Water-based coating composition and method for forming multilayer coating film

The water-based coating composition with controlled viscosity and thixotropic agent, combined with high-boiling organic solvents, addresses adhesion and workability issues in water-based paints, resulting in superior film appearance and application performance.

JP2024146708APending Publication Date: 2024-10-15DAI NIPPON TORYO CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023169819
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2023-09-29
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Conventional water-based paints exhibit poor adhesion to plastic surfaces and have low workability due to their hydrophilic nature, leading to issues with coating film appearance and ease of application.

Method used

A water-based coating composition with specific viscosity behavior and the inclusion of a thixotropic agent, adjusted to maintain high shear viscosities at different time intervals, along with the use of organic solvents with high boiling points for improved adhesion and pigment orientation.

Benefits of technology

The composition achieves excellent coating film appearance and workability by ensuring uniform pigment arrangement and preventing sagging, while maintaining low VOC emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146708000004
    Figure 2024146708000004
  • Figure 2024146708000005
    Figure 2024146708000005
  • Figure 2024146708000001
    Figure 2024146708000001
Patent Text Reader

Abstract

To provide a water-based coating composition excellent in coating film appearance and workability during coating, and a method for forming a multilayer coating film.SOLUTION: The water-based coating composition of the present invention contains water, resin, and at least one of a bright pigment and a coloring pigment. When the viscosity of the water-based coating composition is adjusted to 65 KU at a measurement temperature of 25°C, the ratio V2 / V1 between the shear viscosity V1 at time T1 60 seconds after the shear rate is set to 1000 sec-1 and the shear viscosity V2 at time T2 one second after time T1 when the shear rate is set to 0.1 sec-1 is 10 or more, and the ratio V3 / V2 of the shear viscosity V2 at time T2 to the shear viscosity V3 at time T3 one second after time T2 is 1.3 or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a water-based coating composition and a method for forming a multi-layer coating film. [Background technology]

[0002] Conventionally, organic solvent-based paints have generally been used to paint plastic materials (for example, Patent Document 1). Organic solvent-based paints contain an organic solvent that etches the surface of the plastic material, and the coating film formed adheres well to the etched surface due to the anchor effect, making them suitable as paints for plastics. However, organic compounds (hereinafter also referred to as VOCs) in paints are released into the atmosphere during painting and drying, which has the drawback of polluting the air and becoming a major environmental problem, and in line with the trend toward stricter VOC regulations, there is an active trend toward solvent-free (VOC-free) paints in various industries.

[0003] In recent years, the paint industry has been shifting from organic solvent-based paints to water-based paints that contain little or no VOCs, against the backdrop of these global environmental issues. Also, in the field of automotive interiors, the introduction of water-based paints is being promoted, taking into consideration the effects on the human body of organic solvents released from coatings and adhesives applied to interior materials in rooms that tend to be closed spaces, and people who suffer from chemical hypersensitivity.

[0004] Plastic materials are mainly used in automotive interior parts and home appliances, but water-based paints do not contain sufficient organic solvents that etch the surface of plastic materials as described above, and therefore tend to have lower adhesion to the plastic surface than organic solvent-based paints.

[0005] For example, Patent Document 2 discloses an aqueous coating composition, which is a glittering pigment dispersion containing water, a scaly aluminum pigment, and a cellulose-based viscosity modifier, and a method for forming a multilayer coating film using the same. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2018-069185 A [Patent Document 2] International Publication No. 2017 / 175468 Summary of the Invention [Problem to be solved by the invention]

[0007] However, the invention described in Patent Document 2 is limited to a metallic water-based paint containing a cellulose-based viscosity modifier. In addition, the water-based paint composition uses a hydrophilic resin suitable for water-based paint compositions, which causes problems such as easy dripping and poor workability during painting. Thus, the conventional water-based paint composition and coating film forming method still have room for improvement in the appearance of the coating film after painting. The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a water-based coating composition and a method for forming a multi-layer coating film which are excellent in coating film appearance and workability during painting. [Means for solving the problem]

[0008] The present invention is a coating composition containing water, a resin, and at least one of a bright pigment and a coloring pigment, and is an aqueous coating composition having the following viscosity behaviors (a) and (b) when the viscosity at a measurement temperature of 25°C is adjusted to 65 KU. (a) Shear rate is 1000 sec -1 The shear viscosity V1 at time T1 60 seconds after the shear rate was increased to 0.1 sec -1 and V2 / V1, which is the ratio of the shear viscosity V2 at time T2, one second after time T1, is 10 or more. (b) The ratio V3 / V2 of the shear viscosity V2 at time T2 to the shear viscosity V3 at time T3, which is one second after time T2, is 1.3 or more.

[0009] The solid hydroxyl value of the acrylic resin is preferably 2% or less.

[0010] The water-based coating composition further contains a thixotropic agent, and the solid content of the thixotropic agent in the water-based coating composition is preferably 0.1% by mass or more and 1.5% by mass or less.

