Wiping cloth

The use of ultrafine polyamide fibers and alkali-soluble polyester in a splittable conjugate fiber structure addresses the contamination and particle generation issues of conventional wiping tapes, providing high wiping performance and cleanliness for magnetic recording media.

JP2024146754APending Publication Date: 2024-10-15KB SEIREN LTD

Patent Information

Application Number
JP2024013462
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-01-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Conventional wiping tapes for magnetic recording media, such as hard disks, suffer from insufficient wiping performance due to the use of long fiber yarns with thick single fiber fineness and round cross-sections, leading to contamination and particle generation during friction, which can damage the media.

Method used

A wiping cloth composed of ultrafine polyamide fibers with a single filament fineness of 0.7 dtex or less, containing at least 40% by mass of polyamide fibers, and using a splittable conjugate fiber structure made of polyamide and alkali-soluble polyester without a matting agent, is woven to form a fabric that is treated with an alkaline solution to split and remove contaminants, resulting in a high-density and bulky structure.

Benefits of technology

The wiping cloth significantly reduces particle generation and residue, ensuring high wiping performance and cleanliness suitable for precision equipment, particularly in clean room environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146754000003
    Figure 2024146754000003
  • Figure 2024146754000004
    Figure 2024146754000004
  • Figure 2024146754000005
    Figure 2024146754000005
Patent Text Reader

Abstract

To provide a wiping cloth suitable for media cleaning applications that suppresses increasing particles due to friction during wiping, does not cause contamination problems, has high wiping performance, and leaves little residue.SOLUTION: A wiping cloth made of a fiber structure using ultrafine polyamide fibers is a wiping cloth in which a single yarn fineness of the polyamide ultrafine fiber is 0.7dtex or less, a content of polyamide ultrafine fibers in the entire wiping cloth is 40 mass% or more, and an average number of airborne particles having a diameter of 0.1 μm or more is 10 / cm2 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a wiping cloth that is suitable for use in cleaning media in magnetic recording media such as hard disks. [Background technology]

[0002] 2. Description of the Related Art Conventionally, for cleaning magnetic recording media such as hard disks, woven fabrics made of ultrafine fibers have often been used as wiping tapes.

[0003] The weft yarn in the wiping direction (perpendicular to the direction of travel) is mostly made of polyester single yarn or split yarn made of a polyester / polyamide composite fiber that has been split by chemical or physical treatment.

[0004] Compared to polyamide, polyester has excellent shape stability, less oligomer generation and dust pickup, and excellent processability in dyeing tanks, so polyester fibers are preferred for use in wiping tapes, and most wiping tapes contain more than 60% by mass of polyester.

[0005] Although polyamide is inferior to polyester in the above respects, it has strong abrasion resistance and generates less particles due to friction when wiping media. The use of polyamide is also preferable in that it generates less particles, but polyamide is prone to contamination by oligomers and the like (hereinafter referred to as contamination). Too much contamination can damage the media when wiping, so it was necessary to reduce contamination.

[0006] As a means for reducing contamination, it has been proposed to make a wiping tape using fibers that do not contain matting agents such as titanium oxide as the weft or warp (Patent Document 1). [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2017-147017 A Summary of the Invention [Problem to be solved by the invention]

[0008] Patent Document 1 states that long fiber yarn or split yarn not chemically split is used as the fiber not containing the matting agent, but the examples specifically cite long fiber yarn, not split yarn, and the long fiber yarn described in the examples has a thick single fiber fineness and a round fiber cross section, so the wiping performance is insufficient. In addition, as a split yarn not chemically split, a split yarn split due to the difference in shrinkage rate by heat treatment, which is a physical splitting process after weaving, is cited as the split yarn not chemically split. Split yarn obtained by physical splitting generates a thin peeling film at the split part, which causes self-dust generation and deteriorates the cleanness level.

