Production method of single surface metal foil laminate

By forming unevenness on the protective material surface, the method addresses low productivity and appearance defects in single-sided metal-clad laminate production, resulting in higher quality and more efficient manufacturing.

JP2024146253APending Publication Date: 2024-10-15KANEKA CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023059037
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Conventional methods for producing single-sided metal-clad laminates have low productivity due to the lack of effective methods to improve peeling performance and reduce appearance defects such as scratches during thermal lamination.

Method used

The method involves forming unevenness on the surface of a protective material used in thermal lamination by methods like embossing, hairline processing, blasting, or adding particles during film formation, which is then used to create a single-sided metal-clad laminate with a metal foil and adhesive sheet configuration.

Benefits of technology

This approach enhances the peeling performance and reduces appearance defects, allowing for the production of single-sided metal-clad laminates with improved productivity and quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146253000001
    Figure 2024146253000001
Patent Text Reader

Abstract

To provide a production method of a single surface metal foil laminate, which uses an adhesive sheet which has on both surfaces thereof, a thermoplastic resin layer, for producing the single surface metal foil laminate by heat lamination, the method capable of acquiring the single surface metal foil laminate having preferable appearance, and reducing poor appearance such as scratch.SOLUTION: There is provided a production method of a single surface metal foil laminate comprising: an adhesive sheet comprising on both surfaces of a heat resistant film, a thermoplastic resin layer; and a metal foil on one surface of the adhesive sheet. The production method comprises processing for forming irregularity on a surface of a protective material contacting the adhesive sheet, and in an order of the protective material / metal foil / adhesive sheet / protective material (subjected to irregularity formation processing), heat lamination is executed and then the protective materials are removed, for acquiring the single surface metal foil laminate having a configuration of the metal foil / adhesive sheet, for solving above-mentioned problem.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a protective material used in the manufacture of single-sided flexible printed circuit boards (hereinafter also referred to as FPCs). [Background technology]

[0002] Electronic devices are rapidly becoming more powerful, more functional, and more compact, and this is accompanied by a growing demand for smaller and thinner electronic components used in these devices. In addition, costs are being reduced, and the materials that make up FPCs are becoming more diverse in response to these demands.

[0003] Conventionally, as a metal foil laminate suitable for a printed circuit board for electronic and electrical devices, a single-sided metal-clad laminate in which a metal foil is laminated only on one side of a polyimide film, or a double-sided metal-clad laminate in which a metal foil is laminated on both sides, has been known. As a method for producing a double-sided metal-clad laminate having such a structure, a method has been proposed in which a polyimide film and a metal foil are thermally pressed (hereinafter also referred to as thermal lamination) between a pair of metal rolls at high temperatures with a protective film interposed therebetween (for example, Patent Document 1). There is also a method in which a polyimide film and a metal foil are thermally laminated between a pair of metal rolls without a protective film interposed therebetween. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2001-129918 A Summary of the Invention [Problem to be solved by the invention]

[0005] In principle, single-sided metal-clad laminates can also be manufactured by the method of Patent Document 1. That is, by placing a metal foil on only one side, they can be manufactured by thermal lamination in the same way as double-sided metal-clad laminates. However, this manufacturing method has low productivity.

[0006] The present invention has been made in consideration of the above-mentioned problems, and its object is to improve peel performance by imparting irregularities to the surface of a heat-resistant film that comes into contact with a thermoplastic resin layer during production by thermal lamination, thereby obtaining a single-sided metal-clad laminate with good appearance, and to reduce appearance defects such as scratches by transferring the irregularities of a protective material to the surface of an adhesive sheet. [Means for solving the problem]

[0007] As a result of intensive research aimed at solving the above problems, the present inventors have found that the desired metal-clad laminate can be obtained by the following method, and have completed the present invention. That is, the present invention has the following configuration. 1) A method for producing a single-sided metal-clad laminate comprising laminating an adhesive sheet having a thermoplastic resin layer on both sides of a heat-resistant film and a metal foil on one side of the adhesive sheet, The surface of the protective material that comes into contact with the adhesive sheet is treated to create irregularities. Put together the protective material, metal foil, adhesive sheet, and protective material (with textured surface treatment) in that order, and then heat laminate them. A method for producing a single-sided metal-clad laminate, comprising removing a protective material to obtain a single-sided metal-clad laminate having a metal foil / adhesive sheet configuration.

