Ni PLATED STEEL SHEET AND BATTERY CONTAINER
By controlling the grain size and Fe indexing ratio on Ni-plated steel sheets, the issue of iron elution during overdischarge is addressed, improving electrolyte resistance and preventing corrosion in battery containers.
Patent Information
- Application Number
- JP2023059384
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Conventional Ni-plated steel sheets used in battery containers face issues with iron elution from the Fe-Ni diffusion layer into the electrolyte during overdischarge, leading to corrosion, as the positive electrode potential increases with battery capacity.
The solution involves controlling the average grain size and Fe indexing ratio on the outermost surface of the Ni-plated steel sheet by adjusting the Ni plating amount and thermal diffusion treatment conditions, ensuring an average grain size of 0.32 μm or more and an Fe indexing ratio of 0.0% to 6.0% through EBSD measurement.
This approach effectively suppresses iron elution into the electrolyte, enhancing the electrolyte resistance and preventing corrosion during overdischarge.
Smart Images

Figure 2024146470000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a Ni-plated steel sheet and a battery container. [Background technology]
[0002] Conventionally, Ni-plated steel sheets have been widely used as materials for battery containers. Patent Document 1 discloses a Ni-plated steel sheet for battery containers, which has an iron-nickel diffusion layer formed by forming a nickel plating layer on the steel sheet and then carrying out a thermal diffusion treatment to prevent the occurrence of pitting corrosion and leakage, and in which the ratio of Ni and Fe in the outermost layer is controlled. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2014-47359 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, with the increase in battery capacity, there is a problem in that in the battery container using the Ni-plated steel sheet disclosed in Patent Document 1, when an abnormality occurs in the battery management system or overdischarge occurs during the aging process of battery production, the potential of the Fe-Ni diffusion layer approaches the positive electrode potential, causing iron to dissolve from the Fe-Ni diffusion layer into the electrolyte, resulting in corrosion of the inner wall of the battery container. As the battery capacity increases, the positive electrode potential tends to become even higher, and there is a demand for a Ni-plated steel sheet in which the Fe-Ni diffusion layer has even better electrolyte resistance during overdischarge.
[0005] An object of the present invention is to provide a Ni-plated steel sheet that has excellent electrolyte resistance during overdischarge. [Means for solving the problem]
[0006] As a result of intensive research into achieving the above-mentioned object, the inventors have found that in a Ni-plated steel sheet having an Fe-Ni diffusion layer formed on at least one surface of the steel sheet, the above-mentioned object can be achieved by appropriately controlling the average crystal grain size obtained by EBSD measurement and the proportion of the region that can be indexed by Fe, and have thus completed the present invention.
[0007] [1] That is, according to a first aspect of the present invention, there is provided a Ni-plated steel sheet comprising a steel sheet and an Fe-Ni diffusion layer formed on at least one surface of the steel sheet, wherein the Ni-plated steel sheet has an average crystal grain size of 0.32 μm or more obtained by EBSD measurement at an outermost surface thereof, and the proportion of a region that can be indexed by Fe is 0.0% or more and 6.0% or less.
[0008] [2] According to the second aspect of the present invention, the Ni coating weight per one side of the Ni-plated steel sheet is 0.8 to 8.9 g / m 2 The Ni-plated steel sheet according to the first aspect is provided,
[0009] [3] According to a third aspect of the present invention, there is provided the Ni-plated steel sheet according to the second aspect, which comprises a Ni layer formed on the Fe-Ni diffusion layer, and in which a proportion of the region that can be indexed with Fe obtained by EBSD measurement on an outermost surface of the Ni-plated steel sheet is 0.0% or more and 1.0% or less.
[0010] [4] According to a fourth aspect of the present invention, there is provided the Ni-plated steel sheet according to any one of the first to third aspects, wherein the steel sheet has a thickness of 0.03 to 1.5 mm.
[0011] [5] According to a fifth aspect of the present invention, there is provided the Ni-plated steel sheet according to any one of the first to fourth aspects, wherein the steel sheet is a low carbon steel or an extra-low carbon steel.
[0012] [6] According to a sixth aspect of the present invention, there is provided a battery container made using the Ni-plated steel sheet according to any one of the first to fifth aspects. Effect of the Invention
[0013] According to the present invention, it is possible to provide a Ni-plated steel sheet that is capable of suppressing the elution of iron (Fe) into an electrolyte during overdischarge and has excellent electrolyte resistance. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a schematic cross-sectional view showing the configuration of a Ni-plated steel sheet according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a phase map obtained by EBSD measurement of the Ni-plated steel sheet obtained in Example 7. [Diagram 3] FIG. 3 is an example of a chart obtained by high-frequency glow discharge optical emission spectrometry of a standard sample. [Figure 4] FIG. 4 is another example of a chart obtained by high-frequency glow discharge optical emission spectrometry of a standard sample. [Diagram 5] FIG. 5 shows an example of a temperature profile of a plated steel sheet to illustrate a method of calculating the thermal history Y in a thermal diffusion treatment. [Figure 6] FIG. 6 is a schematic cross-sectional view showing the configuration of a modified Ni-plated steel sheet according to an embodiment of the present invention. [Figure 7] FIG. 7 is a schematic diagram of a measuring jig used for evaluating the electrolyte resistance of Ni-plated steel sheets by the LSV method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Fig. 1 is a schematic cross-sectional view showing the configuration of a Ni-plated steel sheet in this embodiment. As shown in Fig. 1, the Ni-plated steel sheet in this embodiment includes a steel sheet and an Fe-Ni diffusion layer formed on at least one surface of the steel sheet.
[0016] The steel sheet is not particularly limited as long as it has excellent formability, but for example, low carbon steel such as low carbon aluminum killed steel (carbon content 0.01 to 0.15% by weight), ultra-low carbon steel with a carbon content of less than 0.01% by weight, or non-aging ultra-low carbon steel obtained by adding Ti, Nb, or the like to ultra-low carbon steel can be used. In this embodiment, hot rolled sheets of these steels are pickled to remove surface scale (oxide film), then cold rolled, and then electrolytically cleaned such as alkaline electrolytic degreasing, followed by annealing and / or temper rolling, or sheets that are cold rolled, electrolytically cleaned, and then not annealed or temper rolled, etc. can also be used. In addition, from the viewpoint of productivity, it is preferable to use a continuous steel strip as the steel sheet.
[0017] The thickness of the steel sheet may be appropriately selected depending on the application of the Ni-plated steel sheet and is not particularly limited, but from the viewpoint of reducing the manufacturing cost, the thickness is preferably 1.5 mm or less, more preferably 1.25 mm or less, and even more preferably 0.9 mm or less. Also, from the viewpoint of improving the mechanical properties of the Ni-plated steel sheet, the thickness of the steel sheet is preferably 0.03 mm or more, more preferably 0.1 mm or more, even more preferably 0.15 mm or more, and particularly preferably 0.2 mm or more.
[0018] The Ni-plated steel sheet of the present embodiment includes an Fe-Ni diffusion layer on the steel sheet. The Fe-Ni diffusion layer is formed by forming a Ni plating layer on the steel sheet, and then performing a thermal diffusion treatment on the steel sheet on which the Ni plating layer has been formed, thereby thermally diffusing iron (Fe) constituting the steel sheet and nickel (Ni) constituting the Ni plating layer. The Fe-Ni diffusion layer needs to be formed on at least one surface of the steel sheet, and may be formed on both surfaces of the steel sheet.