[0009] The present invention has been made in consideration of the above-mentioned background art, and an object of the present invention is to provide a wiping cloth suitable for media cleaning applications, which suppresses an increase in particles due to friction during wiping, does not cause problems due to contamination, has high wiping properties, and leaves little unwiped residue. [Means for solving the problem]

[0010] The object of the present invention is to provide a wiping cloth made of a fiber structure using polyamide ultrafine fibers, the polyamide ultrafine fibers having a single yarn fineness of 0.7 dtex or less, a content of polyamide ultrafine fibers in the entire wiping cloth being 40 mass% or more, and an average number of airborne particles having a diameter of 0.1 μm or more being 10 particles / cm 2 This is achieved by the wiping cloth, which is as follows:

[0011] It is also preferred that the polyamide ultrafine fibers are polyamide fibers obtained by dissolving an alkali-soluble polyester resin of a splittable conjugate fiber that is composed of a polyamide component and an alkali-soluble polyester component and does not substantially contain a matting agent, and that the cross-sectional shape of the polyamide fiber is a modified cross-sectional shape.

[0012] The fiber structure is preferably a woven fabric using the polyamide ultrafine fibers as at least the weft.

[0013] The object of the present invention can also be achieved by a method for producing the wiping cloth, comprising the steps of weaving a fabric using, at least as a weft, a splittable conjugate fiber that is made of a polyamide component and an alkali-soluble polyester component and that is substantially free of a matting agent, and immersing the obtained fabric in an alkaline solution to dissolve the alkali-soluble polyester resin. Effect of the Invention

[0014] The wiping cloth of the present invention contains an extremely small amount of ultrafine particles, so there is no contamination. Furthermore, by containing a specific amount or more of polyamide fibers, an increase in particles due to friction during wiping is suppressed. Furthermore, by using ultrafine polyamide fibers with a single fiber fineness of 0.7 dtex or less, the wiping cloth has high wiping properties and leaves little residue, making it a wiping cloth suitable for media cleaning applications. In addition, a splittable composite fiber made of a polyamide resin and an alkali-soluble polyester resin and containing substantially no matting agent is used at least as a weft yarn to form a fabric, and then the alkali-soluble polyester resin is dissolved in an alkaline solution to remove oligomers and the like contained in the polyamide and the polyester that is not easily soluble in alkali, thereby reducing the number of particles generated by the wiping cloth itself. [Brief description of the drawings]

[0015] [Figure 1] FIG. 2 is an explanatory diagram showing an example of a cross-sectional shape of an ultrafine fiber according to the present invention. [Diagram 2] FIG. 4 is an explanatory diagram showing another example of the cross-sectional shape of the ultrafine fiber according to the present invention. [Diagram 3] FIG. 4 is an explanatory diagram showing another example of the cross-sectional shape of the ultrafine fiber according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The present invention will be described in detail below.

[0017] The wiping cloth of the present invention is a fiber structure using ultrafine polyamide fibers.

[0018] The ultrafine fibers constituting the wiping cloth must be polyamide fibers having a single-filament fineness of 0.7 dtex or less. The single-filament fineness is preferably 0.6 dtex or less. If the single-filament fineness is 0.7 dtex or less, the wiping cloth obtained will have better flexibility and density, and will be suitable for polishing and cleaning performance.

[0019] The content of polyamide ultrafine fibers in the entire wiping cloth of the present invention must be 40% by mass or more. If the content is 40% or more, generation of particles due to friction during wiping with a media is reduced.

[0020] The wiping cloth of the present invention preferably contains 30% or more polyester. By using polyester fibers or composite fibers containing polyester for the warp, the shape stability is improved and the tape width is easily maintained when used as a wiping tape.

[0021] The wiping cloth of the present invention has an average number of airborne particles with a diameter of 0.1 μm or more of 10 or less. 2 The media is less likely to be scratched if it is below this.

[0022] The wiping cloth of the present invention has excellent wiping performance when used in a clean room for precision equipment, such as in the manufacturing process of hard disks, etc. The wiping cloth may be in the form of a string, tape, square, or the like, and may be cut to a predetermined size and shape.

[0023] The ultrafine polyamide fibers in the present invention are preferably fibers formed by using splittable conjugate fibers comprising a polyamide component and an alkali-soluble polyester component and splitting the splittable conjugate fibers by alkali treatment.

[0024] Examples of the polyamide component include aliphatic polyamides such as polyamide 6, polyamide 6,6, and polyamide 4,6.

[0025] The polyamide component may be a polyamide resin composition containing an aromatic polyamide and an aliphatic polyamide. Examples of the aromatic polyamide include polyamides having an aliphatic dicarboxylic acid and an aromatic diamine as main structural units. The polyamide resin composition has a large shrinkage property and therefore shows good splittability when treated with alkaline solution or hot water. The fiber structure after the treatment has high density and bulkiness, and therefore has wiping properties suitable for polishing and cleaning hard disks, etc.

