Insulated wire, wire harness for automobile, and resin composition
The use of a resin composition with low-density polyethylene or ethylene/α-olefin copolymer in the insulating layer addresses the challenge of balancing flexibility and wear resistance in large-diameter electric cables for vehicles, enhancing performance in automotive wire harnesses.
Patent Information
- Application Number
- JP2023058934
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing insulated wires for large-diameter electric cables in hybrid and electric vehicles face challenges in achieving both high flexibility and wear resistance, as adding rubber to the insulating resin layer enhances flexibility but reduces abrasion resistance, while increasing the resin layer thickness compromises flexibility.
A resin composition using low-density polyethylene resin or ethylene/α-olefin copolymer as the base resin for the insulating layer, with a specific outer diameter ratio and thickness, ensuring both flexibility and wear resistance are maintained.
The insulated wire achieves excellent flexibility and wear resistance, suitable for automotive wire harnesses, particularly in high-voltage applications, by utilizing a resin composition with controlled density and layer thickness.
Smart Images

Figure 2024146185000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an insulated wire, an automotive wire harness, and a resin composition. [Background technology]
[0002] With the recent progress in the development of hybrid vehicles and the like, insulated electric wires used in automobiles and the like are required to have more excellent properties than ever before in terms of flexibility, hardness, degree of cross-linking, abrasion resistance, flame retardancy, cold resistance, heat resistance, and the like. To date, many studies have been conducted on resin compositions that can be used as a covering material for a conductor to realize an insulated electric wire having flame retardancy, heat resistance, flexibility (flexibility), and mechanical properties, and many reports have been published. As resin compositions that constitute insulated electric wires having such desired properties, resins such as specific types of polyethylene and ethylene-vinyl acetate copolymers are widely used.
[0003] High-voltage cables used in motors and inverters in hybrid and electric vehicles use so-called thick-diameter wires in order to handle large currents. Because thick-diameter wires must be routed in a small space with a small bending radius, the insulating resin layer (insulating resin) of the thick-diameter wires must be highly flexible. For example, Patent Document 1 discloses a wire having a wire diameter of 0.15 mm to 0.5 mm and a cross-sectional area of 20 mm 2 The electrical cable is characterized in that the outer circumference of the above conductor is covered with an insulating resin containing a flame retardant, the electrical cable diameter / conductor diameter is 1.15 to 1.40, and the secant modulus of the insulating resin is 10 MPa to 50 MPa. The technology described in Patent Document 1 uses copolymers such as ethylene-vinyl acetate copolymer (EVA) and ethylene-ethylene acrylate copolymer (EEA) as the resin material, and uses insulating resin with added rubber as necessary, which ensures flexibility not found in the past, facilitates wiring work (routing) in narrow spaces, and enables space saving by reducing the bending radius, etc. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2014-139932 A Summary of the Invention [Problem to be solved by the invention]
[0005] In order to improve the flexibility of the insulating resin layer constituting the large-diameter electric wire, it is known to add rubber to the insulating resin of the insulated electric wire, as disclosed in the above-mentioned Patent Document 1, for example. However, adding rubber to the insulating resin reduces the abrasion resistance, which causes the coating wear at vibrating and oscillating parts, which makes the insulation breakdown more likely to occur. In order to prevent the insulation breakdown, it is considered to make the insulating resin layer thick to a certain extent. However, thickening the insulating resin layer reduces the flexibility of the insulated electric wire. Thus, it is difficult to achieve both insulation and flexibility at a high level in a large-diameter electric wire.
[0006] In view of the above circumstances, an object of the present invention is to provide an insulated electric wire that can achieve both high levels of flexibility and abrasion resistance, and an automobile wiring harness having the insulated electric wire. Another object of the present invention is to provide a resin composition that can impart high levels of flexibility and abrasion resistance to the insulated electric wire. [Means for solving the problem]
[0007] As a result of intensive research aimed at solving the above problems, the present inventors have found that by using a resin composition having a low-density polyethylene resin or an ethylene-α-olefin copolymer as a base resin as a material for forming an insulating resin layer, the resulting insulated wire can achieve both flexibility and abrasion resistance at a high level. Based on these findings, further research has led to the completion of the present invention.
