Method of joining dissimilar metallic materials and dissimilar-metal joined structure

The method of using a joining auxiliary member with limited contact areas effectively joins dissimilar metals, addressing shape and thickness limitations and preventing damage during welding, ensuring high-quality bonding.

JP2024145996AActive Publication Date: 2024-10-15KOBE STEEL LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023058650
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

Conventional methods for joining dissimilar metal materials, such as steel and low-melting point materials like resin, face challenges including increased manufacturing steps, limited shape and thickness constraints, and damage to low-melting point materials during welding.

Method used

A method involving a joining auxiliary member with a flange and shaft inserted into a through hole of the low-melting point material, where the auxiliary member and material contact only at specific partial areas, minimizing heat transfer and using arc welding to form a weld metal with the same components as the high-strength material.

Benefits of technology

Enables high-quality joining of dissimilar metals without damaging the low-melting point material, allowing for efficient bonding while maintaining structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145996000001_ABST
    Figure 2024145996000001_ABST
Patent Text Reader

Abstract

To provide a method of joining dissimilar metallic materials capable of easily joining different kinds of materials with high quality, especially capable of joining even members one of which is composed of a material having a low melting point without damaging the member.SOLUTION: The method of joining dissimilar metallic materials includes: a base metal arrangement step of arranging a CFRP plate (second member) 2 having a first through-hole 2a on a steel plate (first member) 1; a joining auxiliary member arrangement step of inserting a joining auxiliary member 3 having a second through-hole 3a into the first through-hole 2a; and a joining step of forming a weld metal 8 in the second through-hole 3a by arc-welding to join the joining auxiliary member 3 and the steel plate 1. In the joining auxiliary member arrangement step, a first partial contact region 6 in which the CFRP plate 2 and a flange part 4 of the joining auxiliary member 3 are in point or line contact with each other and a second partial contact region 7 in which the inner side surface of the first through-hole 2a and the shaft part 5 are in point or line contact with each other are formed, and the joining auxiliary member 3 is not brought into contact with the CFRP plate 2 in other regions.SELECTED DRAWING: Figure 1C
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for joining dissimilar metal materials, which is capable of joining plate materials made of different materials with high strength, and to a dissimilar metal joined structure joined by the joining method. [Background technology]

[0002] For transportation equipment, such as automobiles, there is a constant demand for improving fuel efficiency in order to reduce (1) the consumption of petroleum fuel, which is a limited resource, (2) the greenhouse gas CO2 generated by combustion, and (3) driving costs. As a means to achieve this, in addition to improving power system technologies such as the use of electric drive, weight reduction of the vehicle body is also one of the improvement measures. One way to reduce weight is to replace steel, which is currently the main material, with lightweight materials such as aluminum or aluminum alloys, magnesium or magnesium alloys, carbon fiber, resin, and carbon fiber reinforced plastics (CFRP). However, replacing everything with these lightweight materials has issues such as high costs and insufficient strength, and as a solution, a design method called multi-material, which combines steel and lightweight materials in the right places, is attracting attention.

[0003] Incidentally, Patent Document 1 discloses a joining structure in which, for example, a steel material and a non-ferrous metal material that is difficult to weld to the steel material are joined. In the joining structure, a first material having a protruding portion and being a first homogeneous metal material, and a third material having a protruding portion and being a second homogeneous metal material are arranged so that the protruding portions face each other, and a second material having a through portion and being a dissimilar material is sandwiched between them, and the protruding portions are fused and joined to each other. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 6811380 Summary of the Invention [Problem to be solved by the invention]

[0005] However, in order to form the joining structure described in the above Patent Document 1, it is necessary to form a protrusion on the third material that is the lower plate, which increases the number of manufacturing steps and limits the shape of the lower plate. In addition, the above Patent Document 1 also describes a structure in which a protrusion is not formed, but when this method is used, the thicknesses of the first material, the second material, and the third material are also limited. Furthermore, when a low-melting-point material such as resin is selected as the second material of the dissimilar materials, a problem occurs in that the second material is damaged by heat during welding. Such a problem also occurs with conventional welding methods using rivets. Therefore, a method for joining a high-strength member such as steel and a member made of a low-melting-point material such as resin without causing damage has not yet been established.

[0006] The present invention has been made in consideration of such problems, and has an object to provide a method for joining dissimilar metal materials, which can easily join dissimilar materials with high quality, and in particular can join dissimilar metal materials without damaging them, even if one of the materials is made of a material with a low melting point, and a joined structure of dissimilar metal materials joined by the above-mentioned joining method. [Means for solving the problem]

[0007] The above object of the present invention can be achieved by the following configuration [1] or [2] relating to a method for joining dissimilar metal materials.