[0026] Specifically, the aromatic polyamide is a resin obtained from metaxylylenediamine and adipic acid (polyamide MXD6), and the aliphatic polyamide is a resin obtained from ε-caprolactam (polyamide 6). The mass mixing ratio of the polyamide MXD6 and polyamide 6 is preferably 35:65 to 70:30.

[0027] On the other hand, the above-mentioned alkali-soluble polyester component is a polyester component copolymerized with polyalkylene glycols, a metal sulfonate group-containing isophthalic acid component, or adipic acid.

[0028] Particularly preferred is a polyester in which the main repeating unit is ethylene terephthalate, the acid component contains 2.0 to 3.0 mol % of a metal sulfonate group-containing isophthalic acid component, and the polymer contains 9 to 13 mass % of a polyalkylene glycol having an average molecular weight of 1000 to 10000. Furthermore, a polyester component in which the mol % of DEG contained in the glycol component is 4.7 to 5.7 mol % and the ratio of the maximum value [η]max to the minimum value [η]min of the intrinsic viscosity is 1.0≦[η]max / [η]min≦1.02 is preferred.

[0029] The metal sulfonate group-containing isophthalic acid component used in the present invention is 5-dimethyl metal sulfoisophthalate (hereinafter referred to as SIPM) or a compound in which the methyl group is esterified with ethylene glycol (hereinafter referred to as SIPE). Since the physical properties of the slurry may deteriorate if a large amount of SIPM is added to the slurry tank, it is preferable to use SIPE. The metal in SIPM or SIPE is sodium, potassium, lithium, etc., but sodium is most preferable. The copolymerization rate of SIPE is preferably 2.0 to 3.0 mol% in the acid component of the polymer. If the copolymerization rate of SIPE is lower than this, it tends to be difficult to obtain sufficient alkali solubility. On the other hand, if the copolymerization rate is higher than this, thickening and gelation due to the charge of SIPE occur during the melt spinning process, and operability tends to decrease significantly.

[0030] Polyalkylene glycols have the general formula HO(C n H 2n O) mH (where n and m are positive integers), with polyethylene glycol (hereinafter referred to as PEG) where n=2 being versatile and most preferred. The molecular weight of the polyalkylene glycol used in the present invention is preferably 1000 to 10000. If the molecular weight is less than 1000, the hydrolysis reaction of the modified polyester is likely to occur during melt spinning, the heat resistance of the polyester is insufficient, and the polyester pellets tend to fuse together or produce white powder during the false twisting process. If the molecular weight exceeds 10000, the polymerization reactivity becomes poor, and the polyalkylene glycol is difficult to copolymerize in the molecular chain of the polyester, so the oxidation resistance of the polyester tends to be poor.

[0031] The copolymerization amount of polyalkylene glycol needs to be 9 to 13% by mass relative to the polymer. If the copolymerization amount is less than 9% by mass, the alkaline water dissolving performance tends to be insufficient. On the other hand, if it exceeds 13% by mass, the heat resistance and oxidation resistance of the polymer deteriorate.

[0032] The intrinsic viscosity of the polyester is such that the ratio of the maximum value [η]max to the minimum value [η]min of the intrinsic viscosity is 1.0≦[η]max / [η]min≦1.02. If [η]max / [η]min is outside the above range, there is a tendency for operability to be poor, such as frequent occurrence of yarn breakage during melt spinning and a shortened spinneret life due to poor spinning filterability.

[0033] In addition, the alkali-soluble polyester component used in the present invention preferably contains 4.7 to 5.7 mol % of diethylene glycol (DEG) in the glycol component. This DEG is generated by a side reaction during polymerization. If it is less than 4.7 mol %, the alkali water solubility is poor. If it exceeds 5.7 mol %, the heat resistance and oxidation resistance of the polymer are poor, and the operability during melt spinning is significantly deteriorated.