[0008] That is, the above problems were solved by the following means. <1> An insulated wire comprising a conductor and an insulating resin layer covering the outer periphery of the conductor, The cross-sectional area of the conductor is 19.5 mm 2 That's all. The insulating resin layer is a base resin having a density of 0.857 to 0.908 g / cm 3 The present invention relates to a polyethylene resin or a crosslinked body of an ethylene-α-olefin copolymer, An insulated wire, wherein the ratio of the outer diameter of the insulating resin layer to the outer diameter of the conductor [outer diameter of insulating resin layer / outer diameter of conductor] is 1.10 or more and 1.40 or less, and the thickness of the insulating resin layer is 0.7 to 2.0 mm. <2> The cross-sectional area of the conductor is 30 mm 2 The above <1> 2. The insulated wire according to claim 1 . <3> a ratio of the outer diameter of the insulating resin layer to the outer diameter of the conductor [outer diameter of the insulating resin layer / outer diameter of the conductor] is 1.10 or more and 1.30 or less; <1> or <2> 2. The insulated wire according to claim 1 . <4> The above <1> ~ <3> 2. An automobile wire harness comprising the insulated electric wire according to claim 1. <5> A resin composition for use in forming an insulating resin layer constituting an insulated electric wire, comprising: The insulated wire has a conductor cross-sectional area of 19.5 mm 2 That's all. The resin composition has a density of 0.857 to 0.908 g / cm as a base resin. 3 A resin composition comprising a polyethylene resin or an ethylene-α-olefin copolymer.
[0009] In the present invention, a numerical range expressed using "to" means a range including the numerical values before and after it as the lower limit and upper limit. Effect of the Invention
[0010] The insulated wire of the present invention has excellent flexibility and excellent abrasion resistance. In addition, the insulated wire constituting the automotive wire harness of the present invention has excellent flexibility and excellent abrasion resistance. Furthermore, the resin composition of the present invention can be suitably used for the insulated wire of the present invention. [Brief description of the drawings]
[0011] [Figure 1] 1 is a schematic diagram illustrating one embodiment of an insulated wire according to the present invention. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Preferred embodiments of the present invention will be described below, but the present invention is not limited to the following embodiments except as defined in the present invention. [Insulated wire] The insulated wire of the present invention has a conductor and an insulating resin layer covering the outer periphery of the conductor. Hereinafter, preferred embodiments of the present invention will be described with reference to the drawings. Note that the present invention is not limited to the embodiments shown below, except as specified in the present invention. Furthermore, the description of the insulated wire and the like described with reference to the drawings below is not limited to the forms shown in the drawings, but is applied as a description of the configuration or invention-specific matters of the present invention.
[0013] Fig. 1 is a schematic diagram showing one embodiment of an insulated wire of the present invention. The insulated wire 1 shown in Fig. 1 has a conductor 11 which is a concentric strand formed by twisting together a plurality of wires, and an insulating resin layer 12 which covers the outer periphery of the conductor 11. In the insulated wire 1, the cross-sectional area of the conductor 11 is 19.5 mm 2 1, the conductor 11 is shown as a concentric strand in which seven strands 13 are stranded together, and the number and diameter of the strands 13 are appropriately determined so as to satisfy the above-mentioned cross-sectional area of the conductor 11. The insulating resin layer 12 is a base resin having a density of 0.857 to 0.908 g / cm. 3 The insulating layer is formed by crosslinking a resin composition containing the polyethylene resin or ethylene-α-olefin copolymer.3 When referring to "polyethylene resin or ethylene-α-olefin copolymer," the term "density is 0.857 to 0.908 g / cm 3 Polyethylene resin with density of 0.857~0.908g / cm 3 The term "ethylene-α-olefin copolymer" means "at least one selected from the group consisting of ethylene-α-olefin copolymers." In addition, in the insulated wire 1 of the present invention, when the outer diameter of the conductor 11 (conductor outer diameter) is D1 and the outer diameter of the insulating resin layer 12 (insulating resin layer outer diameter) is D2 (D2 is synonymous with the outer diameter of the insulated wire 1), the ratio (D2 / D1) of the insulating resin layer outer diameter D2 to the conductor outer diameter D1 is controlled to be 1.10 or more and 1.40 or less. The insulated wire 1 of the present invention may have an intermediate layer or a shielding layer between the conductor 11 and the insulating resin layer 12. The insulated wire 1 consisting of the conductor 11 and the insulating resin layer 12 may serve as a core wire, the outside of which may be covered with a sheath, and a shield may further be provided between the core wire and the sheath. The insulated wire 1 of the present invention is used for wiring of power supply systems such as motors and inverters in hybrid cars and electric cars, for example. The characteristic features of the insulated wire of the present invention will be described below.
