Polyol liquid for filling, polyurethane composition for filling, and polyurethane foam
The polyol liquid agent with a reaction retarder and flame retardants addresses density and flame retardancy issues in polyurethane foams, ensuring uniform filling and improved structural integrity.
Patent Information
- Application Number
- JP2023059649
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing polyurethane foams used for filling cavities in structures suffer from variations in density and poor flame retardancy due to uneven curing, especially near the filling port and at the cavity's end.
A polyol liquid agent containing a polyol, catalyst, reaction retarder, and filler, which controls curing time and density variation by using a reaction retarder such as hydroxycarboxylic acids or acid block catalysts, along with flame retardants like red phosphorus and boron-containing compounds.
The solution provides polyurethane foams with consistent density and excellent flame retardancy throughout the cavity, ensuring uniform filling and improved structural integrity.
Smart Images

Figure 2024146628000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a liquid filling polyol, a filling polyurethane composition containing the liquid polyol, and a polyurethane foam formed from the polyurethane composition. [Background technology]
[0002] Conventionally, polyurethane foams have been used as heat insulating materials in vehicles such as automobiles, building materials, etc. In general, polyurethane foams are formed by discharging and mixing a polyol liquid agent and a polyisocyanate liquid agent filled in separate containers. A polyol liquid often contains a blowing agent such as hydrofluoroolefin and a catalyst, and in this case, good storage stability is required so that the catalyst is not deactivated by the blowing agent during storage of the polyol liquid. For example, Patent Document 1 discloses a polyol composition for rigid polyurethane foams that contains a polyol compound, a catalyst, and at least 1-chloro-3,3,3-trifluoropropene as a blowing agent and has excellent storage stability. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-169337 A Summary of the Invention [Problem to be solved by the invention]
[0004] By the way, some polyurethane foams are formed in the cavity of a structure such as a panel or a flat deck in order to improve the insulation and flame retardancy of the structure. In this case, it is necessary to fill the cavity of the structure with a polyol liquid together with a polyisocyanate liquid. However, for example, when the above-mentioned polyol composition for rigid polyurethane foam is used, foam is formed near the filling port immediately after filling, and it may not be possible to fill the cavity to the end. Even if the polyurethane foam can be filled to a certain extent, the density of the polyurethane foam formed is significantly different between the filling port of the cavity and the end of the cavity, and there is a problem of high and low density depending on the location, which causes variations in quality such as insulation and flame retardancy.
[0005] Therefore, an object of the present invention is to provide a filling polyol liquid agent that has excellent filling properties when filling hollow spaces in a structure, and can form a polyurethane foam with little density variation from place to place and excellent flame retardancy. [Means for solving the problem]
[0006] As a result of extensive research, the present inventors have found that the above problems can be solved by controlling the curing time using a reaction retarder. That is, the present invention provides the following [1] to
[12] .
[0007] [1] A filling polyol liquid containing a polyol, a catalyst, a filler and a reaction retarder. [2] The filling polyol liquid according to [1], further comprising a foaming agent. [3] The filling polyol liquid according to [1] or [2], wherein the polyol comprises at least one selected from polyester polyols and polyether polyols. [4] The filling polyol liquid agent according to any one of [1] to [3], wherein the catalyst comprises a resinification catalyst and a trimerization catalyst. [5] The filling polyol liquid agent according to any one of [1] to [4], wherein the filler contains a solid flame retardant. [6] The filling polyol liquid according to any one of [1] to [5], further comprising a foam stabilizer. [7] The filling polyol liquid according to any one of [1] to [6], further comprising a settling inhibitor. [8] A filling polyurethane composition comprising the filling polyol liquid agent according to any one of [1] to [7] and a polyisocyanate liquid agent containing a polyisocyanate. [9] The filling polyurethane composition according to [8], which has a gel time of 4 to 60 seconds at a liquid temperature of 40°C.
[10] A polyurethane foam formed from the filling polyurethane composition according to [8] or [9].
[11] A method for producing a filling polyurethane composition, comprising mixing at least a polyol, a polyisocyanate, a catalyst, a filler, and a reaction retarder to obtain a filling polyurethane composition.
[12] A method for producing a filling polyurethane composition according to
[11] , comprising the steps of: mixing at least the polyol and the filler to obtain a mixed liquid; adding the catalyst and the reaction retarder to the obtained mixed liquid to obtain a polyol liquid; and mixing the obtained polyol liquid with a polyisocyanate liquid containing the polyisocyanate to obtain a filling polyurethane composition. Effect of the Invention
[0008] According to the present invention, it is possible to provide a filling polyol liquid agent which has excellent filling properties when filling hollow spaces in a structure, and can form a polyurethane foam having little density variation from place to place and excellent flame retardancy. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] [Filling polyol liquid] The filling polyol liquid of the present invention contains a polyol, a catalyst, a filler, and a reaction retarder. Here, filling means that it is used for the purpose of filling the cavity of a structure, unlike the use mode of forming polyurethane foam on the surface of a structure such as a fitting by spraying work on site. More specifically, it means that it is used for the purpose of filling the cavity inside the structure as a finished product by providing an injection port, or for the purpose of filling the cavity of an unfinished structure in the manufacturing stage of the structure as a part of the manufacturing process (part of the manufacturing line). The cavity of the structure has a certain shape, and when filling the cavity with a polyurethane composition containing a polyol liquid and a polyisocyanate liquid, the polyol composition is filled from the vicinity of the filling port along the inner wall of the cavity toward the end of the cavity, and foams and hardens to form a polyurethane foam corresponding to the shape of the cavity. The filling polyol liquid of the present invention has excellent filling properties when filling the cavity of the structure together with the polyisocyanate liquid, and can form a polyurethane foam with little variation in density from place to place.
[0010] [Reaction retarder] The filling polyol liquid of the present invention contains a reaction retarder. By containing the reaction retarder, the curing time when the polyurethane foam is formed can be controlled, and the polyurethane foam can be formed with excellent filling properties when filling the hollow part of the structure and with little variation in density depending on the location. The reaction retarder preferably has an acid component, and more preferably is at least one selected from carboxylic acids and acid blocking catalysts. When the reaction retarder has an acid component, it becomes easier to control the curing time when the polyurethane foam is formed. Although the principle by which the curing time is controlled by the reaction retarder is unclear, it is presumed that the acid component in the reaction retarder blocks the amine catalyst described below, slowing down the rate of the curing reaction between the polyol and the polyisocyanate. The reaction retarder may be contained alone or in combination of two or more kinds.
[0011] As the carboxylic acid, a hydroxycarboxylic acid compound or a carboxylic acid having no hydroxyl group can be used, but it is preferable to use a hydroxycarboxylic acid compound, which is more likely to inhibit the reaction by reacting with the polyisocyanate described later due to the hydroxyl group. Hydroxycarboxylic acid compounds are compounds having a hydroxyl group and a carboxyl group. Specific examples of hydroxycarboxylic acid compounds include aliphatic hydroxycarboxylic acid compounds such as lactic acid, glycolic acid, 2-hydroxybutyric acid, and 3-hydroxybutyric acid, and aromatic hydroxycarboxylic acid compounds such as salicylic acid, coumaric acid, mandelic acid, benzilic acid, atrolactic acid, ferulic acid, sinapic acid, vanillic acid, and 4-hydroxybenzoic acid. As the hydroxycarboxylic acid compound, a reaction product obtained by esterification reaction of a divalent carboxylic acid component and a dihydric alcohol component can also be used. Such a reaction product preferably has one hydroxyl group and one carboxyl group. Examples of the divalent carboxylic acid component include phthalic acid, phthalic anhydride, isophthalic acid, and terephthalic acid. Examples of the dihydric alcohol component include ethylene glycol, diethylene glycol, and triethylene glycol. The divalent carboxylic acid component and the dihydric alcohol component may each be used alone or in combination of two or more. The hydroxycarboxylic acid compound preferably has one hydroxyl group, and more preferably has one hydroxyl group and one carboxyl group.
[0012] As the carboxylic acid without a hydroxyl group, an aliphatic carboxylic acid or a carboxylic acid having an aromatic ring can be used. The aliphatic carboxylic acid is not particularly limited, and may be saturated or unsaturated, and may be linear or branched. Examples of the aliphatic carboxylic acid include an aliphatic carboxylic acid having an aliphatic hydrocarbon group having 1 to 10 carbon atoms, such as formic acid, acetic acid, propionic acid, butyric acid, and valeric acid. Examples of the carboxylic acid having an aromatic ring include a carboxylic acid having a monocyclic (non-polycyclic) aromatic ring and a carboxylic acid having a polycyclic aromatic ring. Examples of carboxylic acids having a monocyclic (non-polycyclic) aromatic ring include benzoic acid, phthalic acid (orthophthalic acid, isophthalic acid, terephthalic acid), etc. Examples of carboxylic acids having a polycyclic aromatic ring include naphthoic acid, etc. As the carboxylic acid not having a hydroxyl group, among those mentioned above, it is preferable to use an aliphatic carboxylic acid having an aliphatic hydrocarbon group having 1 to 10 carbon atoms, and it is more preferable to use formic acid.
