Decorative sheet and decorative member
A decorative sheet with a polyvinyl chloride-based structure and ultraviolet absorbers enhances processing suitability by preventing cracks and whitening, ensuring durability and recyclability.
Patent Information
- Application Number
- JP2023058870
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Decorative sheets formed from polyolefin resin suffer from low processing suitability, leading to issues such as cracks and whitening at corners when wrapped around building materials.
A decorative sheet comprising a base layer of colored polyvinyl chloride resin, a pattern layer, a transparent resin layer with a benzotriazole-based or triazine-based ultraviolet absorber, and a surface protection layer with a triazine-based ultraviolet absorber and light stabilizer, with specific mechanical properties to enhance processing suitability.
The decorative sheet improves processing suitability by reducing corner cracking and whitening, maintaining ultraviolet absorption over time, and enabling easy handling and recycling.
Smart Images

Figure 2024146139000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a decorative sheet and a decorative member that are used, for example, as building materials for exterior use. [Background technology]
[0002] As a technique relating to a decorative sheet, for example, there is a technique disclosed in Patent Document 1. In the technology disclosed in Patent Document 1, liposomes formed by supercritical reverse phase evaporation so as to encapsulate a carbon dioxide absorbent and a crystal nucleating agent for a polyolefin-based resin are added to a polyolefin-based resin to produce a resin composition. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 6060451 Summary of the Invention [Problem to be solved by the invention]
[0004] In the technology disclosed in Patent Document 1, a decorative sheet is formed using a polyolefin resin. This results in low processability, and for example, when wrapping a building material with the decorative sheet, there is a problem that cracks, whitening, etc. occur at the corners of the part wrapped with the decorative sheet. The present invention has been made in view of the above-mentioned problems, and has an object to provide a decorative sheet and a decorative member that are capable of improving processability. [Means for solving the problem]
[0005] In order to solve the above problems, one aspect of the present invention is a decorative sheet comprising a base layer, a pattern layer, a transparent resin layer, and a surface protective layer. The base layer is a layer formed using a colored polyvinyl chloride resin. The pattern layer is a layer laminated on one side of the base layer. The transparent resin layer is a layer laminated on one side of the pattern layer and formed using a transparent polyvinyl chloride resin. The surface protective layer is a layer laminated on one side of the transparent resin layer. The yield strength is in the range of 8 MPa to 70 MPa, and the whitening initiation elongation is 3% or more. In order to solve the above problems, one aspect of the present invention is a decorative member comprising a decorative sheet and a substrate disposed on the other surface side of the base layer. Effect of the Invention
[0006] According to one aspect of the present invention, it is possible to provide a decorative sheet and a decorative member that are capable of improving processability. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a cross-sectional view showing a decorative sheet according to a first embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing the decorative member of the first embodiment. [Diagram 3] FIG. 4 is a cross-sectional view showing a decorative sheet in a modified example of the first embodiment. [Figure 4] FIG. 4 is a cross-sectional view showing a decorative member in a modified example of the first embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] A first embodiment of the present invention will be described below with reference to the drawings. In the drawings referred to in the following description, the same or similar parts are denoted by the same or similar reference numerals. However, it should be noted that the drawings are schematic, and the relationship between thickness and planar dimensions, the thickness ratio of each layer, etc., are different from the actual ones. Therefore, the specific thickness and dimensions should be determined with reference to the following description. In addition, it goes without saying that the drawings include parts with different dimensional relationships and ratios.
[0009] Furthermore, the first embodiment shown below is an example of a configuration for embodying the technical idea of the present invention, and the technical idea of the present invention does not specify the materials of the components, their shapes, structures, arrangements, etc., as described below. The technical idea of the present invention can be modified in various ways within the technical scope defined by the claims. In addition, the directions of "left and right" and "up and down" in the following explanation are merely defined for the convenience of explanation and do not limit the technical idea of the present invention. Therefore, for example, if the paper is rotated 90 degrees, "left and right" and "up and down" are read interchangeably, and of course, if the paper is rotated 180 degrees, "left" becomes "right" and "right" becomes "left".