[0034] Moreover, the polyamide component and the alkali-soluble polyester component preferably do not contain a matting agent. A matting agent is an inorganic particle or an organic particle such as titanium dioxide, silicon oxide, or aluminum oxide that is usually added to suppress the gloss of the yarn or improve the spinning operability. Moreover, the meaning of not containing a matting agent here is that a matting agent such as titanium dioxide that is usually added to suppress the gloss of the yarn or improve the spinning operability is not actively added. This is because if a matting agent is contained, the matting agent will fall off due to a physical external force when wiping, causing scratches on a magnetic recording medium, etc. Trace amounts of ash may be present due to contamination during manufacturing and processing. Even in such cases, if the analytical value according to a general ash content measurement method is less than 50 ppm in the polymer, the surface will not be damaged when polishing or cleaning a hard disk.

[0035] In the splittable composite fiber having the above-mentioned components, when the polyester component is entirely dissolved and split by alkali dissolution processing, the polyamide component shrinks due to heating in the alkali dissolution processing step or a separate heat treatment, and a high-density and bulky wiping cloth can be obtained.

[0036] The cross-sectional shape of the splittable conjugate fiber is preferably such that the polyamide component and the alkali-soluble polyester component are bonded together along the longitudinal direction of the single fiber in such a manner that one component does not completely encompass the other component in the cross section of the single fiber.Specific examples include radial splittable conjugate fibers bonded together in a radial and complementary manner as shown in Figures 1 and 2, and a central circular splittable conjugate fiber as shown in Figure 3.

[0037] In the figure, 1 and 2 respectively represent a polyamide component or an alkali-soluble polyester component. That is, if one is a polyamide component, the other is an alkali-soluble polyester component. In the present invention, it is preferable to use a splittable conjugate fiber in which 1 is an alkali-soluble polyester component and 2 is a polyamide component, in order to further exhibit the abrasion resistance of the polyamide.

[0038] As described above, the ultrafine polyamide fibers in the present invention preferably have a modified fiber cross-sectional shape in terms of wiping performance during media cleaning.

[0039] The total fineness of the splittable conjugate fiber may be appropriately determined within the range that allows spinning. From the viewpoint of fiber shrinkage performance that affects the wiping performance of the wiping cloth, the total fineness is preferably 30 to 300 dtex, more preferably 40 to 200 dtex, and particularly preferably 50 to 150 dtex.

[0040] Examples of fiber structures using the splittable composite fiber include threads, woven fabrics, knitted fabrics, nonwoven fabrics, etc., among which woven fabrics are preferred. Even when used as a wiping tape, woven fabrics are less likely to stretch in the warp direction. If the tape stretches in the warp direction during use, it will be difficult to wind the tape correctly. In addition, narrowing the width of the tape will cause problems such as leaving parts of the wiping surface unwiped when it is brought into contact with the wiping surface.

[0041] When the fiber structure is a woven fabric, examples of the weave include plain weave, satin weave, twill weave, etc. As the wiping cloth, for example, plain weave, satin weave, and twill weave are preferable. Satin weave is preferable because it can be made into a denser fabric.

[0042] When the fiber structure is a woven fabric, the splittable composite fiber can be used for the weft or warp or both the warp and weft.

[0043] In this case, it is preferable to use regular polyester fiber (polyethylene terephthalate fiber) or polyamide fiber for the warp yarn.

[0044] In particular, when the wiping cloth of the present invention is used in the form of a tape, it is preferable that the weft is made of ultrafine polyamide fibers. The wiping performance is improved by using ultrafine polyamide fibers as the weft in the wiping direction (perpendicular to the direction of travel). Therefore, it is preferable to use the above-mentioned splittable composite fibers as the weft during weaving.

[0045] In this case, it is preferable to use regular polyester fibers (polyethylene terephthalate fibers) for the warp yarns.

[0046] When the fabric is made into a woven fabric, the suitable finished cover factor (K) calculated by the following formula is, in the case of plain weave, preferably 1000 or more in the warp direction and 800 or more in the weft direction, and in the case of satin weave, preferably 1200 or more in the warp direction, more preferably 1500 or more, 800 or more in the weft direction, and more preferably 1000 or more.

[0047]

number

[0048] When the fiber structure of the present invention is a knitted fabric, it may be either warp knitted or weft knitted. Specifically, a weft knitted structure is preferred, and when used as a wiping cloth, for example, an interlock structure is preferred. When the knitted fiber structure of the present invention is used as a wiping cloth to be used in a clean room, for example, it is preferred that the number of wales is 70 to 100 per inch and the number of courses is 70 to 100 per inch. In the case of a tricot, it is preferable to use about 28G. In addition, the above split type fiber may be used for all of the front yarn, back yarn, and middle yarn, or only a part of them may be split type fibers, but it is more preferable to use them for at least the front and back.

