Three-dimensional molding material, three-dimensional molding powder, molded body and production method thereof
A resin composition with ultra-high molecular weight polyethylene addresses the challenges of impact resistance and printability in 3D printing, enhancing the suitability of molded products for functional parts in various applications.
Patent Information
- Application Number
- JP2024022218
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-02-16
- Publication Date
- 2024-10-15
AI Technical Summary
Existing 3D printing technologies using the powder bed fusion method face challenges in achieving high impact resistance and printability, particularly for functional parts in practical applications, due to void formation and inferior mechanical properties in molded products, and existing solutions like ethylene-propylene copolymers and talc pose safety and procurement issues.
A resin composition containing ultra-high molecular weight polyethylene in a specific proportion with a thermoplastic resin, where the ultra-high molecular weight polyethylene is present in a range of 1 to 50 parts by mass, ensuring excellent interlayer adhesion and impact resistance in molded products.
The resin composition improves printability and impact resistance of molded products, making them suitable for practical applications such as components in home appliances, building materials, and aircraft, while maintaining safety during production.
Smart Images

Figure 2024146766000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a material for three-dimensional modeling, and more particularly to a material for three-dimensional modeling containing ultra-high molecular weight polyethylene. The present invention also relates to a powder for three-dimensional modeling made of the material for three-dimensional modeling, a molded body using the material for three-dimensional modeling, and a method for producing the same. [Background technology]
[0002] Today, three-dimensional printers (hereinafter sometimes referred to as "3D printers") that use various additive manufacturing methods (e.g., binder jetting, material extrusion, liquid vat photopolymerization, etc.) are available on the market. Among these, 3D printer systems using the Powder Bed Fusion method, such as the system manufactured by 3D Systems in the United States, print a thin layer of powder material such as resin (powder bed) using high-power CO 2 The resin powder is heated to a temperature near its melting point using a heating means such as a laser, and melted, and used to build a three-dimensional object in layers based on a computer-aided design (CAD) model. Here, the laser used as the heating means scans the cross section in the XY direction on the surface of the powder bed formed based on the 3D CAD data, and selectively melts the powder material. In this way, a three-dimensional molded body can be obtained by forming a laminate by repeating the formation of the powder bed and melting with the laser. This system does not require the use of a mold, and various resin powders can be used as raw materials as long as they have a certain degree of heat resistance, and the obtained molded body is highly reliable, so it is a technology that has attracted attention in recent years.
[0003] Due to the modeling principle, crystalline thermoplastic resins are used as the material type of resin powder used in 3D printers, and polyamide resins such as nylon 12 and nylon 11 are particularly widely used. In recent years, in addition to polyamide resins, polyester resins such as polybutylene terephthalate, polyolefin resins such as polypropylene, and elastomer resins such as thermoplastic polyurethane have also been used.
[0004] Traditionally, 3D printers have been widely used for product prototyping, but in recent years, their application to functional parts for practical use has also been considered. When considering practical use, for example, as components for home appliances, building materials, aircraft, and automotive materials, it is desirable for the molded products obtained by 3D printers using 3D modeling materials to have high mechanical properties. However, due to the molding principle, compacts produced by the Powder Bed Fusion method are prone to voids inside the compacts, and have poor mechanical properties. In particular, it is difficult to impart high impact resistance like the materials currently used in automotive components.
[0005] As an investigation into improving the mechanical properties of molded bodies by the Powder Bed Fusion method, for example, Patent Document 1 discloses a method for obtaining powder with excellent tensile elongation at break by specifying the ethylene molar ratio and melt flow rate of a polypropylene resin within a specific range. Furthermore, Patent Document 2 discloses a method for obtaining a powder having excellent strength in the layering direction of a molded body by melt-kneading talc as a filler into a polypropylene resin and specifying the mass ratio of silicon oxide to the total mass of the obtained resin powder within a specific range. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2020 / 213586 [Patent Document 2] JP 2020-93515 A Summary of the Invention [Problem to be solved by the invention]
[0007] In order for 3D printers to be widely used for functional parts that are also used for practical purposes, it is desirable to be able to use existing resin powders to improve the shaping properties using 3D printers and the impact resistance of the resulting molded bodies, while also ensuring safety during material production.
[0008] However, in the above-mentioned Patent Document 1, it is necessary to polymerize an ethylene-propylene copolymer having a specific composition, which is not preferable from the viewpoint of the production and procurement of raw materials. Patent Document 2 contains talc which falls under the GHS classification, so there are concerns about safety during grinding. Moreover, in none of the examples has it been possible to confirm any improvement in the impact resistance of the resulting molded article.
[0009] The present invention solves the above-mentioned problems, and has an objective of providing a material for 3D modeling that contains a resin composition, which uses existing resin powders, maintains safety during powder production, and has excellent modeling properties in 3D printers and excellent impact resistance of the resulting molded bodies. [Means for solving the problem]
[0010] As a result of intensive research conducted by the present inventors to solve the above problems, they discovered that these problems could be solved by using a resin composition containing a specific proportion of ultra-high molecular weight polyethylene, and thus developed the present invention.
[0011] That is, the gist of the present invention is as follows.