[0008] [1] A base material arrangement process for arranging a plate-shaped second member on a first member, the second member being made of a material different from that of the first member and having a first through hole penetrating in a plate thickness direction; a joining auxiliary member placement step of inserting a joining auxiliary member having a second through hole and having the same main component as the first member into the first through hole; a joining step of melting at least a part of the first member and at least a part of the joining auxiliary member through the second through hole by arc welding, and forming a weld metal having the same main component as the first member, the joining auxiliary member includes a flange portion disposed on a surface of the second member opposite to a contact surface with the first member, and a shaft portion inserted into the first through hole, a first partial contact region where the second member and the flange portion contact at a point or a line, and a second partial contact region where the inner surface of the first through hole and the shaft portion contact at a point or a line, are formed in the joining auxiliary member positioning process, and the joining auxiliary member is not brought into contact with the second member in a region other than the first partial contact region and the second partial contact region.

[0009] [2] A base material arrangement process of arranging a plate-shaped second member on a first member, the second member being made of a material different from that of the first member and having a first through hole penetrating in a plate thickness direction; a joining auxiliary member placement step of inserting a joining auxiliary member having a second through hole and having the same main component as the first member into the first through hole; a joining step of melting at least a part of the first member and at least a part of the joining auxiliary member through the second through hole by arc welding, and forming a weld metal having the same main component as the first member, the joining auxiliary member includes a flange portion disposed on a surface of the second member opposite to a contact surface with the first member, and a shaft portion inserted into the first through hole, a first partial contact area in which the second member and the flange portion are in contact at a point or a line in the joining auxiliary member positioning process, and the joining auxiliary member is not in contact with the second member in an area other than the first partial contact area.

[0010] Further, preferred embodiments of the present invention relating to a method for joining dissimilar metal materials relate to the following [3] to [7].

[0011] [3] The method for joining dissimilar metal materials described in [1] or [2], characterized in that the melting point of the material constituting the second member is lower than the melting point of the material constituting the first member.

[0012] [4] The method for joining dissimilar metal materials according to any one of [1] to [3], wherein the second member is made of resin.

[0013] [5] The method for joining dissimilar metal materials according to any one of [1] to [4], wherein the thermal conductivity of the joining auxiliary member is lower than the thermal conductivity of the first member.

[0014] [6] The method for joining dissimilar metal materials described in any one of [1] to [5], characterized in that the outer diameter of the shaft portion of the joining auxiliary member has a tapered shape that becomes smaller from the end portion on the flange portion side toward the other end portion.

[0015] [7] The method for joining dissimilar metal materials described in any one of [1] to [6], characterized in that the inner diameter of the second through hole in the joining auxiliary member has a tapered shape that becomes smaller from the end on the flange portion side toward the other end.

[0016] The above object of the present invention can be achieved by the following configuration [8] or [9] relating to a dissimilar metal bonded structure.

[0017] [8] A first member; a second member disposed on a surface perpendicular to a thickness direction of the first member, made of a material different from that of the first member, and having a first through hole; a joining auxiliary member having a shaft portion and a flange portion and a second through hole parallel to the axial direction of the shaft portion, the shaft portion being inserted into the first through hole; a weld metal formed inside the second through hole and including a molten portion in which at least a part of the first member and at least a part of the joining auxiliary member are melted, the joining auxiliary member and the weld metal each have the same main component as the first member, and the first member and the second member are joined by the joining auxiliary member and the weld metal, A dissimilar metal joint structure, characterized in that a first partial contact region where the second member and the flange portion are in contact at a point or line, and a second partial contact region where the inner surface of the first through hole and the shaft portion are in contact at a point or line, are formed, and the joining auxiliary member and the second member are not in contact in regions other than the first partial contact region and the second partial contact region.

[0018] [9] A first member; a second member disposed on the first member, made of a material different from that of the first member, and having a first through hole; a joining auxiliary member having a shaft portion and a flange portion and a second through hole parallel to the axial direction of the shaft portion, the shaft portion being inserted into the first through hole; a weld metal formed inside the second through hole and including a molten portion in which at least a part of the first member and at least a part of the joining auxiliary member are melted, the joining auxiliary member and the weld metal each have the same main component as the first member, and the first member and the second member are joined by the joining auxiliary member and the weld metal, A dissimilar metal joint structure, characterized in that a first partial contact area is formed in which the second member and the flange portion are in contact at a point or line, and the joining auxiliary member and the second member are not in contact in areas other than the first partial contact area. Effect of the Invention

[0019] According to the present invention, it is possible to provide a method for joining dissimilar metal materials, which can easily join dissimilar materials with high quality, and in particular, can join even components made of a material with a low melting point without damaging them, and a joined structure of dissimilar metal materials joined by the above-mentioned joining method. [Brief description of the drawings]

