Method for manufacturing geopolymer solidified body
A two-stage curing process for geopolymer concrete addresses the inefficiency in manufacturing by enhancing strength and acid resistance, enabling efficient formwork reuse and improved productivity.
Patent Information
- Application Number
- JP2023059080
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Geopolymer concrete products with excellent acid resistance cannot be efficiently manufactured due to the lengthy curing time required, which hinders the efficient use of formwork and reduces productivity.
A two-stage curing process involving a first curing step to develop demolding strength followed by a second curing step to enhance acid resistance, utilizing heating and sealed conditions to accelerate curing and improve strength and resistance.
The method enables the production of geopolymer concrete products with practically sufficient strength and acid resistance, allowing efficient reuse of formwork and increasing productivity by shortening the overall curing time.
Smart Images

Figure 2024146280000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a geopolymer solidified body used in structures in, for example, civil engineering and architecture. [Background technology]
[0002] Traditionally, structures in civil engineering, architecture, and the like have generally been made from concrete and mortar. In recent years, however, geopolymer compositions have been attracting attention as alternative materials to concrete and mortar, and their application to various concrete structures as geopolymer concrete has been considered (see, for example, Patent Document 1).
[0003] Geopolymer compositions are hardened bodies obtained by mixing and reacting alkali-active amorphous powders (active fillers) such as fly ash (coal ash), metakaolin, and blast furnace slag with an alkaline solution that activates them. Geopolymer concrete, for example, is a composition that exhibits strength equivalent to that of cement concrete, achieved by adding fine aggregate, coarse aggregate, etc. to alkali-active amorphous powders and an alkaline solution.
[0004] Incidentally, cement concrete manufactured in factories (hereinafter referred to as secondary concrete products) is a product that is used when mass-producing high-quality concrete with stable quality. Secondary concrete products are produced by pouring well-mixed pre-hardened cement concrete (hereinafter referred to as ready-mixed concrete) into a formwork with high shape precision, and after the ready-mixed concrete has sufficiently hardened, it is removed from the formwork (hereinafter referred to as demolding), completing the product with the desired shape. Furthermore, the formwork is generally expensive because it requires a certain level of strength and precision. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 5091519 Summary of the Invention [Problem to be solved by the invention]
[0006] In order to effectively use expensive formwork during the production of the secondary concrete products, it is necessary to shorten the process from pouring the fresh concrete to removing it from the formwork, and so-called steam curing is generally used to accelerate curing. Steam curing is a curing method in which steam generated in a boiler is used to promote hardening by placing the formwork filled with fresh concrete in a tent. By steam curing the secondary concrete products for 1 to 8 hours, concrete with the specified strength and quality can be obtained.
[0007] On the other hand, geopolymer concrete can achieve a certain strength by steam curing for 1 to 8 hours, just like secondary concrete products, but in order to improve the acid resistance function, which is a characteristic of geopolymer concrete, curing for 20 to 100 hours is required, and this requires a long period of curing before demolding. For this reason, the current issue is that geopolymer concrete products with excellent acid resistance cannot be efficiently manufactured.
[0008] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide a method for producing a geopolymer solidified body that can efficiently produce a geopolymer concrete product having excellent strength and acid resistance. [Means for solving the problem]
[0009] In order to achieve the above-mentioned object, the present invention provides a method for producing a geopolymer solidified body, which involves kneading a material containing an active filler, an alkaline activator, and water, and then hardening the material in a mold to produce a geopolymer solidified body, the method comprising a first curing step in which the kneaded material is heated and cured in the mold for a predetermined first curing time until the material reaches a predetermined demolding strength or greater, and a second curing step in which, after the first curing time has elapsed, the mold is removed and the material is heated and cured until a predetermined second curing time has elapsed.
[0010] As a result, after the first curing process has developed the strength necessary for removal from the form, the acid resistance is increased in the second curing process, resulting in a geopolymer solidified body that has sufficient strength and acid resistance for practical use. Effect of the Invention
[0011] According to the present invention, it is possible to produce a geopolymer solidified body having sufficient strength and acid resistance for practical use, and the formwork removed after the first curing time has elapsed can be efficiently used to produce other geopolymer concrete products, thereby increasing the number of products produced using the same formwork and improving productivity. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a diagram showing a manufacturing process of a geopolymer solidified body according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The geopolymer solidified body of this embodiment is used, for example, in concrete products in civil engineering, construction, etc., and is produced by kneading a material containing an active filler, an alkaline activator, and water, and then hardening it in a mold.
[0014] The activated filler is made of alumina-silica powder that is activated and solidified by mixing with an alkaline activator. For example, fly ash (coal ash), metakaolin, silica fume, or other amorphous powder that does not contain calcium components may be used, or ground granulated blast furnace slag that contains calcium components may be used.
[0015] The alkaline activator is, for example, an alkaline solution such as an aqueous solution of sodium silicate or an aqueous solution of potassium silicate.
