Polycarbonate resin composition and molded product composed of the same

The use of an aliphatic polycarbonate resin with specific structural units and aluminate-based luminescent agents in a balanced composition addresses decomposition issues, resulting in a molded product with enhanced luminance and hue.

JP2024146263AInactive Publication Date: 2024-10-15MITSUBISHI CHEM CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023059057
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Polycarbonate resin compositions containing luminescent agents face issues of decomposition, leading to darkening and reduced luminance when blended, which existing stabilizers like phosphite esters and organic silane compounds fail to adequately address, also impairing transparency.

Method used

A polycarbonate resin composition comprising an aliphatic polycarbonate resin with specific structural units derived from aliphatic dihydroxy compounds, such as isosorbide, and an aluminate-based luminescent agent, with a balanced ratio to minimize decomposition and enhance luminance and hue.

Benefits of technology

The composition achieves a molded product with improved external hue and high luminance, maintaining aesthetic appearance and mechanical properties while sustaining luminescence over time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146263000001
    Figure 2024146263000001
  • Figure 2024146263000002
    Figure 2024146263000002
  • Figure 2024146263000003
    Figure 2024146263000003
Patent Text Reader

Abstract

To provide a polycarbonate resin composition that yields a molded product with an excellent color hue in appearance and high luminous intensity, and a molded product thereof.SOLUTION: The present invention provides a polycarbonate resin composition comprising an aliphatic polycarbonate resin (A) and a luminescent storage agent (B) and a molded product composed of the same. The aliphatic polycarbonate resin (A) preferably comprises a structural unit derived from a dihydroxy compound represented by the formula (2).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polycarbonate resin composition containing an aliphatic polycarbonate resin and a luminescent agent, and to a molded article made of this polycarbonate resin composition. [Background technology]

[0002] When exposed to ultraviolet light or visible light contained in sunlight or artificial light, the material absorbs and stores the light, and even after the light irradiation has stopped, i.e., even in a dark place, the material emits a long-lasting glow that can be seen by the naked eye. Luminous materials are widely used in luminous signs and decorations, etc., because they can repeatedly absorb light energy, store light, and emit light.

[0003] As a luminous agent, in particular, a zinc sulfide-based luminous agent has been used for a long time. In recent years, a luminous agent having an aluminate as a host crystal (hereinafter, sometimes simply referred to as an "aluminate-based luminous agent") has become known, which has significantly improved luminance and afterglow time compared to a zinc sulfide-based luminous agent (see Patent Documents 1 to 4).

[0004] On the other hand, polycarbonate resin is an engineering plastic that has excellent impact resistance and transparency, and furthermore, exhibits little change in mechanical and electrical properties over a wide temperature range and has excellent dimensional stability. Taking advantage of these characteristics, it is used in a wide range of applications, from electrical and electronic devices, precision machinery, automotive parts, to sheet films.

[0005] When a luminescent agent is blended with a polycarbonate resin and then melt-kneaded, the polycarbonate resin decomposes due to the properties of the luminescent agent, causing the molded product to darken and impair the aesthetic appearance, which in turn reduces the luminance of the emitted light. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 8-127772 [Patent Document 2] Japanese Patent Application Publication No. 9-208948 [Patent Document 3] JP 2005-82647 A [Patent Document 4] JP 2009-215415 A Summary of the Invention [Problem to be solved by the invention]

[0007] In order to solve this problem, it is possible to limit the amount of the phosphorescent agent to suppress its decomposition, but this method reduces the phosphorescent performance and makes it difficult to obtain the desired characteristics. Patent Document 3 proposes adding a phosphorous ester to stabilize the molecular weight and hue of the resin during processing, but the effect of improving blackening is still insufficient. Patent Document 4 also proposes adding an organic silane compound and / or a silicone compound, but although it can suppress blackening, there remains the problem that the transparency is impaired and the luminance is reduced.

[0008] The present invention has been made in view of the above background, and aims to provide a polycarbonate resin composition which can give a molded article having a good appearance hue and high luminance, and a molded article made from the composition. [Means for solving the problem]

[0009] That is, the present invention has the following aspects [1] to [9]. [1] A polycarbonate resin composition containing an aliphatic polycarbonate resin (A) and a luminescent agent (B).

[0010] [2] The polycarbonate resin composition according to [1], wherein the aliphatic polycarbonate resin (A) contains a structural unit derived from a dihydroxy compound having a moiety represented by the following formula (1):

[0011] [ka]

[0012] [3] The polycarbonate resin composition according to [2], wherein the dihydroxy compound having a moiety represented by the above formula (1) is a dihydroxy compound represented by the following formula (2):

[0013] [ka]

[0014] [4] The polycarbonate resin composition according to any one of [1] to [3], wherein the luminescent agent (B) is an aluminate-based luminescent agent. [5] The polycarbonate resin composition according to [4], wherein the aluminate-based luminescent agent contains an alkaline earth metal or a lanthanoid metal. [6] The aluminate-based phosphorescent agent is SrAl2O4:Eu,Dy,Sr4Al 14 O 25 The polycarbonate resin composition according to [4] or [5], wherein the component (A) is at least one selected from the group consisting of CaAl2O4:Eu,Dy, and CaAl2O4:Eu,Nd. [7] The polycarbonate resin composition according to any one of [1] to [6], wherein a mass ratio of the aliphatic polycarbonate resin (A) to the luminescent agent (B) (wherein the aliphatic polycarbonate resin (A) : the luminescent agent (B)) is 50:50 to 99:1.

[0015] [8] A molded article obtained by molding the polycarbonate resin composition according to any one of [1] to [7]. [9] The molded article described in [8] used for evacuation guidance signs, nighttime display signs, sign buttons, clock faces, switches, connector parts, or accessories. Effect of the Invention

[0016] According to the above-mentioned aspects of the present invention, it is possible to provide a polycarbonate resin composition capable of giving a molded article having a good external hue and high luminance, and a molded article thereof. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The embodiment of the present invention will be described in detail below, but the description of the configuration described below is one example (i.e., a representative example) of the embodiment of the present invention, and the present invention is not limited to the following content as long as it does not exceed the gist of the present invention. In this specification, the term "structural unit" refers to a partial structure constituting a resin, and a specific partial structure contained in a repeating structural unit. For example, it refers to a partial structure sandwiched between adjacent linking groups in a resin, or a partial structure sandwiched between a polymerizable reactive group present at the end of a polymer and a linking group adjacent to the polymerizable reactive group. More specifically, in the case of a polycarbonate resin, a carbonyl group is a linking group, and a partial structure sandwiched between adjacent carbonyl groups is called a structural unit. In addition, when the expression "~" is used in this specification, it is used in a sense including the numerical value or physical value described before and after it. In addition, the numerical value or physical value described as the upper limit and lower limit is used in a sense including the value. In addition, "parts by weight" and "parts by mass", "% by weight" and "% by mass" are substantially synonymous.

[0018] [Polycarbonate resin composition] In this specification, the polycarbonate resin composition is appropriately referred to as the “resin composition.” The resin composition contains an aliphatic polycarbonate resin (A) and a luminous agent (B).

[0019] [Aliphatic polycarbonate resin (A)] The aliphatic polycarbonate resin (A) is a polycarbonate resin containing a structural unit derived from an aliphatic dihydroxy compound (hereinafter, this structural unit is appropriately referred to as "structural unit (a1)"), and is preferably a polycarbonate resin in which the main component of the structural units constituting the polymer is the structural unit (a1) or the structural unit (b) described below. The aliphatic polycarbonate resin (A) is appropriately referred to as "polycarbonate resin (A)". By containing the polycarbonate resin containing the structural unit (a1), the resin composition can obtain a molded article with a good hue and high luminance. This is believed to be because the polycarbonate resin (A) containing the structural unit (a1) suppresses the decomposition of the polycarbonate resin (A) caused by the properties of the phosphorescent agent, and the processing temperature can be lowered, so that the decomposition rate is slowed down.

[0020] Examples of the aliphatic dihydroxy compound include linear aliphatic dihydroxy compounds such as ethylene glycol, 1,3-propanediol, 1,2-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, and 1,12-dodecanediol; branched aliphatic dihydroxy compounds such as 1,3-butanediol, 1,2-butanediol, 2-ethyl-1,6-hexanediol, 2,2,4-trimethyl-1,6-hexanediol, neopentyl glycol, and hexylene glycol; and alicyclic dihydroxy compounds described below. Among these, alicyclic dihydroxy compounds are preferred.

[0021] The alicyclic dihydroxy compound is not particularly limited, but may be, for example, a compound having a 5-membered ring structure or a 6-membered ring structure. When the alicyclic dihydroxy compound contains a 5-membered ring structure or a 6-membered ring structure, the heat resistance of the aliphatic polycarbonate resin can be improved. The 6-membered ring structure may be fixed in a chair or boat shape by a covalent bond. The number of carbon atoms contained in the alicyclic dihydroxy compound is usually 70 or less, preferably 50 or less, and more preferably 30 or less. If the number of carbon atoms is excessively large, the heat resistance is high, but the synthesis becomes difficult, the purification becomes difficult, and the cost tends to be high. The smaller the number of carbon atoms, the easier it is to purify and the easier it is to obtain.

[0022] Specific examples of the alicyclic dihydroxy compound containing a 5-membered ring structure or a 6-membered ring structure include alicyclic dihydroxy compounds represented by the following formula (I) or (II). 5 and R 6 each independently represents a substituted or unsubstituted divalent group containing a cycloalkane structure having 4 to 20 carbon atoms (that is, a cycloalkylene group). HOCH2-R 5 -CHOH (I) H.O.R. 6 -OH (II)

[0023] An example of the alicyclic dihydroxy compound represented by formula (I) is cyclohexanedimethanol. Cyclohexanedimethanol is represented by the formula (I) R 5 The cyclohexanedimethanol includes various isomers represented by the following formula (Ia). Specifically, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, etc. are used as the cyclohexanedimethanol. In formula (Ia), R 3 represents a hydrogen atom, or a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms.

