Suspension polymerization method for polyvinyl chloride resin, polyvinyl chloride resin, and polyvinyl chloride resin molded product

The suspension polymerization of vinyl chloride resin with hydrophobic fibers addresses the issue of decreased tensile elongation by ensuring uniform dispersion, thereby improving mechanical properties.

JP2024146698APending Publication Date: 2024-10-15SEKISUI CHEMICAL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023142740
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2023-09-04
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing methods for reinforcing vinyl chloride resins with fillers result in decreased tensile elongation due to poor adhesion and aggregation of fillers, which worsens mechanical properties.

Method used

A suspension polymerization method involving hydrophobic fibers with specific properties is used to disperse these fibers uniformly within the vinyl chloride resin, enhancing tensile elongation and mechanical strength.

Benefits of technology

The method achieves improved dispersibility of hydrophobic fibers in vinyl chloride resin, resulting in a molded article with enhanced tensile elongation and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146698000001
    Figure 2024146698000001
Patent Text Reader

Abstract

To provide a suspension polymerization method for polyvinyl chloride resins that facilitates dispersion of hydrophobic fibers into polyvinyl chloride resins, while enabling production of a polyvinyl chloride resin molded product with resistance to reduction in tensile elongation, a polyvinyl chloride resin prepared by the method, and a polyvinyl chloride resin molded product.SOLUTION: The present invention provides a suspension polymerization method for polyvinyl chloride resins that includes the step where a vinyl chloride monomer alone or a vinyl chloride-based monomer containing a vinyl chloride monomer as the main component is suspension-polymerized in the presence of hydrophobic fibers with a fiber length of 0.001 μm and 200 μm, as well as a polyvinyl chloride resin prepared by the method, and a polyvinyl chloride resin molded product.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for suspension polymerization of a vinyl chloride resin, a vinyl chloride resin, and a vinyl chloride resin molded article. [Background technology]

[0002] Resin compositions in which vinyl chloride resin is reinforced with high aspect ratio fillers such as fibrous, needle-like, or plate-like fillers are widely known. By adding fillers to vinyl chloride resin, mechanical strength and heat resistance can be improved.

[0003] However, these fillers generally have poor adhesion to vinyl chloride resins, and although the mechanical strength and heat resistance of the resin molded body are improved by filling the resin molded body with these fillers, the tensile elongation is often reduced. Usually, when preparing a molded body of polyvinyl chloride resin containing a filler (hereinafter referred to as a "filler-containing polyvinyl chloride resin molded body"), a polyvinyl chloride resin powder and a filler are mixed to prepare a vinyl chloride resin composition, and then molding is performed. However, in this method, the filler, which has low compatibility with vinyl chloride resins, aggregates in the filler-containing polyvinyl chloride resin molded body, further worsening the tensile elongation. Therefore, in order to improve the dispersibility of the filler in the vinyl chloride resin, a method has been proposed in which an inorganic substance is introduced into the resin as a filler in advance during suspension polymerization to prepare the polyvinyl chloride resin.

[0004] For example, Patent Document 1 discloses a method for obtaining an inorganic-containing vinyl chloride resin by polymerizing a vinyl chloride monomer in the presence of an inorganic substance treated with a silane coupling agent. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 57-192412 Summary of the Invention [Problem to be solved by the invention]

[0006] However, while the method described in Patent Document 1 improves the strength of polyvinyl chloride resin molded products, the elongation of the tensile properties is lower than that of the comparative examples, and good results were not obtained in terms of elongation (%).

[0007] In view of the above, an object of the present invention is to provide a method for suspension polymerization of a vinyl chloride-based resin, which makes it easy to disperse hydrophobic fibers in a vinyl chloride-based resin and which can produce a vinyl chloride-based resin molded article in which a decrease in tensile elongation is suppressed, a vinyl chloride resin obtained by the method, and a vinyl chloride-based resin molded article. [Means for solving the problem]