[0013] As described above, an acid-blocked catalyst can also be used as a reaction retarder. The activity of the acid-blocked catalyst is low at low temperatures, and increases with increasing temperature. Specifically, in the initial stage of the curing reaction of polyol and polyisocyanate, the carboxylic acid blocks the activity of the amine, so that the reaction rate is suppressed. After that, the acid block is removed with the increase in temperature due to the reaction heat of the curing reaction, and the original activity of the amine is expressed, and the curing reaction is promoted.
[0014] As the acid blocking catalyst, it is preferable to use an amino compound blocked with a carboxylic acid. As the carboxylic acid, the above-mentioned ones can be suitably used, but it is preferable to use formic acid.
[0015] Examples of the amino compound include aliphatic amines and aromatic amines. The amine compound is preferably a tertiary amine, and more preferably a tertiary aliphatic amine. Examples of the amino compound include those having about 6 to 18 carbon atoms. Specifically, triethylamine, N-methylmorpholine bis(2-dimethylaminoethyl) ether, N,N,N',N",N"-pentamethyldiethylenetriamine, N,N,N'-trimethylaminoethyl-ethanolamine, bis(2-dimethylaminoethyl) ether, N-methyl-N',N'-dimethylaminoethylpiperazine, N,N-dimethylcyclohexylamine, diazabicycloundecene, diazabicyclononene, trimethylaminoethylpiperazine, tripropylamine, bisdiethylaminoethyl ether, and the like can be used. Among these, tertiary aliphatic amines having multiple nitrogen atoms are preferred, and among these, it is preferable to use at least one selected from N,N,N',N",N"-pentamethyldiethylenetriamine, diazabicycloundecene, diazabicyclononene, triethylenediamine, and bisdiethylaminoethyl ether, and it is more preferable to use N,N,N',N",N"-pentamethyldiethylenetriamine.
[0016] In the present invention, it is preferable to use at least one selected from a hydroxycarboxylic acid compound and an acid blocking catalyst as the reaction retarder, more preferably to use at least one selected from a hydroxycarboxylic acid compound and a formic acid blocking catalyst, and even more preferably to use a hydroxycarboxylic acid compound. When these substances are used as reaction retarders, it is easy to suppress the density variation of the polyurethane foam and to impart excellent flame retardancy to the polyurethane foam. In addition, since the molecular weight of the reaction retarder is increased overall, it is easy to improve the storage stability of the polyol liquid.
[0017] The content of the reaction retarder is preferably 0.1 to 10 parts by mass, more preferably 0.3 to 7 parts by mass, and even more preferably 0.5 to 4 parts by mass, relative to 100 parts by mass of polyol. When the content of the reaction retarder is equal to or greater than the lower limit, it is easy to impart excellent filling properties to the polyol liquid. When the content of the reaction retarder is equal to or less than the upper limit, the rate of the curing reaction between the polyol and the polyisocyanate is guaranteed to be at a certain level or higher, so that the density of the polyurethane foam to be filled becomes appropriate, and it is easy to impart excellent flame retardancy to the polyurethane foam.
[0018] [Polyol] The polyol contained in the polyol liquid is a compound having two or more hydroxyl groups. As the polyol, any polyol other than the reaction retarder may be used, specifically, any polyol having no carboxyl group may be used. In the present invention, examples of the polyol include polyester polyol, polyether polyol, polylactone polyol, polycarbonate polyol, and polymer polyol. The polyol preferably includes at least one selected from polyester polyol and polyether polyol, and more preferably includes polyester polyol.
[0019] <Polyester polyol> Examples of polyester polyols include aromatic polyester polyols and aliphatic polyester polyols, but when considering the flame retardancy of the resulting polyurethane foam, it is preferable to use aromatic polyester polyols. The aromatic polyester polyol is preferably a condensate of an aromatic dicarboxylic acid such as o-phthalic acid (phthalic acid), m-phthalic acid (isophthalic acid), p-phthalic acid (terephthalic acid), or naphthalenedicarboxylic acid with a glycol. Among them, the polyol preferably contains a phthalic acid-based polyester polyol, which is a condensate of phthalic acid and a glycol, and more preferably contains a p-phthalic acid-based polyester polyol, which is a condensate of p-phthalic acid and a glycol. The glycol is not particularly limited, but it is preferable to use low molecular weight aliphatic glycols known as components of polyester polyols, such as ethylene glycol, propylene glycol, and diethylene glycol.
[0020] The content of the aromatic polyester polyol is preferably 50 parts by mass or more, more preferably 70 parts by mass or more, even more preferably 90 parts by mass or more, and still more preferably 100 parts by mass, based on 100 parts by mass of the polyol. As described above, the aromatic polyester polyol is preferably a phthalic acid-based polyester polyol, and therefore, an embodiment in which the content of the phthalic acid-based polyester polyol is within the above range is more preferable.
[0021] The hydroxyl value of the polyester polyol is preferably from 100 to 400 mgKOH / g, more preferably from 150 to 350 mgKOH / g, and further preferably from 170 to 280 mgKOH / g.
[0022] <Polyether polyol> Polyether polyol is a polyoxyalkylene polyol obtained by ring-opening addition polymerization of an alkylene oxide to an initiator having two or more active hydrogen atoms. Specific examples of the initiator include aliphatic polyhydric alcohols (e.g., glycols such as ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, 1,4-butanediol, 1,3-butanediol, 1,6-hexanediol, neopentyl glycol, cyclohexylene glycol, and cyclohexanedimethanol, triols such as trimethylolpropane and glycerin, tetrafunctional alcohols such as pentaerythritol, and highly functional alcohols such as sucrose and sorbitol), aliphatic amines (e.g., alkylenediamines such as ethylenediamine, propylenediamine, butylenediamine, hexamethylenediamine, and neopentyldiamine, and alkanolamines such as monoethanolamine and diethanolamine), and aromatic amines (e.g., aniline, tolylenediamine, xylylenediamine, diphenylmethanediamine, and Mannich condensation products). These may be used alone or in combination of two or more.
[0023] The polyether polyol is preferably a tolylenediamine-based polyether polyol, a Mannich-based polyether polyol, a sucrose-based polyether polyol, a sorbitol-based polyether polyol, or an ethylenediamine-based polyether polyol. These polyether polyols may be used alone or in combination of two or more.
[0024] The tolylenediamine-based polyether polyol is a polyether polyol obtained by using tolylenediamine as an initiator. The same applies to sucrose-based polyether polyol, sorbitol-based polyether polyol, and ethylenediamine-based polyether polyol. The Mannich polyether polyol is a polyether polyol obtained by utilizing the Mannich reaction, which is a Mannich condensation product having two or more hydroxyl groups in the molecule, or an alkylene oxide added to such a Mannich condensation product. More specifically, it is a Mannich condensation product obtained by the Mannich reaction of at least one of phenol and its alkyl-substituted derivatives, formaldehyde and alkanolamine, or a polyether polyol obtained by ring-opening addition polymerization of at least one of ethylene oxide and propylene oxide to this compound.
[0025] The hydroxyl value of the polyether polyol is preferably from 200 to 1,000 mgKOH / g, more preferably from 250 to 800 mgKOH / g, and further preferably from 300 to 500 mgKOH / g. The hydroxyl value is a value measured in accordance with JIS K1557-1:2007.
[0026] Examples of the polylactone polyol include polypropiolactone glycol, polycaprolactone glycol, and polyvalerolactone glycol. Examples of polycarbonate polyols include polyols obtained by dealcoholization reaction of hydroxyl group-containing compounds such as ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, octanediol, and nonanediol with ethylene carbonate, propylene carbonate, and the like.
[0027] Examples of the polymer polyol include polymers obtained by graft polymerizing an ethylenically unsaturated compound such as acrylonitrile, styrene, methyl acrylate, or methacrylate with an aromatic polyol, an alicyclic polyol, an aliphatic polyol, or a polyester polyol, or polybutadiene polyol, or hydrogenated products thereof.
[0028] [catalyst] The filling polyol liquid agent of the present invention (hereinafter also simply referred to as polyol liquid agent) contains a catalyst. Examples of the catalyst include a resinification catalyst and a trimerization catalyst. From the viewpoint of appropriately progressing the urethanization reaction and the trimerization reaction and obtaining a polyurethane foam having excellent flame retardancy, it is preferable that the catalyst contains both a resinification catalyst and a trimerization catalyst.