[0010] First embodiment Hereinafter, a first embodiment of the present invention will be described with reference to the drawings. (Composition of decorative sheet) The structure of the decorative sheet 1 will be described with reference to FIG. As shown in FIG. 1, the decorative sheet 1 comprises a base layer 2, a design layer 4, a transparent resin layer 6, and a surface protective layer 8.
[0011] The total thickness of the base layer 2 and the transparent resin layer 6 is, for example, within a range of 90 μm to 310 μm. This makes it possible to suppress the deterioration of heat-shielding properties compared to when the sum of the thickness of the base layer 2 and the thickness of the transparent resin layer 6 is less than 90 μm or exceeds 310 μm. In the first embodiment, as an example, a case will be described in which the total thickness of the base layer 2 and the transparent resin layer 6 is within a range of 120 μm to 200 μm. This makes it possible to suppress the deterioration of heat insulation properties compared to when the sum of the thickness of the base layer 2 and the thickness of the transparent resin layer 6 is less than 120 μm or exceeds 200 μm.
[0012] (base material layer) The base layer 2 is formed using a colored polyvinyl chloride resin. In addition, the base layer 2 contains an inorganic material. The inorganic material contained in the base layer 2 is at least one of calcium carbonate, titanium oxide, silica, chromium, antimony, carbon black, and a titanium composite.
[0013] (Picture layer) The pattern layer 4 is a layer that imparts a pattern to the decorative sheet 1, and is laminated on one surface of the base layer 2 (the upper surface in FIG. 1). There are no particular restrictions on the type of pattern formed by the pattern layer 4, and for example, wood grain patterns, stone patterns, fabric patterns, abstract patterns, geometric figures, letters, symbols, etc. may be formed alone or in combination of two or more types. The design layer 4 is formed using a black pigment that is an organic pigment (for example, perylene black) or a black pigment that is an inorganic pigment (for example, carbon black).
[0014] The design layer 4 is formed using at least one pigment selected from the group consisting of isoindolinone, disazo, polyazo, diketopyrrolopyrrole, quinacridone, phthalocyanine, and titanium oxide. The binder resin contained in the design layer 4 is not particularly limited, but it is preferable to use a resin with good adhesion. Therefore, it is preferable to use a resin that has thermal adhesion to polyvinyl chloride resin, such as a vinyl chloride-vinyl acetate copolymer, an acrylic resin alone or a mixture thereof, etc.
[0015] (Transparent resin layer) The transparent resin layer 6 is laminated on one surface of the design layer 4 (the upper surface in FIG. 1). The transparent resin layer 6 is made of a transparent polyvinyl chloride resin. As the transparent polyvinyl chloride resin, for example, "vinyl chloride, vinyl chloride-vinyl acetate copolymer, ethylene-vinyl chloride copolymer, vinyl chloride-acrylic resin" can be used, but it is preferable to use a vinyl chloride resin alone with a polymerization degree of 500 to 3000. The transparent polyvinyl chloride resin forming the transparent resin layer 6 contains a benzotriazole-based or triazine-based ultraviolet absorbing agent.
[0016] (Surface protective layer) The surface protective layer 8 is a layer provided to impart functions such as weather resistance, scratch resistance, stain resistance, and design properties to the decorative sheet 1, and is laminated on one side of the transparent resin layer 6 (the upper side in Figure 1). The material constituting the surface protective layer 8 is not particularly limited, and can be appropriately selected from, for example, urethane-based, acrylic-based, acrylic silicone-based, fluorine-based, epoxy-based, and other resin materials. Note that the surface protective layer 8 may contain various additives, such as a heat stabilizer, an antiblocking agent, a catalyst capture agent, a colorant, a light scattering agent, and a gloss adjuster, as necessary. Moreover, the surface protective layer 8 contains a triazine-based ultraviolet absorbing agent and a light stabilizer.
[0017] <Triazine-based UV absorbers> As the triazine-based ultraviolet absorbent, for example, a hydroxyphenyltriazine-based ultraviolet absorbent is used. By using a hydroxyphenyltriazine-based ultraviolet absorbent, the triazine skeleton suppresses bleeding, and the triazine skeleton is chemically stable compared to the skeletons of benzotriazole-based ultraviolet absorbents and benzophenone-based ultraviolet absorbents, making it possible to maintain ultraviolet absorption performance for a long period of time.
