Sliding member

The sliding member with a porous sintered metal and resin layer, combined with inclined recesses and balanced graphite/hard particle mix, addresses the issue of seizure in sliding bearings by ensuring continuous lubrication and improved wear resistance.

JP2024146414AInactive Publication Date: 2024-10-15DAIDO METAL IND CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023059288
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing sliding bearings for rotating shafts in gear pumps face challenges in preventing seizure when lubricating oil supply is insufficient, leading to wear and potential burning, as they rely on air layers that fail to function without lubrication.

Method used

A sliding member with a metal layer containing porous sintered metal and a sliding layer impregnated with resin, featuring recesses with inclined inner walls to collect and supply lubricating oil, and a balanced mixture of graphite and hard particles to maintain low friction and wear resistance.

Benefits of technology

The design ensures continuous lubrication even with depleted oil supply, preventing seizure by maintaining an oil film and reducing temperature rise, thus enhancing seizure resistance and wear resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146414000001_ABST
    Figure 2024146414000001_ABST
Patent Text Reader

Abstract

To provide a sliding member having good seizure resistance.SOLUTION: A sliding member includes: a metal layer containing porous sintered metal; and a sliding layer containing a resin material. The sliding layer is a portion where holes of the porous sintered metal are impregnated with the resin material. The sliding layer has a sliding surface and at least one concave part. An internal wall surface of the concave part is a part of the sliding layer. A bottom surface of the concave part is a part of an upper surface of the metal layer. The internal wall surface of the concave part has an inclination less than 90° with respect to the sliding surface.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates generally to a sliding member, and more particularly to a sliding member of a plain bearing. [Background technology]

[0002] Conventionally, in a sliding bearing used for a rotating shaft of a gear pump, etc., it has been an issue to improve the seizure resistance of the sliding surface. For example, Patent Document 1 describes a configuration in which a cylindrical base material that supports a shaft member via an oil film is provided with multiple recesses on the inner peripheral surface, and an air layer is interposed between the base material and the shaft member when the shaft member rotates, thereby reducing the friction of the oil film. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-1053334 A Summary of the Invention [Problem to be solved by the invention]

[0004] In a configuration with a resin layer on the inner peripheral surface of a substrate, such as the sliding bearing of Patent Document 1, if the supply of lubricating oil is insufficient, the resin layer will wear away, exposing the inner peripheral surface of the substrate, which may cause the bearing to seize. In addition, the sliding bearing of Patent Document 1 reduces the friction of the oil film by interposing an air layer between the substrate and the oil film, but this effect is not achieved when the lubricating oil runs out, and there is a similar risk of the bearing seizing.

[0005] SUMMARY OF THE PRESENT EMBODIMENTS An object of the present invention is to provide a sliding bearing which can effectively prevent seizure of the sliding surfaces even when the supply of lubricating oil is insufficient. [Means for solving the problem]

[0006] In order to achieve the above object, the present invention provides a sliding member including a metal layer containing a porous sintered metal and a sliding layer containing a resin material. The sliding layer has a portion in which the resin material is impregnated in the pores of the porous sintered metal. The sliding layer has a sliding surface and at least one recess, an inner wall surface of the recess being a part of the sliding layer, a bottom surface of the recess being a part of the upper surface of the metal layer, and the inner wall surface of the recess being inclined at an angle of less than 90° with respect to the sliding surface.

[0007] Preferably, the sliding layer further contains graphite and hard particles, and the volume ratio of the graphite to the hard particles is 6:1 to 2:1.

[0008] The resin material is made of a fluororesin.

[0009] Preferably, the recess is 1 mm above the sliding surface. 2 More than one is formed per

[0010] Preferably, the inner wall surface of the recess has an inclination of 60° to 86° with respect to the sliding surface.

[0011] Preferably, the diameter of the recess is 0.02 mm to 0.2 mm.

[0012] Preferably, the depth from the bottom surface of the recess to the sliding surface is 5 μm to 30 μm.