[0029] <Resinification catalyst> The resinification catalyst is a catalyst that promotes the reaction between polyol and polyisocyanate. Examples of the resinification catalyst include amine catalysts such as imidazole compounds and piperazine compounds, and metal catalysts. When using an amine catalyst, it is preferable to use one other than the above-mentioned reaction retarder, more specifically, it is preferable to use an amine catalyst other than the above-mentioned acid block catalyst. The amine catalyst may be the same as or different from the amino compound that can generate the acid block catalyst. Examples of the imidazole compound include tertiary amines in which the secondary amine at the 1-position of the imidazole ring is substituted with an alkyl group, an alkenyl group, or the like. Specific examples include N-methylimidazole, 1,2-dimethylimidazole, 1-ethyl-2-methylimidazole, 1-methyl-2-ethylimidazole, 1,2-diethylimidazole, and 1-isobutyl-2-methylimidazole. In addition, examples include imidazole compounds in which the secondary amine in the imidazole ring is substituted with a cyanoethyl group. Furthermore, examples of the piperazine compound include tertiary amines such as N-methyl-N',N'-dimethylaminoethylpiperazine and trimethylaminoethylpiperazine. Examples of the amine catalyst include, in addition to imidazole compounds and piperazine compounds, various tertiary amines such as pentamethyldiethylenetriamine, triethylamine, N-methylmorpholinebis(2-dimethylaminoethyl)ether, N,N,N',N",N"-pentamethyldiethylenetriamine, N,N,N'-trimethylaminoethyl-ethanolamine, bis(2-dimethylaminoethyl)ether, N,N-dimethylcyclohexylamine, diazabicycloundecene, triethylenediamine, tetramethylhexamethylenediamine, and tripropylamine.
[0030] Examples of the metal catalyst include metal salts of lead, tin, bismuth, copper, zinc, cobalt, nickel, etc., and preferably organic acid metal salts of lead, tin, bismuth, copper, zinc, cobalt, nickel, etc. More preferred are organic acid tin salts such as dibutyltin dilaurate, dioctyltin dilaurate, dioctyltin versatate, and organic acid bismuth salts such as bismuth trioctate, bismuth tris(2-ethylhexanoate), and among these, organic acid bismuth salts are preferred. The resinification catalyst may be used alone or in combination of two or more. The resinification catalyst is preferably at least one selected from amine-based catalysts and metal-based catalysts, and among them, amine-based catalysts are more preferable from the viewpoint of controlling the reaction rate by a reaction retarder and easily suppressing the variation in density of the polyurethane foam.
[0031] The content of the resinification catalyst in the polyol liquid is preferably 0.1 to 15 parts by mass, more preferably 0.3 to 10 parts by mass, and even more preferably 0.5 to 8 parts by mass, based on 100 parts by mass of the polyol. When the content of the resinification catalyst is in such a range, the reaction between the polyol and the isocyanate tends to proceed appropriately. In addition, when the resinification catalyst and the trimerization catalyst are used in combination, the content of the resinification catalyst is set to the above range, and the content of the trimerization catalyst is adjusted to a predetermined range described later, thereby improving the filling property of the polyurethane composition into the cavity of the structure, and improving the physical properties such as flame retardancy of the polyurethane foam formed.
[0032] <Trimerization catalyst> The trimerization catalyst is a catalyst that reacts the isocyanate group contained in the polyisocyanate to trimerize it and promote the formation of an isocyanurate ring. As the trimerization catalyst, it is preferable to use one other than the above-mentioned reaction retarder, and it is preferable to use a trimerization catalyst other than the above-mentioned acid block catalyst. Specifically, nitrogen-containing aromatic compounds such as tris(dimethylaminomethyl)phenol, 2,4-bis(dimethylaminomethyl)phenol, and 2,4,6-tris(dialkylaminoalkyl)hexahydro-S-triazine, carboxylic acid alkali metal salts such as potassium acetate, potassium 2-ethylhexanoate, and potassium octylate, tertiary ammonium salts such as trimethylammonium salt, triethylammonium salt, and triphenylammonium salt, and quaternary ammonium salts such as tetramethylammonium salt, tetraethylammonium salt, tetraphenylammonium salt, and triethylmonomethylammonium salt can be used. The trimerization catalyst may be used alone or in combination of two or more. As the trimerization catalyst, an alkali metal carboxylate is preferred, and potassium 2-ethylhexanoate is more preferred.
[0033] The content of the trimerization catalyst is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 8 parts by mass, and even more preferably 1 to 5 parts by mass, based on 100 parts by mass of the polyol. When the content of the trimerization catalyst is within such a range, the trimerization reaction can be appropriately promoted. In addition, when the resinification catalyst and the trimerization catalyst are used in combination, the content of the resinification catalyst and the content of the trimerization catalyst are adjusted to the above-mentioned predetermined ranges, respectively, to improve the filling property of the polyurethane composition into the hollow part of the structure, and the physical properties such as flame retardancy of the polyurethane foam formed are also improved.
[0034] The polyol liquid of the present invention preferably has a catalyst content of 0.3 to 5 mass%, more preferably 0.4 to 4 mass%, and even more preferably 0.6 to 3.5 mass%. When the catalyst content is equal to or greater than the lower limit, the reaction between the polyol and the polyisocyanate is sufficient, and it is easy to obtain a polyurethane foam having excellent flame retardancy. When the catalyst content is equal to or less than the upper limit, the reactivity between the polyol and the polyisocyanate is appropriate, and when the polyurethane composition is filled into the hollow part of the structure, a polyurethane foam is formed in a short time near the filling port, making it easy to fill the entire hollow part of the structure with the composition, and making it easy to suppress the variation in density of the polyurethane foam. The amount of the catalyst described above is the amount of the catalyst itself based on the total amount of the polyol liquid.For example, catalysts are often sold as products by dissolving them in a solvent, and in this case, the content of the catalyst of the present invention does not include the amount of the solvent in which the catalyst is dissolved, but means the amount of the catalyst itself dissolved in the solvent.
[0035] [Filler] The polyol liquid contains a filler. By containing the filler, it is possible to impart a function to the polyurethane foam according to the type of filler. The filler preferably contains a flame retardant. By using the flame retardant as a filler, it is possible to impart high flame retardant performance to the polyurethane foam. The flame retardant used as the filler is a solid flame retardant. In the present invention, the use of a solid flame retardant can more effectively improve flame retardancy. The solid flame retardant is a flame retardant that is solid at room temperature (23°C) and normal pressure (1 atm).
[0036] From the viewpoint of more effectively enhancing flame retardancy, the solid flame retardant is preferably at least one selected from the group consisting of red phosphorus-based flame retardants, boron-containing flame retardants, bromine-containing flame retardants, phosphate-containing flame retardants, chlorine-containing flame retardants, antimony-containing flame retardants, metal hydroxides, and needle-shaped fillers.
[0037] <Red phosphorus flame retardant> The red phosphorus-based flame retardant may be made of red phosphorus alone, may be red phosphorus coated with a resin, a metal hydroxide, a metal oxide, or may be red phosphorus mixed with a resin, a metal hydroxide, a metal oxide, or the like. The resin that coats the red phosphorus or mixes with the red phosphorus is not particularly limited, but examples thereof include thermosetting resins such as phenol resin, epoxy resin, unsaturated polyester resin, melamine resin, urea resin, aniline resin, and silicone resin. From the viewpoint of flame retardancy, metal hydroxide is preferable as the compound to be coated or mixed. The metal hydroxide to be used may be appropriately selected from those described later.
[0038] The amount of the red phosphorus-based flame retardant is preferably 3 to 60 parts by mass, more preferably 10 to 50 parts by mass, and even more preferably 20 to 45 parts by mass, relative to 100 parts by mass of the polyol. By making the amount of the red phosphorus-based flame retardant equal to or greater than these lower limits, the effect of containing the red phosphorus-based flame retardant is easily exhibited. On the other hand, by making the amount equal to or less than the upper limits, foaming is not inhibited by the red phosphorus-based flame retardant.
[0039] <Boron-containing flame retardants> Examples of boron-containing flame retardants include borax, boron oxide, boric acid, borates, etc. Examples of boron oxide include diboron trioxide, boron trioxide, diboron dioxide, tetraboron trioxide, and tetraboron pentoxide. Examples of borates include borates of alkali metals, alkaline earth metals, elements of Groups 4, 12, and 13 of the periodic table, and ammonium. Specific examples include alkali metal borates such as lithium borate, sodium borate, potassium borate, and cesium borate, alkaline earth metal borates such as magnesium borate, calcium borate, and barium borate, zirconium borate, zinc borate, aluminum borate, and ammonium borate. The boron-containing flame retardants may be used alone or in combination of two or more kinds. Preferably, the boron-containing flame retardant is a borate, more preferably zinc borate.
[0040] The amount of the boron-containing flame retardant is not particularly limited, but is preferably 3 to 45 parts by mass, more preferably 5 to 40 parts by mass, and even more preferably 10 to 25 parts by mass, relative to 100 parts by mass of the polyol. By making the amount of the boron-containing flame retardant equal to or more than these lower limits, the effect of the boron-containing flame retardant is easily exhibited, and flame retardancy is improved. On the other hand, by making the amount equal to or less than the upper limits, foaming is not inhibited by the boron-containing flame retardant.