[0012] [1] A three-dimensional modeling material containing a resin composition, the resin composition comprising: a thermoplastic resin (A) having a viscosity average molecular weight (Mv) of less than 500,000; and an ultra-high molecular weight polyethylene (B) having a viscosity average molecular weight (Mv) of 500,000 or more and 10 million or less, the content of the ultra-high molecular weight polyethylene (B) being 1 part by mass or more and less than 50 parts by mass per 100 parts by mass of the combined weight of the thermoplastic resin (A) and the ultra-high molecular weight polyethylene (B).
[0013] [2] The material for three-dimensional modeling according to [1], wherein the ultra-high molecular weight polyethylene (B) is in powder form.
[0014] [3] The material for three-dimensional modeling according to [1] or [2], wherein the powder of the ultra-high molecular weight polyethylene (B) has an average particle size (D50) measured by a laser diffraction method of 10 μm or more and 200 μm or less.
[0015] [4] The three-dimensional modeling material according to any one of [1] to [3], wherein the three-dimensional modeling material, the thermoplastic resin (A) and the ultra-high molecular weight polyethylene (B) are in powder form, and the average particle size (D50) of the powder of the three-dimensional modeling material and the thermoplastic resin (A) as determined by a laser diffraction method is larger than the average particle size (D50) of the powder of the ultra-high molecular weight polyethylene (B).
[0016] [5] The material for three-dimensional modeling according to any one of [1] to [4], wherein the difference in melting point (Tm) between the thermoplastic resin (A) and the ultra-high molecular weight polyethylene (B) is 70°C or less, as measured at a heating rate of 10°C / min in differential scanning calorimetry according to JIS K7121.
[0017] [6] The material for three-dimensional modeling according to any one of [1] to [5], wherein the thermoplastic resin (A) is a polyolefin resin.
[0018] [7] The material for three-dimensional modeling according to [6], wherein the polyolefin-based resin is a propylene-based polymer.
[0019] [8] A powder for three-dimensional modeling obtained by using the material for three-dimensional modeling according to any one of [1] to [7].
[0020] [9] The powder for three-dimensional modeling according to [8], having an average particle size (D50) measured by a laser diffraction method of 5 μm or more and 250 μm or less.
[0021]
[10] A molded product obtained by using the material for three-dimensional modeling according to any one of [1] to [7].
[0022]
[11] A method for producing a molded body, comprising a step of three-dimensionally molding a molded body by a Powder Bed Fusion method using a material for three-dimensional molding according to any one of [1] to [7].
[0023]
[12] A molded product obtained by using the powder for three-dimensional modeling described in [8] or [9].
[0024]
[13] A method for producing a molded body, comprising a step of three-dimensionally molding a molded body by a Powder Bed Fusion method using the powder for three-dimensional molding according to [8] or [9]. Effect of the Invention
[0025] According to the present invention, it is possible to provide a material for three-dimensional modeling that contains a resin composition, which can be used with existing resin powders and has excellent modeling properties in a 3D printer and excellent impact resistance of the resulting molded body while maintaining safety during powder production. Furthermore, according to the present invention, a powder for three-dimensional modeling for a Powder Bed Fusion method, a molded body, and a manufacturing method thereof are provided using this material for three-dimensional modeling. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] Hereinafter, an embodiment for carrying out the present invention (hereinafter referred to as "the present embodiment") will be described in detail. The present embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content. The present invention can be carried out in various modifications within the scope of its gist.
[0027] [3D modeling materials] The three-dimensional modeling material of the present invention is a three-dimensional modeling material containing a resin composition, the resin composition comprising a thermoplastic resin (A) having a viscosity average molecular weight (Mv) of less than 500,000, and an ultra-high molecular weight polyethylene (B) having a viscosity average molecular weight (Mv) of 500,000 or more and 10 million or less, and the content of the ultra-high molecular weight polyethylene (B) is 1 part by mass or more and less than 50 parts by mass per 100 parts by mass of the total of the thermoplastic resin (A) and the ultra-high molecular weight polyethylene (B).
[0028] [mechanism] Although the details of the mechanism by which the present invention exhibits the above-mentioned effects are not clear, it is presumed as follows. In other words, in the 3D modeling material of the present invention, the ultra-high molecular weight polyethylene (B) contained in the resin composition contained in the 3D modeling material is a polymer that melts but does not flow at the temperature of 3D modeling, and therefore, in the 3D printing process, it exhibits excellent interlayer adhesion to the thermoplastic resin (A), which is the main component resin powder, when melted, and because it does not flow itself, the particles maintain the same shape. Therefore, it is possible to impart the impact resistance characteristic of the ultra-high molecular weight polyethylene (B) to the molded body obtained by the 3D printer, and it is presumed that a molded body with excellent impact resistance can be produced.
[0029] [Definition of physical properties] The various physical properties in the present invention are values measured as follows.
[0030] <Viscosity average molecular weight (Mv)> The viscosity average molecular weight (Mv) of the thermoplastic resin (A) and the ultra-high molecular weight polyethylene (B) is a value calculated in accordance with the method shown in JIS K-7367 for the thermoplastic resin (A) or the method shown in ASTM D4020 for the ultra-high molecular weight polyethylene (B), using the specific viscosity ηsp (dl / g) of a 0.05% decalin solution at 135°C instead of the intrinsic viscosity [η] (dl / g).
[0031] <Average particle size (D50)> The average particle size (D50) of the powders of the thermoplastic resin (A), ultra-high molecular weight polyethylene (B), and material for 3D modeling is determined by measuring the particle size distribution of the powder on a volume basis using a particle size distribution measuring device that uses the laser diffraction method, and finding the particle size at 50% of the frequency distribution of the powder among the detected particle size distributions.