[0024] [ka]

[0025] Examples of the alicyclic dihydroxy compound represented by formula (I) include tricyclodecane dimethanol and pentacyclopentadecanedimethanol. Tricyclodecane dimethanol and pentacyclopentadecanedimethanol are represented by the formula (I) R 5 In the formula (Ib), n is 0 or 1.

[0026] [ka]

[0027] Examples of the alicyclic dihydroxy compound represented by formula (I) include decalin dimethanol and tricyclotetradecane dimethanol. Decalin dimethanol and tricyclotetradecane dimethanol are represented by the formula (I) R 5 The decalin dimethanol includes various isomers represented by the following formula (Ic). Specific examples of decalin dimethanol that can be used include 2,6-decalin dimethanol, 1,5-decalin dimethanol, and 2,3-decalin dimethanol. In formula (Ic), m represents 0 or 1.

[0028] [ka]

[0029] Moreover, an example of the alicyclic dihydroxy compound represented by formula (I) is norbornane dimethanol. Norbornane dimethanol is a compound represented by the formula (I) 5 The norbornane dimethanol includes various isomers represented by the following formula (Id): Specific examples of such norbornane dimethanol include 2,3-norbornane dimethanol and 2,5-norbornane dimethanol.

[0030] [ka]

[0031] An example of the alicyclic dihydroxy compound represented by formula (I) is adamantane dimethanol. 5 The adamantane dimethanol includes various isomers represented by the following formula (Ie): Specifically, 1,3-adamantanedimethanol and the like are used as such adamantane dimethanol.

[0032] [ka]

[0033] An example of the alicyclic dihydroxy compound represented by formula (II) is cyclohexanediol. 6 The cyclohexanediols include various isomers represented by the following formula (IIa). Specific examples of such cyclohexanediols include 1,2-cyclohexanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, and 2-methyl-1,4-cyclohexanediol. In formula (IIa), R 3 represents a hydrogen atom or a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms.

[0034] [ka]

[0035] Examples of the alicyclic dihydroxy compound represented by formula (II) include tricyclodecanediol and pentacyclopentadecanediol. Tricyclodecanediol and pentacyclopentadecanediol are represented by the formula (II) R 6 In the formula (IIb), n is 0 or 1.

[0036] [ka]

[0037] The alicyclic dihydroxy compound represented by formula (II) includes decalindiol and tricyclotetradecanediol. Decalindiol and tricyclotetradecanediol are represented by the formula (II) R 6 The decalindiols include various isomers represented by the following formula (IIc). Specific examples of decalindiols include 2,6-decalindiol, 1,5-decalindiol, and 2,3-decalindiol. In formula (IIc), m represents 0 or 1.

[0038] [ka]

[0039] An example of the alicyclic dihydroxy compound represented by formula (II) is norbornanediol. Norbornanediol is a dihydroxy compound represented by formula (II) 6 The norbornanediol includes various isomers represented by the following formula (IId): Specific examples of such norbornanediol include 2,3-norbornanediol and 2,5-norbornanediol.

[0040] [ka]

[0041] An example of the alicyclic dihydroxy compound represented by formula (II) is adamantanediol. Adamantanediol is a compound represented by the general formula (II) in which R 6 The adamantanediol includes various isomers represented by the following formula (IIe): Specifically, 1,3-adamantanediol and the like are used as such adamantanediol.

[0042] [ka]

[0043] The alicyclic dihydroxy compound is preferably at least one selected from the group consisting of cyclohexane dimethanols, tricyclodecane dimethanols, adamantane diols, and pentacyclopentadecanedimethanols. From the viewpoints of availability and ease of handling, the alicyclic dihydroxy compound is more preferably at least one selected from the group consisting of 1,4-cyclohexane dimethanol, 1,3-cyclohexane dimethanol, 1,2-cyclohexane dimethanol, and tricyclodecane dimethanol, and further preferably 1,4-cyclohexane dimethanol and / or tricyclodecane dimethanol.

[0044] The content of the structural unit (a1) in the aliphatic polycarbonate resin (A) is preferably 10 mol% or more, more preferably 20 mol% or more, and even more preferably 30 mol% or more, based on 100 mol% of all structural units derived from dihydroxy compounds constituting the aliphatic polycarbonate resin. The content of the structural unit (a1) is preferably 70 mol% or less, more preferably 60 mol% or less, and even more preferably 50 mol% or less. By having the structural unit (a1) within the above range, both the impact resistance and heat resistance of the aliphatic polycarbonate resin (A) can be improved in a balanced manner.

[0045] The polycarbonate resin (A) preferably further has a structural unit derived from a dihydroxy compound having a moiety represented by the following formula (1).

[0046] [ka]

[0047] The structural unit derived from a dihydroxy compound having a moiety represented by the above formula (1) is preferably a structural unit derived from a dihydroxy compound represented by the following formula (2) (hereinafter, appropriately referred to as "compound (1)") (hereinafter, this structural unit is appropriately referred to as "structural unit (a2)"). In this case, the weather resistance, optical properties, moldability, and heat resistance of the aliphatic polycarbonate resin (A) are improved, and it can contribute to carbon neutrality. The above-mentioned structural unit (a1) is a structural unit derived from an aliphatic dihydroxy compound other than the structural unit (a2).

[0048] [ka]

[0049] Compound (1) includes isosorbide, isomannide, and isoidet, which are stereoisomers, and one type may be used alone or two or more types may be used. Of these, isosorbide is the most preferable. Isosorbide is obtained by dehydration condensation of sorbitol, which is produced from various starches that are abundant as a plant-derived resource and are easily available, and therefore is easy to obtain and produce, and can contribute to carbon neutrality. In addition, an aliphatic polycarbonate resin (A) containing a structural unit derived from isosorbide can be obtained by the following method. It has excellent moldability, heat resistance, impact resistance, and surface hardness.

[0050] The content of the structural unit (a2) in the aliphatic polycarbonate resin (A) is preferably 30 mol% or more, more preferably 40 mol% or more, and even more preferably 50 mol% or more, based on 100 mol% of all structural units derived from dihydroxy compounds. Also, it is preferably 95 mol% or less, more preferably 90 mol% or less, and even more preferably 80 mol% or less. By adjusting the content of the structural unit (a2) within this range, both the impact resistance and heat resistance of the aliphatic polycarbonate resin (A) can be improved in a balanced manner.

[0051] The aliphatic polycarbonate resin (A) may further contain a structural unit derived from another dihydroxy compound (hereinafter, appropriately referred to as "structural unit (a3)"). Examples of the other dihydroxy compound include an ether group-containing dihydroxy compound other than the compound (1) and an acetal ring-containing dihydroxy compound.

[0052] Examples of ether group-containing dihydroxy compounds other than the above compound (1) include oxyalkylene glycols and dihydroxy compounds containing an acetal ring. Examples of oxyalkylene glycols include diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, and polypropylene glycol.

[0053] Examples of the dihydroxy compound containing an acetal ring include spiro glycol represented by the following formula (3) and dioxane glycol represented by the following formula (4).

[0054] [ka]

[0055] [ka]

[0056] In the aliphatic polycarbonate resin (A), the content of the structural unit (a3) ​​is preferably 10 mol% or more, more preferably 20 mol% or more, and even more preferably 30 mol% or more, based on 100 mol% of all structural units derived from dihydroxy compounds. Also, it is preferably 70 mol% or less, more preferably 60 mol% or less, and even more preferably 50 mol% or less. By having the structural unit (a3) ​​within the above range, both the impact resistance and heat resistance of the aliphatic polycarbonate resin (A) can be improved in a balanced manner.

[0057] In addition, within the scope of the present invention, the aliphatic polycarbonate resin (A) may contain a structural unit (a4) derived from a dihydroxy compound containing an aromatic group (hereinafter referred to as "compound (4)" as appropriate). However, when the aliphatic polycarbonate resin (A) contains a large amount of structural units (a4) derived from a dihydroxy compound containing an aromatic group, the polycarbonate resin may decompose due to the properties of the phosphorescent agent, and the color tone of the molded product may deteriorate. In addition, the molecular weight of the polycarbonate resin may decrease, and the impact resistance may be impaired. From the viewpoint of preventing a decrease in impact resistance and a deterioration in color tone, the content ratio of the structural unit (a4) is preferably less than 50 mol%, more preferably 10 mol% or less, even more preferably 5 mol% or less, and even more preferably 1 mol% or less, relative to 100 mol% of all structural units derived from dihydroxy compounds constituting the aliphatic polycarbonate resin. It is most preferable that the aliphatic polycarbonate resin (A) is substantially free of the structural unit (a4).

[0058] Compound (4) is not particularly limited, and examples thereof include the following compounds. Specifically, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 2,2-bis(4-hydroxy-3,5-diethylphenyl)propane, 2,2-bis(4-hydroxy-(3-phenyl)phenyl)propane, 2,2-bis(4-hydroxy-(3,5-diphenyl)phenyl)propane, 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane, bis(4-hydroxyphenyl)propane, bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)pentane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, bis(4-hydroxyphenyl)diphenylmethane, 1,1-bis(4-hydroxyphenyl)-2-ethylhexane, 1,1-bis(4-hydroxyphenyl)decane, bis(4-hydroxy-3-nitrophenyl)methane, 3,3-bis(4-hydroxyphenyl)pentane, 1, 3-Bis(2-(4-hydroxyphenyl)-2-propyl)benzene, 1,3-bis(2-(4-hydroxyphenyl)-2-propyl)benzene, 2,2-bis(4-hydroxyphenyl)hexafluoropropane, 1,1-bis(4-hydroxyphenyl)cyclohexane, bis(4-hydroxyphenyl)sulfone, 2,4'-dihydroxydiphenyl sulfone, bis(4-hydroxyphenyl)sulfide, bis(4-hydroxy-3-methylphenyl)sulfide, bis(4-hydroxyphenyl)disulfide, 4 aromatic bisphenol compounds such as 4,4'-dihydroxydiphenyl ether and 4,4'-dihydroxy-3,3'-dichlorodiphenyl ether; dihydroxy compounds having an ether group bonded to an aromatic group such as 2,2-bis(4-(2-hydroxyethoxy)phenyl)propane, 2,2-bis(4-(2-hydroxypropoxy)phenyl)propane, 1,3-bis(2-hydroxyethoxy)benzene, 4,4'-bis(2-hydroxyethoxy)biphenyl, and bis(4-(2-hydroxyethoxy)phenyl)sulfone;9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene, 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxypropoxy)phenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxypropoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxypropoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isopropylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isobutylphenyl)fluorene, 9, Examples of dihydroxy compounds having a fluorene ring include 9-bis(4-(2-hydroxyethoxy)-3-tert-butylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-cyclohexylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3,5-dimethylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butyl-6-methylphenyl)fluorene, and 9,9-bis(4-(3-hydroxy-2,2-dimethylpropoxy)phenyl)fluorene.

