Nonwoven fabric and production method of nonwoven fabric
A nonwoven fabric made of 4-methyl-1-pentene polymer fibers with controlled diameter and composition ensures stable filtration performance in acidic and basic solutions by resisting dissolution, addressing the issue of conventional fabrics degrading in such environments.
Patent Information
- Application Number
- JP2023059207
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional liquid filters made from PVA or PEs nonwoven fabrics dissolve in acidic or basic solutions, leading to a deterioration of filtration performance over time.
A nonwoven fabric composed of 4-methyl-1-pentene polymer fibers with a standard deviation of average fiber diameter of 0.25 μm or less, an endothermic end temperature of 230°C or less, and a specific composition that maintains stability in acidic and basic solutions, produced through an electrospinning method using a solvent with a Hildebrand solubility parameter of 8.0 or more.
The nonwoven fabric maintains high filtration performance in acidic and basic solutions, with improved durability and filtration efficiency due to the uniform fiber diameter and resistance to dissolution.
Smart Images

Figure 2024146361000005 
Figure 2024146361000006 
Figure 2024146361000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to nonwoven fabrics and methods for making nonwoven fabrics. [Background technology]
[0002] Synthetic fibers (hereinafter, simply referred to as "fibers") and fiber structures made of synthetic fibers are used in various fields such as clothing, construction, and electrical fields. In recent years, due to the diversification of applications of these fibers and fiber structures, there is a demand for fibers with small fiber diameters.
[0003] The characteristics of a fiber structure using fibers with a small fiber diameter include a large surface area, a high porosity, a small pore size, high air permeability, a high fluid permeation rate, etc. Therefore, the fiber structure using fibers with a small fiber diameter is used particularly for filters.
[0004] For example, electrospinning is known as one method for producing fibers with a small fiber diameter (for example, an average fiber diameter of 1 μm or less). In the electrospinning method, nanofibers with an average fiber diameter of several tens of nm to several μm can be easily produced by applying a voltage to various spinning solutions (for example, Patent Document 1). Patent Document 2 discloses a fiber structure using polyvinyl alcohol fibers (hereinafter, also referred to as "PVA nonwoven fabric"). Patent Document 3 discloses a nonwoven fabric made of aliphatic polyester fibers (hereinafter, also referred to as "PEs nonwoven fabric"). Non-Patent Document 1 discloses a nonwoven fabric made of poly-4-methyl-1-pentene fibers. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent Publication No. 2009-523196 [Patent Document 2] JP 2008-179629 A [Patent Document 3] International Publication No. 2020 / 013199 [Non-patent literature]
[0006] [Non-Patent Document 1] K.-H.Lee, S.Givens, DBChase, JFRabolt, Polymer, Vol.47, 8013-8018(2006) Summary of the Invention [Problem to be solved by the invention]
[0007] Liquid filters remove solid foreign matter from solutions. Liquid filters used for CMP (Chemical Mechanical Polishing) slurries and the like are required to maintain high filtering performance not only in neutral water, but also when immersed in acidic or basic solutions for a long period of time (e.g., 3 hours).
[0008] However, when the PVA nonwoven fabric disclosed in Patent Document 2 or the PEs nonwoven fabric disclosed in Patent Document 3 is used as a liquid filter, the resin constituting the liquid filter may dissolve in an acidic or basic solution. As a result, when the conventional liquid filter is immersed in an acidic or basic solution for a long period of time (e.g., 3 hours), the filtering performance may deteriorate.
[0009] As a result of the inventor's investigation, it was found that the fiber diameters of the fibers constituting the nonwoven fabric made of the poly(4-methyl-1-pentene) fibers disclosed in Non-Patent Document 1 vary. As a result, it was found that there is room for improvement in the filtration performance.
[0010] The embodiments of the present disclosure have been made in consideration of the above, and have an objective of providing a nonwoven fabric that can maintain high filtration performance in acidic solutions and basic solutions, and a method for manufacturing the nonwoven fabric. [Means for solving the problem]
[0011] Means for solving the above problems include the following embodiments. <1> The fiber comprises a plurality of fibers each containing a 4-methyl-1-pentene polymer (A), The standard deviation of the average fiber diameter of the plurality of fibers is 0.25 μm or less; The plurality of fibers satisfy the following requirement (I): Requirement (I): The endothermic end temperature (TmE) in the melting curve measured by differential scanning calorimetry is 230°C or lower. <2> The standard deviation of the average fiber diameter of the plurality of fibers is 0.22 μm or less. <1> The nonwoven fabric described in <3> The average fiber diameter of the plurality of fibers is 0.45 μm or less. <1> or <2> The nonwoven fabric described in <4> The content of the 4-methyl-1-pentene polymer (A) relative to the total amount of the plurality of fibers is 90 mass% or more. <1> ~ <3> 13. The nonwoven fabric according to any one of claims 1 to 12. <5> The plurality of fibers further satisfy the following requirement (II): <1> ~ <4> 13. The nonwoven fabric according to any one of claims 1 to 12. Requirement (II): The difference ΔT (TmE-Tm) between the endothermic temperature (TmE) in the melting curve measured by differential scanning calorimetry and the melting point (Tm) measured by differential scanning calorimetry is 10℃ to 30℃. <6> The 4-methyl-1-pentene polymer (A) satisfies the following requirement (i): <1> ~ <5> 13. The nonwoven fabric according to any one of claims 1 to 12. Requirement (i): Contains a structural unit (P) derived from 4-methyl-1-pentene and at least one structural unit (AQ) derived from a linear α-olefin having 6 to 20 carbon atoms (excluding 4-methyl-1-pentene). <7> The 4-methyl-1-pentene polymer (A) satisfies the following requirement (ii): <6> The nonwoven fabric described in Requirement (ii): the amount (U1) of the structural unit (P) and the total amount (U2) of the at least one kind of structural unit (AQ) is 84.0 mol% to 95 mol%, and the total amount (U2) of the at least one kind of structural unit (AQ) is 16.0 mol% to 5 mol%, relative to the total of 100 mol% of the amount (U1) of the structural unit (P) and the total amount (U2) of the at least one kind of structural unit (AQ). <8> The at least one type of constitutional unit (AQ) includes at least two types of the constitutional units (AQ). <7> The nonwoven fabric described in <9> The intrinsic viscosity [η] of the plurality of fibers at 135° C. is 1.7 dl / g to 5.5 dl / g. <1> ~ <8> 13. The nonwoven fabric according to any one of claims 1 to 12. <10> The number of polymer spheres observed on the surface was 2.0 / mm 2 The above-mentioned <1> ~ <9> 13. The nonwoven fabric according to any one of claims 1 to 12. <11> The method includes spinning the electrospinning composition by an electrospinning method, The method for producing a nonwoven fabric, wherein the electrospinning composition contains a 4-methyl-1-pentene polymer (A) that satisfies the following requirement (I) and a solvent having a Hildebrand solubility parameter of 8.0 or more: Requirement (I): The endothermic end temperature (TmE) in the melting curve measured by differential scanning calorimetry is 230°C or lower. <12> The solvent has a Hildebrand solubility parameter of 8.3 or more. <11> A method for producing the nonwoven fabric described above. <13> The solvent is a poor solvent having a Hildebrand solubility parameter of 8.0 or more; a good solvent having a Hildebrand solubility parameter of less than 8.0; Including, a ratio of the poor solvent to the total amount of the good solvent and the poor solvent is 5% by volume to 45% by volume; The ratio of the good solvent to the total amount of the good solvent and the poor solvent is 55% by volume to 95% by volume. <11> or <12> A method for producing the nonwoven fabric described above. Effect of the Invention
[0012] According to an embodiment of the present disclosure, a nonwoven fabric capable of maintaining high filtration performance in an acidic solution and a basic solution, and a method for manufacturing the nonwoven fabric are provided. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a schematic diagram showing an example of an electrospinning apparatus. [Diagram 2] FIG. 2 is a photograph showing an example of polymer spheres present within a nonwoven fabric. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] In the present disclosure, the use of "to" indicating a numerical range means that the numerical values before and after it are included as the lower limit and upper limit. In the present disclosure, in the ranges described stepwise, the upper or lower limit value described in one range may be replaced with the upper or lower limit value of another range described stepwise. In the ranges described in the present disclosure, the upper or lower limit value of the range may be replaced with the value shown in the examples. In the present disclosure, the term "step" refers not only to an independent step, but also to a step that cannot be clearly distinguished from other steps, as long as the intended purpose of the step is achieved. In this disclosure, when referring to the amount of each component in a composition, if multiple substances corresponding to each component are present in the composition, it means the total amount of multiple substances present in the composition, unless otherwise specified. In this disclosure, "nonwoven fabric" refers to a flat assembly of fibers that has a certain level of structural strength achieved by physical and / or chemical processes, excluding weaving, knitting, and papermaking.
[0015] (1) Nonwoven fabric The nonwoven fabric of the present disclosure (hereinafter also simply referred to as "nonwoven fabric") is made of a plurality of fibers (hereinafter also simply referred to as "fibers") containing a 4-methyl-1-pentene polymer (A). The standard deviation of the average fiber diameter of the plurality of fibers is 0.25 μm or less. The plurality of fibers satisfy the following requirement (I). Requirement (I): The endothermic end temperature (TmE) in the melting curve measured by differential scanning calorimetry (hereinafter also referred to as "DSC") is 230°C or less.
[0016] Since the nonwoven fabric of the present disclosure has the above-described configuration, it can maintain high filtration performance in acidic and basic solutions. This effect is believed to be due to, but not limited to, the following reasons. In the present disclosure, each of the multiple fibers constituting the nonwoven fabric contains a 4-methyl-1-pentene polymer (A), and therefore the multiple fibers constituting the nonwoven fabric are unlikely to dissolve in an acid-resistant solution or a basic solution. In other words, the filtration performance of the nonwoven fabric of the present disclosure is unlikely to deteriorate even if it is immersed in an acidic solution or a basic solution for a long period of time (e.g., 3 hours). The standard deviation of the average fiber diameter of the plurality of fibers being 0.25 μm or less and the plurality of fibers satisfying the above requirement (I) indicates that the plurality of fibers constituting the nonwoven fabric of the present disclosure are thin (e.g., 1.0 μm or less) and each of the plurality of fibers constituting the nonwoven fabric of the present disclosure has little fiber unevenness, i.e., the nonwoven fabric of the present disclosure has an excellent balance between filtration performance and liquid permeability. From the above, it is presumed that the nonwoven fabric of the present disclosure, because of the above-mentioned configuration, is able to maintain high filtration performance in acidic and basic solutions.