[0008] 2) A method for producing a single-sided metal-clad laminate according to 1), characterized in that the unevenness of the protective material is formed by an embossing process. 3) The method for producing a single-sided metal-clad laminate according to 1), characterized in that the unevenness of the protective material is formed by a hairline processing method. 4) A method for producing a single-sided metal-clad laminate according to 1), characterized in that the unevenness of the protective material is formed by a blast treatment method.

[0009] 5) The method for producing a single-sided metal-clad laminate according to 1), characterized in that the unevenness of the protective material is formed by adding particles during film formation.

[0010] 6) A method for producing a single-sided metal-clad laminate according to 1), characterized in that the unevenness of the protective material is formed by a coating method.

[0011] 7) A method for producing a single-sided metal-clad laminate according to 1), characterized in that the unevenness of the protective material is formed by a vapor deposition method.

[0012] 8) A method for producing a single-sided metal-clad laminate according to 1), characterized in that the unevenness of the protective material is formed by a sputtering method. 9) The method for producing a single-sided metal-clad laminate according to any one of 1) to 8), wherein the heat-resistant film is a non-thermoplastic polyimide film. 10) The method for producing a single-sided metal-clad laminate according to any one of 1) to 9), wherein the thermoplastic resin layer contains a thermoplastic polyimide resin.

[0013] 11) The method for producing a single-sided metal-clad laminate according to any one of 1) to 10), characterized in that the temperature range of Tg of the thermoplastic resin layer is 150°C to 250°C. Effect of the Invention

[0014] According to the present invention, it is possible to use a thermal lamination device for double-sided metal laminates that has been conventionally produced, and to reduce appearance defects such as scratches, thereby enabling the production of single-sided metal-clad laminates with high productivity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, the embodiments of the present invention will be described in detail. However, the present invention is not limited to these embodiments, and various modifications can be made within the scope of the description.

[0016] Unless otherwise specified in this specification, "A to B" expressing a numerical range means "A or more (including and greater than A) to B or less (including and smaller than B)."

[0017] <Heat-resistant film> In the present invention, "heat resistance" means that the film can withstand the heating temperature during thermal lamination. Therefore, the heat-resistant film is not particularly limited as long as it satisfies the above-mentioned properties, and various known films such as polyimide films and polyethylene naphthalate films can be used. Among them, heat-resistant polyimide films are preferable because they are excellent not only in heat resistance but also in physical properties such as electrical properties.

[0018] The "heat-resistant polyimide film" refers to a polyimide film which contains 90% by weight or more of polyimide resin in the resin component and which retains its shape without wrinkling or stretching when heated in a film state at 380°C for 2 minutes. In the present invention, this is also called a non-thermoplastic polyimide.

[0019] Generally, polyimide films can be produced using polyamic acid as a precursor. Any known method can be used to produce polyamic acid. Usually, polyamic acid can be produced by dissolving substantially equimolar amounts of aromatic tetracarboxylic dianhydride and aromatic diamine in an organic solvent and stirring the mixture under controlled temperature conditions until the polymerization of the aromatic tetracarboxylic dianhydride and aromatic diamine is completed. These polyamic acid solutions are usually obtained at a concentration of 5 to 35% by weight, preferably 10 to 30% by weight. When the concentration is within this range, suitable molecular weight and solution viscosity can be obtained.