[0032] <Melting point (Tm)> The melting points (Tm) of the thermoplastic resin (A) and the ultra-high molecular weight polyethylene (B) are the crystalline melting temperatures (melting points Tm) (°C) (re-heating process) determined from thermograms measured using a differential scanning calorimeter in accordance with JIS K7121, in which the temperature is increased from room temperature to 200°C at a heating rate of 10°C / min, the temperature is maintained at that temperature for 1 minute, the temperature is decreased to 50°C at a heating rate of 10°C / min, and the temperature is increased again to 200°C at a heating rate of 10°C / min.
[0033] [Resin composition] The resin composition used in the 3D modeling material of the present invention (hereinafter sometimes referred to as "the resin composition of the present invention" or "this resin composition") contains a thermoplastic resin (A) and ultra-high molecular weight polyethylene (B). Since the ultra-high molecular weight polyethylene (B) is a thermoplastic resin with excellent impact resistance, this resin composition, unlike general thermoplastic molding methods such as extrusion molding and injection molding, is able to maintain good interlayer adhesion and impart impact resistance to the resulting molded body in 3D modeling, in which heat and light are applied directly to the material and a molded body is produced by layering it one layer at a time based on 3D-CAD or 3D-CG data.
[0034] The present resin composition may contain other resins, additives, reinforcing materials, etc., in addition to the thermoplastic resin (A) and the ultra-high molecular weight polyethylene (B), as long as the effects of the present invention are not impaired.
[0035] [Thermoplastic resin (A)] The thermoplastic resin (A) used in the present invention may be any material that exhibits thermoplasticity due to the heat or light of the 3D printer device, and may be appropriately selected depending on the function to be imparted to the molded article to be formed.
[0036] As the thermoplastic resin (A), a commercially available thermoplastic resin material for three-dimensional modeling may be used. In addition, when using a material for three-dimensional modeling for the Powder Bed Fusion method, the material for three-dimensional modeling remaining after the modeling object is produced by the Powder Bed Fusion method may be reused. The resin composition of the present invention contains ultra-high molecular weight polyethylene (B), and thus can form a molded article having excellent impact resistance with excellent moldability by using an existing resin powder for powder bed fusion as the thermoplastic resin (A). However, the thermoplastic resin (A) used in the present invention is not limited to the existing resin powder for powder bed fusion.
[0037] Examples of the thermoplastic resin (A) include polyacetal, polyacrylate, polyacrylic acid, polyamide, polyamideimide, polyacid anhydride, polyarylate, polyarylene ether, polyarylene sulfide, polybenzoxazole, polyester, polyetheretherketone, polyetherimide, polyetherketoneketone, polyetherketone, polyethersulfone, polyimide, polymethacrylate, polyolefin, polyphthalide, polysilazane, polysiloxane, polystyrene, polysulfide, polysulfonamide, polysulfonate, polythioester, polytriazine, polyurea, polyurethane, polyvinyl alcohol, polyvinyl ester, polyvinyl ether, polyvinyl halide, polyvinyl ketone, polyvinyl fluoride, polyvinyl aromatic, polysulfone, polyarylene sulfone, polyaryl ether ... Examples of the thermoplastic elastomer include terketone, polylactic acid, polyglycolic acid, poly-3-hydroxybutyrate, polyhydroxyalkanoate, starch, cellulose ester, poly(phenylene ether), poly(methyl methacrylate), styrene-acrylonitrile copolymer resin, poly(ethylene oxide), epichlorohydrin polymer, polycarbonate homopolymer, polycarbonate copolymer, poly(ester carbonate), poly(ester-siloxane-carbonate), poly(carbonate-siloxane), vinyl polymer, acrylonitrile-butadiene-styrene copolymer resin (ABS resin), methyl methacrylate-butadiene-styrene copolymer resin (MBS resin), polyvinyl chloride, olefin-based thermoplastic elastomer, styrene-based thermoplastic elastomer, polyurethane-based thermoplastic elastomer, and polyester-based thermoplastic elastomer. These resins may be used in combination of two or more kinds, if desired.
[0038] The thermoplastic resin (A) used in the present invention has a viscosity average molecular weight (Mv) of less than 500,000. If the viscosity average molecular weight (Mv) of the thermoplastic resin (A) is 500,000 or more, the melt viscosity of the thermoplastic resin (A) becomes large, which may impair the spreadability and moldability of the molding material during powder bed fusion molding, and is therefore undesirable. The lower limit of the viscosity average molecular weight (Mv) of the thermoplastic resin (A) is not particularly limited, but is preferably 10,000 or more. If the viscosity average molecular weight of the thermoplastic resin (A) is less than 10,000, the mechanical strength of the molded body obtained by the powder bed fusion method may be insufficient, and it may not be possible to obtain one having sufficient mechanical strength. From these viewpoints, the viscosity average molecular weight (Mv) of the thermoplastic resin (A) is preferably 450,000 or less, more preferably 50,000 or more, and even more preferably 100,000 or more.
