Thermally expandable refractory material

A thermally expandable refractory material with a rubber component, resin, and low-temperature foaming agents addresses the issue of insufficient low-temperature expansion in conventional materials, enhancing fireproofing by sealing gaps and improving fire resistance at both low and high temperatures.

JP2024146319APending Publication Date: 2024-10-15SEKISUI CHEMICAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023059142
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Conventional thermally expandable fireproofing materials do not effectively close gaps in fittings at low temperatures, leading to insufficient smoke intrusion control and fire spread prevention during the early stages of a fire.

Method used

A thermally expandable refractory material containing a matrix component selected from a rubber component and a resin, thermally expandable graphite, and a low-temperature foaming material, such as thermally expandable microcapsules, with specific expansion ratios and temperature ranges to enhance expandability at both low and high temperatures.

Benefits of technology

The material effectively expands to seal gaps at low temperatures, improving smoke control and fire resistance across a wide temperature range, maintaining shape retention and fireproofing capabilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146319000001
    Figure 2024146319000001
  • Figure 2024146319000002
    Figure 2024146319000002
Patent Text Reader

Abstract

To provide a thermally expandable refractory material that is capable of expanding sufficiently to close gaps in fittings at low temperatures while delivering superior expansion performance and fire resistance at high temperatures.SOLUTION: A thermally expandable refractory material includes at least one matrix component selected from the group consisting of rubber components and resins, thermally expandable graphite, and a low-temperature foaming substance other than the thermally expandable graphite.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermally expandable fire-resistant material. [Background technology]

[0002] In the field of construction, fireproof materials are used in building materials such as fittings, pillars, and wall materials for fire prevention. As fireproof materials, thermally expandable fireproof materials, which are resins mixed with thermally expandable graphite in addition to flame retardants and inorganic fillers, are used (see, for example, Patent Document 1). Such thermally expandable fireproof materials expand when heated, and the combustion residue forms a fireproof insulation layer, thereby exhibiting fireproof insulation performance. A thermally expandable fire-resistant material containing thermally expandable graphite is placed, for example, in the gap between fittings such as doors and windows installed in openings of a building and the frames surrounding them, such as door frames and window frames; in the event of a fire, the sheet expands in the thickness direction to close the gap between the fittings and the frames and prevent the fire from spreading. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2017-141463 A Summary of the Invention [Problem to be solved by the invention]

[0004] Conventional heat-expandable fire-resistant materials containing heat-expandable graphite expand significantly when exposed to high temperatures of 200°C or above, and are able to seal gaps in fittings and other objects and prevent the spread of fire. However, at low temperatures below 200°C, they do not expand, or expand too little to seal gaps, meaning that they are insufficient in preventing smoke from entering and preventing the spread of fire in the early stages of a fire when temperatures are low. Therefore, an object of the present invention is to provide a heat-expandable fire-resistant material which can expand at low temperatures to an extent that it can close gaps in fittings and the like, and which has good expandability and excellent fire resistance even at high temperatures. [Means for solving the problem]

[0005] As a result of intensive research aimed at solving the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by a thermally expandable fire-resistant material containing at least one matrix component selected from the group consisting of a rubber component and a resin, thermally expandable graphite, and a low-temperature foaming substance other than the thermally expandable graphite, and have completed the present invention. That is, the present invention relates to the following [1] to [7]. [1] A thermally expandable fire-resistant material comprising at least one matrix component selected from the group consisting of a rubber component and a resin, thermally expandable graphite, and a low-temperature foaming substance other than the thermally expandable graphite. [2] The thermally expandable fireproof material according to the above [1], which has an expansion ratio of 5 to 80 times when expanded at 150°C. [3] The thermally expandable fireproof material according to the above [1] or [2], which has an expansion ratio of 30 to 80 times when expanded at 400°C. [4] The thermally expandable fireproof material according to any one of the above [1] to [3], which contains thermally expandable microcapsules as the low-temperature foaming substance. [5] The thermally expandable fireproof material according to any one of the above [1] to [4], wherein the low-temperature foaming substance has a foaming initiation temperature of 100 to 140°C. [6] The thermally expandable fireproof material according to any one of the above [1] to [5], wherein the thermally expandable graphite has an expansion starting temperature of 160 to 260°C. [7] The thermally expandable fire-resistant material according to any one of the above [1] to [6], which is for use in building materials. Effect of the Invention

[0006] According to the present invention, it is possible to provide a thermally expandable fire-resistant material which can expand at low temperatures to an extent that it can close gaps in fittings and the like, and which has good expandability and excellent fire resistance even at high temperatures. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] [Thermally expandable fireproof material] The thermally expandable fireproof material of the present invention is a thermally expandable fireproof material containing at least one matrix component selected from the group consisting of a rubber component and a resin, thermally expandable graphite, and a low-temperature foaming substance other than the thermally expandable graphite. Hereinafter, the thermally expandable fireproof material of the present invention may also be simply referred to as a fireproof material.

