Method of manufacturing building materials and building materials

By applying a coating layer and a functional film layer with an adhesive on building materials, the method addresses adhesion issues, ensuring long-term durability and appearance in outdoor environments.

JP2024146382AInactive Publication Date: 2024-10-15DAI NIPPON TORYO CO LTD

Patent Information

Application Number
JP2023059245
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for attaching decorative films to inorganic building materials face issues with adhesion, particularly in outdoor environments, where films may peel off due to uneven surfaces and harsh conditions, leading to durability and appearance problems.

Method used

A method involving the application of at least one coating layer on a base material followed by a functional film layer via an adhesive layer, which enhances adhesion and durability, using resins like acrylic and acrylic silicone for improved bonding.

Benefits of technology

The method ensures long-term maintenance of the functional film's appearance and adhesion, even in outdoor conditions, by providing a uniform film that adheres well to uneven surfaces and withstands environmental stress.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146382000001_ABST
    Figure 2024146382000001_ABST
Patent Text Reader

Abstract

To provide building materials that can maintain appearance, durability and adhesion of functional film layers for a long period of time even in outdoor environments.SOLUTION: A method for manufacturing building materials, comprising the steps of providing at least one coating layer 2 on a base material 1, and providing a functional film layer 3 on at least the one coating layer 2 via an adhesive layer 5, and one surface of the functional film layer 3 is provided with the adhesive layer 5.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a manufacturing method for a building material and a building material, and more particularly to a manufacturing method for a building material that can maintain its appearance, durability, and adhesion of a functional film layer over a long period of time even in an outdoor environment. [Background technology]

[0002] Currently, the most common method for protecting and decorating building materials is to paint them, forming a protective or decorative layer, but as another method for protecting and decorating, a technique for attaching a film to the object has also been proposed.

[0003] Japanese Patent Laid-Open Publication No. 2002-234077 (Patent Document 1) describes a coating film laminated inorganic building material obtained by bonding a coating film to the surface of an inorganic building material by heat and / or pressure. Patent Document 1 describes that inorganic building materials generally used have a porous structure and are subjected to various processes, so that it is difficult to form a uniform coating film when painted with paint, and there are problems such as cracking and peeling of the coating film itself, but that the problems caused by painting with paint can be solved by using a technique in which a coating film is bonded to the surface of an inorganic building material by heat and / or pressure. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2002-234077 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the method of directly attaching a decorative film to the surface of an inorganic building material as described in Patent Document 1, there is a problem that the adhesive strength to the substrate cannot be sufficiently guaranteed. Usually, inorganic substrates with hollow walls are often used for building materials for heat insulation and fire resistance. In addition, the substrate surface may have an uneven shape to improve the design of the substrate itself. In the case of painting with paint, the paint is impregnated into the hollow walls, so although there are problems such as cracking and peeling over time, problems such as full peeling are unlikely to occur. On the other hand, since the decorative film has difficulty following the hollow walls and uneven shape of the substrate, problems such as full peeling of the decorative film from the substrate may occur in parts where the film does not follow sufficiently or under harsh conditions such as outdoor environments. Furthermore, such inorganic building materials may contain fragile parts, and there was a problem that the decorative film is easily peeled off at the joint between the fragile substrate and the decorative film.

[0006] Therefore, an object of the present invention is to provide a building material that can maintain its appearance, durability, and adhesion of a functional film layer for a long period of time even in an outdoor environment. [Means for solving the problem]

[0007] As a result of intensive research to achieve the above-mentioned object, the inventors have discovered that by first providing at least one coating layer on a substrate and then applying a functional film layer via an adhesive layer, it is possible to provide a building material that can maintain the appearance, durability, and adhesion of the functional film layer for a long period of time even in outdoor environments, and have thus completed the present invention.

[0008] Therefore, the manufacturing method for building materials of the present invention includes a step of providing at least one coating layer on a substrate, and a step of providing a functional film layer on the at least one coating layer via an adhesive layer, and the adhesive layer is provided on one surface of the functional film layer.