[0014] <Conductor> The conductor used in the insulated wire of the present invention has a circular or nearly circular cross-sectional shape perpendicular to the longitudinal direction of the conductor. In the insulated wire of the present invention, the conductor may be an assembly conductor made of a plurality of element wires. The assembly conductor is preferably an assembly conductor made by bundling or twisting a plurality of element wires. The shape, assembly method, etc. of the assembly conductor are not particularly limited, and for example, the assembly conductor may be a bunched stranded wire, a concentric stranded wire, or a composite stranded wire (rope stranded wire). The element wire diameter of the element wires can be appropriately set according to the cross-sectional area and number of element wires of the conductor, and can be, for example, 0.15 mm or more and 0.5 mm or less, or 0.18 mm or more and 0.35 mm or less. The shape and material of the conductor (or the wires constituting the conductor) may be any shape and material that is generally used for insulated electric wires in automotive wire harnesses. The conductor (or the wires constituting the conductor) may be, for example, a bare wire or a tin-plated or enamel-coated wire. Metal materials for forming the conductor or wires include soft copper, copper alloy, aluminum, and aluminum alloy.
[0015] The insulated wire of the present invention has a cross-sectional area of 19.5 mm 2 In order to further increase the allowable current of the insulated wire of the present invention, the cross-sectional area is set to 25 mm 2 It is preferable that the thickness is 30 mm or more. 2 More preferably, it is 40 mm or more. 2 The upper limit of the cross-sectional area is not particularly limited. For example, from the viewpoint of reducing the weight of the wire harness for an automobile, it is preferably 120 mm 2 It can be less than 100mm 2 It can be less than 80mm 2 It can also be the following: When the conductor is an assembly conductor, the cross-sectional area of the conductor can be calculated by calculating the cross-sectional area of each wire constituting the assembly conductor and adding them up.
[0016] In the insulated wire of the present invention, when the outer diameter of the conductor (conductor outer diameter) is D1 and the outer diameter of the insulating resin layer (insulating resin layer outer diameter) is D2 (D2 is synonymous with the outer diameter of the insulated wire), the ratio of the insulating resin layer outer diameter D2 to the conductor outer diameter D1 (D2 / D1) is 1.10 or more, preferably 1.15 or more, and more preferably 1.20 or more, as described above. Also, the ratio is 1.40 or less, preferably 1.35 or less, and more preferably 1.30 or less, as described above. In addition, when the conductor is an aggregate conductor consisting of multiple wires, the outer diameter D1 of the conductor is defined as the maximum distance from one point to another point on the outer circumference of the aggregate conductor when viewed in a plan view of a cross section perpendicular to the longitudinal direction of the aggregate conductor.
[0017] <Insulating resin layer> In the insulated wire of the present invention, the insulating resin layer contains a base resin having a density of 0.857 to 0.908 g / cm 3 The insulating resin layer can be formed by extruding a resin composition containing at least the polyethylene resin or ethylene-α-olefin copolymer onto the outer periphery of the conductor to a uniform thickness, and crosslinking the resin composition by a crosslinking treatment while covering the conductor or after covering the conductor.
[0018] The insulated wire of the present invention has an insulating resin layer having a density of 0.857 to 0.908 g / cm as a base resin. 3 Since the insulating resin layer contains the polyethylene resin or the crosslinked body of ethylene-α-olefin copolymer, it has excellent abrasion resistance, and therefore good abrasion resistance can be maintained even if the insulating resin layer is thinned. The thickness of the insulating bark layer is 0.7 to 2.0 mm as described above. From the viewpoint of further improving the flexibility of the electric wire, the thickness of the insulating resin layer is preferably 1.8 mm or less, more preferably 1.5 mm or less, and even more preferably 1.3 mm or less. From the viewpoint of further improving the abrasion resistance, the thickness of the insulating resin layer is preferably 0.8 mm or more, more preferably 0.9 mm or more, and even more preferably 1.0 mm or more. The preferable range of the thickness of the insulating resin layer can be appropriately set according to the outer diameter of the conductor.