[0039] The thermoplastic resin (A) used in the present invention can be selected according to the thermal properties such as the melting point and crystallization temperature of the ultra-high molecular weight polyethylene (B) from the viewpoint of shapeability for obtaining a molded body having excellent impact resistance from the ultra-high molecular weight polyethylene (B) using a 3D printer, and it is preferable that the thermoplastic resin (A) is a resin whose melting point (Tm) measured by differential scanning calorimetry (DSC) is close to the melting point (Tm) of the ultra-high molecular weight polyethylene (B). Specifically, the difference between the melting point (Tm) of the thermoplastic resin (A) and the melting point (Tm) of the ultra-high molecular weight polyethylene (B) is preferably 70° C. or less, more preferably 40° C. or less, and even more preferably 20° C. or less. In this way, since the melting points (Tm) of the thermoplastic resin (A) and the ultra-high molecular weight polyethylene (B) are close to each other, both resins melt during Powder Bed Fusion modeling, and the resins can be sufficiently bonded to each other, which is preferable because it increases the interlayer adhesion in the modeled object.
[0040] Examples of such thermoplastic resins (A) include vinyl polymers, fluorine-based resins, polyolefins, polyesters, polyamides, polyarylene ethers, polyarylene sulfides, polyether ketones, polyether ether ketones, polyacetals, thermoplastic polyurethanes, polyvinyl chloride, olefin-based, styrene-based, and polyester-based thermoplastic elastomers, and copolymers thereof. In particular, as the thermoplastic resin (A) having a melting point (Tm) close to the melting point (Tm) of the ultra-high molecular weight polyethylene (B), polyolefin-based resins, thermoplastic polyurethanes, and thermoplastic elastomers are more preferable, and from the viewpoint of interlayer adhesion, polyolefin-based resins are particularly preferable.
[0041] Also, the thermoplastic resin (A) is preferably in powder form since, when used in a Powder Bed Fusion process, the molding material is in powder form. The average particle size (D50) of the powdered thermoplastic resin (A) is preferably larger than the average particle size (D50) of the ultra-high molecular weight polyethylene (B) described below. Specifically, the average particle size (D50) of the thermoplastic resin (A) is preferably 50 μm or more and 250 μm or less, more preferably 55 μm or more and 200 μm or less, and even more preferably 60 μm or more and 150 μm or less. The average particle size (D50) of the thermoplastic resin (A) is preferably 1.2 to 30 times, particularly preferably 2 to 20 times, the average particle size (D50) of the ultra-high molecular weight polyethylene (B) described below. When the average particle size (D50) of the thermoplastic resin (A) is equal to or greater than the above lower limit, the bulk density of the thermoplastic resin (A) is maintained, and a decrease in density of the molded object can be suppressed during Powder Bed Fusion modeling. When the average particle size (D50) is equal to or less than the above upper limit, the entire thermoplastic resin (A) can be sufficiently melted during Powder Bed Fusion modeling, and the dimensional accuracy of the molded object can be improved.
[0042] Each of the thermoplastic resins (A) used in the present invention will be described below.
[0043] <Polyolefin resin> The polyolefin resin used in the present invention is a polymer obtained by polymerization of a monomer having a polyolefin skeleton. Polyolefin is a hydrocarbon resin having a carbon-carbon double bond.
[0044] The polyolefin resin is not particularly limited, and olefin homopolymers, block copolymers, random copolymers, etc. can be suitably used, including polypropylene; propylene copolymers obtained by copolymerizing propylene with α-olefins such as ethylene, 1-butene, 1-hexene, and 4-methyl-1-pentene; polyethylenes such as low-density polyethylene, linear low-density polyethylene, medium-density polyethylene, and high-density polyethylene; ethylene copolymers obtained by copolymerizing ethylene with α-olefins such as 1-butene, 1-hexene, and 4-methyl-1-pentene; poly(1-butene), poly(4-methyl-1-pentene), etc. These may be used alone or in combination of two or more different copolymerization component compositions and physical properties.
[0045] Among them, from the viewpoint of obtaining a molded body having excellent heat resistance, a propylene-based polymer is particularly preferable as a polyolefin-based resin. Furthermore, from the viewpoint of moldability, a propylene-based copolymer obtained by copolymerizing propylene with an α-olefin such as ethylene, 1-butene, 1-hexene, or 4-methyl-1-pentene is more preferable so that deformation such as crystallization shrinkage during cooling and warping of the molded body during molding can be suppressed. Here, the propylene-based copolymer is a polypropylene-based resin containing 50% by mass or more of propylene units in all monomer units.
[0046] Examples of the propylene copolymer include products manufactured by Japan Polypropylene Corporation under the trade names "Novatec (registered trademark) PP," "Wintech (registered trademark)," "Newcon (registered trademark)," and "Wellnex (registered trademark)," products manufactured by ExxonMobil Corporation under the trade name "Vistamax (registered trademark)," and products manufactured by The Dow Chemical Company under the trade name "Versify (registered trademark)." These products may be appropriately selected from the group of products and used alone or in combination of two or more types.
[0047] <Thermoplastic polyurethane> The thermoplastic polyurethane used in the present invention is not particularly limited as long as it is a condensation polymer of a polyol and a polyisocyanate.
[0048] The polyol is not particularly limited, and conventionally known polyols can be used. Examples of the polyol include polymer polyols such as polyester polyols, polyether polyols, polycarbonate polyols, and polylactone polyols. These polyols may be used alone or in combination of two or more.
[0049] The polyester polyol is not particularly limited as long as it is a condensation product of a polyvalent carboxylic acid or a reactive derivative thereof with a polyhydric alcohol, and may be, for example, one obtained by condensation polymerization of a dicarboxylic acid with a glycol.