[0009] In a preferred embodiment of the method for producing a building material of the present invention, the functional film layer includes at least one layer selected from the group consisting of a protective layer and a decorative layer.

[0010] In another preferred embodiment of the method for producing a building material of the present invention, the method further comprises the step of providing at least one coating layer on the functional film layer.

[0011] The building material of the present invention is a building material comprising a substrate, at least one coating layer disposed on the substrate, and a functional film layer disposed on the at least one coating layer, and an adhesive layer is present between the at least one coating layer and the functional film layer. Effect of the Invention

[0012] According to the present invention, it is possible to provide a building material that can maintain its appearance, durability, and adhesion of a functional film layer for a long period of time even in an outdoor environment. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a schematic diagram showing one embodiment of a building material of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The present invention relates to a method for producing a building material and a building material.

[0015] In the present invention, the building materials are materials used in construction, and specific examples thereof preferably include wood building materials such as veneer, plywood, particle board, and medium density fiberboard (MDF); ceramic building materials such as ceramic siding board, flexible board, calcium silicate board, gypsum slag barite board, wood chip cement board, pulp cement board, precast concrete board, lightweight aerated concrete (ALC) board or ALC panel, and gypsum board; various building materials (particularly building boards) such as metal building materials such as metal siding board, aluminum, iron, and stainless steel. Specific examples of building materials also include PVC sheets, tarpaulins, plastic cardboard, plastic substrates such as acrylic boards, tiles, and glass plates.

[0016] In the present invention, the building material includes at least a substrate. In this specification, the substrate means an object to which the coating layer and the functional film layer are applied.

[0017] Examples of the substrate include metal substrates such as iron, stainless steel, aluminum, copper, titanium, and alloys thereof, inorganic substrates other than metals such as cement, concrete, gypsum, calcium silicate, calcium carbonate, marble, artificial marble, glass, and ceramics, wood substrates, epoxy resins, ABS resins, polycarbonates, polyvinyl chloride, polystyrene, acrylic resins, particularly plastic substrates such as polymethyl methacrylate (PMMA), polyethylene terephthalate (PET), and polypropylene (PP), as well as composite substrates combining two or more of these substrates. Among these, the effects of the present invention are more pronounced in substrates including porous or fragile portions on the surface of inorganic substrates such as cement, concrete, gypsum, calcium silicate, calcium carbonate, marble, artificial marble, and ceramics, and wood substrates.

[0018] In the present invention, the building materials and substrates are available in various shapes, for example, two-dimensional substrates such as films, sheets, and plates, and three-dimensional substrates that are complex three-dimensional objects, etc. The surfaces of the building materials and substrates may be smooth or may have irregularities.

[0019] First, the method for producing a building material of the present invention will be described. The method for producing a building material of the present invention is a method for producing a building material comprising the following two steps. The first step is to provide at least one coating layer on a substrate. The second step is to provide a functional film layer on at least one coating layer via an adhesive layer.

[0020] In the manufacturing method of the building material of the present invention, by providing at least one coating layer on the substrate before providing the functional film layer, the adhesion with the adhesive layer is improved, and thus peeling of the functional film layer from the substrate can be prevented. Furthermore, by providing at least one coating layer on the substrate beforehand, if there is a fragile part on the surface of the substrate, this can be reinforced, and peeling of the functional film layer due to the presence of the fragile part can be prevented. This allows the adhesion of the functional film layer to the substrate to be maintained for a long period of time even in an outdoor environment.

[0021] In the present invention, the coating layer means a coating layer formed by painting, among layers disposed on a substrate.

[0022] In the first step, the coating layer provided on the substrate may be a single layer or may be two or more layers.

[0023] In the first step, the coating layer provided on the substrate preferably has a thickness of 120 μm or less, more preferably 5 to 80 μm. When the coating layer is made up of multiple layers, the numerical range described here refers to the total thickness of the coating layers.