[0018] Examples of hydroxyphenyltriazine-based ultraviolet absorbers include 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[2-(2-ethylhexanoyloxy)ethoxy]phenol, 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine, 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[(hexyl)oxy]phenol, 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-ethyl-hexanoic acid, 2-[4-(4,6-diphenyl-[1,3,5]triazin-2-yl) -3-hydroxy-phenoxy]-ethyl ester, octanoic acid, 2-[4-(4,6-diphenyl-[1,3,5]triazin-2-yl)-3-hydroxy-phenoxy]-ethyl ester, 2,4,6-tris{2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)}-1,3,5-triazine, 2,4-bis(2-hydroxy-4-butyloxyphenyl)-6-(2,4-bis-butyloxyphenyl)-1,3,5-triazine, 2,4-bis(2,4-dimethylphenyl)-6-(2-hydroxy-4-iso-octyloxyphenyl)-s-triazine, 2,4-bis(2-hydroxy-4-butyloxyphenyl)-6-(2,4-bis-butyloxyphenyl)-1,3,5-triazine, and the like.
[0019] In the first embodiment, 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine (hereinafter, for convenience, referred to as "ultraviolet absorber A") may be contained in the surface protective layer 8. Note that 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine, which is the ultraviolet absorber A, is generally known as the main component of "Tinuvin 479: manufactured by BASF Japan Ltd."
[0020] In the first embodiment, the amount of the hydroxyphenyltriazine-based ultraviolet absorber is preferably in the range of 1 part by mass to 30 parts by mass with respect to 100 parts by mass of the acrylic resin composition. By setting the amount of the ultraviolet absorber to 1 part by mass or more, the effect of improving weather resistance is exhibited, and by setting the amount to 30 parts by mass or less, it is possible to suppress the influence on physical properties other than the weather resistance of the surface protective layer 8 to a level that does not cause practical problems.
[0021] In particular, when ultraviolet absorber A is used as the ultraviolet absorber added to the surface protective layer 8, the amount of ultraviolet absorber A added is preferably in the range of 1 part by mass to 20 parts by mass, more preferably in the range of 5 parts by mass to 15 parts by mass, and even more preferably in the range of 8 parts by mass to 12 parts by mass, relative to 100 parts by mass of the acrylic resin composition. By setting the amount of ultraviolet absorber A to 1 part by mass or more, an effect of improving weather resistance is exhibited, and by setting it to 20 parts by mass or less, it is possible to suppress the influence on physical properties other than the weather resistance of the surface protective layer 8 to a level that does not cause practical problems.
[0022] In the first embodiment, by using the ultraviolet absorber A and 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[2-(2-ethylhexanoyloxy)ethoxy]phenol (hereinafter, for convenience, referred to as "ultraviolet absorber B") in combination as a hydroxyphenyltriazine ultraviolet absorber, it is possible to impart even better weather resistance. This is because the ultraviolet absorber B has a high ultraviolet absorption capacity in the short wavelength region, which is relatively high energy among ultraviolet rays, and is chemically stable compared to other ultraviolet absorbers that absorb in approximately the same wavelength region, and therefore the wavelength region in which ultraviolet rays are absorbed is broadened by using them in combination. The ultraviolet absorber B, 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[2-(2-ethylhexanoyloxy)ethoxy]phenol, is commonly known as the main component of "ADEKA STAB LA-46: manufactured by ADEKA Corporation."
[0023] In the first embodiment, the amount of ultraviolet absorber A added is preferably in the range of 10 parts by mass to 200 parts by mass, more preferably in the range of 20 parts by mass to 100 parts by mass, and even more preferably in the range of 40 parts by mass to 80 parts by mass, relative to 100 parts by mass of ultraviolet absorber B. By setting the amount of ultraviolet absorber A added within the above numerical range, it is possible to impart even better weather resistance.
[0024] (Example of surface protection layer) An example of the configuration of the surface protective layer 8 will be described below with reference to a specific example. The surface protection layer 8 may be mainly composed of an acrylic resin composition containing, for example, cyclohexyl (meth)acrylate as a monomer component. Here, cyclohexyl (meth)acrylate means cyclohexyl acrylate or cyclohexyl methacrylate. By containing cyclohexyl (meth)acrylate as a monomer component, it is possible to reduce affinity for water, and it is possible to suppress deterioration due to hydrolysis and the like.