[0008] <Low temperature foaming material> The fireproof material of the present invention contains a low-temperature foaming substance other than thermally expandable graphite. The low-temperature foaming substance means, for example, a substance whose foaming start temperature is in the range of 100 to 150° C. When the fireproof material contains the low-temperature foaming substance, the fireproof material is easily expanded at low temperatures in the early stages of a fire, and can block gaps in fittings and the like, thereby quickly exerting functions of suppressing smoke intrusion and preventing the spread of fire.

[0009] The foaming start temperature of the low-temperature foaming substance is not particularly limited, but is preferably 100 to 150° C., more preferably 100 to 140° C., and even more preferably 110 to 140° C. When the foaming start temperature of the low-temperature foaming substance is equal to or higher than these lower limits, foaming during the production of the fireproof material can be suppressed. When the foaming start temperature of the low-temperature foaming substance is equal to or lower than these upper limits, the expansion ratio can be increased in the low-temperature region where it is difficult to increase the expansion ratio using thermally expandable graphite alone. From the viewpoint of exhibiting good fire resistance in a wide range from low to high temperatures, the difference between the expansion start temperature of the thermally expandable graphite described below and the foaming start temperature of the low-temperature foaming substance (expansion start temperature-foaming start temperature) is preferably 10 to 70°C, more preferably 20 to 60°C. When the difference between the expansion start temperature of the thermally expandable graphite and the foaming start temperature of the low-temperature foaming substance is equal to or greater than these lower limits, the expansion of the thermally expandable graphite and the foaming start temperature of the low-temperature foaming substance are less likely to be hindered by each other, and as a result, the expansion ratio can be increased. When the difference between the expansion start temperature of the thermally expandable graphite and the foaming start temperature of the low-temperature foaming substance is equal to or less than these upper limits, the expansion of the thermally expandable graphite is less likely to be hindered by the expansion residue of the low-temperature foaming substance, and as a result, the expansion ratio can be increased. The foaming initiation temperature of the low-temperature foaming substance can be measured by the method described in the Examples.

[0010] The low-temperature foaming substance is preferably a particle having thermal foaming properties that foams and expands when heated, and more preferably a thermally expandable microcapsule.

[0011] A thermally expandable microcapsule is a microcapsule in which a volatile substance such as a low boiling point solvent is encapsulated inside a shell resin. When the shell resin is softened by heating, the volatile substance evaporates or expands, and the shell expands under the pressure, increasing the particle size and forming hollow particles. The foaming start temperature of the thermally expandable microcapsule can be adjusted by the type of shell resin and volatile substance. The temperature at which the thermally expandable microcapsule is foamed is not particularly limited, but is generally higher than the foaming start temperature.

[0012] The outer shell of the thermally expandable microcapsule is preferably formed from a thermoplastic resin. The thermoplastic resin may be one or more selected from vinyl polymers such as ethylene, styrene, vinyl acetate, vinyl chloride, vinylidene chloride, acrylonitrile, methacrylonitrile, butadiene, chloroprene, and the like, copolymers thereof, polyamides such as nylon 6 and nylon 66, and polyesters such as polyethylene terephthalate. Among them, acrylonitrile copolymers are preferred because they are less permeable to volatile substances contained therein. The volatile substance to be encapsulated inside the thermally expandable microcapsules is one or more low-boiling point liquids selected from the following: hydrocarbons having 3 to 8 carbon atoms, such as propane, propylene, butene, normal butane, isobutane, isopentane, neopentane, normal pentane, hexane, heptane, octane, and isooctane; methane halides, such as methyl chloride and methylene chloride; chlorofluorocarbons, such as CCl3F and CCl2F2; tetraalkylsilanes, such as tetramethylsilane and trimethylethylsilane; and petroleum ether. Suitable examples of thermally expandable microcapsules include microcapsules having a shell resin made of a copolymer mainly composed of acrylonitrile, methacrylonitrile, vinylidene chloride, etc., and encapsulating a hydrocarbon having 3 to 8 carbon atoms, such as isobutane.

[0013] The thermally expandable microcapsules preferably have an average particle size of 1 μm or more, more preferably 4 μm or more, and also preferably less than 50 μm, more preferably less than 40 μm. The average particle size is the average value of the measurements when the primary particle sizes of 100 particles in a visual field observed using a scanning electron microscope, an optical microscope, or the like are measured. The average particle size means the average value of the diameter of the particles when the particles are spherical, and means the average value of the major axis of the particles when the particles are non-spherical.

[0014] The content of the low-temperature foaming substance in the fireproof material of the present invention is not particularly limited, but is preferably 1 to 100 parts by mass, more preferably 5 to 50 parts by mass, and even more preferably 10 to 20 parts by mass, relative to 100 parts by mass of the matrix component. When the content of the low-temperature foaming substance is equal to or greater than these lower limits, the fireproof material has high expandability at low temperatures, and the fireproof material has improved fire resistance at the early stage of a fire. When the content of the low-temperature foaming substance is equal to or less than these upper limits, the fireproof material can be appropriately expanded from low to high temperatures, and the shape retention ability of the fireproof material after expansion can be improved, and the processability is also improved.