[0016] Aggregates consist of sand, gravel, artificial aggregates, etc., and are classified into fine aggregates and coarse aggregates depending on the particle size.
[0017] Hereinafter, with reference to FIG. 1, a method for producing a geopolymer solidified body in this embodiment will be described.
[0018] First, the material is put into a mixer (S1) and mixed (S2). After mixing is completed (S3), the material is filled into a form (or mold) for molding a geopolymer concrete product (S4), and the first curing process is started (S5). The first curing process is, for example, a heating curing at a predetermined temperature (for example, 60°C) using a hot heater, and is, for example, a sealed curing in a sealed tent. Next, after the first curing time (for example, 3 hours) has elapsed (S6), the form is removed (S7). At that time, the removed form is used to mold another geopolymer concrete product. After the form is removed, the second curing process is started (S8). The second curing process is, like the first curing process, a heating curing at a predetermined temperature (for example, 60°C) using a hot heater, and is, for example, a sealed curing covered with an airtight sheet. Then, after a second curing time (for example, 65 hours) has elapsed (S9), the curing is completed (S10).
[0019] The first curing time is set to a predetermined demold strength (e.g., 5 N / mm 2 The second curing time is the time until the geopolymer concrete exhibits sufficient acid resistance, and is preferably set to 20 to 100 hours.
[0020] According to this embodiment, the method includes a first curing step in which the mixed material is heated and cured in a formwork for a predetermined first curing time until the material reaches a predetermined demolding strength or greater, and a second curing step in which, after the first curing time has elapsed, the formwork is removed and the material is heated and cured until a predetermined second curing time has elapsed. Therefore, after the material has developed strength sufficient for demolding in the first curing step, the acid resistance can be increased in the second curing step, and a geopolymer solidified body having sufficient strength and acid resistance for practical use can be produced.
[0021] In this case, the formwork removed after the first curing time has elapsed can be efficiently used to produce other geopolymer concrete products, thereby increasing the number of products produced using the same formwork and improving productivity.
[0022] Furthermore, since the first and second curing steps are performed by heat curing, hardening can be promoted by heating, and the curing time can be shortened.
[0023] Furthermore, by carrying out the first and second curing steps using sealed curing, the humidity can be kept high by the water evaporated by heating, which can prevent cracks caused by drying and improve the strength.
[0024] In addition, by setting the first curing time to 1 hour or more and 8 hours or less, the first curing step using a formwork can be shortened. This makes it possible to manufacture multiple products using the same formwork on the same day, for example, thereby improving productivity.
[0025] Furthermore, by setting the second curing time to 20 hours or more and 100 hours or less, the second curing step after removing the formwork can be extended, and acid resistance can be sufficiently improved. In this case, if the product after removal from the formwork is stored in large quantities in a temporary storage area, productivity can be further improved.
[0026] The above-described embodiment is one embodiment of the present invention, and the present invention is not limited to the above-described embodiment. EXAMPLES
[0027] Examples and comparative examples of the present invention are shown below, but the present invention is not limited to these examples.
[0028] As examples and comparative examples of the present invention, compressive strength tests and acid resistance tests were conducted on geopolymer concrete (GPC) containing active fillers (metakaolin and silica fume), K-based water glass (50% by mass is water), an alkaline agent consisting of sodium hydroxide, and water, and further containing aggregates (coarse aggregate and fine aggregate). [Compressive strength test] In the compressive strength test, Comparative Examples 1 to 4 and Examples 1 to 4 were filled into a formwork with an inner diameter of 50 mm x 100 mm immediately after mixing, and cured under the following curing conditions, and then a compressive strength test was performed. Note that geopolymer concrete was used as the test specimen in Comparative Examples 1 to 4 and Examples 1 and 2, and geopolymer slurry was used as the test specimen in Examples 3 and 4.
[0029] In Comparative Example 1, after filling the formwork, the material was stored at room temperature and the test was carried out on the sixth day.
[0030] In Comparative Examples 2 to 4, after filling the formwork, heat curing at 60°C was performed continuously by sealed curing. In this case, the heat curing time was 68 hours for Comparative Example 2, 24 hours for Comparative Example 3, and 3 hours for Comparative Example 4. Furthermore, the test was performed on the 7th day of material age in Comparative Example 2, the 5th day of material age in Comparative Example 3, and the 6th day of material age in Comparative Example 4.
[0031] In Examples 1 to 4, after filling the formwork, the concrete was subjected to 60°C warm curing by sealed curing until the first curing time (3 hours) had elapsed (first curing step), and then, after a 24-hour room temperature storage period, the concrete was subjected to 60°C warm curing until the second curing time (65 hours) had elapsed (second curing step). In this case, in the second curing step, Examples 1 and 3 were subjected to sealed curing, and Examples 2 and 4 were subjected to curing in an open state. In addition, Examples 1 to 3 were tested on the 6th day of material age, and Example 4 was tested on the 28th day of material age. The reason for providing a room temperature storage period between the first curing step and the second curing step is that it is assumed that the time required for the work of demolding after the first curing step and the work of moving the demolded product to a storage location where the second curing step is performed is required in the actual production of geopolymer concrete products.