[0041] <Bromine-containing flame retardants> The bromine-containing flame retardant is not particularly limited as long as it contains bromine in its molecular structure and is a solid at room temperature and pressure. Examples of the bromine-containing flame retardant include brominated aromatic ring-containing aromatic compounds. Examples of the brominated aromatic ring-containing aromatic compound include monomeric organic bromine compounds such as hexabromobenzene, pentabromotoluene, hexabromobiphenyl, decabromobiphenyl, decabromodiphenyl ether, octabromodiphenyl ether, hexabromodiphenyl ether, bis(pentabromophenoxy)ethane, ethylene bis(pentabromophenyl), ethylene bis(tetrabromophthalimide), and tetrabromobisphenol A.
[0042] In addition, the brominated aromatic ring-containing aromatic compound may be a bromine compound polymer.Specific examples include brominated polycarbonates such as polycarbonate oligomers produced from brominated bisphenol A as a raw material, copolymers of this polycarbonate oligomer and bisphenol A, and diepoxy compounds produced by the reaction of brominated bisphenol A and epichlorohydrin.Furthermore, examples include brominated epoxy compounds such as monoepoxy compounds obtained by the reaction of brominated phenols and epichlorohydrin, poly(brominated benzyl acrylate), brominated phenol condensates of brominated polyphenylene ether, brominated bisphenol A, and cyanuric chloride, brominated (polystyrene), poly(brominated styrene), brominated polystyrene such as crosslinked brominated polystyrene, crosslinked or non-crosslinked brominated poly(-methylstyrene), and the like. In addition, compounds other than brominated aromatic ring-containing aromatic compounds such as hexabromocyclododecane may be used. These bromine-containing flame retardants may be used alone or in combination of two or more. Among the above, brominated aromatic ring-containing aromatic compounds are preferred, and among them, monomeric organic bromine compounds such as ethylenebis(pentabromophenyl) are preferred.
[0043] The amount of the bromine-containing flame retardant is preferably 3 to 60 parts by mass, more preferably 10 to 50 parts by mass, and even more preferably 20 to 45 parts by mass, based on 100 parts by mass of the polyol. By making the amount of the bromine-containing flame retardant equal to or greater than these lower limits, the effect of the inclusion of the bromine-containing flame retardant is easily exhibited. On the other hand, by making the amount equal to or less than the upper limits, foaming is not inhibited by the bromine-containing flame retardant.
[0044] <Phosphate-containing flame retardants> Examples of the phosphate-containing flame retardant include phosphates consisting of salts of various phosphoric acids and at least one metal or compound selected from metals in Groups IA to IVB of the periodic table, ammonia, aliphatic amines, aromatic amines, and heterocyclic compounds containing nitrogen in the ring. The phosphoric acid is not particularly limited, but examples thereof include monophosphoric acid, pyrophosphoric acid, and polyphosphoric acid. Examples of metals in Groups IA to IVB of the periodic table include lithium, sodium, calcium, barium, iron (II), iron (III), and aluminum. Examples of the aliphatic amine include methylamine, ethylamine, diethylamine, triethylamine, ethylenediamine, piperazine, etc. Examples of the aromatic amine include aniline, o-triidine, 2,4,6-trimethylaniline, anisidine, 3-(trifluoromethyl)aniline, etc. Examples of the heterocyclic compound containing nitrogen in the ring include pyridine, triazine, melamine, etc.
[0045] Specific examples of phosphate-containing flame retardants include monophosphates such as aluminum triphosphate, pyrophosphates, polyphosphates, etc. Here, the polyphosphates are not particularly limited, but include, for example, ammonium polyphosphate, piperazine polyphosphate, melamine polyphosphate, ammonium amide polyphosphate, aluminum polyphosphate, etc. The phosphate-containing flame retardant may be used alone or in combination of two or more of the above-mentioned compounds.
[0046] The amount of the phosphate-containing flame retardant is not particularly limited, but is 3 to 40 parts by mass, more preferably 5 to 35 parts by mass, and even more preferably 10 to 30 parts by mass, relative to 100 parts by mass of the polyol. By making the amount of the phosphate-containing flame retardant equal to or greater than these lower limits, the effect of the inclusion of the phosphate-containing flame retardant is easily exhibited. On the other hand, by making the amount equal to or less than the upper limits, foaming is not inhibited by the phosphate-containing flame retardant.
[0047] <Chlorine-containing flame retardants> Chlorine-containing flame retardants include those commonly used in flame-retardant resin compositions, such as polychlorinated naphthalenes, chlorendic acid, and dodecachlorododecahydrodimethanodibenzocyclooctene sold under the trade name "Dechlorane Plus." The blending amount of the chlorine-containing flame retardant is not particularly limited, but is preferably 3 to 40 parts by mass, more preferably 5 to 35 parts by mass, and even more preferably 10 to 30 parts by mass, relative to 100 parts by mass of the polyol. By making the blending amount of the chlorine-containing flame retardant equal to or more than these lower limit values, the effect of containing the chlorine-containing flame retardant is easily exhibited. On the other hand, by making it equal to or less than the upper limit values, foaming is not inhibited by the chlorine-containing flame retardant.
[0048] <Antimony-containing flame retardants> Examples of antimony-containing flame retardants include antimony oxide, antimony salts, and pyroantimony salts. Examples of antimony oxide include antimony trioxide and antimony pentoxide. Examples of antimony salts include sodium antimonate and potassium antimonate. Examples of pyroantimonate include sodium pyroantimonate and potassium pyroantimonate. The antimony-containing flame retardants may be used alone or in combination of two or more. The preferred antimony-containing flame retardant for use in the present invention is antimony trioxide.
[0049] The amount of the antimony-containing flame retardant is not particularly limited, but is preferably 1 to 40 parts by mass, more preferably 2 to 35 parts by mass, and even more preferably 3 to 30 parts by mass, relative to 100 parts by mass of the polyol. By making the amount of the antimony-containing flame retardant equal to or greater than these lower limits, the effect of the inclusion of the antimony-containing flame retardant is easily exhibited, and flame retardancy is improved. On the other hand, by making the amount equal to or less than the upper limits, foaming is not inhibited by the antimony-containing flame retardant.
[0050] <Metal hydroxide> Examples of metal hydroxides used in the present invention include magnesium hydroxide, calcium hydroxide, aluminum hydroxide, iron hydroxide, nickel hydroxide, zirconium hydroxide, titanium hydroxide, zinc hydroxide, copper hydroxide, vanadium hydroxide, tin hydroxide, etc. The metal hydroxides may be used alone or in combination of two or more kinds.
[0051] The amount of the metal hydroxide is, for example, 0.1 to 50 parts by mass, preferably 0.2 to 30 parts by mass, more preferably 0.3 to 20 parts by mass, and even more preferably 0.5 to 15 parts by mass, relative to 100 parts by mass of the polyol. By making the amount of the metal hydroxide equal to or more than these lower limits, the effect of the inclusion of the metal hydroxide is easily exhibited, and the flame retardancy is improved. On the other hand, by making the amount equal to or less than the upper limits, foaming is not inhibited by the metal hydroxide.
[0052] Of the above-mentioned solid flame retardants, red phosphorus-based flame retardants, boron-containing flame retardants, bromine-containing flame retardants, and the like are preferred. It is also preferable to use a plurality of solid flame retardants in combination. In this case, it is preferable to use a red phosphorus-based flame retardant, a boron-containing flame retardant, and a bromine-containing flame retardant in combination. By using these in combination, it is easier to further improve the flame retardancy.
[0053] <Solid flame retardant content> The amount of the solid flame retardant is not particularly limited, but is, for example, 10 to 150 parts by mass, preferably 20 to 120 parts by mass, and more preferably 40 to 80 parts by mass, relative to 100 parts by mass of the polyol. By making the amount of the solid flame retardant equal to or greater than these lower limits, it is possible to impart appropriate flame retardancy to the polyurethane foam. By making the amount of the solid flame retardant equal to or less than these upper limits, it becomes easier to fill the polyurethane composition inside the structure, and it becomes easier to obtain a polyurethane foam with less density difference depending on the location.
[0054] As the filler, an inorganic filler other than the above-mentioned flame retardant may be blended in. For example, an inorganic filler other than the flame retardant may be a needle-shaped filler.
[0055] <Needle filler> Examples of needle-like fillers include potassium titanate whiskers, aluminum borate whiskers, magnesium-containing whiskers, silicon-containing whiskers, wollastonite, sepiolite, zonolite, elestadite, boehmite, rod-shaped hydroxyapatite, glass fibers, carbon fibers, graphite fibers, metal fibers, slag fibers, gypsum fibers, silica fibers, alumina fibers, silica alumina fibers, zirconia fibers, boron nitride fibers, boron fibers, and stainless steel fibers. These needle-like fillers can be used alone or in combination of two or more.