[0024] In the first step, the coating layer is obtained by applying a paint to the substrate by a known coating means, such as brush coating, roller coating, trowel coating, spatula coating, roll coater coating, flow coater coating, spray coating (e.g., air spray coating, airless spray coating), shower coater coating, dipping coating, etc.

[0025] In the first step, the means for drying the coating layer is not particularly limited, and may be either natural drying at ambient temperature or forced drying using a dryer or the like.

[0026] In the first step, the coating layer provided on the substrate usually contains a resin. The amount of resin in the coating layer is preferably 10 to 100% by mass, more preferably 20 to 95% by mass. When the coating layer is composed of multiple layers, the numerical range described here refers to the amount of resin in each coating layer.

[0027] In the first step, the coating layer provided on the substrate may be made of a resin that is commonly used in the paint industry. Examples include acrylic resin, silicone resin, acrylic silicone resin, styrene-acrylic copolymer resin, polyester resin, fluororesin, rosin resin, petroleum resin, coumarone resin, phenolic resin, urethane resin, melamine resin, urea resin, epoxy resin, cellulose resin, xylene resin, alkyd resin, aliphatic hydrocarbon resin, butyral resin, maleic acid resin, fumaric acid resin, vinyl resin, amine resin, ketimine resin, etc. The resin may be used alone or in combination of two or more kinds.

[0028] In the first step, the coating layer provided on the substrate preferably contains an acrylic resin or an acrylic silicone resin. By using an acrylic resin or an acrylic silicone resin in the coating layer provided between the substrate and the functional film layer, the adhesion of the functional film layer to the substrate can be further improved.

[0029] In the first step, the coating layer provided on the substrate may contain other components, such as pigments, dispersants, antioxidants, anti-settling agents, antifoaming agents, silane coupling agents, adhesion imparting agents, anti-algae agents, anti-fungal agents, preservatives, insecticides, antibacterial agents, antiviral agents, ultraviolet absorbers, radical scavengers, antistatic agents, conductivity imparting agents, etc., as necessary.

[0030] In the method for producing a building material of the present invention, a functional film layer is provided on at least one coating layer obtained in the first step via an adhesive layer (second step). By using a film, rather than a coating, to impart a function to the building material, the appearance and durability can be maintained for a long period of time even in an outdoor environment. For example, when a coating is used to impart a function to a building material as in the past, a decrease in appearance and physical properties is observed in areas where uneven painting occurs, but when a functional film is used, a uniform film can be placed on the substrate, thereby eliminating such a drawback. In addition, according to the method for producing a building material of the present invention, by providing at least one coating layer on the substrate in advance, the adhesion of the functional film layer to the substrate can be maintained for a long period of time even in an outdoor environment, and therefore an excellent effect can be exhibited in maintaining the appearance and durability of the building material.

[0031] In the present invention, the functional film layer refers to a layer of a film that is disposed on a substrate in order to impart a specific function to the substrate. For example, the functional film layer includes a layer that imparts functions such as design (including imparting gloss) and durability to the substrate.

[0032] In the present invention, the film layer means a layer that is already formed into a film shape when placed on a substrate, and is distinguished from a coating layer that is formed by painting when placed on a substrate.

[0033] The functional film layer may be a film formed by molding a resin (molded film), a coating film formed by painting a paint (painted film), a film formed by printing an ink (printed film), or a composite film formed by combining at least two of the molded film, the painted film, and the printed film. The functional film layer may be a film consisting of one layer (single layer film), or a film consisting of multiple layers (laminated film).

[0034] As the molding method, coating method and printing method that can be used for producing the film, conventionally known molding methods, coating methods and printing methods can be used. For example, when using a film composed only of a coating film or a film composed only of a printed film, a coating film (single layer or laminate) or a printed film (single layer or laminate) is formed on a support such as polypropylene, and the coating film or the printed film is peeled off from the support to obtain a coated film.

[0035] Examples of molding methods that can be used to produce the film include injection molding, blow molding, extrusion molding, vacuum molding, and pressure molding.