[0020] As the polymerization method, any known method or a combination of these methods can be used. The polymerization method for polyamic acid polymerization is characterized by the order of monomer addition, and the physical properties of the resulting polyimide can be controlled by controlling the order of monomer addition. Therefore, in the present invention, any method of monomer addition can be used for the polymerization of polyamic acid. Representative polymerization methods include the following methods 1) to 5), and these methods can be used alone or in partial combination. 1) A method in which an aromatic diamine is dissolved in an organic polar solvent and reacted with an aromatic tetracarboxylic dianhydride in a substantially equimolar amount to polymerize the resulting solution. 2) A method in which an aromatic tetracarboxylic dianhydride is reacted with an aromatic diamine compound in a molar amount smaller than that of the aromatic tetracarboxylic dianhydride in an organic polar solvent to obtain a prepolymer having acid anhydride groups at both ends, and then polymerized using an aromatic diamine compound so that the aromatic tetracarboxylic dianhydride and the aromatic diamine compound are substantially equimolar in all steps. 3) A method in which an aromatic tetracarboxylic dianhydride is reacted with an excess molar amount of an aromatic diamine compound in an organic polar solvent to obtain a prepolymer having amino groups at both ends, and then the prepolymer is polymerized using an aromatic tetracarboxylic dianhydride such that the aromatic tetracarboxylic dianhydride and the aromatic diamine compound are substantially equimolar in all steps. 4) A method in which an aromatic tetracarboxylic dianhydride is dissolved and / or dispersed in an organic polar solvent, and then polymerized using an aromatic diamine compound in a substantially equimolar amount. 5) A method of polymerizing a mixture of substantially equimolar amounts of an aromatic tetracarboxylic dianhydride and an aromatic diamine by reacting them in an organic polar solvent.

[0021] In the present invention, a polyamic acid obtained by any of the above polymerization methods may be used, and the polymerization method is not particularly limited.

[0022] Examples of the aromatic diamine include, but are not limited to, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 2,2-bis{4-(4-aminophenoxy)phenyl}propane, 2,2-bis{4-(4-aminophenoxy)phenyl}hexafluoropropane, bis{4-(3-aminophenoxy)phenyl}sulfone, bis{4-(4-aminophenoxy)phenyl}sulfone, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 3,3'-diaminobenzophenone, 4,4'-diaminobenzophenone, Examples of the amines include 1,4-diaminobenzene (p-phenylenediamine), 1,3-diaminobenzene (m-phenylenediamine), 4,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone, 9,9-bis(4-aminophenyl)fluorene, 4,4'-(1,4-phenylenebis(1-methylethylidene))bisaniline, 4,4'-(1,3-phenylenebis(1-methylethylidene))bisaniline, 4,4'-diaminobenzanilide, and the like, or a combination of two or more of these.

[0023] In addition, examples of the aromatic tetracarboxylic dianhydride include, but are not limited to, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 2,2',3,3'-benzophenone tetracarboxylic dianhydride, 4,4'-oxydiphthalic dianhydride, 3,4'-oxyphthalic dianhydride, ethylene bis(trimellitic monoester acid anhydride), bisphenol A bis(trimellitic monoester acid anhydride), pyromellitic dianhydride, 2,3,6,7-naphthalene tetracarboxylic dianhydride, 1,4,5,8-naphthalene tetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfone tetracarboxylic dianhydride, 3,3',4, Examples of the aromatic tetracarboxylic acid dianhydride include 4'-dimethyldiphenylsilane tetracarboxylic acid dianhydride, 3,3',4,4'-tetraphenylsilane tetracarboxylic acid dianhydride, 1,2,3,4-furan tetracarboxylic acid dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenylpropane dianhydride, 4,4'-hexafluoroisopropylidenediphthalic anhydride, 3,3',4,4'-biphenyl tetracarboxylic acid dianhydride, 2,3,3',4'-biphenyl tetracarboxylic acid dianhydride, p-phenylene bis(trimellitic acid monoester anhydride), p-phenylene diphthalic anhydride, and the like, and combinations of two or more of these.

[0024] The aromatic diamine and the aromatic tetracarboxylic dianhydride may be reacted in substantially equimolar amounts, and the order of addition, combination of monomers, and composition are not particularly limited.

[0025] The organic solvent used as the polymerization solvent for producing polyamic acid is not particularly limited as long as it dissolves aromatic diamine, aromatic tetracarboxylic dianhydride, and the resulting polyamic acid. As the polymerization solvent, for example, amide solvents such as N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone are preferable, and by using these, the resulting organic solvent solution of polyamic acid (polyamic acid solution) can be used as it is to prepare a resin solution.

