Phosphor and light-emitting device
A Y3-xCe xAl5-y-zMg yZr zO12 phosphor with a garnet-type structure addresses temperature quenching issues in blue laser excitation, maintaining warm-colored fluorescence and high brightness by optimizing composition and structure for high-intensity blue laser use.
Patent Information
- Application Number
- JP2023058395
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Blue laser light, with its higher intensity, causes temperature quenching in existing orange phosphors, leading to a loss of warm color fluorescence, while YAG:Ce phosphors have high temperature quenching resistance but are not suitable for high-intensity blue laser excitation.
A Y3-xCe xAl5-y-zMg yZr zO12 single crystal phosphor with a garnet-type crystal structure is developed, where x is 0.03 to 0.15, y is 0.05 to 0.6, and z is 0.05 to 0.6, which has high internal quantum yield and emits warm-colored fluorescence with a peak wavelength of 550 to 570 nm, suppressing concentration quenching and maintaining fluorescence even under high-intensity blue laser excitation.
The Y3-xCe xAl5-y-zMg yZr zO12 phosphor maintains warm-colored fluorescence and high brightness by suppressing temperature quenching, allowing the use of blue laser light sources without losing warm color emission.
Smart Images

Figure 2024145854000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a phosphor and a light emitting device. [Background technology]
[0002] Spot lighting designed to emit a so-called incandescent light is used for lighting in stores and on the streets.
[0003] In typical incandescent lighting, blue LED light is used as excitation light to hit a warm-colored phosphor, the wavelength is converted to adjust the color of the fluorescence to a warm color, and the blue LED light and warm-colored fluorescence are mixed to create the incandescent light.
[0004] However, blue laser light is more suitable than blue LED light as the excitation light for spot lighting, which focuses light on a specific spot. This is because blue laser light has a smaller light-emitting area than blue LED light, making it easier to focus the light.
[0005] As an example of a warm-color phosphor, Patent Document 1 describes an orange phosphor in which trivalent cerium is introduced as an activator into calcium aluminum silicon nitride, called cCaAlSiN3·(1-c)LiSi2N3:Ce 3+ (0.2≦c≦0.8) is disclosed.
[0006] However, blue laser light is stronger than blue LED light, and when blue laser light is incident on a phosphor, the phosphor becomes hot locally due to the strong light. 3+ Since orange phosphors such as these are prone to temperature quenching, even if blue laser light is incident on this orange phosphor, the orange color tends to be lost and the fluorescence tends to be less warm.
[0007] In contrast, YAG:Ce is a type of YAG that uses cerium as an activator. 3+ has high temperature quenching resistance. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] International Publication No. 2012 / 014702 Summary of the Invention [Problem to be solved by the invention]
[0009] The present invention has been made in view of the above-mentioned circumstances, and provides a YAG:Ce luminescent material having a high internal quantum yield and emitting warm-color fluorescence. 3+ The object of the present invention is to provide a phosphor. [Means for solving the problem]
[0010] In order to achieve the above object, the phosphor according to the present invention is Y 3-x Ce x Al 5-y-z Mg y Zr z O 12 A phosphor that is a single crystal having a garnet-type crystal structure represented by The x is 0.03 to 0.15, The y is 0.05 to 0.6, The z is 0.05 to 0.6.
[0011] The phosphor of the present invention is a YAG:Ce phosphor that has a high internal quantum yield and emits warm colors. 3+ The phosphor according to the present invention is a Ce:YAG phosphor. Here, "warm color fluorescence" refers to fluorescence whose fluorescence emission spectrum has a peak wavelength in the range of 550 to 570 nm. Since the phosphor according to the present invention is a Ce:YAG phosphor, it has good temperature quenching resistance.
[0012] Preferably, the x is in the range of 0.06 to 0.12, the y is in the range of 0.1 to 0.6, and the z is in the range of 0.1 to 0.6.
