Battery positive electrode material, processing method therefor, and battery

Cold plasma treatment of battery cathode materials with carbon layers doped by active particles enhances interfacial affinity and conductivity, addressing slow ion diffusion issues in lithium-ion and sodium-ion batteries, resulting in improved energy density and stability.

JP2024146670AActive Publication Date: 2024-10-15KUNMING UNIV OF SCI & TECH
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023090284
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2023-05-31
Publication Date
2024-10-15
Estimated Expiration
2043-05-31

AI Technical Summary

Technical Problem

Current lithium-ion and sodium-ion batteries suffer from slow diffusion rates of lithium/sodium ions, leading to low energy and power density, which is addressed by enhancing the surface energy of battery cathode particles and improving interfacial affinity with the electrolyte.

Method used

A cold plasma treatment is applied to a battery positive electrode material with a carbon layer, doping it with active particles such as oxygen or nitrogen, forming a NaF layer to enhance surface energy and interfacial properties.

Benefits of technology

The treatment method improves the interfacial affinity and conductivity, resulting in higher energy density, cycle life, and stability of lithium-ion and sodium-ion batteries with reduced polarization and increased ion transmission rates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146670000001_ABST
    Figure 2024146670000001_ABST
Patent Text Reader

Abstract

To provide a processing method for a battery positive electrode material that increases particle surface energy of the battery positive electrode material and then improves boundary surface affinity between it and an electrolyte to obtain a positive electrode material which has uniform material quality, low porosity and high ion conductivity and electron conductivity.SOLUTION: A processing method for a battery positive electrode material comprises: performing cold plasma processing on a battery positive electrode material having a carbon layer at at least a part of a surface to be processed and doping the carbon layer. Here, a doping amount is 50 ppm or larger. At least the part of the surface of the battery positive electrode material includes the carbon layer and also has a rod-like shape. The carbon layer is doped with active particles after the cold plasma processing, and an NaF layer with high sodium ion conductivity is formed on the surface of the positive electrode material.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of battery materials, and more specifically to battery cathode materials, processing methods thereof, and batteries. [Background technology]

[0002] In recent years, industries such as mobile consumer electronics and electric vehicles have developed rapidly, and there is an urgent need to develop new energy batteries with high energy density and high safety stability to increase the driving time and long-term stable operation of these devices. Therefore, lithium-ion batteries or sodium-ion batteries are considered to be one of the most promising candidate batteries for large-scale energy storage applications. However, all currently known positive electrode materials have a bottleneck of slow lithium / sodium ion diffusion speed, which results in low energy and power density of lithium-ion or sodium-ion batteries. On the other hand, high-performance positive electrode materials can increase the energy density, cycle life, and multiplication rate of lithium-ion or sodium-ion batteries. Therefore, the development of high-performance positive electrode materials is particularly important. Summary of the Invention [Problem to be solved by the invention]

[0003] In view of the deficiencies of the prior art, one of the objectives of the present invention is to solve one or more problems existing in the above prior art. For example, one objective of the present invention is to provide a treatment method that can enhance the surface energy of battery positive electrode particles and improve the interfacial affinity between the particles and the electrolyte. [Means for solving the problem]

[0004] In order to achieve the above object, one aspect of the present invention provides a method for treating a battery cathode material, comprising the step of performing a cold plasma treatment on a battery cathode material having a carbon layer on at least a portion of a treated surface thereof, thereby doping the carbon layer with active particles, wherein the doping amount of the active particles is 50 ppm (mole fraction or volume fraction, parts per billion, ppm) or more.

[0005] In an exemplary embodiment of the method for treating a battery positive electrode material according to the present invention, the power of the cold plasma treatment may be 100W to 500W.

[0006] In one exemplary embodiment of the method for treating a battery positive electrode material according to the present invention, the voltage of the cold plasma treatment may be 50V-150V, and the current of the cold plasma treatment may be 0.4A-2A.

[0007] In one exemplary embodiment of the method for treating a battery positive electrode material according to the present invention, the duration of the cold plasma treatment may be 1 min to 60 min.

[0008] In one exemplary embodiment of the method for treating a battery cathode material according to the present invention, the discharge generating the cold plasma may be selected from one or a combination of a radio frequency plasma discharge, a corona discharge, a dielectric barrier discharge, and a sliding arc discharge.

[0009] In an exemplary embodiment of the method for treating a battery cathode material according to the present invention, the doping may be one of oxygen doping, nitrogen doping, or a combination of both.

[0010] In an exemplary embodiment of the method for treating a battery cathode material according to the present invention, the cold plasma treatment may include inputting a precursor gas, which is one or a combination of oxygen and nitrogen gas, into a cold plasma generator to generate active particles, and doping the active particles into a carbon layer, where the flow rate of the precursor gas may be 1 ml / s to 15 ml / s.

[0011] In an exemplary embodiment of the method for treating a battery cathode material according to the present invention, the battery cathode material may be a polyanionic compound, a layered oxide, a spinel compound, Prussian blue, or a ternary lithium battery cathode material. For example, the battery cathode material may include sodium vanadium phosphate, lithium iron phosphate, sodium titanium phosphate, sodium fluorophosphate, LiMO2, NaMO2, LiN2O4, lithium nickel cobalt manganate, or lithium nickel cobalt aluminate, where M is Co, Ni, Mn, V, or Fe, and N is Co, Nix, Mn, or V.

[0012] In one exemplary embodiment of the method for treating a battery cathode material according to the present invention, at least a portion of the surface of the doped battery cathode material has a rod-like morphology.