[0036] Examples of coating methods that can be used in producing the film include dipping and coating methods using a coater such as a bar coater, die coater, roll coater, comma coater, knife coater, or gravure coater.

[0037] Examples of printing methods that can be used in producing the film include inkjet (IJ) printing, gravure printing, flexographic printing, and design spray printing.

[0038] The functional film layer preferably has a thickness of 250 μm or less, more preferably 30 to 180 μm. If the functional film layer is too thick, the pattern of the substrate may not be recognized from above the functional film layer. In addition, for example, when the functional film layer is provided on a substrate having an uneven shape, it is preferable that the functional film layer is not too thick from the viewpoint of providing the functional film in a state following the unevenness of the substrate. In the case where the functional film layer is made of a plurality of layers, the numerical range of thickness described here refers to the total thickness of the functional film layer. In addition, it is preferable that the thickness of the functional film layer (the total thickness in the case of a plurality of layers) is the same as the thickness of the coating layer provided by the first step (the total thickness in the case of a plurality of layers) or is thicker than the thickness of the coating layer provided by the first step (the total thickness in the case of a plurality of layers).

[0039] The functional film layer may be colored or transparent.

[0040] The functional film layer usually contains a resin. The amount of the resin in the functional film layer is preferably 10 to 100% by mass, more preferably 20 to 95% by mass. When the functional film layer is composed of a plurality of layers, the numerical range described here refers to the amount of the resin in each functional film layer.

[0041] Examples of resins that can be used in the functional film layer include acrylic resins, silicone resins, acrylic silicone resins, styrene-acrylic copolymer resins, polyester resins, fluororesins, rosin resins, petroleum resins, coumarone resins, phenolic resins, urethane resins, melamine resins, urea resins, epoxy resins, cellulose resins, xylene resins, alkyd resins, aliphatic hydrocarbon resins, butyral resins, maleic acid resins, fumaric acid resins, vinyl resins, amine resins, ketimine resins, etc. The resins may be used alone or in combination of two or more.

[0042] The functional film layer preferably contains an acrylic resin or an acrylic silicone resin. This can improve the durability of the building material, and when the coating layer or the adhesive layer contains an acrylic resin or an acrylic silicone resin, the adhesion of the functional film layer can be further improved. When the functional film layer is composed of multiple layers, it is preferable that at least the layer facing the adhesive layer contains an acrylic resin or an acrylic silicone resin, and it is more preferable that all of the layers contain an acrylic resin or an acrylic silicone resin.

[0043] The functional film layer may contain other components, such as pigments, dispersants, antioxidants, anti-settling agents, defoamers, silane coupling agents, adhesion imparting agents, anti-algae agents, anti-fungal agents, preservatives, insecticides, antibacterial agents, antiviral agents, ultraviolet absorbers, radical scavengers, antistatic agents, and conductivity imparting agents, as necessary.

[0044] The functional film layer preferably includes at least one layer selected from the group consisting of a protective layer and a decorative layer.

[0045] In the present invention, the protective layer is a layer for protecting the surface of the base material of the building material. When the functional film layer includes the protective layer, the durability of the building material can be improved. In addition, in the present invention, the decorative layer means a layer intended to provide a design to the base material or to impart a texture different from that of the base material. Here, the design refers to a shape, a pattern, a color, or a combination of these.

[0046] In addition, an adhesive layer is provided on one surface of the functional film layer. According to the present invention, the functional film layer is attached to the substrate (particularly the coating layer present on the substrate) via the adhesive layer. Therefore, in the second step, the functional film layer is disposed on the coating layer by attaching the adhesive layer provided on the surface of the functional film layer to the coating layer.

[0047] The adhesive layer is a layer composed of an adhesive. The adhesive layer and the adhesive may be called a pressure-sensitive adhesive layer and a pressure-sensitive adhesive, respectively. Examples of the adhesive include a urethane adhesive, an acrylic adhesive, an epoxy adhesive, and a rubber adhesive, and among these, an acrylic adhesive is preferred.