[0008] As a result of extensive investigations into the above-mentioned problems, the present inventors have found the following: That is, they have found that by adding hydrophobic fibers as a filler when carrying out suspension polymerization of vinyl chloride monomer alone or a vinyl chloride monomer mainly composed of vinyl chloride monomer, it is possible to easily incorporate the hydrophobic fibers into a vinyl chloride resin, and to obtain a polyvinyl chloride resin composition having a high tensile elongation at the same filler content, as compared with a method in which a filler is blended into a vinyl chloride resin, and have arrived at the present invention. That is, the present invention provides the following [1] to [9]. [1] A method for suspension polymerization of a vinyl chloride resin, comprising a step of suspension polymerizing vinyl chloride monomer alone or a vinyl chloride monomer mainly composed of vinyl chloride monomer in the presence of hydrophobic fibers having a fiber length of 0.001 μm to 200 μm. [2] The method for suspension polymerization of a vinyl chloride resin according to [1], wherein the hydrophobic fiber is at least one type selected from the group consisting of polyester fiber, polyethylene terephthalate fiber, carbon nanotube, and carbon nanofiber. [3] The method for suspension polymerization of a vinyl chloride resin according to [2], wherein the hydrophobic fiber is a carbon nanofiber. [4] The method for suspension polymerization of a vinyl chloride resin according to any one of [1] to [3], wherein the amount of the hydrophobic fiber added is 0.1 to 100 parts by mass per 100 parts by mass of the vinyl chloride monomer. [5] The method for suspension polymerization of a vinyl chloride resin according to [3], wherein the carbon nanofibers have an aspect ratio of 1 to 1,000. [6] The method for suspension polymerization of a vinyl chloride resin according to any one of [1] to [5], wherein the step of suspension polymerization is carried out in an aqueous medium containing a dispersant. [7] A vinyl chloride resin obtained by the method for suspension polymerization of a vinyl chloride resin according to any one of [1] to [6], wherein the content of the hydrophobic fiber is 1 to 50 parts by mass per 100 parts by mass of the vinyl chloride monomer. [8] The polyvinyl chloride resin according to [7], wherein the inclusion rate of the hydrophobic fibers is 50.0% by mass to 99.0% by mass. [9] A vinyl chloride resin molded product comprising the vinyl chloride resin according to [7] or [8]. Effect of the Invention

[0009] According to the present invention, there are provided a method for suspension polymerization of a vinyl chloride-based resin which makes it easy to disperse hydrophobic fibers in a vinyl chloride-based resin and which can produce a vinyl chloride-based resin molded article in which a decrease in tensile elongation is suppressed, a vinyl chloride-based resin obtained by the method, and a vinyl chloride-based resin molded article. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, the embodiments of the method for suspension polymerization of a vinyl chloride resin, the vinyl chloride resin, and the vinyl chloride resin molded article of the present invention will be described in detail, but the following description is one example of the embodiment of the present invention, and the present invention is not limited to these. In addition, in this specification, the symbol "to" indicating a numerical range means a range including the numerical values ​​before and after it.

[0011] The method for suspension polymerization of a vinyl chloride resin in this embodiment of the present invention includes a step of suspension polymerizing a vinyl chloride monomer alone or a vinyl chloride monomer containing a vinyl chloride monomer as a main component in the presence of hydrophobic fibers having a fiber length of 0.001 μm to 200 μm. It is known that inorganic fillers are added during the polymerization of vinyl chloride, but inorganic materials are difficult to disperse in vinyl chloride monomers, and therefore difficult to incorporate into vinyl chloride resins. Therefore, the dispersion state in vinyl chloride resins is insufficient, and physical properties may deteriorate. Hydrophobic fibers have hydrophobic groups such as methyl groups, chain-like or cyclic alkyl groups, aryl groups, and benzene rings, or have a graphite crystal structure, which makes them less compatible with water and more compatible with vinyl chloride monomers, making them easier to disperse in vinyl chloride monomers. The average fiber length of the hydrophobic fibers is preferably 0.001 μm to 200 μm, more preferably 0.01 μm to 100 μm, and even more preferably 0.05 μm to 50 μm. If the average fiber length of the hydrophobic fibers is less than 0.001 μm, the mechanical strength of the molded body made of vinyl chloride resin decreases, which is not preferable. Also, if it exceeds 200 μm, the tensile elongation decreases, which is not preferable.