[0050] Examples of dicarboxylic acids include aliphatic dicarboxylic acids such as succinic acid, glutaric acid, adipic acid, azelaic acid, sebacic acid, dodecanedicarboxylic acid, fumaric acid, and maleic acid; aromatic dicarboxylic acids such as orthophthalic acid, terephthalic acid, isophthalic acid, and 2,6-naphthalenedicarboxylic acid; alicyclic dicarboxylic acids such as 1,3-cyclopentanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and 1,4-cyclohexanedicarboxylic acid; and reactive derivatives thereof. These dicarboxylic acids may be used alone or in combination of two or more. Among them, adipic acid is preferred.
[0051] Examples of glycols include dimethylene glycol, ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, 1,3-propanediol, neopentyl glycol, 2,2-diethyl-1,3-propanediol, butylethylpropanediol, 1,2-butanediol, butylene glycol, 1,4-butanediol, dimethylbutanediol, 1,5-pentanediol, 2,4-diethylpentanediol, and 1,6-hexanediol. Examples of the glycols include aliphatic glycols such as 1,3-cyclopentanediol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, 2,2-bis(4-hydroxycyclohexyl)propane, and aromatic glycols such as m-xylylene glycol, p-xylylene glycol, bisphenol A, bisphenol F, and bisphenol S. These glycols may be used alone or in combination of two or more. Among them, aliphatic glycols are preferred, and polyethylene butylene glycol is more preferred.
[0052] Examples of polyester polyols include condensation polyester polyols such as polyethylene adipate glycol, polybutylene adipate glycol, polyhexamethylene adipate glycol, and polyethylene butylene adipate glycol.
[0053] Examples of polyether polyols include aliphatic polyether polyols such as polytetramethylene glycol, polyethylene glycol, and polypropylene glycol.
[0054] Examples of polycarbonate-based polyols include polyols obtained by dealcoholization reaction between low molecular weight polyols such as ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, octanediol, nonanediol, and 1,4-cyclohexanedimethanol and carbonate compounds such as diethylene carbonate, dipropylene carbonate, and diphenyl carbonate.
[0055] Examples of the polylactone polyol include polylactone diols obtained by ring-opening polymerization of lactone using the above-mentioned low molecular weight polyols as an initiator, lactone polyester diols such as polycaprolactone diol and polymethylvalerolactone diol.
[0056] The polyol used in the thermoplastic polyurethane of the present invention preferably contains one or more selected from the group consisting of polycarbonate, polycaprolactone and polyester polyols from the viewpoint of further improving the hardness of the molded body by a 3D printer. Also, from the viewpoint of low-temperature properties during powder production, polyether or polyester polyols are preferred, and polyester polyols are generally preferred.
[0057] The polyisocyanate is not particularly limited as long as it has two or more isocyanate groups, and conventionally known polyisocyanates can be used. Examples of diisocyanates having two isocyanate groups include aliphatic isocyanates such as 1,6-hexamethylene diisocyanate (HDI), 2,2,4-trimethylhexamethylene diisocyanate, methylene diisocyanate, isopropylene diisocyanate, lysine diisocyanate, lysine diisocyanate methyl ester, and 1,5-octylene diisocyanate; 4,4'-dicyclohexylmethane diisocyanate, isophorone diisocyanate (IPDI), norbornene diisocyanate, hydrogenated tolylene diisocyanate, methylcyclohexane diisocyanate, and isopropylidene diisocyanate. alicyclic isocyanates such as tetramethylphenyl ether diisocyanate, tetramethylphenyl ether diisocyanate, diphenyl ether diisocyanate, diphenyl ether diisocyanate, diphenyl ether diisocyanate, diphenyl ether diisocyanate, diphenyl ether diisocyanate, diphenyl ether diisocyanate, diphenyl ether diisocyanate, dianisidine ... Examples of polyisocyanates having three or more isocyanate groups include triphenylmethane triisocyanate, triisocyanate phenyl thiophosphate, polymethylene polyphenylene polyisocyanate (polymeric MDI), isocyanurate modified products which are trimers of HDI or TDI, and biuret modified products.
[0058] These polyisocyanates may be used alone or in combination of two or more kinds. Among them, the polyisocyanate is preferably a diisocyanate having two isocyanate groups, more preferably an aromatic diisocyanate, and even more preferably 4,4'-diphenylmethane diisocyanate (MDI). In addition, when a function such as discoloration resistance is to be imparted, 1,6-hexamethylene diisocyanate (HDI), 4,4'-dicyclohexylmethane diisocyanate, etc. can also be used.
[0059] The chain extender used in the production of thermoplastic polyurethane is not particularly limited, and any conventionally known one can be used. As the chain extender, for example, any conventionally known polyhydric alcohols or amines can be used, but a low molecular weight polyol having 2 to 10 carbon atoms is preferred.
[0060] Examples of low molecular weight polyols include aliphatic polyols such as ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, 1,3-butanediol, 1,4-butanediol, 2-methylpentanediol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, octanediol, nonanediol, decanediol, trimethylpropane, and glycerin; alicyclic polyols such as cyclohexanediol and cyclohexanedimethanol; and aromatic polyols such as bishydroxyethoxybenzene and xylene glycol. These chain extenders may be used alone or in combination of two or more. Among them, aliphatic polyols are preferred as the chain extender, and 1,4-butanediol is more preferred.