[0013] This results in a peak wavelength of the fluorescent emission spectrum of 553.0 to 565.0 nm.
[0014] Preferably, the half-width of the peak in the excitation light absorption spectrum is 110 nm or less.
[0015] This makes it possible to suppress concentration quenching, and therefore to suppress a decrease in the internal quantum yield.
[0016] The light emitting device according to the present invention comprises a blue light emitting element and the phosphor.
[0017] According to the light emitting device of the present invention, the projected light, which is a mixture of blue light from the blue light emitting element and warm fluorescent light from the phosphor, has an incandescent color.
[0018] The blue light emitting element may be a blue laser light source. According to the light emitting device of the present invention, even if a blue laser light source is used for the blue light emitting element, thermal quenching can be suppressed, so that the fluorescent light can maintain a warm color, and the projected light, which is a mixture of blue light and warm fluorescent light, can be made to have an incandescent color. [Brief description of the drawings]
[0019] [Figure 1] FIG. 1 is a schematic cross-sectional view of a light emitting device according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view of an apparatus for producing a phosphor according to one embodiment of the present invention. [Diagram 3] FIG. 3 is a schematic cross-sectional view of a light emitting device according to another embodiment of the present invention. [Figure 4] FIG. 4 is a graph relating to Example 1. [Diagram 5] FIG. 5 is a graph relating to Comparative Example 1. [Figure 6] FIG. 6 is a graph showing the relationship between the amount of cerium added and the peak wavelength of the fluorescent emission spectrum. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] [ First embodiment ] < Light-emitting device > As shown in FIG. 1, a light emitting device 2 according to this embodiment is a reflective light emitting device, and includes a phosphor 4 and a blue light emitting element 6. The light emitting device 2 is a reflective light emitting device.
[0021] The reflection-type light-emitting device 2 has the advantage that high brightness can be easily obtained since the reflection surface 44 side can be effectively used for heat dissipation.
[0022] < Blue light emitting element > 1, the blue light emitting element 6 emits blue light LB, which is excitation light for exciting the fluorescent component of the phosphor 4. The blue light LB from the blue light emitting element 6 usually has a peak wavelength of 425 nm to 500 nm. A part of the blue light LB that enters the phosphor 4 from the incident surface 42 is absorbed by the phosphor 4 and undergoes wavelength conversion, resulting in the emission of fluorescence.
[0023] Incidentally, the incident surface 42 of the phosphor 4 is the surface of the phosphor 4 facing the blue light emitting element 6, and in this embodiment, the incident surface 42 is also the exit surface. The reflective surface 44 of the phosphor 4 is the surface on the opposite side of the phosphor 4 from the blue light emitting element 6 side, and faces the incident surface 42. In other words, the incident surface 42 and the reflective surface 44 are substantially parallel. Incidentally, "substantially parallel" means that they may have some portions that are not parallel.
[0024] Blue light LB is incident on the incident surface 42, and fluorescence is emitted in all directions starting from the irradiation position of the blue light LB. A part of the blue light LB that has not been wavelength-converted undergoes surface scattering at the irradiation position of the blue light LB, and the blue light LB is emitted in all directions starting from the irradiation position of the blue light LB (Lambertian light distribution). The fluorescence and blue light LB emitted from the exit surface (incident surface) 42 toward the outside of the phosphor 4 are mixed to emit light L of an incandescent color. Note that if the color temperature is, for example, in the range of 2500 to 3500 K, and preferably in the range of 2700 to 3000 K, it can be determined that the color is incandescent.
[0025] The blue light-emitting element 6 is not particularly limited as long as it can emit blue light LB that can be mixed with fluorescence to emit incandescent light L and can be wavelength-converted to fluorescence by the phosphor 4, but examples of the blue light-emitting element 6 include a blue light-emitting diode (blue LED) or a blue semiconductor laser (blue laser, blue LD).