[0049] The wiping cloth of the present invention is preferably obtained by producing a fiber structure from the above-mentioned splittable conjugate fiber by an appropriate conventional method, subjecting the fiber structure to an alkali dissolution treatment to split the splittable conjugate fiber, and further subjecting the fiber structure to a heat treatment or the like as necessary.

[0050] By the alkaline dissolution treatment, oligomers contained in polyamide or polyester are removed by the alkaline aqueous solution, thereby reducing the number of self-generated particles in the wiping cloth.

[0051] The alkali dissolution treatment is a method for splitting the splittable conjugate fiber of the present invention by, for example, immersing it in a heated alkaline solution to dissolve the alkali-soluble polyester component and at the same time shrinking the polyamide component, thereby splitting the fiber. During this process, the self-generated dust particles and low molecular weight substances originating mainly from oligomers contained in the alkali-soluble polyester component are dissolved and removed by the alkaline solution, so that the number of self-generated dust particles in the product can be reduced.

[0052] The conditions for the alkali dissolution treatment may be those generally used in the weight reduction process of polyester fiber structures, such as a method using an aqueous sodium hydroxide solution of 0.5 to 5 mass %, more preferably 1 to 3 mass %, and particularly preferably 1 to 2 mass %. The treatment temperature is preferably 85 to 100°C, more preferably 90 to 98°C.

[0053] Furthermore, it is preferable to subject the fiber structure obtained by the above-mentioned alkali dissolution treatment to a heat treatment. Such a heat treatment can shrink the fibers, increase the density of the woven fabric, and increase the surface area of ​​the fabric to improve wiping properties. The heat treatment can be performed, for example, under moist heat conditions at 120 to 150°C for about 0.5 to 1 hour, or under dry heat conditions at 150°C to 190°C for about 30 seconds to 1 minute. The heat treatment may be performed simultaneously with the dyeing treatment. That is, the heat treatment for dyeing may shrink the fibers.

[0054] In the method for producing a wiping cloth of the present invention, it is preferable to obtain a final fiber structure by subjecting a green fabric obtained through processes such as weaving and knitting to the above-mentioned processes, thereby shrinking the woven fabric by 10 to 30% in the width direction and the knitted fabric by 40 to 60% in the width direction. Obtaining such a shrinkage rate is preferable in that excellent wiping properties can be obtained. The above shrinkage rate is expressed by assuming that the width of the green fabric is W0 and the width after shrinkage is W, 100×{(W0-W) / (W0)}(%) It can be calculated using the formula:

[0055] When the fabric is used for polishing or cleaning precision electronic devices such as hard disks used in a clean room, the fabric is washed with pure water in the clean room, dried, and cut to a desired size as needed. After that, the fabric is washed with pure water in the clean room and dried as needed to obtain a wiping cloth. The wiping cloth obtained is preferably sealed and packed in a resin film. When the wiping cloth is used in the manufacturing process of a hard disk or the like, the sealed package is opened and the wiping cloth can be used.

[0056] The wiping cloth of the present invention obtained as described above contains a large amount of ultrafine polyamide fibers, and the average number of airborne particles having a diameter of 0.1 μm or more is 10 particles / cm. 2 Since the above conditions are met, no contamination occurs and the wiping properties are excellent. EXAMPLES

[0057] The present invention will be specifically described below with reference to examples, but the present invention is not limited to the examples described below.

[0058] The evaluation methods are as follows.

[0059] <Intrinsic viscosity of polyester> The intrinsic viscosity [η] was measured in a mixed solvent of phenol / tetrachloroethane = 6 / 4 (mass ratio) at 20°C by a conventional method using an automatic viscometer.

[0060] <Relative viscosity of polyamide> The relative viscosity ηrel was measured in a sulfuric acid solvent at 20° C. by a conventional method using an Oswald viscometer.

[0061] <Measurement of the number of particles in the air> A 1 cm wide tape-like wiping cloth was cut to a length of 20 cm to be used as a sample. In a Class 100 clean room, the sample was placed on the measurement stage of a surface particle detector (QIII Ultra (registered trademark) manufactured by Pentagon Technologies) with both ends fixed with jigs, and the total number of particles of 0.1 μm or more and 5 μm or less on the sample surface was measured. Three different points on the same sample were measured, and the average value was taken as the number of airborne particles with a diameter of 0.1 μm or more. The unit of the total number of particles is particles / cm. 2 It is.