[0020] [Figure 1A] FIG. 1A is a diagram showing a method for joining dissimilar metal materials according to a first embodiment of the present invention, and is a cross-sectional view showing a base material arrangement step. [Figure 1B] FIG. 1B is a cross-sectional view showing the method for joining dissimilar metal materials according to the first embodiment of the present invention, illustrating a joining auxiliary member arranging step. [Figure 1C] FIG. 1C is a cross-sectional view showing a dissimilar metal joint structure obtained by the method for joining dissimilar metal materials according to the first embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing a joining method for dissimilar metal materials according to a second embodiment of the present invention, illustrating a joining auxiliary member arranging step. [Diagram 3] FIG. 3 is a schematic diagram showing the size of the auxiliary joining members used in the examples. [Figure 4A] FIG. 4A is a photograph, substituted for a drawing, showing a cross section of a dissimilar metal joint structure produced by the method for joining dissimilar metal materials of an example. [Figure 4B] FIG. 4B is a photograph showing an enlarged view of the flange portion shown in FIG. 4A. [Figure 5A] FIG. 5A is a photograph showing a cross section of a dissimilar metal joint structure produced by a method for joining dissimilar metal materials of a comparative example. [Figure 5B] FIG. 5B is a photograph showing an enlarged view of the flange portion shown in FIG. 5A. [Figure 6A] FIG. 6A is a photograph showing an enlarged view of region (a) in FIG. 5A. [Figure 6B] FIG. 6B is a photograph showing an enlarged view of region (b) in FIG. 5A. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] The inventors of the present application have conducted various studies into the causes of damage to the low-melting-point member when joining dissimilar metal materials, particularly when one of the members has a low melting point. First, a method using a general rivet was used in which an upper plate made of resin was placed on a lower plate made of steel, a steel auxiliary joining member was inserted into a hole formed in the upper plate, and the auxiliary joining member and the lower plate were joined by arc welding. As a result, the inventors of the present application found that the arc heat during arc welding is thermally conducted to the upper plate via the auxiliary joining member, damaging the upper plate, which has a low melting point, and causing poor joining. In other words, by reducing the joining area between the auxiliary joining member and the upper plate as much as possible and performing welding with the auxiliary joining member positioned so as not to conduct the arc heat to the upper plate, damage to the upper plate can be prevented and high-quality joining can be achieved. The present invention was made based on these findings.

[0022] Hereinafter, an embodiment of the present invention (hereinafter, referred to as "the present embodiment") will be described in detail with reference to the drawings. Note that the present invention is not limited to the embodiment described below, and can be modified and implemented as desired without departing from the gist of the present invention.

[0023] [Method of joining dissimilar metal materials] (First embodiment) 1A to 1C are cross-sectional views showing a method for joining dissimilar metal materials according to a first embodiment of the present invention in the order of steps. Note that the embodiment shown below is a method for joining a steel plate (first member) 1 and a CFRP plate (second member) 2 by element arc spot welding.

[0024] <Base material placement process> 1A, a first through hole 2a penetrating through the CFRP plate 2 in the plate thickness direction is formed at a position to be joined to the steel plate 1. Next, the CFRP plate 2 is placed on a surface of the steel plate 1 perpendicular to the plate thickness direction.

[0025] <Joining auxiliary parts placement process> Thereafter, as shown in FIG. 1B, a steel joint auxiliary member 3 is inserted into the first through hole 2a. The joint auxiliary member 3 has a disk-shaped flange portion 4 and a shaft portion 5 having an axis in the same axial direction as the central axis of the disk. The joint auxiliary member 3 also has a second through hole 3a that penetrates in the same axial direction as the shaft portion 5. Note that inserting the joint auxiliary member 3 into the first through hole 2a means inserting the shaft portion 5 of the joint auxiliary member 3 into the first through hole 2a, and at this time, the flange portion 4 is disposed on the surface of the CFRP plate 2 opposite to the contact surface with the steel plate 1, i.e., on the upper surface 2b.

[0026] In this embodiment, the flange portion 4 of the joining auxiliary member 3 is inclined toward the shaft portion 5 as it approaches the radial end. The outer diameter Do of the shaft portion 5 is formed so as to become smaller from the flange portion 4 side toward the other end, forming a tapered shape. Similarly, the inner diameter Di of the second through hole 3a in the joining auxiliary member 3 is also formed so as to become smaller from the end on the flange portion 4 side toward the other end, forming a tapered shape.

[0027] Therefore, in this embodiment, when the joining auxiliary member 3 is inserted into the first through hole 2a, the upper surface 2b of the CFRP plate 2 and the outer diameter side end of the flange portion 4 come into line contact along the circumferential direction of the flange portion 4, forming a first partial contact region 6. Also, the end of the inner circumferential surface of the first through hole 2a on the upper surface 2b side of the CFRP plate 2 and the shaft portion 5 of the joining auxiliary member 3 come into line contact along the circumferential direction of the shaft portion 5, forming a second partial contact region 7. Thus, in the joining auxiliary member arranging step, the joining auxiliary member 3 is not brought into contact with the CFRP plate 2 in areas other than the first partial contact region 6 and the second partial contact region 7, and is arranged so that a gap portion 9 is formed.