[0056] The aspect ratio (length / diameter) of the needle-like filler used in the present invention is preferably in the range of 5 to 50, and more preferably in the range of 10 to 40. The aspect ratio can be determined by observing the needle-like filler with a scanning electron microscope and measuring its length and width.
[0057] The amount of the needle-like filler is not particularly limited, but is, for example, 10 to 100 parts by mass, preferably 20 to 90 parts by mass, more preferably 30 to 80 parts by mass, and further preferably 40 to 70 parts by mass, relative to 100 parts by mass of the polyol. By making the amount of the needle-like filler equal to or greater than these lower limits, the shape of the polyurethane foam after combustion is easily maintained. On the other hand, by making the amount equal to or less than these upper limits, foaming is less likely to be hindered by the needle-like filler.
[0058] Inorganic fillers other than needle-shaped fillers can also be used, and alumina, titanium oxide, calcium oxide, magnesium oxide, iron oxide, tin oxide, ferrites, basic magnesium carbonate, calcium carbonate, magnesium carbonate, zinc carbonate, barium carbonate, dawsonite, hydrotalcite, calcium sulfate, barium sulfate, calcium silicate, talc, mica, montmorillonite, bentonite, activated clay, imogolite, sericite, glass beads, aluminum nitride, boron nitride, silicon nitride, various metal powders, magnesium sulfate, lead zirconate titanate, molybdenum sulfide, silicon carbide, various magnetic powders, fly ash, etc. can be appropriately used. The inorganic fillers may be used alone or in combination of two or more.
[0059] The content of the filler in the polyol liquid is, for example, 10 to 200 parts by mass, preferably 20 to 130 parts by mass, and more preferably 40 to 80 parts by mass, relative to 100 parts by mass of the polyol. By making the amount of the filler blended equal to or greater than these lower limits, it becomes easier to impart a function to the polyurethane foam according to the type of filler. By making the amount of the filler blended equal to or less than these upper limits, it becomes easier to fill the polyurethane composition inside the structure, and it becomes easier to obtain a polyurethane foam with less density difference depending on the location.
[0060] [Liquid flame retardant] The polyol liquid may contain a liquid flame retardant. A liquid flame retardant is a flame retardant that is liquid at room temperature (23°C) and normal pressure (1 atm). A specific example of a liquid flame retardant is a phosphoric acid ester. Unlike solid flame retardants, liquid flame retardants are less likely to produce precipitation during storage and are easy to handle.
[0061] As the phosphoric acid ester, it is preferable to use a monophosphoric acid ester, a condensed phosphoric acid ester, etc. Examples of the monophosphoric acid ester include trialkyl phosphates such as trimethyl phosphate, triethyl phosphate, tributyl phosphate, and tri(2-ethylhexyl)phosphate, halogen-containing phosphoric acid esters such as tris(β-chloropropyl)phosphate, trialkoxy phosphates such as tributoxyethyl phosphate, aromatic ring-containing phosphoric acid esters such as tricresyl phosphate, trixylenyl phosphate, tris(isopropylphenyl)phosphate, cresyl diphenyl phosphate, and diphenyl(2-ethylhexyl)phosphate, and acidic phosphoric acid esters such as monoisodecyl phosphate and diisodecyl phosphate.
[0062] Examples of the condensed phosphate ester include aromatic condensed phosphate esters such as trialkyl polyphosphate, resorcinol polyphenyl phosphate, bisphenol A polycresyl phosphate, and bisphenol A polyphenyl phosphate. Commercially available condensed phosphate esters include, for example, "CR-733S", "CR-741", and "CR747" manufactured by Daihachi Chemical Industry Co., Ltd., and "ADEKA STAB PFR" and "FP-600" manufactured by ADEKA Corporation.
[0063] The liquid flame retardant may be one of the above-mentioned compounds, or two or more of them may be used in combination. Among them, from the viewpoint of facilitating the production of polyurethane foam and improving the flame retardancy of the polyurethane foam, monophosphate ester is preferred, and tris(β-chloropropyl)phosphate is more preferred.
[0064] When a liquid flame retardant is contained, the blending amount thereof is preferably from 5 to 80 parts by mass, more preferably from 10 to 70 parts by mass, and further preferably from 20 to 60 parts by mass, based on 100 parts by mass of the polyol.
[0065] [Settling inhibitor] The polyol liquid preferably contains a sedimentation inhibitor. The sedimentation inhibitor inhibits the precipitation of the filler dispersed in the polyol liquid during long-term storage at room temperature or low temperature. In addition, the settled filler does not cause caking, and even if the filler settles after long-term storage, the filler can be easily and uniformly dispersed by stirring with a stirrer or the like. The sedimentation inhibitor generally becomes solid at room temperature and normal pressure, and usually becomes a solid content (insoluble content) in the liquid.
[0066] The settling inhibitor is not particularly limited. Specific examples of the settling inhibitor include powdered silica, organic clay, carbon black, hydrogenated castor oil wax, fatty acid amide wax, etc. One or more of these may be used. As the powdered silica, fumed silica, colloidal silica, silica gel, etc. can be used. Among these, fumed silica is preferable, and hydrophobic fumed silica is particularly preferable. As the fumed silica, Aerosil (registered trademark) of Nippon Aerosil Co., Ltd. can be used. As the organoclay, organophilic phyllosilicates and the like can be used. The carbon black may be produced by a furnace method, a channel method, a thermal method, etc. The carbon black may be appropriately selected from commercially available products. Hydrogenated castor oil wax, fatty acid amide wax, etc. form a swollen gel structure in liquid. These are generally commercially available under names such as thixotropic agents, thickeners, anti-settling agents, and anti-sagging agents, and commercially available products can be appropriately selected and used.
[0067] The preferred settling inhibitor is a thickening agent, and more preferably contains Si as an element constituting the settling inhibitor. Specific examples of the thickening agent include fumed silica and organophilic phyllosilicate, and more preferably fumed silica.
[0068] When a sedimentation inhibitor is contained, its content is not particularly limited, but is, for example, 0.1 to 20 parts by mass, preferably 0.5 to 10 parts by mass, and more preferably 1 to 5 parts by mass, relative to 100 parts by mass of polyol. By making the content of the sedimentation inhibitor equal to or more than the lower limit, the polyol liquid is thickened, the sedimentation of the filler is suppressed, and the dispersibility of the filler can be improved. In addition, by making the content of the sedimentation inhibitor equal to or less than the upper limit, the viscosity of the liquid is prevented from becoming too high, which would cause a decrease in the ease of handling.
[0069] [Foaming agent] The polyol liquid of the present invention preferably contains a foaming agent. The foaming agent can be used to mix the polyol liquid and the polyisocyanate liquid and foam them to form a polyurethane foam. The foaming agent is contained in at least one of the polyol liquid and the polyisocyanate liquid described below, but is preferably contained in the polyol liquid. The foaming agent is not particularly limited, but examples thereof include organic foaming agents such as hydrocarbon compounds, chlorinated aliphatic hydrocarbon compounds, hydrofluorocarbons, hydrochlorofluorocarbon compounds, and hydrofluoroolefins, and inorganic foaming agents such as nitrogen gas, oxygen gas, argon gas, and carbon dioxide gas. Among these, it is preferable to use organic foaming agents.
[0070] Examples of the hydrocarbon compound include propane, butane, pentane, hexane, heptane, cyclopropane, cyclobutane, cyclopentane, cyclohexane, and cycloheptane. Examples of the chlorinated aliphatic hydrocarbon compounds include dichloroethane, propyl chloride, isopropyl chloride, butyl chloride, isobutyl chloride, pentyl chloride, and isopentyl chloride. Examples of the hydrofluorocarbon include CHF3, CH2F2, and CH3F.
[0071] Examples of the hydrochlorofluorocarbon compounds include dichloromonofluoroethane (for example, HCFC141b (1,1-dichloro-1-fluoroethane), HCFC22 (chlorodifluoromethane), HCFC142b (1-chloro-1,1-difluoroethane)), HFC-245fa (1,1,1,3,3-pentafluoropropane), and HFC-365mfc (1,1,1,3,3-pentafluorobutane).
[0072] The hydrofluoroolefin may be, for example, a fluoroalkene having a carbon number of 3 to 6. The hydrofluoroolefin may be a hydrochlorofluoroolefin having a chlorine atom, and therefore may be a chlorofluoroalkene having a carbon number of 3 to 6. The hydrofluoroolefin preferably has 3 or 4 carbon atoms. More specific examples include trifluoropropene, tetrafluoropropenes such as HFO-1234, pentafluoropropenes such as HFO-1225, chlorotrifluoropropenes such as HFO-1233, chlorodifluoropropene, chlorotrifluoropropene, and chlorotetrafluoropropene. More specifically, 1,3,3,3-tetrafluoropropene (HFO-1234ze), 1,1,3,3-tetrafluoropropene, 1,2,3,3,3-pentafluoropropene (HFO-1225ye), 1,1,1-trifluoropropene, 1,1,1,3,3-pentafluoropropene (HFO-1225zc), 1,1,1,3,3,3-hexafluorobut-2-ene, 1,1,2,3,3-pentafluoropropene (HFO-1225yc), 1,1,1,2,3-pentafluoropropene (HFO-1225yez), (E)-1-chloro-3,3,3-trifluoropropene (HFO-1233zd(E)), (Z)-1-chloro-3,3,3-trifluoropropene (HFO-1233zd(Z)), (Z)-1,1,1,4,4,4-hexafluorobut-2-ene (HFO-1336mzz(Z)), (E)-1,1,1,4,4,4-hexafluorobut-2-ene (HFO-1336mzz(E)), 2,3,3,3-tetrafluoropropene (HFO-1234yf), trifluoroethylene (HFO-1123), (E)-1-chloro-3,3,3-trifluoropropene (HCFO-1233zd(E)), (Z)-2,3,3,3-tetrafluoro-1-chloropropene (HCFO-1224yd(Z)), and the like.