[0025] The content of cyclohexyl (meth)acrylate is preferably within the range of 5 mass [%] or more and 50 mass [%] or less of the monomer components of the acrylic resin composition which is the main component of the surface protective layer 8. By making the content of cyclohexyl (meth)acrylate 5 mass [%] or more, it is possible to obtain a sufficient deterioration suppression effect. In addition, by making the content of cyclohexyl (meth)acrylate 50 mass [%] or less, it is possible to impart high weather resistance over time without significantly changing the performance of the surface protective layer 8, such as improving the maintenance of surface hardness, improving the stain resistance, and adjusting the surface gloss. Here, the above-mentioned "main component" means that the content of the acrylic resin composition which constitutes the surface protective layer 8 is 50 mass [%] or more with respect to the mass of the entire surface protective layer 8.
[0026] Examples of monomer components of the acrylic resin composition that can be used for the surface protective layer 8 include, in addition to cyclohexyl(meth)acrylate, cyclohexylmethyl(meth)acrylate, cyclohexylethyl(meth)acrylate, cyclohexylpropyl(meth)acrylate, cyclohexylbutyl(meth)acrylate, dimethylcyclohexane mono(meth)acrylate, dimethylcyclohexane di(meth)acrylate, trimethylcyclohexane mono(meth)acrylate, trimethylcyclohexane di(meth)acrylate, trimethylcyclohexane tri(meth)acrylate, tetramethylcyclohexane mono(meth)acrylate, tetramethylcyclohexane di(meth)acrylate, tetramethylcyclohexane tri(meth)acrylate, tetramethylcyclohexane tetra(meth)acrylate, dicyclohexylmethyl(meth)acrylate, dicyclohexylmethyl(meth)acrylate, phenoxycyclohexylmethyl(meth)acrylate, methoxycyclohexylmethyl(meth)acrylate, and the like. Among these, those containing isomers may be at least one of each isomer alone and each isomer mixture.
[0027] The surface protective layer 8 may be formed by applying a coating liquid containing the above-mentioned acrylic resin composition containing cyclohexyl (meth)acrylate as a monomer component and a weathering agent such as an ultraviolet absorber described below, onto the outermost surface of the decorative sheet 1. For example, the surface protective layer 8 may be formed by applying a coating liquid containing the above-mentioned acrylic resin composition and a weathering agent to a transparent resin layer 6 having recesses 10 shown in Fig. 1, and then wiping the coating liquid to fill the recesses 10 with the coating liquid.
[0028] As a method for curing the coating liquid for forming the surface protective layer 8, for example, any of a one-component curing type, a two-component curing type using a curing agent, and an active energy ray curing type that is cured by irradiation with ultraviolet light, ionizing radiation, etc., can be used. In particular, in consideration of weather resistance, the two-component curing type or the active energy ray curing type is preferable, and in consideration of post-processability after being laminated to various substrates to become a decorative member, the two-component curing type that is crosslinked by isocyanate curing is desirable. Furthermore, by configuring the decorative sheet 1 in such a manner that recesses 10 are formed in the transparent resin layer 6 and the surface protection layer 8 as shown in FIG. 1, it is possible to provide an embossed design on the outermost surface of the decorative sheet 1.
[0029] As the two-component curing type acrylic resin composition, for example, a composition containing an acrylic resin having two or more functional groups selected from hydroxyl groups, amino groups, and carboxyl groups in one molecule, and a polyisocyanate compound having two or more isocyanate groups in one molecule that can react with the functional groups is preferred. Particularly preferred is a composition containing an acrylic polyol having two or more hydroxyl groups in one molecule, and a polyisocyanate compound.
[0030] As the acrylic polyol having two or more hydroxyl groups in one molecule, in addition to the above-mentioned cyclohexyl (meth)acrylate, for example, a (meth)acrylic acid ester copolymer containing hydroxyethyl (meth)acrylate as a monomer component can be used. On the other hand, as the polyisocyanate compound having two or more isocyanate groups in one molecule, for example, tolylene diisocyanate (TDI), 4,4'-diphenylmethane diisocyanate (MDI), xylylene diisocyanate (XDI) and hydrogenated compounds thereof, isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HDI), and trimer type, TMP adduct type, biuret type, etc., synthesized by a known technique using one or more compounds selected from these, can be mentioned.