[0019] In the Ni-plated steel sheet of the present embodiment, the average crystal grain size obtained by EBSD (Electron Backscatter Diffraction Pattern) measurement of the outermost surface of the Ni-plated steel sheet is 0.32 μm or more, and the ratio of the area indexed by Fe is 0.0% or more and 6.0% or less. In the Ni-plated steel sheet shown in FIG. 1, an Fe-Ni diffusion layer is formed on the outermost surface, so that the average crystal grain size of the surface of the Fe-Ni diffusion layer obtained by EBSD measurement and the ratio of the area indexed by Fe are controlled within the above range. Since the Ni-plated steel sheet of the present embodiment has the above characteristics, it is possible to suppress the dissolution of iron into the electrolyte during overdischarge, and is excellent in electrolyte resistance. Note that the area indexed by Fe in the present invention refers to an area indexed using material data of Fe(α) in an EBSD pattern obtained by EBSD measurement.
[0020] The average crystal grain size on the outermost surface of Ni-plated steel sheet can be obtained as follows. That is, by performing EBSD measurement on the outermost surface of Ni-plated steel sheet, the EBSD pattern is indexed using two material data of Fe(α) and Ni, and mapping data containing information on each phase and orientation is obtained for each measurement field. The average crystal grain size can be obtained by the Number method using analysis software for the obtained mapping data. Note that the analysis software that can be used is, for example, OIM Analysis Version 7.3.
[0021] The average crystal grain size of the outermost surface of the Ni-plated steel sheet is 0.32 μm or more, preferably 0.36 μm or more, and more preferably 0.5 μm or more. If the average crystal grain size of the outermost surface of the Ni-plated steel sheet is too small, the number of paths through which the electrolyte penetrates from the outermost surface into the inside of the Ni-plated steel sheet increases, and the electrolyte resistance of the Ni-plated steel sheet may decrease. The upper limit of the average crystal grain size of the outermost surface of the Fe-Ni diffusion layer is not particularly limited, but is usually 4.0 μm or less.
[0022] The region that can be indexed with Fe obtained by EBSD measurement is, as described above, a region that can be indexed using the material data of Fe(α) and is determined to have a structure similar to the crystal structure of Fe(α). FIG. 2 is a phase map obtained by EBSD measurement of the Ni-plated steel sheet obtained in Example 7. The region that can be indexed with Fe is the region displayed in white in FIG. 2. Note that, in FIG. 2, the region displayed in gray is the region that can be indexed using the material data of Ni (hereinafter referred to as the region that can be indexed with Ni), that is, the region that is determined to have a structure similar to the crystal structure of Ni, and the region displayed in black is the region that has been deleted by the cleanup process and the lower limit setting of the CI value (described later) performed when analyzing the results obtained by EBSD.
[0023] The ratio of the area indexed by Fe obtained by EBSD measurement (hereinafter also referred to as Fe indexing ratio) is obtained as follows. First, EBSD measurement is performed on a Ni-plated steel sheet in the same manner as in the calculation of the average grain size described above to obtain mapping data, and then a phase map in which Fe and Ni are color-coded (indexed) is created using analysis software. The ratio of the area of the area indexed by Fe to the total area of the area indexed by Fe or Ni in the phase map (excluding areas deleted by cleanup processing or lower limit setting of CI value, etc.) can be obtained as the Fe indexing ratio of this embodiment. Although not particularly limited, the Fe indexing ratio can be obtained as the numerical value of the partition fraction of Fe by analysis software. The ratio of the area indexed by Ni (hereinafter also referred to as Ni indexing ratio) is also expressed in the same manner as the Fe indexing ratio, and can be obtained as the numerical value of the partition fraction of Ni by analysis software.
[0024] The Fe indexing ratio of the outermost surface of the Ni-plated steel sheet is 6.0% or less, preferably 5.0% or less, more preferably 3.0% or less, and particularly preferably 1.0% or less. If the Fe indexing ratio is too large, the elution of Fe from the outermost surface increases, and the electrolyte resistance of the Ni-plated steel sheet may decrease. The lower limit of the Fe indexing ratio of the outermost surface of the Ni-plated steel sheet is not particularly limited, and since a region that can be indexed with Fe does not need to be formed on the outermost surface, it is usually 0.0% or more.
[0025] The Ni index ratio of the outermost surface of the Ni-plated steel sheet is not particularly limited, but is preferably 94% or more, more preferably 95% or more, even more preferably 97% or more, and particularly preferably 99% or more.
[0026] The penetration depth into the sample in the EBSD measurement is very shallow at several tens of nm, so that the crystalline state of the portion closer to the surface of the sample (the outermost surface) can be measured. In the Ni-plated steel sheet of the present embodiment, the proportion of the region that can be indexed with Fe obtained by the EBSD measurement is 0.0% or more and 6.0% or less, so that the state of the Fe-Ni alloy of the outermost surface is appropriately controlled, the electrolyte resistance during overdischarge is high, and the occurrence of corrosion due to the dissolution of iron can be suppressed.
[0027] In addition, when analyzing, it is preferable to perform cleanup processing (Grain CI standardization) by analysis software and evaluate using data measurement points with a confidence index (CI value) of more than 0.1. The CI value is an index that indicates the reliability of the results of indexing and orientation calculation by the EBSD method, and a measurement point with a CI value of more than 0.1 indicates that correct indexing and orientation calculation were performed with an accuracy of more than 95%. The calculation of the average grain size by the Number method is not particularly limited, but can be performed under the conditions of Grain Tolerance: 5, Minimum Grain: 2 for all data of Fe and Ni that have been cleaned up as described above. In addition, for twin crystals, analysis can be performed in which they are regarded as separate grains by adopting default conditions without making special settings. In addition, in the EBSD measurement, partial processing distortion and unevenness are introduced on the sample surface by temper rolling after heat treatment, and it may be difficult to detect patterns at those locations, so it is preferable that the average CI value of the mapping data obtained under the above measurement conditions is not too low, and specifically, it is preferable that the average CI value is 0.04 or more.
[0028] In this embodiment, in addition to the average grain size and Fe indexing ratio measured by EBSD measurement, it is preferable that the Fe ratio at the outermost surface of the Fe-Ni diffusion layer and the thickness of the Fe-Ni diffusion layer measured using a high-frequency glow discharge optical emission spectroscopy (GDS) device are within a predetermined range. The Fe ratio at the outermost surface of the Fe-Ni diffusion layer and the thickness of the Fe-Ni diffusion layer can be obtained by continuously measuring the changes in Fe intensity and Ni intensity in the depth direction from the outermost surface to the steel sheet using a high-frequency glow discharge optical emission spectroscopy.
[0029] The proportion of Fe (mass%) in the outermost surface of the Fe-Ni diffusion layer measured by GDS (hereinafter also referred to as the Fe proportion by GDS) is preferably more than 10%, more preferably 20% or more, even more preferably 25% or more, and particularly preferably 30% or more from the viewpoint of improving weldability. Moreover, the proportion of Fe in the outermost surface of the Fe-Ni diffusion layer is preferably 75% or less, more preferably 72% or less, even more preferably 70% or less, and particularly preferably 65% or less from the viewpoint of rust suppression during storage before assembling a battery using the Ni-plated steel sheet.