[0019] In addition, the insulated wire of the present invention has an insulating resin layer having a density of 0.857 to 0.908 g / cm as a base resin. 3 The insulating resin layer contains a crosslinked body of the polyethylene resin or ethylene-α-olefin copolymer, and thus has excellent flexibility. From the viewpoint of further improving flexibility, the secant modulus of the insulating resin layer is preferably set to 5 Pa or more and 60 MPa or less. By setting the value of the secant modulus within the above-mentioned preferred range, flexibility and handleability can be imparted to the insulated electric wire even in the case of an insulated electric wire with a large conductor size.
[0020] (Resin composition) The resin composition of the present invention is a resin composition (resin composition for large diameter electric wire) to be used for forming the insulating resin layer that constitutes the insulated electric wire. Each of the components constituting the resin composition (each component of the resin composition before the crosslinking reaction) may be used alone or in combination of two or more kinds. Each component contained in the resin composition will be described below.
[0021] -resin- The resin composition has a density of 0.857 to 0.908 g / cm as a base resin. 3 The polyethylene resin or ethylene-α-olefin copolymer has a density of 0.875 to 0.900 g / cm 3 The density of the resin can be determined in accordance with JIS K 7112:1999. The base resin has a density of 0.857 to 0.908 g / cm3 as a whole. 3 It is preferable that the density is 0.875 to 0.900 g / cm 3 For example, when the base resin contains a plurality of resins, the density can be calculated as a weighted average of the densities of the respective resins. For example, when the density is 0.850 g / cm 3 The ethylene-α-olefin copolymer A is 30% by mass and has a density of 0.900 g / cm 3 When the ethylene-α-olefin copolymer B is contained at 70 mass%, the density of the entire base resin is [(0.850 g / cm 3 × 0.3) + (0.900g / cm 3 × 0.7) = 0.885g / cm 3 ] can be calculated as follows. Density of base resin is 0.857~0.908g / cm 3The proportion of the polyethylene resin or ethylene-α-olefin copolymer is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, still more preferably 95% by mass or more, and even more preferably 99% by mass or more. In addition, all of the resins contained in the base resin have a density of 0.857 to 0.908 g / cm 3 The polyethylene resin may be an ethylene-α-olefin copolymer.
[0022] The resin used in the present invention can be synthesized by a conventional method, or a commercially available product can be used, such as the ENGAGE series manufactured by The Dow Chemical Company.
[0023] The content of the base resin in the resin composition can be 30 to 80% by mass, can be 40 to 75% by mass, or can be 50 to 75% by mass.
[0024] -Flame retardants- The resin composition preferably contains a bromine compound (bromine-based flame retardant) and an antimony compound (antimony-based flame retardant) as a flame retardant. The ratio of the bromine compound to the antimony compound in the resin composition is preferably 2 to 5 times the molar amount of bromine element per 1 mole of antimony element. The total content of the flame retardant in the resin composition is preferably 20 to 45 parts by mass with respect to 100 parts by mass of the base resin.
[0025] Examples of bromine compounds used as flame retardants in the present invention include organic bromine-containing flame retardants such as brominated N,N'-ethylenebisphthalimide or compounds derived therefrom (collectively referred to as "brominated N,N'-ethylenebisphthalimide compounds"); N,N'-bis(bromophenyl)terephthalamide or compounds derived therefrom (collectively referred to as "N,N'-bis(bromophenyl)terephthalamide compounds"); brominated bisphenol or compounds derived therefrom (collectively referred to as "brominated bisphenol compounds"); and 1,2-bis(bromophenyl)alkane. Among these, it is preferable to use, for example, brominated N,N'-ethylenebisphthalimide and / or 1,2-bis(bromophenyl)ethane. The bromine compound used in the resin composition may be a commercially available bromine compound, for example, Cytex 8010 (trade name, manufactured by Albemarle Corporation).
[0026] From the viewpoint of flame retardancy, the content of the bromine compound in the resin composition is preferably 15 to 30 parts by mass, more preferably 20 to 30 parts by mass, and even more preferably 24 to 30 parts by mass, per 100 parts by mass of the base resin.