[0017] The nonwoven fabric is a sheet-like material. The structure of the nonwoven fabric is appropriately selected depending on the application of the nonwoven fabric, and may be, for example, a single-layer structure or a multi-layer structure of two or more layers.
[0018] The thickness of the nonwoven fabric is not particularly limited and is appropriately selected depending on the application. The thickness of the nonwoven fabric is preferably 0.005 mm to 10 mm, more preferably 0.01 mm to 2 mm. When the thickness is 0.005 mm or more, the balance between the dust collection efficiency and the pressure loss is preferably ensured when the nonwoven fabric is used as a filter, and the filtration performance tends to be improved. When the thickness is 10 μm or less, the thickness of the filter tends to be thin. According to the nonwoven fabric of the present disclosure, the variation in fiber diameter is suppressed, and the collection efficiency is improved. Therefore, even if the thickness is made thinner than that of conventional nonwoven fabrics, the filtration performance of the nonwoven fabric of the present disclosure tends to be excellent. The method for measuring the thickness of the nonwoven fabric is the same as the method described in the examples.
[0019] The basis weight of the nonwoven fabric is not particularly limited and is appropriately selected depending on the application. The basis weight of the nonwoven fabric is preferably 0.001 g / m 2 ~30g / m 2 , more preferably 0.002 g / m 2 ~20g / m 2 The basis weight is 0.001g / m 2 When the fiber density is 30 g / m or more, the strength of the nonwoven fabric is improved, and the nonwoven fabric tends to be easier to manufacture. 2 When the nonwoven fabric has a surface area of 10 mm or less, the pressure loss of the nonwoven fabric does not become too high, and the nonwoven fabric tends to be suitable for use as a filter. The method for measuring the basis weight of the nonwoven fabric is the same as that described in the Examples.
[0020] The number of polymer spheres observed on the surface of the nonwoven fabric was 2.0 / mm 2 It is preferable that the number of polymer spheres observed on the surface of the nonwoven fabric is 1.0 spheres / mm or less. This improves the filtration performance of the nonwoven fabric. From the viewpoint of further improving the filtration performance of the nonwoven fabric, it is more preferable that the number of polymer spheres observed on the surface of the nonwoven fabric is 1.0 spheres / mm or less. 2 Less than or equal to 0.85 pieces / mm 2 Less than 0.7 pieces / mm 2 The following is the result. The lower limit of the number of polymer balls is not particularly limited, but is, for example, 0.01 balls / mm 2 More than 0.05 pieces / mm 2 It may be more than that. The method for measuring the number of polymer spheres is the same as that described in the Examples.
[0021] The filtration performance of a nonwoven fabric is expressed as a quality factor (hereinafter also referred to as "Q value"). Hereinafter, the filtration performance of a nonwoven fabric in a basic solution is also referred to as "Q value (basic)", and the filtration performance of a nonwoven fabric in an acidic solution is also referred to as "Q value (acidic)".
[0022] The Q value (basicity) is calculated from the pressure loss and particle rejection rate by the following formula (a1): As shown in formula (a1), the lower the pressure loss and the higher the particle collection performance, the higher the Q value (basicity), indicating that the filtration performance is good when the nonwoven fabric is used as a filter. Formula (a1): Q value (basicity) (Pa -1 )=-[ln(1-[rejection rate]) / (pressure loss (Pa))] In formula (a1), "rejection rate" indicates the rate at which a nonwoven fabric in a basic test liquid containing a specific particle blocks a specific particle attempting to pass through the nonwoven fabric, and is measured by a method similar to that described in the Examples. "Pressure loss" indicates the pressure difference before and after the nonwoven fabric when the basic test liquid is passed through the nonwoven fabric at a specific flow rate, and is measured by a method similar to that described in the Examples.
[0023] The Q value (acidity) is calculated from the pressure loss and particle rejection rate by the following formula (a2): As shown in formula (a2), the lower the pressure loss and the higher the particle collection performance, the higher the Q value (acidity), indicating that the filtration performance is good when the nonwoven fabric is used as a filter. Formula (a2): Q value (acidity) (Pa -1 )=-[ln(1-[rejection rate]) / (pressure loss (Pa))] In formula (a2), "rejection rate" indicates the rate at which a nonwoven fabric in an acidic test liquid containing a specific particle blocks a specific particle attempting to pass through the nonwoven fabric, and is measured by a method similar to that described in the Examples. "Pressure loss" indicates the pressure difference before and after the nonwoven fabric when the flow rate of the acidic test liquid is a specific flow rate, and is measured by a method similar to that described in the Examples.
[0024] From the viewpoint of improving the filtration performance, the Q value (acidity) and the Q value (basicity) are both preferably 0.0028 or more, more preferably 0.0030 or more, even more preferably 0.0035 or more, particularly preferably 0.0038 or more, and even more preferably 0.0040 or more. The Q value (acidity) and the Q value (basicity) are not particularly limited, and may be 0.5 or less, or may be 0.4 or less. From these viewpoints, the Q value (acidity) and the Q value (basicity) of the nonwoven fabric are both preferably 0.0028 to 0.5, more preferably 0.0030 to 0.5, even more preferably 0.0035 to 0.4, particularly preferably 0.0038 to 0.4, and even more preferably 0.0040 to 0.4.
[0025] The nonwoven fabric of the present disclosure may be subjected to various post-treatments, if necessary, so that the nonwoven fabric is suitable for various applications. Examples of post-treatments include heat treatment and calendaring for the purpose of improving mechanical strength. The nonwoven fabric of the present disclosure may be used as a single nonwoven fabric, may be used as a fiber assembly, or may be used as a laminate. The fiber assembly is formed by accumulating fibers such as woven fabrics, knitted fabrics, and nonwoven fabrics. The laminate has a fiber assembly and a fiber layer for improving various physical properties such as strength. The fiber layer is laminated and integrated with the fiber assembly. The nonwoven fabric of the present disclosure may be subjected to secondary processing (e.g., bending, cutting, etc.) so that it can be applied to various applications.
[0026] (1.1) Fiber The fibers contained in the nonwoven fabric of the present disclosure include a 4-methyl-1-pentene polymer (A). Details of the 4-methyl-1-pentene polymer (A) will be described later.
[0027] From the viewpoint of improving the filtration performance of the nonwoven fabric, the average fiber diameter of the fibers is preferably 1 μm or less, more preferably 0.6 μm or less, even more preferably 0.45 μm or less, particularly preferably 0.4 μm or less, and even more preferably 0.28 μm or less. The average fiber diameter of the fibers may be, for example, 0.2 μm or more. From the viewpoint of improving the filtration performance of the nonwoven fabric, the average fiber diameter of the fibers is preferably 0.2 μm to 1 μm, more preferably 0.2 μm to 0.6 μm, even more preferably 0.2 μm to 0.45 μm, particularly preferably 0.2 μm to 0.40 μm, and even more preferably 0.2 μm to 0.28 μm. When the average fiber diameter of the fibers is 0.45 μm or less, high filtration performance can be maintained in an acidic solution and a basic solution. The method for measuring the average fiber diameter of the fibers is the same as the method described in the Examples.
[0028] The standard deviation of the average fiber diameter of the fibers is 0.25 μm or less. From the viewpoint of improving the filtration performance of the nonwoven fabric, the standard deviation of the average fiber diameter of the fibers is preferably 0.23 μm or less, more preferably 0.22 μm or less, even more preferably 0.20 μm or less, particularly preferably 0.18 μm or less, even more preferably 0.16 μm or less, and even more preferably 0.14 μm or less. The standard deviation of the average fiber diameter of the fibers may be, for example, 0.03 μm or more, or may be 0.05 μm or more. From the viewpoint of improving the filtration performance of the nonwoven fabric, the standard deviation of the average fiber diameter of the fibers is preferably 0.03 μm to 0.25 μm, more preferably 0.03 μm to 0.23 μm, even more preferably 0.03 μm to 0.20 μm, particularly preferably 0.05 μm to 0.18 μm, even more preferably 0.05 μm to 0.16 μm, and even more preferably 0.05 μm to 0.14 μm. When the standard deviation of the average fiber diameter of the fibers is 0.22 μm or less, high filtration performance can be maintained in an acidic solution and a basic solution. The method for measuring the standard deviation of the average fiber diameter of the fibers is the same as that described in the Examples.
[0029] From the viewpoint of improving filtration performance, the coefficient of variation value (hereinafter also referred to as "CV value") of the fiber is preferably 80% or less, more preferably 70% or less, even more preferably 60% or less, and particularly preferably 55% or less. The CV value of the fiber may be, for example, 20% or more. The CV value is preferably 20% to 80%, more preferably 20% to 70%, even more preferably 20% to 60%, and particularly preferably 20% to 55%. The method for measuring the CV value of the fiber is the same as the method described in the Examples.
[0030] The endothermic end temperature (TmE) in the melting (endothermic) curve of the fiber measured by DSC is not higher than 230° C. This makes it possible to obtain a nonwoven fabric having a small average fiber diameter and small variation in the average fiber diameter of the fibers, as described below. The "endothermic end temperature" means the temperature at which melting ends. The endothermic end temperature and the exothermic start temperature described below are indicators different from the onset and offset, which are generally the intersection points between the baseline and the tangent to the steady line. The endothermic end temperature (TmE) is preferably less than 230° C., more preferably 228° C. or less, and even more preferably less than 228° C. The method for measuring the endothermic end temperature (TmE) of the fiber is the same as that described in the Examples.
[0031] From the viewpoint of improving the heat resistance of the fiber, the melting point (Tm) of the fiber is preferably 170°C to 220°C, more preferably 175°C to 215°C, and further preferably 180°C to 210°C. The melting point (Tm) of the fiber tends to depend on the stereoregularity of the 4-methyl-1-pentene polymer (A) and the content of the α-olefin structural unit contained in the 4-methyl-1-pentene polymer (A). Therefore, the melting point (Tm) can be adjusted by using an olefin polymerization catalyst described later and further controlling the content of the α-olefin structural unit. The method for measuring the melting point (Tm) of the fiber is the same as that described in the Examples.
[0032] From the viewpoint of improving the filtration performance, the heat generation onset temperature (TcS) in the crystallization (heat generation) curve measured by DSC is preferably 205° C. or less, more preferably 200° C. or less, and further preferably 195° C. or less. The method for measuring the heat generation onset temperature (TcS) is the same as that described in the Examples. "Exotherm onset temperature" refers to the temperature at which crystallization of the fiber begins.
[0033] From the viewpoint of improving the filtration performance, the crystallization temperature (Tc) of the fiber measured by DSC is preferably 110°C to 220°C, more preferably 120°C to 205°C. The crystallization temperature (Tc) value tends to depend on the stereoregularity of the 4-methyl-1-pentene polymer (A) and the content of linear α-olefin structural units having 6 to 20 carbon atoms. It can be adjusted by using an olefin polymerization catalyst described later and further controlling the content of linear α-olefin structural units having 6 to 20 carbon atoms.