[0026] The reaction temperature for producing polyamic acid is preferably -10°C to 50°C. By controlling the temperature within this range, the reaction proceeds at a good reaction rate, and the productivity is excellent, which is preferable. The reaction time is not particularly limited, but is usually several minutes to several hours.

[0027] In the present invention, the curing agent is intended to include at least one of a dehydrating agent and a catalyst.

[0028] Here, the dehydrating agent is not particularly limited as long as it can dehydrate the polyamic acid by dehydration ring closure, but examples thereof include aliphatic acid anhydrides, aromatic acid anhydrides, N,N'-dialkylcarbodiimides, lower aliphatic halides, halogenated lower aliphatic acid anhydrides, arylsulfonic acid dihalides, thionyl halides, etc. These may be used alone or in appropriate combination of two or more kinds. Among these, aliphatic acid anhydrides and aromatic acid anhydrides are particularly suitable.

[0029] The catalyst is not particularly limited as long as it is a component that has the effect of promoting the dehydration ring-closing action of the dehydrating agent on the polyamic acid. Specific examples of the catalyst include aliphatic tertiary amines, aromatic tertiary amines, and heterocyclic tertiary amines.

[0030] A filler can be added to the heat-resistant film (A) for the purpose of improving various film properties such as sliding properties, thermal conductivity, electrical conductivity, corona resistance, loop stiffness, etc. Any filler may be used, but preferred examples include silica, titanium oxide, alumina, silicon nitride, boron nitride, calcium hydrogen phosphate, calcium phosphate, mica, etc.

[0031] <Thermoplastic resin layer> In the present invention, examples of the thermoplastic resin layer include polycarbonate resins, acrylonitrile-styrene copolymer resins, and thermoplastic polyimide resins, but from the viewpoint of heat resistance, thermoplastic polyimide resins are particularly preferred. The content, molecular structure, and thickness of the thermoplastic polyimide resin contained in the layer are not particularly limited as long as the desired characteristics, such as significant adhesive strength with the metal foil and a suitable linear expansion coefficient, are expressed. However, in order to express the desired characteristics, such as significant adhesive strength and a suitable linear expansion coefficient, it is preferable that the thermoplastic polyimide resin is substantially contained in the thermoplastic resin layer in an amount of 50% by weight or more. Furthermore, it is preferable that the thermoplastic polyimide resin contained in the thermoplastic resin layer facing each other through the heat-resistant film is the same type from the viewpoint of the balance of the linear expansion coefficient in the entire adhesive sheet and the simplification of the manufacturing process.

[0032] As the thermoplastic polyimide resin contained in the thermoplastic resin layer, for example, thermoplastic polyamideimide, thermoplastic polyetherimide, thermoplastic polyesterimide, etc. can be suitably used.

[0033] The thermoplastic polyimide contained in the thermoplastic resin layer can be obtained by a conversion reaction from its precursor, polyamic acid. As a method for producing the polyamic acid, any known method can be used, as in the case of the precursor of the non-thermoplastic polyimide resin that can be used in the heat-resistant film.

[0034] From the viewpoint of exhibiting significant adhesive strength with the metal foil and not impairing the heat resistance of the resulting single-sided metal-clad laminate (E), the thermoplastic polyimide resin used in the present invention preferably has a glass transition temperature (Tg) in the range of 150° C. to 300° C. Furthermore, it is preferable that the Tg is in the range of 150° C. to 250° C., which is the temperature range in which the effect of improving adhesion by imparting unevenness to the protective film can be confirmed. Note that Tg can be determined from the inflection point value of the storage modulus measured by a dynamic viscoelasticity measuring device (DMA).

[0035] The polyamic acid precursor of the thermoplastic polyimide that can be used in the present invention is not particularly limited, and any known polyamic acid can be used. The polyamic acid solution can also be produced by appropriately selecting the above-mentioned raw materials and production conditions.

[0036] The properties of thermoplastic polyimides can be adjusted by combining various raw materials such as aromatic tetracarboxylic dianhydrides and aromatic diamines, but generally, when the ratio of aromatic diamines having a rigid structure is increased, the glass transition temperature increases, the storage modulus during heating increases, and adhesiveness and processability may decrease. For example, the ratio of aromatic diamines having a rigid structure to the total amount of aromatic diamines is preferably 40 mol% or less, more preferably 30 mol% or less, and particularly preferably 20 mol% or less.