[0026] < Phosphor > The phosphor 4 according to this embodiment is a single crystal having a garnet-type crystal structure. The shape of the phosphor 4 is not particularly limited and may be, for example, a disk shape, a flat plate shape, or a rectangular column shape, and has a pair of mutually opposing surfaces that function as an incident surface 42 or a reflecting surface 44.
[0027] The size of phosphor 4 is not particularly limited. For example, if phosphor 4 has a flat plate shape, the width direction (X0) is 1 to 10 mm, the depth direction is 1 to 10 mm, and the thickness direction (Y0) is 0.03 to 1 mm.
[0028] The chemical formula of phosphor 4 is Y 3-x Ce x Al 5-y-z Mg y Zr z O 12 It is.
[0029] The value of x is 0.03 to 0.15, and preferably 0.06 to 0.12.
[0030] The value of y is in the range of 0.05 to 0.6, and preferably in the range of 0.1 to 0.6.
[0031] The value of z is from 0.05 to 0.6, and preferably from 0.1 to 0.6.
[0032] The concentration of each component in the phosphor 4 can be measured by laser ablation inductively coupled plasma mass spectrometry (LA-ICP-MS), an electron probe microanalyzer (EPMA), an energy dispersive spectrometer (EDX), or the like.
[0033] Phosphor 4 emits warm color fluorescence of red, orange, and yellow. The peak wavelength of the fluorescence emission spectrum of phosphor 4 is preferably 550 to 570 nm, and more preferably 553 to 565 nm. The peak wavelength of the fluorescence emission spectrum is the wavelength at which the intensity is maximum in the fluorescence emission spectrum.
[0034] The half width of the peak in the excitation light absorption spectrum of the phosphor 4 is preferably 110 nm or less, and more preferably 70 to 90 nm. The peak in the excitation light absorption spectrum is the maximum value of the intensity of the excitation light absorption spectrum.
[0035] < Phosphor manufacturing method > The phosphor 4 according to this embodiment is not particularly limited, and can be obtained by, for example, the micro-pulling down method (μ-PD method), the Czochralski method (CZ method), the Bridgman method, or the Edge-defined Film-fed Growth method (EFG method).
[0036] The μ-PD method makes it easier to adjust the composition in the single crystal to the above range compared to the conventional CZ method and the like. In addition, the μ-PD method can distribute the activator uniformly, so that concentration quenching can be suppressed. For this reason, it is preferable that the phosphor 4 according to this embodiment is a single crystal produced by the μ-PD method.
[0037] 2 shows a schematic cross-sectional view of a single crystal manufacturing apparatus 22 using the μ-PD method. The μ-PD method is a melting and solidification method. Specifically, in the μ-PD method, a crucible 24 containing a sample is heated directly or indirectly to obtain a melt of the target substance in the crucible 24, and a seed crystal 34 placed below the crucible 24 is brought into contact with the opening at the bottom end of the crucible 24, where a solid-liquid interface is formed, and the seed crystal 34 is pulled down to grow a single crystal.
[0038] 2, single crystal manufacturing apparatus 22 for manufacturing phosphor 4 according to this embodiment includes crucible 24 installed with its opening facing downward and refractory furnace 26 surrounding it. Refractory furnace 26 is further covered with quartz tube 28, and induction heating coil 30 for heating crucible 24 is installed near the center of quartz tube 28 in the vertical direction.
[0039] A seed crystal 34 held by a seed crystal holding jig 32 is placed at the opening of the crucible 24. An after-heater 36 is placed near the opening of the crucible 4 to prevent rapid cooling.
[0040] A single crystal cut into a rod shape is used as the seed crystal 34. The seed crystal 34 is preferably a single crystal that does not contain any additives.
[0041] Next, a method for producing the phosphor 4 according to this embodiment will be specifically described.
[0042] First, the raw materials for the single crystal, Y2O3, Al2O3, CeO2, MgO and ZrO2, are placed in the crucible 24 inside the refractory furnace 26, and the atmosphere inside the furnace is replaced with a gas such as H2+N2, N2 or argon (Ar).