[0034] From the viewpoint of reducing the number of polymer spheres and improving the filtration performance of the nonwoven fabric, the intrinsic viscosity [η] of the fiber measured in decalin at 135°C is preferably 0.5 dl / g to 6.0 dl / g, more preferably 1.7 dl / g to 5.5 dl / g, even more preferably 1.8 dl / g to 5.3 dl / g, particularly preferably 2.0 dl / g to 5.3 dl / g, even more preferably 2.2 dl / g to 5.3 dl / g, and even more preferably 2.2 dl / g to 5.2 dl / g. When the intrinsic viscosity [η] of the fiber at 135°C is 1.7 dl / g to 5.5 dl / g, a fiber having a small fiber diameter can be spun, and therefore a nonwoven fabric that maintains high filtration performance in an acidic solution and a basic solution can be obtained. The value of the intrinsic viscosity [η] can be adjusted by the amount of hydrogen added in the polymerization step when producing the 4-methyl-1-pentene polymer (A). The method for measuring the intrinsic viscosity [η] in the fiber is the same as that described in the Examples.
[0035] The fibers preferably further satisfy the following requirement (II). The fact that the fibers further satisfy the following requirement (II) indicates that the crystal size and lamellar thickness of the resin constituting the fibers are uniform, and that the molecular weight distribution of the resin constituting the fibers is narrow. This indicates that the resin constituting the fibers does not contain molecules significantly larger than the average, and that the 4-methyl-1-pentene polymer (A) does not reaggregate in the solvent of the electrospinning composition in the fiber manufacturing method described below. Therefore, it is soluble in a solvent with a relatively high Hildebrand solubility parameter (hereinafter also referred to as "SP value") (for example, 8.0 or more), and the interaction between the electric field and the solution containing the fibers can be increased. As a result, a fiber with a small standard deviation of the average fiber diameter can be manufactured in electrospinning. Requirement (II): The difference ΔT (TmE-Tm) between the endothermic temperature (TmE) in the melting (endothermic) curve measured by DSC and the melting point (Tm) measured by DSC is 10℃ to 30℃. From the viewpoint of improving the filtration performance, ΔT (TmE-Tm) may be 10° C. to 80° C., 10° C. to 70° C., 10° C. to 50° C., or 10° C. to 30° C. ΔT (TmE-Tm) is more preferably 12° C. to 25° C., and further preferably 13° C. to 22° C.
[0036] The content of the 4-methyl-1-pentene polymer (A) relative to the total amount of the plurality of fibers is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 99% by mass or more, from the viewpoint of excellent filtration performance. The content of the 4-methyl-1-pentene polymer (A) relative to the total amount of the plurality of fibers is not particularly limited, but may be 100% by mass or less. The content of the 4-methyl-1-pentene polymer (A) relative to the total amount of the plurality of fibers is preferably 90% by mass to 100% by mass, more preferably 95% by mass to 100% by mass, and even more preferably 99% by mass to 100% by mass. When the content of the 4-methyl-1-pentene polymer (A) relative to the total amount of the plurality of fibers is 90% by mass or more, a nonwoven fabric that maintains high filtration performance in acidic solutions and basic solutions can be obtained.
[0037] The fibers contained in the nonwoven fabric of the present disclosure may contain commonly used additives as necessary, such as various known additives, such as antioxidants, weathering stabilizers, heat stabilizers, light stabilizers, antistatic agents, antifogging agents, lubricants, dyes, pigments, natural oils, synthetic oils, and waxes.
[0038] (1.2) 4-Methyl-1-pentene polymer (A) In the melting (endothermic) curve measured by DSC, the endothermic end temperature (TmE) of the 4-methyl-1-pentene polymer (A) is preferably 230° C. or lower. The preferred range of the endothermic end temperature (TmE) of the 4-methyl-1-pentene polymer (A) is the same as the preferred range of the endothermic end temperature (TmE) of the fiber. The method for measuring the endothermic end temperature (TmE) of the 4-methyl-1-pentene polymer (A) will be described in detail in the Examples.
[0039] The melting point (Tm) of the 4-methyl-1-pentene polymer (A) measured by DSC is the same as the range exemplified as the preferred range of the melting point (Tm) of the fiber. The melting point (Tm) of the 4-methyl-1-pentene polymer (A) tends to depend on the stereoregularity of the 4-methyl-1-pentene polymer (A) and the content of the α-olefin structural unit contained in the 4-methyl-1-pentene polymer (A). Therefore, the melting point (Tm) of the 4-methyl-1-pentene polymer (A) can be adjusted by using an olefin polymerization catalyst described later and further controlling the content of the α-olefin structural unit. The method for measuring the melting point (Tm) of the 4-methyl-1-pentene polymer (A) is the same as the method described in the Examples.
[0040] The exothermic onset temperature (TcS) of the 4-methyl-1-pentene polymer (A) in the crystallization (exothermic) curve measured by DSC is the same as the range exemplified as the preferred range of the exothermic onset temperature (TcS) of the fiber. The method for measuring the exothermic onset temperature (TcS) of the 4-methyl-1-pentene polymer (A) is the same as the method described in the Examples.
[0041] The crystallization temperature (Tc) of the 4-methyl-1-pentene polymer (A) measured by DSC is the same as the range exemplified as the preferred range of the crystallization temperature (Tc) of the fiber. The value of the crystallization temperature (Tc) of the 4-methyl-1-pentene polymer (A) tends to depend on the stereoregularity of the 4-methyl-1-pentene polymer (A) and the content of the linear α-olefin structural unit having 6 to 20 carbon atoms, and can be adjusted by using an olefin polymerization catalyst described later and further controlling the content of the linear α-olefin structural unit having 6 to 20 carbon atoms. The method for measuring the crystallization temperature (Tc) of the 4-methyl-1-pentene polymer (A) is the same as the method described in the Examples.
[0042] The intrinsic viscosity [η] of the 4-methyl-1-pentene polymer (A) measured in decalin at 135°C is the same as the range exemplified as the preferred range of the intrinsic viscosity [η] of the fiber. The value of the intrinsic viscosity [η] of the 4-methyl-1-pentene polymer (A) can be adjusted by the amount of hydrogen added in the polymerization step for producing the 4-methyl-1-pentene polymer (A). The method for measuring the intrinsic viscosity [η] of the 4-methyl-1-pentene polymer (A) is the same as the method described in the Examples.
[0043] The 4-methyl-1-pentene polymer (A) may be modified or unmodified. Even if the 4-methyl-1-pentene polymer (A) is unmodified, it can be dissolved in a solvent and the above-mentioned object can be achieved. The 4-methyl-1-pentene polymer (A) may be a polymer that is entirely unmodified or a polymer that is partially unmodified.
[0044] The 4-methyl-1-pentene polymer (A) preferably satisfies the following requirement (i). Requirement (i): Contains a structural unit (P) derived from 4-methyl-1-pentene and at least one structural unit (AQ) derived from a linear α-olefin having 6 to 20 carbon atoms (excluding 4-methyl-1-pentene).
[0045] When the 4-methyl-1-pentene polymer (A) satisfies the above requirement (i), a nonwoven fabric that maintains high filtration performance in acidic and basic solutions can be obtained.
[0046] The 4-methyl-1-pentene polymer (A) preferably satisfies the following requirement (ii) in addition to satisfying the above requirement (i). Requirement (ii): the amount (U1) of the structural unit (P) and the total amount (U2) of the at least one kind of structural unit (AQ) is 84.0 mol% to 95 mol%, and the total amount (U2) of the at least one kind of structural unit (AQ) is 16.0 mol% to 5 mol%, relative to the total of 100 mol% of the amount (U1) of the structural unit (P) and the total amount (U2) of the at least one kind of structural unit (AQ).
[0047] When the 4-methyl-1-pentene polymer (A) satisfies the above requirement (ii) in addition to the above requirement (i), a nonwoven fabric that maintains high filtration performance in acidic and basic solutions can be obtained.
[0048] When the 4-methyl-1-pentene polymer (A) satisfies the above requirements (i) and (ii), the at least one structural unit (AQ) preferably contains at least two of the structural units (AQ), which results in a nonwoven fabric that maintains high filtration performance in acidic and basic solutions. The number of types of structural units (AQ) is preferably 2 to 5, more preferably 2 to 4, even more preferably 2 to 3, and particularly preferably 2, from the viewpoint of obtaining a nonwoven fabric that maintains high filtration performance in acidic and basic solutions.
[0049] The amount (U1) of the structural unit (P) derived from 4-methyl-1-pentene is preferably 84.0 mol% to 100 mol%, more preferably 90.0 mol% to 99.0 mol%, even more preferably 94.0 mol% to 98.5 mol%, and particularly preferably 94.5 mol% to 98.0 mol%, based on the total amount (U2) of the structural unit (P) (U1) and the at least one structural unit (AQ) (100 mol%). When the amount (U1) of the structural unit (P) is within the above range, the heat resistance of the nonwoven fabric is more excellent.
[0050] The total amount (U2) of at least one structural unit (AQ) derived from a linear α-olefin having 6 to 20 carbon atoms is preferably 16.0 mol% to 0 mol%, more preferably 10.0 mol% to 1.0 mol%, even more preferably 6.0 mol% to 1.5 mol%, and particularly preferably 5.5 mol% to 2.0 mol%, relative to the total amount (U2) of the structural unit (P) (U1) and the at least one structural unit (AQ) (100 mol%). When the total amount (U2) of the at least one structural unit (AQ) is within the above range, the heat resistance of the nonwoven fabric is more excellent.
[0051] From the viewpoint of improving the filter performance, the linear α-olefin having 6 to 20 carbon atoms is preferably a linear α-olefin having 6 to 18 carbon atoms. Specifically, the linear α-olefin having 6 to 20 carbon atoms is preferably 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-heptadecene, 1-octadecene, etc., and among these, 1-decene, 1-hexadecene, and 1-octadecene are preferable. The linear α-olefin having 6 to 20 carbon atoms may be used alone, but it is preferable to use two or more kinds.