[0012] The vinyl chloride monomer used in the present invention may be a vinyl chloride monomer alone or a vinyl chloride monomer containing a vinyl chloride monomer as a main component. The vinyl chloride monomer containing vinyl chloride monomer as a main component is a mixed monomer of 50 mass % or more of vinyl chloride monomer and a monomer copolymerizable with vinyl chloride monomer.

[0013] The monomer copolymerizable with the vinyl chloride monomer usable in the suspension polymerization method of the present invention is not particularly limited as long as it can be polymerized with the vinyl chloride monomer, and examples thereof include alkyl vinyl esters such as vinyl acetate and vinyl propionate; alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate and octyl (meth)acrylate; α-monoolefins such as ethylene and propylene; maleic anhydride, acrylonitrile, vinylidene chloride, styrene and maleimides, and at least one of these is used.

[0014] Specific examples of hydrophobic fibers that can be used in the suspension polymerization method of the present invention include polymer fibers made of polypropylene, polyester, aromatic polyester, polyethylene terephthalate, aramid, acetate, nylon, polyacrylic, polyvinyl formal, poly-p-benzobisoxazole, etc., and fibrous carbon materials such as silicon carbide fibers, carbon nanotubes, carbon nanofibers, and carbon fibers, and at least one of these is used. From the viewpoints of track record in vinyl chloride resin molded products, economic efficiency, and improvement of mechanical strength, etc., polymer fibers and carbon fibers are preferred, polyester fibers, polyethylene terephthalate fibers, carbon nanotubes, and carbon nanofibers are more preferred, and carbon nanofibers are even more preferred.

[0015] The amount of hydrophobic fiber added is preferably 0.1 to 100 parts by mass, more preferably 0.5 to 50 parts by mass, and even more preferably 1 to 30 parts by mass, based on 100 parts by mass of vinyl chloride monomer. By making the amount equal to or greater than the lower limit, it is possible to improve the mechanical properties. Also, by making the amount equal to or less than the upper limit, it is possible to suppress aggregation of the hydrophobic fibers, and to suppress instability of the suspension polymerization.

[0016] The fibrous carbon material is preferably one that has been surface-treated in advance. The surface treatment can improve the reactivity and compatibility with vinyl chloride monomers in suspension polymerization, so that the material is easily mixed with vinyl chloride resins and incorporated into polymers. Furthermore, the surface treatment can suppress the aggregation of the fibrous carbon material, and improve mechanical properties such as impact resistance. The surface treatment of the fibrous carbon material is not particularly limited, and the surface can be treated by oxidation treatment, sizing treatment, fatty acid treatment, coupling treatment oil, or the like. If necessary, the surface treatment can be performed in a combination of these forms.

[0017] Furthermore, when carbon nanofibers are used as the fibrous carbon material, the aspect ratio (average fiber length / average fiber width) of the carbon nanofibers is preferably 1 to 1000, more preferably 2.5 to 500, and even more preferably 5 to 250. By making the aspect ratio of the carbon nanofibers 1 or more, it is possible to improve the mechanical strength. Furthermore, by making the aspect ratio 1000 or less, it is possible to suppress the aggregation of hydrophobic fibers.

[0018] In one example of the suspension polymerization method of the present invention, water, a dispersant, the above-mentioned hydrophobic fiber, and a polymerization initiator are first charged into a polymerization vessel equipped with a temperature regulator and a stirrer. Then, air is removed from the polymerization vessel using a vacuum pump to create a vacuum atmosphere. Next, all other raw materials such as vinyl chloride monomer are charged under stirring conditions. Then, the temperature inside the reaction vessel is raised, and the polymerization reaction of the materials is allowed to proceed at the desired polymerization temperature. Through these steps, a vinyl chloride resin integrated with the hydrophobic fiber can be obtained.

[0019] After completion of the reaction in the suspension polymerization method of the present invention, for example, vinyl monomer having unreacted vinyl chloride can be removed to give a slurry, which can then be dehydrated and dried to obtain the desired vinyl chloride resin.

[0020] The temperature during polymerization in the suspension polymerization method of the present invention is not particularly limited, but is preferably in the range of 40° C. to 80° C., which is easy to control the temperature during industrial production. The polymerization time in the suspension polymerization method of the present invention is preferably 2 to 20 hours.