[0073] From the viewpoints of good foam formation and reducing the environmental load, it is preferable to use a hydrofluoroolefin as the foaming agent.
[0074] The content of the blowing agent is preferably 15 to 90 parts by mass, more preferably 25 to 80 parts by mass, and even more preferably 30 to 70 parts by mass, based on 100 parts by mass of the polyol. When the content of the blowing agent is equal to or more than the lower limit, the foaming is promoted, the fluidity is increased, and the density of the resulting polyurethane foam can be reduced. On the other hand, when the content of the blowing agent is equal to or less than the upper limit, the foaming can be prevented from proceeding excessively.
[0075] [water] The polyol liquid may contain water, which improves foaming properties when forming a polyurethane foam. The amount of water to be added is, for example, 0.1 to 10 parts by mass, preferably 0.2 to 5 parts by mass, and more preferably 0.3 to 3 parts by mass, relative to 100 parts by mass of polyol. By setting the amount of water to be added within this range, the polyurethane composition can be easily foamed appropriately.
[0076] [Foam stabilizer] The polyol liquid preferably contains a foam stabilizer, which improves the foamability of the polyurethane composition obtained from the polyol liquid and the polyisocyanate liquid. Examples of the foam stabilizer include surfactants such as polyoxyalkylene-based foam stabilizers, such as polyoxyalkylene alkyl ethers, and silicone-based foam stabilizers, such as organopolysiloxanes. Among these, silicone-based foam stabilizers are preferred. These foam stabilizers may be used alone or in combination of two or more. The amount of the foam stabilizer is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 8 parts by mass, and even more preferably 1 to 5 parts by mass, based on 100 parts by mass of the polyol. When the amount of the foam stabilizer is equal to or greater than these lower limits, the polyurethane composition is easily foamed, and a homogeneous polyurethane foam is easily obtained. When the amount of the foam stabilizer is equal to or less than these upper limits, the balance between the production cost and the obtained effect is good.
[0077] [Other ingredients] The polyol liquid may contain one or more additives selected from additives such as phenol-based, amine-based, and sulfur-based antioxidants, heat stabilizers, metal damage inhibitors, antistatic agents, stabilizers, crosslinking agents, lubricants, softeners, pigments, and tackifying resins, tackifiers such as polybutene and petroleum resins, etc., as necessary, within the scope of the present invention.
[0078] <Undissolved components> The polyol liquid agent of the present invention contains a filler such as a solid flame retardant as described above, and contains a certain amount of insoluble components that do not dissolve in the polyol liquid agent. The mass fraction of the insoluble components in the polyol liquid agent of the present invention is preferably 3 to 25%. When the mass fraction of the insoluble components is 3% or more, various properties such as flame retardancy can be appropriately imparted to the polyurethane foam formed. In addition, when the mass fraction of the insoluble components is 25% or less, excellent fluidity can be easily imparted to the polyurethane composition. Therefore, when the polyurethane composition is filled into a structure having a hollow portion, the density of the polyurethane foam formed is unlikely to be high, and it is easy to adjust the density to a desired value. From the viewpoint of improving performance such as flame retardancy while also achieving excellent fluidity, the mass fraction of the undissolved components in the polyol liquid is preferably 5 to 23%, more preferably 8 to 22%, and even more preferably 10 to 20%.
[0079] The term "non-soluble components" refers to components that are not dissolved in the polyol liquid, and may be fillers, i.e., solid flame retardants, inorganic fillers other than solid flame retardants, etc. Therefore, the mass fraction of the non-soluble components can be adjusted by adjusting the blending amount of each of these components. The mass fraction of the undissolved components means the ratio of the undissolved components in the polyol liquid to the total amount of the polyol liquid, and is calculated by the following formula. Mass fraction (%) of undissolved components in polyol solution = [Amount of undissolved components in polyol solution (g) / Mass of polyol solution (g)] x 100 Here, the amount of undissolved components in the polyol solution is measured by filtering the polyol solution at room temperature (23° C.) using filter paper and drying the filtration residue (residue) on the filter paper. The filter paper used should have a particle retention capacity of 5 μm, and an example of such a filter paper is Advantec's "Circular Quantitative Filter Paper No. 3."
[0080] [Filling polyurethane composition] The filling polyurethane composition of the present invention (hereinafter, simply referred to as polyurethane composition) contains the above-mentioned polyol liquid agent and polyisocyanate liquid agent. The polyurethane foam of the present invention is formed from the polyurethane composition. Specifically, it is a reaction product obtained by reacting and foaming a polyurethane composition obtained by mixing a polyol liquid agent and a polyisocyanate liquid agent. The polyurethane composition used in the present invention is generally a two-liquid type, and it is preferable to mix the polyol liquid of the present invention and the polyisocyanate liquid, which are stored separately, and react and foam to obtain a polyurethane foam. Note that the polyisocyanate liquid may contain components other than polyisocyanate, such as the above-mentioned filler, blowing agent, catalyst, and other components, as necessary.
[0081] (Polyisocyanate) The polyisocyanate liquid agent contains a polyisocyanate. As the polyisocyanate, a known polyisocyanate used in the formation of polyurethane foam can be used, and examples thereof include aromatic polyisocyanates, alicyclic polyisocyanates, and aliphatic polyisocyanates. Examples of aromatic polyisocyanates include phenylene diisocyanate, tolylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate, dimethyldiphenylmethane diisocyanate, triphenylmethane triisocyanate, naphthalene diisocyanate, and polymethylene polyphenyl polyisocyanate.
[0082] Examples of the alicyclic polyisocyanate include cyclohexylene diisocyanate, methylcyclohexylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, and dimethyldicyclohexylmethane diisocyanate.
[0083] Examples of the aliphatic polyisocyanate include methylene diisocyanate, ethylene diisocyanate, propylene diisocyanate, tetramethylene diisocyanate, and hexamethylene diisocyanate.
[0084] Among these, from the viewpoints of ease of use and availability, aromatic polyisocyanates are preferred, and diphenylmethane diisocyanate is more preferred. The polyisocyanates may be used alone or in combination of two or more.
[0085] (Isocyanate Index) The isocyanate index of the polyurethane composition of the present invention is not particularly limited, but is preferably 200 to 600, more preferably 350 to 550. If the isocyanate index is equal to or greater than the lower limit, the amount of polyisocyanate relative to the polyol becomes excessive, which makes it easier to form isocyanurate bonds due to the trimer of polyisocyanate, and as a result, the flame retardancy of the polyurethane foam is improved. Furthermore, if the isocyanate index is equal to or greater than the lower limit, it is easy to produce a polyurethane foam having isocyanurate bonds, i.e., a polyurethane foam having both flame retardancy and heat insulation at a high level. Furthermore, if the isocyanate index is equal to or less than the upper limit, the balance between the flame retardancy and production cost of the resulting polyurethane foam is good.
[0086] The isocyanate index can be calculated by the following method. Isocyanate Index = equivalents of polyisocyanate ÷ (equivalents of polyol + equivalents of water) × 100 Here, each equivalent number can be calculated as follows: Equivalent number of polyisocyanate = Amount of polyisocyanate used (g) × NCO content (mass%) / Molecular weight of NCO (mol) × 100 Equivalent weight of polyol = OHV × amount of polyol used (g) ÷ molecular weight of KOH (mmol) OHV is the hydroxyl value of the polyol (mg KOH / g). Equivalents of water = amount of water used (g) / molecular weight of water (mol) × number of OH groups in water In the above formulas, the molecular weight of NCO is 42 (mol), the molecular weight of KOH is 56100 (mmol), the molecular weight of water is 18 (mol), and the number of OH groups in water is 2.
[0087] Furthermore, when mixing the polyol liquid agent and the polyisocyanate liquid agent, the volume ratio of the two (polyol liquid agent / polyisocyanate liquid agent) may be set within the range of, for example, 1 / 1.4 to 1.4 / 1, and preferably 1 / 1.2 to 1.2 / 1.