[0061] The hardness (Shore A) of the thermoplastic polyurethane in the present invention is not particularly limited, but is preferably 80A or more and 98A or less, more preferably 85A or more, and even more preferably 87A or more, from the viewpoint of general-purpose availability. By making the hardness 80A or more, blocking during raw material supply is unlikely to occur, and productivity is improved. In addition, by making the hardness 98A or less, flexibility and impact resistance are improved. The hardness of the thermoplastic polyurethane can be measured by a method based on JIS K7311-1995 (Shore A).
[0062] Examples of the thermoplastic polyurethane include "Elastollan (registered trademark)" manufactured by BASF, "Miractran (registered trademark)" manufactured by Nippon Miractoran Co., Ltd., and "Pellethane (registered trademark)" manufactured by Lubrizol Co., Ltd., and one type may be selected from these product groups and used alone or in combination of two or more types.
[0063] <Thermoplastic elastomer> The thermoplastic elastomer used in the present invention is not particularly limited as long as it has impact resistance and flexibility. Among them, it is preferable to use one or more selected from styrene-based thermoplastic elastomers (SBC), polyolefin-based thermoplastic elastomers (TPO), urethane-based thermoplastic elastomers (TPU), polyester-based thermoplastic elastomers (TPEE), polyamide-based elastomers (TPA), silicone-based thermoplastic elastomers, and fluorine-based thermoplastic elastomers. In particular, from the viewpoint of moldability, polyester-based thermoplastic elastomers and polyolefin-based thermoplastic elastomers are more preferable. These may be used alone or in combination of two or more types having different copolymer component compositions, physical properties, etc.
[0064] The polyester thermoplastic elastomer is preferably a saturated polyester thermoplastic elastomer, and particularly preferably a saturated polyester thermoplastic elastomer containing a polyalkylene ether glycol segment. For example, a preferred example is one having an aromatic polyester as the hard segment and a polyalkylene ether glycol or aliphatic polyester as the soft segment. In particular, a polyester polyether block copolymer using a polyalkylene ether glycol as the soft segment is preferred.
[0065] The content of the polyalkylene ether glycol segment in the polyester polyether block copolymer is preferably 30% by mass, more preferably 40% by mass, and even more preferably 50% by mass, and preferably 90% by mass, more preferably 85% by mass, and even more preferably 80% by mass, based on the block copolymer produced. The content of the polyalkylene ether glycol segment is preferably below the upper limit in terms of hardness and mechanical strength, and above the lower limit in terms of flexibility and impact resistance. The content of the polyalkylene ether glycol segment can be calculated based on the chemical shift of the hydrogen atom and its content using nuclear magnetic resonance spectroscopy (NMR).
[0066] The polyester polyether block copolymer is preferably one obtained by polycondensing an oligomer obtained by an esterification reaction or an ester exchange reaction using (i) an aliphatic diol and / or an alicyclic diol having 2 to 12 carbon atoms, (ii) an aromatic dicarboxylic acid and / or an alicyclic dicarboxylic acid or an alkyl ester thereof, and (iii) a polyalkylene ether glycol as raw materials.
[0067] The aliphatic and / or alicyclic diol having 2 to 12 carbon atoms may be any of those generally used as raw materials for polyesters, particularly raw materials for polyester-based thermoplastic elastomers. Specific examples include ethylene glycol, propylene glycol, trimethylene glycol, 1,4-butanediol, 1,4-cyclohexanediol, and 1,4-cyclohexanedimethanol. Among these, 1,4-butanediol or ethylene glycol is preferred, and 1,4-butanediol is particularly preferred. Two or more of these diols may be used in combination.
[0068] As the aromatic dicarboxylic acid, those generally used as raw materials for polyesters, particularly raw materials for polyester-based thermoplastic elastomers, can be used. Specific examples thereof include terephthalic acid, isophthalic acid, phthalic acid, and 2,6-naphthalenedicarboxylic acid. Among these, terephthalic acid or 2,6-naphthalenedicarboxylic acid is preferred, and terephthalic acid is particularly preferred. These aromatic dicarboxylic acids may be used in combination of two or more. As the alkyl ester of the aromatic dicarboxylic acid, dimethyl ester, diethyl ester, etc. of the aromatic dicarboxylic acid are used. Among these, dimethyl terephthalate and 2,6-dimethylnaphthalenedicarboxylate are preferred.
[0069] The alicyclic dicarboxylic acid is preferably cyclohexanedicarboxylic acid, and the alkyl ester thereof is preferably a dimethyl ester, a diethyl ester, or the like.
[0070] In addition to the above components, a small amount of a trifunctional alcohol, tricarboxylic acid or its ester may be copolymerized, and further, an aliphatic dicarboxylic acid such as adipic acid or its dialkyl ester can also be used as a copolymerization component.
[0071] Specific examples of the polyalkylene ether glycol include polyethylene glycol, poly(1,2-propylene ether) glycol, poly(1,3-propylene ether) glycol, poly(tetramethylene ether) glycol, and poly(hexamethylene ether) glycol.
[0072] Examples of polyester-based thermoplastic elastomers include polyether-ester-based elastomers that combine polybutylene terephthalate and polytetramethylene ether glycol, polyester-ester-based elastomers that combine polybutylene terephthalate and polycaprolactone, etc. These can be used alone or in combination of two or more types.
[0073] Examples of the polyester-based thermoplastic elastomer include "TEFABLOCK (registered trademark)" manufactured by Mitsubishi Chemical Corporation and "PELPRENE (registered trademark)" manufactured by Toyobo Co., Ltd., and the like. One type may be selected from these product groups and used alone or in combination of two or more types.