[0043] Next, inert gas is pumped at 10 to 100 cm 3 1 / min, the crucible 24 is heated by an induction heating coil (high frequency coil for heating) 30 to melt the raw materials and obtain a molten liquid.
[0044] When the raw material is sufficiently melted, a seed crystal 34 is gradually brought closer to the bottom of the crucible 24 until the seed crystal 34 comes into contact with the opening at the bottom of the crucible 24. When the melt comes out of the opening at the bottom of the crucible 24, the seed crystal 34 is lowered to start crystal growth. The speed at which the seed crystal 34 is lowered here is called the growth speed.
[0045] The growth rate and temperature can be controlled manually while observing the state of the solid-liquid interface with a CCD camera or a thermo camera.
[0046] The temperature gradient can be selected in the range of 10 to 100° C. / mm by moving the induction heating coil 30. The single crystal growth speed can also be selected in the range of 0.01 to 0.20 mm / min.
[0047] The seed crystal 34 is lowered until the melt in the crucible 24 stops flowing out, and after the seed crystal 34 is separated from the crucible 24, the single crystal is cooled so as not to crack. The cooling rate of the single crystal varies depending on the growth rate and can be selected, for example, within the range of 70 to 300°C / hour.
[0048] The obtained single crystal is cut to a desired size. In this way, a garnet-type crystal structure having the chemical formula Y 3-x Ce x Al 5-y-z Mg y Zr z O 12 It is possible to obtain a single crystal phosphor having the above formula:
[0049] The phosphor 4 according to this embodiment has a high internal quantum yield, emits warm-colored fluorescence, and has good temperature quenching resistance. The reasons for this are considered to be as follows.
[0050] When cerium is added to YAG, the peak wavelength of the fluorescence emission spectrum shifts to the longer wavelength side. However, cerium, which has a large ionic radius, has difficulty entering the crystal lattice of YAG, which has a garnet-type crystal structure, when x is 0.03 or more, so the amount of shift of the peak wavelength of the fluorescence emission spectrum to the longer wavelength side is limited.
[0051] In contrast, in this embodiment, magnesium and zirconium expand the Al sites (a sites) of the YAG crystal lattice, making it easier for cerium to enter the Y sites (c sites). Then, by introducing cerium with x of 0.03 or more into the YAG crystal lattice, the peak wavelength of the fluorescence emission spectrum can be significantly shifted to the long wavelength side.
[0052] In this manner, in this embodiment, by setting x, y, and z within the above ranges, the peak wavelength of the fluorescent emission spectrum can be shifted to the longer wavelength side, making it possible to emit warm-colored fluorescent light.
[0053] In this embodiment, the Al sites of the YAG crystal lattice are replaced with zirconium and magnesium. When the Al sites are replaced with zirconium and magnesium, the peak of the excitation light absorption spectrum becomes sharp and the half-width becomes narrow. Furthermore, when the material is rapidly crystallized by a single crystal growth method such as the μ-PD method, the added elements such as cerium are less likely to segregate, and the half-width of the peak of the excitation light absorption spectrum becomes narrow.
[0054] When the half-width of the peak of the excitation light absorption spectrum is narrowed, the overlapping portion between the excitation light absorption spectrum and the fluorescence emission spectrum is reduced, so that self-absorption is reduced and concentration quenching can be suppressed. In particular, when the half-width of the peak of the excitation light absorption spectrum is 110 nm or less, concentration quenching is further suppressed and the decrease in the internal quantum yield can be further suppressed.
[0055] As a phosphor that emits warm-colored fluorescence, for example, Y3Al5O 12 :Ce 3+ and CaAlSiN3:Eu 2+ or Gd3Al5O 12 :Ce 3+ etc. are known.