[0030] In the Ni-plated steel sheet of the present embodiment, the Fe indexing ratio by EBSD measurement and the Fe ratio by GDS are completely different parameters. Specifically, the Fe indexing ratio by EBSD measurement focuses on the crystal structure of the outermost surface of the Ni-plated steel sheet and indicates the extent to which a structure similar to the Fe crystal structure exists relative to Ni or a structure similar to the Ni crystal structure. In contrast, the Fe ratio by GDS only indicates the extent to which the Fe element exists on the surface in mass ratio, and does not reflect information on the state in which Fe and Ni exist when both exist on the surface. In the course of intensively studying the improvement of the electrolyte resistance of Ni-plated steel sheet, the present inventors noticed that the electrolyte resistance during overdischarge changes even when the abundance ratio of the Fe element by GDS is the same, and found that it can be controlled by the Fe indexing ratio obtained by EBSD measurement. In other words, the inventors discovered that it is important to control the alloy state of Fe and Ni at the outermost surface, rather than simply the proportion of Fe element present, and that even when Fe element is present at the surface, it is possible to improve electrolyte resistance during overdischarge by suppressing the formation of a crystal structure similar to Fe at the outermost surface and setting the Fe indexing proportion by EBSD measurement to 0.0% or more and 6.0% or less.
[0031] From the viewpoint of production costs, the thickness of the Fe-Ni diffusion layer is preferably 4.0 μm or less, more preferably 3.0 μm or less, even more preferably 2.5 μm or less, and particularly preferably 2.0 μm or less. Also, from the viewpoint of improving the electrolyte resistance of the Ni-plated steel sheet during overdischarge, the thickness of the Fe-Ni diffusion layer is preferably 0.36 μm or more, more preferably 0.45 μm or more, even more preferably 0.6 μm or more, and particularly preferably 0.7 μm or more.
[0032] Specifically, the Fe content in the outermost surface of the Fe-Ni diffusion layer and the thickness of the Fe-Ni diffusion layer can be determined by the following steps. Measurement step 1: High-frequency glow discharge optical emission spectroscopy is performed on the standard sample to obtain intensity data for each etching time, and the saturation value of Fe intensity, the maximum value of Ni intensity, and the etching rate of Ni are confirmed. If the saturation value of Fe intensity and the maximum value of Ni intensity are not the same value in the measurement data of the standard sample obtained in this way, correction coefficients are calculated for Fe and Ni respectively so that the saturation value of Fe intensity and the maximum value of Ni intensity become the same value (for example, 10), and all intensity data are corrected. Measurement step 2: Analyze the target test piece of Ni-plated steel sheet under the same analytical conditions as in measurement step 1 to obtain strength data for each etching time. If a correction factor was applied in measurement step 1, apply the correction factor to the target test piece data in the same way, and use the strength data obtained to proceed to the subsequent steps. Measurement step 3: For the data obtained in measurement step 2, the Fe ratio and Ni ratio are calculated for each measurement point using the following formula. Fe ratio = Fe strength / (Fe strength + Ni strength) Ni ratio = Ni strength / (Fe strength + Ni strength) Measurement step 4: In a chart obtained from the data obtained in measurement step 3, the point at which the Fe ratio first reaches a minimum value is determined as the outermost surface. Measurement step 5: The outermost surface determined in measurement step 4 is taken as the starting point, and the point where the Ni intensity in the data is 10% of the maximum Ni intensity of the standard sample is taken as the interface point, the difference in etching time between the starting point and the interface point is calculated, and the etching depth calculated by multiplying the difference in etching time by the etching rate is the thickness of the Fe-Ni diffusion layer. The interface point refers to the interface between the Fe-Ni diffusion layer and the steel sheet. Measurement step 6: The Fe ratio at the outermost surface determined in measurement step 4 is the Fe ratio at the surface of the Fe-Ni diffusion layer.
[0033] Measurement step 1 will be explained. In measurement step 1, radio frequency glow discharge optical emission spectroscopy is performed on the standard sample to obtain intensity data for each etching time, and the saturation value of Fe intensity, the maximum value of Ni intensity, and the etching rate of Ni are confirmed. First, a standard sample is prepared consisting of a steel sheet with Ni plating that has not been subjected to heat treatment and whose plating layer thickness (or deposition amount) is known. For example, a standard Ni-plated steel sheet is prepared by applying a matte Ni plating of 1.1 μm to a low carbon steel sheet with a thickness of 0.3 mm. For this standard sample, the Fe intensity and Ni intensity in the standard Ni-plated steel sheet are measured using a radio frequency glow discharge optical emission spectroscopy analyzer until the Fe intensity is saturated. By obtaining the Fe intensity and Ni intensity, a chart like that shown in Figure 3 can be obtained. Figure 3 is an example of a chart obtained by radio frequency glow discharge optical emission spectroscopy of a standard sample. In Figure 3, the vertical axis indicates Fe intensity and Ni intensity, and the horizontal axis indicates the measurement time when the measurement is performed in the depth direction from the surface of the standard Ni-plated steel sheet (the surface on which the Ni plating is formed) using a radio frequency glow discharge optical emission spectroscopy analyzer.
[0034] The saturation value of Fe intensity is determined from the resulting chart. The saturation value of Fe intensity can be determined from the change in Fe intensity per second, that is, the time rate of change of Fe intensity (Fe intensity change / second). The time rate of change of Fe intensity increases rapidly when Fe is detected after measurement begins, and decreases after passing the maximum value, stabilizing at approximately zero. The value of Fe intensity when the time rate of change of Fe intensity stabilizes at approximately zero is the saturation value of Fe intensity. Specifically, the saturation value of Fe intensity is the value when the time rate of change of Fe intensity becomes 0.02 or less.
[0035] Next, the maximum Ni intensity is calculated. For example, in Figure 3, the Ni intensity of 10 at a measurement time of 9.9 seconds is the maximum Ni intensity. Note that the saturation value of Fe intensity and the maximum Ni intensity may not be the same value as in Figure 4, depending on the GDS measurement conditions. In this case, a correction coefficient is calculated to multiply the Fe intensity or Ni intensity so that the saturation value of Fe intensity and the maximum Ni intensity are the same value, and the subsequent steps are carried out. For example, in the case of Figure 3, the saturation value of Fe intensity of 10 is used as the standard, and a correction coefficient is calculated to multiply the Ni intensity so that the maximum Ni intensity after correction is 10. Figure 4 is another example of a chart obtained by radio frequency glow discharge optical emission spectroscopy of a standard sample.
[0036] Next, the etching rate of Ni is obtained. The etching rate can be obtained based on the thickness of the Ni plating and the etching time. Regarding the etching time, since Ni is considered to exist up to the point where the Ni intensity is 10% of the maximum Ni intensity in the GDS analysis, the etching time is set to the time from the start of measurement to the point where the Ni intensity is 10% of the maximum Ni intensity in the standard sample. For example, in the case of FIG. 3, the etching rate can be obtained by dividing the thickness of the Ni plating, 1.1 μm, by the time from the start of measurement to the time where the Ni intensity is 10% of the maximum Ni intensity. Since the etching rates of Ni and Fe are approximately the same, in the present invention, the thickness of the Fe-Ni diffusion layer is determined using the etching rate of Ni obtained as described above.
[0037] Measurement step 2 will now be described. In measurement step 2, a GDS analysis is performed on the Ni-plated steel sheet of this embodiment. The Ni-plated steel sheet of this embodiment is used as a target test piece, and is measured using GDS under the same conditions as in step 1 above to obtain the Fe intensity and Ni intensity in the Ni-plated steel sheet. If a correction coefficient is applied in measurement step 1, the subsequent steps are carried out using strength data obtained by correcting the data of the target test piece with the same value as the correction coefficient used for the standard sample. In this embodiment, Fe is diffused up to the surface, so strength data is obtained in which the Fe intensity on the surface does not become 0.