[0027] Examples of antimony compounds include antimony trioxide, antimony tetroxide, antimony pentoxide, and sodium antimonate. Antimony reacts with chlorine (halogen), and the generated gas is thought to block oxygen, promoting the formation of a carbonized layer and trapping free radicals (stopping the pyrolysis chain reaction). Among them, from the viewpoint of forming a more stable carbonized layer, it is preferable to contain antimony trioxide in the present invention. In the present invention, commercially available antimony trioxide may be used, for example, PATOX-C (trade name, manufactured by Nippon Seiko Co., Ltd.).
[0028] When the resin composition contains an antimony compound, from the viewpoint of flame retardancy, the content is preferably 5 to 15 parts by mass, more preferably 8 to 13 parts by mass, and even more preferably 10 to 12 parts by mass, per 100 parts by mass of the base resin.
[0029] The resin composition may contain, in addition to the bromine compound and antimony compound, a flame retardant that can be generally used in the insulating resin layer of an insulated electric wire. Examples of such flame retardants include metal hydroxides (hydroxide-based flame retardants) such as magnesium hydroxide and aluminum hydroxide. When the resin composition contains a hydroxide-based flame retardant, the amount of the hydroxide-based flame retardant is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, per 100 parts by mass of the base resin.
[0030] -Antioxidants- The resin composition may contain, as an antioxidant (antiaging agent), an imidazole compound (imidazole-based antioxidant), a phenol compound (phenol-based antioxidant), and / or a thioether compound (thioether-based antioxidant). Each of the above antioxidants will be described below.
[0031] Examples of the imidazole compound (a compound having a benzimidazole skeleton) include 2-sulfanylbenzimidazole, 2-sulfanylmethylbenzimidazole, 4-sulfanylmethylbenzimidazole, 5-sulfanylmethylbenzimidazole, and zinc salts thereof, with 2-sulfanylbenzimidazole and the zinc salt thereof being preferred. In the present invention, a commercially available imidazole compound may be used, for example, Nocrac MBZ (trade name, manufactured by Ouchi Shinko Chemical Industry Co., Ltd.). From the viewpoint of further improving heat resistance and crosslinkability, and from the viewpoint of dispersibility in the resin and suppressing the occurrence of bleeding, the content of the imidazole compound is preferably 14 to 24 parts by mass, more preferably 16 to 24 parts by mass, and even more preferably 16 to 20 parts by mass, relative to 100 parts by mass of the base resin constituting the resin composition.
[0032] Examples of the phenol compound (a compound having a phenol skeleton) include triethylene glycol-bis(3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate), 1,6-hexanediol-bis(3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate), pentaerythrityl-tetrakis(3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate), octadecyl- Examples include 3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, 1,3,5-tris(3,5-di-t-butyl-4-hydroxybenzyl)isocyanuric acid, and isooctyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate. One or more of these can be used. Among these, from the viewpoint of imparting high heat resistance to automotive wire harnesses, those having two or more 3,5-di-t-butyl-4-hydroxyphenyl groups or 3,5-di-t-butyl-4-hydroxybenzyl groups are preferred, and 1,3,5-tris(3,5-di-t-butyl-4-hydroxybenzyl)isocyanuric acid and pentaerythrityl-tetrakis(3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate) are particularly preferred. In the present invention, commercially available phenol compounds may be used, such as Irganox 1010 (product name, manufactured by BASF) and Adeka STAB AO-20 (product name, manufactured by ADEKA). From the viewpoint of further improving heat resistance and crosslinkability, and from the viewpoint of suppressing the occurrence of bleeding, the content of the phenol compound is preferably 1.0 to 2.0 parts by mass, and more preferably 1.5 to 2.0 parts by mass, per 100 parts by mass of the base resin constituting the resin composition.