[0013] In one exemplary embodiment of the method for treating a battery positive electrode material according to the present invention, the rod-like morphology may have an average length of 1.5 μm to 3 μm. In one exemplary embodiment of the method for treating a battery positive electrode material according to the present invention, a NaF layer is formed on at least a part of the surface of the battery positive electrode material after doping, and the average thickness of the NaF layer may be 6 nm to 10 nm.

[0014] In one exemplary embodiment of the method for treating a battery cathode material according to the present invention, the content of the NaF layer is 500 ppm or more.

[0015] According to another aspect of the present invention, a battery cathode material has a rod-like morphology and at least a part of its surface includes a carbon layer, the carbon layer being a carbon layer doped with active particles after being cold plasma treated, and the doping amount is 50 ppm or more.

[0016] In one exemplary embodiment of the battery cathode material according to the present invention, the active particles may be one or a combination of both oxygen and nitrogen.

[0017] In one exemplary embodiment of the battery positive electrode material according to the present invention, the rod-like morphology has an average length of 1.5 μm to 3 μm.

[0018] Yet another aspect of the present invention provides a cathode sheet which can include a cathode material treated by the above-described method for treating a battery cathode material or the above-described battery cathode material.

[0019] Yet another aspect of the present invention provides a battery that can include the positive electrode sheet described above. Effect of the Invention

[0020] Compared with the prior art, the beneficial effects of the present invention include at least one of the following: (1) The treatment method of the present invention enhances the surface energy of battery positive electrode material particles and improves the interfacial affinity between the particles and the electrolyte, resulting in a positive electrode material with uniform properties, low porosity, and high ionic and electronic conductivity. (2) The positive electrode material of the present invention has high electronic conductivity, good compatibility with the electrolyte interface, and a “rod-like” surface morphology, which provides good stability in the contact between the battery positive electrode material and the electrolyte interface, thereby enhancing the sodium ion transmission rate and electronic conductivity. (3) The treatment method of the present invention can form a NaF layer on the surface of the battery positive electrode material, and this layer has ultra-high sodium ion conductivity, which limits the occurrence of side reactions between the positive electrode material and the electrolyte and increases the transmission rate of sodium ions at the solid-liquid interface. (4) The lithium-ion and sodium-ion batteries manufactured using the treated battery cathode material of the present invention have high energy density, cycle life and multiplicity. (5) The treatment method of the present invention has a simple process flow, low energy consumption, low investment in equipment, no generation of "three wastes", is environmentally friendly, and is suitable for large-scale production application. [Brief description of the drawings]

[0021] The above and other objects and features of the present invention will become more apparent from the following description taken in conjunction with the drawings.

[0022] [Figure 1] FIG. 1 is a schematic diagram of a battery structure according to an embodiment of the present application. [Diagram 2] FIG. 2 shows a comparison diagram of XRD (X-ray diffraction, Diffraction of x-rays, XRD) of sodium vanadium phosphate positive electrode material before and after treatment in Example 1. [Diagram 3] FIG. 2 is a comparative XPS (X-ray photoelectron spectroscopy, XPS) diagram of the sodium vanadium phosphate positive electrode material before and after the treatment in Example 1. [Figure 4] 1 shows a SEM (scanning electron microscope) image of untreated sodium vanadium phosphate cathode material in Example 2. [Diagram 5] FIG. 2 shows an SEM image of the sodium vanadium phosphate cathode material after treatment in Example 2. [Figure 6] 1 shows a voltage-capacity graph of the battery in Example 2. [Figure 7] FIG. 13 is a diagram showing the contact angle of an untreated sodium vanadium phosphate positive electrode material in Example 3 with an electrolyte solution. [Figure 8] FIG. 11 is a diagram showing the contact angle of the sodium vanadium phosphate positive electrode material after treatment in Example 3 with respect to an electrolyte solution. [Figure 9] FIG. 2 shows an EIS (Electrochemical Impedance Spectroscopy, EIS) diagram of the sodium vanadium phosphate positive electrode material after treatment in Example 3. [Figure 10] 1 shows the XPS of untreated sodium vanadium phosphate cathode material in Example 4. [Figure 11] 1 shows the XPS of the sodium vanadium phosphate cathode material after treatment in Example 4. [Figure 12] 1 shows a voltage-capacity graph of the battery in Example 6. [Figure 13] FIG. 1 shows the long circulation diagram of sodium vanadium phosphate after treatment in Example 6. [Figure 14] 1 shows a voltage-capacity graph of the battery in Example 8. [Figure 15] FIG. 1 shows the long cycle diagram of lithium iron phosphate after treatment in Example 8. [Figure 16] 1 shows EIS diagrams of lithium iron phosphate before and after treatment in Example 9. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The battery cathode material, its processing method and battery according to the present invention will now be described in detail with reference to the drawings and exemplary embodiments.

[0024] As shown in FIG. 1, the method for treating a battery cathode material according to one aspect of the present invention is used for the battery shown in FIG. 1. The battery includes an anode structure 12, a cathode structure 11, and a separator 13 located between the anode structure 12 and the cathode structure 11. The anode structure 12 includes an anode sheet 121 and an electrolyte 122. The cathode structure 11 includes an electrolyte 122 and a cathode sheet 110. The cathode sheet 110 includes a current collector 115 and a cathode material layer 112 disposed on the current collector 115. At least a part of the surface of the cathode material layer 112 has a carbon layer 113. In addition, at least a part of the surface of the cathode material layer 112 has a rod-like shape and a NaF layer is formed. Here, the carbon layer 113 is doped with active particles 114 after being subjected to a cold plasma treatment. The cathode material layer 112 may further include a coating layer or an adhesive layer 116. In this embodiment, adhesion layer 116 is a layer of NaF.