[0052] The 4-methyl-1-pentene polymer (A) may contain structural units derived from other polymerizable compounds, as long as the object of the present invention is not impaired. Examples of such other polymerizable compounds include vinyl compounds having a cyclic structure (e.g., styrene, vinylcyclopentene, vinylcyclohexane, vinylnorbornane, etc.), vinyl esters (e.g., vinyl acetate, etc.), unsaturated organic acids (e.g., maleic anhydride, etc.) or derivatives thereof, conjugated dienes (e.g., butadiene, isoprene, pentadiene, 2,3-dimethylbutadiene, etc.), and non-conjugated polyenes. Examples of non-conjugated polyenes include 1,4-hexadiene, 1,6-octadiene, 2-methyl-1,5-hexadiene, 6-methyl-1,5-heptadiene, 7-methyl-1,6-octadiene, dicyclopentadiene, cyclohexadiene, dicyclooctadiene, methylenenorbornene, 5-vinylnorbornene, 5-ethylidene-2-norbornene, 5-methylene-2-norbornene, 5-isopropylidene-2-norbornene, 6-chloromethyl-5-isopropenyl-2-norbornene, 2,3-diisopropylidene-5-norbornene, 2-ethylidene-3-isopropylidene-5-norbornene, and 2-propenyl-2,2-norbornadiene.
[0053] The 4-methyl-1-pentene polymer (A) may contain units derived from such other polymerizable compounds in an amount of preferably 10 mol % or less, more preferably 5 mol % or less, and even more preferably 3 mol % or less, relative to 100 mol % in total of structural units derived from all polymerizable compounds contained in the 4-methyl-1-pentene polymer (A).
[0054] The method for measuring the content of the structural units derived from 4-methyl-1-pentene and the structural units derived from at least one selected from linear α-olefins having 6 to 20 carbon atoms in the 4-methyl-1-pentene polymer (A) is the same as that described in the Examples.
[0055] The density of the 4-methyl-1-pentene polymer (A) is preferably 820 kg / m 3~850kg / m 3 , more preferably 825 kg / m 3 ~850kg / m 3 , more preferably 825 kg / m 3 ~845kg / m 3 , particularly preferably 825 kg / m 3 ~840kg / m 3 The density value of the 4-methyl-1-pentene polymer (A) can be adjusted by selecting the type and content of other olefins to be polymerized together with 4-methyl-1-pentene. The density can be measured according to JIS K6268. The 4-methyl-1-pentene polymer (A) having a density in the above range has excellent filtration performance.
[0056] The molecular weight distribution (Mw / Mn), which is the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the 4-methyl-1-pentene polymer (A) measured by gel permeation chromatography (GPC), is preferably 1.0 to 3.5, more preferably 1.3 to 3.0, and even more preferably 1.5 to 2.5. The molecular weight distribution (Mw / Mn) can be adjusted by the type of olefin polymerization catalyst, particularly the metallocene catalyst, described later. The molecular weight distribution (Mw / Mn) can be measured using a gel permeation chromatograph Alliance GPC-2000 manufactured by Waters. The 4-methyl-1-pentene polymer (A) having a molecular weight distribution (Mw / Mn) in the above range is preferable from the viewpoints of transparency and mechanical properties. When the molecular weight distribution of the 4-methyl-1-pentene polymer (A) is in the above range, the affinity with the solvent described below is increased, and the stability of the composition is improved.
[0057] The 4-methyl-1-pentene polymer (A) can be obtained by polymerizing 4-methyl-1-pentene with the specific olefin described above, and, if necessary, with other polymerizable compounds described above, in the presence of an olefin polymerization catalyst by a known method. The olefin polymerization catalyst is preferably a metallocene catalyst, such as those described in WO 01 / 53369, WO 01 / 27124, JP-A 3-193796, JP-A 02-41303, or WO 06 / 025540.
[0058] The monomer constituting the 4-methyl-1-pentene polymer (A) may be derived from biomass.
[0059] (1.3) Uses of nonwoven fabrics The nonwoven fabric of the present disclosure can be used in a wide variety of applications in which nonwoven fabrics are typically used. The nonwoven fabric of the present disclosure can be preferably used, among others, as a filter such as a liquid filter, etc. The nonwoven fabric of the present disclosure is preferably used for a high-performance filter that has excellent filtering performance in water under acidic or basic conditions.
[0060] The nonwoven fabrics of the present disclosure have potential applications in liquid and gas filtration, and molecular filters. Additional applications of the nonwoven fabrics of the present disclosure include, for example, composite reinforcement, protective clothing, protective masks, medical prostheses, tissue engineering molds, wound dressings, biomedical applications such as drug delivery systems and pharmaceutical compositions, cell culture scaffolds, protein adsorbents, cosmetic skin care and cleaning, etc.
[0061] Applications of the nonwoven fabric of the present disclosure include, for example, articles that require blocking liquids (liquid-blocking articles), such as filters such as gas filters (air filters) and liquid filters, wipers, protective clothing, and medical gowns (particularly, disposable protective clothing and disposable medical gowns), and other medical supplies.
[0062] The nonwoven fabric of the present disclosure has small variation in fiber diameter, and therefore is less likely to form relatively large holes (defective areas) between the fibers, making the nonwoven fabric of the present disclosure suitable for use in high-performance filters with excellent filtration performance.
[0063] The liquid filter may be made of a single layer of nonwoven fabric, or may be made of a laminate of two or more layers of nonwoven fabric. The liquid filter may be made of a laminate of a nonwoven fabric and a resin film. When a laminate of two or more layers of nonwoven fabric is used as the liquid filter, the two or more layers of nonwoven fabric may simply be stacked on top of each other.
[0064] The liquid filter may be made by combining the nonwoven fabric of the present disclosure with another nonwoven fabric depending on the purpose and the liquid to be applied. In order to increase the strength of the liquid filter, a spunbond nonwoven fabric may be used as the other nonwoven fabric. The liquid filter may be a laminate of the nonwoven fabric of the present disclosure, the spunbond nonwoven fabric, and a mesh material.
[0065] The liquid filter may be subjected to, for example, a calendering process. In the calendering process, a pair of rolls with a clearance between flat rolls or crown rolls may be used in order to control the pore size and porosity to be small. In the calendering process, a pair of rolls that can apply a constant pressure without a clearance may be used. The clearance between the rolls may be appropriately changed depending on the thickness of the nonwoven fabric, and it is preferable that the gaps between the fibers of the nonwoven fabric are not eliminated.
[0066] (2) Manufacturing method of nonwoven fabric The method for producing a nonwoven fabric according to the present disclosure includes spinning an electrospinning composition by an electrospinning method (hereinafter also referred to as the "spinning step"). The electrospinning composition contains a 4-methyl-1-pentene polymer (A) that satisfies the following requirement (I) and a solvent having a Hildebrand solubility parameter of 8.0 or more. Requirement (I): The endothermic end temperature (TmE) in the melting curve measured by differential scanning calorimetry is 230°C or lower.
[0067] Since the manufacturing method for the nonwoven fabric of the present disclosure has the above-mentioned configuration, it is possible to obtain a nonwoven fabric that can maintain high filtration performance in acidic and basic solutions.
[0068] [2.1] Spinning process In the spinning step, the electrospinning composition is spun by an electrospinning method.
[0069] [2.1.1] Electrospinning The "electrospinning method" is a method in which an electrospinning composition is discharged into an electric field while a high voltage is applied, and the discharged electrospinning composition is electrically charged and stretched into a long and thin shape to form a fiber with a small fiber diameter. Specifically, a high voltage is applied to the electrospinning composition to charge it, thereby stretching the fibers into a long and thin shape, and the fibers with a small fiber diameter are deposited to obtain a nonwoven fabric.
[0070] The method of charging the electrospinning composition includes a method of electrically connecting an electrode connected to a high-voltage power supply to the electrospinning composition itself or to a container. The voltage applied to the electrode is preferably 1 kV to 100 kV, more preferably 5 kV to 50 kV. The type of voltage may be either direct current or alternating current.
[0071] The temperature during electrospinning is not particularly limited, and when a nonwoven fabric is produced using an electrospinning composition containing a solvent as described below, the temperature may be appropriately adjusted depending on the boiling point and volatility of the solvent contained in the electrospinning composition. The temperature during electrospinning is preferably 10°C to 60°C.
[0072] The inventors conducted extensive research into methods for efficiently producing nonwoven fabrics that can maintain high filtration performance in acidic and basic solutions, and as a result, discovered that conventional thermoplastic resins known thus far (such as PP (polypropylene) and poly-4-methyl-1-pentene) have low solubility in solvents, and that the SP values of solvents that dissolve thermoplastic resins are low (SP values less than 8.0).
[0073] When the solubility of the thermoplastic resin in the solvent is low, insoluble components are precipitated in the electrospinning composition. Therefore, there is a risk that thread breakage occurs easily during spinning. Furthermore, when the charged electrospinning composition is stretched into a long and thin shape, the presence of insoluble components may cause the electrospinning composition to be non-uniformly stretched. This may result in a large standard deviation of the fiber diameters of the multiple fibers contained in the obtained nonwoven fabric.
[0074] In general, the higher the SP value of a solvent, the higher the polarity of the solvent tends to be. When the SP value of a solvent that dissolves a thermoplastic resin is less than 8.0, the polarity of the solvent is relatively low. When the SP value of a solvent that dissolves a thermoplastic resin is less than 8.0, the electrospinning composition is less likely to be dielectrically polarized than when the SP value of the solvent is 8.0 or more. In other words, during electrospinning, the electrical interaction between the electric field and the electrospinning composition is small, and therefore the electrospinning composition is less likely to be stretched by the electric field. As a result, the fiber diameter of the multiple fibers contained in the obtained nonwoven fabric becomes thicker.
[0075] The inventors have succeeded in obtaining a nonwoven fabric having a small fiber diameter and small variation by using a 4-methyl-1-pentene polymer (A) having an endothermic end temperature (TmE) of 230° C. or less in the melting (endothermic) curve measured by DSC. This is believed to be because the high melting point component in the 4-methyl-1-pentene polymer (A) is reduced by setting the endothermic end temperature (TmE) of the melting (endothermic) curve measured by DSC to 230° C. or less, and as a result, the 4-methyl-1-pentene polymer (A) can be dissolved in an electrostatically charged solvent (SP value: 8.0 or more).
[0076] According to the present disclosure, a nonwoven fabric having similar performance can be obtained whether the 4-methyl-1-pentene polymer (A) is spun immediately after being dissolved in a solvent or after a certain time (e.g., 24 hours) has elapsed since being dissolved. Conventional thermoplastic resins (such as PP and poly(4-methyl-1-pentene)) known so far may precipitate over time. Therefore, the spinnability after a certain time has been extremely low.
[0077] The spinning by the electrospinning method may be carried out using an electrospinning apparatus as shown in FIG.
[0078] The electrospinning apparatus 100 includes a discharge device 101, a target electrode 102 disposed to face the discharge device 101, and a voltage application device 103. The discharge device 101 discharges an electrospinning composition. The voltage application device 103 applies a voltage between the discharge device 101 and the target electrode 102.