[0038] In this embodiment, whether the surface of the Ni-plated steel sheet is an Fe-Ni diffusion layer can be determined by whether the Fe intensity of the surface of the Ni-plated steel sheet exceeds 10% of the saturation value of the Fe intensity. If the Fe intensity of the outermost surface exceeds 10%, the surface can be determined to be an Fe-Ni diffusion layer, and conversely, if it does not exceed 10%, it is determined that a Ni layer exists on the Fe-Ni diffusion layer.
[0039] Measurement step 3 will now be described. In measurement step 3, the Fe ratio and Ni ratio at each depth position in the Fe-Ni diffusion layer are obtained. In the data obtained in measurement step 2 above, the Fe ratio at each time, i.e., at each depth position, can be obtained by calculating the percentage of the Fe and Ni intensity values (corrected intensity values if a correction factor is used) at each time. In other words, the Fe ratio and Ni ratio can be obtained by the following formula. Fe ratio = Fe intensity / (Fe intensity + Ni intensity) x 100 Ni ratio = Ni intensity / (Fe intensity + Ni intensity) x 100
[0040] Measurement step 4 will now be described. In measurement step 4, the depth position of the outermost surface of the Fe-Ni diffusion layer is defined. In a high-frequency glow discharge optical emission spectrometer, signals containing noise may appear due to the effects of surface contamination at the start of etching, so in order to correctly determine the Fe ratio at the outermost surface, the point (depth position) where the Fe ratio is at its minimum is defined as the outermost surface of the Fe-Ni diffusion layer. Under normal measurement conditions, this minimum value of the Fe ratio appears between 0 and 5 seconds into the measurement time.
[0041] Measurement step 5 will be described. In measurement step 5, the thickness of the Fe-Ni diffusion layer is obtained by determining the etching depth from the outermost surface to the boundary between the Fe-Ni diffusion layer and the steel sheet. The position of the outermost surface is the position defined in measurement step 4. The boundary between the Fe-Ni diffusion layer and the steel sheet is the point (depth position) where the Ni intensity of the target sample is 10% of the maximum Ni intensity of the standard sample. In other words, if the maximum Ni intensity of the standard sample in step 1 is 10, the point where the Ni intensity of the target sample obtained in step 2 is 1 is the boundary between the Fe-Ni diffusion layer and the steel sheet. Note that the point where the Ni intensity is 1 is naturally a position deeper than the outermost surface, so the point where the Ni intensity is 1 at the beginning of the measurement (a depth position smaller than the depth position at the maximum Ni intensity) is excluded. Next, the difference between the etching time from depth position 0 (i.e., measurement time 0) to the outermost surface and the etching time from depth position 0 to the boundary between the Fe-Ni diffusion layer and the steel sheet is calculated, and this difference is multiplied by the etching rate calculated in measurement step 1 to calculate the thickness of the Fe-Ni diffusion layer.
[0042] In this way, the thickness of the Fe-Ni diffusion layer of the Ni-plated steel sheet of this embodiment can be obtained by using a numerical value indicating the relationship between the depth time (measurement time by a radio frequency glow discharge optical emission spectrometer) and the actual thickness, which is obtained by measuring a steel sheet having a Ni-plated layer that has not been subjected to thermal diffusion treatment and has a known Ni-plating thickness, using a radio frequency glow discharge optical emission spectrometer. The actual Ni-plating thickness before heat treatment can be obtained by measuring the thickness by observing the cross section of the steel sheet having a Ni-plated layer using a SEM, or by converting the Ni deposition amount obtained by fluorescent X-ray analysis into a thickness using the specific gravity of Ni.
[0043] The measurement step 6 will now be described. In the measurement step 6, the Fe ratio at the outermost surface of the Fe-Ni diffusion layer is determined. The Fe ratio at the outermost surface of the Fe-Ni diffusion layer can be determined as the Fe ratio at the depth position of the outermost surface determined in the measurement step 4.
[0044] The lower limit of the Ni coating mass on one side of the steel sheet is 0.45 g / m from the viewpoint of controlling the average grain size and Fe indexing ratio obtained by EBSD measurement within an appropriate range. 2 More than 0.8 g / m is preferable. 2 More preferably, 2.5 g / m 2 More preferably, 3.0 g / m or more. 2 The upper limit of the Ni coating amount on one side of the steel sheet is 26.7 g / m2, because it is difficult for Fe to diffuse to the outermost surface and it is necessary to increase the heat treatment temperature or extend the heat treatment time in order to sufficiently diffuse Fe. 2 Less than 17.8 g / m is preferred. 2 Less than 8.9 g / m is more preferable. 2 More preferably, 7.2 g / m 2 The following is particularly preferred. The amount of Ni deposited can be determined by X-ray fluorescence measurement. In X-ray fluorescence measurement, quantification can be performed using a calibration curve method. X-ray fluorescence measurement may be performed on a Ni-plated steel sheet on which an Fe-Ni diffusion layer has been formed by thermal diffusion treatment, or on a steel sheet on which a Ni-plated layer has been formed before thermal diffusion treatment.
[0045] In this embodiment, as shown in FIG. 1, the Fe-Ni diffusion layer is formed only on one side of the steel sheet, but the configuration of the Ni-plated steel sheet is not particularly limited thereto, and it is sufficient that the Fe-Ni diffusion layer is formed on at least one outermost surface of the steel sheet. For example, the Fe-Ni diffusion layer may be formed on the outermost surface of both sides of the steel sheet. Alternatively, the Fe-Ni diffusion layer may be formed on both sides of the steel sheet, and a Ni layer may be formed on the Fe-Ni diffusion layer on one of the two sides. In particular, when the Ni-plated steel sheet of this embodiment is used for a battery container having a can shape, it is preferable that an Fe-Ni diffusion layer having a controlled average crystal grain size and Fe indexing ratio is formed on the outermost surface of the surface that will become the inner surface of the battery container, and further, an Fe-Ni diffusion layer is formed on the surface that will become the outer surface of the battery container, and a Ni layer is formed on the Fe-Ni diffusion layer. In this case, the total Ni deposition amount contained in the Fe-Ni diffusion layer and the Ni layer on the surface that will become the outer surface of the battery container is 9.0 to 90 g / m 2 is preferred.
[0046] The Ni-plated steel sheet in this embodiment can be produced as follows.
[0047] First, a Ni plating layer is formed on a steel sheet. The Ni plating bath used to form the Ni plating layer may be a commonly used plating bath, such as a Watts bath, a sulfamic acid bath, a boron fluoride bath, or a chloride bath. For example, the Ni plating layer is formed using a Watts bath with a bath composition of 200-350 g / L of nickel sulfate hexahydrate, 20-60 g / L of nickel chloride hexahydrate, and 10-50 g / L of boric acid, at pH 3.0-5.0, bath temperature 40-70°C, and current density 10-40 A / dm 2 The Ni plating layer may be formed on at least one side of the steel sheet.