[0048] In the manufacturing method of the building material of the present invention, from the viewpoint of adhesion of the functional film layer, it is preferable that either one of the coating layer obtained in the first step or the adhesive layer provided on the surface of the functional film layer contains an acrylic resin, and it is even more preferable that both the coating layer and the adhesive layer contain an acrylic resin.

[0049] The thickness of the adhesive layer is preferably 20 to 200 μm.

[0050] The adhesive layer can be formed by applying an adhesive to the surface of the functional film layer. A film-like adhesive layer can also be attached to the functional film layer.

[0051] In the second step, a conventionally known film attachment method can be used to provide a functional film layer on the coating layer formed on the substrate, and preferred methods include vacuum forming, pressure forming, and three-dimensional surface decoration forming.

[0052] The method for producing a building material of the present invention may further include the following steps. The third step is to provide at least one coating layer on the functional film layer.

[0053] In the manufacturing method of the building material of the present invention, by providing a coating layer in addition to the functional film layer, it is possible to impart further functions to the substrate or to reinforce the functions imparted by the functional film layer.

[0054] In the third step, the coating layer provided on the functional film layer may be one layer or two or more layers.

[0055] In the third step, the coating layer provided on the functional film layer preferably has a thickness of 50 μm or less, more preferably 1 to 40 μm. When the coating layer is made up of multiple layers, the numerical range described here refers to the total thickness of the coating layers.

[0056] In the third step, the coating layer is obtained by applying a paint to the substrate by a known coating means, such as brush coating, roller coating, trowel coating, spatula coating, roll coater coating, flow coater coating, spray coating (e.g., air spray coating, airless spray coating), shower coater coating, dipping coating, etc.

[0057] In the third step, the means for drying the coating layer is not particularly limited, and may be either natural drying at ambient temperature or forced drying using a dryer or the like.

[0058] In the third step, the coating layer provided on the functional film layer may be colored or transparent.

[0059] In the third step, the coating layer provided on the functional film layer may not contain a resin, such as a photocatalyst or hydrophilic layer, but may contain a resin. When the coating layer contains a resin, the amount of the resin in the coating layer is preferably 10 to 100% by mass, more preferably 20 to 95% by mass. When the coating layer is composed of multiple layers, the numerical range described here refers to the amount of resin in each coating layer.

[0060] In the third step, the coating layer provided on the functional film layer can be made of resins commonly used in the paint industry. Examples include acrylic resins, silicone resins, acrylic silicone resins, styrene-acrylic copolymer resins, polyester resins, fluororesins, rosin resins, petroleum resins, coumarone resins, phenolic resins, urethane resins, melamine resins, urea resins, epoxy resins, cellulose resins, xylene resins, alkyd resins, aliphatic hydrocarbon resins, butyral resins, maleic acid resins, fumaric acid resins, vinyl resins, amine resins, and ketimine resins. The resins may be used alone or in combination of two or more.

[0061] In the third step, the coating layer provided on the functional film layer preferably contains an acrylic resin or an acrylic silicone resin. By the coating layer provided on the functional film layer containing an acrylic resin or an acrylic silicone resin, the durability of the building material is improved, and by the other layers also containing an acrylic resin or an acrylic silicone resin, the adhesion with the functional film layer is improved.

[0062] In the third step, the coating layer provided on the functional film layer may contain other components, such as pigments, dispersants, antioxidants, anti-settling agents, defoamers, silane coupling agents, adhesion promoters, anti-algae agents, anti-fungal agents, preservatives, insecticides, antibacterial agents, antiviral agents, UV absorbers, radical scavengers, antistatic agents, conductivity promoters, etc., as necessary.

[0063] In the third step, the coating layer provided on the functional film layer preferably includes at least one layer selected from the group consisting of a protective layer and a decorative layer. By forming a protective layer, the durability of the building material can be further improved, and by fixing the decorative layer by inkjet printing, building materials with various designs can be provided.

[0064] Next, the building material of the present invention will be described.