[0062] <Media wiping evaluation> The disk-shaped glass media was attached to a device that could rotate at 1000 to 3000 rpm, and the wiping cloth was 150 g / cm 2 The test was carried out at a rotation speed of 1000 rpm and 3000 rpm, where the media was pressed against the plate with a pressure of 1000 rpm and rotated for 1 minute. The number of bright spots, which are believed to be dust particles, transferred onto the media was counted using a Vision Cytec Micro-MAX. All of these operations were carried out in a Class 100 clean room.

[0063] Example 1 The polyamide component used was polyamide 6 (manufactured by Ube Industries, Ltd.) that contained substantially no matting agent (titanium oxide) and had a relative viscosity of 2.7. On the other hand, the alkali-soluble polyester component used was copolymerized polyethylene terephthalate (mainly composed of terephthalic acid and ethylene glycol, containing 2.3 mol % SIPE in the acid component, 10 mass % polyethylene glycol with an average molecular weight of 8000, and 5.5 mol % DEG) that contained substantially no matting agent and had an intrinsic viscosity of 0.77. The volume ratio of radially branched segment 1 to segment 2 replenishing the radial portions was 3:7, and melt conjugate spinning was performed at a spinning temperature of 295°C and a spinning speed of 1050 m / min, so that the alkali-soluble polyester component constituted radially branched segment 1 and the polyamide component constituted segment 2 replenishing the radial portions, to obtain an undrawn yarn having a fiber cross section similar to that in Figure 2. The obtained undrawn yarn was then drawn using a roller heater at 85°C, a plate heater at 150°C, and a draw ratio of 3.0 to obtain a splittable conjugate fiber of 84 dtex / 25 f. Then, a back satin fabric was obtained by using this drawn yarn as the weft and regular polyester fiber (intrinsic viscosity 0.61, 84 dtex / 36 f) spun using polyethylene terephthalate without a matting agent as the warp. The obtained fabric was immersed in a 2% by mass aqueous solution of sodium hydroxide (temperature 95°C) for 30 minutes to carry out an alkali dissolution treatment. After the alkali dissolution treatment, the fabric was washed with pure water, divided, and shrunk to obtain a wiping cloth. The polyamide fiber in the weft of the obtained wiping cloth was 60 dtex / 200 f, and the single yarn fineness was 0.29 dtex. The content of polyamide fiber in the entire obtained wiping cloth was 40% by mass. The obtained wiping cloth was heat-cut so that the weft direction was the width direction to give a 1 cm wide tape-shaped wiping cloth, which was then evaluated. The results are also shown in Table 1.

[0064] Example 2 A wiping cloth was obtained in the same manner as in Example 1, except that the volume ratio of the radially branched segment 1 to the segment 2 replenishing the radial portion was 3:7, the alkali-soluble polyester component constituted the radially branched segment 1, and the polyamide component constituted the segment 2 replenishing the radial portion, and a splittable conjugate fiber (84 dtex / 28 f) having the same fiber cross-sectional shape as in FIG. 1 was used as the weft. The polyamide fiber in the weft of the obtained wiping cloth was 60 dtex / 112 f, and the single yarn fineness was 0.53 dtex. The content of polyamide fiber in the entire obtained wiping cloth was 40 mass%. The obtained wiping cloth was heat-cut so that the weft direction was the width direction to give a 1 cm wide tape-shaped wiping cloth, which was then evaluated. The results are also shown in Table 1.

[0065] Example 3 Except for using regular polyester fibers (intrinsic viscosity 0.61, 33 dtex / 12 f) substantially free of a matting agent as the warp yarn, a wiping cloth was obtained in the same manner as in Example 1. The content of polyamide fibers in the entire wiping cloth obtained was 45% by mass. The obtained wiping cloth was heat-cut so that the weft direction was the width direction to give a 1 cm wide tape-shaped wiping cloth, which was then evaluated. The results are also shown in Table 1.