[0011] The method for forming a multilayer coating film of the present invention is a method for forming a multilayer coating film, comprising: a base coating film forming step of applying the aqueous coating composition of the present invention onto a substrate to form a wet base coating film; a topcoat coating film forming step of applying a topcoat coating composition onto the resulting wet base coating film to form a wet topcoat coating film; and a drying step of simultaneously drying the resulting wet base coating film and wet topcoat coating film to form a multilayer coating film. Effect of the Invention

[0012] According to the present invention, it is possible to obtain a water-based coating composition and a method for forming a multi-layer coating film which are excellent in coating film appearance and workability during painting. [Brief description of the drawings]

[0013] [Figure 1] 1 is a graph showing the shear viscosity of one embodiment of the water-based coating composition of the present invention. [Diagram 2] 2 is an enlarged graph of a portion of the graph shown in FIG. 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The water-based coating composition of the present invention will now be described in detail.

[0015] [Water-based paint composition] The aqueous coating composition of the present invention is a coating composition containing water, a resin, and at least one of a glittering pigment and a coloring pigment, and when the viscosity at a measurement temperature of 25°C is adjusted to 65 KU, the aqueous coating composition has the following viscosity behaviors (a) and (b): (a) Shear rate is 1000 sec -1The shear viscosity V1 at time T1 60 seconds after the shear rate was increased to 0.1 sec -1 and V2 / V1, which is the ratio of the shear viscosity V2 at time T2, one second after time T1, is 10 or more. (b) The ratio V3 / V2 of the shear viscosity V2 at time T2 to the shear viscosity V3 at time T3, which is one second after time T2, is 1.3 or more. Here, "measurement temperature 25°C" refers to a state in which both the environmental temperature and the liquid temperature of the composition are 25°C. First, the components of the water-based coating composition will be described below.

[0016] <Water> In this specification, the term "water-based coating composition" refers to a coating composition that contains water as the main solvent. By "main solvent" it is meant that the proportion of the solvent used, i.e. water, is at least 50% by mass or more. The water used in the aqueous coating composition of the present invention is not particularly limited, and examples thereof include pure water such as ion-exchanged water and distilled water, groundwater, tap water, industrial water, etc. Furthermore, when the aqueous coating composition is to be stored for a long period of time, water that has been sterilized by ultraviolet irradiation or the like may be used in order to prevent the growth of mold and bacteria.

[0017] (Organic solvent) The water-based coating composition of the present invention may contain an organic solvent. The content of the organic solvent in the water-based coating composition is preferably 15% by mass or less, most preferably 10% by mass. From the viewpoint of reducing VOC, it is preferable that the content of the organic solvent is small, but by using a small amount of the organic solvent, for example, the adhesion to the plastic substrate can be improved, and in the case of a water-based metallic coating composition, the dispersibility of the scaly metal pigment in the composition and the film-forming property of the water-based metallic coating composition can be maintained well. The organic solvent that can be used in the water-based coating composition of the present invention is not particularly limited, and various hydrophilic or hydrophobic organic solvents can be used.

[0018] As the hydrophilic organic solvent, for example, it is preferable to use an alcohol solvent or a glycol ether solvent. Examples of the alcohol solvent include isobutyl alcohol, n-butyl alcohol, isoamyl alcohol, n-amyl alcohol, hexyl alcohol, 2-ethylbutyl alcohol, methylamyl alcohol, cyclohexanol, 2-ethylhexyl alcohol, octyl alcohol, benzyl alcohol, dimethylaminoethanol, butanol, etc., and examples of the glycol ether solvent include ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, tetraethylene glycol dimethyl ether, etc.

[0019] Examples of the hydrophobic organic solvent include 2-ethylhexanol, dipropylene glycol monobutyl ether, and ethylene glycol monobutyl ether acetate. Of the organic solvents in the water-based coating composition, the ratio of hydrophilic organic solvents:hydrophobic organic solvents is preferably 100:0 or more and 33:67 or less.

[0020] When the water-based coating composition of the present invention is directly applied to a plastic substrate, it is preferable that the coating composition contains 0.5 to 5.0 mass% of an organic solvent having a high boiling point and high solubility in the substrate. In the case of a water-based coating, the content of the organic solvent is low compared to an organic solvent-based coating, so it is considered that the effect of etching the surface of a plastic substrate is small. However, by using an organic solvent having a high boiling point and high solubility in the substrate, the time that the highly soluble solvent remains on the substrate after coating is extended, so that even a small amount of the organic solvent is considered to show a high etching effect.

[0021] The high boiling point organic solvent preferably has a boiling point of 160° C. or higher, and particularly preferably in the range of 180 to 300° C. Examples of such organic solvents include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, butyl glycol acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, diethylene glycol monopropyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol ethyl methyl ether, diethylene glycol dibutyl ether, diethylene glycol butyl methyl ether, dipropylene glycol monomethyl ether, triethylene glycol monomethyl ether, triethylene glycol butyl methyl ether, triethylene glycol dimethyl ether, tripropylene glycol monomethyl ether, tetraethylene glycol dimethyl ether, and polyethylene glycol dimethyl ether.