[0031] It is also possible to use a composition in which one or more types selected from these different types of polyisocyanates are mixed. Among them, HDI, HDI trimer type, TMP adduct type, and biuret type are preferable from the viewpoint of weather resistance. The content of the isocyanate compound relative to the above-mentioned resin components can be set arbitrarily, but it is preferable to set the equivalent ratio of hydroxyl group / isocyanate group to about 1 / 1 to 1 / 3. In particular, if the equivalent of hydroxyl group is greater than the equivalent of isocyanate group, crosslinking may not proceed sufficiently, and the desired performance may not be imparted to the surface protective layer 8, which is not preferable.
[0032] When the coating liquid for forming the surface protective layer 8 is cured by active energy ray curing, known monomers, oligomers, etc. having a (meth)acryloyl group can be used as the active energy ray curable acrylic resin composition. In addition to the known monomers and oligomers having a (meth)acryloyl group, the above-mentioned cyclohexyl (meth)acrylate may be blended.
[0033] <Yield strength and whitening elongation of decorative sheets> The decorative sheet 1 has a yield strength in the range of 8 [Mpa] or more and 70 [Mpa] or less. This is because if the yield strength is less than 8 [Mpa], the decorative sheet 1 loses its stiffness (e.g., low rigidity) and becomes less easy to handle. In addition, if the yield strength exceeds 70 [Mpa], the decorative sheet 1 becomes too rigid, and is more likely to be damaged during processing, etc. In the first embodiment, a case will be described in which the yield strength of the decorative sheet 1 is within a range of 10 [Mpa] or more and 60 [Mpa] or less, as an example.
[0034] The whitening initiation elongation percentage of the decorative sheet 1 is 3% or more. This is because if the whitening initiation elongation rate is less than 3%, whitening will occur in the decorative sheet 1 even if the decorative sheet 1 is stretched even slightly, and the corners of the component wrapped with the decorative sheet 1 will quickly whiten. In the first embodiment, a case will be described where the whitening initiation elongation percentage of the decorative sheet 1 is 5% or more, as an example.
[0035] In addition, decorative sheet 1 having a yield strength exceeding 70 [Mpa] and a whitening initiation elongation rate of less than 3 [%] has been confirmed to crack and whiten in a cold impact resistance test based on the standard test method for brittle temperature of plastic sheets due to impact (ASTM D1790). The yield strength and whitening initiation elongation of the decorative sheet 1 are values measured in accordance with JIS K5602, for example. The measurement conditions for the yield strength and whitening elongation are, for example, a temperature of 20°C, a tensile speed of 50 mm / min, a chuck distance of 70 mm, and a gauge distance of 40 mm. In addition, the thickness of the test piece is 130 μm, and the width of the test piece is 10 mm.
[0036] Furthermore, the yield strength and whitening initiation elongation of the decorative sheet 1 are controlled by, for example, the amount of plasticizer added to the transparent resin layer 6. Examples of the plasticizer that can be used include phthalic acid, polyester, adipic acid, epoxy, and trimellitate.
[0037] The amount of plasticizer added is, for example, within the range of 8% (8 parts) to 35% (35 parts) relative to 100% (100 parts of transparent polyvinyl chloride resin). That is, the amount of plasticizer added is, for example, within the range of 8 PHR to 35 PHR. In the first embodiment, as an example, a case will be described in which the amount of plasticizer added to the transparent resin layer 6 is within a range of 12 [PHR] or more and 30 [PHR] or less.
[0038] (Composition of decorative parts) The configuration of the decorative member 100 will be described with reference to FIG. As shown in FIG. 2, the decorative member 100 is formed, for example, in a plate shape, and includes a decorative sheet 1, an adhesive layer 12, and a substrate 20. (adhesive layer) The adhesive layer 12 is laminated on the other surface of the base layer 2, for example, by applying a primer (undercoat) to the other surface of the base layer 2 (the lower surface in Figures 1 and 2).