[0025] The cathode material layer 112 is treated by a method for treating the battery cathode material, comprising the steps of: performing a cold plasma treatment on the cathode material layer 112 having a carbon layer 113 on at least a part of the treated surface, to dope the carbon layer 113, where the doping amount is 50 ppm or more.

[0026] The positive electrode material layer 112 is doped with the carbon layer 113 attached or coated on the surface of the positive electrode material layer 112 by the highly active particles generated by the cold plasma, and more recesses can be formed on the surface of the carbon layer 113, which enhances the stability when the positive electrode material layer 112 contacts with the liquid-collecting interface, and further enhances the transmission rate of sodium ions or lithium ions and the electronic conductivity. In addition, it enhances the affinity between the positive electrode material layer 112 and the electrolyte 122, mitigates the serious volume effect caused by the large radius of the sodium ions or lithium ions, and makes the active material have good structural stability during the long cycle process. Compared with the untreated positive electrode material layer 112, the battery 10 using the treated positive electrode material layer 112 has a lower polarization voltage, a lower interface impedance, a more stable charge / discharge platform, and a higher specific capacity.

[0027] In some embodiments, the treated cathode material layer 112 is shown to have at least a portion of the carbon layer 113 to allow doping of the carbon layer 113. The carbon layer 113 may be coated or partially coated on the entire surface of the cathode material layer 112 to be treated. That is, the carbon layer 113 described herein may form the entire surface or only a portion of the surface of the cathode material layer 112. In some embodiments, the carbon layer 113 may be one layer or multiple layers. For example, the carbon layer 113 may be two layers, three layers, four layers, more layers, or six layers or more. It should be understood that the surface of the cathode material layer 112 may include not only the carbon layer 113 but also other coating or attachment layers that can improve the performance of the cathode material on the surface of the cathode material layer 112.

[0028] In some embodiments, the doping amount affects the electronic conductivity of the carbon layer 113 on the surface of the positive electrode material layer 112. If the doping amount is less than 50 ppm, the improvement of the electronic conductivity of the carbon layer 113 on the surface of the positive electrode material layer 112 is not obvious, so the doping amount may be 50 ppm or more, 70 ppm or more, 85 ppm or more, 105 ppm or more, 123 ppm or more, 152 ppm or more, 160 ppm to 246 ppm, 214 ppm to 318 ppm, 259 ppm to 413 ppm, 586 ppm to 793 ppm, or 803 ppm to 1050 ppm. Note that if the doping amount exceeds 600 ppm, it may cause the destruction of the surface carbon layer 113 and reduce the circulation stability of the active particles 114. Therefore, a doping amount of 50 ppm to 600 ppm is preferred.

[0029] In some embodiments, the thickness of the cathode material layer 112 to be processed can be adjusted. As described herein, any thickness of the cathode material layer 112 may be processed by the processing methods herein. In some embodiments, the cathode material layer 112 to be processed may have a thickness between 30 μm and 100 μm. For example, the cathode material to be processed may have a thickness less than 28 μm or greater than 110 μm. Alternatively, the cathode material to be processed may have a thickness of 15 μm, 45 μm, 84 μm, or 141 μm.

[0030] In some embodiments, the power of the cold plasma treatment may be 100W to 500W. In the range of 100W to 500W, doping can be realized while ensuring the stability of the carbon layer 113 on the surface of the positive electrode material layer 112. If the power is less than 100W, the energy for breaking the carbon-carbon bond cannot be reached, and the active particles 114 cannot be doped. If the energy exceeds 500W, the structure of the carbon layer 113 on the surface of the positive electrode material layer 112 is destroyed, and its electrochemical properties are reduced. In addition, within this power range, the positive electrode material layer 112 can have a high surface energy and increase its affinity with the interface of the electrolyte 122. For example, the generation of cold plasma may be by transporting a gas source such as oxygen, nitrogen, or a mixed gas into a cold plasma generator to generate the active particles 114. Meanwhile, as for the above applied power, this power is the power that acts directly on the precursor gas, that is, the power that the gas source directly receives. In an embodiment, the power of the cold plasma treatment may be 150W or more, 245W or more, 289W or more, or 423W or more.

[0031] In some embodiments, the voltage of the cold plasma treatment may be 50 V to 150 V, and the current of the cold plasma treatment may be 0.4 A to 2 A. By applying the voltage and current within the above ranges, the power of the cold plasma treatment can be 100 W to 500 W, and the carbon bonds can be cut off and the stability of the carbon layer 113 on the surface of the positive electrode material layer 112 can be ensured. It should be understood by those skilled in the art that the voltage and current in this specification are the voltage and current applied to a cold plasma generator.

[0032] In some embodiments, the voltage of the cold plasma treatment may be 60V or more, 72V or more, 83V or more, 114V or more, 127V or more, or 142V or more, or a combination of the above ranges. The current of the cold plasma treatment may be 0.5A to 1.8A, 0.7A to 1.6A, 0.9A to 1.4A, 1.1A to 1.3A, or a combination of the above ranges. Under the above applied voltage, current, and power, the surface of the positive electrode material layer 112 can have a rod-like form (rod-like structure), and the positive electrode material layer 112 can have the performance described herein.