[0022] An organic solvent that has high solubility in a substrate is an organic solvent that can dissolve the surface of a plastic substrate when dropped onto it, and has an SP value (solubility parameter) of 20.0 (J / cm 3 ) 1 / 2 It is preferable that the concentration is 18.0 (J / cm 3 ) 1 / 2 More preferably, the organic solvent is a glycol-based organic solvent, and more preferably, a water-soluble glycol-based organic solvent. Examples of organic solvents having a high boiling point and high solubility in the substrate include triethylene glycol butyl methyl ether (boiling point: 261°C, SP value: 16.6), diethylene glycol diethyl ether (boiling point: 189°C, SP value: 17.8), diethylene glycol dimethyl ether (boiling point: 162°C, SP value: 18.2), diethylene glycol butyl methyl ether (boiling point: 212°C, SP value: 16.1), and tetraethylene glycol dimethyl ether (boiling point: 275°C, SP value: 17.5).

[0023] The SP value is a guideline for determining compatibility, and there are various calculation and measurement methods. In this specification, the SP value is the Hansen solubility parameter value, and is calculated using the Y-MB method.

[0024] -How to calculate the average SP value- When a plastic substrate is composed of n types of polymerizable compounds, the SP values ​​of each polymerizable compound are SP1, SP2, ..., SPn, and the mass fractions of each polymerizable compound are W1, W2, ..., Wn (W1+W2+...+Wn=1), and the average SP value can be calculated using the following formula: Average SP value = SP1 x W1 + SP2 x W2+...+SPn x Wn

[0025] -Solid content of water-based paint composition- The solid content of the aqueous coating composition of the present invention is preferably 5% by mass or more and 30% by mass or less when the viscosity is adjusted to 65KU. In addition, when a glittering pigment is contained, it is particularly preferably 8% by mass or more and 20% by mass or less. By setting the solid content of the aqueous coating composition in the above range, the orientation of the pigment and the sagging during coating can be improved.

[0026] The aqueous coating composition of the present invention can be prepared by mixing various components appropriately selected as necessary. The aqueous coating composition of the present invention may be a one-component type or a two-component type, but is preferably used as a one-component type from the viewpoint of eliminating the need to consider the labor of mixing during coating and the usable time.

[0027] <Resin> The resin used in the water-based coating composition of the present invention is appropriately selected in consideration of the application, etc., and is not particularly limited, but examples thereof include acrylic resin, epoxy resin, urethane resin, alkyd resin, polyester resin, silicone resin, etc., and known resins such as amino resin, melamine resin, isocyanate resin, urea resin, etc. as a crosslinking component. When making a one-liquid type water-based coating composition, it is preferable to use acrylic resin, urethane resin, etc., taking into consideration the orientation of the pigment and the coating workability. The resin in the present invention may be used alone or in combination of two or more types.

[0028] (Acrylic resin) The acrylic resin contained in the aqueous coating composition of the present invention may be any resin having one or more (meth)acrylic monomers as constituent units, and may contain monomers other than (meth)acrylic monomers as constituent units as long as the effects of the present invention are not impaired. The (meth)acrylic monomer means a monomer having a (meth)acryloyl group, such as (meth)acrylic acid, (meth)acrylic acid ester, etc. For example, the constituent monomer of the acrylic resin used in the present invention is preferably an alkyl ester of (meth)acrylic acid, and the alkyl group in this ester preferably has 1 to 10 carbon atoms, particularly preferably 1 to 8 carbon atoms, and a functional group may be introduced into this alkyl group, or this alkyl group may be a cyclic group. Examples of such constituent monomers include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, t-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, stearyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, glycidyl (meth)acrylate, cyclopentyl (meth)acrylate, and cyclohexyl (meth)acrylate.

[0029] Examples of the resin form of the acrylic resin include an acrylic emulsion resin which can be produced by an emulsion polymerization method, and an aqueous acrylic dispersion resin which can be produced by a solution polymerization method in a common organic solvent.

[0030] - Weight average molecular weight Mw of acrylic resin - The weight average molecular weight Mw of the acrylic resin is not particularly limited, but is preferably 50,000 or more, and more preferably 100,000 or more. The weight average molecular weight Mw of the acrylic resin can be measured by SEC (size exclusion chromatography, product name "HLC-8420GPC", manufactured by Tosoh Corporation) equipped with a differential refractive index (RI) detector using a TSKgel column SuperMultiporeHZ-M (manufactured by Tosoh Corporation). The SEC conditions are tetrahydrofuran as the developing solvent, a flow rate of 0.35 ml / min, and a temperature of 40°C, and TSK standard polystyrene (manufactured by Tosoh Corporation) is used as the standard substance. In general, emulsion resins obtained by emulsion polymerization tend to have large molecular weights, and emulsion resins having a crosslinked structure in particular cannot be accurately measured by gel permeation chromatography, so the molecular weight is set to 100,000 or more in this specification.

[0031] -Hydroxyl value of acrylic resin- In the water-based coating composition of the present invention, when it is used as a one-component coating, the hydroxyl value of the solid content of the acrylic resin is preferably 2% or less. If the hydroxyl value of the solid content of the acrylic resin exceeds 2%, many hydroxyl groups remain in the coating film, resulting in a decrease in water resistance.