[0032] As a result of the test, as shown in Tables 1 and 2, Comparative Example 2, in which 60°C heating curing was performed continuously for 68 hours, showed the highest compressive strength, but it was confirmed that the other Comparative Examples 1, 3-4, and Examples 1-4 also showed compressive strength sufficient for practical use as a concrete product. Note that, under the same curing conditions, Examples 1 and 2 of geopolymer concrete showed higher compressive strength than Examples 3 and 4 of geopolymer slurry. This is thought to be because geopolymer concrete containing aggregate is less likely to undergo volumetric changes or internal stress changes due to temperature changes when demolding and curing is resumed.
[0033] [Table 1]
[0034] [Table 2]
[0035] [Acid resistance test] In the acid resistance test, for Comparative Examples 5 to 7 and Example 5, a disk-shaped sample of the geopolymer slurry was immersed in sulfuric acid for several days, and then the mass loss rate and the healthy layer remaining rate were measured. In this case, the smaller the mass loss rate, the better the acid resistance was evaluated. In addition, the healthy layer remaining rate was measured by measuring the thickness of the healthy layer (uneroded part) after the test, and the greater the thickness (remaining rate) of the healthy layer compared to the thickness before the test, the better the acid resistance was evaluated.
[0036] In Comparative Example 5, after filling the formwork, it was stored at room temperature, and the mass reduction rate was measured on the seventh day of the immersion period, and the healthy layer remaining rate was measured on the third day of the immersion period.
[0037] In Comparative Example 6, after filling the formwork, heat curing at 60°C was performed continuously by sealed curing. In this case, the heat curing time was 68 hours, and the mass loss rate and the healthy layer remaining rate were measured on the 7th day of the immersion period.
[0038] In Comparative Example 7 and Example 5, after filling the formwork, heat curing at 60°C was performed by sealed curing until the first curing time (3 hours) had elapsed (first curing step), followed by a 24-hour room temperature storage period and sealed curing until the second curing time had elapsed (second curing step). In this case, in the second curing step, curing was performed at room temperature for 28 days in Comparative Example 7, and heat curing at 60°C was performed for 65 hours in Example 5. The mass reduction rate and healthy layer remaining rate were measured on the 7th day of the immersion period in Comparative Example 7, and on the 8th day of the immersion period in Example 5.
[0039] As a result of the test, Comparative Example 6, in which warm curing at 60°C was performed continuously for 68 hours, and Example 5, in which warm curing was performed in both the first curing step and the second curing step, showed excellent acid resistance in terms of the mass loss rate shown in Tables 3 and 4 and the healthy layer survival rate shown in Tables 5 and 6. On the other hand, Comparative Example 5, in which warm curing was not performed at all, and Comparative Example 7, in which warm curing was performed only in the first curing step and not in the second curing step, showed inferior acid resistance in terms of the mass loss rate and healthy layer survival rate compared to Comparative Example 6 and Example 5.
[0040] According to the above test results, in Examples 1 to 5, in which the first curing step and the second curing step are each performed in two stages by heated curing, it was confirmed that it is possible to produce a geopolymer solidified body having sufficient compressive strength and acid resistance, even when the first curing step is followed by a period of room temperature for demolding work, etc., before moving on to the second curing step.
[0041] [Table 3]
[0042] [Table 4]
[0043] [Table 5]
[0044]
Table 6
Claims
1. A method for producing a geopolymer solidified body, comprising kneading a material containing an active filler, an alkaline activator, and water, and then hardening the material in a mold to produce a geopolymer solidified body, A first curing step of heating and curing the kneaded material in a mold for a predetermined first curing time until the kneaded material reaches a predetermined demold strength or more; After the first curing time has elapsed, the mold is removed and the product is heated and cured until a predetermined second curing time has elapsed. A method for producing a geopolymer solidified body, comprising the steps of:
2. The first and second curing steps are carried out by sealed curing. The method for producing a geopolymer solidified body according to claim 2 .
3. The first curing time is from 1 hour to 8 hours. The method for producing a geopolymer solidified body according to claim 1 or 2.
4. The second curing time is from 20 hours to 100 hours. The method for producing a geopolymer solidified body according to claim 1 or 2.
Citation Information
Patent Citations
Hardenable inorganic composition
JP1994211557A
Acid resistant box culvert and its production
JP2000053458A
Moisture-adsorbing and releasing inorganic formed body
JP2003165762A
Hydraulic hardened material and its manufacturing process
JP2004217436A
Method for producing geopolymer hardened body
JP2017100905A