[0065] The building material of the present invention is a building material comprising a substrate, at least one coating layer disposed on the substrate, and a functional film layer disposed on the at least one coating layer, with an adhesive layer present between the at least one coating layer and the functional film layer. The building material, substrate, coating layer, functional film layer, and adhesive layer in the building material of the present invention are as described in the description of the manufacturing method for the building material of the present invention.

[0066] The building material of the present invention may further include at least one coating layer disposed on the functional film layer. The coating layer disposed on the functional film layer is also as described in the description of the manufacturing method of the building material of the present invention.

[0067] The building material of the present invention can be produced by the above-mentioned method for producing a building material of the present invention.

[0068] Fig. 1 is a schematic diagram showing one embodiment of the building material of the present invention. The building material shown in Fig. 1 includes a substrate 1, a coating layer 2 disposed on the substrate 1, a functional film layer 3 disposed on the coating layer 2, and a coating layer 4 disposed on the functional film layer 3, with an adhesive layer 5 present between the coating layer 2 and the functional film layer 3. EXAMPLES

[0069] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.

[0070] <Paint preparation> The following paints were prepared based on each water-based resin emulsion. The resin ratios in each paint are shown in the "Resin Composition" in Tables 1 to 3. The values ​​shown in the "Resin Composition" in Tables 1 to 3 are based on mass. (Paint No. for coating layer (2)) 1. Water-based paint based on acrylic resin emulsion 2. Water-based paint based on acrylic silicone resin emulsion 3. Water-based paint made by mixing acrylic resin emulsion and acrylic silicone resin emulsion at a ratio of 50:50 (mass ratio) 4.Water-based paint based on epoxy resin emulsion 5. Water-based paint based on fluororesin emulsion 6. Water-based paint based on urethane resin emulsion (Paint No. for Functional Film Layer (3)) 1. Water-based paint based on acrylic resin emulsion 2. Water-based paint made by mixing acrylic resin emulsion:acrylic silicone resin emulsion = 50:50 (mass ratio) 3. Water-based paint made by mixing acrylic resin emulsion and urethane resin emulsion in a ratio of 50:50 (mass ratio) 4. Water-based paint based on urethane resin emulsion (Paint No. for coating layer (4)) 1. Water-based paint based on acrylic resin emulsion

[0071] <Adhesive sheet used> The adhesive layer (5) was formed using the following adhesive sheets. The resin compositions of the adhesive sheets are shown in the "Resin Composition" column of Tables 1 to 3. The thickness of each adhesive sheet was 50 μm. (Adhesive sheet No. for adhesive layer (5)) 1. Acrylic resin adhesive sheet HJ-9150W (manufactured by Nitto Denko Corporation) 2. PET resin adhesive sheet FB-ML80 (manufactured by Nitto Denko Corporation)

[0072] Example 1 Building material No. 1 was prepared in the following manner. <Step of Providing Coating Layer (2) on Substrate (1)> A building exterior material (210 mm × 110 mm × 10 mm) having an uneven surface as the substrate (1) was coated with paint No. 1 for the coating layer (2) by air spray to the dry film thickness shown in Table 1, and dried at 130°C for 5 minutes to provide the coating layer (2).

[0073] <Preparation of functional film layer (3)> A polypropylene plate (300 mm x 300 mm x 2 mm) was coated with paint No. 1 for the functional film layer (3) using a bar coater so as to obtain the dry film thickness shown in Table 1, and the coating was dried at 50°C for 5 minutes and at 80°C for 10 minutes to produce a functional film layer (3).

[0074] <Attaching the adhesive layer> The pressure-sensitive adhesive sheet No. 1 for the adhesive layer (5) was attached to the functional film layer (3) to provide the adhesive layer (5) on the surface of the functional film layer (3).

[0075] <Molding> The functional film layer (3) having the adhesive layer (5) on the substrate (1) having the coating layer (2) was subjected to three-dimensional surface decoration molding using a TOM (three-dimensional surface decoration) molding machine (NGF-0709-S, manufactured by Fuse Vacuum) so that the adhesive layer (5) was in contact with the coating layer (2), thereby producing building material No. 1.

