Geopolymer composition and concrete structure using the same

A geopolymer composition combining metakaolin, fly ash, and silica fume addresses stability and strength issues, enhancing acid resistance and cost-effectiveness in geopolymer products.

JP2024146284APending Publication Date: 2024-10-15IHI CORP +2
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023059085
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Conventional geopolymer compositions using single active fillers or Ca-containing substances face issues with long-term stability, strength, acid resistance, and cost, while metakaolin and fly ash have specific drawbacks such as volume change and cost, respectively.

Method used

A geopolymer composition utilizing a combination of metakaolin, fly ash, and silica fume as active fillers, avoiding calcium and leveraging their respective advantages to enhance strength, acid resistance, and reduce costs.

Benefits of technology

The composition achieves high strength and acid resistance with long-term stability, reducing the need for expensive metakaolin and stabilizing fly ash variability, while maintaining workability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146284000001_ABST
    Figure 2024146284000001_ABST
Patent Text Reader

Abstract

To provide a geopolymer composition from which a geopolymer product can be inexpensively produced, the geopolymer product having stable performance in a long term, in strength and acid proofness, and being also excellent in working properties, and a concrete structure using the same.SOLUTION: There is provided a geopolymer composition which uses three kinds of active fillers being, metakaolin, fly ash and silica fume, for making up for disadvantageous and making the most of respective advantageous features, and which does not cause reduction of acid proofness due to calcium in a blast furnace slag. Namely, in both of two-kinds blending geopolymer including metakaolin and silica fume, and two-kinds blending geopolymer including fly ash and silica fume, the geopolymer composition having excellent intensity and acid proofness and having stable performance for long term, can be achieved.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a geopolymer composition used in structures in, for example, civil engineering, architecture, etc., and a concrete structure using the same. [Background technology]

[0002] Traditionally, structures in civil engineering, architecture, and the like have generally been made from concrete and mortar. In recent years, however, geopolymer compositions have been attracting attention as alternative materials to concrete and mortar, and their application to various concrete structures as geopolymer concrete has been considered (see, for example, Patent Document 1).

[0003] A geopolymer composition is a hardened body obtained by mixing and reacting an alkali-active amorphous powder (active filler) such as fly ash (coal ash), metakaolin, or blast furnace slag with an alkaline solution that activates it. Geopolymer concrete is a composition that exhibits the same strength as cement concrete, for example, by adding fine aggregate, coarse aggregate, etc. to an alkali-active amorphous powder and an alkaline solution. The active filler currently widely used in geopolymer concrete is coal ash (fly ash) or coal ash with blast furnace slag added. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 5091519 Summary of the Invention [Problem to be solved by the invention]

[0005] However, the above-mentioned coal ash (fly ash) is a by-product of thermal power generation, and has low stability in its properties, making it unsuitable as a raw material for manufacturing geopolymer products that are stable over the long term. In addition, as carbon neutrality is promoted in the future, there is a possibility that production volume will become unstable. Furthermore, there is also the problem that sufficient strength cannot be obtained due to low activity against alkali. Currently, blast furnace slag is sometimes added to compensate for this instability and low strength, but since the main constituent element of blast furnace slag is Ca (calcium), it ends up having properties similar to cement, such as low chemical resistance (acid resistance).

[0006] On the other hand, metakaolin, a mineral-based raw material mainly used academically, has stable properties and production volume, but has problems in that it is less fluid than coal ash, making it less workable when used, and is more expensive than coal ash, which is a by-product.Furthermore, because it is highly reactive to alkali, it has the disadvantage of being prone to defects such as cracks due to large volume changes, especially volume shrinkage, caused by the reaction.

[0007] In addition, although silica fume is an alkali-active powder that has a volume expansion effect, it cannot be used alone to create geopolymers because it only has one major skeletal element necessary for geopolymer formation.

[0008] Therefore, conventional formulations that use only one type of active filler as a raw material or that add Ca-containing substances to supplement performance have the problem that they cannot inexpensively produce geopolymer products that have stable long-term performance and workability in terms of strength and acid resistance.