[0048] The amount W of Ni attached to the steel sheet by the formation of the Ni plating layer is not particularly limited as long as an Fe-Ni diffusion layer can be formed as the outermost surface of the Ni-plated steel sheet and its configuration can be controlled. However, if the amount of attachment is too large, it becomes difficult for Fe to diffuse to the outermost surface, and it becomes necessary to increase the heat treatment temperature or lengthen the heat treatment time in order to sufficiently diffuse Fe, which may make it difficult to set the average crystal grain size and the proportion of the area that can be indexed by Fe to appropriate ranges. Therefore, the amount of attachment is set to 26.7 g / m 2 Less than 17.8 g / m is preferred. 2 Less than 8.9 g / m is more preferable. 2 More preferably, 7.2 g / m 2 On the other hand, if the Ni coating weight W is too small, it is difficult to control the average crystal grain size and Fe indexing ratio obtained by EBSD measurement within an appropriate range, and there is a risk that the electrolyte resistance during overdischarge will decrease. 2 More than 0.8 g / m is preferable. 2 More preferably, 2.5 g / m 2 More preferably, 3.0 g / m or more. 2 The above is particularly preferable. When the Fe-Ni diffusion layer is formed on the outermost surface of both sides of the steel sheet, it is preferable that the Ni coating weight W on each side is within the above range. When the Ni-plated steel sheet of this embodiment is used for a battery container in the shape of a can, it is preferable to form an Fe-Ni diffusion layer on the surface that will become the outer surface of the battery container, and to form a Ni layer on the Fe-Ni diffusion layer. In order to configure the outer surface of the battery container in this way, the Ni coating weight on the surface that will become the outer surface of the battery container is 9.0 to 90 g / m 2 is preferred.
[0049] Next, the steel sheet on which the Ni plating layer has been formed (hereinafter referred to as the plated steel sheet) is subjected to a thermal diffusion treatment to form an Fe-Ni diffusion layer. By appropriately controlling the conditions of the thermal diffusion treatment, the average grain size and the Fe indexing ratio on the surface of the Ni plating steel sheet obtained by EBSD measurement can be controlled within an appropriate range.
[0050] The thermal diffusion treatment may be either a continuous annealing method or a box annealing method, and is not particularly limited, but the heat treatment atmosphere is preferably a non-oxidizing atmosphere or a reducing protective gas atmosphere, and when a reducing protective gas atmosphere is used, it is preferable to use a mixed gas of H2 and N2 called HNX gas, for example. In this embodiment, the thermal diffusion treatment includes an initial heating step, a final heating step, and a cooling step.
[0051] The initial heating step is a step of heating the plated steel sheet from room temperature to the start temperature of the final heating step (final heating start temperature) described later. The temperature rise rate in the initial heating step (hereinafter also referred to as the initial heating rate) is a rate that can be found by calculating the slope in the temperature profile of the plated steel sheet in the initial heating step. In other words, it can be calculated by dividing the temperature difference from the start temperature of the initial heating step to the start temperature of the final heating step by the required time. The initial heating rate is preferably set to be higher than the temperature rise rate in the final heating step described later. Specifically, the initial heating rate is preferably more than 4° C. / sec and not more than 14° C. / sec.
[0052] The maximum heating rate in the initial heating step (hereinafter also referred to as the maximum heating rate) is a rate obtained by calculating the maximum slope in the temperature profile of the plated steel sheet in the initial heating step, that is, the temperature profile from room temperature to the start temperature of the final heating step, and is preferably 4° C. / sec or more. In addition, from the viewpoint of controlling the average crystal grain size and the Fe indexing ratio within an appropriate range, the maximum heating rate in the initial heating step is preferably 14° C. / sec or less, more preferably 12° C. / sec or less, and even more preferably 10° C. / sec or less. If the maximum heating rate is too high, Fe diffuses before the crystal grains are coarsened and easily reaches the outermost surface, and a sudden change in the crystal structure is easily caused, and as a result, it is presumed that the Fe indexing ratio in the outermost surface of the Ni-plated steel sheet increases and the electrolyte resistance decreases. In particular, from the viewpoint of suppressing the diffusion of Fe to the outermost surface, the maximum heating rate in the temperature profile of 450° C. or more in the initial heating step is preferably 14° C. / sec or less, more preferably 12° C. / sec or less, and even more preferably 10° C. / sec or less.
[0053] The final heating step is a step of heating from the final heating start temperature to the maximum temperature in the thermal diffusion treatment (hereinafter referred to as the final temperature). The final heating start temperature is preferably 550°C or higher at which Ni in the Ni plating layer and Fe in the steel sheet begin to diffuse actively, more preferably 600°C or higher at which they begin to diffuse more actively, and even more preferably 650°C or higher. The final heating start temperature is preferably less than 900°C, more preferably less than 850°C. From the viewpoint of controlling the average crystal grain size and the Fe indexing ratio within an appropriate range, the final heating start temperature is preferably less than 930°C, more preferably less than 900°C, and even more preferably less than 870°C. The final heating temperature can be set based on the final heating start temperature so that the temperature difference from the final heating start temperature is a predetermined temperature difference, as described later.
[0054] In this embodiment, from the viewpoint of improving the electrolyte resistance of the Ni-plated steel sheet during overdischarge as described later, the temperature rise rate in the final heating step (hereinafter also referred to as the final temperature rise rate) is preferably 4° C. / sec or less, more preferably 3° C. / sec or less, and further preferably 1° C. / sec or less. The temperature rise rate in the final heating step is preferably 0.1° C. / sec or more, and more preferably 0.2° C. / sec or more.
[0055] The temperature difference between the final heating temperature and the final heating start temperature should be at least 10°C, but is preferably at least 30°C, and more preferably at least 40°C. If the temperature difference is too small, the heating time in the final heating step (final heating time) may be insufficient, and the desired alloy state of the Fe-Ni diffusion layer may not be obtained. In particular, when the Ni deposition weight is 2.5 g / m 2When the temperature difference is 60° C. or more, the temperature difference is preferably 30° C. or more, more preferably 40° C. or more, and even more preferably 60° C. or more. By making the temperature difference 60° C. or more, the desired surface alloy state can be obtained, and a Ni-plated steel sheet having higher electrolyte resistance during overdischarge can be stably obtained. The upper limit of the temperature difference is preferably 150° C. or less, more preferably 120° C. or less, and even more preferably 100° C. or less. In this embodiment, it is preferable to set the final heating rate to 4° C. / sec or less. Therefore, if the temperature difference is too large, the time in the high temperature range becomes too long, the Fe indexing ratio becomes too large, and there is a risk that the desired surface alloy state cannot be obtained.
[0056] In the cooling step, the plated steel sheet heated to the ultimate temperature is cooled to 120° C. or lower. There are no particular limitations on the cooling rate, but from the viewpoint of preventing defects in shape and wrinkles, the cooling rate is preferably 1° C. / sec to 20° C. / sec, and more preferably 1° C. / sec to 10° C. / sec.
[0057] FIG. 5 is an example of a temperature profile of a plated steel sheet, illustrating a method for calculating the thermal history Y in a thermal diffusion treatment.
[0058] From the viewpoint of improving the electrolyte resistance of the Ni-plated steel sheet during overdischarge, the thermal history Y applied to the plated steel sheet through the initial heating step, final heating step, and cooling step in the thermal diffusion treatment is preferably 150,000°C·sec or less, more preferably 120,000°C·sec or less, and even more preferably 100,000°C·sec or less. From the viewpoint of sufficiently thermally diffusing Fe and Ni to obtain the desired alloy state, the thermal history Y is preferably 15,000°C·sec or more, more preferably 35,000°C·sec or more, and even more preferably 45,000°C·sec or more. By setting the thermal history Y in the above range, the thickness of the Fe-Ni diffusion layer is also in the preferred range, and the thermal history Y can be obtained by integrating the amount of change in the heating temperature and cooling temperature with respect to time at 450°C or more. That is, the area of the shaded area in FIG. 5 corresponds to the thermal history Y in the thermal diffusion treatment. In order to set the thermal history Y of the plated steel sheet within the above range, the heating rate (including the maximum heating rate) at 450°C or higher in the initial heating step and the final heating step, the heating start temperature, the ultimate temperature, and the cooling rate in the cooling step may be appropriately adjusted.