[0079] When the electrospinning composition is discharged from the discharge device 101 while a voltage is applied between the discharge device 101 and the target electrode 102 by the voltage application device 103, the electrospinning composition is stretched by the electric field while moving between the discharge device 101 and the target electrode 102. As a result, fibers 104 having a small average fiber diameter are formed. The fibers 104 are deposited on the target electrode 102, and as a result, a nonwoven fabric 105 is obtained.
[0080] [2.1.2] Electrospinning composition The electrospinning composition contains a 4-methyl-1-pentene polymer (A) and a solvent having an SP value of 8.0 or more. The 4-methyl-1-pentene polymer (A) is dissolved in the solvent having an SP value of 8.0 or more. The electrospinning composition is a liquid.
[0081] The content of the 4-methyl-1-pentene polymer (A) in the electrospinning composition is preferably 0.2% by mass to 40% by mass, more preferably 0.5% by mass to 30% by mass, even more preferably 1% by mass to 25% by mass, and particularly preferably 5% by mass to 20% by mass. The content of the solvent in the electrospinning composition is preferably 60% by mass to 99.8% by mass, more preferably 70% by mass to 99.5% by mass, even more preferably 75% by mass to 99% by mass, and particularly preferably 80% by mass to 95% by mass. When the contents of the 4-methyl-1-pentene polymer (A) and the solvent in the electrospinning composition are within the above ranges, the electrospinning composition has a good balance between the ease of solubility of the 4-methyl-1-pentene polymer (A) or the resin composition containing the 4-methyl-1-pentene polymer (A) in a solvent, and the ease of removal of the solvent after spinning.
[0082] [2.1.2.1] 4-Methyl-1-pentene polymer (A) Examples of the 4-methyl-1-pentene polymer (A) include the same as those exemplified as the 4-methyl-1-pentene polymer (A) contained in the fibers contained in the nonwoven fabric of the present disclosure.
[0083] In the 4-methyl-1-pentene polymer (A), the difference ΔT (TmE-Tm) between the endothermic end temperature (TmE) in the melting curve measured by differential scanning calorimetry and the melting point (Tm) measured by differential scanning calorimetry is preferably in a specific range (for example, 10°C to 30°C). That is, crystallization can be suppressed by adjusting the content of linear α-olefins having 6 to 20 carbon atoms so that the temperature at which crystallization begins and the temperature at which the crystals completely melt are as low as possible. As a result, the storage stability of the electrospinning composition is guaranteed. This is preferable because it is possible to produce a nonwoven fabric having a small average fiber diameter and a small variation in the average fiber diameter by spinning the solution by the electrospinning method described later after holding it for a certain period of time.
[0084] [2.1.2.2] Solvent The SP value, which is the solubility parameter of the solvent, is 8.0 or more. The SP value is preferably 8.3 or more, and more preferably 8.5 or more. The SP value is not particularly limited and may be 20 or less, or 15 or less. The SP value is preferably 8.0 to 20, more preferably 8.3 to 20, and even more preferably 8.5 to 15. When the SP value of the solvent is 8.3 or more, a nonwoven fabric having a small fiber diameter and small variation in diameter can be obtained.
[0085] The SP value can be expressed as follows using Hansen's SP values [δD, δP, δH]: SP value = "Square root of (δD2, δP2, δH2)"
[0086] The SP value is expressed in a three-dimensional space consisting of three components introduced by Hildebrand: the dispersion term δD, the polar term δP, and the hydrogen bond term δH. The dispersion term δD indicates the effect of dispersion forces. The polar term δP indicates the effect of dipole-dipole forces. The hydrogen bond term δH indicates the effect of hydrogen bonding forces. The definition and calculation of the SP value are described in the following Non-Patent Document 2. The SP value can be easily estimated by using computer software Hansen Solubility Parameters in Practice (HSPiP). In the present invention, the software HSPiP ver. 4.1 created by Hansen et al. is used for the actual calculation of Hansen's SP value [δD, δP, δH]. Non-patent document 2: Charles M. Hansen, Hansen Solubility Parameters: A Users Handbook (CRC Press, 2007)
[0087] The solvent may be a mixed solvent containing a good solvent and a poor solvent. A "good solvent" refers to a solvent that has a high ability to dissolve the 4-methyl-1-pentene polymer (A). Specifically, a "good solvent" refers to a solvent having an SP value of less than 8.0. A "poor solvent" refers to a solvent that has a low ability to dissolve the 4-methyl-1-pentene polymer (A). Specifically, a solvent having an SP value of 8.0 or more. Note that 4-methyl-1-pentene has low polarity. Therefore, 4-methyl-1-pentene is easily dissolved in a solvent having an SP value of less than 8.0.
[0088] It is preferable that the solvent contains a poor solvent having a Hildebrand solubility parameter of 8.0 or more and a good solvent having a Hildebrand solubility parameter of less than 8.0, the ratio of the poor solvent to the total amount of the good solvent and the poor solvent is 5% by volume to 45% by volume, and the ratio of the good solvent to the total amount of the good solvent and the poor solvent is 55% by volume to 95% by volume. This makes it possible to obtain a nonwoven fabric that can maintain higher filtration performance in acidic and basic solutions.
[0089] The SP value of the good solvent is less than 8.0, preferably 7.9 or less, and more preferably less than 7.9. The SP value of the good solvent is not particularly limited, and may be, for example, 6.0 or more, or 6.5 or more. The SP value of the good solvent is preferably 6.0 or more and less than 8.0, more preferably 6.0 to 7.9, and more preferably 6.5 or more and less than 7.9.
[0090] Specifically, examples of the good solvent include aliphatic hydrocarbons (e.g., n-hexane, n-heptane, n-octane, cyclohexane, methylcyclohexane, ethylcyclohexane, etc.), aromatic hydrocarbons (e.g., toluene, xylene, etc.), diethyl ether (DEE), etc. Among these, the good solvent is preferably toluene, cyclohexane, or methylcyclohexane. The good solvents can be used alone or in combination.
[0091] The SP value of the poor solvent is not particularly limited, and may be 25 or less, 20 or less, or 15 or less. The SP value of the poor solvent is preferably 8.0 or more, more preferably 8.5 or more, even more preferably 9.0 or more, and particularly preferably 10 or more. The SP value of the poor solvent is preferably 8.0 to 25, more preferably 8.5 to 20, even more preferably 9.0 to 20, and particularly preferably 10 to 15.
[0092] Specifically, examples of poor solvents include water, methanol, dimethyl sulfoxide (DMSO), phenol, sulfolane (SL), propylene carbonate (PC), ethanol, 1,4-butyrolactone (BL), benzyl alcohol, N,N-dimethylformamide (DMF), 2,3-butylene carbonate (BC), 1-propanol, acetonitrile (AN), 2-propanol, 1-methyl-2-pyrrolidone (NMP), N,N-dimethylacetamide (DMAc), pyridine, 1,4-dioxane, and acetic acid. Examples of poor solvents include acid, methyl formate (MF), 1,2-dichlorobenzene (DCB), acetone, cyclohexanone, dimethyl carbonate (DMC), dichloromethane, 1,1,2-trichloroethane, chloroform, methyl ethyl ketone (MEK), benzene, tetrahydrofuran (THF), toluene, methyl propionate (MP), diethyl carbonate (DEC), p-xylene, decahydronaphthalene (Decalin), carbon tetrachloride, 1,3-dioxolane (DOL), 1,1,1-trichloroethane, etc. The poor solvents can be used alone or in combination.
[0093] The SP values of each of the good solvent and the poor solvent may be confirmed by the following Non-Patent Documents 3 and 4, etc. Non-patent literature 3: Gamsjager, H., Lorimer, JW, Scharlin, P., & Shaw, DG (2008). Glossary of terms related to solubility (IUPAC Recommendations 2008). Pure and applied chemistry, 80(2), 233-276. Non-Patent Document 4: Toshikatsu Kobayashi et al. Solubility Parameter Application Examples: Based on Mechanisms and Solubility Evaluations and Calculation Examples, Information Mechanism, 2007
[0094] The ratio of the poor solvent to the total amount of the good solvent and the poor solvent is preferably 5 vol % to 45 vol %, more preferably 10 vol % to 40 vol %, and further preferably 15 vol % to 35 vol %. The ratio of the good solvent to the total amount of the good solvent and the poor solvent is preferably 55 vol % to 95 vol %, more preferably 60 vol % to 90 vol %, and further preferably 65 vol % to 85 vol %.
[0095] The SP value of the mixed solvent is in the same range as the range exemplified as the SP value of the solvent. The SP value of a mixed solvent consisting of solvent A and solvent B (hereinafter also referred to as "SPmix") is calculated by the following formula. The following formula is described in Non-Patent Document 3 mentioned above.
[0096]
number
[0097] In the above formula, "SPa" is the SP value of solvent A [(cal / cm 3 ) 0.5 "SPb" indicates the SP value of solvent B [(cal / cm 3 ) 0.5 "MVa" is the molar volume of solvent A [cm 3 / mol]. "MVb" is the molar volume of solvent B [cm 3 / mol]. "Fa" indicates the volumetric mixture fraction [-] of solvent A. "Fb" indicates the volumetric mixture fraction [-] of solvent B. "Fa" and "Fb" satisfy the relationship "Fa+Fb=1."
[0098] The electrospinning composition may further contain additives as necessary within the scope of the present disclosure, such as antioxidants, heat stabilizers, weather stabilizers, antistatic agents, slip agents, leveling agents, reinforcing agents, antiblocking agents, antifogging agents, lubricants, dyes, pigments, natural oils, synthetic oils, waxes, and fillers.
[0099] The antioxidant may be a known antioxidant. Specific examples of the antioxidant include hindered phenol compounds, sulfur-based antioxidants, lactone-based antioxidants, organic phosphite compounds, and organic phosphonite compounds. The antioxidants may be used alone or in combination.
[0100] Examples of lubricants include sodium, calcium, and magnesium salts of saturated fatty acids (e.g., lauric acid, palmitic acid, stearic acid, etc.) or unsaturated fatty acids (e.g., oleic acid, etc.). The lubricants can be used alone or in combination of two or more. The amount of the lubricant is usually 0.1 to 3 parts by mass, and preferably 0.1 to 2 parts by mass, per 100 parts by mass of the electrospinning composition.
[0101] Examples of slip agents include amides of saturated fatty acids (e.g., lauric acid, palmitic acid, stearic acid, hebenic acid, etc.) or unsaturated fatty acids (e.g., oleic acid, erucic acid, etc.), and bisamides of saturated or unsaturated fatty acids. Among them, the slip agent is preferably erucic acid amide and / or ethylene bisstearamide. The content of the slip agent is preferably 0.01 to 5 parts by mass with respect to 100 parts by mass of the 4-methyl-1-pentene polymer (A).