[0013] Preferably, the porous sintered metal is a spherical or irregularly shaped metal powder made of one or more of copper, a copper alloy, aluminum, and an aluminum alloy.

[0014] Preferably, the sliding layer further contains a liquid crystal polymer or molybdenum disulfide.

[0015] Preferably, the fluororesin includes one or more of PTFE (polytetrafluoroethylene), PFA (perfluoroalkoxycane), and EFFE (ethylene tetrafluoroethylene copolymer).

[0016] Preferably, the sliding layer contains 5 to 30 volume % graphite and 1 to 15 volume % hard particles.

[0017] Preferably, the graphite is scaly or flaky and has an average particle size of 3 μm to 20 μm.

[0018] Preferably, the hard particles have an average particle size of 0.1 μm to 30 μm.

[0019] Preferably, the hard particles include one or more of iron oxide, boron nitride, Tismo, copper sulfate, magnesium oxide, zinc oxide, and magnesium carbonate, and have a Mohs hardness of 3-6. Effect of the Invention

[0020] In the sliding member of the present invention, the sliding surface and the recessed portion wall surface are made of resin, so that even if the resin wears to a certain extent in an environment where the supply of lubricating oil is insufficient, the metal layer is not exposed and the seizure resistance of the sliding surface can be improved. In addition, since the recessed portion wall surface has an inclination of less than 90° with respect to the sliding surface, the lubricating oil easily flows into the recessed portion while the oil film is formed on the sliding surface, and there is an oil pool effect. When the lubricating oil runs out and the wear of the resin progresses, the lubricating oil pooled in the recessed portion is supplied to the sliding surface, the low friction of the oil film can be maintained, and the seizure resistance of the sliding surface can be improved. Furthermore, the lubricating oil that has entered the recessed portion is replaced sequentially as the sliding member slides, so that the temperature rise in the recessed portion and therefore the temperature rise of the sliding surface can be suppressed, and the softening of the sliding layer containing a large amount of resin material can be prevented.

[0021] The invention and its advantages will be explained in more detail below with reference to the accompanying drawings, which show non-limiting examples for illustrative purposes only, and in which: [Brief description of the drawings]

[0022] [Figure 1] 1 is a schematic cross-sectional view of a sliding member according to an embodiment of the present invention; [Diagram 2] FIG. 4 is a schematic cross-sectional view of another sliding member according to an embodiment of the present invention. [Diagram 3] FIG. 11 is a schematic cross-sectional view of a sliding member according to a conventional example. [Figure 4] In one embodiment of the present invention, a process for forming a sliding layer on a substrate is shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Hereinafter, embodiments of the present invention will be described with reference to the drawings, but the present invention is not limited to these embodiments.

[0024] The structure and manufacturing method of a slide member 1 according to an embodiment of the present invention will be described in detail below.

[0025] (Structure of sliding members) FIG. 1 is a schematic cross-sectional view of a sliding member 1. The sliding member 1 includes a metal layer 10 and a sliding layer 20. In FIG. 1, the upper surface of the sliding member 1 is a sliding surface 30, and a recess 40 is formed in the sliding surface 30. A bottom surface 40a of the recess 40 corresponds to the upper surface of the metal layer 10, and a wall surface 40b of the recess 40 corresponds to the side surface of the sliding layer 20. As shown in FIG. 1, the recess 40 has a shape in which the upper portion is wider than the bottom portion, and the angle α between the wall surface 40b of the recess 40 and the sliding surface 30 is less than 90°. The cross sections of the wall surface 40b and the sliding surface 30 are both shown as straight lines in FIG. 1, but the connecting portion between the wall surface 40b and the sliding surface 30 may have a rounded shape as shown in FIG. 2.