[0033] In some embodiments, the duration of the cold plasma treatment may be 1 min to 60 min. In the duration of the cold plasma treatment, the applied treatment voltage and treatment current can be coordinated to ensure that the carbon layer 113 on the surface of the positive electrode material layer 112 is doped to 50 ppm or more. For example, the duration of the treatment may be 2 min or more, 15 min or more, 23 min or more, 38 min or more, 47 min or more, or 52 min or more. In some cases, the duration of the cold plasma treatment may be greater than about 30 s, or greater than about 45 s. However, it should be understood that the duration of the treatment may be adjusted as desired, provided that the doping amount described herein can be achieved.

[0034] In some embodiments, the content of NaF produced affects the electrochemical properties of the electrode surface. If the content of NaF is less than 50 ppm, the improvement in ion conductivity of the surface of the positive electrode material layer 112 is not significant, so the content of NaF is 50 ppm or more, 70 ppm or more, 85 ppm or more, 105 ppm or more, 123 ppm or more, 152 ppm or more, 160 ppm to 246 ppm, 214 ppm to 318 ppm, 259 ppm to 413 ppm, 586 ppm to 793 ppm, or 803 ppm to 1050 ppm. In addition, doping of more than 500 ppm may cause the adhesive on the electrode surface to break and reduce the adhesive force between the active materials, so a doping amount of 50 ppm to 500 ppm is preferred.

[0035] In some embodiments, the discharge for generating cold plasma is selected from one or a combination of radio frequency plasma discharge (RF), corona discharge (CD), dielectric barrier discharge (DBD), and glide arc discharge (GAD). The above-mentioned cold plasma device can be used to stably discharge under high pressure, is easy to operate, and can form a plasma discharge region with a larger area. This increases the action range of the active particles 114 in the discharge region, providing a basis for an efficient doping process. Of course, it should be understood that the processing method described herein can also be applied to other discharges suitable for generating cold plasma.

[0036] In some embodiments, the doped active particles 114 or doped active material may be one or a combination of oxygen doping and nitrogen doping. For example, in some embodiments, it may be simply oxygen doping, simply nitrogen doping, or oxygen-nitrogen doping. Doping the carbon layer 113 with highly active particles generated by cold plasma can provide the positive electrode material layer 112 with better electrochemical properties. Of course, those skilled in the art should understand that achieving the doping of the active particles 114 includes inputting a precursor gas consisting of one or a combination of oxygen and nitrogen gas into a cold plasma generator to generate the active particles 114, and then doping the carbon layer 113 on the surface of the positive electrode material layer 112. However, in certain embodiments, the doping of the active particles 114 can also be achieved by other forms of cold plasma generators.

[0037] In some embodiments, the flow rate of the precursor gas flowing into the cold plasma generator may be 1 ml / s to 15 ml / s. Under the above flow rate of the precursor gas, the voltage and current applied in cooperation can ensure that the doping of the carbon layer 113 is achieved. In one set of embodiments, the cathode material layer 112 to be treated is placed in the cold plasma generator and passed through the precursor gas at a rate described herein, and the cold plasma generator is adjusted to the voltage and current described herein, after which the cathode material layer 112 to be treated can be treated. Of course, it should be understood that in order to achieve oxygen doping, it is necessary to complete the oxygen doping in a short time under an oxygen atmosphere, and at the same time ensure that the oxidation effect is extremely low while introducing the oxygen-containing functional group, and avoid the oxidation effect caused by too long a time or too high a power. For the mixed gas containing oxygen, the oxygen content is low, so that the oxidation effect can be neglected.

[0038] In some embodiments, the cathode material layer 112 after the treatments described herein has different morphology characteristics compared to the existing cathode material layer 112. The treatments applied to the cathode material layer 112 cause at least a portion of the surface of the cathode material layer 112 to have a rod-like morphology. For example, sodium vanadium phosphate cathode material exhibits a large number of rod-like or rod-like or sheet-like structures on its surface after being treated by the treatment methods described herein.

[0039] In some embodiments, the surface of the positive electrode material can have all of a rod morphology, or at least 0.01% of the surface area has a rod morphology, or at least 0.1% of the surface area has a rod morphology, or at least 5% of the surface area has a rod morphology, or at least 9.8% of the surface area has a rod morphology, or at least 15.3% of the surface area has a rod morphology, or at least 21.5% of the surface area has a rod morphology, or at least 35.4% of the surface area has a rod morphology, or at least 41.2% of the surface area has a rod morphology, or at least 49.8% of the surface area has a rod morphology, or at least 55.1% of the surface area has a rod morphology, or at least 61.5% of the surface area has a rod morphology, or at least 73.5% of the surface area has a rod morphology, or at least 84.5% of the surface area has a rod morphology. Providing a rod-like morphology on the surface of the positive electrode material can increase the stability of the interface between the positive electrode material and the collecting fluid, and can also increase the rate of sodium ion transport and electronic conductivity. However, it should be understood that rod-like as used herein can refer to an elongated morphology, exhibit an elongated structure, or can be described as columnar, etc.

[0040] In some embodiments, the rod-like morphology can have a particular length. That is, the average length of the rod-like morphology can be 1.6 μm or more, 2.1 μm or more, 2.4 μm or more, 2.6 μm or more, 2.8 μm or more, 2.9 μm or more. In some embodiments, the rod-like morphology can have a particular diameter (i.e., the radial diameter of the rod). That is, the average diameter of the rod-like morphology can be 154 nm or more, 167 nm or more, 179 nm or more, 189 nm or more, 208 nm or more, 238 nm or more, 268 nm or more, 294 nm or more, or 283 nm or more.