[0059] The type of compound (4) can be appropriately selected according to the properties required for the aliphatic polycarbonate resin (A). In addition, as the compound (4), only one type may be used, or multiple types may be used in combination. By using the compound (4) in combination with the compound (1), it is possible to improve the flexibility and mechanical properties of the aliphatic polycarbonate resin (A), and to improve the moldability.

[0060] The dihydroxy compound used as a raw material for the polycarbonate resin (A) may contain a reducing agent, an antioxidant (i.e., an antioxidant), an oxygen scavenger, a light stabilizer, an antacid, a stabilizer (specifically, a pH stabilizer, a heat stabilizer), and the like. In particular, the compound (1) has a property of being easily degraded under acidic conditions. In order to suppress this degeneration, a basic stabilizer can be used in the synthesis process of the polycarbonate resin (A). As a result, the quality of the resin composition and the molded product can be further improved.

[0061] Examples of the basic stabilizer include hydroxides, carbonates, phosphates, phosphites, hypophosphites, borates, and fatty acid salts of metals in Group 1 or 2 of the long-form periodic table (Nomenclature of Inorganic Chemistry IUPAC Recommendations 2005). Examples of the basic stabilizer include basic ammonia such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, trimethylethylammonium hydroxide, trimethylbenzylammonium hydroxide, trimethylphenylammonium hydroxide, triethylmethylammonium hydroxide, triethylbenzylammonium hydroxide, triethylphenylammonium hydroxide, tributylbenzylammonium hydroxide, tributylphenylammonium hydroxide, tetraphenylammonium hydroxide, benzyltriphenylammonium hydroxide, methyltriphenylammonium hydroxide, and butyltriphenylammonium hydroxide. amine compounds such as diethylamine, dibutylamine, triethylamine, morpholine, N-methylmorpholine, pyrrolidine, piperidine, 3-amino-1-propanol, ethylenediamine, N-methyldiethanolamine, diethylethanolamine, diethanolamine, triethanolamine, 4-aminopyridine, 2-aminopyridine, N,N-dimethyl-4-aminopyridine, 4-diethylaminopyridine, 2-hydroxypyridine, 2-methoxypyridine, 4-methoxypyridine, 2-dimethylaminoimidazole, 2-methoxyimidazole, imidazole, 2-mercaptoimidazole, 2-methylimidazole, and aminoquinoline; and hindered amine compounds such as di-(tert-butyl)amine and 2,2,6,6-tetramethylpiperidine.

[0062] The content of the basic stabilizer in the dihydroxy compound is not particularly limited. When used for compound (1), since compound (1) is unstable in an acidic state, it is preferable to set the content of the basic stabilizer so that the pH of an aqueous solution of the dihydroxy compound containing the basic stabilizer is around 7. More specifically, the content of the basic stabilizer relative to compound (1) is preferably 0.0001 to 1% by weight. In this case, the effect of preventing the deterioration of compound (1) is sufficiently obtained. From the viewpoint of further enhancing this effect, the content of the basic stabilizer is more preferably 0.001 to 0.1% by weight.

[0063] As the light stabilizer, any commonly known light stabilizer can be used, and the light stabilizer is not particularly limited. Specifically, for example, a hindered amine light stabilizer is used.

[0064] As the carbonic acid diester used as a raw material for the polycarbonate resin (A), a compound represented by the following formula (5) can usually be used. As the carbonic acid diester, one type may be used alone, or two or more types may be used in combination.

[0065] [ka]

[0066] In the above formula (5), A 1 and A 2 are each independently a substituted or unsubstituted aliphatic hydrocarbon group having 1 to 18 carbon atoms or a substituted or unsubstituted aromatic hydrocarbon group. 1 and A 2 may be the same or different. A 1 and A 2 is preferably a substituted or unsubstituted aromatic hydrocarbon group, and more preferably an unsubstituted aromatic hydrocarbon group.

[0067] As the carbonate diester represented by formula (5), for example, diphenyl carbonate (DPC) and substituted diphenyl carbonate such as ditolyl carbonate can be used. Also, dimethyl carbonate, diethyl carbonate, di-tert-butyl carbonate, etc. can be used. Among these carbonate diesters, it is preferable to use diphenyl carbonate and substituted diphenyl carbonate, and it is particularly preferable to use diphenyl carbonate. Note that the carbonate diester may contain impurities such as chloride ions, which may inhibit the polycondensation reaction or deteriorate the color tone of the resulting aliphatic polycarbonate resin (A). Therefore, it is preferable to use a carbonate diester purified by distillation or the like, as necessary.

[0068] The aliphatic polycarbonate resin (A) is synthesized, for example, by polycondensing a dihydroxy compound and a carbonic acid diester through an ester exchange reaction. More specifically, the aliphatic polycarbonate resin (A) is synthesized by removing from the system a monohydroxy compound and the like that are by-produced in the ester exchange reaction during the polycondensation.

[0069] The transesterification reaction proceeds in the presence of a transesterification catalyst (hereinafter, the transesterification catalyst is referred to as a "polymerization catalyst.") The type of polymerization catalyst can affect the reaction rate of the transesterification reaction and the quality of the resulting aliphatic polycarbonate resin (A).

[0070] As the polymerization catalyst, various catalysts can be used within the scope of the intended object of the present invention. As the polymerization catalyst, for example, metal compounds of Group I or Group II (hereinafter simply referred to as "Group 1" and "Group 2") in the long-form periodic table, basic compounds such as basic boron compounds, basic phosphorus compounds, basic ammonium compounds, and amine compounds can be used, and among them, Group 1 metal compounds and / or Group 2 metal compounds are preferred.

[0071] Examples of Group 1 metal compounds include sodium hydroxide, potassium hydroxide, lithium hydroxide, cesium hydroxide, sodium hydrogen carbonate, potassium hydrogen carbonate, lithium hydrogen carbonate, cesium hydrogen carbonate, sodium carbonate, potassium carbonate, lithium carbonate, cesium carbonate, sodium acetate, potassium acetate, lithium acetate, cesium acetate, sodium stearate, potassium stearate, lithium stearate, cesium stearate, sodium borohydride, potassium borohydride, lithium borohydride, cesium borohydride, sodium borophenylide, potassium borophenylide, lithium borophenylide, cesium phenylide, sodium benzoate, Examples of the metal compounds include thorium, potassium benzoate, lithium benzoate, cesium benzoate, disodium hydrogen phosphate, dipotassium hydrogen phosphate, dilithium hydrogen phosphate, dicesium hydrogen phosphate, disodium phenylphosphate, dipotassium phenylphosphate, dilithium phenylphosphate, dicesium phenylphosphate, sodium alcoholate, potassium alcoholate, lithium alcoholate, cesium alcoholate, sodium phenolate, potassium phenolate, lithium phenolate, cesium phenolate, disodium salt of bisphenol A, dipotassium salt of bisphenol A, dilithium salt of bisphenol A, dicesium salt of bisphenol A, etc. Among these, lithium compounds are preferred as the Group 1 metal compounds from the viewpoints of polymerization activity and color tone of the resulting polycarbonate resin (A).

[0072] Examples of the Group 2 metal compound include calcium hydroxide, barium hydroxide, magnesium hydroxide, strontium hydroxide, calcium hydrogen carbonate, barium hydrogen carbonate, magnesium hydrogen carbonate, strontium hydrogen carbonate, calcium carbonate, barium carbonate, magnesium carbonate, strontium carbonate, calcium acetate, barium acetate, magnesium acetate, strontium acetate, calcium stearate, barium stearate, magnesium stearate, strontium stearate, etc. Among these, the Group 2 metal compound is preferably a magnesium compound, a calcium compound, or a barium compound, and from the viewpoint of polymerization activity and the color tone of the resulting polycarbonate resin (A), more preferably a magnesium compound and / or a calcium compound, and most preferably a calcium compound.

[0073] Although it is possible to use a basic compound such as a basic boron compound, a basic phosphorus compound, a basic ammonium compound, or an amine compound in combination with the above-mentioned Group 1 metal compound and / or Group 2 metal compound as an auxiliary, it is particularly preferable to use only the Group 1 metal compound and / or Group 2 metal compound.

[0074] Examples of the basic boron compound include metal salts of tetramethyl boron, tetraethyl boron, tetrapropyl boron, tetrabutyl boron, trimethylethyl boron, trimethylbenzyl boron, trimethylphenyl boron, triethylmethyl boron, triethylbenzyl boron, triethylphenyl boron, tributylbenzyl boron, tributylphenyl boron, tetraphenyl boron, benzyltriphenyl boron, methyltriphenyl boron, butyltriphenyl boron, etc. Specific examples of the metal salt include sodium salt, potassium salt, lithium salt, calcium salt, barium salt, magnesium salt, strontium salt, etc.

[0075] Examples of basic phosphorus compounds include triethylphosphine, tri-n-propylphosphine, triisopropylphosphine, tri-n-butylphosphine, triphenylphosphine, tributylphosphine, and quaternary phosphonium salts.

[0076] Examples of basic ammonium compounds include tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, trimethylethylammonium hydroxide, trimethylbenzylammonium hydroxide, trimethylphenylammonium hydroxide, triethylmethylammonium hydroxide, triethylbenzylammonium hydroxide, triethylphenylammonium hydroxide, tributylbenzylammonium hydroxide, tributylphenylammonium hydroxide, tetraphenylammonium hydroxide, benzyltriphenylammonium hydroxide, methyltriphenylammonium hydroxide, and butyltriphenylammonium hydroxide.