[0015] <Thermal expandable graphite> The fireproof material of the present invention contains thermally expandable graphite. By containing thermally expandable graphite, the expandability of the fireproof material at high temperatures (e.g., 200°C or higher) can be improved, and gaps in fittings and the like can be blocked at high temperatures. In addition, since the shape retention after expansion is high, falling off and the like is unlikely to occur, and fire resistance is improved.

[0016] The expansion initiation temperature of the thermally expandable graphite is preferably 160 to 260° C., more preferably 160 to 230° C., and even more preferably 160 to 200° C., from the viewpoint of improving the expandability of the fireproof material at high temperatures and from the viewpoint of improving the overall fire resistance from low to high temperatures when used in combination with a low-temperature foaming substance. The expansion initiation temperature of the thermally expandable graphite can be measured by the method described in the Examples.

[0017] Thermally expandable graphite is a conventionally known substance that expands when heated, and is produced by treating raw material powders such as natural scaly graphite, pyrolytic graphite, and kish graphite with a strong oxidizing agent to produce a graphite intercalation compound. Examples of the strong oxidizing agent include inorganic acids such as concentrated sulfuric acid, nitric acid, and selenic acid, concentrated nitric acid, perchloric acid, perchlorates, permanganates, dichromates, and hydrogen peroxide. Thermally expandable graphite is a crystalline compound that maintains the layered structure of carbon. The thermally expandable graphite may be subjected to a neutralization treatment. That is, the thermally expandable graphite obtained by treating with a strong oxidizing agent or the like as described above may be further neutralized with ammonia, an aliphatic lower amine, an alkali metal compound, an alkaline earth metal compound, or the like.

[0018] The average particle size of the thermally expandable graphite is not particularly limited, but is preferably 50 to 500 μm, and more preferably 100 to 400 μm. The average particle size of the thermally expandable graphite is determined as the average value of the maximum dimensions of 10 or more (e.g., 50) pieces of thermally expandable graphite. The above-mentioned minimum and maximum dimensions of the thermally expandable graphite can be measured, for example, by using a field emission scanning electron microscope (FE-SEM).

[0019] The content of thermally expandable graphite in the fireproof material of the present invention is preferably 5 to 300 parts by mass, more preferably 10 to 100 parts by mass, and even more preferably 15 to 50 parts by mass, based on 100 parts by mass of the matrix component. When the content of thermally expandable graphite is equal to or greater than these lower limits, the expandability of the fireproof material at high temperatures is easily increased. When the content of thermally expandable graphite is equal to or less than these upper limits, shape retention, processability, etc. are improved.

[0020] <Matrix components> The fire-resistant material of the present invention contains a matrix component which is at least one selected from a rubber component and a resin.

[0021] (Rubber component) Examples of rubber components include natural rubber, isoprene rubber, butyl rubber, butadiene rubber (BR), 1,2-polybutadiene rubber, styrene-butadiene rubber (SBR), chloroprene rubber, acrylonitrile rubber-butadiene rubber (NBR), ethylene-propylene rubber, ethylene-propylene-diene rubber (EPDM), chlorosulfonated polyethylene, acrylic rubber, epichlorohydrin rubber, multi-vulcanized rubber, non-vulcanized rubber, silicone rubber, fluororubber, and urethane elastomer. Among these, from the viewpoints of improving the expandability from low temperatures to high temperatures and improving fire resistance, at least one rubber selected from the group consisting of acrylonitrile-butadiene rubber and chloroprene rubber is preferred.

[0022] The nitrile content of the acrylonitrile-butadiene rubber is preferably 8 to 40 mass%, more preferably 10 to 35 mass%, and further preferably 20 to 30 mass%. The acrylonitrile-butadiene rubber having a nitrile content in the above range is likely to increase the expansion pressure of the fire-resistant material and is likely to improve the fire resistance. The Mooney viscosity ML(1+4) of the acrylonitrile-butadiene rubber at 100°C is preferably 20-90, more preferably 30-85, and even more preferably 50-80.

[0023] Chloroprene rubber can reduce the proportion of carbon contained in the fire-resistant material, so from the viewpoint of improving fire resistance, it is also preferable to use chloroprene rubber as the rubber contained in the fire-resistant material. As the chloroprene rubber, a sulfur-modified type (G type), a non-sulfur-modified type (W type), etc. can also be used. The Mooney viscosity ML(1+4) of the chloroprene rubber at 100°C is preferably 60-120, and more preferably 70-90. In this specification, the Mooney viscosity is measured in accordance with JIS K6300.