[0076] Examples 2 to 10, Examples 12 to 16 Building materials Nos. 2 to 10 and 12 to 16 were produced in the same manner as in Example 1. However, the type and thickness of the paint used to form each layer and the type of adhesive sheet used for the adhesive layer (5) are as shown in Tables 1 to 3.

[0077] Example 11 The building material No. 1 obtained in Example 1 above was coated with paint No. 1 for coating layer (4) by air spray so as to have a dry film thickness shown in Table 1, and dried at 80°C for 10 minutes to provide a coating layer (4), thereby producing building material No. 11.

[0078] Comparative Example 1 A functional film layer (3) provided with an adhesive layer (5) was prepared in the same manner as in Example 1 above, and then the functional film layer (3) provided with the adhesive layer (5) was subjected to three-dimensional surface decoration molding using a TOM molding machine to a building exterior material (210 mm × 110 mm × 10 mm) having an uneven surface as the substrate (1) so that the adhesive layer (5) was in contact with the building exterior material, thereby producing building material No. 17.

[0079] Comparative Example 2 As in Example 1, a building exterior material (210 mm × 110 mm × 10 mm) having an uneven surface as a substrate (1) was coated with paint No. 1 for coating layer (2) by air spray to a dry film thickness shown in Table 3, and dried at 130°C for 5 minutes to provide a coating layer (2), thereby producing building material No. 18.

[0080] Comparative Example 3 A coating layer (2) was provided on a building exterior material (210 mm x 110 mm x 10 mm) having an uneven surface as a substrate (1) in the same manner as in Example 1. Next, a functional film layer (3) was produced, and then the functional film layer (3) was three-dimensionally surface-decorated on the coating layer (2) of the substrate (1) provided with the coating layer (2) using a TOM molding machine, to produce building material No. 19.

[0081] The obtained building materials Nos. 1 to 19 were evaluated according to the following methods. <Evaluation method> <Formability of functional film layer> During and after the three-dimensional surface decoration molding, the condition of the building material was visually observed, and the moldability of the functional film layer was evaluated according to the following criteria. The results are shown in Tables 1 to 3. (Evaluation Criteria) ◯: The functional film layer (3) was molded to conform to the irregularities of the substrate (1) without being torn. △: The functional film layer (3) is molded to conform to the irregularities of the substrate (1) without tearing, but there are some areas where the thickness of the functional film layer (3) covering the protrusions of the substrate (1) is thin. ×: The functional film layer (3) was not molded to conform to the irregularities of the substrate (1).

[0082] <Appearance of building materials> The appearance of the building materials was visually observed and evaluated according to the following criteria. The results are shown in Tables 1 to 3. (Evaluation Criteria) ◯: There is no lifting of the functional film layer (3) from the substrate (1), no pinch marks or blister marks on the functional film layer (3). In addition, the functional film layer (3) is embedded in the unevenness of the substrate (1), and the pattern on the surface of the substrate (1) can be clearly recognized from the appearance of the building material. △: There is no lifting of the functional film layer (3) from the substrate (1), no pinch marks or blister marks on the functional film layer (3), and the functional film layer (3) has penetrated into the unevenness of the substrate (1), but the pattern on the surface of the substrate (1) is thin and cannot be recognized from the appearance of the building material. Or, there are parts where the thickness of the functional film layer (3) covering the convex parts of the substrate (1) is thin. ×: The functional film layer (3) is lifted from the substrate (1), there are armpit marks or blister marks on the functional film layer (3), or the functional film layer (3) does not penetrate into the unevenness of the substrate (1).