[0077] Examples of amine compounds include 4-aminopyridine, 2-aminopyridine, N,N-dimethyl-4-aminopyridine, 4-diethylaminopyridine, 2-hydroxypyridine, 2-methoxypyridine, 4-methoxypyridine, 2-dimethylaminoimidazole, 2-methoxyimidazole, imidazole, 2-mercaptoimidazole, 2-methylimidazole, aminoquinoline, and guanidine.

[0078] The amount of the polymerization catalyst used is preferably 0.1 to 300 μmol, more preferably 0.5 to 100 μmol, and particularly preferably 1 to 50 μmol, per mol of the total dihydroxy compounds used in the reaction.

[0079] When a compound containing at least one metal selected from the group consisting of Group 2 metals in the long periodic table and lithium is used as a polymerization catalyst, particularly when a magnesium compound and / or a calcium compound is used, the amount of the polymerization catalyst used is preferably 0.1 μmol or more, more preferably 0.3 μmol or more, and particularly preferably 0.5 μmol or more, per mol of the total dihydroxy compounds used in the reaction, as the metal atomic weight of the compound containing the metal. The upper limit is preferably 10 μmol or less, more preferably 5 μmol or less, and particularly preferably 3 μmol or less.

[0080] By adjusting the amount of the polymerization catalyst used within the above range, the polymerization rate can be increased, and it is possible to obtain a polycarbonate resin (A) having a desired molecular weight without necessarily increasing the polymerization temperature, and therefore deterioration of the color tone of the polycarbonate resin (A) can be suppressed. In addition, it is possible to prevent the unreacted raw materials from volatilizing during the polymerization, which would cause the molar ratio of the dihydroxy compound and the carbonic acid diester to be lost, and therefore it is possible to more reliably obtain a resin having a desired molecular weight. Furthermore, it is possible to suppress the occurrence of side reactions, and therefore it is possible to further prevent deterioration of the color tone of the polycarbonate resin (A) or coloring during molding.

[0081] Considering the adverse effect of sodium, potassium, or cesium among the group 1 metals on the color tone of the polycarbonate resin (A) and the adverse effect of iron on the color tone of the polycarbonate resin (A), the total content of sodium, potassium, cesium, and iron in the polycarbonate resin (A) is preferably 1 weight ppm or less. In this case, the deterioration of the color tone of the polycarbonate resin (A) can be further prevented, and the color tone of the polycarbonate resin (A) can be further improved. From the same viewpoint, the total content of sodium, potassium, cesium, and iron in the polycarbonate resin (A) is more preferably 0.5 weight ppm or less. Note that these metals may be mixed in not only from the catalyst used, but also from the raw materials or reaction equipment. Regardless of the source, the total amount of the compounds of these metals in the polycarbonate resin (A) is preferably within the above-mentioned range as the total content of sodium, potassium, cesium, and iron.

[0082] (Physical properties of polycarbonate resin (A)) The average molecular weight of the polycarbonate resin (A) can be expressed by reduced viscosity, and the higher the reduced viscosity, the higher the average molecular weight. The reduced viscosity is preferably 0.30 dL / g or more, more preferably 0.35 dL / g or more. On the other hand, the reduced viscosity is preferably 1.20 dL / g or less, more preferably 1.00 dL / g or less, and even more preferably 0.80 dL / g or less. By adjusting the reduced viscosity within the above range, it is possible to improve the mechanical properties and improve the fluidity during molding, and to further improve the productivity and moldability. Therefore, molded products having excellent mechanical properties and complex shapes can be produced with good productivity, and the molded products are suitable for applications such as electric and electronic equipment parts and automobile interior and exterior parts. The reduced viscosity of the polycarbonate resin (A) is measured, for example, as follows. First, the polycarbonate resin (A) is dissolved in a solvent such as methylene chloride, and the polycarbonate resin concentration of the solution is precisely adjusted to 0.6 g / dL. Using this solution, the reduced viscosity can be measured using an Ubbelohde viscometer at a temperature of 20.0°C ± 0.1°C.

[0083] The glass transition temperature of the polycarbonate resin (A) is preferably 90°C or higher. In this case, the heat resistance of the polycarbonate resin composition is further improved. From the same viewpoint, the glass transition temperature of the polycarbonate resin (A) is more preferably 100°C or higher, and even more preferably 110°C or higher. On the other hand, the glass transition temperature of the polycarbonate resin (A) is preferably 145°C or lower. In this case, the flowability during molding is increased, the resin composition is easily delivered to the end of the mold, and a molded product having a desired shape can be obtained even if the shape is complicated. In addition, the decrease in strength at the weld portion can be suppressed. From the viewpoint of further enhancing these effects, the glass transition temperature of the polycarbonate resin (A) is more preferably 135°C or lower, and even more preferably 125°C or lower.

[0084] The resin composition may contain one type of resin alone as the aliphatic polycarbonate resin (A), but may contain a plurality of resins having different types and copolymerization ratios of the structural units (a1) to (a3) ​​and different physical properties. The resin composition may contain an aromatic polycarbonate resin together with the aliphatic polycarbonate resin (A) as long as it does not impair the intended object of the present invention. From the viewpoint of preventing adverse effects associated with resin decomposition due to the phosphorescent agent, the content ratio of the aromatic polycarbonate resin is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, even more preferably 1 part by mass or less, and particularly preferably substantially 0, relative to 100 parts by mass of the aliphatic polycarbonate resin (A).

[0085] (Synthesis of Aliphatic Polycarbonate Resin (A)) The aliphatic polycarbonate resin (A) can be obtained, for example, by polycondensing a dihydroxy compound such as compound (1) with a carbonic acid diester through an ester exchange reaction in the presence of a polymerization catalyst.

[0086] The dihydroxy compound and the carbonic acid diester are preferably mixed uniformly before the transesterification reaction. The mixing temperature is usually 80°C or higher, preferably 90°C or higher, and usually 250°C or lower, preferably 200°C or lower, more preferably 150°C or lower. The mixing temperature is particularly preferably 100°C or higher and 120°C or lower. In this case, the dissolution rate can be increased and the solubility can be sufficiently improved, and problems such as solidification can be sufficiently avoided. Furthermore, in this case, the thermal deterioration of the dihydroxy compound can be sufficiently suppressed. As a result, the color tone of the polycarbonate resin (A) becomes even better, and the weather resistance can also be improved.

[0087] The operation of mixing the dihydroxy compound and the carbonic acid diester is usually carried out under atmosphere control. Specifically, the oxygen concentration during mixing is preferably 10 vol% or less, more preferably 0.0001 to 10 vol%, further preferably 0.0001 to 5 vol%, and even more preferably 0.0001 to 1 vol%. In this case, the color tone of the polycarbonate resin (A) becomes more favorable and the reactivity can be increased.

[0088] In order to obtain the aliphatic polycarbonate resin (A), it is preferable to use the carbonic acid diester in a molar ratio of 0.90 to 1.20 relative to the total dihydroxy compounds used in the reaction. In this case, the increase in the amount of hydroxyl group terminals in the aliphatic polycarbonate resin can be suppressed, and the thermal stability of the polymer can be improved. Therefore, coloring during molding can be further prevented and the rate of the transesterification reaction can be improved. In addition, it is possible to more reliably obtain a desired high molecular weight material. Furthermore, by adjusting the amount of the carbonic acid diester used within the above range, the decrease in the rate of the transesterification reaction can be suppressed, and the aliphatic polycarbonate resin (A) having the desired molecular weight can be more reliably produced. In addition, in this case, the increase in the thermal history during the reaction can be suppressed, and the color tone and weather resistance of the aliphatic polycarbonate resin (A) can be further improved. Furthermore, in this case, the amount of the remaining carbonic acid diester in the aliphatic polycarbonate resin (A) can be reduced, and the generation of stains and odors during molding can be avoided or alleviated. From the same viewpoint as above, the amount of the carbonic acid diester used relative to the total dihydroxy compounds is more preferably 0.95 to 1.10 in terms of molar ratio.

[0089] The method of polycondensing a dihydroxy compound and a carbonic acid diester is carried out in multiple stages using multiple reactors in the presence of the above-mentioned catalyst. The reaction may be carried out in a batchwise manner, a continuous manner, or a combination of a batchwise manner and a continuous manner, but it is preferable to adopt a continuous manner, which is excellent in productivity and can obtain a polycarbonate resin (A) with less heat history.

[0090] From the viewpoint of controlling the polymerization rate and the quality of the resulting aliphatic polycarbonate resin (A), it is preferable to appropriately select the jacket temperature, the internal temperature, and the pressure in the reaction system according to the reaction stage. Specifically, it is preferable to obtain a prepolymer at a relatively low temperature and low vacuum in the early stage of the polycondensation reaction, and to increase the molecular weight to a predetermined value at a relatively high temperature and high vacuum in the later stage of the reaction. In this case, the distillation of unreacted monomers is suppressed, and it becomes easier to adjust the molar ratio of the dihydroxy compound and the carbonate diester to a desired ratio. As a result, it is possible to suppress a decrease in the polymerization rate. In addition, it becomes possible to more reliably obtain a polymer having a desired molecular weight and terminal group.

[0091] In addition, the polymerization rate in the polycondensation reaction is controlled by the balance between the hydroxyl group terminals and the carbonate group terminals. Therefore, if the balance of the terminal groups fluctuates due to the distillation of unreacted monomers, it becomes difficult to control the polymerization rate at a constant rate, and there is a risk that the molecular weight of the resulting resin will fluctuate greatly. Since the molecular weight of the resin correlates with the melt viscosity, when the resulting resin is melt-processed, the melt viscosity may fluctuate, making it difficult to maintain a constant quality of the molded product. This problem is particularly likely to occur when the polycondensation reaction is carried out in a continuous manner.