[0037] Specific examples of preferred thermoplastic polyimide resins include aromatic diamines and aromatic tetracarboxylic dianhydrides that can be used in the above-mentioned heat-resistant polyimide film, and more preferably, those obtained by polymerizing an acid dianhydride such as benzophenone tetracarboxylic dianhydride, biphenyl tetracarboxylic dianhydride, oxydiphthalic dianhydride, or biphenyl sulfone tetracarboxylic dianhydride with an aromatic diamine having an aminophenoxy group.

[0038] <Metal foil> In the present invention, the metal foil is not particularly limited, but when the single-sided metal-clad laminate of the present invention is used for electronic and electrical equipment applications, examples of the metal foil include foils made of copper or copper alloys, stainless steel or its alloys, nickel or nickel alloys (including 42 alloy), and aluminum or aluminum alloys. In general flexible laminates, copper foils such as rolled copper foils and electrolytic copper foils are often used, but they can also be preferably used in the present invention. The surfaces of these metal foils may be coated with an anti-rust layer, a heat-resistant layer, or an adhesive layer. The thickness of the metal foil is not particularly limited, and may be any thickness that can exhibit sufficient functions depending on the application. The thickness of the metal foil is preferably, for example, 3 μm to 30 μm, and more preferably 5 μm to 20 μm. The surface roughness (Rz) of the metal foil is preferably 0.01 μm to 1 μm. If the surface roughness (Rz) of the metal foil is outside this range, the adhesion to the thermoplastic resin layer may be poor.

[0039] <Protective material> In the present invention, a protective material may be used from the viewpoint of ensuring good appearance and peel strength of the single-sided metal-clad laminate. Specifically, the protective material is laminated between the pressing surface (for example, a metal roll) and the metal foil.

[0040] The protective material is not particularly limited as long as it can withstand the heating temperature in the thermocompression bonding process, and heat-resistant plastics such as non-thermoplastic polyimide films, metal foils such as copper foils, aluminum foils, and SUS foils can be preferably used. Among them, non-thermoplastic polyimide films are more preferably used because of their excellent balance between heat resistance, recyclability, and the like. As the non-thermoplastic polyimide film, various known films can be used, and examples thereof include Apical (registered trademark) manufactured by Kaneka Corporation, Upilex (registered trademark) manufactured by Ube Industries, Ltd., and Kapton (registered trademark) manufactured by DuPont-Toray Co., Ltd.

[0041] As for the conditions for the unevenness of the protective material, it is preferable that the center line average roughness (Ra) of the protective material is 0.01 μm to 1 μm, and the surface roughness (Rz) of the protective material is 0.1 μm to 10 μm.

[0042] <Processing method for forming unevenness on protective material> The surface irregularities may be formed by any method, and can be appropriately selected from known methods such as (1) embossing, (2) hairline processing, (3) blasting, (4) matte kneading, (5) matte coating, (6) vapor deposition, and (7) sputtering. (1) The embossing method can be carried out by using a commonly known embossing roll during the film formation process or after the film has been formed. (2) The hairline processing method can be used to transfer a hairline pattern during the film formation process or after the film has been formed. (3) The blasting method can be carried out by a method commonly known as sandblasting. (4) The kneading matte method can be used to produce a film by adding particles during film formation. The particles to be added may be selected appropriately from inorganic particles such as silicon oxide, titanium oxide, aluminum silicate, lead oxide, zirconium oxide, calcium carbonate, magnesium carbonate, clay, kaolin, talc, kaolinite, alumina, dolomite, zeolite, and organic particles such as polyimide, divinylbenzene cross-linked polystyrene copolymer, and fluororesin, but are not limited thereto. These particles may be used alone or in combination of two or more kinds. The average particle size of these particles is preferably 0.05 μm to 10 μm, and more preferably 0.1 μm to 8 μm. The coating mat method (coating method) of (5) can be produced by applying a solution of polyimide, polyamideimide, etc. before ring-closing polycondensation or an aromatic polyamide solution in which particles are distributed to at least one side of a heat-resistant film by a commonly known method, heating, ring-closing polycondensation, or drying. Among these, it is preferable to use a solution in which particles are dispersed in a solution of polyimide before ring-closing polycondensation. The thickness of the coating mat layer is preferably 0.1 μm to 8 μm, and more preferably 2 μm to 4 μm. The particles to be added are assumed to be those described in (4). The average particle size of these particles is preferably 0.05 μm to 10 μm, and more preferably 1 μm to 5 μm. (6) The deposition method involves evaporating a substance in a vacuum to form a film. (7) The sputtering method can be used to deposit a film by applying a high voltage between the film and the target object in an inert gas atmosphere.