[0033] The thioether compound (compound having a thioether bond) may be a thioether compound used as an antioxidant for wire coating materials. For example, dilauryl 3,3'-thiodipropionate, dimyristyl 3,3'-thiodipropionate, distearyl 3,3'-thiodipropionate, 2,2-bis{[3-(dodecylthio)-1-oxopropoxy]methyl}propane-1,3-diyl bis[3-dodecylthiopropionate] (also known as bis[3-(dodecylthio)propionic acid]2,2-bis[[3-(dodecylthio)-1-oxopropyloxy]methyl]-1,3-propanediyl), etc. may be used alone or in combination. Among these, 2,2-bis{[3-(dodecylthio)-1-oxopropoxy]methyl}propane-1,3-diyl bis[3-dodecylthiopropionate] is preferred from the viewpoint of long-term thermal stability. In the present invention, a commercially available thioether compound may be used, for example, Adeka STAB AO-412S (trade name, manufactured by ADEKA Corporation). From the viewpoint of improving heat resistance, improving slipperiness, and suppressing crosslinking inhibition, the content of the thioether compound is preferably 0.3 to 0.9 parts by mass, and more preferably 0.3 to 0.6 parts by mass, relative to 100 parts by mass of the base resin constituting the resin composition.
[0034] The resin composition may contain an antioxidant other than the imidazole compound, phenol compound, and thioether compound. Examples of such antioxidants include copper inhibitors and zinc compounds, and one or more of these can be used. Specific examples of zinc compounds include zinc sulfide and zinc oxide. The total content of the antioxidants is preferably 10 to 35 parts by mass, more preferably 15 to 30 parts by mass, and even more preferably 20 to 26 parts by mass, relative to 100 parts by mass of the base resin constituting the resin composition.
[0035] -Crosslinking agent- The resin composition also preferably contains a crosslinking aid. Examples of the crosslinking aid include polyfunctional compounds, and preferably compounds having two or more (preferably three or more, more preferably three to six) ethylenically unsaturated bonds (carbon-carbon double bonds) in the molecule. Specific examples of the crosslinking auxiliary include (meth)acrylate compounds such as polypropylene glycol di(meth)acrylate and trimethylolpropane tri(meth)acrylate, allyl compounds such as triallyl cyanurate, maleimide compounds, and divinyl compounds. In the present invention, a commercially available crosslinking aid may be used. An example of a commercially available product is Ogmont T200 (trade name, manufactured by Shin-Nakamura Chemical Co., Ltd.). The resin composition preferably contains 2 to 6 parts by mass, and more preferably 3 to 5 parts by mass, of the crosslinking aid relative to 100 parts by mass of the base resin.
[0036] - Processing aids - The oil composition also preferably contains a processing aid, and a preferred example of the processing aid is a metal soap (lubricant). Examples of metal soaps (lubricants) that can be used in the present invention include calcium stearate, zinc stearate, and magnesium stearate. In the present invention, a commercially available metal soap may be used, for example, Sinaka Red ZS-101 (trade name, manufactured by Shinagawa Kako Co., Ltd.). When the resin composition contains a lubricant, the lubricant is preferably contained in an amount of 0.5 to 2 parts by mass per 100 parts by mass of the base resin.
[0037] -Other ingredients- In addition to the above components, the resin composition may contain components such as a dispersant, a plasticizer, a filler, and a pigment, as long as the effects of the present invention are not impaired.
[0038] The resin composition can be obtained by mixing each component such as a resin, an antioxidant, a flame retardant, and the like, and further, if necessary, the optional components described above, and melt-kneading the mixture in a commonly used kneading device such as a batch-type kneader such as a roll, a kneader, or a Banbury mixer, or a twin-screw extruder.
[0039] [Automotive Wire Harnesses] In the present invention and this specification, an automotive wire harness is a general term for a bundle of electric wires arranged in various places of a vehicle, such as the engine room, the instrument panel, and inside the doors, according to environmental performance. The automotive wire harness of the present invention has the insulated electric wire of the present invention. Since the insulated electric wire of the present invention has excellent flexibility and abrasion resistance, a wire harness incorporating the insulated electric wire of the present invention can be suitably used for automotive applications. In particular, the insulated electric wire of the present invention has a conductor cross-sectional area of 19.5 mm 2 For these reasons, the material can also be used in wire harnesses for high voltage and large current applications, such as the power supply circuits of electric vehicles (electric cars, hybrid cars, etc.).