[0092] In order to suppress the amount of unreacted monomers distilled off, it is effective to use a reflux condenser in the polymerization reactor, and this is particularly effective in the early stage of the reaction when there is a large amount of unreacted monomers. The temperature of the coolant introduced into the reflux condenser can be appropriately selected depending on the monomers used, but the temperature of the coolant introduced into the reflux condenser is usually 45 to 180°C, preferably 80 to 150°C, and more preferably 100 to 130°C at the inlet of the reflux condenser. By adjusting the coolant temperature within these ranges, the reflux amount can be sufficiently increased, the effect can be fully obtained, and the efficiency of distilling off the monohydroxy compound to be distilled off can be sufficiently improved. As a result, the reaction rate can be prevented from decreasing, and coloring of the obtained resin can be further prevented. As the coolant, hot water, steam, heat transfer oil, etc. are used, and steam and heat transfer oil are preferred.

[0093] In order to obtain a better color tone of the resulting polycarbonate resin (A) while maintaining an appropriate polymerization rate and suppressing distillation of monomers, it is preferable to appropriately select the type and amount of the above-mentioned polymerization catalyst.

[0094] The polycarbonate resin (A) is usually produced through two or more steps using a polymerization catalyst. The polycondensation reaction may be carried out in two or more steps using one polycondensation reactor, with the conditions being changed sequentially, but from the viewpoint of production efficiency, it is preferable to carry out the reaction in multiple steps using multiple reactors, with the conditions being changed for each step.

[0095] From the viewpoint of efficiently carrying out the polycondensation reaction, in the early stage of the reaction in which the reaction solution contains a large amount of monomers, it is preferable to suppress the volatilization of the monomers while maintaining the necessary polymerization rate. In addition, in the later stage of the reaction, it is preferable to shift the equilibrium to the polycondensation reaction side by sufficiently distilling off the by-product monohydroxy compound. Therefore, the reaction conditions suitable for the early stage of the reaction and the reaction conditions suitable for the later stage of the reaction are usually different. Therefore, by using a plurality of reactors arranged in series, the respective conditions can be easily changed, and the production efficiency can be improved.

[0096] As described above, the number of polymerization reactors used in the production of the polycarbonate resin (A) may be at least two, but from the viewpoint of production efficiency, etc., the number is three or more, preferably 3 to 5, and particularly preferably 4. When the number of polymerization reactors is two or more, each polymerization reactor may further carry out a plurality of reaction stages under different conditions, or the temperature and pressure may be changed continuously.

[0097] The polymerization catalyst can be added to a raw material preparation tank or a raw material storage tank, or can be added directly to a polymerization reactor. From the viewpoint of supply stability and control of the polycondensation reaction, it is preferable to install a catalyst supply line in the raw material line before the raw material is supplied to the polymerization reactor, and supply the polymerization catalyst in the form of an aqueous solution.

[0098] By adjusting the temperature of the polycondensation reaction, it is possible to improve productivity and prevent the increase of the heat history of the product. Furthermore, it is possible to further prevent the volatilization of the monomer and the decomposition and coloration of the polycarbonate resin (A). Specifically, the following conditions can be adopted as the reaction conditions in the first stage reaction. That is, the maximum temperature inside the polymerization reactor is set in the range of usually 150 to 250°C, preferably 160 to 240°C, and more preferably 170 to 230°C. In addition, the pressure of the polymerization reactor (hereinafter, pressure refers to absolute pressure) is set in the range of usually 1 to 110 kPa, preferably 5 to 70 kPa, and more preferably 7 to 30 kPa. In addition, the reaction time is set in the range of usually 0.1 to 10 hours, and preferably 0.5 to 3 hours. It is preferable that the first stage reaction is carried out while distilling off the generated monohydroxy compound outside the reaction system.

[0099] From the second stage onwards, it is preferable to gradually reduce the pressure of the reaction system from the pressure of the first stage, and to finally reduce the pressure (absolute pressure) of the reaction system to 1 kPa or less while removing the monohydroxy compound that is subsequently generated from the reaction system. The maximum internal temperature of the polymerization reactor is usually set in the range of 200 to 260° C., preferably 210 to 250° C. The reaction time is usually set in the range of 0.1 to 10 hours, preferably 0.3 to 6 hours, more preferably 0.5 to 3 hours.

[0100] From the viewpoint of further suppressing coloration and thermal deterioration of the polycarbonate resin (A) and achieving a better color tone, it is preferable that the maximum internal temperature of the polymerization reactor in all reaction stages is 210 to 240° C. In order to prevent a decrease in the polymerization rate in the latter half of the reaction and to minimize deterioration due to thermal history, it is preferable to use a horizontal reactor having excellent plug flow properties and interface renewal properties in the final stage of the polycondensation reaction.

[0101] In the continuous polymerization, in order to control the molecular weight of the finally obtained polycarbonate resin (A) at a constant level, it is preferable to adjust the polymerization rate as necessary. In this case, from the viewpoint of good operability, it is preferable to adjust the pressure of the polymerization reactor in the final stage.

[0102] In addition, since the polymerization rate changes depending on the ratio of the hydroxyl group end and the carbonate group end as described above, the polymerization rate is suppressed by intentionally reducing one of the end groups, and the pressure of the final stage polymerization reactor is kept at a high vacuum, so that the remaining low molecular weight components in the resin, including monohydroxy compounds, can be reduced. However, if one of the ends is too small, even a slight change in the end group balance can cause the reactivity to drop extremely, and the molecular weight of the polycarbonate resin (A) may not reach the desired molecular weight. From the viewpoint of suppressing the drop in reactivity and increasing the molecular weight, it is preferable that the polycarbonate resin in the final stage polymerization reactor contains both hydroxyl group end and carbonate group end at 10 mol / ton or more. In addition, if both end groups are too large, the polymerization rate becomes fast and the molecular weight becomes too high, so it is preferable that one of the end groups is 60 mol / ton or less.

[0103] In this way, by adjusting the amount of terminal groups and the pressure of the final stage polymerization reactor within a preferred range, the amount of monohydroxy compounds remaining in the resin at the outlet of the polymerization reactor can be reduced. The amount of monohydroxy compounds remaining in the resin at the outlet of the polymerization reactor is preferably 2000 ppm by weight or less, more preferably 1500 ppm by weight or less, and even more preferably 1000 ppm by weight or less. By reducing the content of monohydroxy compounds at the outlet of the polymerization reactor in this way, it is possible to easily remove the monohydroxy compounds and the like in the subsequent steps.

[0104] Although it is preferable that the amount of remaining monohydroxy compounds is small, in order to reduce it to less than 100 ppm by weight, it is necessary to extremely reduce the amount of one of the terminal groups and adopt operating conditions such as maintaining the pressure of the polymerization reactor at a high vacuum. In this case, as described above, it becomes difficult to maintain the molecular weight of the obtained polycarbonate resin at a constant level, so the amount is usually 100 ppm by weight or more, preferably 150 ppm by weight or more.

[0105] From the viewpoint of effective resource utilization, it is preferable to reuse the by-produced monohydroxy compound as a raw material for other compounds after purifying it as necessary. For example, when the monohydroxy compound is phenol, it can be used as a raw material for diphenyl carbonate, bisphenol A, etc.

[0106] The polycarbonate resin (A) preferably contains a catalyst deactivator. The catalyst deactivator is not particularly limited as long as it is an acidic substance and has a function of deactivating the polymerization catalyst, but specifically includes phosphoric acid, trimethyl phosphate, triethyl phosphate, phosphorous acid, octyl sulfonate tetrabutyl phosphonium salt, benzenesulfonate tetramethyl phosphonium salt, benzenesulfonate tetrabutyl phosphonium salt, dodecylbenzenesulfonate tetrabutyl phosphonium salt, p-toluenesulfonate tetrabutyl phosphonium salt and other phosphonium salts; decylsulfonate tetramethyl ammonium salt, dodecylbenzenesulfonate tetrabutyl ammonium salt and other ammonium salts; benzenesulfonate methyl, benzenesulfonate butyl, p-toluenesulfonate methyl, p-toluenesulfonate butyl, hexadecylsulfonate ethyl and other alkyl esters.

[0107] The catalyst deactivator preferably contains a phosphorus-based compound (hereinafter referred to as a "specific phosphorus-based compound") containing either a partial structure represented by the following formula (6) or the following formula (7). Such a specific phosphorus-based compound can be added after the completion of the polycondensation reaction, that is, for example, during the kneading process or the pelletizing process, to deactivate the polymerization catalyst and suppress the unnecessary polycondensation reaction from proceeding. As a result, even if a resin composition containing the polycarbonate resin (A) is heated in, for example, a molding process, the progress of polycondensation can be suppressed. Furthermore, the elimination of the monohydroxy compound can be suppressed. In addition, by deactivating the polymerization catalyst, coloration of the polycarbonate resin (A) at high temperatures can be further suppressed.

[0108] [ka]

[0109] [ka]

[0110] The specific phosphorus-based compound containing the partial structure represented by formula (6) or formula (7) may be phosphoric acid, phosphorous acid, phosphonic acid, hypophosphorous acid, polyphosphoric acid, phosphonate ester, acidic phosphate ester, etc. Among these, from the viewpoint of more excellent effects of catalyst deactivation and coloration inhibition, the specific phosphorus-based compound is preferably phosphorous acid, phosphonic acid, or phosphonate ester, and more preferably phosphorous acid.

[0111] Phosphonic acids include, for example, phosphonic acid (i.e., phosphorous acid), methylphosphonic acid, ethylphosphonic acid, vinylphosphonic acid, decylphosphonic acid, phenylphosphonic acid, benzylphosphonic acid, aminomethylphosphonic acid, methylene diphosphonic acid, 1-hydroxyethane-1,1-diphosphonic acid, 4-methoxyphenylphosphonic acid, nitrilotris(methylenephosphonic acid), propylphosphonic anhydride, and the like.