[0102] Examples of the antiblocking agent include finely divided silica, finely divided aluminum oxide, finely divided clay, powdered or liquid silicone resin, tetrafluoroethylene resin, finely divided crosslinked resin, such as crosslinked acrylic or methacrylic resin powder, etc. Among them, the antiblocking agent is preferably finely divided silica and crosslinked acrylic or methacrylic resin powder.
[0103] Examples of the reinforcing agent include oxides of metals (e.g., silicon, titanium, aluminum, zirconium, etc.), polyfunctional alkoxy compounds or oligomers thereof, clay minerals, etc. The content of the reinforcing agent is 5 parts by mass to 50 parts by mass with respect to 100 parts by mass of the 4-methyl-1-pentene polymer (A) in the electrospinning composition.
[0104] The method for producing the composition for electrospinning is not particularly limited, and it can be produced by a commonly used method. For example, it can be produced by adding 4-methyl-1-pentene polymer (A) to a solvent and stirring the mixture at a temperature equal to or lower than the boiling point of the solvent for a predetermined period of time. The 4-methyl-1-pentene polymer (A) has excellent storage stability and solubility when dissolved in a solvent. 4-methyl-1-pentene polymers generally have unique properties such as electrical insulation and chemical resistance. Therefore, the electrospinning composition containing the polymer (A) can be used for various purposes. EXAMPLES
[0105] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples.
[0106] [1] Measurement methods for various physical properties The methods for measuring various physical properties are as follows.
[0107] [1.1] Amount of structural units in 4-methyl-1-pentene polymer (A) The amount of structural units derived from 4-methyl-1-pentene (hereinafter also referred to as "4-methyl-1-pentene content") and the amount of structural units derived from α-olefins other than 4-methyl-1-pentene (hereinafter referred to as "α-olefin content") are 13 Calculated from C-NMR spectrum. Specifically, the fibers constituting the nonwoven fabric were used as the sample. The sample was dissolved in a mixed solvent to obtain a measurement solution. The mixed solvent consisted of o-dichlorobenzene and heavy benzene. The ratio of the content of o-dichlorobenzene to the content of heavy benzene (o-dichlorobenzene / heavy benzene) was (80% by volume / 20% by volume). The concentration of the sample in the measurement solution was 55 mg / 0.6 mL. The mixing solution was measured under the following measurement conditions. 13 The composition of 4-methyl-1-pentene and α-olefins was quantified by C-NMR spectroscopy.
[0108] [1.1.1] Measurement conditions Measurement equipment: JEOL Ltd. ECP500 nuclear magnetic resonance spectrometer Measurement temperature: 120℃ Observation kernel: 13 C(125MHz) Sequence: Single pulse proton decoupling Pulse width: 4.7μsec (45° pulse) Repeat time: 5.5 seconds Number of times: 10,000 or more Chemical shift reference value: 27.50 ppm
[0109] [1.2] Intrinsic viscosity [η] The intrinsic viscosity [η] was measured at 135°C using decalin solvent. In particular, the intrinsic viscosity [η] of the polymer was measured using a polymer powder, pellets, or resin block. The intrinsic viscosity [η] of the nonwoven fabric was measured using the fibers constituting the nonwoven fabric. Approximately 20 mg of the sample was dissolved in 15 mL of decalin, and the specific viscosity ηsp was measured in an oil bath at 135°C. After diluting the decalin solution by adding 5 mL of decalin solvent, the specific viscosity ηsp was measured in the same manner. This dilution operation was repeated two more times. As shown in the following formula (M1), the value of ηsp / C when the concentration (C) was extrapolated to 0 was taken as the "intrinsic viscosity [η]". Formula (M1): [η]=lim(ηsp / C)(C→0)
[0110] [1.3] Tm, Tc, TmE, and TcS Using a DSC measuring device (DSC220C) manufactured by Seiko Instruments Inc., an exothermic-endothermic curve was obtained in accordance with ASTM D3418, and the melting point (Tm) and crystallization temperature (Tc) were calculated as follows. Specifically, for the measurement of the physical properties of the polymer, the polymer powder, pellets, or resin mass of the polymer was used as the sample. For the measurement of the physical properties of the fiber, the fiber constituting the nonwoven fabric was used as the sample. Approximately 5 mg of the sample was placed in an aluminum pan for measurement, and the temperature was raised from 20°C to 280°C at a heating rate of 10°C / min, and the sample was held at 280°C for 5 minutes. The temperature was then lowered to 20°C at a cooling rate of 10°C / min, and the sample was held at 20°C for 5 minutes. The temperature was then raised again from 20°C to 280°C at a heating rate of 10°C / min. The crystallization peak that appeared during the first temperature drop was taken as the "crystallization temperature (Tc)". When multiple peaks were detected, the one with the highest temperature was taken as the crystallization temperature (Tc). The melting peak that appeared during the second temperature rise was taken as the "melting point (Tm)". When multiple peaks were detected, the one with the highest temperature was taken as the melting point (Tm). The temperature at which the endotherm of the melting (endotherm) curve ended was designated as the "endotherm end temperature (TmE)." The temperature at which the exotherm of the crystallization (exotherm) curve began was designated as the "exotherm start temperature (TcS)." The above-mentioned start and end points are the points at which it can be confirmed that the curve deviates from the baseline where the amount of heat becomes constant at the start or end of endothermic or exothermic reaction, and a difference in the amount of heat begins to appear.
[0111] [1.4] Average fiber diameter, standard deviation of average fiber diameter, CV value A photograph of the nonwoven fabric was taken at a magnification of 1000 times using an electron microscope (Hitachi S-3500N). The fiber diameter was measured from the obtained photograph. Specifically, fibers were randomly selected from the obtained photograph, and the photographing and diameter measurement were repeated until the total number of fibers exceeded 100. The arithmetic mean value of the obtained fiber diameters was defined as the "average fiber diameter (Da)". The standard deviation (Dp) calculated using this measurement result was defined as the "standard deviation of the average fiber diameter". As shown in the following formula (M2), the standard deviation (Dp) was divided by the average fiber diameter (Da), and the calculated value was defined as the "coefficient of variation of the fiber diameter (CV value)". Formula (M2): CV value = [standard deviation (Dp) / average fiber diameter (Da)] x 100
[0112] [1.5] Weight Three samples (size: 100 mm lengthwise × 100 mm widthwise) were taken from the nonwoven fabric, and the mass of each sample was measured. The average value obtained was converted to a value per unit area, and the calculated value obtained by rounding off to the first decimal place was defined as the "basis weight (g / m2)." 2 )".
[0113] [1.6] Thickness The thickness of the sample, which had its basis weight measured, was measured at five points, namely the center and four corners, using a thickness gauge (PEACOCK, product number "R1-250", measuring probe 25 mmφ) under a load of 7 g / m 2 The thickness of 10 samples for which the basis weight was measured was measured by this method, and the average value was taken as "thickness (mm)."
[0114] [1.7] Number of polymer balls The nonwoven fabric thus produced was photographed using an SEM. The measurement field of view at each SEM magnification was 12.7 μm × 9.3 μm at 10,000 times, 21.1 μm × 15.9 μm at 6,000 times, and 31.7 μm × 23.9 μm at 4,000 times. Ten SEM images were taken randomly under the above conditions, and the polymer spheres observed on the surface of the nonwoven fabric were measured to within 1 mm 2 The number of polymer spheres was measured per unit area. As shown in Figure 2, "polymer spheres" refer to spherical objects having a diameter larger than the fiber diameter. The polymer spheres mainly contain the resin that constitutes the fiber. The spherical objects indicated by the arrows in Figure 2 are polymer spheres. Nonwoven fabrics with a smaller number of polymer spheres tend to be more uniform and have a higher specific surface area.
[0115] [1.8] Q value As the Q value, which is an index of filtration performance, the following Q value (basicity) and Q value (acidity) were measured.
[0116] [1.9.1] Q value (basic) The manufactured nonwoven fabric was left to stand in a 25% aqueous solution of sodium hydroxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., JIS K 8576 special grade) for 3 hours and then used as a filter. Specifically, a test liquid in which polystyrene latex particles having a spherical particle diameter of 0.50 μm were dispersed at a concentration of 0.01 mass% in the aqueous solution of sodium hydroxide was used, and the concentration in the filtrate that passed through the nonwoven fabric under a pressure condition of 0.3 MPa using a filtration device (TSU-90B manufactured by ADVANTEC): C1, and the concentration in the original solution: C0 were measured, and the rejection rate was calculated by the following formula. The concentrations of the test solutions and filtrates were determined by measuring the absorbance at a wavelength of 500 nm using a spectrophotometer (Shimadzu UV3100) and calculating from a previously determined calibration curve. Interdiction rate = [(C0-C1) / C0] x 100(%)
[0117] The pressure difference before and after the filter media when the flow rate during the liquid passage was set to 25 mL / min was defined as the "pressure loss". Using the rejection rate and the pressure loss, the Q value (basicity) was calculated according to the following formula (a). The allowable range of the Q value (basicity) is 2.8 × 10 -3 That's all. Formula (a1): Q value (basicity) (Pa -1 )=-[ln(1-[rejection rate]) / (pressure loss (Pa))]
[0118] [1.9.2] Q value (acidity) The rejection rate and pressure loss were measured under the same conditions as for the Q value (basic), except that the sodium hydroxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., JIS K 8576 special grade) was replaced with hydrochloric acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., JIS K 8180 special grade). The Q value (acidic) was measured using the rejection rate and pressure loss measured under the same conditions as for the Q value (basic). The allowable range of the Q value (acidic) is 2.8 x 10 -3 That's all. Formula (a2): Q value (acidity) (Pa -1 )=-[ln(1-[rejection rate]) / (pressure loss (Pa))]
[0119] [2] Preparation The 4-methyl-1-pentene polymers (A-1) to (A-6) and the resins (B-1) to (B-3) other than the 4-methyl-1-pentene polymer (A) were prepared as follows.