[0056] However, CaAlSiN3:Eu 2+ Since the thermal quenching is significant, Y3Al5O 12 :Ce 3+ and CaAlSiN3:Eu 2+ When a phosphor containing these is irradiated with blue laser light, the red color disappears and it no longer emits warm colors.
[0057] Also, Gd3Al5O 12 :Ce 3+Since the amount of fluorescent light emitted by this compound is very small and it is subject to significant thermal quenching, it is difficult to use this compound in a phosphor that uses a blue laser as a light source.
[0058] In contrast, the phosphor 4 according to this embodiment is YAG:Ce 3+ According to the phosphor 4 of this embodiment, thermal quenching is suppressed even when a high-intensity blue laser beam is incident thereon, so that the phosphor 4 can maintain the emission of warm-colored fluorescent light even when the temperature of the phosphor 4 rises.
[0059] [ Second embodiment ] The light emitting device according to this embodiment is similar to the light emitting device 2 of the first embodiment, except as described below.
[0060] As shown in FIG. 3, a light emitting device 2a according to this embodiment is of a transmissive type.
[0061] In this embodiment, the emission surface 48 of the phosphor 4 is the surface of the phosphor 4 opposite to the blue light emitting element 6 side, and faces the incidence surface 42. In other words, the incidence surface 42 and the emission surface 48 are substantially parallel. Note that "substantially parallel" means that they may have some portions that are not parallel to each other.
[0062] Blue light LB is incident on the incident surface 42, and the fluorescent light emitted from the exit surface 48 toward the outside of the phosphor 4 is mixed with the blue light LB to emit projection light L with a warm white color.
[0063] The present invention is not limited to the above-described embodiment, and various modifications can be made within the scope of the present invention. EXAMPLES
[0064] The present invention will be described in more detail below by way of examples of the present invention, but the present invention is not limited to these examples.
[0065] < Examples 1 to 9, Comparative Examples 2 to 4 > As starting materials, Y2O3, Al2O3, CeO2, MgO, and ZrO2 were prepared, and Y2O3 was placed in an Ir crucible 24 with an inner diameter of 16 mm. 1.5 , AlO 1.5 2 g of Y2O3, Al2O3, CeO2, MgO and ZrO2 were added so that the composition ratios of CeO2, MgO and ZrO2 were as shown in Table 1.
[0066] The crucible 24 used had melt leakage ports arranged at the four corners.
[0067] The crucible 24 containing the starting materials was placed in a refractory furnace. The atmosphere in the refractory furnace 26 was replaced with N2 containing 3% H2, and gas was introduced at a rate of 50 cm3 while maintaining the pressure at normal pressure. 3 Flows were given as flow rate / min.
[0068] Thereafter, heating of the crucible 24 was started and gradually heated over one hour until the temperature reached the melting point of the YAG single crystal.
[0069] A YAG single crystal was used as the seed crystal 34, and the tip of the seed crystal 34 was brought into contact with the opening at the bottom of the crucible 24. After confirming that the melt had come out of the opening, crystal growth was started while lowering the seed crystal 34. At this time, the crystal growth was performed by changing the growth speed in the range of 0.01 to 0.20 mm / min for each sample.
[0070] During crystal growth, an after-heater 36 was installed below the crucible 24 in order to prevent rapid cooling.
[0071] The cooling rate of the crystal varies depending on the growth rate, and in this example was adjusted to be 70 to 300° C. / hour.
[0072] As a result of growing the single crystal, a columnar CeMgZr-substituted YAG single crystal (phosphor) with dimensions of 3×3 mm square and 65 mm length was obtained.
[0073] The diffraction peaks of phosphor 4 were confirmed by X-ray diffraction (XRD) using a fully automated multipurpose X-ray diffraction device SmartLab (manufactured by Rigaku Corporation), and it was determined that the sample was a single crystal because no heterophase components were contained and a (100) diffraction spot with three-fold rotational symmetry was observed by pole measurement at (100). As a result, it was confirmed that single crystals were generated in Examples 1 to 9 and Comparative Examples 2 to 4.