[0024] When a rubber component is used as the matrix component, the fireproof material preferably contains a plasticizer, which will be described later. By using a plasticizer, the moldability of the fireproof material can be improved, and the expandability can also be improved. When chloroprene rubber is used, an aliphatic ester plasticizer or the like can be used. An example of the aliphatic ester plasticizer is an aliphatic ester plasticizer having an ether bond, such as dibutoxyethoxyethyl adipate. An example of a commercially available product of dibutoxyethoxyethyl adipate is Adeka Cizer RS-107 manufactured by ADEKA Corporation, which is called an adipic acid ether ester type.

[0025] (resin) The resin may be a thermosetting resin or a thermoplastic resin, but is preferably a thermoplastic resin. The thermoplastic resin is not particularly limited, but examples thereof include polyolefin resins such as polypropylene resin, polyethylene resin, and ethylene-vinyl acetate copolymer, fluororesins such as polyvinyl acetate resin, polyvinyl chloride resin, and polytetrafluoroethylene, phenol resin, polycarbonate resin, polyacrylonitrile resin, and urethane-based resins such as urethane elastomer. Among these, from the viewpoint of improving the expansibility from low temperatures to high temperatures and improving the fire resistance, the resin contained in the fire-resistant material is preferably at least one selected from the group consisting of polypropylene resin, polyethylene resin, ethylene-vinyl acetate copolymer, and polyvinyl chloride resin. When any of polypropylene resin, polyethylene resin, and ethylene-vinyl acetate copolymer is used as the resin, the resin decomposes at high temperatures, the viscosity tends to decrease, and the expansion ratio tends to be increased. When polyvinyl chloride resin is used, the expansion ratio tends to be increased by using a plasticizer described later in combination. In addition, since the fireproof material of the present invention contains a low-temperature foaming substance, it is preferable that the material can be processed at a lower temperature in order to suppress foaming during production. From this viewpoint, ethylene-vinyl acetate copolymer is preferable among the above-mentioned resins.

[0026] The polypropylene resin may be a homopolypropylene or a copolymer of propylene and a monomer other than propylene (eg, ethylene), but is preferably a homopolypropylene. From the viewpoint of increasing the expansion ratio of the fire-resistant material, the melt flow rate (MFR) of the polypropylene resin at 230° C. is preferably 1 to 20 g / 10 min, and more preferably 5 to 15 g / 10 min.

[0027] The polyethylene resin may be any of high density polyethylene, low density polyethylene, and linear low density polyethylene, with low density polyethylene being preferred. From the viewpoint of increasing the expansion ratio of the fire-resistant material, the melt flow rate (MFR) of the polyethylene resin at 190° C. is preferably 0.5 to 10 g / 10 min, and more preferably 2 to 6 g / 10 min.

[0028] The ethylene-vinyl acetate copolymer may be, for example, a copolymer of ethylene and vinyl acetate having an ethylene content of 50% by mass or more. The ethylene-vinyl acetate copolymer has a vinyl acetate content measured in accordance with JIS K7192:1999 of preferably 10 to 50% by mass, more preferably 13 to 35% by mass, and even more preferably 15 to 25% by mass. By setting the vinyl acetate content to the above lower limit or more, good fire resistance is obtained. In addition, by setting the vinyl acetate content within the above range, moldability and the like are easily improved.

[0029] Examples of polyvinyl chloride resins include polyvinyl chloride homopolymers, copolymers of vinyl chloride monomers and monomers having unsaturated bonds copolymerizable with vinyl chloride monomers, graft copolymers obtained by graft copolymerization of vinyl chloride with polymers other than vinyl chloride, etc., which may be used alone or in combination of two or more. In addition, chlorinated polyvinyl chloride resins, which are chlorinated polyvinyl chloride resins, are also included in polyvinyl chloride resins.

[0030] (Plasticizer) The fireproof material may contain a plasticizer. By containing a plasticizer, flexibility and moldability are easily improved. In addition, as described above, by using acrylonitrile-butadiene rubber, chloroprene rubber, polyvinyl chloride resin, or the like in combination with a plasticizer, the expansion ratio of the fireproof material is easily increased.

[0031] Examples of the plasticizer include phthalate plasticizers such as di-2-ethylhexyl phthalate (DOP), dibutyl phthalate (DBP), diheptyl phthalate (DHP), and diisodecyl phthalate (DIDP); di-2-ethylhexyl adipate (DOA), diisobutyl adipate (DIBA), dibutyl adipate (DBA), di-2-ethylhexyl azelate (DOZ), di-2-ethylhexyl sebacate (DOS), diisononyl adipate (DINA), and diisodecyl azelate (DIDP); Examples of suitable plasticizers include aliphatic diesters such as bis[2-(2-butoxyethoxy)ethyl]adipate (DIDA) and bis[2-(2-butoxyethoxy)ethyl]adipate (BXA-N), fatty acid ester plasticizers such as adipic acid polyester, epoxidized ester plasticizers such as epoxidized soybean oil, adipate esters, adipate polyesters, and other adipate ester plasticizers, trimellitic acid ester plasticizers such as tri-2-ethylhexyl trimellitate (TOTM) and triisononyl trimellitate (TINTM), and process oils such as mineral oil, etc. Among these, phthalic acid ester plasticizers are preferred, and diisodecyl phthalate (DIDP) is more preferred. The plasticizers may be used alone or in combination of two or more.