[0032] (urethane resin) The urethane resin used in the water-based coating composition of the present invention can be any conventionally known urethane resin without any particular limitation. For example, there can be mentioned a urethane resin obtained by reacting at least one diisocyanate compound selected from the group consisting of aliphatic diisocyanate compounds, alicyclic diisocyanate compounds, and aromatic diisocyanate compounds with at least one polyol compound selected from the group consisting of polyether polyol, polyester polyol, and polycarbonate polyol; a urethane resin obtained by reacting the above acrylic resin, polyester resin, or epoxy resin with a dipolyisocyanate compound to obtain a high molecular weight; and the like.

[0033] <Luminous pigment or color pigment> The water-based coating composition of the present invention contains at least one of a bright pigment and a coloring pigment. The luster pigment and coloring pigment are appropriately selected depending on the color and luster of the coating film, painting workability, strength and physical properties of the coating film, etc.

[0034] (Luminous pigment) The luster pigment means a pigment that gives a metallic luster to the coating film by reflection or interference of light, and examples thereof include aluminum powder pigments, nickel powder pigments, gold powder, silver powder, bronze powder, copper powder, stainless steel powder pigments, mica pigments, graphite pigments, glass flake pigments, metal-coated glass powder, metal-coated mica powder, metal-coated plastic powder, and scaly iron oxide pigments, and aluminum pigments are particularly preferred. The luster pigment may be used alone or in combination of two or more types, and is preferably 5% by mass or more and 30% by mass or less, and more preferably 7% by mass or more and 20% by mass or less, in the solid content of the coating composition.

[0035] (Color pigments) The color pigment is not particularly limited, and pigments commonly used in the paint industry can be used. Specific examples include inorganic pigments such as titanium dioxide, iron oxide, and carbon black, and organic pigments such as phthalocyanine pigments and azo pigments. The color pigment may be used alone or in combination of two or more, and is preferably 30% by mass or more and 70% by mass or less, more preferably 40% by mass or more and 60% by mass or less, based on the solid content of the paint composition.

[0036] (Extender pigment) The water-based coating composition of the present invention may contain a body pigment. Examples of the body pigment include silica, talc, mica, calcium carbonate, barium sulfate, clay, etc. Among them, by containing a body pigment with an oil absorption of 5 to 30 ml / g, more preferably 5 to 20 ml / g, the viscosity is unlikely to become high even in the case of a coating composition with a relatively high solid content, so that the coating workability is excellent and the amount of coating composition to be applied to obtain a target film thickness can be reduced. In the water-based coating composition of the present invention, the amount of the body pigment in the solid content is preferably 1% by mass or more and 50% by mass or less. The body pigment may be used alone or in combination of two or more kinds. The body pigment may be used from the viewpoint of adjusting the gloss of the coating film.

[0037] <Other ingredients> To the aqueous coating composition of the present invention, various additives commonly used in the field of coatings, such as crosslinking components, thixotropic agents, dispersants, thickeners, neutralizing agents, defoamers, surface conditioners, emulsifiers, surfactants, silane coupling agents, pH adjusters, and preservatives, may be added within limits that do not impair the effects of the present invention.

[0038] (crosslinking component) When the substrate to be coated is metal, the water-based coating composition of the present invention can be baked at high temperatures, and therefore may contain acrylic resins, amino resins, melamine resins, urea resins, etc., which have a high hydroxyl value. In addition, in the aqueous coating composition of the present invention, a blocked polyisocyanate can be used when improving the storage stability of the coating at room temperature or when coating and drying a plastic material such as polyimide having excellent heat resistance. From the viewpoints of storage stability and workability, such as ease of uniform mixing with the aqueous acrylic resin, it is more preferable to use a water-dispersible blocked polyisocyanate.

[0039] (thixotropic agent) The aqueous coating composition of the present invention can use any conventionally known thixotropic agent as the thixotropic agent without any particular limitation. For example, polymer association type thixotropic agent, alkali thickening type thixotropic agent, polyamide type thixotropic agent, polyethylene type thixotropic agent, bentonite type thixotropic agent, etc. can be mentioned. Among them, it is preferable to contain at least one of polymer association type thixotropic agent, alkali thickening type thixotropic agent, and polyamide type thixotropic agent. The thixotropic agent imparts thixotropic properties to the coating material, so that sagging during coating is unlikely to occur, the film thickness per coating can be increased, and further, the thixotropic agent is added for the purpose of improving workability by reducing the viscosity of the coating material during coating. The thixotropic agent may be used alone or in combination of two or more types.

[0040] -Solid content of thixotropic agent- When the viscosity of the aqueous coating composition is adjusted to 65 KU at a measurement temperature of 25° C., the solid content of the thixotropic agent in the aqueous coating composition is preferably 0.1% by mass to 1.0% by mass, more preferably 0.3% by mass to 0.9% by mass. When the content of the thixotropic agent is within the above range, the viscosity behavior described below is easily obtained, and therefore a coating film having excellent coating workability and excellent appearance can be formed.