[0009] The present invention has been made in consideration of the above problems, and its object is to provide a geopolymer composition that has long-term stable performance in terms of strength and acid resistance, and can inexpensively produce geopolymer products that are also excellent in workability, and a concrete structure using the same. It is to provide. [Means for solving the problem]

[0010] In order to achieve the above object, the present invention provides a geopolymer composition containing an active filler and an alkali activator as raw materials, wherein the active filler contains metakaolin, fly ash and silica fume.

[0011] As a result, instead of adding blast furnace slag as in the past, three types of active fillers - metakaolin, fly ash and silica fume - are used in combination, making use of the advantageous properties of each while compensating for their disadvantages, resulting in a geopolymer composition that does not suffer from the reduced acid resistance caused by the calcium in blast furnace slag. Effect of the Invention

[0012] According to the present invention, a geopolymer composition having excellent strength and acid resistance and long-term stable performance can be obtained for both a two-component geopolymer containing metakaolin and silica fume and a two-component geopolymer containing fly ash and silica fume. In this case, in addition to obtaining a high-performance geopolymer, by replacing a part of the fly ash with metakaolin, it is possible to suppress the variation in strength due to the instability of the properties of the fly ash, and by replacing a part of the metakaolin with fly ash, it is possible to reduce the amount of expensive metakaolin used while maintaining performance, thereby reducing costs. [Brief description of the drawings]

[0013] [Figure 1] Graph showing the relationship between compressive strength and (Na+K) / Al according to one embodiment of the present invention [Diagram 2] Graph showing the relationship between mass loss rate on the first day after immersion in sulfuric acid and (Na+K) / Al DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The geopolymer composition of this embodiment is used for structures in, for example, civil engineering, architecture, etc., and contains an active filler and an alkali activator as raw materials, and is composed of metakaolin, fly ash, and silica fume as the active filler.

[0015] Fly ash (coal ash), metakaolin, and silica fume used as the activated filler are alumina-silica powders that are activated and solidified by mixing with an alkaline activator, and are amorphous powders that do not contain calcium components.

[0016] The alkaline activator is, for example, an alkaline solution such as an aqueous solution of sodium silicate or an aqueous solution of potassium silicate.

[0017] Fly ash is a by-product of thermal power generation and is therefore relatively inexpensive, but it has low activity against alkali and, being a by-product, does not always have stable properties, so fly ash alone is insufficient to obtain high strength. Also, adding blast furnace slag to supplement stability and strength is not preferable because calcium reduces acid resistance. On the other hand, fly ash has the characteristic that the water ratio can be reduced due to its high fluidity, so the hardened body has a high density and is difficult for water to penetrate.

[0018] Metakaolin has more stable properties than fly ash and is highly active in alkali, so it can always achieve high strength. On the other hand, metakaolin is less workable than fly ash and more expensive, and because it is highly active in alkali, it shrinks in volume due to the reaction, making it more susceptible to cracks. In addition, because it has low fluidity, it requires a high water ratio, which means that fine voids are likely to form after drying and the moisture is removed, and water penetrates more easily than with hardened fly ash.

[0019] Silica fume has only one major skeletal element necessary for geopolymer formation, so it cannot be used alone to create geopolymers. However, it is active in alkali and has a volume expansion effect, so by using it in combination with an active filler that has volume contraction properties such as fly ash and metakaolin, it is possible to suppress the volume change of the entire geopolymer.

[0020] Therefore, the applicant discovered a geopolymer composition that uses three types of active fillers, metakaolin, fly ash, and silica fume, in combination, rather than adding blast furnace slag as in the past, making use of the advantageous properties of each while compensating for their disadvantages, and that does not cause the decrease in acid resistance caused by the calcium in blast furnace slag.

[0021] In other words, in this embodiment, a geopolymer composition having excellent strength and acid resistance and stable performance over the long term can be obtained for both a two-component geopolymer containing metakaolin and silica fume and a two-component geopolymer containing fly ash and silica fume.

[0022] In this case, in addition to obtaining a high-performance geopolymer, by replacing part of the fly ash with metakaolin, it is possible to suppress variations in strength due to the instability of the fly ash properties, and by replacing part of the metakaolin with fly ash, it is possible to reduce the amount of expensive metakaolin used while maintaining performance, thereby reducing costs.