[0074] Polyolefin-based thermoplastic elastomers include polypropylene-based ones and polyethylene-based ones. For example, there are types (reactor type) in which uncrosslinked or partially crosslinked ethylene-propylene rubber or ethylene-propylene-diene rubber is dispersed as a soft segment in a homogeneous or random polypropylene hard segment during polymerization of the hard segment, types in which a homogeneous or random polypropylene hard segment and an uncrosslinked or partially crosslinked ethylene-propylene rubber or ethylene-propylene-diene rubber soft segment are dynamically crosslinked during kneading, propylene-butene copolymers, propylene-ethylene-butene copolymers, propylene-butadiene copolymers, propylene-ethylene-butadiene copolymers, syndiotactic polypropylene, α-olefin copolymers, etc.
[0075] Examples of the olefin-based elastomer include Prime TPO (registered trademark) manufactured by Prime Polymer Co., Ltd., Thermorun (registered trademark) and ZELAS (registered trademark) manufactured by Mitsubishi Chemical Corporation, and Wellnex (registered trademark) manufactured by Japan Polypropylene Corporation. Products may be appropriately selected from this product group and used alone or in combination of two or more types.
[0076] [Ultra-high molecular weight polyethylene (B)] The ultra-high molecular weight polyethylene (B) used in the present invention is an ultra-high molecular weight polyethylene having a viscosity average molecular weight (Mv) of 500,000 or more and 10 million or less. Ultra-high molecular weight polyethylene having a viscosity average molecular weight (Mv) of 500,000 or more is a polyethylene resin having an extremely large molecular weight and a linear molecular structure with almost no branched chains, and is known to have an excellent effect of imparting impact resistance.
[0077] If the viscosity average molecular weight (Mv) of the ultra-high molecular weight polyethylene (B) is less than 500,000, the effect of the present invention, that is, the effect of imparting impact resistance to a molded body obtained by a 3D printer, cannot be achieved. From the viewpoint of imparting impact resistance, the viscosity average molecular weight (Mv) of the ultra-high molecular weight polyethylene (B) used in the present invention is preferably 1 million or more, more preferably 2 million or more. On the other hand, if the viscosity average molecular weight (Mv) of the ultra-high molecular weight polyethylene (B) is excessively large, the fluidity of the ultra-high molecular weight polyethylene (B) is poor, and there is a risk of impairing the spreadability and modeling properties of the modeling material during powder bed fusion modeling, so the viscosity average molecular weight (Mv) of the ultra-high molecular weight polyethylene (B) is 10 million or less, preferably 6 million or less, and more preferably 3 million or less.
[0078] Such ultra-high molecular weight polyethylene (B) is produced or provided not in the form of pellets but in the form of powder, that is, in the form of particles (powder). The average particle size (D50) of the ultra-high molecular weight polyethylene (B) powder is preferably 10 μm or more and 200 μm or less, more preferably 15 μm or more and 150 μm or less, and even more preferably 20 μm or more and 100 μm or less. When the average particle size (D50) of the ultra-high molecular weight polyethylene (B) is 200 μm or less, it is smaller than the molding material of the powder bed fusion method, which usually has an average particle size of about 50 μm or more and 250 μm or less, and the uneven distribution of coarse particles is reduced, and the dispersion in the resin composition of the present invention tends to be good, and when it is 10 μm or more, scattering and aggregation tend not to occur when handling as a material for three-dimensional modeling or during modeling, which is preferable. The average particle size (D50) of the ultra-high molecular weight polyethylene (B) in the present invention may be that of the particles before being made into a resin composition, or may be the average particle size of the particles dispersed in the resin composition by melt-kneading or the like. As described above, the average particle size of the particles before being made into a resin composition is the particle size (D50) at 50% of the frequency distribution of the powder in the particle size distribution detected by the laser diffraction method. Alternatively, the average particle size may be measured by an electrical resistance method. When the particles are dispersed in a resin composition, the average particle size may be obtained from 50 representative particles of the ultra-high molecular weight polyethylene (B) magnified by an optical microscope or the like. It has been confirmed that almost the same values are obtained regardless of the average particle size.
[0079] The melting point (Tm) of the ultra-high molecular weight polyethylene (B) is preferably from 100 to 150°C, and more preferably from 120 to 140°C, because the effects of the present invention are more excellent. As described above, the melting point (Tm) of the ultra-high molecular weight polyethylene (B) is preferably close to the melting point (Tm) of the thermoplastic resin (A).
[0080] Commercially available examples of the ultra-high molecular weight polyethylene (B) include those manufactured by Mitsui Chemicals under the trade names "Hiex Million (registered trademark)" and "Mipelon (registered trademark)" and those manufactured by Celanese Corporation under the trade name "GUR (registered trademark)".
[0081] The ultra-high molecular weight polyethylene (B) may be used alone or in combination of two or more kinds having different viscosity average molecular weights (Mv) or average particle sizes (D50).