[0021] The vinyl chloride resin obtained by the suspension polymerization method in the present invention may have an average degree of polymerization of 250 to 5000, preferably 250 to 4000, more preferably 300 to 3000, and even more preferably 400 to 2000. By having the average degree of polymerization within the above range, processability at an appropriate temperature can be ensured during molding, and deterioration of long-term performance such as fatigue properties can be prevented during use. The average degree of polymerization of the vinyl chloride resin can be measured in accordance with JIS K 6726.

[0022] The vinyl chloride resin obtained by the suspension polymerization method in the present invention is preferably produced in a particulate form. The particulate vinyl chloride resin has an average particle size of, for example, preferably 0.05 to 500 μm, more preferably 0.1 to 450 μm, and even more preferably 0.15 to 400 μm. By using a particulate vinyl chloride resin with an average particle size within the above range, problems such as an unstable reaction system during polymerization do not occur, and handling properties can be ensured even during drying. In this specification, the average particle size refers to the average value of the measured values ​​when the primary particle sizes of 100 particles in a visual field observed are measured using a scanning electron microscope (SEM) etc. The average particle size refers to the average value of the diameters of the particles when the particles are spherical, and refers to the average value of the major axes of the particles when the particles are non-spherical.

[0023] The suspension polymerization step of the suspension polymerization method of the present invention is preferably carried out in an aqueous medium containing a dispersant. The dispersant in the present invention means a substance having a function of dispersing vinyl chloride monomers uniformly and stably in an aqueous medium when the vinyl chloride monomers are polymerized, and may also have various dispersing functions such as an emulsifying function and a thickening function at the same time.

[0024] Examples of dispersants include partially saponified polyvinyl acetate; cellulose derivatives such as methyl cellulose, ethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, and hydroxypropyl methyl cellulose; water-soluble polymers such as vinyl acetate-maleic anhydride copolymer, polyacrylic acid, polyethylene oxide, gelatin, and starch; oil-soluble emulsifiers such as sorbitan monolaurate, sorbitan monostearate, and glycerin tristearate; water-soluble emulsifiers such as polyoxyethylene sorbitan monolaurate, polyoxyethylene glycerin oleate, and sodium laurate, which can be used alone or in combination of two or more. The amount of dispersant added is preferably 10 to 20,000 ppm, more preferably 50 to 17,500 ppm, and even more preferably 100 to 15,000 ppm, relative to 100 parts by mass of vinyl chloride monomer.

[0025] As the polymerization initiator used in the suspension polymerization method of the present invention, a known oil-soluble radical initiator generally used in the polymerization of vinyl chloride resins is used. For example, perester compounds such as t-butyl peroxyneodecanoate, t-hexyl peroxyneodecanoate, t-hexyl peroxypivalate, α-cumyl peroxyneodecanoate, t-hexyl neohexanoate, and 2,4,4-trimethylpentyl-2-peroxy-2-neodecanoate; diisopropyl peroxydicarbonate, di-2-ethylhexyl peroxydicarbonate, di-2-ethoxyethyl peroxydicarbonate, dimethoxyisopropyl peroxydicarbonate, and the like. peroxide compounds such as decanoyl peroxide, lauroyl peroxide, benzoyl peroxide, cumene hydroperoxide, cyclohexanone peroxide, 2,4-dichlorobenzoyl peroxide, p-menthane hydroperoxide, 3,5,5-trimethylhexanoyl peroxide, isobutyl peroxide, and other azo compounds such as α,α'-azobisisobutyronitrile, α,α-azobis(2,4-dimethylvaleronitrile), and α,α'-azobis(4-methoxy-2,4-dimethylvaleronitrile), and at least one of these is used. The amount of the polymerization initiator added is preferably 10 to 20,000 ppm, more preferably 50 to 17,500 ppm, and further preferably 100 to 15,000 ppm, based on 100 parts by mass of the vinyl chloride monomer.

[0026] The polymerization conditions and polymerization formulation are not limited to those described above, and a polymerization regulator, a chain transfer agent, an antistatic agent, a crosslinking agent, a stabilizer, a scale inhibitor, and a gelation improver may be appropriately added.