[0066] Example 4 A wiping cloth was obtained in the same manner as in Example 1, except that the warp yarn was a core-sheath type composite fiber (56 dtex / 24 f) in which the core was made of regular polyester (intrinsic viscosity 0.61) substantially free of a matting agent, and the sheath was made of polyamide 6 (manufactured by Ube Industries, Ltd.) having a relative viscosity of 2.7 and substantially free of a matting agent. The polyamide content in the entire wiping cloth obtained was 50% by mass. The obtained wiping cloth was heat-cut so that the weft direction was the width direction to give a 1 cm wide tape-shaped wiping cloth, which was then evaluated. The results are also shown in Table 1.

[0067] Comparative Example 1 A woven fabric was obtained in the same manner as in Example 1, except that the volume ratio of the radially branched segment 1 to the segment 2 replenishing the radial portion was 3:7, the radially branched segment 1 was constituted by polyamide 6 (manufactured by Ube Industries, Ltd.) having a relative viscosity of 2.7 and substantially free of a matting agent (titanium oxide), the segment 2 replenishing the radial portion was constituted by regular polyester having an intrinsic viscosity of 0.61 and substantially free of a matting agent, and a splittable composite fiber (56 dtex / 28 f) having the same fiber cross-sectional shape as in FIG. 1 was used as the weft. The obtained woven fabric was immersed in a 2% by mass aqueous sodium hydroxide solution (temperature 95°C) for 20 minutes to perform a splitting treatment. After the splitting treatment, the fabric was shrunk by washing with pure water to obtain a wiping cloth. The single yarn fineness of the polyamide fiber in the weft of the obtained wiping cloth was 0.60 dtex. The content of polyamide fiber in the entire obtained wiping cloth was 15% by mass. The obtained wiping cloth was heat-cut so that the weft direction was the width direction to give a 1 cm wide tape-shaped wiping cloth, which was then evaluated. The results are also shown in Table 1.

[0068] Comparative Example 2 A woven fabric was obtained in the same manner as in Example 1, except that the volume ratio of the radially branched segment 1 to the radially supplemented segment 2 was 3:7, the radially branched segment 1 was constituted by a regular polyester having an intrinsic viscosity of 0.61 and substantially free of a matting agent, the segment 2 supplementing the radial portion was constituted by a polyamide 6 (manufactured by Ube Industries, Ltd.) having a relative viscosity of 2.7 and substantially free of a matting agent, and a splittable composite fiber (56 dtex / 28 f) having the same fiber cross-sectional shape as in FIG. 1 was used as the weft. The resulting woven fabric was immersed in a 2% by mass aqueous sodium hydroxide solution (temperature 95°C) for 20 minutes to perform a splitting treatment. After the splitting treatment, the fabric was shrunk by washing with pure water to obtain a wiping cloth. The single yarn fineness of the polyamide fiber in the weft of the obtained wiping cloth was 0.35 dtex. The content of polyamide fiber in the entire obtained wiping cloth was 35% by mass. The obtained wiping cloth was heat-cut so that the weft direction was the width direction to give a 1 cm wide tape-shaped wiping cloth, which was then evaluated. The results are also shown in Table 1.

[0069] Comparative Example 3 The volume ratio of the radially branched segment 1 to the segment 2 replenishing the radial portion was 3:7, the radially branched segment 1 was constituted by polyamide 6 (manufactured by Ube Industries, Ltd.) having a relative viscosity of 2.7 and substantially no matting agent, the segment 2 replenishing the radial portion was constituted by regular polyester having an intrinsic viscosity of 0.61 containing 0.3 mass% of a matting agent, and a splittable composite fiber (56 dtex / 28 f) having the same fiber cross-sectional shape as in FIG. 1 was used as the weft yarn. A woven fabric was obtained in the same manner as in Example 1. The obtained woven fabric was immersed in a 2 mass% aqueous sodium hydroxide solution (temperature 95°C) for 20 minutes to perform a splitting treatment. After the splitting treatment, the fabric was washed with pure water to perform a shrinking treatment, and a wiping cloth was obtained. The single yarn fineness of the polyamide fiber in the weft yarn of the obtained wiping cloth was 0.60 dtex. The content of polyamide fiber in the entire obtained wiping cloth was 15 mass%. The obtained wiping cloth was heat-cut so that the weft direction was the width direction to give a 1 cm wide tape-shaped wiping cloth, which was then evaluated. The results are also shown in Table 1.