[0120] [2.1] 4-Methyl-1-pentene polymer (A-1) The inside of a 1.5L stainless steel polymerization vessel equipped with an agitator was thoroughly replaced with nitrogen. 500mL of 4-methyl-1-pentene and 230mL of heptane were charged into the polymerization vessel at 23°C. 20mL of "Linearene 168" (Idemitsu Kosan Co., Ltd.) and 0.3mL of a 1.0mmol / mL toluene solution of triisobutylaluminum (TIBAL) were charged into the autoclave in succession, and stirring was started. Next, 140mL of hydrogen was charged, and the autoclave was heated to an internal temperature of 60°C. 2mL of a toluene solution prepared in advance was pressed into the autoclave with nitrogen, and polymerization was started. The toluene solution contained 0.033 mmol of methylaluminoxane and 0.00011 mmol of (8-octamethylfluoren-12'-yl-(2-(adamantan-1-yl)-8-methyl-3,3b,4,5,6,7,7a,8-octahydrocyclopenta[a]indene))zirconium dichloride in terms of Al. During the polymerization reaction, the temperature inside the autoclave was adjusted to 60°C. 13 minutes after the start of polymerization, 5 mL of methanol was injected into the autoclave with nitrogen to terminate the polymerization, and the autoclave was depressurized to atmospheric pressure. The reaction solution was poured into acetone while stirring to precipitate the polymer. The obtained polymer containing the solvent was dried at 130°C under reduced pressure for 10 hours. As a result, 4-methyl-1-pentene polymer (A-1) was obtained. The yield of the obtained 4-methyl-1-pentene polymer (A-1) was 68.4 g. The 4-methyl-1-pentene content in the 4-methyl-1-pentene polymer (A-1) was 97.6 mol %, and the α-olefin (1-hexadecene, 1-octadecene) content was 2.4 mol %.
[0121] [2.2] 4-Methyl-1-pentene polymer (A-2) [2.2.1] Slurry of prepolymerized catalyst components in decane A slurry of a prepolymerized catalyst component in decane was prepared in the manner described below in "Synthesis Example 1" to "Synthesis Example 3."
[0122] [2.2.1.1] Synthesis example 1 (transition metal compound) (8-octamethylfluoren-12'-yl-(2-(adamantan-1-yl)-8-methyl-3,3b,4,5,6,7,7a,8-octahydrocyclopenta[a]indene))zirconium dichloride (hereinafter also referred to as "the transition metal compound of Synthesis Example 1") was synthesized according to a known method (i.e., the method described in Preliminary Experiment 5 of WO 2014 / 123212).
[0123] [2.2.1.2] Synthesis Example 2 (Olefin Polymerization Catalyst) Solid polymethylaluminoxane (hereinafter also referred to as "solid MAO") was synthesized according to a known method (i.e., the method described in International Publication No. 2014 / 123212). The solid MAO was particulate. The D50 of the solid MAO was 28 μm. The aluminum atom content of the solid MAO was 43 mass%. The "D50" of the solid MAO indicates the particle size corresponding to the cumulative 50 volume% from the fine particle side in the volume-based particle size distribution measured by a particle size distribution measuring device based on the laser light diffraction scattering method. At 30°C, in a 200 mL three-neck flask equipped with a stirrer and thoroughly purged with nitrogen, 30 mL of purified decane and 14.65 mmol of solid MAO (calculated as aluminum atom) were charged under a nitrogen stream to prepare a suspension. The transition metal compound described in Synthesis Example 1 was added to toluene to obtain a toluene solution. The concentration of the transition metal compound in the toluene solution was 4.58 mmol / L. The toluene solution was added to the suspension while stirring so that the amount of the transition metal compound described in Synthesis Example 1 added was 50.0 mg (0.0586 mmol). One hour after the toluene solution was added to the suspension, stirring was stopped to obtain a mixture. The obtained mixture was washed with 100 mL of decane by decantation, and then decane was added to obtain 50 mL of a slurry liquid. The Zr support rate was 98%. The "Zr support rate" refers to the ratio (by mass) of Zr atoms supported on the solid catalyst component among the Zr atoms in the added transition metal compound.
[0124] [2.2.1.3] Synthesis Example 3 (Prepolymerization Catalyst Component) A decane solution of triisobutylaluminum was prepared. The concentration of triisobutylaluminum in the decane solution was 0.5 mmol / mL in terms of aluminum atom. The slurry liquid prepared in Synthesis Example 2 was charged into the reactor. 1.0 mL of a decane solution of triisobutylaluminum was charged into the slurry liquid prepared in Synthesis Example 2 at 25°C under a nitrogen stream. After cooling to 15°C, 10 mL of 4-methyl-1-pentene was charged into the reactor over 60 minutes. The start of charging was defined as the start of prepolymerization. Stirring was stopped 2.0 hours after the start of prepolymerization, and the resulting mixture was washed three times with 100 mL of decane by decantation. The prepolymerization catalyst component was a decane slurry (9.5 g / L, 0.56 mmol-Zr / L).
[0125] [2.2.2] Synthesis A SUS polymerization vessel with an internal volume of 1 L and an agitator was prepared. At room temperature and under a nitrogen stream, 425 mL of purified decane was charged into the polymerization vessel, and the temperature was raised to 40°C. After reaching 40°C, 0.8 mL (0.4 mmol in terms of aluminum atoms) of a decane solution of triisobutylaluminum (0.5 mmol / mL in terms of aluminum atoms) was charged. Next, 0.002 mmol in terms of zirconium atoms of the decane slurry of the prepolymerization catalyst component of Synthesis Example 3 previously prepared was charged. 16.25 NmL of hydrogen was charged. Next, the previously prepared mixed solution was continuously charged into the polymerization vessel at a constant rate over 2 hours. The mixed solution consisted of 234 mL of 4-methyl-1-pentene and 18.5 mL of a C16 / C18 α-olefin mixture (trade name: "Linearene 168", manufactured by Idemitsu Kosan Co., Ltd.). The start of this charging was regarded as the polymerization start time, and the temperature was kept at 45°C for 4.5 hours. 1 hour and 2 hours after the polymerization start time, 16.25 NmL of hydrogen was charged, respectively. After 4.5 hours had passed from the polymerization start time, the temperature was lowered to room temperature, the pressure was released, and the polymerization liquid containing a white solid was immediately filtered to obtain a solid substance. This solid substance was dried under reduced pressure at 80°C for 8 hours to obtain a 4-methyl-1-pentene polymer (A-2). The yield of the 4-methyl-1-pentene polymer (A-2) was 124 g. The 4-methyl-1-pentene content in the 4-methyl-1-pentene polymer (A-2) was 97.5 mol%, and the α-olefin (1-hexadecene, 1-octadecene) content was 2.5 mol%.
[0126] [2.3] 4-Methyl-1-pentene polymer (A-3) The inside of a 1.5L stainless steel polymerization vessel equipped with an agitator was fully replaced with nitrogen. 500mL of 4-methyl-1-pentene and 220mL of heptane were charged into the polymerization vessel at 23°C. 30mL of 1-decene and 0.3mL of a 1.0mmol / mL toluene solution of triisobutylaluminum (TIBAL) were charged into the autoclave in succession, and stirring was started. Next, 140mL of hydrogen was charged, and the autoclave was heated to an internal temperature of 60°C. 2mL of a toluene solution prepared in advance was pressed into the autoclave with nitrogen, and polymerization was started. The toluene solution contained 0.039 mmol of methylaluminoxane and 0.00013 mmol of (8-octamethylfluoren-12'-yl-(2-(adamantan-1-yl)-8-methyl-3,3b,4,5,6,7,7a,8-octahydrocyclopenta[a]indene))zirconium dichloride in terms of Al. During the polymerization reaction, the temperature inside the autoclave was adjusted to 60°C. 10 minutes after the start of polymerization, 5 mL of methanol was injected into the autoclave with nitrogen to terminate the polymerization, and the autoclave was depressurized to atmospheric pressure. The reaction solution was poured into acetone while stirring to precipitate a polymer. The obtained polymer containing the solvent was dried at 130°C under reduced pressure for 10 hours. As a result, a 4-methyl-1-pentene polymer (A-3) was obtained. The yield of the obtained 4-methyl-1-pentene polymer (A-3) was 66.5 g. The 4-methyl-1-pentene content in the 4-methyl-1-pentene polymer (A-3) was 94.1 mol %, and the α-olefin (1-decene content) was 5.9 mol %.
[0127] [2.4] 4-Methyl-1-pentene polymer (A-4) The inside of a 1.5L stainless steel polymerization vessel equipped with an agitator was thoroughly replaced with nitrogen. 500mL of 4-methyl-1-pentene and 230mL of heptane were charged into the polymerization vessel at 23°C. 15mL of 1-decene and 0.3mL of a 1.0mmol / mL toluene solution of triisobutylaluminum (TIBAL) were charged into the autoclave in succession, and stirring was started. Next, 140mL of hydrogen was charged, and the autoclave was heated to an internal temperature of 60°C. 2mL of a toluene solution prepared in advance was pressed into the autoclave with nitrogen, and polymerization was started. The toluene solution contained 0.06 mmol of methylaluminoxane and 0.0002 mmol of (8-octamethylfluoren-12'-yl-(2-(adamantan-1-yl)-8-methyl-3,3b,4,5,6,7,7a,8-octahydrocyclopenta[a]indene))zirconium dichloride in terms of Al. During the polymerization reaction, the temperature inside the autoclave was adjusted to 60°C. 30 minutes after the start of polymerization, 5 mL of methanol was injected into the autoclave with nitrogen to terminate the polymerization, and the autoclave was depressurized to atmospheric pressure. The reaction solution was poured into acetone while stirring to precipitate the polymer. The obtained polymer containing the solvent was dried at 130°C under reduced pressure for 10 hours. As a result, 4-methyl-1-pentene polymer (A-4) was obtained. The yield of the obtained 4-methyl-1-pentene polymer (A-4) was 35.6 g. The 4-methyl-1-pentene content in the 4-methyl-1-pentene polymer (A-4) was 96.7 mol %, and the α-olefin (1-decene content) was 3.3 mol %.
[0128] [2.5] 4-Methyl-1-pentene polymer (A-5) A 4-methyl-1-pentene polymer (A-5) was obtained according to a known method (i.e., the polymerization method described in Comparative Example 9 of WO 2006 / 054613). The 4-methyl-1-pentene content in the 4-methyl-1-pentene polymer (A-5) was 97.2 mol%, and the α-olefins (1-hexadecene and 1-octadecene) were 2.8 mol%.
[0129] [2.6] 4-Methyl-1-pentene polymer (A-6) A 4-methyl-1-pentene polymer (A-6) was obtained by a method similar to a known method (i.e., the polymerization method described in Comparative Example 7 or Comparative Example 9 of WO 2006 / 054613). The 4-methyl-1-pentene content in the 4-methyl-1-pentene polymer (A-6) was 100 mol%.
[0130] [2.7] Resin other than 4-methyl-1-pentene polymer (A) (B-1) As the resin (B-1), PET (polyethylene terephthalate, manufactured by Mitsui Chemicals, Inc., Mitsui PET, IV: 0.62) was prepared. The 4-methyl-1-pentene content in the resin (B-1) was 0 mol%.