[0059] If the thermal history Y in the thermal diffusion treatment is too large, the Fe indexing ratio increases, and the electrolyte resistance during overdischarge tends to decrease. On the other hand, if the thermal history Y in the thermal diffusion treatment is too small, the average crystal grain size in the outermost surface of the Ni-plated steel sheet becomes fine, and the electrolyte resistance during overdischarge may decrease.
[0060] Ni adhesion weight W (g / m 2 ) and the thermal history Y ratio W / Y×10 5 is preferably 1.0 or more. 5 If the amount of Ni applied W (g / m2) is less than 1.0, the Fe indexing ratio becomes too large, and the desired surface alloy state cannot be obtained, and the electrolyte resistance during overdischarge may deteriorate. 2 ) and the thermal history Y ratio W / Y×10 5 is preferably 20.0 or less, more preferably 10.0 or less, and further preferably 7.0 or less. 5If it exceeds 20.0, there is a risk that the average crystal grain size and Fe indexing ratio at the outermost surface of the Ni-plated steel sheet obtained by EBSD measurement cannot be controlled within an appropriate range.
[0061] As described above, the inventors have found that by controlling the Ni adhesion amount W on the steel sheet within the above range and performing thermal diffusion treatment of the Ni-plated steel sheet under the above conditions, the Ni in the Ni plating layer and the Fe in the steel sheet can be mutually diffused to form an Fe-Ni diffusion layer in which the crystal state of the outermost surface is appropriately controlled so that the average crystal grain size is 0.32 μm or more and the Fe indexing ratio is 0.0% or more and 6.0% or less. The Ni-plated steel sheet manufactured by the above method has excellent electrolyte resistance during overdischarge because the average crystal grain size and the Fe indexing ratio are appropriately controlled.
[0062] Conventionally, in order to suppress the formation of corrosion paths and improve electrolyte resistance, the average crystal grain size of the outermost surface of the Fe-Ni plating layer or Ni plating layer has generally been increased by increasing the temperature in the thermal diffusion treatment or increasing the thermal history. In contrast, the inventors have conducted extensive research and found that if the heat treatment temperature is too high or the thermal history is too long, the Fe indexing ratio at the outermost surface increases, which may increase the dissolution of Fe into the electrolyte, or the average crystal grain size at the outermost surface may become smaller. Although it is unclear why the average crystal grain size becomes smaller when the heat treatment temperature is too high, the thermal history is too large, or the above W / Y is less than the lower limit, it is believed that this is because the crystal grain growth is hindered by the excessive diffusion of Fe. In addition, even under the same heat treatment conditions, the Fe indexing ratio changes depending on the thickness of the Ni plating layer (Ni deposition amount). In this way, the inventors have found that in order to improve the electrolyte resistance of a Ni-plated steel sheet, it is necessary to control not only the average crystal grain size at the outermost surface of the Ni-plated steel sheet but also the Fe indexing ratio, and have further found the Ni plating coverage and thermal diffusion treatment conditions necessary to appropriately control these.
[0063] Although it is unclear why the average grain size and Fe indexing ratio of the outermost surface of the Ni-plated steel sheet can be controlled within the above ranges by heating under the above conditions, it is believed that it is possible to suppress the migration of Fe to the outermost surface and suppress the increase in the Fe indexing ratio by setting the heat history Y in a temperature range of 450°C or higher within an appropriate range for the Ni coating weight W. Furthermore, it is believed that by continuing to heat the plated steel sheet at a relatively slow rate in the final heating process, which is performed near the maximum temperature, it is possible to suppress a sudden change in the crystal structure and diffuse it evenly, thereby reducing the Fe indexing ratio and controlling the average grain size of the outermost surface within an appropriate range.
[0064] In addition, a method of controlling the Fe ratio in the outermost surface obtained by GDS has been known to improve the electrolyte resistance of Ni-plated steel sheets. In contrast, the present inventors have found that in order to improve the electrolyte resistance during overdischarge, it is not sufficient to simply control the abundance ratio (mass%) of the Fe element in the outermost surface, such as the Fe ratio obtained by GDS, but it is more important to control the Fe indexing ratio obtained by EBSD measurement, and have found an appropriate range for this.
[0065] In particular, in a conventional thermal diffusion treatment method for a typical Ni-plated steel sheet, the plated steel sheet is heated, soaked at the highest temperature for a predetermined time, and then cooled. In this series of steps, the soaking step is the step in which Fe is most likely to diffuse due to mutual diffusion, and the amount of Fe that reaches the outermost surface is likely to increase rapidly. In contrast, in the thermal diffusion treatment method of the present embodiment, after initial heating, the initial heating does not reach the highest temperature, and heating is continued at a relatively slow heating rate in the final heating step, and soaking at the same temperature is not performed, and then cooling is performed. In other words, since the ease of diffusion continues to change after Fe and Ni are in a mutual diffusion state, it is considered that, compared to the conventional manufacturing method in which Fe is diffused while maintaining a constant temperature, a sudden change in the crystal structure is suppressed, the Fe indexing ratio is reduced by diffusing evenly, and the average crystal grain size of the outermost surface can be controlled to an appropriate range. As a result, the thermal diffusion treatment method of the present embodiment can more appropriately control the alloy state of the outermost surface of the Fe-Ni diffusion layer compared to the thermal diffusion treatment method in which soaking is performed.
[0066] In this manner, the Ni-plated steel sheet of the present embodiment is manufactured.
[0067] After the thermal diffusion treatment, the Ni-plated steel sheet may be subjected to temper rolling as necessary. By temper rolling, it is possible to control mechanical properties, correct the shape, and impart surface roughness.
[0068] In addition, the Ni-plated steel sheet in FIG. 1 has an Fe-Ni diffusion layer formed on the outermost surface, but the configuration of the Ni-plated steel sheet is not particularly limited thereto, so long as the average crystal grain size of the outermost surface of the Ni-plated steel sheet obtained by EBSD measurement is 0.32 μm or more, and the Fe indexing ratio is 0.0% or more and 6.0% or less. For example, as shown in FIG. 6, the Ni-plated steel sheet may have a Ni layer formed on the Fe-Ni diffusion layer, and the outermost surface of the Ni-plated steel sheet may be composed of the Ni layer. FIG. 6 is a schematic diagram showing the configuration of a modified example of the Ni-plated steel sheet in this embodiment. In this case, the Ni adhesion amount in the Ni-plated steel sheet, i.e., the total adhesion amount of Ni contained in the Fe-Ni diffusion layer and the Ni layer thereon, is 0.8 to 8.9 g / m 2 From the viewpoint of ease of forming the Ni layer and controlling the average crystal grain size and the Fe indexing ratio within an appropriate range, it is more preferably 4.0 to 8.0 g / m 2 It is.
[0069] As described above, it can be determined by GDS analysis of the Ni-plated steel sheet that the outermost surface of the Ni-plated steel sheet is a Ni layer. If the Fe intensity of the surface of the Ni-plated steel sheet measured in measurement step 2 of the GDS analysis described above is 10% or less of the saturated value of the Fe intensity, it is determined that a Ni plating layer is formed on the Fe-Ni diffusion layer and that the outermost surface of the Ni-plated steel sheet is a Ni layer. If it is determined that the outermost surface of the Ni-plated steel sheet is a Ni layer, the thickness determined in measurement step 5 of the GDS analysis represents the combined thickness of the Ni layer and the Fe-Ni diffusion layer.