[0070] Comparative Example 4 The volume ratio of the radially branched segment 1 to the segment 2 replenishing the radial portion was 3:7, the radially branched segment 1 was constituted by polyamide 6 (manufactured by Ube Industries, Ltd.) having a relative viscosity of 2.7 that was substantially free of matting agent, the segment 2 replenishing the radial portion was constituted by regular polyester having an intrinsic viscosity of 0.61 that was substantially free of matting agent, a splittable composite fiber (56 dtex / 25 f) having a fiber cross-sectional shape similar to that of FIG. 2 was used as the weft, and a core-sheath composite fiber (56 dtex / 24 f) in which the core was a regular polyester component (intrinsic viscosity 0.61) that was substantially free of matting agent, and the sheath was polyamide 6 (manufactured by Ube Industries, Ltd.) having a relative viscosity of 2.7 that was substantially free of matting agent was used as the warp. A woven fabric was obtained in the same manner as in Example 1. The obtained woven fabric was immersed in a 2% by mass aqueous sodium hydroxide solution (temperature 95°C) for 20 minutes to perform a splitting treatment. After the splitting treatment, the fabric was washed with pure water to perform a shrinking treatment, and a wiping cloth was obtained. The polyamide fiber in the weft of the obtained wiping cloth had a single fiber fineness of 0.67 dtex, and the content of polyamide fiber in the entire obtained wiping cloth was 15% by mass. The obtained wiping cloth was heat-cut so that the weft direction was the width direction to give a 1 cm wide tape-shaped wiping cloth, which was then evaluated. The results are also shown in Table 1.

[0071] Comparative Example 5 A back satin fabric was obtained by using regular polyester fiber (33 dtex / 12 f) with an intrinsic viscosity of 0.61 that was substantially free of a matting agent as the warp yarn, and a single yarn (44 dtex / 36 f) of polyamide 6 (manufactured by Ube Industries, Ltd.) with a relative viscosity of 2.7 that was substantially free of a matting agent as the weft yarn. The fabric was shrunk by washing with pure water to obtain a wiping cloth. The single yarn fineness of the polyamide fiber in the weft yarn of the obtained wiping cloth was 1.22 dtex. The content of polyamide fiber in the entire obtained wiping cloth was 40% by mass. The obtained wiping cloth was heat-cut so that the weft direction was the width direction to give a 1 cm wide tape-shaped wiping cloth, which was then evaluated.

[0072] [Table 1]

[0073] The wiping cloths of Examples 1 to 4 had few airborne particles with a diameter of 0.1 μm or more, and also had few particles remaining after wiping, suppressing an increase in contamination during wiping. On the other hand, the wiping cloths of Comparative Examples 1 to 4 were wiping tapes mainly made of polyester, and as the rotation speed of the media increased, particles increased, and wiping was insufficient. [Explanation of symbols]

[0074] 1 Radial branching segments 2 Segments that fill the radial part

Claims

1. A wiping cloth made of a fiber structure using polyamide ultrafine fibers, the polyamide ultrafine fibers having a single yarn fineness of 0.7 dtex or less, a content of polyamide ultrafine fibers in the entire wiping cloth being 40 mass% or more, and an average number of airborne particles having a diameter of 0.1 μm or more being 10 particles / cm 2 Below is the wiping cloth.

2. The wiping cloth according to claim 1, wherein the polyamide ultrafine fibers are polyamide fibers obtained by dissolving the alkali-soluble polyester component of a splittable composite fiber that is substantially free of a matting agent and is made of a polyamide component and an alkali-soluble polyester component, and the fiber cross-sectional shape is an irregular cross-sectional shape.

3. 3. The wiping cloth according to claim 2, wherein the fiber structure is a woven fabric using the polyamide ultrafine fibers as at least a weft thread.

4. 4. A method for producing a wiping cloth according to claim 1, 2 or 3, comprising the steps of: weaving a fabric using, at least as a weft, a splittable conjugate fiber made of a polyamide component and an alkali-soluble polyester component, which is substantially free of a matting agent; and immersing the resulting fabric in an alkaline solution to dissolve the alkali-soluble polyester component.

Citation Information

Patent Citations

  • Fabric wiper

    JP2017147017A

Cited By

  • Wiping cloth, method for producing wiping cloth, wiping tape, method for producing wiping tape, and heat cutting device for wiping tape

    WO2026071267A1