[0032] When the fireproof material contains a plasticizer, the content of the plasticizer is preferably 5 to 300 parts by mass, more preferably 20 to 200 parts by mass, and even more preferably 50 to 120 parts by mass, relative to 100 parts by mass of the matrix component. When the content of the plasticizer is within the above range, it is possible to obtain a good balance of moldability, fire resistance, mechanical strength, adhesiveness, etc.

[0033] (Crosslinking agent) The fireproof material of the present invention may contain a crosslinking agent. By using the crosslinking agent, crosslinking of the resin proceeds due to heat during a fire, and the expansion property of the fireproof material increases, thereby improving the fireproof property.

[0034] As the crosslinking agent, any known agent can be used without limitation, and examples thereof include organic peroxides and azo compounds. Examples of organic peroxides include 2,5-dimethylhexane-2,5-dihydroperoxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 3-di-t-butyl peroxide, t-dicumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne, dicumyl peroxide, α,α'-bis(t-butylperoxyisopropyl)benzene, n-butyl-4,4-bis(t-butylperoxy)butane, 2,2-bis(t-butylperoxy)butane, 1,1-bis(t-butylperoxy)cyclohexane, 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane, t-butylperoxybenzoate, benzoyl peroxide, and t-butylperoxy-2-ethylhexyl carbonate. Examples of the azo compound include azobisisobutyronitrile and azobis(2,4-dimethylvaleronitrile).

[0035] When the fireproof material contains a crosslinking agent, the content of the crosslinking agent is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 7 parts by mass, and even more preferably 1 to 5 parts by mass, relative to 100 parts by mass of the matrix component.

[0036] (Flame retardant) The fire-resistant material of the present invention preferably contains a flame retardant, which improves fire resistance. Examples of the flame retardant include various phosphoric acid esters such as triphenyl phosphate (triphenyl phosphate), tricresyl phosphate, trixylenyl phosphate, cresyl diphenyl phosphate, and xylenyl diphenyl phosphate, metal phosphates such as sodium phosphate, potassium phosphate, and magnesium phosphate, metal phosphites such as sodium phosphite, potassium phosphite, magnesium phosphite, and aluminum phosphite, ammonium polyphosphate, red phosphorus, etc. Examples of the flame retardant also include compounds represented by the following general formula (1).

[0037] [ka]

[0038] In the general formula (1), R 1 and R 3 R are the same or different and represent hydrogen, a linear or branched alkyl group having 1 to 16 carbon atoms, or an aryl group having 6 to 16 carbon atoms. 2 represents a hydroxyl group, a linear or branched alkyl group having 1 to 16 carbon atoms, a linear or branched alkoxyl group having 1 to 16 carbon atoms, an aryl group having 6 to 16 carbon atoms, or an aryloxy group having 6 to 16 carbon atoms.

[0039] Specific examples of the compound represented by the general formula (1) include methylphosphonic acid, dimethyl methylphosphonate, diethyl methylphosphonate, ethylphosphonic acid, n-propylphosphonic acid, n-butylphosphonic acid, 2-methylpropylphosphonic acid, t-butylphosphonic acid, 2,3-dimethyl-butylphosphonic acid, octylphosphonic acid, phenylphosphonic acid, dioctylphenylphosphonate, dimethylphosphinic acid, methylethylphosphinic acid, methylpropylphosphinic acid, diethylphosphinic acid, dioctylphosphinic acid, phenylphosphinic acid, diethylphenylphosphinic acid, diphenylphosphinic acid, bis(4-methoxyphenyl)phosphinic acid, etc. The flame retardants may be used alone or in combination of two or more.

[0040] As the flame retardant of the present invention, boron compounds and metal hydroxides can also be used. The boron-based compound may, for example, be zinc borate. Examples of metal hydroxides include aluminum hydroxide, magnesium hydroxide, calcium hydroxide, hydrotalcite, etc. When a metal hydroxide is used, water is generated by the heat generated by ignition, and the fire can be quickly extinguished.

[0041] Among the flame retardants, red phosphorus, phosphate esters such as triphenyl phosphate (triphenyl phosphate), aluminum phosphite, ammonium polyphosphate, and zinc borate are preferred from the viewpoints of safety, cost, etc. Among them, aluminum phosphite and ammonium polyphosphate are more preferred, and aluminum phosphite is even more preferred. Aluminum phosphite is expandable, and therefore easily improves fire resistance effectively.

[0042] The average particle size of the flame retardant is preferably 1 to 200 μm, more preferably 1 to 60 μm, further preferably 3 to 40 μm, and further preferably 5 to 20 μm. When the average particle size of the flame retardant is within the above range, the dispersibility of the flame retardant in the fire-resistant material is improved, the flame retardant can be uniformly dispersed in the matrix component, and the amount of the flame retardant blended with respect to the matrix component can be increased. The average particle size of the flame retardant is the median diameter (D50) measured by a laser diffraction / scattering particle size distribution measuring device.