[0043] <Manufacturing method for single-sided metal-clad laminate: Configuration 1 (protective material / heat-resistant double-sided adhesive sheet / metal foil / protective material> In other words, the manufacturing method for a single-sided metal-clad laminate that is an embodiment of the present invention is a method of manufacturing a single-sided metal-clad laminate in a manner similar to the manufacturing method of a conventional double-sided metal-clad laminate, by improving the peelability between the adhesive layer and the protective material by imparting unevenness to one side of the protective material.

[0044] As a lamination method, various known methods can be applied, but a thermocompression bonding method in which the sheets are bonded together by thermocompression is preferred because it can suppress the occurrence of wrinkles in the single-sided metal-clad laminate. Examples of a method for bonding an adhesive sheet and a metal foil include a thermocompression bonding method by batch processing using a single plate press, a thermocompression bonding method by continuous processing using a thermoroll laminator (also called a thermolaminator) or a double belt press (DBP) device, and the like. From the viewpoint of productivity and equipment costs including maintenance costs, a thermocompression bonding method using a thermoroll laminator having one or more pairs of metal rolls is preferred. The "thermoroll laminator having one or more pairs of metal rolls" referred to here may be any device having metal rolls for heating and pressurizing a material, and the specific device configuration is not particularly limited.

[0045] The heating method of the laminated material in the thermocompression bonding means is not particularly limited, and for example, a heating means adopting a conventionally known method capable of heating at a predetermined temperature, such as a heat circulation method, a hot air heating method, an induction heating method, etc. Similarly, the pressurizing method of the laminated material in the thermocompression bonding means is not particularly limited, and for example, a pressurizing means adopting a conventionally known method capable of applying a predetermined pressure, such as a hydraulic method, an air pressure method, an inter-gap pressure method, etc., can be used.

[0046] In the present invention, from the viewpoint of properties such as peel strength, dimensional stability, and suppression of warping, the heating temperature of the first thermal lamination, i.e., the thermocompression bonding temperature (lamination temperature), is preferably a temperature of the glass transition temperature (Tg) of the adhesive sheet used +0° C. to 180° C. In addition, the lamination speed in the thermocompression bonding step, the pressure in the thermocompression bonding step (lamination pressure), the film payout tension, the metal foil tension, the outfeed tension, the winding tension of the single-sided metal-clad laminate, and the like can be appropriately adjusted from the viewpoint of suppressing warping, etc.

[0047] In order to obtain the single-sided metal-clad laminate of the present invention, it is preferable to use a thermal roll laminating device that continuously heats and presses the laminated material, and in this thermal roll laminating device, a laminated material feeding means for feeding the laminated material may be provided in the upstream of the thermal laminating means, or a laminated material winding means for winding the laminated material may be provided in the downstream of the thermal laminating means. By providing these means, the productivity of the thermal roll laminating device can be further improved. The specific configurations of the laminated material feeding means and the laminated material winding means are not particularly limited, and examples thereof include known roll-shaped winders that can wind up adhesive sheets, metal foils, or the resulting single-sided metal-clad laminate.

[0048] Furthermore, when a protective material is used, it is more preferable to provide a winding means or a payout means for winding and paying out the protective material. If the winding means and the payout means are provided, the protective material once used in the thermocompression bonding process can be reused by winding it up and placing it again on the payout side. In addition, an end position detection means and a winding position correction means may be provided to align both ends of the protective film or protective material when it is wound up. This allows the ends to be accurately aligned when wound up, thereby increasing the efficiency of reuse. The specific configurations of the winding means, the payout means, the end position detection means, and the winding position correction means are not particularly limited, and various conventionally known devices can be used. EXAMPLES

[0049] The method for producing single-sided and double-sided metal-clad laminates according to the present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.