[0041] Commercially available thixotropic agents include, for example, trade names "AS1130", "AS1137", and "AS1180" (all manufactured by BASF), trade names "RHEOBYK H7625VF", "RHEOBYK L1400VF", "RHEOBYK-420", and "RHEOBYK-425" (all manufactured by BYK-Chemie), trade names "ACRYSOL RM-8W" and "ACRYSOL RM-12W" (all manufactured by DOW Chemical), trade names "Thixol 53L", "Viscoatex 46", "Viscoatex 146", "Viscoatex 730", "Viscoatex146", "Lheotech 4800", "Coapur XS83", "Coapur 6050", "Coapur Examples of such polyester resins include "830W" and "BR100P" (both manufactured by COATEX Co., Ltd.), trade name "Nopal 3303" (manufactured by San Nopco Ltd.), and trade name "Disparlon 4200-20" (manufactured by Kusumoto Chemicals Co., Ltd.).

[0042] (Dispersant) The dispersant is not particularly limited, and commercially available dispersants for water-based paints such as the BYK series (manufactured by BYK-Chemie), the EFKA series (manufactured by EFKA Chemical), and the FLOWRENE series (manufactured by Kyoeisha Chemical Co., Ltd.) can be used.

[0043] (Neutralizer) The aqueous coating composition of the present invention is preferably neutralized with ammonia or an amine-based neutralizing agent in terms of water resistance, dispersion stability, reactivity, weather resistance, contamination resistance, etc. The amine-based neutralizing agent is not particularly limited as long as it can neutralize the acidic group, and examples thereof include diethylamine, triethylamine, monoethanolamine, diethanolamine, triethanolamine, dimethylethanolamine, diethylethanolamine, isopropylethanolamine, diisopropanolamine, 2-amino-2-methylpropanol, 2-(dimethylamino)-2-methylpropanol, morpholine, N-methylmorpholine, and N-ethylmorpholine. The neutralizing agent is preferably added in an amount such that the pH of the aqueous coating composition after neutralization is about 6.5 to 9.0.

[0044] (Antifoaming agent) The water-based coating composition of the present invention may contain a defoaming agent. The defoaming agent may be any commercially available one, but it is preferable to use one that has little odor. The defoaming agent is generally classified into mineral oil type, silicone type, polyether type, etc. according to the carrier oil, and usually contains a carrier and a nucleating agent such as hydrophobic silica, wax, amide, metal soap, etc. as a constituent. The amount of the defoaming agent in the aqueous coating composition of the present invention is preferably 0.01% by mass or more and 5% by mass or less. The defoaming agents may be used alone or in combination of two or more kinds.

[0045] (Surface conditioner) Examples of the surface conditioner include silicone-based, acrylic-based, vinyl-based, and fluorine-based surface conditioners. From the viewpoint of the metallic luster and water resistance of the resulting coating film, silicone-based surface conditioners are preferred. As the silicone-based surface conditioner, polydimethylsiloxane and modified silicone obtained by modifying it are used. As the modified silicone, polyether-modified silicone, acrylic-modified silicone, polyester-modified silicone, etc. can be mentioned. The surface conditioner may be used alone or in combination of two or more. An example of a commercially available surface conditioner is SURFYNOL SF104BC (acetylene dialcohol-based surface conditioner, manufactured by EVONIK).

[0046] <Solid content in water-based paint composition> The solids concentration in the water-based coating composition, when adjusted to 65 KU (approximately 430 mPa·s in mPa), is preferably 5% by mass or more and 30% by mass or less, and more preferably 7% by mass or more and 25% by mass or less.

[0047] <Viscosity> The viscosity of the water-based coating composition of the present invention varies depending on the coating method and coating conditions, but for example, in the case of rotary disk coating using a bell-shaped coating gun, it can be suitably used in the range of 60 KU to 70 KU (approximately 0.30 Pa·s to approximately 0.58 Pa·s in mPa equivalent) at a measurement temperature of 25° C., and in the case of air spray coating, it can be suitably used in the range of 40 KU to 50 KU (approximately 0.10 Pa·s to approximately 0.18 Pa·s in mPa equivalent) at a measurement temperature of 25° C. A diluent such as water can be used to adjust the viscosity. When the viscosity of the water-based coating composition during coating is 40 KU or more and 70 KU or less, it is suitable for coating uneven or flowing substrates such as automobile parts. The viscosity of the water-based coating composition is a value measured using a Stormer viscometer at a measurement temperature of 25°C in accordance with JIS K 5600-2-2:1999.

[0048] <Viscosity behavior> The viscosity behavior of the water-based coating composition of the present invention will now be described. The water-based coating composition of the present invention has the following viscosity behaviors (a) and (b) when the viscosity at a measurement temperature of 25° C. is adjusted to 65 KU. (a) Shear rate is 1000 sec -1 The shear viscosity V1 at time T1 60 seconds after the shear rate was increased to 0.1 sec -1and V2 / V1, which is the ratio of the shear viscosity V2 at time T2, one second after time T1, is 10 or more. (b) The ratio V3 / V2 of the shear viscosity V2 at time T2 to the shear viscosity V3 at time T3, which is one second after time T2, is 1.3 or more.