[0026] (Comparison with conventional structure) FIG. 3 is a schematic cross-sectional view of a sliding member 1' according to a conventional example. As shown in FIG. 3, in the sliding member 1' according to the conventional example, a wall surface 40b' of a recess 40' and a sliding surface 30' are formed at a substantially right angle. In such a configuration, lubricating oil does not easily flow from the sliding surface 30' into the recess 40 while the sliding member 1' is sliding, and the recess 40' does not function as an oil reservoir, so that the effect of preventing seizure of the sliding surface cannot be obtained. In view of this point, the present invention sets the angle α between the wall surface 40b and the sliding surface 30 to less than 90° in order to make the recess 40 function as an oil reservoir for the lubricating oil.

[0027] (Characteristics and Effects of the Recesses) The metal layer 10 contains a porous sintered metal. The pores of the porous sintered metal are impregnated with a resin material. The upper surface of the metal layer 10 has a portion that is covered with a sliding layer 20 containing a resin material and a portion that is not covered by the sliding layer 20 and is exposed on the sliding surface. A recess 40 is formed on the sliding surface 30 of the sliding member 1, which contains the resin material impregnated in the porous sintered metal. When the sliding member 1 slides, the lubricating oil is supplied to the sliding surface 30, and an oil film is formed to cover the sliding surface 30. At that time, since the wall surface 40b of the recess 40 is inclined at an angle α of less than 90° with respect to the sliding surface 30, the lubricating oil easily flows from the oil film covering the sliding surface 30 into the recess 40, and the recess 40 easily functions as an oil reservoir. When the amount of lubricating oil decreases with the sliding of the sliding member 1, the oil film covering the sliding surface 30 becomes thinner or is lost, and the wear of the sliding layer 20 progresses, and the depth h of the recess 40 becomes smaller. In such a case, the lubricating oil stored in the recess 40 is supplied to the sliding surface 30, and further wear of the sliding layer 20 can be prevented.

[0028] The lubricating oil that has entered the recess 40 is successively replaced as the sliding member 1 slides, preventing a temperature rise within the recess 40. This effect suppresses a temperature rise on the sliding surface 30, prevents softening of the sliding layer 20, which contains a large amount of resin material, and improves the seizure resistance of the sliding member 1.

[0029] The recess 40 may be one or more on the sliding surface 30, and is preferably a recess of 1 mm 2 ) may include one or more recesses 40. The diameter of the bottom surface of recess 40 (hereinafter referred to as "diameter of recess 40") may be 0.02 mm to 0.2 mm. By setting the diameter of recess 40 to be in the range of 0.02 mm to 0.2 mm, lubricating oil is easily drawn into recess 40, and recess 40 can easily function as an oil reservoir. The depth h from the bottom surface 40a of the recess 40 to the sliding surface 30 may be 5 μm to 30 μm. If the depth h is 5 μm or more, even if the sliding layer 20 wears after the sliding member 1 starts to slide, the resin of the sliding layer 20 remains in the early stage of the sliding, and the seizure resistance of the sliding member 1 is maintained. If the depth h of the recess 40 is 30 μm or less, lubricating oil easily enters the recess 40 during sliding of the sliding member 1, and excellent seizure resistance can be exhibited.

[0030] The angle α between the wall surface 40b of the recess 40 and the sliding surface 30 may be less than 90°, and preferably 60° to 86°. By setting the angle α to 60° to 86°, the lubricating oil easily enters the recess 40, and the recess 40 easily functions as an oil reservoir for the lubricating oil. In addition, the oil that has entered the recess 40 is easily discharged as the sliding member 1 slides. As a result, the sliding heat in the recess 40 during sliding can be easily released, and the seizure resistance of the sliding member 1 is improved.

[0031] The bottom surface 40a of the recess 40 corresponds to the upper surface of the metal layer 10. The metal layer 10 may contain a porous sintered metal, which may contain spherical or irregularly shaped metal powder of copper, a copper alloy, aluminum, an aluminum alloy, or the like. The bottom surface 40a of the recess 40 is preferably approximately parallel to the sliding surface 30, but does not have to be parallel. The bottom surface 40a may be a flat surface or a curved surface.