[0070] As shown in Fig. 6, when the outermost surface of the Ni-plated steel sheet is composed of a Ni layer, the average grain size and Fe indexing ratio of the surface of the Ni layer obtained by EBSD measurement may be controlled within the above ranges. The Fe indexing ratio obtained by EBSD measurement is 0.0% or more and 6.0% or less, and preferably 0.0% or more and 1.0% or less. The Ni-plated steel sheet of the modified example can be manufactured by appropriately adjusting the conditions of Ni plating and thermal diffusion treatment.
[0071] In the Ni-plated steel sheet of the modified example, the reason why the electrolyte resistance during overdischarge can be improved by controlling the average crystal grain size and the Fe indexing ratio of the surface of the Ni layer within the above range is as follows. 2 and when the Fe-Ni diffusion layer and the Ni layer thereon are formed, the thickness of the Ni layer at the outermost surface becomes relatively thin. When the Ni layer is thin, even if the Fe element is below the detection limit in a wide area measured by GDS, Fe may reach the vicinity of the outermost surface partially (especially around the grain boundaries, etc.), which may affect the electrolyte resistance during overdischarge. In addition, since the Ni layer is relatively thin, it is considered that the state of the Ni layer, that is, the average crystal grain size and the crystal structure, are strongly influenced by the formation of the Fe-Ni diffusion layer immediately below it. Therefore, it is presumed that good electrolyte resistance during overdischarge can be obtained by controlling the average crystal grain size and Fe indexing ratio obtained by EBSD measurement in the same manner as in the embodiment in which the outermost surface is the Fe-Ni diffusion layer described above.
[0072] When the Ni-plated steel sheet of the modified example is used for a battery container in the shape of a can, it is preferable that an Fe-Ni diffusion layer is formed on the surface that will become the inner surface of the battery container, and a Ni layer having a controlled average crystal grain size and Fe indexing ratio is formed on the outermost surface of the Fe-Ni diffusion layer, and further, an Fe-Ni diffusion layer is formed on the surface that will become the outer surface of the battery container, and a Ni layer is formed on the Fe-Ni diffusion layer. In this case, the total Ni coating amount contained in the Fe-Ni diffusion layer and the Ni layer on the surface that will become the outer surface of the battery container is preferably 9.0 to 90 g / m2.
[0073] <Battery container> The battery container in this embodiment is obtained by forming the Ni-plated steel sheet so that the surface on which the Fe-Ni diffusion layer is formed faces the inside of the battery container. Specifically, the Ni-plated steel sheet is formed into the shape of the battery container by drawing, ironing, DI (Draw and Ironing) or DTR (Draw and Thin Redraw) forming.
[0074] The battery container obtained by forming the Ni-plated steel sheet in this embodiment has a high electrolyte resistance during over-discharge and can suppress the occurrence of corrosion due to Fe elution because the average crystal grain size on the outermost surface of the surface in contact with the electrolyte and the ratio of the region indexed by Fe are appropriately controlled.
Example
[0075] Hereinafter, the present invention will be described more specifically with reference to examples, but the present invention is not limited to these examples. The evaluation methods for each property are as follows.
[0076] <Ni deposition amount, Ni plating layer thickness> In the plated steel sheet on which the Ni plating layer was formed in each example and comparative example, the Ni deposition amount per one surface of the Ni-plated steel sheet was determined by measuring with a fluorescent X-ray device. As the fluorescent X-ray device, ZSX100e (manufactured by Rigaku Corporation) was used, and the measurement was performed by the calibration curve method. The Ni deposition amount was converted into thickness using the density of Ni (8.9 g / cm 3 ) to obtain the thickness of the Ni plating layer. <Fe-Ni diffusion layer thickness and Fe ratio by GDS> Using a high-frequency glow discharge optical emission spectrometer (manufactured by Horiba, Ltd., model number: GD-PROFILER2), the ratio of Fe by GDS (hereinafter also referred to as the ratio of Fe) was determined. The ratio of Fe was determined by the above-described measurement steps 1 to 6 using a high-frequency glow discharge optical emission spectrometer. Similarly, for Examples 1 to 8 and Comparative Example 3, the Fe-Ni diffusion layer thickness by GDS was determined by the above-described measurement steps 1 to 5. The specific measurement conditions of the high-frequency glow discharge optical emission spectrometer were set as follows. · Measurement mode: HDD mode · Excitation mode: RF (normal) · Output: 35 W · Pressure: 600 Pa · Module: 7 V · Fuse: 7 V · Anode path: 4 mm · Gas replacement time: 30 seconds · Preliminary sputtering time: 30 seconds · Background measurement time: 10 seconds · Measurement time: 80 seconds · Sampling interval: 0.1 second
[0077] When the ratio of Fe obtained by GDS analysis exceeded 10%, it was determined that Fe had reached the outermost surface and an Fe-Ni diffusion layer had been formed on the outermost surface. On the other hand, when the ratio of Fe was 10% or less, it was determined that Fe had not reached the outermost surface and the outermost surface was a Ni layer.
[0078] <Average crystal grain size of the outermost surface of Ni-plated steel sheet> An electron beam was irradiated onto the surface of the Ni-plated steel sheet using a scanning electron microscope (SEM) (model: SU8020, manufactured by Hitachi High-Technologies Corporation), and the generated EBSD pattern was acquired with an EBSD detector. Indexing was performed using an OIM (Orientation Imaging Microscopy) crystal orientation analysis device (manufactured by TSL Solutions) and measurement software (OIM Data Collection Version 6.2.1). The measurement conditions for SEM and EBSD were as follows. The number of measurement fields of view for EBSD was 3. (SEM measurement conditions) · Accelerating voltage: 20 kV · Emission current: 20 μA · W.D.: 20 mm · Measurement magnification: 7000 times (EBSD measurement conditions) · Measurement area: 7 μm × 7 μm · Step: 0.05 μm · Material data: Fe(α) and Ni (EBSD analysis conditions) · Grain Tolerance: 5 · Minimum Grain: 2
[0079] For each measurement field of view, indexing was performed using two material data, namely the material data of Fe(α) and the material data of Ni, by means of EBSD measurement under the above conditions, thereby obtaining mapping data having information on each phase and orientation. With respect to the obtained mapping data, by analyzing using analysis software (OIM Analysis Version 7.3) and the above analysis conditions, the ratio of the area of the region that can be indexed by Fe and the average crystal grain size in each measurement field of view were obtained. When analyzing, a cleanup process (Grain CI standardization) by the analysis software was performed, and the data measurement points with a confidence index (CI value) exceeding 0.1 were used for evaluation. For all the data of Fe and Ni subjected to the above cleanup process, the crystal grain size distribution was determined using Grain Size (diameter) from which information on the crystal grain size based on the diameter of a circle with the same area as each crystal grain was obtained, and the average crystal grain size was calculated using the Number method. In this way, the average value of the average crystal grain sizes obtained for each measurement field of view was calculated.
[0080] <Ratio of Fe Indexing on the Outermost Surface of Ni-Plated Steel Sheet> From the data obtained by the above EBSD measurement and analysis, a Phase Map of Fe and Ni was created. In the Phase Map, with the total area of the regions that can be indexed by Fe or Ni (excluding the regions removed as data in the above cleanup process and the lower limit setting of the CI value) taken as 100%, the ratio of the area of the region that can be indexed by Fe to this total area was calculated as the Fe indexing ratio. The average value of the Fe indexing ratios obtained for each measurement field of view was calculated.