[0039] (Board configuration) The substrate 20 is disposed on the other surface side of the base layer 2 of the decorative sheet 1, with the adhesive layer 12 sandwiched therebetween. The substrate 20 is made of a wood-based material or a metal-based material. Examples of wood-based materials that can be used include wooden veneer, plywood, laminated lumber, particle board, medium density fiberboard, and hard fiberboard. As the metallic material, a steel plate, a brass plate, an aluminum plate, a duralumin plate, a stainless steel plate, or the like can be used. Furthermore, the substrate 20 has a folded structure or a three-dimensional structure. When the decorative sheet 1 is laminated onto the substrate 20, it may be laminated via an appropriately selected adhesive as necessary, or it may be laminated directly without an adhesive or the like.
[0040] Methods for laminating and adhering the decorative sheet 1 to the substrate 20 include a method of pressing with a metal plate and a continuous lamination method using a circular pressure system. In particular, the continuous lamination method using an endless metal belt makes it possible to continuously produce, at high speed, a high-quality decorative member 100 that is free from surface warping or waviness, has good interlayer adhesion, and is densely cured and integrated. The decorative member 100 is formed, for example, by wrapping the substrate 20 with the decorative sheet 1.
[0041] The above-described first embodiment is one example of the present invention, and the present invention is not limited to the above-described first embodiment. Various modifications can be made depending on the design, etc., even in forms other than this embodiment, as long as they do not deviate from the technical idea of the present invention.
[0042] (Effects of the First Embodiment) The decorative sheet 1 of the first embodiment can achieve the effects described below. (1) The laminate comprises a base layer 2 formed using a colored polyvinyl chloride resin, a pattern layer 4 laminated on the base layer 2, a transparent resin layer 6 laminated on the pattern layer 4 and formed using a transparent polyvinyl chloride resin, and a surface protective layer 8 laminated on the transparent resin layer 6. The laminate has a yield strength in the range of 8 [Mpa] or more and 70 [Mpa] or less, and a whitening initiation elongation rate of 3 [%] or more. As a result, it is possible to provide a decorative sheet 1 that can be improved in terms of processability.
[0043] The decorative sheet is used as a building material, for example, by wrapping a member, and the mechanical properties of the decorative sheet greatly affect its suitability for processing (wrapping, etc.) Specifically, the suitability for processing refers to the resistance to cracking and whitening at corners, ease of handling during production, etc. For example, a decorative sheet with a high yield strength is too hard and easily breaks during processing, but if the yield strength is low, it has no stiffness and is inconvenient to handle. Also, if the whitening initiation elongation is too low, the sheet will whiten with only a small amount of elongation, so the corners will whiten quickly during processing, damaging the design. In contrast, with the decorative sheet 1 of the first embodiment, by setting the ranges of the mechanical properties (yield strength, whitening initiation elongation), it is possible to provide a decorative sheet 1 with good processability.
[0044] (2) The yield strength is within the range of 10 [Mpa] or more and 60 [Mpa] or less. As a result, compared to a configuration in which the yield strength is less than 10 [Mpa], it is possible to improve the ease of handling of the decorative sheet 1. In addition, compared to a configuration in which the yield strength is more than 70 [Mpa], it is possible to reduce damage to the decorative sheet 1 that occurs during processing, etc.
[0045] (3) The elongation at which whitening begins is 5% or more. As a result, compared to a configuration in which the whitening initiation elongation is less than 5%, it is possible to suppress the occurrence of whitening in the decorative sheet 1. (4) The transparent polyvinyl chloride resin forming the transparent resin layer 6 contains a benzotriazole-based or triazine-based ultraviolet absorbing agent. As a result, the decorative sheet 1 is able to maintain its ultraviolet absorbing performance for a long period of time. (5) The surface protective layer 8 contains a triazine-based ultraviolet absorbing agent and a light stabilizer. As a result, the decorative sheet 1 is able to maintain its ultraviolet absorbing performance for a long period of time.
[0046] Moreover, the decorative member 100 of the first embodiment can achieve the effects described below. (6) The decorative sheet 1 and the substrate 20 are disposed on the other side of the base layer 2. As a result, it is possible to provide a decorative member 100 that can be improved in terms of processability. This makes it possible to reduce deformation, expansion, and the like that occurs in a resin sash or window frame that has been decorated using the decorative member 100.