[0028] <Joining process> 1C , at least a part of the steel plate 1 and at least a part of the auxiliary joining member 3 are melted by arc welding through the second through hole 3a, and a welding wire (not shown) is melted to form a weld metal 8. Since the auxiliary joining member 3 and the steel plate 1 are joined by the weld metal 8, the auxiliary joining member 3 and the welding wire are made of materials that can be joined to the steel plate 1, i.e., have the same main components as the steel plate 1.

[0029] According to the joining method of this embodiment, the auxiliary joining member 3, the steel plate 1, and the weld metal 8 all have the same main components, and are therefore firmly fixed together by welding. Furthermore, the CFRP plate 2 is physically fixed to the steel plate 1 by the flange portion 4 of the auxiliary joining member 3. Therefore, a dissimilar metal joined structure 10 in which the steel plate 1 and the CFRP plate 2 are joined together can be obtained.

[0030] In this embodiment, the auxiliary joining member 3 and the CFRP plate 2 are in contact only at the first partial contact region 6 and the second partial contact region 7, and the contact region is extremely small, so that damage to the CFRP plate 2 due to heat conduction during welding can be suppressed. Furthermore, the inner diameter portion of the second through hole 3a in the auxiliary joining member 3 is formed in a tapered shape, so that the auxiliary joining member 3 and the steel plate 1 can be joined with only a small amount of weld metal. Therefore, the amount of heat during welding can be further reduced, and damage to the CFRP plate 2 can be further suppressed. As a result, dissimilar materials can be easily joined with high quality.

[0031] Second embodiment A method for joining dissimilar metal materials according to a second embodiment of the present invention will be described below with reference to Fig. 2. In the second embodiment, since the contact area between the joining auxiliary member 3 and the CFRP plate 2 is different from that in the first embodiment, Fig. 2 is shown instead of Fig. 1B, and drawings showing other steps are omitted.

[0032] <Base material placement process> As in the first embodiment, a CFRP plate 2 having a first through hole 2a is placed on a surface perpendicular to the thickness direction of a steel plate 1. As shown in Fig. 2, in the second embodiment, an annular groove 22 for positioning a joining auxiliary member 3 is provided on an upper surface 2b of the CFRP plate 2 radially outward of the first through hole 2a.

[0033] <Joining auxiliary parts placement process> Next, the steel joint auxiliary member 3 is inserted into the first through hole 2a. As in the first embodiment, the joint auxiliary member 3 has a disk-shaped flange portion 4 and a shaft portion 5, and is formed with a second through hole 3a. The flange portion 4 of the joint auxiliary member 3 is inclined toward the shaft portion 5 as it approaches its radial end. However, the outer diameter of the shaft portion 5 and the inner diameter of the second through hole 3a are formed to be the same size from the flange portion 4 side toward the other end.

[0034] In the second embodiment, when the joining auxiliary member 3 is inserted into the first through hole 2a, the outer diameter side end of the lower surface of the flange portion 4 fits into the groove 22 of the CFRP plate 2, and the joining auxiliary member 3 is positioned. At this time, the flange portion 4 of the joining auxiliary member 3 and the CFRP plate 2 come into line contact in the circumferential direction in the area where the groove 22 is formed, and first partial contact areas 26a, 26b are formed, but the shaft portion 5 of the joining auxiliary member 3 and the CFRP plate 2 do not come into contact, and a gap portion 9 is formed.

[0035] <Joining process> Thereafter, at least a part of the steel plate 1 and at least a part of the joining auxiliary member 3 are melted through the second through hole 3a by arc welding, and a welding wire (not shown) is melted to form a weld metal 8 as in FIG. 1C.

[0036] The joining method according to the second embodiment also makes it possible to obtain a dissimilar metal joined structure in which a steel plate 1 and a CFRP plate 2 are joined. In this embodiment, the joining auxiliary member 3 and the CFRP plate 2 are in contact only at the first partial contact regions 26a, 26b, which are extremely small, and the first partial contact regions 26a, 26b are separated from the region to which high welding heat is applied, so that damage to the CFRP plate 2 due to heat conduction during welding can be further suppressed. As a result, dissimilar materials can be easily joined with high quality.

[0037] The method for positioning the auxiliary joining member 3 is not limited to the method of forming the groove 22 in the CFRP plate 2, and various methods can be used, such as using other members or devices. In the second embodiment, two first partial contact regions 26a, 26b are formed, but the number of first partial contact regions where the flange portion 4 and the CFRP plate 2 come into contact may be one or three or more, as long as they are in contact at a point or a line. In this embodiment, the shape of the shaft portion 5 of the auxiliary joining member 3 does not need to be formed to have the same size from the flange portion 4 side to the other end, and may be tapered as in the first embodiment.