[0040] [Manufacturing method of insulated wires for automotive wiring harnesses] The insulated wire used in the automotive wire harness of the present invention can be obtained, for example, by extrusion coating the resin composition on a conductor to provide a layer of the resin composition, and then irradiating the layer of the resin composition with an electron beam of 80 to 250 kGy. This electron beam irradiation causes a crosslinking reaction in the layer of the resin composition, forming a coating layer (insulating resin layer) made of an insulating resin. The crosslinking reaction by electron beam irradiation can be carried out by a usual method and under usual conditions, and is not limited thereto. The irradiation conditions of the electron beam are preferably a dose of 80 to 200 kGy, more preferably 80 to 160 kGy, and the acceleration voltage is preferably 300 to 3000 keV, more preferably 500 to 2500 keV. Furthermore, a multi-layer structure may be used in which an intermediate layer or a shielding layer is provided between a conductor and a coating layer, or between coating layers.
[0041] The conditions for extrusion molding the resin composition are not particularly limited as long as the resin composition can be extruded. However, the extrusion temperature (head) is preferably 100 to 230°C, more preferably 120 to 200°C, in order to reduce the load on the extruder (extrusion molding machine) and ensure shape retention. Other conditions for the extrusion molding can be appropriately set depending on the purpose. The screw configuration of the extruder is not particularly limited, and a normal full-flight screw, double-flight screw, end double-flight screw, Maddock screw, etc. can be used. EXAMPLES
[0042] The present invention will be described in more detail based on the following examples and comparative examples, but the present invention is not limited to these.
[0043] [Formulation examples 1-7] The materials used to prepare the resin compositions of Blend Examples 1 to 7 are shown in Table 1 below. Details of the materials used are as follows. Note that (1) to (10) below correspond to (1) to (10) in Table 1 below.
[0044] <Materials used> (resin) (1) ENGAGE 8150: Product name, ethylene-octene polyolefin elastomer (density 0.868 g / cm 3 ), manufactured by The Dow Chemical Company (2) ENGAGE 8452: Product name, ethylene-octene polyolefin elastomer (density 0.875 g / cm 3 ), manufactured by The Dow Chemical Company (3) ENGAGE 7256: Product name, ethylene-octene polyolefin elastomer (density 0.885 g / cm 3 ), manufactured by The Dow Chemical Company (4) ENGAGE 8440: Product name, ethylene-octene polyolefin elastomer (density 0.897 g / cm 3 ), manufactured by The Dow Chemical Company (5) NUC-3195: Product name, ethylene-vinyl acetate copolymer, comonomer content: 24% by mass, manufactured by ENEOS NUC Corporation
[0045] (Brominated flame retardants) (6) Scitex 8010 (product name, manufactured by Albemarle) (Antimony Trioxide) (7) PATOX-C (product name, manufactured by Nihon Seiko Co., Ltd.) (Antioxidants) (8) Nocrac MBZ (product name, manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) (Crosslinking aid) (9) Ogmont T200 (product name, manufactured by Shin-Nakamura Chemical Co., Ltd.) (lubricant) (10) Sinaka Red ZS-101 (product name, manufactured by Shinagawa Kako Co., Ltd.)
[0046] [Table 1]
[0047] The content of each component in the table is in parts by mass. "-" means that the corresponding component is not included.
[0048] [Examples 1 to 9 and Comparative Example 1] The resin compositions of the above Blending Examples 1 to 7 were used to obtain insulated wires of Examples 1 to 9 and Comparative Example 1. The method for producing each insulated wire is described below in detail.
[0049] Example 1 According to the composition shown in Formulation Example 1 in Table 1 above, the mixture was melt-kneaded at 180° C. using a 1.7 liter Banbury mixer, and the mixture was discharged and granulated through an extruder to obtain resin composition pellets. The obtained resin composition pellets were extrusion coated onto a copper conductor (strand number 19 / strand number 13 / strand diameter 0.32 mm) shown in Table 2 below, using an extruder set at a temperature of 90 to 190°C, to a thickness shown in Table 2 below. The formed layer of the resin composition was cross-linked by electron beam irradiation. Thus, a copper conductor having a cross-sectional area of about 20 mm 2 An insulated wire (finished outer diameter: about 8.3 mm) of Example 1 was obtained, which had an insulating resin layer with a thickness of about 0.90 mm around a conductor with an outer diameter of about 6.5 mm made of copper (about 20 sq). Crosslinking with an electron beam was performed under conditions of an acceleration voltage of 3000 keV and a dose of 160 kGy.
[0050] (Examples 2 to 9, Comparative Example 1) Each of the insulated wires of Examples 2 to 9 and Comparative Example 1 was obtained in the same manner as above, except that the conductor configuration and the resin composition used were as shown in Table 2 below.