[0047] (7) The substrate 20 is made of polyvinyl chloride resin. Therefore, the transparent resin layer 6 formed using polyvinyl chloride resin and the substrate 20 formed using polyvinyl chloride resin make it possible to form the substrate 7 and the decorative sheet 1 into a mono-material. As a result, recycling of the decorative member 100 becomes easier, compared to a configuration in which the layer formed between the design layer 4 and the surface protective layer 8 is made of polyolefin or polypropylene.
[0048] <Modification of the first embodiment> (1) In the first embodiment, the decorative sheet 1 is configured to include the recesses 10, but this is not limited to this. That is, the decorative sheet 1 may be configured without the recesses 10, as shown in FIG. (2) In the first embodiment, the decorative member 100 is configured to include the recess 10, but this is not limited to this. That is, the decorative member 100 may be configured not to include the recess 10, as shown in FIG. EXAMPLES
[0049] With reference to the first embodiment, the decorative members of Examples 1 to 3 and the decorative members of Comparative Examples 1 and 2 will be described in the following examples. Example 1 The decorative member of Example 1 has the following configuration. ·Base material layer Material: Colored PVC resin
[0050] Pattern layer Materials: PVC printing ink, binder resin, pigment Binder resin: Acrylic resin and polyvinyl chloride-vinyl acetate copolymer resin Pigments: Pigments including isoindolinone, polyazo, phthalocyanine, and perylene black Pattern:Wood grain pattern Printing method: Gravure printing
[0051] ·Transparent resin layer Material: transparent polyvinyl chloride resin, UV absorber UV absorber: Triazine-based UV absorber Amount of UV absorber added: 0.5 parts by weight per 100 parts by weight of transparent polyvinyl chloride resin
[0052] ·Surface protective layer Materials: Acrylic resin composition, UV absorber, light stabilizer, hardener, solvent Coating amount: 3 [g / m 2 ] Base: Copolymer of methyl methacrylate and 2-hydroxyethyl methacrylate Mixing ratio: methyl methacrylate / 2-hydroxyethyl methacrylate = 95 / 5 Amount of base agent added: 90 parts by weight UV absorber: "Tinuvin 479" manufactured by BASF Japan Ltd. Amount of UV absorber added: 9 parts by weight Light stabilizer: "Tinuvin 123" manufactured by BASF Japan Ltd. Amount of light stabilizer added: 1 part by weight Hardener: "Takenate D170" by Mitsui Chemicals, Inc. Amount of hardener added: 10 parts by weight Solvent: Ethyl acetate Amount of solvent added: 240 parts by weight
[0053] ·Adhesive layer Material: Urethane adhesive ·substrate Material: Wood-based material ·Yield point strength: 28[Mpa] Whitening start elongation rate: The elongation rate at which the decorative sheet does not whiten
[0054] Example 2 The decorative member of Example 2 has the same structure as the decorative member of Example 1, except that the decorative sheet has a yield strength of 50 [Mpa] and a whitening initiation elongation of 5 [%]. Example 3 The decorative member of Example 2 has the same structure as the decorative member of Example 1, except that the yield strength of the decorative sheet is 13 [Mpa].
[0055] Comparative Example 1 The decorative member of Comparative Example 1 has the same structure as the decorative member of Example 1, except that the decorative sheet has a yield strength of 74 [Mpa] and a whitening initiation elongation rate of 1 [%]. Comparative Example 2 The decorative member of Comparative Example 2 has the same structure as the decorative member of Example 1, except that the yield strength of the decorative sheet is 6 [Mpa].
[0056] (Performance evaluation) A performance evaluation was carried out on the processing suitability of each of the decorative members of Examples 1 to 3 and the decorative members of Comparative Examples 1 and 2. The evaluation results are shown in Table 1. (Processing suitability) The decorative members of the examples and the decorative members of the comparative examples were each measured for crack resistance, ease of handling, and whitening resistance, and the overall suitability for processing was evaluated. As a standard for evaluating the overall processing suitability, "◎" and "○" were considered to be passing marks, and if there was even one item marked with "×", it was considered to be failing.