[0043] The content of the flame retardant in the fire-resistant material of the present invention is preferably 1 to 200 parts by mass, more preferably 3 to 100 parts by mass, and even more preferably 5 to 30 parts by mass, relative to 100 parts by mass of the matrix component. When the content of the flame retardant is equal to or greater than these lower limits, the fire resistance of the fire-resistant material is improved. When the content of the flame retardant is equal to or less than these upper limits, the flame retardant is easily dispersed uniformly in the matrix component, and the moldability is excellent.

[0044] (Inorganic filler) The fireproof material of the present invention may further contain an inorganic filler other than the flame retardant and the thermally expandable graphite. By containing the inorganic filler, the mechanical properties such as the shape retention after expansion of the fireproof material can be improved, and the fireproofness is improved. The inorganic filler other than the flame retardant and the thermally expandable graphite is not particularly limited, and examples thereof include metal oxides such as alumina, zinc oxide, titanium oxide, calcium oxide, magnesium oxide, iron oxide, tin oxide, antimony oxide, and ferrite, metal carbonates such as basic magnesium carbonate, calcium carbonate, magnesium carbonate, zinc carbonate, strontium carbonate, and barium carbonate, silica, diatomaceous earth, dawsonite, barium sulfate, talc, clay, mica, montmorillonite, bentonite, activated clay, sepiolite, imogolite, sericite, glass fiber, glass beads, silica-based balloons, aluminum nitride, boron nitride, silicon nitride, carbon black, graphite, carbon fiber, carbon balloons, charcoal powder, various metal powders, potassium titanate, magnesium sulfate, lead zirconate titanate, zinc stearate, calcium stearate, aluminum borate, molybdenum sulfide, silicon carbide, stainless steel fiber, various magnetic powders, slag fiber, fly ash, and dewatered sludge. These inorganic fillers may be used alone or in combination of two or more kinds.

[0045] The average particle size of the inorganic filler is preferably 0.5 to 100 μm, more preferably 1 to 50 μm. When the content of the inorganic filler is low, a small particle size is preferable from the viewpoint of improving dispersibility, whereas when the content is high, a large particle size is preferable because the viscosity of the refractory material increases and the moldability decreases as the content increases.

[0046] When the fireproof material of the present invention contains an inorganic filler other than the flame retardant and the thermally expandable graphite, the content thereof is preferably 1 to 200 parts by mass, more preferably 2 to 50 parts by mass, and more preferably 3 to 10 parts by mass, relative to 100 parts by mass of the matrix component. When the content of the inorganic filler is within the above range, the mechanical properties of the fireproof material can be improved.

[0047] The fireproof material of the present invention can contain various additive components as required within the scope of the invention. The type of the additive component is not particularly limited, and various additives can be used. Examples of such additives include lubricants, shrinkage inhibitors, crystal nucleating agents, colorants (pigments, dyes, etc.), ultraviolet absorbers, antioxidants, antiaging agents, dispersants, gelation accelerators, fillers, reinforcing agents, flame retardant assistants, antistatic agents, surfactants, vulcanizing agents, and surface treatment agents. The amount of additive added can be appropriately selected within a range that does not impair moldability, etc. The additives may be used alone or in combination of two or more.

[0048] The fireproof material is preferably in the form of a sheet, and the thickness thereof is not particularly limited, but is preferably 0.2 to 10 mm, more preferably 0.5 to 3.0 mm, from the viewpoints of fire resistance and ease of handling.

[0049] (Expansion ratio) The expansion ratio of the fireproof material of the present invention when expanded at 150°C is preferably 5 to 80 times, more preferably 10 to 70 times, and even more preferably 30 to 70 times. By making the expansion ratio at 150°C equal to or greater than the above lower limit, the fireproof material can have high expandability at low temperatures, and can improve the smoke intrusion suppression and fire spread prevention functions at the early stage of a fire. When the expansion ratio at 150°C is equal to or less than the above upper limit, the shape is easily maintained, and as a result, a decrease in fire resistance can be prevented.

[0050] The expansion ratio of the fireproof material of the present invention when expanded at 400°C is preferably 30 to 80 times, more preferably 35 to 80 times, and even more preferably 40 to 75 times. By making the expansion ratio at 400°C equal to or more than the above lower limit, the expandability of the fireproof material at high temperatures can be increased, and it becomes easier to prevent the fireproof material from falling off from fittings after expansion, and the fireproof property is improved. If the expansion ratio at 400°C is equal to or less than the above upper limit, the residual hardness of the fireproof material after expansion can be kept at a certain level or more, so that the shape retention is good and the fireproof property is improved.