[0023] In addition, in this embodiment, these three types of active fillers are blended so that the molar ratio of the sum of sodium and potassium to aluminum in the entire geopolymer composition ((Na+K) / Al) is 0.6 or more and 1.2 or less (preferably, 0.7 or more and 1.1 or less), and the molar ratio of silicon to aluminum in the entire geopolymer composition (Si / Al) is 1.9 or more and 2.6 or less (preferably, 2.0 or more and 2.4 or less).

[0024] As a result, when the three types of active fillers were adjusted to have the same working feel as when they were used alone, it was confirmed that a geopolymer with superior strength and acid resistance could be obtained by replacing part of the metakaolin with fly ash in a two-component geopolymer that combines metakaolin, the most active of the three and capable of producing high strength, and silica fume, which has a high crack prevention effect.

[0025] The above-described embodiment is one embodiment of the present invention, and the present invention is not limited to the above-described embodiment. EXAMPLES

[0026] Examples 1 to 7 of the present invention and Comparative Examples 1 and 2 are shown below, but the present invention is not limited to these examples.

[0027] As Examples 1 to 7 of the present invention and Comparative Examples 1 and 2, strength tests and acid resistance tests were conducted on geopolymer slurries (GPS) prepared by kneading active filler, K-based water glass (50% by mass is water), an alkaline agent consisting of sodium hydroxide, and water.

[0028] In Comparative Example 1, two types of active fillers, metakaolin and silica fume, were used, and as shown in Table 2, the molar ratio of the sum of sodium and potassium to aluminum ((Na+K) / Al) was 1, the molar ratio of silicon to aluminum (Si / Al) was 2.2, and the molar ratio of water to alumina in the entire geopolymer composition (H2O / Al2O3) was 10.

[0029] In Comparative Example 2, 100% of the metakaolin in Comparative Example 1 was replaced with fly ash as an active filler, and as shown in Table 2, the molar ratio of the sum of sodium and potassium to aluminum ((Na+K) / Al) was 0.8, the molar ratio of silicon to aluminum (Si / Al) was 2.2, and the molar ratio of water to alumina in the entire geopolymer composition (H2O / Al2O3) was 7.

[0030] In Example 1, 30% of the metakaolin in Comparative Example 1 was replaced with fly ash as an active filler, and as shown in Table 2, the molar ratio of the sum of sodium and potassium to aluminum ((Na+K) / Al) was 1.1, the molar ratio of silicon to aluminum (Si / Al) was 2.2, and the molar ratio of water to alumina in the entire geopolymer composition (H2O / Al2O3) was 8.2.

[0031] In Example 2, 30% of the metakaolin in Comparative Example 1 was replaced with fly ash as an active filler, and as shown in Table 2, the molar ratio of the sum of sodium and potassium to aluminum ((Na+K) / Al) was 0.94, the molar ratio of silicon to aluminum (Si / Al) was 2.2, and the molar ratio of water to alumina in the entire geopolymer composition (H2O / Al2O3) was 8.6.

[0032] In Example 3, 30% of the metakaolin in Comparative Example 1 was replaced with fly ash as an active filler, and as shown in Table 2, the molar ratio of the sum of sodium and potassium to aluminum ((Na+K) / Al) was 0.88, the molar ratio of silicon to aluminum (Si / Al) was 2.2, and the molar ratio of water to alumina in the entire geopolymer composition (H2O / Al2O3) was 8.8.

[0033] In Example 4, 30% of the metakaolin in Comparative Example 1 was replaced with fly ash as an active filler, and as shown in Table 2, the molar ratio of the sum of sodium and potassium to aluminum ((Na+K) / Al) was 0.7, the molar ratio of silicon to aluminum (Si / Al) was 2.2, and the molar ratio of water to alumina in the entire geopolymer composition (H2O / Al2O3) was 9.3.

[0034] In Example 5, 50% of the metakaolin in Comparative Example 1 was replaced with fly ash as an active filler, and as shown in Table 2, the molar ratio of the sum of sodium and potassium to aluminum ((Na+K) / Al) was 0.9, the molar ratio of silicon to aluminum (Si / Al) was 2.2, and the molar ratio of water to alumina in the entire geopolymer composition (H2O / Al2O3) was 8.1.