[0050] (Peel strength) The resulting single-sided or double-sided metal-clad laminate was etched with an aqueous ferric chloride solution to form a 1 mm wide metal foil pattern, and the peel strength of the metal foil pattern was measured at an angle of 90° and a speed of 50 mm / min.

[0051] (Dimensional change rate) The obtained single-sided or double-sided metal-clad laminate was cut to a size of 200 mm, and a 1 mm diameter hole was drilled in a 150 mm square. In this state, the dimensional measurement of the 1 mm diameter hole (A) was performed. Furthermore, the metal foil was entirely etched with an aqueous ferric chloride solution, dried at 50°C for 30 minutes, and left in an environment with a temperature of 25°C and a humidity of 50% for 24 hours, after which the dimensional measurement of the 1 mm diameter hole (B) was performed, and the dimensional change rate was calculated using the following formula. The calculation was performed as the average value of the two sides for the longitudinal direction (MD) and transverse direction (TD) of the metal-clad laminate. 100×(BA) / A (%) (warp) The obtained single-sided metal-clad laminate was placed on a flat table, the height of the warpage at each of the four corners was measured with a ruler, and the average value of the warpage heights at the four points was calculated as the warpage. (Measurement of linear expansion coefficient) The linear expansion coefficient was measured using a TMA120C manufactured by Seiko Electronics Co., Ltd. The sample size was 3 mm in width and 10 mm in length. The temperature of the sample was once raised from 10°C to 400°C at 10°C / min with a load of 3 g, then cooled to 10°C, and the temperature of the sample was further raised at 10°C / min, and the average value was calculated from the thermal expansion coefficient during the second heating from 100°C to 200°C. Example 1 A 25 μm heat-resistant double-sided adhesive sheet (Pixio IB manufactured by Kaneka Corporation; Tg 210° C.) was laminated on the upper surface, a 12 μm thick rolled copper foil (BHM-102F-HA-V2 manufactured by JX Nippon Mining & Metals Corporation) was used as the metal foil, and a 125 μm heat-resistant polyimide film (Apical (registered trademark) 125NPI manufactured by Kaneka Corporation) was used as the protective material. A protective material with an embossed surface was placed on the exposed adhesive sheet surface on the lower surface, and a laminate structure of protective material / rolled copper foil / adhesive sheet / protective material was laminated. The laminate was passed between a pair of metal rolls of a hot roll laminator to perform hot lamination under conditions of a lamination temperature of 360° C., a lamination pressure of 244 N / cm, and a lamination speed of 1 m / min, to obtain a single-sided metal-clad laminate. The peel strength, dimensional stability, warpage, and linear expansion coefficient of the obtained single-sided metal-clad sheet were measured. The results are shown in Table 1. Example 2 In Example 1, the surface of the protective material was given an unevenness by a hairline processing method, and otherwise a single-sided metal-clad laminate was obtained in the same manner as in Example 1. The peel strength, dimensional stability, warpage, and linear expansion coefficient of the obtained single-sided metal-clad laminate were measured, and the results are shown in Table 1. Example 3 In Example 1, the surface of the protective material was roughened by a blast treatment method, and otherwise a single-sided metal-clad laminate was obtained in the same manner as in Example 1. The peel strength, dimensional stability, warpage, and linear expansion coefficient of the obtained single-sided metal-clad laminate were measured, and the results are shown in Table 1. Example 4 In Example 1, the surface of the protective material was given an unevenness by a kneading mat method, and otherwise a single-sided metal-clad laminate was obtained in the same manner as in Example 1. The peel strength, dimensional stability, warpage, and linear expansion coefficient of the obtained single-sided metal-clad laminate were measured, and the results are shown in Table 1. Example 5 In Example 1, the surface treatment method of the protective material was a coating method, and otherwise a single-sided metal-clad laminate was obtained in the same manner as in Example 1. The peel strength, dimensional stability, warpage, and linear expansion coefficient of the obtained single-sided metal-clad laminate were measured, and the results are shown in Table 1. Example 6 In Example 1, the surface of the protective material was provided with unevenness by a vapor deposition method, and otherwise a single-sided metal-clad laminate was obtained in the same manner as in Example 1. The peel strength, dimensional stability, warpage, and linear expansion coefficient of the obtained single-sided metal-clad laminate were measured, and the results are shown in Table 1. Example 7 In Example 1, the surface of the protective material was provided with unevenness by a sputtering method, and otherwise a single-sided metal-clad laminate was obtained in the same manner as in Example 1. The peel strength, dimensional stability, warpage, and linear expansion coefficient of the obtained single-sided metal-clad laminate were measured, and the results are shown in Table 1. Comparative Example 1 A 25 μm heat-resistant double-sided adhesive sheet (Pixio IB, manufactured by Kaneka Corporation; Tg 210° C.) and a 12 μm thick rolled copper foil (BHM-102F-HA-V2, manufactured by JX Nippon Mining & Metals Corporation) were used as the metal foil, and a protective material (Apical (registered trademark) 125NPI, manufactured by Kaneka Corporation) was placed on the outside of the adhesive sheet to form a rolled copper foil / adhesive sheet configuration. The sheet was then passed between a pair of metal rolls of a hot roll laminator to perform hot lamination under conditions of a lamination temperature of 360° C., a lamination pressure of 244 N / cm, and a lamination speed of 1 m / min; however, the adhesive sheet stuck to the hot roll, and a single-sided metal-clad laminate could not be obtained. Comparative Example 2 A single-sided metal-clad laminate was obtained in the same manner as in Comparative Example 1, except that a protective material (Apical (registered trademark) 75KH manufactured by Kaneka Corporation) was disposed and laminated in a configuration of protective material / rolled copper foil / adhesive sheet / protective material. The peel strength, dimensional stability, and warpage of the obtained single-sided metal-clad laminate were measured, and the results are shown in Table 1.