[0049] The shear viscosity at each time is a value measured using a rheometer (MCR rheometer manufactured by Anton Parr) or the like after adjusting the liquid temperature to 25°C.

[0050] "Shear rate is 1000sec -1 "At high shear rates" refers to high shear rates during coating. When the viscosity was adjusted to 65KU at a measurement temperature of 25°C, the shear rate was 1000sec -1 In this case, the shear viscosity V1 of the aqueous coating composition at time T1 is preferably 0.01 Pa s or more and 0.5 Pa s or less, and more preferably 0.01 Pa s or more and 0.2 Pa s or less. In the case of such a high shear rate, a low shear viscosity V1 within the above range means that the workability during coating is good.

[0051] Next, the shear rate was increased to 1000 sec -1 At time T1, 60 seconds after the shear rate was increased to 0.1 sec -1 "When held at low shear rate" refers to a state of low shear rate, such as when left to stand after coating. Shear rate: 0.1sec -1 The shear viscosity V2 at time T2, 1 second after time T1, is preferably 1.5 Pa s or more and 10 Pa s or less, and more preferably 1.5 Pa s or more and 6 Pa s or less. When the shear viscosity V2 is in the above range, the pigments tend to align uniformly in the wet coating film immediately after application, and the appearance of the coating film after formation is good.

[0052] Furthermore, the shear viscosity V3 at time T3, 1 second after time T2, is preferably 2 Pa s to 15 Pa s, more preferably 2 Pa s to 8 Pa s. When the shear viscosity V3 is in the above range, the sagging properties after painting and the appearance of the paint are good.

[0053] The aqueous coating composition of the present invention has a ratio of shear viscosity V1 to shear viscosity V2, V2 / V1, of 10 or more (above (a)), and therefore the viscosity increases significantly within 1 second after application, making it easy for the pigments to align uniformly and enabling the production of a coating film with excellent appearance. V2 / V1 is more preferably 15 or more, and even more preferably 20 or more.

[0054] The aqueous coating composition of the present invention has a ratio of shear viscosity V2 to shear viscosity V3, V3 / V2, of 1.3 or more (above (b)), so that a coating film with good appearance can be obtained without sagging of the coating. It is more preferable that V3 / V2 is equal to or greater than 1.4 and equal to or less than 3.0.

[0055] [Multi-layer coating film formation method] The method for forming a multilayer coating film of the present invention is a method for forming a multilayer coating film, comprising: a base coating film forming step of applying the aqueous coating composition of the present invention onto an object to be coated and forming a wet base coating film; a topcoat coating film forming step of applying a topcoat coating composition onto the obtained wet base coating film and forming a wet topcoat coating film; and a drying step of simultaneously drying the obtained base coating film and topcoat coating film to form a multilayer coating film.

[0056] <Object to be coated> The substrates to which the aqueous coating composition of the present invention is applied include plastic substrates such as epoxy resins, ABS resins, polycarbonates, polyvinyl chloride, polystyrene, acrylic resins, such as polymethyl methacrylate (PMMA), polyethylene terephthalate (PET), polyolefins, such as polypropylene (PP), metal substrates such as steel, galvanized steel, tinned steel, stainless steel, magnesium alloys, aluminum, aluminum alloys, titanium, titanium alloys, inorganic substrates other than metals, such as cement, mortar, concrete, slate, gypsum, calcium silicate, glass, ceramics, calcium carbonate, marble, artificial marble, wood substrates, composite substrates such as combinations of two or more of these substrates, etc. Examples of composite substrates include composite substrates such as wood fiber reinforced cement boards, fiber reinforced cement boards, fiber reinforced cement-calcium silicate boards, metal substrates that have been subjected to various surface treatments, such as oxidation treatments, and plastic substrates whose surfaces are coated with inorganic substances (for example, plastic substrates coated with glass). Furthermore, the above-mentioned substrate may be subjected to various surface treatments, and at least a part of the substrate surface may have an undercoat coating film such as a conductive primer or an old coating film (a coating film that has already been formed before the coating composition of the present invention is applied).

[0057] <Topcoat paint composition> The topcoat paint composition is not particularly limited, and any commonly used topcoat paint can be used. Examples of resins used in the topcoat paint include acrylic resins, fluorine resins, urethane resins, epoxy resins, organic modified silicone resins (e.g., acrylic silicone resins), polyester resins, and melamine resins, and it is particularly preferable to use acrylic resins and urethane resins. In addition, in order to make the most of the appearance of the coating film formed from the water-based paint composition of the present invention, it is preferable that the topcoat paint composition is a clear paint.

[0058] The method for applying the water-based coating composition and the topcoat coating composition is not particularly limited, and known methods such as air spray coating, airless spray coating, rotary disk coating, etc. Also, a method in which electrostatic charge is applied during coating to increase the coating efficiency may be used.