[0027] According to the method for suspension polymerization of vinyl chloride resin of the present invention, hydrophobic fibers can be efficiently introduced into the vinyl chloride resin by adding the hydrophobic fibers. Moreover, the vinyl chloride resin containing the hydrophobic fibers and the vinyl chloride resin molded product obtained by the method have the hydrophobic fibers uniformly dispersed therein, so that the decrease in tensile elongation can be suppressed.

[0028] The content of hydrophobic fibers in the vinyl chloride resin obtained by the vinyl chloride resin suspension polymerization method of the present invention is 1 to 50 parts by mass based on 100 parts by mass of vinyl chloride monomer. If the content of the hydrophobic fiber is less than 1 part by mass relative to 100 parts by mass of the vinyl chloride monomer, the mechanical properties and heat resistance cannot be improved by adding the hydrophobic fiber. If the content of the hydrophobic fiber is more than 50 parts by mass relative to 100 parts by mass of the vinyl chloride monomer, the kneading processability is reduced, and depending on the molding conditions, the surface appearance is deteriorated due to the unevenness of the hydrophobic fiber. From the above viewpoint, the content of the hydrophobic fiber is preferably 2 to 45 parts by mass, more preferably 4 to 40 parts by mass, and even more preferably 6 to 35 parts by mass relative to 100 parts by mass of the vinyl chloride monomer.

[0029] In addition, the inclusion degree of the hydrophobic fiber in the vinyl chloride resin is preferably 50.0% by mass to 99.0% by mass. When the inclusion degree of the hydrophobic fiber is 50.0% by mass or more, the hydrophobic fiber is sufficiently incorporated in the vinyl chloride resin, and aggregation during molding can be suppressed. In addition, when the inclusion degree of the hydrophobic fiber is 99.0% by mass or less, the hydrophobic fiber has excellent dispersibility in water, so that the particle size distribution during polymerization is stable. From the above viewpoint, the inclusion degree of the hydrophobic fiber in the vinyl chloride resin containing the hydrophobic fiber is preferably 50.0% by mass to 99.0% by mass, more preferably 55.0% by mass to 95.0% by mass, and further preferably 60.0% by mass to 90.0% by mass. The definition and method of determination of the inclusion degree are as described in the examples described later. EXAMPLES

[0030] In the following, in order to explain the present invention in more detail, examples and comparative examples are described, but the present invention is not limited to these examples.

[0031] <Evaluation method> The obtained vinyl chloride resin and vinyl chloride resin composition molded samples were evaluated by the following methods.

[0032] <Amount of hydrophobic fibers in polyvinyl chloride resin> Each dehydrated and dried polyvinyl chloride resin was ignited in a crucible and the organic matter was completely incinerated at 500°C. The amount of hydrophobic fiber (A) in the polyvinyl chloride resin was calculated from the amount of remaining ash. Amount of hydrophobic fiber (A) = ash content (g) / polyvinyl chloride resin before heating (g)

[0033] <Evaluation method for dispersibility of hydrophobic fibers (degree of inclusion)> 1 g of the dehydrated and dried polyvinyl chloride resin powder and 40 ml of SPT heavy liquid for specific gravity separation (sodium polytungstate, Sometu, SPT-1) adjusted to a specific gravity of 1.5 were added to a cylindrical funnel, and after stirring with a glass rod, 10 ml of SPT heavy liquid for specific gravity separation was added to wash away the sample adhering to the side of the cylindrical funnel and the glass rod. To prevent the solvent from volatilizing, the funnel was covered with plastic wrap and left to stand for 24 hours, after which the cock at the bottom of the cylindrical funnel was opened and the precipitate that had accumulated at the bottom of the funnel was removed and separated, and the amount of hydrophobic fiber (B) not included in the polyvinyl chloride resin was calculated using the following formula. Amount of unincorporated hydrophobic fiber (B) = Precipitate (g) / Added polyvinyl chloride resin (g) The coverage was calculated using the following formula: Inclusion rate (mass%) = {1 - (amount of unincorporated hydrophobic fiber (B) / amount of hydrophobic fiber (A))} x 100

[0034] When the inclusion rate was 60.0% to 90.0% by mass, it was judged as "Good", when it was 99.0% by mass or more, > 90.0% by mass, or 60.0% by mass > inclusion rate > 50.0% by mass, it was judged as "Good", and when it was more than 99.0% or less than 50.0%, it was judged as "Poor".