[0041] In some embodiments, the mass ratio of the rod-shaped material to the positive electrode material may be specific. For example, the mass ratio of the rod-shaped material to the positive electrode material may be 2% to 10%. In some embodiments, the mass ratio of the rod-shaped material to the positive electrode material may be 0.5% or more, 0.8% or more, 1.5% or more, 2.7% or more, 3.4% or more, 4.7% or more, 5.9% or more, 6.7% or more, or 9.4% or more. In some specific embodiments, the mass ratio is 15.8% or more, 20.1% or more, 30.5% or more, or 36.8% or more.

[0042] In some embodiments, the cathode material layer 112 may be a polyanionic compound, a layered oxide, a spinel type compound, Prussian blue, or a ternary lithium battery cathode material. Polyanionic compounds include sodium vanadium phosphate, sodium vanadium phosphate, lithium iron phosphate, sodium titanium phosphate, and sodium fluorophosphate. Layered oxides include LiMO2 and NaMO2, where M can be Co, Ni, Mn, V, or Fe. Spinel type compounds include LiN2O4, where N can be Co, Nix, Mn, or V. Ternary lithium battery cathode materials include lithium nickel cobalt manganate and lithium nickel cobalt aluminum oxide. It should be understood that the processing methods described herein can also process other cathode materials.

[0043] In some embodiments, other substances may be incorporated that can enhance the electrochemical properties of the cathode materials described herein.

[0044] Another aspect of the present invention provides a type of cathode material. In one exemplary embodiment of the cathode material of the present invention, the cathode material can be obtained by processing according to the battery cathode material processing method described herein. In some embodiments, at least a portion of the surface of the cathode material includes a carbon layer 113 and has a rod-like morphology. Here, the carbon layer is a carbon layer doped with active particles 114 after cold plasma treatment.

[0045] In some embodiments, as described herein, the doping amount may be 50 ppm or more.

[0046] In some embodiments, as described herein, the active particles 114 are one or a combination of oxygen and nitrogen.

[0047] In some embodiments, as described herein, the rod-like morphology may have an average length of between 1.5 μm and 3 μm and an average diameter of between 150 nm and 300 nm.

[0048] In some embodiments, the mass ratio of the rod-shaped material may be specified as described herein, for example, the mass ratio of the rod-shaped material in the positive electrode material may be 2% to 10%.

[0049] Yet another aspect of the invention includes a fluid collector and a layer of positive electrode material disposed on the fluid collector. The positive electrode material is a positive electrode material treated by the method for treating a battery positive electrode material described herein above, or a positive electrode sheet comprising a positive electrode material as described herein above. The positive electrode material layer may include, in addition to the positive electrode material, a conductive agent and an adhesive. The positive electrode material layer may be introduced into the positive electrode sheet by methods known in the art.

[0050] Yet another aspect of the present invention provides a battery, particularly a sodium-ion battery, including a positive electrode sheet as described above, and further including other essential components that constitute the battery, the assembly of which is known in the art.

[0051] In some embodiments, the battery may be a button cell. The assembly of button cells is known in the art. For example, the positive electrode sheet may be placed in a glove box to assemble the button cell.

[0052] In order to better understand the above-described exemplary embodiments of the present invention, specific examples are given below to further illustrate the invention.

[0053] Example 1 A method for treating a battery cathode material, comprising the steps of:

[0054] In step 1, sodium vanadium phosphate positive electrode material is prepared. Using traditional coating technology, coating and cutting is performed on aluminum foil to obtain sodium vanadium phosphate positive electrode material with a thickness of 80 μm.

[0055] In step 2, a nitrogen gas DBD cold plasma activation treatment is performed. First, one side of the sodium vanadium phosphate positive electrode material in step (1) coated with the active material (here, referring to untreated sodium vanadium phosphate) is activated by nitrogen gas DBD cold plasma for 1 minute at a gas flow rate of 10 ml / s, an operating current of 1 A, and a voltage of 150 V, and then cooled to room temperature to obtain a sodium vanadium phosphate positive electrode material after activation treatment.

[0056] In step 3, the button battery is assembled. The sodium vanadium phosphate positive electrode material after the activation treatment in step (2) is placed in a glove box, and the button battery is assembled. After leaving it for 12 hours, the battery is tested.

[0057] The physical properties of the sodium vanadium phosphate cathode material obtained after nitrogen gas DBD cold plasma activation treatment were evaluated. As can be seen from the XRD diagram of sodium vanadium phosphate cathode material in Figure 2, the physical properties of the sodium vanadium phosphate cathode material after nitrogen gas DBD cold plasma activation treatment (DBD-1min in the figure) are unchanged compared to the untreated one (DBD-0min in the figure). It is stated that the nitrogen gas DBD cold plasma treatment does not destroy the crystal structure of sodium vanadium phosphate. Moreover, the XPS diagram of sodium vanadium phosphate cathode material in Figure 3 shows that a NaF layer is generated after nitrogen gas DBD-1min treatment compared to the electrode sheet that has not been subjected to nitrogen gas DBD-0min treatment.

[0058] Example 2 A method for treating a battery cathode material, comprising the steps of:

[0059] In step 1, sodium vanadium phosphate positive electrode material is prepared. Using traditional coating technology, coating and cutting is performed on aluminum foil to obtain sodium vanadium phosphate positive electrode material with a thickness of 80 μm.

[0060] In step 2, a nitrogen gas DBD cold plasma activation treatment is performed. First, one side of the sodium vanadium phosphate positive electrode material coated with the active material in step (1) is activated by nitrogen gas DBD cold plasma at a gas flow rate of 10 ml / s, an operating current of 1 A, and a voltage of 150 V for 2 minutes, and then cooled to room temperature to obtain a sodium vanadium phosphate positive electrode material after activation treatment.