[0059] The dry film thickness of the water-based coating composition of the present invention is, for example, preferably 5 μm to 40 μm, more preferably 5 μm to 30 μm. By having a dry film thickness of 5 μm or more, it is easy to obtain a continuous and uniform film that is not too thin, and the color of the base can be completely concealed. On the other hand, by having a dry film thickness of 40 μm or less, defects such as so-called popping and dripping are unlikely to occur during drying, so a normal dry film can be obtained.

[0060] Before the base coating film forming step of the present invention, a step of forming a primer on the substrate may be included. As the primer, for example, a conductive primer is preferably applied from the viewpoint of the coating efficiency of electrostatic coating. When the coating composition of the present invention is applied as a base coat coating, it is preferable to apply the conductive primer so that the dry film thickness is 10 to 100 μm. EXAMPLES

[0061] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited thereto.

[0062] [Examples 1 to 14, Comparative Examples 1 to 6] The preparation of the coating compositions of the examples and comparative examples will be described. The raw materials and the amounts used in the coating compositions are shown in Tables 1 to 3. The values ​​in the tables are in mass %. Here, the solid content refers to the components remaining in the coating film when the coating film is formed. Each of the raw materials shown in Tables 1 to 3 was mixed using a disperser so as to be uniformly dispersed, to obtain each coating composition.

[0063] Details of the raw materials listed in Table 1 are as follows: (1) Resin Acrylic resin: NeoCry A639 (DSM, solid content: 45%, hydroxyl value: less than 1.0%) Urethane resin 1: DAOTAN TW6450 / 30WA (manufactured by Daicel Allnex, solid content: 35%) Urethane resin 2: Bayhydrol UH2606 (manufactured by Covestro, solid content: 35%) Urethane resin 3: Watersol WTW-315 (DIC, solid content: 41.5%) Melamine resin: Maprenal MF 927 / 70IB (Prefere Resins, solids content: 70%)

[0064] (2) Pigments Luminescent pigment: EMR-DZ460 (manufactured by Toyo Aluminum, NV: 56%, silica-coated aluminum pigment) Color pigment: R960 (DuPont, titanium dioxide) Extender pigment: BF-21 (Sakai Chemical Co., Ltd., barium sulfate)

[0065] (3) Thixotropic agent Alkaline thickening thixotropic agent 1: AS1137 (BASF, NV: 30%) Alkaline thickening thixotropic agent 2: AS1180 (BASF, NV: 30%) Alkaline thickening agent 3: Viscoatex 146 (manufactured by COATEX, NV: 28%) Hydrophobic urethane association type: Coapur 6050 (manufactured by COATEX, NV: 50%) Urethane association type: RHEOBYK-425 (BYK-Chemie, NV: 50%)

[0066] (4) Other additives Dispersant 1: XL250 (Allnex, NV: 47%) Dispersant 2: DISPERBYK-190 (BYK, NV: 40%) Defoamer: BYK024 (BYK-Chemie, NV: 96%) Surface conditioner: SURFYNOL SF104BC (EVONIK, NV: 49%)

[0067] (5) Solvent Water-soluble organic solvent 1: Ethylene glycol monobutyl ether (boiling point: 171°C, SP value: 20.8) Water-soluble organic solvent 2: Dimethylaminoethanol Water-soluble organic solvent 3: Butanol Water-soluble organic solvent 4: Triethylene glycol butyl methyl ether (boiling point: 261°C, SP value: 16.6) Water-soluble organic solvent 5: Diethylene glycol diethyl ether (boiling point: 189°C, SP value: 17.8) Non-water-soluble organic solvent 1: Diethylene glycol butyl methyl ether (boiling point: 212°C, SP value: 16.1) Water-soluble organic solvent 6: Ethylene glycol monomethyl ether (boiling point: 124°C, SP value: 24.8) Water-soluble organic solvent 7: Ethylene glycol dimethyl ether (boiling point: 85°C, SP value: 17.6)

[0068] [Evaluation of paint properties and coating appearance] The coating compositions obtained in the above Examples and Comparative Examples were evaluated as follows. The evaluation results are shown in Tables 1 to 3. The "paint properties after viscosity adjustment (65KU)" refers to the paint properties when water was added to 100 parts by mass of each paint composition until the Stormer viscosity reached 65KU, and the amount of water added was the dilution amount. The viscosity at the time of viscosity adjustment was measured at 25°C using a digital Stormer viscometer (KU2, manufactured by Brookfield Corporation). The shear viscosity at each time point was measured using a rheometer (such as Anton Parr's MCR rheometer) after adjusting the liquid temperature to 25°C.