[0035] <Tensile elongation> A tensile test was carried out on a No. 1 test piece at 23° C. in accordance with the tensile test method for plastics (JIS K 7113) using a molded sample of the vinyl chloride resin composition to determine the tensile elongation.

[0036] Example 1 45 kg of deionized water was placed in a polymerization vessel (pressure-resistant autoclave) with an internal volume of 100 L. Furthermore, 3,000 ppm of a dispersant (hydroxypropyl methylcellulose), 600 ppm of a polymerization initiator (t-butyl peroxy neodecanoate), and 50,000 ppm of hydrophobic fiber (carbon nanofiber, manufactured by Almedio Co., Ltd., reinforcing carbon nanofiber, average fiber length 8.0 μm, aspect ratio 32) were added relative to the vinyl chloride monomer. Next, the inside of the polymerization vessel was degassed to 45 mmHg, and then 30 kg of vinyl chloride monomer was charged and stirring was started.

[0037] The polymerization temperature was set to 57°C and maintained at this temperature until the end of polymerization. The reaction was terminated when the polymerization conversion reached 95%, and the unreacted monomers in the polymerization vessel were recovered, after which the polymer was taken out of the system in a slurry state and dehydrated and dried. The hydrophobic fiber amount (A) of the obtained hydrophobic fiber-containing vinyl chloride resin was determined to be 0.042, and it was confirmed that the obtained hydrophobic fiber-containing vinyl chloride resin contained 4.38 parts by mass of carbon nanofibers per 100 parts by mass of vinyl chloride resin. In addition, the dispersibility in the resin and the tensile elongation were evaluated by the above-mentioned evaluation method. The results are shown in Table 1.

[0038] Example 2 Suspension polymerization was carried out in the same manner as in Example 1, except that the amount of hydrophobic fiber (carbon nanofiber, manufactured by Almedio Co., Ltd., reinforcing carbon nanofiber, average fiber length 8.0 μm, aspect ratio 32) added was changed to 150,000 ppm. The obtained vinyl chloride resin was evaluated in the same manner as in Example 1. The hydrophobic fiber amount (A) of the obtained hydrophobic fiber-containing vinyl chloride resin was calculated to be 0.141, confirming that the obtained hydrophobic fiber-containing vinyl chloride resin contained 16.41 parts by mass of carbon nanofiber per 100 parts by mass of vinyl chloride resin. The results are shown in Table 1.

[0039] Example 3 Suspension polymerization was carried out in the same manner as in Example 1, except that the amount of hydrophobic fiber (carbon nanofiber, manufactured by Almedio Co., Ltd., reinforcing carbon nanofiber, average fiber length 8.0 μm, aspect ratio 32) added was changed to 300,000 ppm. The obtained vinyl chloride resin was evaluated in the same manner as in Example 1. The hydrophobic fiber amount (A) of the obtained hydrophobic fiber-containing vinyl chloride resin was calculated to be 0.248, confirming that the obtained hydrophobic fiber-containing vinyl chloride resin contained 32.98 parts by mass of carbon nanofiber per 100 parts by mass of vinyl chloride resin. The results are shown in Table 1.

[0040] Example 4 Suspension polymerization was carried out in the same manner as in Example 1, except that the hydrophobic fiber was changed to a hydrophobic fiber (carbon fiber (milled fiber), manufactured by Mitsubishi Chemical Corporation, K223HM, average fiber length 50 μm, aspect ratio 4.5) and the amount added was changed to 50,000 ppm. The obtained vinyl chloride resin was evaluated in the same manner as in Example 1. The hydrophobic fiber amount (A) of the obtained hydrophobic fiber-containing vinyl chloride resin was calculated to be 0.048, and it was confirmed that the obtained hydrophobic fiber-containing vinyl chloride resin contained 5.04 parts by mass of carbon fiber (milled fiber) per 100 parts by mass of vinyl chloride resin. The results are shown in Table 1.