[0038] In the above first and second embodiments, an example has been shown in which a steel plate 1 is used as the first member, a CFRP plate 2 is used as the second member, and a steel auxiliary joining member 3 is used, but the present invention is not limited to such a combination. The first member and the auxiliary joining member 3 may be made of various metal materials. Specifically, steel, aluminum, magnesium, etc. may be used as the material for the first member. Also, specifically, steel, aluminum, magnesium, etc. may be used as the material for the auxiliary joining member 3.

[0039] The present invention has an effect of preventing damage to the second member even when a material having a low melting point is used. Therefore, by using a material having a lower melting point than the material of the first member as the material constituting the second member, the effect of the present invention can be fully exhibited. For example, aluminum die-cast, resin, etc. can be used as the material of the second member. In order to further exhibit the effect of the present invention, it is more preferable to select a resin as the material of the second member, and it is even more preferable to use a carbon fiber reinforced plastic (CFRP) among resins, which is lightweight and has excellent strength.

[0040] It is more preferable that the auxiliary joining member 3 is made of a material having a lower thermal conductivity than the first member. If the auxiliary joining member 3 has a low thermal conductivity, the amount of heat generated during welding is less likely to be transmitted to the auxiliary joining member 3, thereby reducing the thermal effect on the second member and further suppressing the occurrence of damage.

[0041] In addition, in the present invention, the shape of the joining auxiliary member 3 is not particularly limited. The outer shape of the shaft portion 5 does not need to be a tapered shape that becomes smaller toward the lower end. As shown in the first embodiment, the outer diameter of the shaft portion 5 can be designed so that the shaft portion 5 and the inner circumferential surface of the first through hole 2a of the CFRP plate 2 contact each other at a point or line. For example, a protrusion may be formed on the outer circumferential surface of the shaft portion 5 of the joining auxiliary member 3, and the protrusion may be brought into contact with the first through hole 2a. Also, as shown in the second embodiment, the shaft portion 5 of the joining auxiliary member 3 does not need to be in contact with the CFRP plate 2.

[0042] The flange portion 4 of the joining auxiliary member 3 is not limited to the inclined shape shown in Figures 1B and 2, and a protrusion may be formed on the surface of the flange portion 4 facing the second member so that the protrusion comes into contact with the second member, or the protrusion may be formed so as to fit into a groove.

[0043] The second through hole 3a formed in the joint auxiliary member 3 does not need to have a tapered shape that becomes smaller toward the lower end, but as described above, a smaller inner diameter of the second through hole 3a can prevent damage to the CFRP plate caused by heat during welding. On the other hand, if the inner diameter of the second through hole 3a is too small, the weld metal 8 shown in Fig. 1C becomes small, which may reduce the joint strength. Therefore, it is preferable to select the size and shape of the inner diameter of the second through hole 3a depending on the material constituting the second member and the required joint strength.

[0044] Furthermore, the shape of the first member does not have to be plate-like, and various shapes can be used. As for the shape of the second member, it is preferable that the joint portion with the first member is plate-like, but it can be freely selected from shapes that are partially bent, shapes that have partially different thicknesses, and the like. In other words, in the present specification, the "plate-like second member" may be one in which only the joint portion is plate-like.

[0045] In the present specification, "contact at a point or a line" means that the flange portion 4 and the shaft portion 5 of the joining auxiliary member 3 and the second member are in contact with each other substantially in a point shape or a line shape. Specifically, it is necessary to make the two members contact each other over a smaller area than when the flange portion 4 of the joining auxiliary member 3 is in complete contact with the upper surface of the second member or when the shaft portion 5 of the joining auxiliary member 3 is in complete contact with the inner circumferential surface of the first through hole 2a of the second member. For example, in this embodiment, the total area of ​​the first partial contact region 6 is preferably 30% or less, more preferably 10% or less, of the area when the flange portion 4 is in complete contact with the upper surface of the second member. In addition, the area of ​​the second partial contact region 7 is preferably 30% or less, more preferably 10% or less, of the area when the shaft portion 5 is in complete contact with the inner circumferential surface of the first through hole 2a of the second member.

[0046] The first partial contact region 6 and the first partial contact regions 26a, 26b, and the second partial contact region 7 may each include a plurality of point contact portions and line contact portions. In the case of line contact, the contact does not necessarily have to be continuous in the circumferential direction of the flange portion 4 or the shaft portion 5, and there may be partial non-contact regions or a mixture of point contact portions and line contact portions.

[0047] Next, a dissimilar metal joint structure joined by the method for joining dissimilar metal materials according to the present embodiment will be described.