[0081] <Evaluation of Electrolyte Resistance during Overdischarge> Regarding the Ni-plated steel sheet, the multi-electrochemical measurement system HZ-Pro (model: HAG-PROM12, manufactured by Hokuto Denko Corporation) was used to evaluate the electrolyte resistance during over-discharge by the LSV (Linear Sweep Voltammetry) method. During the measurement, the measurement jig shown in Figure 7 was used. Figure 7 is a schematic diagram of the measurement jig used for evaluating the electrolyte resistance of the Ni-plated steel sheet by the LSV method. As shown in Figure 7, the Ni-plated steel sheet was attached to the bottom of the measurement jig, the electrolyte (1 mol / L LiPF6, EC:DEC (1:1 v / v%), manufactured by Kishida Chemical Co., Ltd.) was added into the jig, and metallic lithium (manufactured by Honjo Metal Co., Ltd.) was attached as the counter electrode and reference electrode to the upper electrode of the jig. The surface area of the measurement surface was 1.04 cm 2 and the surface areas of the counter electrode and reference electrode were 1.2 cm 2 . The distance between the reference electrode and the working electrode was set to 2 mm, the distance between the counter electrode and the working electrode was set to 2 mm, and the distance between the counter electrode and the reference electrode was set to 12 mm. The measurement was carried out in a dry room with a dew point of -40°C or lower and a room temperature of 25°C. Polarization was performed from the open-circuit potential at a scanning rate of 2 mV / second to +4.1 V (vsLi / Li + ) equivalent to over-discharge, and the current density (nA / cm 2 ) at 4.1 V was measured to evaluate the electrolyte resistance of the Ni-plated steel sheet during over-discharge. The smaller the current density, the less the elution of Fe and the better the electrolyte resistance during over-discharge.
[0082] <<Example 1>> As the substrate, a cold-rolled steel sheet of low-carbon aluminum-killed steel with a thickness of 0.3 mm was prepared.
[0083] Then, for the prepared steel sheet, after performing alkaline electrolytic degreasing and pickling by sulfuric acid immersion, electroplating (Ni plating) was carried out under the following conditions using a Ni plating bath with the following bath composition, and a Ni plating layer with a Ni deposition amount W of 0.87 g / m 2 was formed on the surface of the steel sheet. <Ni Plating Conditions> Bath composition: Nickel sulfate hexahydrate 250 g / L, Nickel chloride hexahydrate 45 g / L, Boric acid 30 g / L pH: 4.0 - 5.0 Bath temperature: 60℃ Current density: 10A / dm 2
[0084] Next, the steel sheet on which the Ni plating layer was formed (plated steel sheet) was subjected to thermal diffusion treatment by continuous annealing in a reducing protective gas atmosphere to form an Fe-Ni diffusion layer, and further, after the thermal diffusion treatment, temper rolling was performed at a rolling reduction rate of 3% or less to obtain a Ni-plated steel sheet. In the continuous annealing, in the initial heating step, the plated steel sheet was heated from room temperature to the final heating start temperature. The final heating start temperature was set within a temperature range of 660 to 694°C. The maximum heating rate (maximum heating rate) in the initial heating step was 4.96°C / sec. Next, in the final heating step, the reaching temperature was set within a temperature range of 695 to 729°C so that the difference between the final heating start temperature and the final heating reaching temperature (temperature difference in the final heating step) was 40°C, and the plated steel sheet was heated at a heating rate of 0.37°C / sec. Next, in the cooling step, the plated steel sheet was cooled to a temperature of 120°C or less by spraying a cooling gas such as HNX gas. The thermal history Y applied to the Ni-plated steel sheet through the initial heating process, the final heating process, and the cooling process was 57,920°C·s.
[0085] The obtained Ni-plated steel sheets were subjected to various evaluations according to the above-mentioned methods, and the results are shown in Tables 1 and 2.
[0086] <<Examples 2 to 8, Comparative Examples 1 to 5>> Ni-plated steel sheets were obtained by changing the type of substrate, the amount of Ni plating, the thermal history Y in the thermal diffusion treatment, and the heat treatment conditions, i.e., the maximum heating rate, the final heating start temperature, the heating rate in the final heating step, the final heating temperature and the temperature difference in the final heating step, and the final heating time, as shown in Table 1, and were evaluated in the same manner. The results are shown in Tables 1 and 2.
[0087] [Table 1]
[0088] [Table 2]
[0089] As shown in Table 1, Ni-plated steel sheets having an average crystal grain size of 0.32 μm or more obtained by EBSD measurement and having a ratio of the region indexable by Fe of 0.0% to 6.0% had a small current density caused by the dissolution of Fe at 4.1 V, which corresponds to overdischarge, and had excellent electrolyte resistance during overdischarge (Examples 1-8).
[0090] In addition, Ni-plated steel sheets having an average crystal grain size of 0.36 μm or more obtained by EBSD measurement and having a ratio of the area indexable by Fe of 0.0% to 1.0% inclusive, had a relatively small current density caused by the dissolution of Fe at 4.1 V, which corresponds to overdischarge, and were particularly excellent in electrolyte resistance during overdischarge (Examples 1-6).
[0091] On the other hand, the Ni-plated steel sheet of Comparative Example 1, which had a small thermal history Y in the thermal diffusion treatment and an average crystal grain size of less than 0.32 μm, had poor electrolyte resistance during overdischarge. The Ni-plated steel sheets of Comparative Examples 2 and 3, which had a small W / Y ratio in the thermal diffusion treatment and an Fe indexing ratio of more than 6.0%, and the Ni-plated steel sheets of Comparative Examples 4 and 5, which had a large maximum heating rate and were soaked without final heating, and therefore had an Fe indexing ratio of more than 6.0%, had poor electrolyte resistance during overdischarge.
Claims
1. A steel plate, A Ni-plated steel sheet having an Fe—Ni diffusion layer formed on at least one surface of the steel sheet, The Ni-plated steel sheet has an average crystal grain size of 0.32 μm or more as measured by EBSD on the outermost surface of the Ni-plated steel sheet, and a ratio of a region that can be indexed with Fe is 0.0% or more and 6.0% or less.
2. The Ni coating weight per one side of the Ni-plated steel sheet is 0.8 to 8.9 g / m 2 The Ni-plated steel sheet according to claim 1 .
3. A Ni layer is formed on the Fe—Ni diffusion layer, The Ni-plated steel sheet according to claim 2, wherein a ratio of the region that can be indexed with Fe obtained by EBSD measurement on the outermost surface of the Ni-plated steel sheet is 0.0% or more and 1.0% or less.
4. The Ni-plated steel sheet according to claim 1 or 3, wherein the thickness of the steel sheet is 0.03 to 1.5 mm.
5. The Ni-plated steel sheet according to claim 1 or 3, wherein the steel sheet is a low carbon steel or an ultra-low carbon steel.
6. A battery container comprising the Ni-plated steel sheet according to claim 1 or 3.
Citation Information
Patent Citations
Surface-treated steel plate for cell container
WO2017094919A1
Ni-plated steel sheet and method for manufacturing ni-plated steel sheet
WO2020137887A1
Surface-treated steel plate for battery container, battery container and battery
JP2014047359A
Cited By
Plated steel sheet and manufacturing method therefor
WO2026134978A1