[0112] Examples of phosphonate esters include dimethyl phosphonate, diethyl phosphonate, bis(2-ethylhexyl) phosphonate, dilauryl phosphonate, dioleyl phosphonate, diphenyl phosphonate, dibenzyl phosphonate, dimethyl methylphosphonate, diphenyl methylphosphonate, diethyl ethylphosphonate, diethyl benzylphosphonate, dimethyl phenylphosphonate, diethyl phenylphosphonate, dipropyl phenylphosphonate, diethyl (methoxymethyl)phosphonate, diethyl vinylphosphonate, and hydroxymethyl phosphonate. diethyl thiophosphonate, dimethyl (2-hydroxyethyl)phosphonate, diethyl p-methylbenzylphosphonate, diethylphosphonoacetic acid, ethyl diethylphosphonoacetate, tert-butyl diethylphosphonoacetate, diethyl (4-chlorobenzyl)phosphonate, diethyl cyanophosphonate, diethyl cyanomethylphosphonate, diethyl 3,5-di-tert-butyl-4-hydroxybenzylphosphonate, diethylphosphonoacetaldehyde diethyl acetal, and diethyl (methylthiomethyl)phosphonate.

[0113] Examples of acidic phosphate esters include phosphate diesters such as dimethyl phosphate, diethyl phosphate, divinyl phosphate, dipropyl phosphate, dibutyl phosphate, bis(butoxyethyl) phosphate, bis(2-ethylhexyl) phosphate, diisotridecyl phosphate, dioleyl phosphate, distearyl phosphate, diphenyl phosphate, dibenzyl phosphate, etc. In addition, mixtures of diesters and monoesters, diethyl chlorophosphate, zinc stearyl phosphate, etc. may also be mentioned.

[0114] The specific phosphorus-based compound may be used alone or in any combination of two or more kinds in any ratio.

[0115] The content of the specific phosphorus compound in the polycarbonate resin (A) is preferably 0.1 ppm by weight or more and 5 ppm by weight or less in terms of phosphorus atom weight. In this case, the effect of catalyst deactivation and coloring inhibition by the specific phosphorus compound can be sufficiently obtained. In addition, in this case, coloring of the polycarbonate resin (A) can be further prevented, especially in durability tests at high temperature and high humidity.

[0116] In addition, the effect of suppressing catalyst deactivation and coloration can be more reliably obtained by adjusting the content of the specific phosphorus compound according to the amount of the polymerization catalyst. The content of the specific phosphorus compound is preferably 0.5 to 5 times the mol of phosphorus atoms, more preferably 0.7 to 4 times the mol of phosphorus atoms, and even more preferably 0.8 to 3 times the mol of phosphorus atoms, per mol of metal atoms of the polymerization catalyst.

[0117] [Luminescent agent (B)] When irradiated with ultraviolet light or visible light contained in sunlight or artificial light, the luminous agent absorbs and stores the light, and continues to emit light for a certain period of time even after the light irradiation is stopped, i.e., even in a dark place. The luminous agent has a persistence of afterglow for several minutes to several tens of hours after the end of photoexcitation, and is distinguished from general fluorescent whitening agents, whose luminescence decays quickly after the light irradiation is stopped.

[0118] The luminescent agent (B) may be any agent having the above-mentioned characteristics, and is not particularly limited. Examples of the luminescent agent include sulfide-based luminescent agents, zinc sulfide-based luminescent agents, silicic acid-based luminescent materials, and aluminate-based luminescent agents. Examples of the sulfide-based luminescent agents include CaS:Bi, CaSrS:Bi, and ZnCdS:Cu. Examples of the zinc sulfide-based luminescent agents include ZnS:Cu. Examples of the silicic acid-based luminescent agents include Sr2MgSi2O7:Eu,Dy, and the like. Examples of the aluminate-based luminescent agents include substances represented by the following formula (III). In formula (III), M represents an alkaline earth metal element, and is preferably at least one element selected from the group consisting of calcium (Ca), strontium (Sr), and barium (Ba). X is an activator, and represents at least one element selected from the group consisting of lanthanoid metal elements, manganese (Mn), tin (Sn), and bismuth (Bi). X is preferably at least one element selected from the group consisting of europium (Eu), lanthanum (La), cerium (Cs), praseodymium (Pr), neodymium (Nd), samarium (Sm), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), ruthenium (Lu), manganese (Mn), tin (Sn), and bismuth (Bi). In formula (III), a, b, and c are integers of 1 to 30. In formula (III), the content of X is, for example, 0.001 to 10 mol% or less with respect to 100 mol% of the alkaline earth metal element M. The aluminate-based phosphorescent agent is, for example, composed of a mother crystal composed of an aluminate and an activator. M a Al b O c :X (III)

[0119] The luminescent agent (B) is preferably an aluminate-based luminescent agent represented by formula (III). In this case, the polycarbonate resin composition exhibits high luminescence brightness. This is believed to be because the ions derived from the activator are excited by light irradiation at the portion substituted with the ions derived from the activator in the mother crystal, and energy is released in the form of strong light emission for a long period of time.

[0120] Examples of aluminate-based phosphorescent agents include GMg2Al 16 O 27 :Eu, GMg2Al 16 O 27 :Eu,Mn,GMg2Al 10 O 17 :Eu, GMg2Al 10 O 17 :Eu,Mn, SrAl2O4:Eu, SrAl2O4:Eu,Dy, Sr4Al 14 O 25 :Eu, Sr4Al 14 O 25 :Eu,Dy, CaAl2O4:Eu,Nd, etc., where G is Sr and / or Ba. Aluminate-based phosphorescent agents include SrAl2O4:Eu,Dy, Sr4Al 14 O 25 It is preferable that the material is at least one selected from the group consisting of CaAl2O4:Eu,Dy, and CaAl2O4:Eu,Nd, in which case the hydrolysis suppression effect and the afterglow sustaining effect are further improved.

[0121] Average particle size D of phosphorescent agent (B) 50 Although there is no particular limitation on the thickness, it is preferably 1 to 300 μm, more preferably 10 to 100 μm, and even more preferably 20 to 50 μm. In this case, the tensile elongation at break, impact strength, appearance, and luminescence properties of the molded article are further improved.

[0122] In the present invention, the average particle size D 50 is the median diameter D measured by a laser diffraction particle size analyzer 50 For example, the average particle size D 50 is measured using a laser diffraction particle size distribution analyzer SALD-2100 manufactured by Shimadzu Corporation, but for commercially available products, for example, catalog values ​​can be used.

[0123] The resin composition may contain one type of luminescent agent, or may contain two or more types of luminescent agents having different chemical compositions. The resin composition may also contain luminescent agents having different average particle sizes.

[0124] [Resin composition] The polycarbonate resin composition contains an aliphatic polycarbonate resin (A) and a luminous agent (B). The aliphatic polycarbonate resin (A) has a structural unit derived from, for example, an aliphatic dihydroxy compound. According to such a polycarbonate resin composition, a molded product having a good external hue and high luminous brightness in a dark place can be obtained.

[0125] In the case of an aromatic polycarbonate resin mainly composed of structural units derived from a dihydroxy compound containing an aromatic group such as bisphenol A, the addition of a luminescent agent (B) reduces the impact resistance of the resin composition due to the decomposition of the polycarbonate resin. Furthermore, the molded product is blackened, which impairs its aesthetic appearance and reduces the luminance. In contrast, the resin composition of the present disclosure contains a polycarbonate resin (specifically, an aliphatic polycarbonate resin (A)) and a luminescent agent (B), but the resin decomposition is suppressed, the external hue of the molded product of the resin composition is improved, and the luminance in the dark is increased.

[0126] The mass ratio of the polycarbonate resin (A) to the luminescent agent (B) in the polycarbonate resin composition (wherein the polycarbonate resin (A) : luminescent agent (B)) is preferably 50:50 to 99:1, more preferably 75:25 to 98:2, and even more preferably 90:10 to 97:3. In this case, the afterglow effect of the luminescent agent (B) is improved, and moldability, thermal stability, and mechanical strength are also improved.

[0127] The resin composition may contain an impact strength modifier (C), an ultraviolet absorber (D) and an ester exchange inhibitor (F).

[0128] (Impact Strength Modifier (C)) As the impact strength modifier (C), any commonly known agent having the effect of improving impact resistance can be used, and the impact strength modifier is not particularly limited. The impact strength modifier is preferably composed of a polymer (including copolymer) of at least one monomer selected from the group consisting of butadiene, alkyl (meth)acrylate, styrene, and acrylonitrile. In this case, the combination of the impact strength modifier (C) and the polycarbonate resin (A) becomes good, and the impact strength modification effect becomes remarkable. As a result, the molded product of the resin composition exhibits excellent impact resistance. In addition, "(meth)acrylic acid" means at least one of acrylic acid and methacrylic acid.

[0129] From the viewpoint of easy availability, it is preferable that the impact strength modifier (C) is composed of a copolymer containing a component derived from butadiene. A copolymer containing a component derived from butadiene is appropriately called a "butadiene-based copolymer". Examples of butadiene-based copolymers include copolymers of butadiene and at least one compound (i.e., monomer) selected from the group consisting of styrene, acrylonitrile, and alkyl (meth)acrylate.

[0130] Specific examples of butadiene-based copolymers include copolymers of butadiene and styrene; copolymers of butadiene, styrene, and acrylonitrile; copolymers of butadiene, styrene, acrylonitrile, and alkyl (meth)acrylate; copolymers of butadiene, styrene, and alkyl (meth)acrylate; and copolymers of butadiene and alkyl (meth)acrylate.

[0131] Preferred specific examples of the butadiene-based copolymer include SBS (styrene-butadiene-styrene block) copolymer, ABS (acrylonitrile-butadiene-styrene) copolymer, MBS (methyl methacrylate-butadiene-styrene) copolymer, MABS (methyl methacrylate-acrylonitrile-butadiene-styrene) copolymer, MB (methyl methacrylate-butadiene) copolymer, and methyl methacrylate-acrylic-butadiene rubber copolymer.

[0132] From the viewpoint of impact strength modifying effect, the butadiene-based copolymer is preferably a copolymer of butadiene and alkyl (meth)acrylate, and more preferably a butadiene-alkyl acrylate-alkyl methacrylate copolymer.