[0052] [Table 1]

Claims

1. A method for producing a single-sided metal-clad laminate, comprising laminating an adhesive sheet having a thermoplastic resin layer on both sides of a heat-resistant film and a metal foil on one side of the adhesive sheet, comprising: The surface of the protective material that comes into contact with the adhesive sheet is treated to create irregularities. Put together the protective material, metal foil, adhesive sheet, and protective material (with uneven surface treatment) in that order, and then heat laminate them. A method for producing a single-sided metal-clad laminate, comprising removing a protective material to obtain a single-sided metal-clad laminate having a metal foil / adhesive sheet configuration.

2. 2. The method for producing a single-sided metal-clad laminate according to claim 1, wherein the unevenness of the protective material is formed by embossing.

3. 2. The method for producing a single-sided metal-clad laminate according to claim 1, wherein the unevenness of the protective material is formed by a hairline processing method.

4. The method for producing a single-sided metal-clad laminate according to claim 1, wherein the unevenness of the protective material is formed by a blast treatment.

5. 2. The method for producing a single-sided metal-clad laminate according to claim 1, wherein the unevenness of the protective material is formed by adding particles during film formation.

6. 2. The method for producing a single-sided metal-clad laminate according to claim 1, wherein the unevenness of the protective material is formed by a coating method.

7. 2. The method for producing a single-sided metal-clad laminate according to claim 1, wherein the unevenness of the protective material is formed by a deposition method.

8. 2. The method for producing a single-sided metal-clad laminate according to claim 1, wherein the unevenness of the protective material is formed by a sputtering method.

9. The method for producing a single-sided metal-clad laminate according to any one of claims 1 to 8, wherein the heat-resistant film is a non-thermoplastic polyimide film.

10. The method for producing a single-sided metal-clad laminate according to any one of claims 1 to 8, wherein the thermoplastic resin layer contains a thermoplastic polyimide resin.

11. The method for producing a single-sided metal-clad laminate according to any one of claims 1 to 8, characterized in that the temperature range of Tg of the thermoplastic resin layer is 150°C to 250°C.

Citation Information