[0074] Furthermore, since garnet diffraction spots were observed by pole measurement, it was confirmed that Examples 1 to 9 and Comparative Examples 2 to 4 had a garnet-type crystal structure.
[0075] The columnar single crystal was cut perpendicularly to the length direction with a wire saw, and a plate-shaped phosphor 4 of 2×2×0.5 mm was obtained from the center.
[0076] ( Composition analysis ) When the central portion of the obtained plate-like phosphor 4 was analyzed for composition by LA-ICP, it was confirmed that the phosphor had the composition shown in Table 1.
[0077] The laser ablation device used for LA-ICP was NWR213 (manufactured by Japan Laser Co., Ltd.), and the ICP mass spectrometry was performed using Agilent8900 (manufactured by Agilent Technologies, Inc.).
[0078] ( Peak wavelength of the fluorescence emission spectrum, peak half-width of the excitation light absorption spectrum, and internal quantum yield ratio ) The incident surface 42 of phosphor 4 was roughened by cutting. The peak wavelength of the fluorescent emission spectrum, the peak half width of the excitation light absorption spectrum, and the internal quantum yield were measured using a fluorescence spectrophotometer. The measurement results of the peak wavelength of the fluorescent emission spectrum and the peak half width of the excitation light absorption spectrum are shown in Table 1. The internal quantum yield ratio was calculated by the following method. The relative internal quantum yield ratio was calculated by using the highest internal quantum yield of Example 4 as the denominator and the internal quantum yield of phosphor 4 produced in each Example as the numerator. The results are shown in Table 1.
[0079] ( Projected light color ) A blue laser beam with an output of 1 W was incident on phosphor 4 at an incident angle of 45°, and the color temperature of the light projected perpendicularly from the laser beam projection surface of phosphor 4 was measured with a color temperature meter. In Example 1, the color temperature was 3500 K, which is the color of an incandescent bulb. In Examples 2 to 9, the projected light also had the color temperature of an incandescent bulb.
[0080] < Comparative Example 1 > The starting materials were prepared as Y2O3, Al2O3, CeO2, MgO and ZrO2. 1.5 , AlO 1.5 , CeO2, MgO and ZrO2 were weighed and mixed to obtain the composition ratio shown in Table 1. The mixed powder was press-molded into a disk shape of 10 mmΦ and 1 mm thick, and reduced and fired at 1650°C in an N2 atmosphere containing 3% H2 to produce a ceramic phosphor. The surface corresponding to the incident surface 42 and the surface corresponding to the reflective surface 44 were polished to produce a phosphor with a thickness of 0.5 mm.
[0081] The resulting phosphor was subjected to composition analysis and the peak wavelength of the fluorescent emission spectrum, the peak half width of the excitation light absorption spectrum, and the internal quantum yield ratio were measured in the same manner as in Examples 1 to 9 and Comparative Examples 2 to 4. The results are shown in Table 1.
[0082] < Comparative Example 5 > YO 1.5 , AlO 1.5 An attempt was made to grow a single crystal in the same manner as in Examples 1 to 9 and Comparative Examples 2 to 4, except that the compositions of CeO2, MgO, and ZrO2 were as shown in Table 1, but a different phase was mixed in and a single crystal could not be grown. It is believed that the single crystal could not be grown because the concentrations of MgO and ZrO2 were too high, resulting in the appearance of a different phase.
[0083] < Comparative Example 6 > YO 1.5 , AlO 1.5A phosphor was produced in the same manner as in Comparative Example 1, except that a powder of CeO2, MgO and ZrO2 was weighed and mixed so as to have the composition ratio shown in Table 1, and the powder was press-molded into a disk shape of 10 mmΦ and 1 mm thickness, and fired at 1650°C in air. The composition of the obtained phosphor was analyzed in the same manner as in Examples 1 to 9 and Comparative Examples 2 to 4, and the peak wavelength of the fluorescent emission spectrum and the peak half-width of the excitation light absorption spectrum were measured, and the internal quantum yield ratio was calculated. The results are shown in Table 1.