[0133] The structure of the impact modifier composed of the butadiene copolymer is not particularly limited, but specific examples include a crosslinked structure, a block structure, and a core-shell structure. A core-shell structure is preferable. The core-shell structure is preferably composed of a core that is a rubber-like polymer and a shell that is composed of a polymer obtained by graft polymerization to the rubber-like polymer. In this case, the dispersibility of the butadiene copolymer in the polycarbonate resin (A) is improved, and the resin composition and its molded article tend to show high impact strength. In addition, in this case, the transparency of the resin composition and its molded article is further improved.

[0134] An example of a butadiene-based copolymer having a core-shell structure is a core-shell type graft copolymer in which a butadiene-containing polymer is used as a core layer and a copolymerizable monomer component is graft-copolymerized to form a shell layer. Among these, a core-shell type graft copolymer in which an alkyl (meth)acrylate is used as a shell layer is preferred. An example of a butadiene-based copolymer composed of such a core-shell type graft copolymer is "Paraloid (registered trademark) EXL2650J" manufactured by Dow Chemical Company.

[0135] From the viewpoint of easy availability, it is preferable that the impact strength modifier is composed of a copolymer containing a component derived from an alkyl (meth)acrylate. A copolymer containing a component derived from an alkyl (meth)acrylate is appropriately called an "alkyl (meth)acrylate copolymer". Examples of the alkyl (meth)acrylate copolymer include, in addition to the above-mentioned butadiene-based copolymers, copolymers of alkyl (meth)acrylate and styrene, copolymers of alkyl (meth)acrylate and acrylic rubber, copolymers of alkyl (meth)acrylate, styrene and acrylic rubber, and copolymers of alkyl (meth)acrylate and acrylic-silicone IPN rubber. IPN means interpenetrating polymer network structure.

[0136] From the viewpoint of further improving the transparency of the resin composition and the molded article thereof, the impact strength modifier (C) is preferably a copolymer of alkyl (meth)acrylate and styrene, and more preferably an alkyl acrylate-alkyl methacrylate-styrene copolymer.

[0137] The structure of the impact modifier (C) composed of an alkyl (meth)acrylate copolymer is not particularly limited, but specific examples include a crosslinked structure, a block structure, and a core-shell structure. Of these, the structure of the impact modifier is preferably a core-shell structure consisting of a core that is a rubber-like polymer and a shell obtained by graft polymerization to the rubber-like polymer. In this case, the dispersibility of the alkyl (meth)acrylate copolymer in polycarbonate is improved, and the polycarbonate resin composition and its molded product tend to exhibit high impact strength. In addition, in this case, the transparency of the polycarbonate resin composition and its molded product is further improved. An example of an alkyl (meth)acrylate copolymer composed of such a core-shell type graft copolymer is "Kane Ace M-590" manufactured by Kaneka Corporation.

[0138] (Ultraviolet absorber (D)) The ultraviolet absorber (D) may be any commonly known ultraviolet absorber, and is not particularly limited. Specific examples include benzotriazole-based ultraviolet absorbers.

[0139] (Interesterification inhibitor (F)) The transesterification inhibitor (F) may be any commonly known agent having the effect of inhibiting transesterification, and is not particularly limited. Specific examples include phosphate esters.

[0140] The resin composition may also contain additives such as a neutralizing agent, a release agent, a colorant, an antistatic agent, a slip agent, a lubricant, a plasticizer, a compatibilizer, a flame retardant, and a filler.

[0141] [Physical properties of resin composition] (1) Liquidity The fluidity of the polycarbonate resin composition is evaluated, for example, by measuring MFR (i.e., melt flow rate). The ratio (i.e., MFR1 / MFR2) of the MFR value of the resin composition (i.e., MFR2) to the MFR value of the polycarbonate resin (A) (i.e., MFR1) is preferably 1.5 or less, more preferably 1.3 or less. This range further suppresses the decomposition of the polycarbonate resin. The method for measuring MFR will be described in the Examples, and the MFR of the resin composition and the polycarbonate resin is a value measured under the conditions of a temperature of 230°C and a load of 2.16 kg.

[0142] (2) Hue The color of the resin composition (specifically, the color of the molded product) is L specified in JIS Z8781-4:2013. * Value, C * It can be evaluated by the value of L * The higher the value, the brighter the color. A value of 40 or more is preferable, and a value of 45 or more is more preferable. * The higher the value, the more vivid the color. 8.2 or more is preferable, and 8.5 or more is even more preferable. * Value, C *By keeping the value within the above range, the molded product will have less blackening and will have an excellent appearance. * Value, C * The method for measuring the values ​​will be described in the Examples.

[0143] (3) Initial luminance The initial luminance of the resin composition (specifically, the initial luminance of the molded article) is evaluated by the luminance in a dark place after light irradiation. The higher the initial luminance, the higher the luminance of the molded article of the resin composition, without inhibiting the inherent luminous performance of the phosphorescent agent. The method for measuring the initial luminance of light will be described in the examples.

[0144] [Method for producing resin composition] The resin composition can be produced by, for example, mechanically melt-kneading the components such as the polycarbonate resin (A) and the luminescent agent (B). Examples of the melt-kneader include a single-screw extruder, a twin-screw extruder, a Brabender, a Banbury mixer, a kneader blender, and a roll mill. It is preferable to use a twin-screw extruder as the melt-kneader.

[0145] From the viewpoint of distilling off the remaining phenol, it is preferable that the melt kneading is carried out under reduced pressure. The kneading temperature is usually 100°C or higher, preferably 145°C or higher, more preferably 160°C or higher. The kneading temperature is usually 350°C or lower, preferably 300°C or lower, more preferably 250°C or lower. When kneading, each component may be kneaded at once, or a multi-stage division kneading method may be adopted. The multi-stage division kneading method is a method in which an arbitrary component is kneaded, and then the remaining components are added and kneaded. The extruded kneaded product is preferably pelletized using a strand cutter or the like, and appropriately dried before use.

[0146] [Method of molding resin composition] The resin composition is molded by various molding methods such as injection molding (specifically, insert molding, two-color molding, sandwich molding, gas injection molding, etc.), extrusion molding, inflation molding, T-die film molding, lamination molding, blow molding, hollow molding, compression molding, and calendar molding. The shape of the molded product is not particularly limited, and examples thereof include sheets, films, plates, particles, lumps, fibers, rods, porous bodies, and foams, and are preferably sheets, films, and plates. The molded film can also be uniaxially or biaxially stretched. Examples of the stretching method include a roll method, a tenter method, and a tubular method. Furthermore, the molded product can be subjected to surface treatment such as corona discharge treatment, flame treatment, plasma treatment, and ozone treatment.

[0147] [Application] The uses of the molded article are not particularly limited, but examples include the following uses: That is, evacuation guidance signs, night display signs, display buttons, clock dials, switches, connector parts, accessories, electric wires, cords, wire harnesses, etc. in the electric and electronic parts field, insulating sheets, displays and touch panels for office equipment, membrane switches, photo covers, relay parts, coil bobbins, IC sockets, fuse cases, camera pressure plates, FDD collets, floppy disk hubs, optical disk substrates, optical disk pickup lenses, optical lenses, LCD substrates, PDP substrates, TV screens for projection TVs, retardation films, fog lamp lenses, illuminated switch lenses, sensor switch lenses, Fresnel lenses, protective glasses, projection lenses, camera lenses, sunglasses, light guide plates, camera strobe reflectors, LED reflectors, headlamp lenses, turn signal lamp lenses, tail lamp lenses, resin window glass, meter covers, outer panels, door handles, rear panels, wheel caps, visors, roof rails, sunroofs, instrument panels, panels, control cable coating materials, Airbag covers, mudguards, bumpers, boots, air hoses, lamp packings, gaskets, window moldings and other moldings, site shields, weather strips, glass run channels, grommets, vibration control and sound insulation materials, joint materials in the building materials field, handrails, windows, table edge materials, sashes, bathtubs, window frames, signs, lighting covers, water tanks, staircase pedestals, carports, highway sound insulation walls, multi-wall sheets, steel wire covering materials, lighting globes, switch breakers, protective covers for machine tools, industrial deep drawn vacuum formed containers, pump hubs Housings, home appliances, various packings in the light electrical field, grips, belts, rubber feet, rollers, protectors, suction cups, gaskets used in refrigerators, etc., switches, connector covers, game machine covers, pachinko machines, OA housings, notebook PC housings, trays for HDD heads, instrument windows, transparent housings, rollers with OA gears, switch case sliders, gas cock knobs, watch frames, watch gear train center pieces, amber caps, various rolls for OA equipment, hoses, tubes and other tubular molded products, irregular extrusion products, leather-like products,Examples of the molded articles include toys such as bite tools, soft-touch dolls, pen grips, straps, suction cups, watches, umbrella bones, cosmetic cases, toothbrush handles, and other general goods, containers such as housewares and Tupperware, cable ties, various bottles such as blow-molded infusion bottles, food bottles, water bottles, and bottles for personal care such as cosmetics, catheters, syringes, syringe gaskets, drip tubes, tubes, ports, caps, rubber stoppers, dialyzers, blood connectors, dentures, disposable containers, and the like in medical parts. The molded articles can be foam molded articles, and can be used in applications where foamed resins are used. The molded articles are also suitable for automobile interior or exterior parts.

[0148] The molded articles are preferably used for evacuation guidance signs, nighttime display signs, indicator buttons, clock dials, switches, connector parts, or accessories. In this case, the molded articles' properties of excellent luminous effect and afterglow effect are fully exhibited, resulting in excellent aesthetics and functionality. EXAMPLES

[0149] The present invention will be described in more detail below with reference to Production Examples, Examples, and Comparative Examples, but the present invention is not limited to these Examples in any way.