[0032] (Characteristics and Effects of the Sliding Layer) The sliding layer 20 may be made of a fluororesin base mixed with graphite and hard particles. It may also contain other additives such as liquid crystal polymer and molybdenum disulfide. Examples of fluororesins include PTFE (polytetrafluoroethylene), PFA (perfluoroalkoxycane), and EFFE (ethylene tetrafluoroethylene copolymer).

[0033] Graphite is generally known as a solid lubricant and has the effect of reducing the coefficient of friction. On the other hand, when hard particles are added to a resin material for a sliding material, they have the effect of increasing the wear resistance of the resin material, but at the same time, they also have the effect of increasing the coefficient of friction. Therefore, when both graphite and hard particles are added to a resin material, in order to obtain favorable performance in terms of the wear coefficient and wear resistance of the resin material, it is necessary to adjust the ratio of graphite to hard particles to an appropriate balance.

[0034] During sliding of the sliding layer 20, the graphite is broken down into small pieces by the presence of the hard particles, and a thin graphite film is formed on the sliding surface 30. The ratio of graphite to hard particles in the sliding layer 20 is preferably 6:1 to 2:1 in volume ratio. By setting the ratio of graphite to hard particles to 6:1 or more, it is possible to maintain low friction characteristics while obtaining the wear resistance effect of the hard particles, and therefore the seizure resistance of the sliding member 1 can be improved. If the ratio of graphite to hard particles is 2:1 or less, the amount of wear of the sliding layer 20 during sliding can be suppressed, and the excellent seizure resistance of the present invention can be exhibited.

[0035] In the sliding layer 20, it is desirable that the graphite is present at a ratio of 5 to 30 volume % and the hard particles are present at a ratio of 1 to 15 volume %. If the graphite is present at 5 volume % or more, in addition to the self-lubricating property of the fluororesin, the effect of reducing the friction coefficient of the graphite as a solid lubricant is exhibited, and if the graphite is present at 30 volume % or less, the effect of low friction characteristics is exhibited without impairing the adhesive strength between the fluororesin material and the porous sintered base material. Furthermore, if the hard particles are present at 1 volume % or more, the effect of wear resistance due to the addition of the hard particles is obtained, and if the hard particles are present at 15 volume % or less, wear resistance can be improved without impairing the low friction characteristics due to the presence of the fluororesin and graphite.

[0036] The graphite may be scaly or flaky and have an average particle size of 3 to 20 μm.

[0037] The hard particles may be an inorganic compound having a Mohs hardness of 3 to 6. If the Mohs hardness is between 3 and 6, the wear resistance can be improved without damaging the counter material. The hard particles may have an average particle size of 0.1 to 30 μm. If the average particle size is 0.1 to 30 μm, the wear resistance can be improved as hard particles, and the graphite is finely crushed during sliding of the sliding member 1, thereby obtaining an effect of improving the sliding properties.

[0038] The hard particles may be iron oxide, boron nitride, Tismo, copper sulfate, magnesium oxide, zinc oxide, magnesium carbonate, or the like, each having a Mohs hardness of 3 to 6. In addition, the hard particles may be one type or a combination of two or more types, as long as they are within the above-mentioned ranges of Mohs hardness, average particle size, and amount added.

[0039] (Method of manufacturing slide member) The sliding member 1 is manufactured by the following steps. (1) After mixing the fluororesin with various fillers, a molding aid is added to the resulting mixture and the mixture is stirred and mixed to obtain a resin raw material. (2) The resin raw material obtained in the above step (1) is spread on a porous metal substrate, which is then rolled with a roller to impregnate the resin raw material into the voids in the porous metal substrate formed by sintering, and to form a coating layer made of the resin raw material uniformly on the surface of the porous metal substrate (see FIG. 4(a)). (3) The part obtained in the above step (2) is placed in a drying furnace heated to 100° C. to 200° C. to remove the molding aid (see FIG. 4(b)). (4) The part from which the molding aid has been removed is introduced into a heating furnace, where it is heated and sintered at a temperature range of 380°C to 420°C, and then cooled (see FIG. 4(c)). (5) The material is rolled to the specified dimensions using rollers to form a component of the specified thickness.