[0084] < Comparative Example 7 > The various inorganic raw materials were weighed and mixed to produce a raw material with a composition of SiO2 20.0 mol%, Al2O3 5.0 mol%, B2O3 28.0 mol%, Na2O 5.0 mol%, K2O 5.0 mol%, CaO 8.0 mol%, BaO 4.0 mol%, and ZnO 25.0 mol%. The raw materials were placed in a platinum crucible and heated and melted at 1100 to 1300°C in an electric furnace for 1 to 2 hours to obtain a glass sample.
[0085] The glass sample was then shaped into flakes using a quenching twin roll molding machine. Yellow phosphor powder (3% by mass) and red phosphor powder (1% by mass) were added to the flake-shaped glass material and mixed to obtain a mixed powder (phosphor content: 4% by mass).
[0086] The yellow phosphor has the chemical formula Y 2.98 Ce 0.02 Al 5.00 O 12 The powder had a composition of yttrium, aluminum, and cerium (central fluorescent emission wavelength: 532 nm), and was a ceramic powder produced by weighing, mixing, and firing (1600°C, 3% H2-containing N2 atmosphere) oxide powders of yttrium, aluminum, and cerium.
[0087] The red phosphor has the chemical formula CaAlSiN3:Eu 2+ (fluorescence emission central wavelength 650 nm) powder.
[0088] Next, the molded body was pressurized in a mold to produce a disk-shaped body with a diameter of 10 mm and a thickness of 1 mm, and then heated in air for 30 minutes to obtain a sintered body. Furthermore, the surface corresponding to the incident surface 42 and the surface corresponding to the reflecting surface 44 were polished to produce a phosphor with a thickness of 0.5 mm.
[0089] The resulting phosphor was subjected to composition analysis, the peak wavelength of the fluorescent emission spectrum was measured, and the internal quantum efficiency ratio was calculated in the same manner as in Examples 1 to 9 and Comparative Examples 2 to 4. The results are shown in Table 1.
[0090] In Comparative Example 7, the fluorescence emission spectrum had two maximum intensity values at 535.0 nm and 648.0 nm. The internal quantum yield ratio of Comparative Example 7 was 95.5%.
[0091] [Table 1]
[0092] From Table 1, Y 3-x Ce x Al 5-y-z Mg y Zr z O 12 It was confirmed that when the phosphor is a single crystal having a garnet-type crystal structure represented by the formula (1), where x is 0.03 to 0.15, y is 0.05 to 0.6, and z is 0.05 to 0.6, the internal quantum efficiency ratio exceeds 76.6% and the peak wavelength of the fluorescence emission spectrum is 550 to 570 nm.
[0093] The internal quantum yield ratio in Comparative Example 1 was a low value of 76.6%, which is believed to be due to concentration quenching.
[0094] Since the peak wavelength of the fluorescence emission spectrum of Comparative Example 2 is 538.8 nm, it cannot be said that the peak wavelength of the fluorescence emission spectrum has shifted to the longer wavelength side.
[0095] The internal quantum efficiency ratio of Comparative Example 3 was a low value of 74.9%, which is believed to be due to concentration quenching.
[0096] The internal quantum efficiency ratio of Comparative Example 4 was a low value of 78.0%, which is believed to be due to concentration quenching.
[0097] The peak wavelength of the fluorescence in Comparative Example 6 was 529.0 nm, and the peak wavelength of the fluorescence emission spectrum was closer to the short wavelength side, closer to blue.
[0098] When the color temperature of the projected light was measured for the phosphor of Comparative Example 7 in the same manner as in Examples 1 to 9 and Comparative Examples 2 to 4, the light was about 6500K daylight color, and was not a light bulb color with a red color mixed in. In Comparative Example 7, it is believed that the laser light was incident on the phosphor, causing it to become hot, and the red phosphor was quenched by temperature.