[0150] <Evaluation method> (1) Liquidity evaluation (MFR measurement) Aliphatic polycarbonate resin and resin composition containing same Using a hot air dryer, the pellets of the aliphatic polycarbonate resin and the pellets of the resin composition were dried for 6 hours or more at 100° C. Next, the MFR of each pellet was measured using a melt indexer (manufactured by Toyo Seiki Seisakusho) under conditions of a temperature of 230° C. and a load of 2.16 kg. Bisphenol A polycarbonate resin composition Using a hot air dryer, pellets of the bisphenol A polycarbonate resin composition were dried for 6 hours or more at 120° C. Next, the MFR of the pellets was measured using a melt indexer (manufactured by Toyo Seiki Seisakusho) under conditions of a temperature of 300° C. and a load of 1.20 kg.

[0151] (2) Glass transition temperature Tg The measurements were performed using a differential scanning calorimeter DSC6220 manufactured by SII Nano Technology. Approximately 10 mg of polycarbonate resin was placed in an aluminum pan manufactured by the same company, sealed, and heated from 30°C to 250°C at a heating rate of 20°C / min under a nitrogen gas flow of 50 mL / min. After holding the temperature for 3 minutes, the sample was cooled to 30°C at a rate of 20°C / min. The sample was held at 30°C for 3 minutes and then heated again to 200°C at a rate of 20°C / min. From the DSC data obtained in the second heating, the extrapolated glass transition onset temperature was calculated, which is the temperature at the intersection of a straight line extending the low-temperature baseline to the high-temperature side and a tangent drawn at the point where the gradient of the curve of the step-like change in the glass transition is maximum. This extrapolated glass transition onset temperature was taken as the glass transition temperature.

[0152] (3) Hue measurement The pellets of the resin composition were dried at 100°C for 6 hours using a hot air dryer. Next, the pellets were fed into an injection molding machine (J85AD type manufactured by Japan Steel Works, Ltd.) and injection molded under conditions of a resin temperature of 240°C, a mold temperature of 60°C, and a molding cycle of 40 seconds to obtain an injection molded plate of width 100 mm x length 100 mm x thickness 2 mm. The injection molded plate was stored in a dark place for 48 hours or more to completely block out light, and then the L of the injection molded plate was measured using a color tone device "CM-5" manufactured by Konica Minolta, Inc. * Value, C * The value was measured. The measurement was performed with the following light source: D 65 The measurement was performed using a reflection method under the conditions of a viewing angle of 10° and a reflection measurement diameter of φ30 mm.

[0153] (4) Evaluation of initial luminance The injection molded plate was stored in a dark place for more than 48 hours, completely blocked from light, and then the D 65 The light source was irradiated for 10 minutes, and the luminance of the light was visually observed in a dark place immediately after the irradiation was stopped. The evaluation was done on a 5-point scale, with 5 being the brightest and smaller numbers being assigned as the dimmer the light became. 1 means the darkest.

[0154] [Component (A): Polycarbonate resin] <Ingredients> ISB: Isosorbide (manufactured by Rocket Fleuret, product name: POLYSORB) CHDM: 1,4-cyclohexanedimethanol (cis-trans mixture, manufactured by SK Chemicals Co., Ltd.) DPC: Diphenyl carbonate (Mitsubishi Chemical Corporation)

[0155] <Production Example 1: Aliphatic Polycarbonate Resin (A-1)> Polycarbonate resin was polymerized using a continuous polymerization system consisting of three vertical stirring reactors, one horizontal stirring reactor, and a twin-screw extruder. ISB, CHDM, and DPC were melted in tanks, respectively, and continuously fed to the first vertical stirring reactor at flow rates of 29.8 kg / hr for ISB, 12.6 kg / hr for CHDM, and 63.1 kg / hr for DPC (molar ratio ISB / CHDM / DPC=0.700 / 0.300 / 1.010). Along with the feeding of each raw material, an aqueous solution of calcium acetate monohydrate, which is a polymerization catalyst, was fed to the first vertical stirring reactor in an amount such that 1.5 μmol of calcium acetate monohydrate was added to 1 mol of all dihydroxy compounds. The internal temperature, internal pressure, and residence time of each reactor were as follows: first vertical stirring reactor: 190°C, 25kPa, 120 minutes, second vertical stirring reactor: 195°C, 10kPa, 90 minutes, third vertical stirring reactor: 205°C, 4kPa, 45 minutes, fourth horizontal stirring reactor: 220°C, 0.1-1.0kPa, 120 minutes. The internal pressure of the fourth horizontal stirring reactor was finely adjusted during operation so that the reduced viscosity of the resulting polycarbonate resin was 0.42dL / g-0.44dL / g.

[0156] The polycarbonate resin extracted from the fourth horizontal stirred reactor was fed in a vented twin-screw extruder TEX30α [manufactured by Japan Steel Works, Ltd.] in a molten state. The extruder had three vacuum vents, where the remaining low molecular weight components in the resin were removed by volatilization, and phosphonic acid was added as a catalyst deactivator just before the first vent at 0.63 ppm by weight relative to the polycarbonate resin, and Irganox1010, AS2112, E-275, and SEESORB709 were added just before the third vent at 1000 ppm by weight, 500 ppm by weight, 3000 ppm by weight, and 200 ppm by weight relative to the polycarbonate resin, respectively. The polycarbonate resin that had passed through the extruder was passed through a 10 μm Ultipleats candle filter [manufactured by PALL] in a molten state to filter out foreign matter. The polycarbonate resin was then extruded from the die in the form of strands, cooled with water, solidified, and cut into pellets with a rotary cutter to obtain an aliphatic polycarbonate resin (A-1). This aliphatic polycarbonate resin had a glass transition temperature of 124°C and an MFR (230°C, 2.16 kg) of 10 g / min.

[0157] <Bisphenol A polycarbonate resin> As the bisphenol A type polycarbonate resin, the following commercially available products (A-1, A-2) were used. A-2: Iupilon H-3000 (Mitsubishi Engineering Plastics, MFR (300°C, 1.20kg) = 30g / min) A-3: Iupilon S-3000 (Mitsubishi Engineering Plastics, MFR (300°C, 1.20kg) = 15g / min)

[0158] <(B) Ingredient: Luminous agent (B)> ·B-1:N luminous G-300M (manufactured by Nemoto Tokushu Kagaku Co., Ltd., SrAl2О4:Eu, Dy, average particle size (D 50 ) 25μm, luminance 80mcd m 5 minutes after light irradiation was stopped -2 (D 65 Light source, 25 lux, exposure time 15 minutes, powder brightness at saturation thickness) ·B-2:N luminous GLL-300M (manufactured by Nemoto Tokushu Kagaku Co., Ltd., SrAl2О4:Eu, Dy, average particle size (D 50 ) 25μm, luminance 143mcd m 5 minutes after light irradiation was stopped -2 (D 65 Light source, 25 lux, exposure time 15 minutes, powder brightness at saturation thickness) In addition, when light irradiation was performed under the above light irradiation conditions, the powder brightness at the saturated thickness of the luminous agent (B) 5 minutes after the light irradiation was stopped was 50 to 180 mcd m -2 Preferably, it is 60 to 170 mcd m -2 More preferably, it is 70 to 160 mcd m -2 More preferably, it is 75 to 150 mcd m -2 It is even more preferred that:

[0159] [Examples 1 to 4, Comparative Examples 1 to 3] The components were mixed according to the composition shown in Table 1, and the mixture was fed to a twin-screw extruder with a shaft diameter of 15 mm ("KZW-15-30MG" manufactured by Technovel Co., Ltd.), where the components were melt-kneaded. The components were added simultaneously, and the melt-kneading was carried out under conditions of a vacuum degree of 0.1 MPa and a kneading temperature of 235°C. As a result, a pellet-shaped resin composition was obtained. The resin compositions were evaluated by the above-mentioned methods, and the evaluation results are shown in Table 1.

[0160] [Table 1]

[0161] As can be seen from Tables 1 and 2, Examples 1 to 4, which contain an aliphatic polycarbonate resin (A) and a luminescent agent (B), show a smaller increase in the fluidity of the resin composition than the Comparative Example. The increase in fluidity is fully understood by comparing the Examples and Comparative Example, which contain the same luminescent agent. Moreover, Examples 1 to 4 show little darkening, are vivid in color, and have high initial luminescence brightness.

[0162] From the above results, it is understood that the polycarbonate resin composition containing the aliphatic polycarbonate resin (A) and the luminescent agent (B) can provide a molded article having a good external hue and high luminescence brightness.

Claims

1. A polycarbonate resin composition containing an aliphatic polycarbonate resin (A) and a luminescent agent (B).

2. 2. The polycarbonate resin composition according to claim 1, wherein the aliphatic polycarbonate resin (A) contains a structural unit derived from a dihydroxy compound having a moiety represented by the following formula (1): 【Chemistry 1】

3. 3. The polycarbonate resin composition according to claim 2, wherein the dihydroxy compound having a moiety represented by the formula (1) is a dihydroxy compound represented by the following formula (2): 【Chemistry 2】

4. 2. The polycarbonate resin composition according to claim 1, wherein the luminescent agent (B) is an aluminate-based luminescent agent.

5. The polycarbonate resin composition according to claim 4, wherein the aluminate-based luminescent agent contains an alkaline earth metal and a lanthanoid metal.

6. The aluminate-based phosphorescent agent is SrAl 2 O 4 : Eu, Dy, Sr 4 A 14 O 25 : Eu, Dy, and CaAl 2 O 4 5. The polycarbonate resin composition according to claim 4, wherein the element is at least one selected from the group consisting of Eu and Nd.

7. The polycarbonate resin composition according to claim 1, wherein the mass ratio of the aliphatic polycarbonate resin (A) to the luminescent agent (B) (wherein the aliphatic polycarbonate resin (A): the luminescent agent (B)) is 50:50 to 99:

1.

8. A molded article obtained by molding the polycarbonate resin composition according to any one of claims 1 to 7.

9. The molded article according to claim 8, which is used for an evacuation guidance sign, a nighttime display sign, an indicator button, a clock face, a switch, a connector part, or an accessory.

Citation Information

Patent Citations

  • Photostimulable phosphor

    JP1996127772A

  • Production of long persistence phosphor

    JP1997208948A

  • Polycarbonate resin composition

    JP2005082647A

  • Thermoplastic resin composition and molded product

    JP2009215415A