[0083] <Adhesion of functional film layer> Two cuts with a central angle of 30° were made in the building material with a utility knife so that the cuts reached the base material. An adhesive tape (Nichiban Cellotape (registered trademark) LP-24) was applied to the cut surface, and the surface of the building material was observed when the adhesive tape was peeled off, and the adhesion of the functional film layer was evaluated according to the following criteria. The results are shown in Tables 1 to 3. (Evaluation Criteria) ⊚: After the adhesive tape was peeled off, the substrate (1), coating layer (2), adhesive layer (5) and functional film layer (3) were completely adhered. ◯: After the adhesive tape was peeled off, the substrate (1), coating layer (2), adhesive layer (5) and functional film layer (3) were completely adhered, but some lifting was observed. Δ: After the adhesive tape was peeled off, the substrate (1), coating layer (2), adhesive layer (5) and functional film layer (3) were completely adhered, but some lifting and chipping were observed. ×: After the adhesive tape was peeled off, peeling occurred between the coating layer (2) and the adhesive layer (5), or between the adhesive layer (5) and the functional film layer (3).

[0084] <Weather resistance (durability)> A weathering test was conducted on the building materials using a super UV accelerated tester (SUV-W261, manufactured by Iwasaki Electric Co., Ltd.) in which the materials were left for 1000 hours in the following cycle. The appearance of the building materials after the weathering test was visually observed and evaluated. The gloss retention was also measured using a gloss meter ("micro-TRI-gloss", manufactured by BYK). The results are shown in Tables 1 to 3. Building materials with evaluation results of ⊚+, ⊚, ◯, or △ can be said to be building materials that can maintain their appearance, durability, and adhesion of the functional film layer for a long period of time even in outdoor environments. In addition, in Comparative Examples 1 and 3, the evaluation of the building materials at the time of production (formability of the functional film layer, appearance of the building materials, and adhesion of the functional film layer) was poor, so weather resistance (durability) was not evaluated. (Test conditions) Irradiation wavelength range: 295-450nm, UV intensity on sample surface: 100mW / cm2±5% During irradiation: Humidity 50% RH Black panel temperature 63℃±2℃ 95% RH or more when condensing Black panel temperature 40℃±2℃ Test conditions: 6 hours of irradiation / 2 hours of condensation (Evaluation Criteria) ◎+: 60° gloss retention is 95% or more and no significant changes such as whitening, yellowing or other discoloration, tearing or peeling of any layer were observed in the appearance. ◎: 60° gloss retention is 90% or more and no significant changes such as discoloration (whitening, yellowing, etc.) or tearing or peeling of any layer were observed in the appearance. ◯: 60° gloss retention was 85% or more and no significant changes in appearance such as discoloration (whitening, yellowing, etc.) or tearing or peeling of any layer were observed. △: 60° gloss retention is 80% or more and no significant changes such as discoloration (whitening, yellowing, etc.) or tearing or peeling of any layer were observed in the appearance. ×: 60° gloss retention rate is less than 80% or significant changes such as discoloration (whitening, yellowing, etc.) or tearing or peeling of layers are observed.

[0085] [Table 1]

[0086] [Table 2]

[0087] [Table 3]

Claims

1. A method for manufacturing a building material, comprising the steps of providing at least one coating layer on a substrate and providing a functional film layer on the at least one coating layer via an adhesive layer, wherein the adhesive layer is provided on one surface of the functional film layer.

2. The method for manufacturing a building material according to claim 1 , wherein the functional film layer includes at least one layer selected from the group consisting of a protective layer and a decorative layer.

3. The method for producing a building material according to claim 1 or 2, further comprising the step of providing at least one coating layer on the functional film layer.

4. A construction material comprising a substrate, at least one coating layer disposed on the substrate, and a functional film layer disposed on the at least one coating layer, wherein an adhesive layer is present between the at least one coating layer and the functional film layer.

Citation Information

Patent Citations

  • Refrigeration cycle

    JP1983148357A

  • Decorative material for facing and manufacture thereof

    JP1992034173A

  • Decorative building material and its manufacture

    JP1998291274A

  • Decorative panel

    JP1999216797A

  • Transfer sheet for molding and method for transfer using the same

    JP2001063290A

Cited By

  • Decorative film for building materials and method for manufacturing decorative film for building materials

    JP2026164494A