[0051] (Method of manufacturing fireproof materials) The fireproof material of the present invention can be produced, for example, as follows. First, predetermined amounts of a matrix component, thermally expandable graphite, a low-temperature foaming substance, and optionally blended plasticizers, flame retardants, crosslinking agents, inorganic fillers, and other components are kneaded in a kneading machine such as a kneading roll to obtain a fire-resistant resin composition. Next, the obtained fire-resistant resin composition is molded into a sheet or the like by a known molding method such as press molding, calendar molding, extrusion molding, etc., to obtain a fire-resistant material. The temperature during kneading and the temperature for forming into a sheet are preferably lower than the expansion start temperature of the thermally expandable graphite and the foaming start temperature of the low-temperature foaming material, and when a crosslinking agent is added, the temperature is preferably such that the crosslinking agent is unlikely to crosslink. Therefore, the kneading temperature is preferably 80 to 120°C, more preferably 90 to 110°C. The temperature for forming into a sheet is preferably 80 to 120°C, more preferably 90 to 110°C.

[0052] (Laminated sheet) The fireproof material of the present invention may be laminated with other sheet members or pressure-sensitive adhesive layers to form a laminate sheet. The laminate sheet includes, for example, a substrate and a fireproof material laminated on one or both sides of the substrate. The substrate is usually a woven fabric or nonwoven fabric. The fibers used for the woven fabric or nonwoven fabric are not particularly limited, but are preferably noncombustible or semi-noncombustible materials, such as glass fibers, ceramic fibers, cellulose fibers, polyester fibers, carbon fibers, graphite fibers, and thermosetting resin fibers. The laminate sheet can be obtained, for example, by forming the fire-resistant resin composition into a sheet on a substrate.

[0053] The laminate sheet may also include a fireproof material and an adhesive layer. The adhesive layer may be laminated on one or both sides of the fireproof material, for example. Furthermore, the laminate sheet may include a fireproof material, a substrate, and an adhesive layer. Such a laminate sheet may have a fireproof material on one side of the substrate and an adhesive layer on the other side, or a fireproof material and an adhesive layer may be provided in this order on one side of the substrate. The adhesive layer can be formed, for example, by transferring an adhesive coated on a release paper to the laminate sheet.

[0054] The fireproof material of the present invention and the laminated sheet using the same can be used specifically for various fittings in detached houses, apartment buildings, high-rise houses, high-rise buildings, commercial facilities, public facilities, and the like, various vehicles such as automobiles and trains, ships, and aircraft, among which it is preferable to use it for fittings. As fittings, specifically, they can be used for walls, beams, pillars, floors, bricks, roofs, boards, windows, shoji screens, doors, doors, sliding doors, transoms, wiring, piping, and the like, but are not limited thereto. The fireproof material of the present invention and the laminated sheet using the same can be applied, particularly to gaps in fittings such as windows, doors, and doors, to prevent flames from penetrating through the gaps in the event of a fire or the like. EXAMPLES

[0055] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.

[0056] <Evaluation method> (Expansion start temperature) In a rheometer ("Discovery HR-2", manufactured by TA Instruments), 0.5 g of a sample of thermally expandable graphite was placed on the sample stage and wrapped in aluminum foil to prevent the powder from falling off. The sample was grounded with a 25 mm diameter cone plate until the load became 0 [N]. From that state, the sample was heated at a constant heating rate (10 °C / min) from the set temperature of 50 °C using a Peltier heater, and the point when the load became 0.1 N was taken as the expansion start temperature.

[0057] (Foaming start temperature) The foaming initiation temperature of the low-temperature foaming material was measured using a thermomechanical analyzer (TMA) (TMA2940, manufactured by TA instruments). Specifically, 25 μg of the sample was placed in an aluminum container with a diameter of 7 mm and a depth of 1 mm, and heated from 50°C to 220°C at a temperature increase rate of 5°C / min with a force of 0.1 N applied from above. The displacement of the measuring probe in the vertical direction was measured, and the temperature at which the displacement began to increase was defined as the foaming initiation temperature.

[0058] (Expansion ratio) The expansion ratio was measured as follows. The fireproof materials of each Example and Comparative Example were cut to a predetermined size (thickness 1.8 mm, width 25 mm, length 25 mm). The fireproof materials of the predetermined size were placed on the bottom surface of a stainless steel plate (98 mm square, thickness 0.3 mm), fed into an electric furnace, and heated at 150°C for 30 minutes. The thickness of the fireproof material after heating was divided by the thickness of the fireproof material before heating to determine the expansion ratio at 150°C. In addition, in the above method, instead of the operation of heating at 150°C for 30 minutes, an operation of heating at 400°C for 30 minutes was performed, and the expansion ratio at 400°C was determined.