[0048] [Dissimilar metal bonded structure] (First embodiment) The dissimilar metal joint structure according to the first embodiment can be manufactured, for example, by the method for joining dissimilar metal materials according to the first embodiment. As shown in FIG. 1C, the dissimilar metal joint structure 10 according to the first embodiment has a first member (steel plate 1), a plate-shaped second member (CFRP plate 2), a joint auxiliary member 3, and a weld metal 8. The second member is made of a material different from that of the first member and is arranged on top of the first member. The second member has a first through hole 2a penetrating in the plate thickness direction. The joint auxiliary member 3 has a shaft portion 5 and a flange portion 4, and has a second through hole 3a parallel to the axial direction of the shaft portion 5, and the shaft portion 5 is inserted into the first through hole 2a. The weld metal 8 is formed inside the second through hole 3a and includes a molten portion in which at least a part of the first member and at least a part of the joint auxiliary member 3 are melted. The auxiliary joining member 3 and the weld metal 8 each have the same main components as the first member, and the first member and the second member are joined together by the auxiliary joining member and the weld metal.

[0049] In this embodiment, the dissimilar metal bonded structure 10 is formed with a first partial contact region 6 where the second member and the flange portion 4 contact at a point or line, and a second partial contact region 7 where the inner circumferential surface of the first through hole 2a and the shaft portion 5 contact at a point or line. In regions other than the first partial contact region 6 and the second partial contact region 7, the bonding auxiliary member 3 and the second member are not in contact with each other.

[0050] Second embodiment The dissimilar metal joint structure according to the second embodiment can be manufactured by, for example, the method for joining dissimilar metal materials according to the second embodiment. In the second embodiment, the description of the same parts as those in the first embodiment will be omitted or simplified. Note that FIG. 2 is a diagram showing a dissimilar metal joint structure according to the second embodiment in the middle of its manufacture, and the configuration of the second embodiment will be described with reference to FIG. 2. In the dissimilar metal joint structure according to the second embodiment, first partial contact regions 26a, 26b are formed in which the CFRP plate 2 and the flange portion 4 are in contact at a point or line. In addition, in the region other than the first partial contact regions 26a, 26b, the joining auxiliary member 3 and the CFRP plate 2 are not in contact. In addition, in the dissimilar metal joint structure according to the second embodiment, a weld metal (not shown) is formed inside the second through hole 3a, similar to the dissimilar metal joint structure 10 according to the first embodiment shown in FIG. 1C, and the steel plate 1 and the CFRP plate 2 are joined by this weld metal and the joining auxiliary member 3.

[0051] The dissimilar metal bonded structure according to the first and second embodiments configured in this manner has an excellent appearance and the desired strength because damage to the second member (CFRP plate 2) due to welding heat is suppressed during the manufacturing process. EXAMPLES

[0052] Examples of the method for joining dissimilar metal materials according to this embodiment will be specifically described below in comparison with comparative examples.

[0053] <Example> As shown in FIG. 1A to FIG. 1C, a CFRP plate 2 having a first through hole 2a was placed on the upper surface of a steel plate 1, and a shaft portion 5 of a joining auxiliary member 3 having a second through hole 3a was inserted into the first through hole 2a. At this time, the shape of the joining auxiliary member 3 was designed so that the flange portion 4 of the joining auxiliary member 3 and the CFRP plate 2 were in line contact along the outer peripheral surface of the flange portion 4, and the shaft portion 5 and the inner peripheral surface of the first through hole 2a of the CFRP plate 2 were in line contact along this inner peripheral surface. After that, a part of the steel plate 1 and a part of the joining auxiliary member 3 were melted by arc spot welding to form a weld metal 8 in the second through hole 3a, thereby joining the steel plate 1 and the CFRP plate 2. The shape and size of the joining auxiliary member used in the examples are shown in FIG. 3 and will be described below. Other welding conditions are also shown below.

[0054] (Size of auxiliary joining parts) Outer diameter of flange part 4 Df: 11 mm Inner diameter of second through hole 3a (end portion on the flange portion side) Di1: 6 mm Inner diameter (other end) Di2 of the second through hole 3a: 4 mm Outer diameter of shaft 5 (end on flange side) Do1: 7 mm Outer diameter (other end) of shaft portion 5 Do2: 6 mm Inclination angle of the outer peripheral surface of the shaft portion 5 (angle with respect to the vertical direction) θ: 21° Inclination of flange portion 4 (height difference from the boundary between the bottom surface of flange portion 4 and the outer peripheral surface of shaft portion 5 to the radial end of the bottom surface of flange portion 4) Hf: 0.2 mm Thickness of flange part 4 (thickness of radial end) T: 1.2 mm Axial height He of auxiliary joining member 3: 2.6 mm Axial height Hs of the inclined portion of the shaft portion 5: 1.1 mm