[0051] [Performance evaluation] The insulated wires produced as described above were subjected to the following performance evaluations.
[0052] <Flexibility (bending rigidity) evaluation> The flexibility (bending rigidity) was evaluated according to the method stipulated in JIS C6870-1-21:2018, Clause 19, E17C of the Japanese Industrial Standards. Each of the above insulated electric wires (samples) was cut to a length of 400 mm, and the cable (insulated electric wire) bent at 180 degrees was placed between parallel plates, the ends of the cable were fixed to the parallel plates, a load cell was placed on the plates, and the maximum load (N) was measured when the cable was bent until the bending interval was 100 mm. The obtained maximum load was evaluated based on the following evaluation criteria. The zero point of the load cell was adjusted before the sample was attached, and the test was carried out at room temperature. -Evaluation criteria- 〇: Maximum load is less than 20N ×: Maximum load is 20N or more
[0053] <Wear resistance evaluation> Abrasion resistance tests (scrape abrasion tests) were conducted based on the method specified in JASO D625-2:2022 4.7.2 of the Automotive Wire Standard. A 1 m sample was taken from each insulated wire of Examples 1 to 9 and Comparative Example 1, and 25 mm of the insulating resin layer (insulator) was removed from one end. A load of 7 N was applied to a needle (made of stainless steel) with a diameter of 0.45 mm on this sample, and it was driven under the following conditions. After one test was completed, the sample was moved 100 mm in the axial direction, rotated 90° around the axis of the sample and fixed, and the test was repeated to record the number of cycles until the needle wore down the insulator and contacted the conductor. - Driving conditions - Operating speed: 55 cycles / min (one cycle is one round trip) Needle movement: 20mm Wear length: 15.5mm Test temperature: 23℃ If the number of cycles until the needle contacted the conductor was 750 or more, it was rated as "Good", and if it was less than 750, it was rated as "Poor".
[0054] The results obtained are summarized in Table 2 below.
[0055] [Table 2]
[0056] The insulated wire of Comparative Example 1 obtained by using a resin composition containing an ethylene-vinyl acetate copolymer as the base resin was shown to have excellent flexibility but poor abrasion resistance. In contrast, the base resin has a density of 0.857 to 0.908 g / cm 3 It was shown that each of the insulated wires of Examples 1 to 9 obtained using the resin composition containing the polyethylene resin or the ethylene-α-olefin copolymer had excellent flexibility and also excellent abrasion resistance. [Explanation of symbols]
[0057] 1. Insulated wire 11 Conductor 12 Insulating resin layer 13 Wire D1 Conductor outer diameter D2 Insulation resin layer outer diameter
Claims
1. An insulated wire comprising a conductor and an insulating resin layer covering the outer periphery of the conductor, The cross-sectional area of the conductor is 19.5 mm 2 That's all. The insulating resin layer has a density of 0.857 to 0.908 g / cm as a base resin. 3 The present invention relates to a polyethylene resin or a crosslinked body of an ethylene-α-olefin copolymer, an insulating resin layer having a thickness of 0.7 to 2.0 mm; and a ratio of an outer diameter of the insulating resin layer to an outer diameter of the conductor [outer diameter of insulating resin layer / outer diameter of conductor] of 1.10 to 1.
40.
2. The cross-sectional area of the conductor is 30 mm 2 The insulated wire according to claim 1 .
3. 2. The insulated wire according to claim 1, wherein a ratio of an outer diameter of the insulating resin layer to an outer diameter of the conductor [outer diameter of insulating resin layer / outer diameter of conductor] is 1.10 or greater and 1.30 or less.
4. A wire harness for an automobile, comprising the insulated wire according to any one of claims 1 to 3.
5. A resin composition for use in forming an insulating resin layer constituting an insulated electric wire, comprising: The insulated wire has a conductor with a cross-sectional area of 19.5 mm 2 That's all. The resin composition has a density of 0.857 to 0.908 g / cm as a base resin. 3 A resin composition comprising the polyethylene resin or ethylene / α-olefin copolymer described above.
Citation Information
Patent Citations
Electric cable
JP2014139932A
Flame-retardant composition and insulated wire using the same
JP2015193689A