[0057] <Crack resistance> The corners of the decorative member wrapped with the decorative sheet were observed with the naked eye and with a microscope, and those in which the decorative sheet had no cracks were rated as "◎". The corners were also observed with the naked eye and with a microscope, and those in which no cracks were observed with the naked eye but cracks were observed with a microscope were rated as "○". The corners were also observed with the naked eye and with a microscope, and those in which cracks were observed with the naked eye were rated as "×".
[0058] <Ease of handling> When a decorative sheet is used to wrap a part to form a decorative member, the decorative sheet is stiff and easy to handle, and is evaluated as "◎". In addition, the decorative sheet is not stiff, but does not cause any problems in processing, and is evaluated as "○". Furthermore, the decorative sheet is not stiff and is difficult to handle, and is evaluated as "×".
[0059] <Whitening resistance> During processing to wrap a part with the decorative sheet to form a decorative member, a decorative sheet that did not whiten when stretched was rated as "◎", a decorative sheet that did not whiten immediately when stretched but whitened gradually was rated as "◯", and a decorative sheet that whitened immediately when stretched was rated as "×".
[0060] [Table 1]
[0061] (Evaluation Results) As shown in Table 1, all of the decorative members of Examples 1 to 3 had good processability. On the other hand, it was confirmed that the decorative members of Comparative Examples 1 and 2 had poor processability. Therefore, it was confirmed that the decorative members 1 of Examples 1 to 3 have better processability than the decorative members of Comparative Examples 1 and 2.
[0062] The present technology can be configured as follows. (1) A base layer formed using a colored polyvinyl chloride resin; A pattern layer laminated on one surface of the base layer; a transparent resin layer laminated on one surface of the design layer and formed using a transparent polyvinyl chloride resin; A decorative sheet comprising: a surface protective layer laminated on one surface of the transparent resin layer, The yield strength is within the range of 8Mpa to 70Mpa, A decorative sheet having a whitening initiation elongation of 3% or more. (2) The decorative sheet according to (1) above, wherein the yield strength is within the range of 10 MPa to 60 MPa. (3) The decorative sheet according to (1) or (2) above, wherein the whitening initiation elongation is 5% or more. (4) The decorative sheet according to any one of (1) to (3) above, wherein the transparent polyvinyl chloride resin contains a benzotriazole-based or triazine-based ultraviolet absorbing agent. (5) The decorative sheet according to any one of (1) to (4) above, wherein the surface protective layer contains a triazine-based ultraviolet absorbing agent and a light stabilizer. (6) A decorative member comprising the decorative sheet according to any one of (1) to (5) above, and a substrate disposed on the other surface side of the base layer. (7) The decorative member according to (6) above, wherein the substrate is formed using a polyvinyl chloride resin. [Explanation of symbols]
[0063] 1...decorative sheet, 2...base material layer, 4...pattern layer, 6...transparent resin layer, 8...surface protection layer, 10...recess, 12...adhesive layer, 20...substrate, 100...decorative member
Claims
1. A base layer formed using a colored polyvinyl chloride resin; A pattern layer laminated on one surface of the base layer; a transparent resin layer laminated on one surface of the design layer and formed using a transparent polyvinyl chloride resin; A decorative sheet comprising: a surface protective layer laminated on one surface of the transparent resin layer, The yield strength is in the range of 8 MPa to 70 MPa, A decorative sheet having a whitening initiation elongation of 3% or more.
2. 2. The decorative sheet according to claim 1, wherein the yield strength is within the range of 10 MPa to 60 MPa.
3. 2. The decorative sheet according to claim 1, wherein said whitening initiation elongation is 5% or more.
4. 2. The decorative sheet according to claim 1, wherein said transparent polyvinyl chloride resin contains a benzotriazole or triazine ultraviolet absorbing agent.
5. 2. The decorative sheet according to claim 1, wherein said surface protective layer contains a triazine-based ultraviolet absorbing agent and a light stabilizer.
6. A decorative member comprising: the decorative sheet according to claim 1 ; and a substrate disposed on the other surface side of the base layer.
7. 7. The decorative member according to claim 6, wherein the substrate is made of polyvinyl chloride resin.
Citation Information
Patent Citations
Water heater
JP1985060451A