[0061] In step 3, the button battery is assembled. The sodium vanadium phosphate positive electrode material after the activation treatment in step (2) is placed in a glove box, and the button battery is assembled. After leaving it for 12 hours, the battery is tested.

[0062] Morphological characterization and physical and electrochemical tests were carried out on the sodium vanadium phosphate cathode material obtained after the nitrogen gas DBD cold plasma activation treatment, and the nitrogen content doped in the carbon layer 113 was 159 ppm. From the SEM images of FIG. 4 and FIG. 5, it can be seen that compared with the sodium vanadium phosphate cathode material not subjected to the nitrogen gas DBD cold plasma treatment (see FIG. 3), the surface of the treated sodium vanadium phosphate cathode material (see FIG. 4) has a rod-like morphology (rod-like structure, elongated structure), which can enhance the interface contact between the sodium vanadium phosphate cathode material and the electrolyte. As shown in the voltage-capacity graph of FIG. 6, the polarization of the battery is reduced to within 0.04V to 0.03V, the charge-discharge platform is more stable, and the specific capacity is relatively high.

[0063] Example 3 A method for treating a battery cathode material, comprising the steps of:

[0064] In step 1, sodium vanadium phosphate positive electrode material is prepared. Using traditional coating technology, coating and cutting is performed on aluminum foil to obtain sodium vanadium phosphate positive electrode material with a thickness of 80 μm.

[0065] In step 2, a nitrogen DBD cold plasma activation treatment is performed. First, one side of the sodium vanadium phosphate positive electrode material coated with the active material in step (1) is activated by nitrogen DBD cold plasma at a gas flow rate of 10 ml / s, an operating current of 1 A, and a voltage of 150 V for 4 minutes, and then cooled to room temperature to obtain a sodium vanadium phosphate positive electrode material after activation treatment.

[0066] In step 3, the button battery is assembled. The activated sodium vanadium phosphate cathode material is placed in a glove box to assemble the button battery. After standing for 12 hours, the battery is tested.

[0067] Physical and electrochemical tests were performed on the sodium vanadium phosphate cathode material obtained after the nitrogen gas DBD cold plasma activation treatment, and the content of nitrogen doped in the carbon layer 113 was 87 ppm. The contact angle of the untreated sodium vanadium phosphate cathode material with the electrolyte is shown in FIG. 7. The contact angle of the treated sodium vanadium phosphate cathode material with the electrolyte is shown in FIG. 8. The contact angle of the treated sodium vanadium phosphate cathode material with the electrolyte is reduced from 14.15° to 12.4°, which proves that the treated sodium vanadium phosphate cathode material has better wettability with the electrolyte. At the same time, the interface impedance is reduced from 3200Ω to 2500Ω compared to the untreated one, as shown in the EIS (electrochemical impedance spectrum) in FIG. 9.

[0068] Example 4 A method for treating a battery cathode material, comprising the steps of:

[0069] In step 1, sodium vanadium phosphate positive electrode material is prepared. Using traditional coating technology, coating and cutting is performed on aluminum foil to obtain sodium vanadium phosphate positive electrode material with a thickness of 80 μm.

[0070] In step 2, a nitrogen DBD cold plasma activation treatment is performed. First, one side of the sodium vanadium phosphate positive electrode material coated with the active material in step (1) is activated by nitrogen DBD cold plasma at a gas flow rate of 10 ml / s, an operating current of 1 A, and a voltage of 150 V for 6 minutes, and then cooled to room temperature to obtain a sodium vanadium phosphate positive electrode material after activation treatment.

[0071] In step 3, a button battery is assembled. The activated sodium vanadium phosphate positive electrode material obtained in step (2) is placed in a glove box, a button battery is assembled, and the battery is tested after being left to stand for 12 hours.

[0072] Physical and electrochemical tests were carried out on the sodium vanadium phosphate positive electrode material obtained by the nitrogen gas DBD cold plasma activation treatment, and the content of nitrogen doped in the carbon layer 113 was 308 ppm. The XPS of the untreated sodium vanadium phosphate positive electrode material is shown in FIG. 10. The XPS of the treated sodium vanadium phosphate positive electrode material is shown in FIG. 11. Here, the content of pyridine nitrogen, pyrrole nitrogen, and graphitized nitrogen is increased (here, pyridine nitrogen, pyrrole nitrogen, and graphitized nitrogen are three different forms of existence when nitrogen particles are doped in the carbon layer 113), thereby increasing the depression of the carbon layer 113, which is conducive to improving the electronic conductivity and ionic conductivity of sodium vanadium phosphate.

[0073] Example 5 A method for treating a battery cathode material, comprising the steps of:

[0074] In step 1, sodium vanadium phosphate positive electrode material is prepared. Using traditional coating technology, coating and cutting is performed on aluminum foil to obtain sodium vanadium phosphate positive electrode material with a thickness of 80 μm.

[0075] In step 2, oxygen RF cold plasma activation is performed. First, one side of the sodium vanadium phosphate positive electrode material coated with the active material in step (1) is activated by nitrogen gas RF cold plasma activation for 6 minutes at a gas flow rate of 10 ml / s, an operating current of 1 A, and a voltage of 100 V under oxygen RF cold plasma, and then cooled to room temperature to obtain a sodium vanadium phosphate positive electrode material after activation.

[0076] In step 3, a button battery is assembled. The activated sodium vanadium phosphate positive electrode material obtained in step (2) is placed in a glove box, and a button battery is assembled. After standing for 12 hours, the battery is tested.