[0035] In Example 6, 50% of the metakaolin in Comparative Example 1 was replaced with fly ash as an active filler, and as shown in Table 2, the molar ratio of the sum of sodium and potassium to aluminum ((Na+K) / Al) was 0.8, the molar ratio of silicon to aluminum (Si / Al) was 2.2, and the molar ratio of water to alumina in the entire geopolymer composition (H2O / Al2O3) was 8.3.

[0036] In Example 7, 50% of the metakaolin in Comparative Example 1 was replaced with fly ash as an active filler, and as shown in Table 2, the molar ratio of the sum of sodium and potassium to aluminum ((Na+K) / Al) was 0.6, the molar ratio of silicon to aluminum (Si / Al) was 2.2, and the molar ratio of water to alumina in the entire geopolymer composition (H2O / Al2O3) was 8.8.

[0037] In this test, the geopolymer slurry was filled into a formwork with an inner diameter of 50 mm x 100 mm immediately after mixing, and the formwork was heated and cured in a steam curing tank. The curing was carried out with steam at 60°C for 68 hours, and then a compressive strength test was conducted.

[0038] In addition, acid resistance tests were performed by immersing a disk-shaped sample of the geopolymer slurry in sulfuric acid and measuring the mass loss rate on the first day. The smaller the mass loss rate, the better the acid resistance.

[0039] As a result of the test, as shown in Table 2 and FIG. 1, Examples 1 to 4, in which the replacement rate of fly ash (FA) in metakaolin (MK) (FA replacement rate) is 30%, and Examples 5 to 7, in which the FA replacement rate is 50%, both have a compressive strength (25 N / mm 2 ), and in particular, Example 1 has a compressive strength of 85.6 N / mm 2 , and Example 2 has a compressive strength of 105N / mm 2 , and Example 3 has a compressive strength of 81 N / mm 2 , and Example 5 has a compressive strength of 106 N / mm 2 , and Example 6 has a compressive strength of 105 N / mm 2 The compressive strength of Comparative Example 2, which has an FA substitution rate of 100%, was 75.1 N / mm 2 In particular, Examples 2, 5 and 6 showed results that exceeded the compressive strength of 94.4 N / mm 2 The results showed better than those shown above.

[0040] 2, the mass loss rate in the acid resistance test was 8.2wt% for Example 1, 7.7wt% for Example 2, 6.6wt% for Example 3, 7.4wt% for Example 4, 6.2wt% for Example 5, 5.5wt% for Example 6, and 6.4wt% for Example 7, and all of the mass loss rates of Examples 1 to 7 were lower than the mass loss rate of 11.8 for Comparative Example 1 with a FA substitution rate of 0%. In particular, the mass loss rates of Examples 3 to 7 were lower than the mass loss rate of 7.6 for Comparative Example 2 with a FA substitution rate of 100%.

[0041] In this test, Comparative Example 2, which has a 100% FA replacement rate, had a compressive strength of 75.1 N / mm 2 The compressive strength and mass loss rate were 7.6, but because fly ash does not always have the same properties, it is possible that the compressive strength is lower or the mass loss rate is higher than the results of this test.

[0042] [Table 1]

Claims

1. In a geopolymer composition comprising an active filler and an alkaline activator in a raw material, The active fillers include metakaolin, fly ash and silica fume. A geopolymer composition comprising:

2. The molar ratio of the sum of sodium and potassium to aluminum in the entire geopolymer composition ((Na + K) / Al) is 0.6 to 1.

2. The geopolymer composition of claim 1.

3. The molar ratio of silicon to aluminum (Si / Al) in the entire geopolymer composition is 1.9 to 2.

6. The geopolymer composition according to claim 1 or 2.

4. The geopolymer composition according to any one of claims 1 to 3 is used. A concrete structure characterized by:

Citation Information

Patent Citations

  • Ultra-high performance geopolymer composite for concrete

    JP2013545714A

  • Geopolymer production apparatus and geopolymer production method

    JP2019156671A

  • Geopolymer composition for solidifying radioactive waste

    JP2022062487A

  • Various functional inorganic binder compound using industrial byproduct