[0055] (Other welding conditions) Steel plate 1 material and thickness: 980MPa grade steel plate, 1.4mm Thickness of CFRP plate 2: 2.0 mm Diameter of the first through hole 2a: 7.0 mm Material of auxiliary joint part 3: Mild steel Welding wire type / wire diameter: JIS Z3312G59J3M1T, 1.2mm Shielding gas type and flow rate: 80% Ar + 20% CO2, 25 liters / min Welding current / voltage: 120A, 23V Arc Time: 0.8 seconds

[0056] <Comparative Example> In the same manner as in the above-mentioned embodiment, the steel plate 1 and the CFRP plate 2 were arranged, and the shaft portion 5 of the joining auxiliary member 3 was inserted into the first through hole 2a. However, the joining auxiliary member 3 used in the comparative example had no inclination of the flange portion 4 and no tapered shape of the shaft portion, and was arranged so that the flange portion 4 and the upper surface of the CFRP plate 2, and the shaft portion 5 and the inner surface of the first through hole 2a of the CFRP plate 2 were in surface contact. Thereafter, arc spot welding was performed in the same manner as in the above-mentioned embodiment, and a part of the steel plate 1 and a part of the joining auxiliary member 3 were melted, and a weld metal was formed to join the steel plate 1 and the CFRP plate 2. Some of the sizes of the joining auxiliary member 3 used in the comparative example are shown below. Other sizes and welding conditions were the same as in the embodiment.

[0057] (Size of auxiliary joining parts) Inner diameter Di of second through hole 3a: 6.0 mm Outer diameter Do of shaft portion 5: 7.0 mm The inner diameter Di of the second through hole 3a and the outer diameter Do of the shaft portion 5 are both the same size from the end on the flange portion side to the other end.

[0058] FIG. 4A is a drawing substitute photograph showing a cross section of a dissimilar metal joint structure manufactured by the joining method of dissimilar metal materials of the embodiment, and FIG. 4B is a drawing substitute photograph showing an enlarged view of the flange portion. In FIG. 4A and FIG. 4B, the same parts as those in FIG. 1C are given the same reference numerals, and detailed explanations thereof are omitted or simplified. As shown in FIG. 4A, in the embodiment, the joining auxiliary member 3 and the CFRP plate 2 are in contact only at the first partial contact region 6 and the second partial contact region 7, and are not in contact at other parts. Therefore, the steel plate 1 and the CFRP plate 2 could be joined without damaging the CFRP plate 2. Also, as shown in FIG. 4B, no damage to the CFRP plate 2 was observed when observing the upper surface of the dissimilar metal joint structure.

[0059] Fig. 5A is a drawing substitute photograph showing a cross section of a dissimilar metal joint structure manufactured by a comparative example of a method for joining dissimilar metal materials, and Fig. 5B is a drawing substitute photograph showing an enlarged view of the flange portion. Fig. 6A is a drawing substitute photograph showing an enlarged view of region (a) in Fig. 5A, and Fig. 6B is a drawing substitute photograph showing an enlarged view of region (b) in Fig. 5A. In the comparative example, the shape of the joint auxiliary member is different from that of the embodiment, but the configurations of the flange portion and the shaft portion are similar. Therefore, in Figs. 5A and 5B, the same reference numerals are used for the same parts as those in Figs. 4A and 4B, and detailed descriptions thereof will be omitted or simplified.

[0060] In the comparative example, the joining auxiliary member 3 and the CFRP plate 2 were joined in a state where they were in surface contact at least in part. However, as shown in FIG. 5A, the weld metal 8 and the joining auxiliary member 3 were not completely joined, and an unjoined portion 14 was formed. As shown in FIG. 5B, no damage was found in the CFRP plate 2 when the upper surface of the dissimilar metal joined structure of the comparative example was observed. Also, as shown in FIG. 6A, in the region (a) separated from the joining auxiliary member 3, a first layer 11 in which a plurality of fibers are arranged in the left-right direction inside the CFRP plate 2 and a second layer 12 in which a plurality of fibers are arranged in the direction perpendicular to the left-right direction are alternately laminated, and no damage was observed.

[0061] However, as shown in FIG. 6B, in the comparative example, even though the input heat was only enough to form an unbonded portion 14, a partially melted damaged portion 13 was observed in the region (b) close to the auxiliary bonding member 3.