[0077] Physical and electrochemical tests were carried out on the sodium vanadium phosphate cathode material obtained by oxygen RF cold plasma activation treatment, and the content of argon doped in the carbon layer 113 was 287 ppm. Compared with the untreated electrode sheet, the polarization and impedance were relatively low, where the polarization decreased by 43% and the impedance decreased by 18%.

[0078] Example 6 A method for treating a battery cathode material, comprising the steps of:

[0079] In step 1, sodium vanadium phosphate positive electrode material is prepared. Using traditional coating technology, coating and cutting is performed on aluminum foil to obtain sodium vanadium phosphate positive electrode material with a thickness of 80 μm.

[0080] In step 2, a nitrogen-oxygen mixed gas CD cold plasma activation process is performed. First, one side of the sodium vanadium phosphate positive electrode material obtained in step (1) on which the active material is coated is activated by nitrogen-oxygen mixed gas CD cold plasma activation process for 4 minutes at a gas flow rate of 10 ml / s, an operating current of 2 A, and a voltage of 100 V under nitrogen-oxygen mixed gas CD cold plasma, and then cooled to room temperature to obtain an activated sodium vanadium phosphate positive electrode material.

[0081] In step 3, the button cell is assembled. The activated sodium vanadium phosphate cathode material obtained in step (2) is placed in a glove box and the button cell is assembled. The cell needs to be left to stand for 12 hours before testing.

[0082] Physical and electrochemical tests were carried out on the sodium vanadium phosphate positive electrode material obtained by cold plasma activation treatment of nitrogen-oxygen mixed gas CD, and the nitrogen-oxygen content doped in the carbon layer 113 was 378 ppm. Compared with the untreated electrode sheet, the polarization and impedance are relatively small. The voltage capacity of sodium vanadium phosphate under 5C conditions is shown in FIG. 12. The capacity of the battery after treatment is improved by 13.6% on the original basis, and the polarization of the battery is reduced by about 45%. The long cycle diagram of sodium vanadium phosphate under 5C conditions is shown in FIG. 13. The capacity retention of the battery after treatment is improved by 14% on the original basis.

[0083] Example 7 A method for treating a battery cathode material, comprising the steps of:

[0084] In step 1, sodium vanadium phosphate positive electrode material is prepared. Using traditional coating technology, coating and cutting is performed on aluminum foil to obtain sodium vanadium phosphate positive electrode material with a thickness of 80 μm.

[0085] In step 2, oxygen CD cold plasma activation is performed. First, one side of the sodium vanadium phosphate positive electrode material obtained in step (1) on which the active material is coated is activated under oxygen CD cold plasma at a gas flow rate of 10 ml / s, an operating current of 2 A, and a voltage of 100 V for 4 minutes, and then cooled to room temperature to obtain an activated sodium vanadium phosphate positive electrode material.

[0086] In step 3, the button cell is assembled. The activated sodium vanadium phosphate cathode material obtained in step (2) is placed in a glove box and the button cell is assembled. The cell needs to be left to stand for 12 hours before testing.

[0087] Physical and electrochemical tests were carried out on the sodium vanadium phosphate cathode material obtained by oxygen CD cold plasma activation treatment, and it was found that the content of oxygen doped in the carbon layer 113 was 587 ppm, and it had lower polarization and impedance than the untreated electrode sheet, where the polarization was reduced by 45% and the impedance was reduced by 20%.

[0088] Example 8 A method for treating a cathode material, comprising the steps of:

[0089] In step 1, the lithium iron phosphate positive electrode material is prepared. Using traditional coating technology, the lithium iron phosphate positive electrode material with a thickness of 80 μm is obtained by coating and cutting aluminum foil.

[0090] In step 2, a nitrogen gas DBD cold plasma activation treatment is performed. First, one side of the lithium iron phosphate positive electrode material obtained in step (1) on which the active material is coated is activated by nitrogen gas DBD cold plasma activation treatment for 4 minutes at a gas flow rate of 10 ml / s, an operating current of 4 A, and a voltage of 100 V under nitrogen gas DBD cold plasma, and then cooled to room temperature to obtain an activated lithium iron phosphate positive electrode material.

[0091] In step 3, the button battery is assembled. The activated lithium iron phosphate cathode material obtained in step (2) is placed in a glove box and the button battery is assembled. The battery must be left to stand for 12 hours before testing.

[0092] Physical and electrochemical tests were carried out on the lithium iron phosphate positive electrode material obtained by nitrogen gas DBD cold plasma activation treatment, and the content of nitrogen doped in the carbon layer 113 was 600 ppm, and it had lower polarization, higher capacity and higher capacity retention compared to the untreated electrode sheet. The voltage capacity of the lithium iron phosphate treated under 5C conditions is shown in FIG. 14. The battery polarization after treatment decreased by about 86%, and the capacity was improved by 42.7% on the original basis. The long cycle diagram of the lithium iron phosphate treated under 5C conditions is shown in FIG. 15. The capacity retention was improved by 69.7% on the original basis.

[0093] Example 9 A method for treating a lithium iron phosphate cathode material includes the following steps:

[0094] In step 1, the lithium iron phosphate positive electrode material is prepared. Using traditional coating technology, the lithium iron phosphate positive electrode material with a thickness of 80 μm is obtained by coating and cutting aluminum foil.

[0095] In step 2, a nitrogen gas DBD cold plasma activation treatment is performed. First, one side of the lithium iron phosphate positive electrode material obtained in step (1) on which the active material is coated is activated by nitrogen gas DBD cold plasma activation treatment for 10 minutes at a gas flow rate of 10 ml / s, an operating current of 4 A, and a voltage of 100 V under nitrogen gas DBD cold plasma, and then cooled to room temperature to obtain an activated lithium iron phosphate positive electrode material.