[0040] The purpose of adding the molding aid in the above step (1) is to facilitate the impregnation of the mixture consisting of the fluororesin and the filler into the porous metal substrate. The amount of the molding aid to be added may be adjusted depending on the type of filler and the ratio of the fluororesin to the filler. In the present invention, the amount of the molding aid added is increased by about 4% to 10% from the conventional amount, and the amount of the molding aid removed in step (3) is increased, and the amount of shrinkage of the resin material during the firing in step (4) is increased. Furthermore, in step (2), the thickness of the coating layer is set to 30 μm or less to obtain the structure of the present invention. When the resin shrinks in step (4), shrinkage occurs toward the thicker coating layer at the location where the distance between the top of the porous sintered substrate and the sliding surface (thickness of the coating layer) is small, so that a recess is formed on the sliding surface, and the structure of the present invention is obtained. In step (4), the diameter of the recess formed can be changed by changing the heating and firing time. In the conventional technology, the heating and baking time was about 2 minutes, but by extending this time by 3 to 8 times, the diameter of the recesses can be within the range of 0.02 mm to 0.2 mm. A specific heating and baking time may be, for example, 10 minutes. EXAMPLES

[0041] (Performance evaluation test) In order to evaluate the seizure resistance of the sliding members according to the present invention, a sliding test was carried out for Examples 1 to 14 and Comparative Example 1.

[0042] (Test conditions) Testing machine: Thrust sliding test machine Load: 2MPa / 10min STEPUP Speed: 0.5m / s Lubricating oil: Supply amount 60cc / min Mating shaft: S55C hardened Test time: 100 min (up to 20 MPa load)

[0043] (Test piece) The sliding member obtained by the manufacturing method including the above-mentioned steps (1) to (5) was cut into a sample having a side length of 40 mm.

[0044] (Examples of materials used) PTFE: Commercially available products include Fluon (registered trademark) CD097E (manufactured by AGC) and Polyflon (registered trademark) F-201 (manufactured by Daikin Industries, Ltd.). Graphite: Commercially available products include the GRAPHITE POWDER series from Nippon Graphite Industry. Hard particles: Commercially available magnesium oxide products include Kyowamag MF30 (manufactured by Kyowa Chemical Industry Co., Ltd.) and RF10C (manufactured by Ube Material Industries, Ltd.) Commercially available iron oxide products include the Bengalese Color series by Morishita Bengalese Industry Co., Ltd.

[0045] (Sample Preparation) The composition of the samples is shown in Table 2. For "PTFE," CD097E manufactured by AGC was used. For "graphite," scaly graphite powder manufactured by Nippon Graphite Industries was used. For "hard particles," iron oxide, zinc oxide, magnesium carbonate, etc. were used. For "other fillers," molybdenum disulfide manufactured by Daizo was used.

[0046] (Method of measuring the inclination of the recess wall) The recess wall was measured with a laser microscope to measure the unevenness of the sliding surface, and the angle of the recess wall relative to the sliding surface was measured from the obtained shape data. The "inclination of the recess wall" in Tables 1 and 3 is the average value measured at five random points on the test piece. Alternatively, it can be measured by cutting a sample from the member and checking its cross section.

[0047] The preparation conditions and test results of the present Examples 1 to 14 and Comparative Example 1 are shown in Table 1-3. In Table 1, the "seizure judgment" was evaluated as "good" when the sliding member 1 was not seized and the test was completed, and was evaluated as "fair" when the sliding member 1 was not seized but the porous sintered metal was exposed. In addition, the sliding member 1 was evaluated as "bad" when seizure occurred during the test. In Table 3, the "seizure judgment" was evaluated as "good" when the sliding member 1 was not seized and the wear amount of the sliding layer was small, and was evaluated as "good" when the sliding member 1 was not seized but the wear amount of the sliding layer was large.