[0062] In this way, it was shown that by using the method for joining dissimilar metal materials of the embodiment, it is possible to join the lower plate (first member) and the upper plate with high quality without damaging the upper plate, even if the upper plate (second member) is formed from a material with a low melting point such as resin. [Explanation of symbols]

[0063] 1 Steel plate (first member) 2 CFRP plate (second member) 2a First through hole 3. Joining auxiliary parts 3a Second through hole 4 Flange 5 Shaft section 6 1st partial contact area 7 Second partial contact area 8 Welding metal 9 Cavity 10 Dissimilar metal bonded structure 13 Damaged area

Claims

1. a base material arrangement step of arranging a plate-shaped second member on a first member, the second member being made of a material different from that of the first member and having a first through hole penetrating in a plate thickness direction; a joining auxiliary member arrangement step of inserting a joining auxiliary member having a second through hole and having the same main component as the first member into the first through hole; a joining step of melting at least a part of the first member and at least a part of the joining auxiliary member through the second through hole by arc welding, and forming a weld metal having the same main component as the first member, the joining auxiliary member includes a flange portion disposed on a surface of the second member opposite to a contact surface with the first member, and a shaft portion inserted into the first through hole, a first partial contact region where the second member and the flange portion contact at a point or a line, and a second partial contact region where the inner surface of the first through hole and the shaft portion contact at a point or a line, wherein the joining auxiliary member is not brought into contact with the second member in a region other than the first partial contact region and the second partial contact region, in the joining auxiliary member positioning process.

2. a base material arrangement step of arranging a plate-shaped second member on a first member, the second member being made of a material different from that of the first member and having a first through hole penetrating in a plate thickness direction; a joining auxiliary member arrangement step of inserting a joining auxiliary member having a second through hole and having the same main component as the first member into the first through hole; a joining step of melting at least a part of the first member and at least a part of the joining auxiliary member through the second through hole by arc welding, and forming a weld metal having the same main component as the first member, the joining auxiliary member includes a flange portion disposed on a surface of the second member opposite to a contact surface with the first member, and a shaft portion inserted into the first through hole, a first partial contact area in which the second member and the flange portion are in contact at a point or a line in the joining auxiliary member positioning process, and the joining auxiliary member is not in contact with the second member in an area other than the first partial contact area.

3. 3. The method for joining dissimilar metal materials according to claim 1, wherein a melting point of the material constituting the second member is lower than a melting point of the material constituting the first member.

4. 3. The method for joining dissimilar metal materials according to claim 1, wherein the second member is made of resin.

5. 3. The method for joining dissimilar metal materials according to claim 1, wherein the thermal conductivity of the joining auxiliary member is lower than the thermal conductivity of the first member.

6. 3. The method for joining dissimilar metal materials according to claim 1, wherein the outer diameter of the shaft portion of the joining auxiliary member has a tapered shape that decreases from the end portion on the flange portion side toward the other end portion.

7. 3. The method for joining dissimilar metal materials according to claim 1 or 2, characterized in that an inner diameter of the second through hole in the joining auxiliary member has a tapered shape that becomes smaller from the end on the flange portion side toward the other end.

8. A first member; a second member disposed on the first member, the second member being made of a different material than the first member, and having a first through hole; a joining auxiliary member having a shaft portion and a flange portion and a second through hole parallel to the axial direction of the shaft portion, the shaft portion being inserted into the first through hole; a weld metal formed inside the second through hole and including a molten portion in which at least a part of the first member and at least a part of the joining auxiliary member are melted, a dissimilar metal joint structure in which the joining auxiliary member and the weld metal each have the same main component as the first member, and the first member and the second member are joined by the joining auxiliary member and the weld metal, a first partial contact region where the second member and the flange portion are in contact at a point or a line, and a second partial contact region where the inner surface of the first through hole and the shaft portion are in contact at a point or a line, and the joining auxiliary member and the second member are not in contact in a region other than the first partial contact region and the second partial contact region.

9. A first member; a second member disposed on the first member, the second member being made of a different material than the first member, and having a first through hole; a joining auxiliary member having a shaft portion and a flange portion and a second through hole parallel to the axial direction of the shaft portion, the shaft portion being inserted into the first through hole; a weld metal formed inside the second through hole and including a molten portion in which at least a part of the first member and at least a part of the joining auxiliary member are melted, a dissimilar metal joint structure in which the joining auxiliary member and the weld metal each have the same main component as the first member, and the first member and the second member are joined by the joining auxiliary member and the weld metal, A dissimilar metal joint structure, characterized in that a first partial contact area is formed in which the second member and the flange portion are in contact at a point or a line, and the joining auxiliary member and the second member are not in contact in an area other than the first partial contact area.

Citation Information

Patent Citations

  • Arc-welding method for joining dissimilar material, joint auxiliary member and dissimilar material welding coupling

    JP2018047477A

  • Dissimilar material jointing spot welding method, joint auxiliary member, and dissimilar material welding coupling

    JP2018051570A

  • Heterogeneous member joining method

    JP2018089657A

  • Piercing metal for joining dissimilar material and dissimilar material joining method with use of piercing metal

    JP2020185602A

  • Joint structure

    JP6811380B2