[0096] In step 3, the button battery is assembled. The activated lithium iron phosphate cathode material obtained in step (2) is placed in a glove box and the button battery is assembled. The battery must be left to stand for 12 hours before testing.

[0097] Physical and electrochemical tests were carried out on the lithium iron phosphate positive electrode material obtained by nitrogen gas DBD cold plasma activation treatment, and it was found that the nitrogen content doped in the carbon layer 113 was 700 ppm, and it had a lower impedance than the untreated electrode sheet. The EIS diagrams of the lithium iron phosphate before and after treatment are shown in FIG. 16. After treatment, the battery impedance decreased from 126.3 Ω to 27.2 Ω.

[0098] Although the present invention has been described in connection with exemplary embodiments thereof, those skilled in the art may make various modifications and improvements to the exemplary embodiments of the present invention without departing from the spirit and scope of the present invention as defined in the appended claims.

Claims

1. 1. A method for treating a battery cathode material, comprising: A battery positive electrode material having a carbon layer on at least a portion of a treated surface is subjected to a cold plasma treatment to dope the carbon layer with active particles; The method for treating a battery positive electrode material is characterized in that the doping amount of the active particles is 50 ppm or more.

2. The power of the cold plasma treatment is 100 W to 500 W; The voltage of the cold plasma treatment is 50V to 150V, and the treatment current of the cold plasma treatment is 0.4A to 2A; 2. The method for treating a battery positive electrode material according to claim 1, wherein the cold plasma treatment time is 1 min to 60 min.

3. 2. The method for treating a battery positive electrode material according to claim 1, wherein the discharge generating the cold plasma is selected from one or a combination of a radio frequency plasma discharge, a corona discharge, a dielectric barrier discharge and a sliding arc discharge.

4. 2. The method of claim 1, wherein the doping of the active particles is one or a combination of oxygen doping and nitrogen doping.

5. The cold plasma treatment includes inputting a precursor gas consisting of one or a combination of oxygen and nitrogen gases into a cold plasma generator to dope the carbon layer with the generated active particles; 2. The method for treating a battery positive electrode material according to claim 1, wherein the flow rate of the precursor gas is 1 ml / s to 15 ml / s.

6. 2. The method for treating a battery positive electrode material according to claim 1, wherein the battery positive electrode material is a polyanion type compound, a layered oxide, a spinel type compound, Prussian blue or a positive electrode material for a ternary lithium battery.

7. The battery positive electrode material is sodium vanadium phosphate, lithium iron phosphate, sodium titanium phosphate, sodium fluorophosphate, LiMO 2 , NaM.O. 2 , LiN 2 O 4 , lithium nickel cobalt manganese oxide or lithium nickel cobalt aluminate; 7. The method of claim 6, wherein M is Co, Ni, Mn, V or Fe, and N is Co, Nix, Mn or V.

8. The method for treating a battery positive electrode material according to claim 7, characterized in that the battery positive electrode material after doping has a rod-like morphology and has a NaF layer formed on at least a part of its surface.

9. 9. The method for treating a battery positive electrode material according to claim 8, wherein the rod-like morphology has an average length of 1.5 μm to 3 μm and an average diameter of 150 nm to 300 nm.

10. 9. The method for treating a battery positive electrode material according to claim 8, wherein the NaF layer has an average thickness of 6 nm to 10 nm and a NaF content of 500 ppm or more.

11. A battery positive electrode material, comprising: At least a portion of the surface of the battery positive electrode material includes a carbon layer and has a rod-like morphology; Moreover, a NaF layer is formed on at least a part of the surface, The battery positive electrode material is characterized in that the carbon layer is a carbon layer doped with active particles after cold plasma treatment, and the doping amount is 50 ppm or more.

12. 12. The battery cathode material of claim 11, wherein the active particles are one or a combination of oxygen and nitrogen.

13. The battery positive electrode material according to claim 11, wherein the rod-like morphology has an average length of 1.5 μm to 3 μm and an average diameter of 150 nm to 300 nm.

14. The battery positive electrode material according to claim 11, characterized in that the NaF layer has an average thickness of 6 nm to 10 nm and the NaF content is 500 ppm or more.

15. A positive electrode sheet, The positive electrode sheet includes a current collector and a positive electrode material layer provided on the current collector, At least a part of a surface of the positive electrode material layer includes a carbon layer, and at least a part of the surface has a rod-like morphology and a NaF layer formed thereon; Here, the carbon layer is doped with active particles after undergoing cold plasma treatment, and the doping amount is 500 ppm or more. A positive electrode sheet characterized by:

16. 16. The positive electrode sheet according to claim 15, wherein the active particles are oxygen, nitrogen or a combination thereof.

17. The positive electrode sheet of claim 15, wherein the rod-like morphology has an average length of 1.5 μm to 3 μm and an average diameter of 150 nm to 300 nm.

18. The positive electrode sheet according to claim 15, wherein the NaF layer has an average thickness of 6 nm to 10 nm and a NaF content of 500 ppm or more.

Citation Information

Patent Citations

  • Preparation method of cold plasma nitrogen-doped multiwalled carbon nanotube

    CN106185866A

  • Porous carbon-coated ternary positive electrode material and preparation method thereof

    CN112038640A

  • Method for recycling ternary battery positive electrode material through combination of plasma and hydrogen peroxide

    CN114597394A

  • Preparation method of boron-doped carbon fluoride positive electrode material with high specific capacity

    CN114927672A

  • Cathode material for lithium-ion secondary battery and its manufacturing method as well as lithium-ion secondary battery using same

    JP2006302671A