[0088] (Cream time, gel time) The gel time of the polyurethane composition of the present invention is preferably 4 to 60 seconds, more preferably 10 to 45 seconds. If the gel time is less than these upper limits, the urethane reaction proceeds appropriately, and the performance of the polyurethane foam is good. If the gel time is more than the lower limit, when the polyurethane composition is filled into the cavity of the structure, filling defects and density variations are unlikely to occur. Here, the gel time is the value when the liquid temperature of the polyurethane composition is adjusted to 40°C. The gel time is the time (seconds) from the time when the polyol liquid agent and the polyisocyanate liquid agent are mixed and stirring is started to the measurement start time (0 seconds) until the foam becomes stringy when a stick is stuck into the foam during foaming. For example, when a spray gun is used, the measurement start time (0 seconds) means the time when the trigger is pulled.
[0089] The cream time of the polyurethane composition of the present invention is preferably 3 to 15 seconds, more preferably 4 to 10 seconds. The cream time is the time from the start of mixing the polyol liquid and the polyisocyanate liquid and starting to stir (measurement start time (0 seconds)) until the mixed solution starts to react and the color of the solution starts to change.
[0090] From the viewpoint of improving the fluidity of the polyol composition when it is filled, the difference between the gel time and the cream time (gel time - cream time) is preferably 10 seconds or more, more preferably 12 seconds or more, and from the viewpoint of ensuring a certain level of flame retardancy, it is preferably 90 seconds or less, more preferably 80 seconds or less. The cream time and gel time can be adjusted to desired values by adjusting the types of polyol and polyisocyanate used, the isocyanate index, the type and amount of the reaction retarder, the type and amount of the catalyst, the liquid temperature, the structure temperature, etc. In the present invention, the gel time can be easily extended by using a reaction retarder.
[0091] [Method for producing liquid polyol, polyurethane composition, and polyurethane foam] The method for producing the filling polyol liquid agent of the present invention and the filling polyurethane composition containing the same is not particularly limited, but preferably includes the following steps (1) to (3). Then, a polyurethane foam may be formed from the polyurethane composition obtained through steps (1) to (3). Step (1): A step of mixing the components constituting the polyol liquid, other than the catalyst and the reaction retarder, to obtain a mixed liquid. Step (2): A step of adding and mixing a catalyst and a reaction retarder to the mixture obtained in step (1) to obtain a polyol liquid. Step (3): A step of mixing the polyol liquid obtained in step (2) with the polyisocyanate liquid to obtain a polyurethane composition.
[0092] The polyol liquid agent and polyurethane composition of the present invention typically contain a blowing agent. Even in such a case, by producing the liquid polyol agent by the production method including the above steps (1) to (3), the functions of the catalyst and the reaction retarder are not impaired by the blowing agent during production or storage of the liquid polyol agent, so that it is easy to suppress the variation in density of the polyurethane foam and to form a polyurethane foam having excellent performance such as flame retardancy. The detailed procedure for each step will be described below.
[0093] In step (1), the components constituting the polyol liquid other than the catalyst and the reaction retarder, i.e., the polyol and the filler, as well as the optional liquid flame retardant, blowing agent, foam stabilizer, etc., may be mixed. In step (2), when the catalyst and the reaction retarder are added to the mixed liquid obtained in step (1), they may be added in a mixed state or may be added separately. The catalyst and the reaction retarder are preferably added immediately before mixing the polyisocyanate liquid with the polyol liquid. The mixing method in steps (1) and (2) is not particularly limited, and the mixture can be produced, for example, by stirring each component at about room temperature using a mixer such as Homo Disper for about 30 seconds to 20 minutes.
[0094] The mixing method in step (3) is not particularly limited, and the polyol liquid agent obtained in step (2) and the polyisocyanate liquid agent may be mixed by a known method. Specifically, the mixture may be obtained by using a known device such as a high-pressure foaming machine, a low-pressure foaming machine, a spray foaming machine, or a hand mixer.
[0095] The polyurethane composition obtained as described above may be filled into the cavity by a spray gun, etc. More specifically, it is preferable to use a foaming device equipped with a spray gun, mix the polyol liquid agent and the polyisocyanate liquid agent in the foaming device, and fill the mixture into the spray gun. The polyurethane composition injected by the spray gun fills the cavity of the structure, and the polyol and polyisocyanate react with each other to cause foaming, thereby forming a polyurethane foam. As described above, the polyurethane composition uses a specific polyol liquid, which makes it easy to fill hollow spaces in a structure, and the polyurethane foam is properly formed. The formed polyurethane foam has little density variation from place to place and is of excellent quality. However, the above manufacturing method is merely an example, and the polyol liquid, polyurethane composition, and polyurethane foam may be manufactured by a method other than the above, so long as the components constituting the polyurethane composition for filling (i.e., polyol, polyisocyanate, catalyst, filler, reaction retarder, and other optional components) are mixed to obtain the polyurethane composition for filling. For example, in the above explanation, in steps (1) and (2), the components other than the catalyst and reaction retarder are mixed to obtain a mixed liquid, and then the catalyst and reaction retarder are added, but the order of addition is not limited to this order, and each component may be added and mixed simultaneously. Also, in steps (1) and (2), the components other than the catalyst and reaction retarder may be added and mixed to the mixed liquid obtained by mixing the catalyst and reaction retarder to obtain the polyol liquid.
[0096] [Use of polyol liquid and polyurethane composition] As described above, the filling polyol liquid of the present invention and the filling polyurethane composition containing the same are used for the purpose of filling the cavity of a structure. The structure may be a completed structure manufactured through a series of steps in a factory or the like, or an unfinished structure before the production of a completed structure. The filling of the polyurethane composition into the cavity of the completed structure is mainly filling into the cavity surrounded by the members constituting the completed structure, for example, by providing an injection port in a part of the completed structure. The filling of the cavity of the unfinished structure is filling carried out as one of the manufacturing processes before forming the completed structure, and is filling into a cavity that is at least partially open. Specifically, in the manufacturing process, an unfinished structure having an open cavity is manufactured, the polyurethane composition is filled into the cavity from the open part to form a polyurethane foam, and then the open part is closed. The opening part can be closed by gluing or welding the opening part. It may also be closed by providing a member to cover the opening part.
[0097] The completed structure is not particularly limited as long as it has a cavity, and may be a member used in a building or a member used in a vehicle such as an automobile. Specific examples of the completed structure include, for example, a plate-like member, a frame material, etc. Examples of the plate-like member include a panel, a flat deck, etc. The panel is not particularly limited as long as it has a cavity, and may be a panel of any shape when viewed from the front, such as a rectangle, a square, a triangle, etc. The entire interior of the panel may be hollow, or a plurality of members may be provided inside the panel, and part of the cavity inside the panel may be an elongated cavity. The flat deck can be obtained, for example, by roll forming a metal plate such as a steel plate. Flat decks are used in floor or roof construction, for example as formwork onto which concrete is poured. The flat deck has a flat portion with a flat upper surface, and a plurality of reinforcing ribs are protruding from the lower surface of the flat portion. Each reinforcing rib is a protrusion with an internal cavity, is arranged extending along the longitudinal direction, and both ends in the longitudinal direction are crushed and closed. The cavity of each reinforcing rib is an elongated cavity. The cross-sectional shape of the reinforcing rib of the flat deck is not particularly limited as long as a cavity is formed inside, and may be a triangle, a rectangle, or other shape. In the flat deck, the polyurethane composition is filled into the cavity of the reinforcing rib, and the reinforcing rib is provided with an injection hole for filling the polyurethane composition by injection.
[0098] The frame material is a component that has an elongated cavity inside and constitutes all or part of a frame that surrounds an opening in a fixture such as a window, a door, etc. For example, the frame is made up of a pair of side frame parts, an upper frame part, and a lower frame part, and the frame material need only constitute at least a part of these frame parts.
[0099] An unfinished structure is, for example, a structure in the manufacturing stage of a completed structure such as the above-mentioned plate-like member or frame material, and is a structure with a part open. An example of an unfinished structure is a flat deck, in which a metal plate such as a steel plate has a plurality of recesses with openings formed therein by a roll molding machine or the like. After filling the recesses of the structure with a polyurethane resin composition from the openings, the openings are closed by means of welding or the like to form reinforcing ribs, and a flat deck can be manufactured. Another example of an unfinished structure is a structure with a part open because a part of the side surface constituting the panel is not provided, and a panel can be manufactured by filling the polyurethane composition from the open parts and then closing them with a member constituting the side surface.