[0069] (Appearance of coating film in bell coating) The viscosity of each coating composition obtained in the above Examples and Comparative Examples was adjusted to 65KU, and then the coating was applied to a polypropylene plate under the following coating conditions using a "Mighty Robobell 21 rotary atomizer electrostatic coating machine" (manufactured by CFT Ransburg) so that the dry film thickness was 10 μm. <Painting conditions> Temperature / Humidity: 25℃ / 70RH% Bell cup diameter: Φ70 Discharge rate: 168cc / min Bell speed: 40,000 rpm Shaving air (in): 200kPa Shaving air (out): 200kPa Applied voltage: -60KV Number of coats: 6 passes (after 3 passes, there is an 82 second interval, then 3 passes again)

[0070] The finished appearance of the coating film was visually observed and rated according to the following criteria. <Evaluation criteria> A: The paint film has no unevenness in color when visually inspected, and no irregularities can be detected on the paint film surface, making the paint appearance excellent. B: Some unevenness in the color of the coating film is visible to the naked eye, but no irregularities are visible on the coating surface, and there are no practical problems with the appearance of the paint. C: Unevenness in the color of the coating film is visually observed, and unevenness can be confirmed on the coating film surface.

[0071] (Sagging immediately after bell painting) Each of the coating compositions obtained in the above Examples and Comparative Examples was applied under the above coating conditions, and after leaving it to stand for 180 seconds, a polypropylene plate was placed vertically and sagging was evaluated according to the following criteria. <Evaluation criteria> A: There is no dripping and the surface is smooth and uniform. B: Slight sagging of paint is observed but does not amount to dripping. C: Dripping has occurred and the base coat is partially visible.

[0072] (Appearance of the coating when sprayed) Each of the coating compositions obtained in the above Examples and Comparative Examples was diluted with water to a viscosity that allowed painting with an air spray, and then coated onto a polypropylene plate using an air spray at 25°C / 70RH% to give a dry film thickness of 10μm. The finished appearance was observed and evaluated according to the following criteria. <Evaluation criteria> A: The paint film has no unevenness in color when visually inspected, and no irregularities can be detected on the paint film surface, making the paint appearance excellent. B: Some unevenness in the color of the coating film is visible to the naked eye, but no irregularities are visible on the coating surface, and there are no practical problems with the appearance of the paint. C: Unevenness in the color of the coating film is visually observed, and unevenness can be confirmed on the coating film surface.

[0073] (Adhesion test to substrate) Each coating composition obtained in the above examples and comparative examples was diluted with water to a viscosity that allows coating with an air spray, and coated on an ABS plate (150 mm x 70 mm x 2 mm) using an air spray under conditions of 25 ° C / 70 RH% so that the dry film thickness is 20 μm, and dried at 100 ° C for 30 minutes to prepare a test specimen. According to JIS K5600-5-6:1999, the coating surface of each test specimen was cut with a cutter to create 100 squares of 2 mm squares, and an adhesive tape was attached on them, and then a forced peeling test was performed, and the number of remaining squares out of the 100 squares was counted, and evaluation was performed according to the following criteria. Incidentally, 100 / 100 indicates that the peeling area of ​​the coating film is 0%, and for example, 80 / 100 indicates that the peeling area of ​​the coating film is 20%. <Evaluation criteria> AA:100 / 100 A:90 / 100~99 / 100 B:70 / 100~89 / 100 C:69 / 100 or less

[0074] [Table 1]

[0075] [Table 2]

[0076] [Table 3]

[0077] As shown in Tables 1 to 3, in the examples where V2 / V1 was 10 or more and V3 / V2 was 1.3 or more, good results were obtained in all of the coating appearance (bell coating), sagging immediately after coating (bell coating), and coating appearance (air spray coating). Also, in Examples 15 to 17, in which an organic solvent with a high boiling point and high solubility in the substrate was added, the results showed that the coating had excellent adhesion to the ABS substrate.

Claims

1. A coating composition containing water, a resin, and at least one of a glittering pigment and a coloring pigment, the coating composition having the following viscosity behaviors (a) and (b) when the viscosity at a measurement temperature of 25°C is adjusted to 65 KU: (a) Shear rate: 1000 sec -1 The shear viscosity V1 at time T1 after 60 seconds has elapsed since the shear rate was set to 0.1 sec at the time T1. -1 and V2 / V1, which is the ratio of the shear viscosity V2 at time T2 one second after the time T1, is 10 or more. (b) The ratio V3 / V2 of the shear viscosity V2 at the time T2 to the shear viscosity V3 at a time T3 one second after the time T2 is 1.3 or more.

2. 2. The water-based coating composition according to claim 1, wherein the acrylic resin has a solid hydroxyl value of 2% or less.

3. 2. The aqueous coating composition according to claim 1, further comprising a thixotropic agent, the solid content of the thixotropic agent in the aqueous coating composition being 0.1% by mass or more and 1.5% by mass or less.

4. A base coating film forming step of coating an object to be coated with the aqueous coating composition according to any one of claims 1 to 3 to form a wet base coating film; A topcoat coating film forming step of applying a topcoat paint composition onto the obtained undried base coating film to form an undried topcoat coating film; and A drying step in which the obtained undried base coating film and the undried top coating film are simultaneously dried to form a multi-layer coating film. The method for forming a multi-layer coating film comprises the steps of:

Citation Information

Patent Citations

  • Multilayer coating film forming method and coating material composition

    JP2018069185A

  • Bright pigment dispersion and method for forming multilayer coating film

    WO2017175468A1