[0041] Comparative Example 1 Suspension polymerization was carried out in the same manner as in Example 1, except that no hydrophobic fiber was added during polymerization. 4.38 parts by mass of hydrophobic fiber (carbon nanofiber, manufactured by Almedio Co., Ltd., reinforcing carbon nanofiber, average fiber length 8.0 μm, aspect ratio 32) was added to 100 parts by mass of the obtained vinyl chloride resin, mixed, and then dehydrated and dried. The obtained hydrophobic fiber-containing vinyl chloride resin was evaluated for dispersibility in the resin and tensile elongation using the above-mentioned evaluation method. The results are shown in Table 1.

[0042] Comparative Example 2 The evaluation was carried out in the same manner as in Comparative Example 1, except that the amount of hydrophobic fiber (carbon nanofiber, manufactured by Almedio Co., Ltd., reinforcing carbon nanofiber, average fiber length 8.0 μm, aspect ratio 32) added was 16.41 parts by mass. The results are shown in Table 1.

[0043] Comparative Example 3 The evaluation was carried out in the same manner as in Comparative Example 1, except that the amount of hydrophobic fiber (carbon nanofiber, manufactured by Almedio Co., Ltd., reinforcing carbon nanofiber, average fiber length 8.0 μm, aspect ratio 32) added was 32.98 parts by mass. The results are shown in Table 1.

[0044] Comparative Example 4 Evaluation was performed in the same manner as in Comparative Example 1, except that the hydrophobic fiber used was a hydrophobic fiber (carbon fiber (milled fiber), manufactured by Mitsubishi Chemical Corporation, K223HM, average fiber length 50 μm, aspect ratio 4.5) and the amount added was 5.04 parts by mass. The results are shown in Table 1.

[0045] <Preparation of vinyl chloride resin composition molding sample> Using the hydrophobic fiber-containing vinyl chloride resins produced in Examples 1 to 4 and Comparative Examples 1 to 4 after dehydration and drying, 2.5 parts by mass of a heat stabilizer (TVS8570, manufactured by Nitto Kasei Co., Ltd.) and 0.5 parts by mass of a lubricant (WAX-OP, manufactured by Hoechst Japan Co., Ltd.) were stirred and mixed with the hydrophobic fiber-containing vinyl chloride resins having weights shown in Table 1 to obtain polyvinyl chloride resin compounds. The obtained compounds were kneaded for 2 minutes after winding at 185°C in a 6-inch roll molding machine, and then formed into a sheet with a thickness of 1 mm, which was then pressed into a press molding machine (195°C preheating for 3 minutes - pressurization for 3 minutes) to obtain vinyl chloride resin composition molded samples.

[0046] [Table 1]

Claims

1. A method for suspension polymerization of a vinyl chloride resin, comprising a step of suspension polymerizing a vinyl chloride monomer alone or a vinyl chloride monomer mainly composed of a vinyl chloride monomer in the presence of hydrophobic fibers having a fiber length of 0.001 μm to 200 μm.

2. 2. The method for suspension polymerization of a vinyl chloride resin according to claim 1, wherein the hydrophobic fiber is at least one selected from the group consisting of polyester fiber, polyethylene terephthalate fiber, carbon nanotube, and carbon nanofiber.

3. 3. The method for suspension polymerization of a vinyl chloride resin according to claim 2, wherein the hydrophobic fiber is a carbon nanofiber.

4. 2. The method for suspension polymerization of a vinyl chloride resin according to claim 1, wherein the amount of the hydrophobic fiber added is 0.1 to 100 parts by mass based on 100 parts by mass of the vinyl chloride monomer.

5. 4. The method for suspension polymerization of a vinyl chloride resin according to claim 3, wherein the aspect ratio of the carbon nanofibers is 1 to 1,000.

6. 2. The method for suspension polymerization of a vinyl chloride resin according to claim 1, wherein the step of suspension polymerization is carried out in an aqueous medium containing a dispersant.

7. A vinyl chloride resin obtained by the suspension polymerization method for a vinyl chloride resin according to any one of claims 1 to 6, The content of the hydrophobic fiber is 1 to 50 parts by mass per 100 parts by mass of the vinyl chloride monomer.

8. The polyvinyl chloride resin according to claim 7, wherein the inclusion rate of the hydrophobic fibers is 50.0% by mass to 99.0% by mass.

9. A vinyl chloride resin molded article comprising the vinyl chloride resin according to claim 7.

Citation Information

Patent Citations

  • Production of polyvinyl chloride composition

    JP1982192412A