[0100] The polyurethane composition containing the polyol liquid of the present invention has excellent filling properties, so that even when a structure has a long and narrow cavity, it can be filled up to the ends, and a polyurethane foam of excellent quality with little density difference depending on the location can be formed. An elongated cavity is one in which the longitudinal length is, for example, at least twice, and preferably at least 2.5 times, the cross-sectional dimension. Here, the cross-sectional dimension refers to the maximum length of the cross section of the cavity, for example, the major axis of an ellipse, and the length of the diagonal of a rectangle or square. If the size of the cross-sectional shape (i.e., the cross-sectional dimension) changes along the longitudinal direction, the maximum cross-sectional dimension of the varying part may be taken as the cross-sectional dimension. In the case of a structure having an elongated cavity, it may be either a completed structure or an unfinished structure, but in the case of a completed structure, it is preferable to fill the cavity with the polyurethane composition from the end of the elongated cavity or from the injection hole as described above. Even in such a case, it is possible to fill the cavity up to the end by using the polyurethane composition. EXAMPLES
[0101] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0102] The components used in each of the examples and comparative examples are as follows.
[0103] <Polyol> p-Phthalic acid-based polyester polyol (Kawasaki Chemical Industries, Ltd., product name: Maximol RLK-087, hydroxyl value 200 mg KOH / g)
[0104] <Reaction retarder> Hydroxycarboxylic acid compound (Kawasaki Chemical Industries, product name: RAK253) Acid blocked catalyst (N,N,N',N”,N”-pentamethyldiethylenetriamine blocked with formic acid, manufactured by Tosoh Corporation, product name: TOYOCAT-TMF, ethylene glycol 25-30% by mass, formic acid 10-30% by mass) Formic acid (manufactured by Asahi Chemical Co., Ltd., product name: formic acid)
[0105] <Catalyst> Trimerization catalyst: Potassium 2-ethylhexanoate (manufactured by Air Products, product name: DABCO K-15), concentration 70 to 80% by mass Resinification catalyst: 1,2-dimethylimidazole (TOYOCAT-DM70 manufactured by Tosoh Corporation) concentration 65-75% by mass
[0106] <Foam stabilizer> Silicone foam stabilizer (Toray Dow Corning, product name: SZ1642)
[0107] <Liquid flame retardant> Tris(β-chloropropyl)phosphate (manufactured by Daihachi Chemical Industry Co., Ltd., product name: TMCPP)
[0108] <Solid flame retardant> Red phosphorus flame retardant (Rinkagaku Kogyo Co., Ltd., product name: Nova Excel 140) Zinc borate (Hayakawa Shoji Co., Ltd., product name: Firebrake ZB) Ethylenebis(pentabromophenyl) (manufactured by Albemarle, product name: SAYTEX 8010)
[0109] <Settling inhibitor> Fumed silica (manufactured by Nippon Aerosil Co., Ltd., product name: Aerosil R976S) <Water> ·water
[0110] <Foaming agent> HFO-1233zd(E) (manufactured by Central Glass, product name: Solstice LBA)
[0111] <Polyisocyanate> Polyisocyanate (MDI, manufactured by Sumitomo Chemical Co., Ltd., product name: Sumidur 44V20)
[0112] <Cream time, gel time> The cream time and gel time were evaluated according to the method described in the specification. The liquid temperature during measurement was 15°C, and the container (body) temperature was room temperature (25°C).
[0113] [Examples 1 to 12, Comparative Example 1] A polyol solution and a polyurethane composition were prepared according to the following procedure. (1) Of the components of the polyol solution, the components other than the reaction retarder and catalyst were mixed in the ratio shown in Table 1. (2) A mixture obtained by mixing a reaction retarder and a catalyst into the mixture obtained in (1) above was added in the proportions shown in Table 1 to obtain a polyol liquid. (3) The polyol liquid obtained in (1) above, and a polyurethane composition comprising the polyol liquid and the polyisocyanate liquid were prepared.
[0114] The polyol liquid and polyurethane composition obtained by the above steps (1) to (3) were evaluated as follows.
[0115] [Liquidity assessment] The fluidity of the polyurethane composition was evaluated by measuring the free density and the packed density as described below and calculating the ratio between the two, based on the following criteria: In other words, the more similar the two densities are, the better the fluidity at the time of packing is. (standard) 〇 (Excellent fluidity) Filling density / free density is less than 1.4 × (poor fluidity) Filling density / free density is 1.4 or more
[0116] (Method of measuring packing density) The polyol liquid agent and the polyisocyanate liquid agent shown in Table 1 were adjusted to a liquid temperature of 15°C. The polyisocyanate liquid agent was added to the polyol liquid agent in the blending amounts shown in Table 1, and the mixture was quickly stirred for 1.5 seconds with a homodisper rotating at 8000 rpm to prepare a polyurethane composition. The polyurethane composition prepared as described above was injected into the longitudinal end of a hollow metal frame having a cross section of 40 mm x 30 mm and a length of 900 mm, which was heated to 60°C, and the injected part was sealed. When sealed, an air hole (φ1 to 5 mm) was provided at the end opposite to the injected end. The injection amount was adjusted so that the length filled in the longitudinal direction of the hollow metal frame (longitudinal filling rate) was 90% or more and 99% or less. The injection port was sealed, and the temperature of the metal frame was maintained at 60° C. for 15 minutes. Thereafter, the weight and dimensions of the resulting polyurethane foam were measured, and the filling density was calculated based on the following formula. Packing density (kg / m 3 ) = (Polyurethane foam weight / Longitudinal filling rate / 100) / (Metal frame cross-sectional area x length)
[0117] (Method of measuring free density) The polyol liquid and polyisocyanate liquid shown in Table 1 were adjusted to a liquid temperature of 15°C. The polyisocyanate liquid was added to the polyol liquid in the blending amounts shown in Table 1, and the mixture was quickly stirred for 2 seconds with a homodisper rotating at 8000 rpm to prepare a polyurethane composition. The polyurethane composition prepared as described above was poured into a metal container with a base of 200 mm x 200 mm and a height of 80 mm, and was foamed and cured to form a polyurethane foam. After the reaction and curing were completely completed, the polyurethane foam was cut on all four sides and processed into a rectangular parallelepiped of 100 mm x 100 mm x 50 mm, and the density was calculated from the dimensions and weight, which was taken as the free density.
[0118] [Flame retardancy evaluation] Using the polyurethane foam produced in the above-mentioned free density measurement, a radiant heat intensity of 50 kW / m was measured in accordance with the ISO-5660 test method. 2The total heat release amount when heated for 20 minutes was measured using a cone calorimeter. Flame retardancy was evaluated according to the following criteria. (standard) ◎ Total calorific value is 6.5MJ / m 2 below Total heat output is 6.5MJ / m 2 Super 8.0MJ / m 2 below △ Total heat output is 8.0MJ / m 2 Super 10.0MJ / m 2 below × Total heat output is 10.0 MJ / m 2 Super
[0119] [Table 1]
[0120] The polyurethane composition formed from the polyol liquid satisfying the requirements of the present invention had a longer gel time, and the polyurethane composition of each example using the liquid had excellent fluidity, and the density of the polyurethane foam formed was maintained low.Furthermore, the flame retardancy was also excellent. On the other hand, in the comparative example using a polyol liquid agent that does not satisfy the requirements of the present invention, the gel time was shorter, and it was confirmed that the fluidity of the polyurethane composition using the liquid agent was deteriorated and the density of the polyurethane foam formed was increased.
Claims
1. A filling polyol solution containing a polyol, a catalyst, a filler and a reaction retarder.
2. 2. The filling polyol liquid according to claim 1, further comprising a foaming agent.
3. The filling polyol liquid according to claim 1 or 2, wherein the polyol comprises at least one selected from polyester polyols and polyether polyols.
4. 3. The filling polyol solution of claim 1 or 2, wherein the catalyst comprises a resinification catalyst and a trimerization catalyst.
5. 3. The filling polyol solution according to claim 1 or 2, wherein the filler comprises a solid flame retardant.
6. The filling polyol liquid according to claim 1 or 2, further comprising a foam stabilizer.
7. The filling polyol liquid according to claim 1 or 2, further comprising a settling inhibitor.
8. A filling polyurethane composition comprising the filling polyol liquid agent according to claim 1 or 2, and a polyisocyanate liquid agent containing a polyisocyanate.
9. 9. The filling polyurethane composition according to claim 8, which has a gel time of 4 to 60 seconds at a liquid temperature of 40°C.
10. A polyurethane foam formed from the filling polyurethane composition according to claim 8 or 9.
11. A method for producing a filling polyurethane composition, comprising mixing at least a polyol, a polyisocyanate, a catalyst, a filler, and a reaction retarder to obtain a filling polyurethane composition.
12. A step of mixing at least the polyol and the filler to obtain a mixed liquid; Adding the catalyst and the reaction retarder to the resulting mixture to obtain a polyol solution; A step of mixing the obtained polyol liquid agent with a polyisocyanate liquid agent containing the polyisocyanate to obtain a filling polyurethane composition; A method for producing the filling polyurethane composition of claim 11, comprising:
Citation Information
Patent Citations
Flame retardant polyurethane foam
JP2015151538A
Flame-retardant urethane resin composition
JP2018065937A
Foamable composition for polyurethane foam and method for producing polyurethane foam using the same
JP2019014839A
Polyol composition and polyurethane foam
JP2020063396A
Urethane foam and production method of urethane foam
JP2022064217A