[0048] [Table 1]

[0049] [Table 2]

[0050] [Table 3]

[0051] From the results of Table 1, it is preferable that the inclination of the recess wall surface is about 60° to 86°. In Examples 1 to 7 in which the inclination of the recess wall surface is less than 90°, no seizure occurred, whereas in Comparative Example 1 in which the inclination of the recess wall surface is 90°, seizure occurred. Furthermore, from the results of Table 3, it is more preferable that the ratio of graphite to hard particles is about 6:1 to 2:1. In Examples 8 to 12 in which the ratio of graphite to hard particles is 6:1 to 2:1, no seizure occurred and the wear amount of the sliding layer was small, whereas in Example 13 in which the ratio of graphite to hard particles is 10:1 and Example 14 in which the ratio is 1:1, no seizure occurred but the wear amount of the sliding layer was large.

[0052] The above describes in detail the embodiments and examples of the present invention with reference to the drawings and in relation to the performance evaluation tests. However, the specific configurations are not limited to these, and modifications that do not depart from the gist of the present invention described in the claims are included in the present invention. [Explanation of symbols]

[0053] 1 Sliding member 10 metal layers 20 Sliding layer 30 Sliding surface 40 Recess 40a Bottom surface of recess 40b Side wall of recess

Claims

1. A sliding member including a metal layer including a porous sintered metal and a sliding layer including a resin material, The sliding layer has a portion in which a resin material is impregnated in the pores of the porous sintered metal, The sliding layer has a sliding surface and at least one recess, an inner wall surface of the recess is a part of the sliding layer, a bottom surface of the recess is a part of an upper surface of the metal layer; A sliding member, wherein the inner wall surface of the recess has an inclination of less than 90° with respect to the sliding surface.

2. The sliding layer further includes graphite and hard particles, 2. The sliding member according to claim 1, wherein a volume ratio of said graphite to said hard particles is 6:1 to 2:

1.

3. 3. The sliding member according to claim 1, wherein the resin material is made of a fluororesin.

4. The recess is located 1 mm above the sliding surface. 2 The sliding member according to claim 1 or 2, wherein one or more of the grooves are formed per one groove.

5. 3. The sliding member according to claim 1, wherein the inner wall surface of the recess has an inclination of 60° to 86° with respect to the sliding surface.

6. 3. The sliding member according to claim 1, wherein the recess has a diameter of 0.02 mm to 0.2 mm.

7. 3. The sliding member according to claim 1, wherein a depth from the bottom surface of the recess to the sliding surface is 5 μm to 30 μm.

8. 3. The sliding member according to claim 1, wherein the porous sintered metal is a spherical or irregularly shaped metal powder made of one or more of copper, a copper alloy, aluminum, and an aluminum alloy.

9. The sliding member according to claim 1 or 2, wherein the sliding layer further contains a liquid crystal polymer or molybdenum disulfide.

10. 3. The sliding member according to claim 2, wherein the fluororesin includes at least one of PTFE (polytetrafluoroethylene), PFA (perfluoroalkoxycane), and EFFE (ethylene tetrafluoroethylene copolymer).

11. 3. The sliding member according to claim 2, wherein the sliding layer contains 5 to 30% by volume of the graphite and 1 to 15% by volume of the hard particles.

12. 3. The sliding member according to claim 2, wherein the graphite is scaly or flaky and has an average particle size of 3 μm to 20 μm.

13. 3. The sliding member according to claim 2, wherein the hard particles have an average particle size of 0.1 μm to 30 μm.

14. 3. The sliding member according to claim 2, wherein the hard particles contain at least one of iron oxide, boron nitride, Tismo, copper sulfate, magnesium oxide, zinc oxide, and magnesium carbonate, and have a Mohs hardness of 3 to 6.