[0059] (Fire resistance time) A door component for evaluating fire resistance time was produced, consisting of a door made of a calcium silicate board (manufactured by Nippon Insulation Co., Ltd.) and a door frame. A gap of 1 cm was left between the side of the door of the door component for evaluating fire resistance time and the door frame. A fireproof material of each Example and Comparative Example cut to a specified size (thickness 1.8 mm, width 25 mm, length 1000 mm) was attached to the side of the door. It was then heated in a fireproof furnace according to the standard heating curve of ISO834, and the time until the fireproof material peeled off was measured. The longer the time until it peeled off, the more excellent the fireproofing of the fireproof material. Evaluation was based on the following criteria S: Time to peel off is 110 minutes or more A: The time it takes to peel off is between 105 and 110 minutes B: Time to peel off is more than 100 minutes but less than 105 minutes C: Time to peel off is between 95 and 100 minutes D: Time to peel off is less than 95 minutes

[0060] The various components used in each of the examples and comparative examples are as follows. <Matrix components> Ethylene vinyl acetate copolymer (EVA): "Evaflex EV460" manufactured by Mitsui DuPont Polychemicals Co., Ltd., vinyl acetate content 19% by mass Chloroprene rubber (CR): "Skyprene TSR-56" manufactured by Tosoh Corporation Acrylonitrile rubber-butadiene rubber (NBR): "Nipol 1043" manufactured by Nippon Zeon Co., Ltd.

[0061] (Thermal Expandable Graphite) Thermally expandable graphite: Fuji Graphite Industries Co., Ltd. "EXP-50S120N", expansion start temperature 120℃ Thermally expandable graphite: Fuji Graphite Industries Co., Ltd. "EXP-42S160N", expansion start temperature 160℃ -Thermal expandable graphite: Fuji Graphite Industries Co., Ltd. "EXP-50HO", expansion start temperature 200℃ -Thermal expandable graphite: Fuji Graphite Industries Co., Ltd. "EXP-50KK", expansion start temperature 260℃

[0062] (Low temperature foaming material) Thermally expandable microcapsules: Sekisui Chemical Co., Ltd. "Advancell EMH204", foaming start temperature 115℃ -Thermal expansion microcapsules: Sekisui Chemical Co., Ltd. "Advancell EM306", foaming start temperature 140℃ -Thermal expansion microcapsules: Sekisui Chemical Co., Ltd. "Advancell EM504", foaming start temperature 170℃

[0063] (Plasticizer) RS-107: Adipic acid ether ester type, "Adeka Cizer RS-107" manufactured by ADEKA Corporation

[0064] (Flame retardant) Aluminum phosphite "APA100" manufactured by Taihei Chemical Industry Co., Ltd.

[0065] (Inorganic filler) Calcium carbonate

[0066] (Examples 1 to 10, Comparative Examples 1 to 4) The matrix component, thermally expandable graphite, low-temperature foaming material (thermally expandable microcapsules), flame retardant, inorganic filler, and plasticizer were charged into a roll and kneaded at 100°C for 5 minutes to obtain a fire-resistant resin composition. The obtained fire-resistant resin composition was press-molded at 100°C for 3 minutes to obtain a sheet-shaped fire-resistant material. The evaluation results are shown in Table 1.

[0067] [Table 1]

[0068] As shown in the above examples, the fire-resistant material of the present invention, which contains at least one matrix component selected from the group consisting of rubber components and resins, heat-expandable graphite, and heat-expandable microcapsules as a low-temperature foaming substance, has high heat expansion at low and high temperatures and is excellent in fire resistance. In contrast, the fire-resistant materials of each comparative example, which do not contain heat-expandable graphite or a low-temperature foaming substance, have low heat expansion at low and high temperatures and are inferior in fire resistance.

Claims

1. A thermally expandable fire-resistant material comprising at least one matrix component selected from the group consisting of a rubber component and a resin, thermally expandable graphite, and a low-temperature foaming substance other than the thermally expandable graphite.

2. The thermally expandable fireproof material according to claim 1, having an expansion ratio of 5 to 80 times when expanded at 150°C.

3. The thermally expandable fireproof material according to claim 1 or 2, having an expansion ratio of 30 to 80 times when expanded at 400°C.

4. The thermally expandable fireproof material according to claim 1 or 2, comprising thermally expandable microcapsules as the low-temperature foaming substance.

5. The thermally expandable fireproof material according to claim 1 or 2, wherein the low-temperature foaming substance has a foaming start temperature of 100 to 140°C.

6. The thermally expandable fireproof material according to claim 1 or 2, wherein the thermally expandable graphite has an expansion start temperature of 160 to 260°C.

7. The thermally expandable fire-resistant material according to claim 1 or 2, which is for building materials.

Citation Information

Patent Citations

  • Thermal expansible fireproof composition

    JP2005054163A

  • Fire-resistant resin composition, fire-resistant resin strip, fire-resistant tape

    JP2007161976A

  • Fire protection construction of compartment through-hole

    JP2016223162A

  • Thermally-expandable refractory material for cabinets, refractory sheet for cabinets, and cabinet for portable electronic devices

    JP2021080382A

  • Composition of matter for a fire retardant intumescent material having two stages of expansion and a process for making thereof

    US5132054A