[0131] [2.8] Resin other than 4-methyl-1-pentene polymer (A) (B-2) As the resin (B-2), PP (polypropylene, manufactured by ExxonMobil, Achieve6936G2, weight average molecular weight: 55,000) was prepared. The 4-methyl-1-pentene content in the resin (B-2) was 0 mol%.
[0132] [2.9] Resins other than 4-methyl-1-pentene polymers (A) (B-3) As resin (B-3), a 5% aqueous solution of polyvinyl alcohol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., polymerization degree: about 1500) was prepared. The 4-methyl-1-pentene content in resin (B-3) was 0 mol%.
[0133] [3] Examples and Comparative Examples [3.1] Example 1 The 4-methyl-1-pentene polymer (A-1) was dissolved in a mixed solvent (SP value: 8.7) at 27°C to prepare an electrospinning composition. The mixed solvent consisted of 70 volume % of methylcyclohexane and 30 volume % of N,N-dimethylformamide. The content of the 4-methyl-1-pentene polymer (A-1) was 10 mass % based on the total mass of the electrospinning composition. Immediately after preparing the electrospinning composition, it was spun using the production apparatus shown in FIG. 1 to obtain a fiber with a basis weight of 0.10 g / m 2The nonwoven fabric was produced under the following electrospinning conditions so that the results are shown in Table 2.
[0134] [3.1.1] Electrospinning conditions -Ejector: Needle (22G) Distance from needle to target electrode: 13cm ·Discharge rate: 0.5mg / min Applied voltage: 12kV
[0135] [3.2] Examples 3, 5, and 7, and Comparative Examples 1, 3, and 5 A nonwoven fabric was obtained in the same manner as in Example 1, except that the temperature of the solvent when mixing the 4-methyl-1-pentene polymer (A), the solvent, and the resin, and the discharge speed were changed as shown in Table 1. The results are shown in Tables 2 and 3. In Examples 3, 5, and 7, and Comparative Example 1, the same mixed solvent was used.
[0136] [3.3] Comparative Example 7 A resin (B-1) other than the 4-methyl-1-pentene polymer (A) was dissolved in formic acid (SP value: 13.5) at 27° C. to prepare an electrospinning composition. The content of the resin (B-1) was 10% by mass based on the total mass of the electrospinning composition. Except for using the resin (B-1) instead of the 4-methyl-1-pentene polymer (A-1), a nonwoven fabric was produced in the same manner as in Example 1. The results are shown in Table 3.
[0137] [3.4] Comparative Example 9 A nonwoven fabric was obtained in the same manner as in Example 1, except that a resin (B-2) other than the 4-methyl-1-pentene polymer (A) was used instead of preparing a composition for electrospinning, and the heating temperature for spinning was changed to 270° C. The results are shown in Table 3.
[0138] [3.5] Comparative Example 11 The resin (B-3) other than the 4-methyl-1-pentene polymer (A) was dissolved in ion-exchanged water to obtain an aqueous polyvinyl alcohol solution (resin concentration: 10 mass %). Immediately after preparing the aqueous polyvinyl alcohol solution, the fibers were spun under the following conditions using the manufacturing apparatus shown in FIG. 1. The fibers were accumulated on a stainless steel drum and the weight per unit area was adjusted to 0.1 g / m. 2 The results are shown in Table 3.
[0139] [3.5.1] Electrospinning conditions Electrode: Metal nozzle (inner diameter: 0.41 mm, tip is spinning solution outlet) and stainless steel drum (collection of spun fibers) ·Discharge amount: 1g / h Applied voltage: 23.4kV
[0140] [3.6] Examples 2, 4, 6, and 8, and Comparative Examples 2, 4, 6, 8, 10, and 12 Except for changing the timing of spinning from "immediately after the electrospinning composition was prepared" to "24 hours after the electrospinning composition was prepared," nonwoven fabrics were produced in the same manner as in Examples 1, 3, 5, and 7 and Comparative Examples 1, 3, 5, 7, 9, and 11. The results are shown in Tables 2 and 3.
[0141] [Table 1]
[0142] [Table 2] [Table 3]
[0143] In Tables 2 and 3, "MCH" refers to methylcyclohexane, and "DMF" refers to N,N-dimethylformamide.
[0144] In Comparative Examples 1 to 6, the standard deviation of the average fiber diameter of the multiple fibers was not 0.25 μm or less. Furthermore, the endothermic end temperature (TmE) of the multiple fibers was not 230° C. or less. Therefore, the Q value (basicity) was 2.8×10 -3It was not more than that. The Q value (acidity) was 2.8 x 10 -3 That was not all. The nonwoven fabrics of Comparative Examples 7 and 8 did not contain fibers containing a 4-methyl-1-pentene polymer (A). Furthermore, the endothermic end temperature (TmE) of the multiple fibers was not 230° C. or lower. Therefore, the Q value (basicity) was 2.8×10 -3 That was not all. The nonwoven fabrics of Comparative Examples 9 and 10 did not contain fibers containing 4-methyl-1-pentene polymer (A). The standard deviation of the average fiber diameter of a plurality of fibers was not 0.25 μm or less. Therefore, the Q value (basicity) was 2.8×10 -3 It was not more than that. The Q value (acidity) was 2.8 x 10 -3 That was not all. The nonwoven fabrics of Comparative Examples 11 and 12 did not contain fibers containing a 4-methyl-1-pentene polymer (A). The nonwoven fabrics of Comparative Examples 11 and 12 were dissolved in a basic aqueous solution and an acidic aqueous solution when evaluating the Q value (basic) and the Q value (acidic). Therefore, the Q value (basic) and the Q value (acidic) could not be evaluated. From the above, it was found that the nonwoven fabrics of Comparative Examples 1 to 12 are not nonwoven fabrics capable of maintaining high filtration performance in acidic and basic solutions.
[0145] The nonwoven fabrics of Examples 1 to 8 were made of a plurality of fibers containing a 4-methyl-1-pentene polymer (A). The standard deviation of the average fiber diameter of the plurality of fibers was 0.25 μm or less. The endothermic end temperature (TmE) of the plurality of fibers was 230° C. or less. Therefore, the Q value (basicity) was 2.8×10 -3 The Q value (acidity) was 2.8×10 -3 That was all. From the above, it was found that the nonwoven fabrics of Examples 1 to 8 were capable of maintaining high filtration performance in acidic and basic solutions.
[0146] Furthermore, as is clear from the comparison between Example 1 and Example 2, between Example 3 and Example 4, between Example 5 and Example 6, and between Example 7 and Example 8, there was no significant difference in the average fiber diameter, standard deviation of the average fiber diameter, CV value, and number of polymer spheres between the two. This indicates that in Examples 2, 4, 6, and 8, even if the electrospinning composition was left to stand for a long time, no insoluble components were precipitated in the electrospinning composition, and the electrospinning composition was spun by the electrospinning method as in Examples 1, 3, 5, and 7. From these results, it was found that the electrospinning compositions of Examples 1 to 8 have excellent pot life. [Explanation of symbols]
[0147] 100 Electrospinning device 101 Discharge device 102 target electrode 103 Voltage application device 104 Textiles 105 Nonwoven fabric
Claims
1. The fiber material comprises a plurality of fibers each containing a 4-methyl-1-pentene polymer (A), The standard deviation of the average fiber diameter of the plurality of fibers is 0.25 μm or less; The nonwoven fabric, wherein the plurality of fibers satisfy the following requirement (I): Requirement (I): The endothermic end temperature (TmE) in the melting curve measured by differential scanning calorimetry is 230°C or lower.
2. 2. The nonwoven fabric according to claim 1, wherein the standard deviation of the average fiber diameter of the plurality of fibers is 0.22 μm or less.
3. 3. The nonwoven fabric according to claim 1, wherein the plurality of fibers have an average fiber diameter of 0.45 μm or less.
4. 3. The nonwoven fabric according to claim 1, wherein a content of the 4-methyl-1-pentene polymer (A) relative to the total amount of the plurality of fibers is 90 mass % or more.
5. 3. The nonwoven fabric according to claim 1 or 2, wherein the plurality of fibers further satisfy the following requirement (II): Requirement (II): The difference ΔT (TmE-Tm) between the endothermic temperature (TmE) in the melting curve measured by differential scanning calorimetry and the melting point (Tm) measured by differential scanning calorimetry is 10°C to 30°C.
6. The nonwoven fabric according to claim 1 or 2, wherein the 4-methyl-1-pentene polymer (A) satisfies the following requirement (i): Requirement (i): Contains a structural unit (P) derived from 4-methyl-1-pentene and at least one structural unit (AQ) derived from a linear α-olefin having 6 to 20 carbon atoms (excluding 4-methyl-1-pentene).
7. The nonwoven fabric according to claim 6, wherein the 4-methyl-1-pentene polymer (A) satisfies the following requirement (ii): Requirement (ii): the amount (U1) of the structural unit (P) is 84.0 mol% to 95 mol%, and the total amount (U2) of the at least one structural unit (AQ) is 16.0 mol% to 5 mol%, relative to the total of the amount (U1) of the structural unit (P) and the total amount (U2) of the at least one structural unit (AQ), which is 100 mol%.
8. The nonwoven fabric according to claim 7, wherein the at least one type of constitutional unit (AQ) comprises at least two types of the constitutional unit (AQ).
9. The nonwoven fabric according to claim 1 or claim 2, wherein the intrinsic viscosity [η] of the plurality of fibers at 135° C. is 1.7 dl / g to 5.5 dl / g.
10. The number of polymer spheres observed on the surface was 2.0 / mm 2 3. The nonwoven fabric according to claim 1 or claim 2, wherein:
11. The method includes spinning the electrospinning composition by an electrospinning method, The method for producing a nonwoven fabric, wherein the electrospinning composition contains a 4-methyl-1-pentene polymer (A) that satisfies the following requirement (I) and a solvent having a Hildebrand solubility parameter of 8.0 or more: Requirement (I): The endothermic end temperature (TmE) in the melting curve measured by differential scanning calorimetry is 230°C or lower.
12. The method for producing a nonwoven fabric according to claim 11, wherein the solvent has a Hildebrand solubility parameter of 8.3 or more.
13. The solvent is a poor solvent having a Hildebrand solubility parameter of 8.0 or more; a good solvent having a Hildebrand solubility parameter of less than 8.0; Including, a ratio of the poor solvent to the total amount of the good solvent and the poor solvent is 5% by volume to 45% by volume; The method for producing a nonwoven fabric according to claim 11 or 12, wherein a ratio of the good solvent to a total amount of the good solvent and the poor solvent is 55 vol% to 95 vol%.
Citation Information
Patent Citations
Cosmetic sheet
JP2008179629A
Spinned nanofibers, medical devices and methods
JP2009523196A
Nonwoven fabric, method for manufacturing same, and composition for electrospinning
WO2020013199A1