[0099] Fig. 4 relates to Example 1, and Fig. 5 relates to Comparative Example 1. The X-axis in Fig. 4 and Fig. 5 is wavelength (unit: nm), the Y-axis is normalized intensity, the solid line indicates the fluorescence emission spectrum, and the dashed line indicates the excitation light absorption spectrum.
[0100] The peak of the excitation light absorption spectrum in FIG. 4 is sharper than that in FIG. 5. This is believed to be because, in Example 1 (FIG. 4), the Al sites of the YAG crystal lattice are substituted with zirconium and magnesium. When the peak of the excitation light absorption spectrum becomes sharper and the half-width becomes narrower, the overlapping portion between the excitation light absorption spectrum and the fluorescent emission spectrum decreases, so that self-absorption decreases and concentration quenching can be suppressed. As a result, it is believed that the decrease in the internal quantum yield can be further suppressed.
[0101] < Comparative Examples 11 to 16 > As starting materials, Y2O3, Al2O3 and CeO2 were prepared, and phosphors were obtained and the peak wavelengths of the fluorescent emission spectra were measured in the same manner as in Examples 1 to 9 and Comparative Examples 2 to 4, except that the amount of cerium added was changed as shown in Table 1. The results are shown in Table 2.
[0102] Also, Table 3 is shown below. Examples 1 to 3, 7 and 9 in Table 3 are the same samples as Examples 1 to 3, 7 and 9 above.
[0103] [Table 2]
[0104] [Table 3]
[0105] FIG. 6 relates to each sample in Tables 2 and 3. The X-axis of FIG. 6 is Y 3-x Ce x AlO 12 or Y 3-x Ce x Al 4.2 Mg 0.4 Zr 0.4 O 12 The x value is the amount of cerium added, and the Y axis is the peak wavelength of the fluorescence emission spectrum (unit: nm). 3-x Ce x Al 4.2 Mg 0.4 Zr 0.4 O 12 For each sample in Table 3, which is represented by the chemical formula 3-x Ce x AlO 12 The respective samples in Table 2 are represented by the chemical formula:
[0106] From Figure 6, Y 3-x Ce x Al 4.2 Mg 0.4 Zr 0.4 O 12 Each sample in Table 3 is represented by the chemical formula Y 3-x Ce x AlO 12 It was confirmed that the peak wavelength of the fluorescence emission spectrum was longer than that of each sample in Table 2 represented by the chemical formula: and that the increase in the peak wavelength of the fluorescence emission spectrum with the addition of cerium was also large. [Explanation of symbols]
[0107] 2… Light source device 4. Phosphor 42…Incidence plane 44… Reflective surface 48… Exit surface 6... Blue light emitting element, blue laser light source 22... Single crystal manufacturing equipment 24… Crucible 26… Refractory furnace 28…Quartz tube 30… Induction heating coil 32… Seed crystal holding jig 34… Seed crystal 36... After heater LB: Excitation light, blue light, blue laser light L… Projection light
Claims
1. Y 3-x C x A 5-y-z Mg y Zr z O 12 A phosphor that is a single crystal having a garnet-type crystal structure represented by The x is 0.03 to 0.15, The y is 0.05 to 0.6, The phosphor wherein z is 0.05 to 0.
6.
2. The x is 0.06 to 0.12, The y is 0.1 to 0.6, 2. The phosphor according to claim 1, wherein z is 0.1 to 0.
6.
3. 2. The phosphor according to claim 1, wherein the half-width of the peak of the excitation light absorption spectrum is 110 nm or less.
4. A light emitting device comprising: a blue light emitting element; and the phosphor according to any one of claims 1 to 3.
5. The light emitting device according to claim 4 , wherein the blue light emitting element is a blue laser light source.