mg, Si, and Zn as main components.

Citation Information

Patent Citations

  • Liquid type writing utensil

    JP1987001594A

  • Plastic fat and oil composition and production thereof

    JP1988039546A

  • Manufacture of cold rolled stainless steel strip

    JP1992017906A

  • Low dielectric loss glass

    JP1999511719A

  • Composite particle

    JP2001342074A