[0082] [Ultra-high molecular weight polyethylene (B) content] The content of the ultra-high molecular weight polyethylene (B) in the resin composition of the present invention may be selected so as to satisfy the sufficient impact resistance and moldability required for the obtained molded body, and specifically, from the viewpoint of imparting impact resistance, it is 1 part by mass or more, preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, relative to 100 parts by mass of the total of the thermoplastic resin (A) and the ultra-high molecular weight polyethylene (B). Also, from the viewpoint of moldability, it is less than 50 parts by mass, preferably 45 parts by mass or less, and more preferably 40 parts by mass or less. If the ultra-high molecular weight polyethylene (B) is contained in an amount of 50 parts by mass or more, many parts in which the molten resin does not flow are generated in each layer in the three-dimensional molding process, and the moldability and the mechanical properties of the obtained molded body tend to decrease due to the decrease in interlayer adhesion.
[0083] [Other ingredients] The resin composition of the present invention may contain additives that are generally blended as appropriate within the range that does not significantly impair the effects of the present invention. Examples of the additives include inorganic particles such as silica, alumina, and kaolin, organic particles such as acrylic resin particles and melamine resin particles, pigments such as titanium oxide and carbon black, weather resistance stabilizers, heat resistance stabilizers, antistatic agents, electromagnetic wave absorbers, melt viscosity improvers, crosslinking agents, lubricants, nucleating agents, plasticizers, antioxidants, antioxidants, light stabilizers, ultraviolet absorbers, neutralizers, antifogging agents, antiblocking agents, slip agents, and colorants, which are added for the purpose of improving and adjusting the moldability, the stability of the three-dimensional molded object, and various physical properties of the three-dimensional molded object. These other components may be blended into the three-dimensional modeling material separately from the resin composition of the present invention.
[0084] The content of these additives is not particularly specified, but from the viewpoint of the stability of the obtained 3D modeling material and the 3D modeled object, the total amount of additives is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, even more preferably 0.08 parts by mass or more, and particularly preferably 0.1 parts by mass or more, relative to 100 parts by mass of the 3D modeling material in total. In addition, from the viewpoint of suppressing a decrease in interlayer adhesion of the molded product to be modeled, the upper limit of the total content of additives is preferably 30 parts by mass or less, more preferably 28 parts by mass or less, and even more preferably 25 parts by mass or less.
[0085] The resin composition of the present invention may contain, in addition to the above-mentioned additives, a reinforcing material that is generally blended, as appropriate, within the range that does not significantly impair the effects of the present invention. These reinforcing materials may be blended into the three-dimensional modeling material separately from the resin composition of the present invention.
[0086] Specific examples of the reinforcing material include inorganic fillers and inorganic fibers. Specific examples of inorganic fillers include calcium carbonate, zinc carbonate, magnesium oxide, calcium silicate, sodium aluminate, calcium aluminate, sodium aluminosilicate, magnesium silicate, potassium titanate, glass balloons, glass flakes, glass powder, silicon carbide, silicon nitride, boron nitride, gypsum, calcined kaolin, zinc oxide, antimony trioxide, zeolite, hydrotalcite, wollastonite, silica, talc, mica, nanocloy, metal powders such as magnesium, alumina, graphite, carbon black, and carbon nanotubes. Specific examples of inorganic fibers include cut glass fibers, milled glass fibers, glass fibers, gypsum whiskers, metal fibers, metal whiskers, ceramic whiskers, carbon fibers, and cellulose nanofibers.
[0087] The content of the reinforcing material in the three-dimensional modeling material or the resin composition of the present invention is not particularly limited, but from the viewpoint of the strength of the molded product to be modeled, it is preferably 1 part by mass or more, more preferably 5 parts by mass or more, and even more preferably 10 parts by mass or more relative to a total of 100 parts by mass of the three-dimensional modeling material. Also, from the viewpoint of suppressing a decrease in interlayer adhesion of the molded product to be modeled, it is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and even more preferably 30 parts by mass or less.
[0088] [Method of producing resin composition] The resin composition of the present invention can be produced by adding and mixing the thermoplastic resin (A), the ultra-high molecular weight polyethylene (B), and the other additives described above, which are blended as necessary, in a predetermined ratio. The method for producing the present resin composition is not particularly limited as long as it contains each component. For example, the thermoplastic resin (A) and other components, such as additives, which are added as necessary, are premixed using various mixers such as a tumbler or a Henschel mixer, and then melt-kneaded using a Banbury mixer, a roll, a Brabender, a single-screw kneading extruder, a twin-screw kneading extruder, a kneader, or the like, to produce the resin composition of the present invention. The ultra-high molecular weight polyethylene (B), inorganic particles, organic particles, and reinforcing materials may be blended as a powder mixture by mixing them with a powder of the thermoplastic resin (A) produced by the method described below, without kneading them with the thermoplastic resin (A).
[0089] [3D modeling materials] The three-dimensional modeling material of the present invention is a material used for modeling a three-dimensional object (resin molded body) using a 3D printer.
[0090] The three-dimensional modeling material of the present invention may be composed of only the present resin composition, or may be a composite with other materials. For example, the three-dimensional modeling material of the present invention may have a single-layer structure composed of a single resin layer composed of the present resin composition. In addition, the three-dimensional modeling material of the present invention may have a multi-layer structure composed of a resin layer composed of the present resin composition and a layer composed of another material.
[0091] The shape of the material for 3D modeling may be any shape that can be applied to various types of 3D printers such as Material Extrusion, Powder Bed Fusion, Material Jetting, etc. Specific shapes of the material for 3D modeling include powder, pellets, granules, filaments, etc.
[0092] [3D modeling powder] The powder for three-dimensional modeling of the present invention is a powdered modeling material used in a powder bed fusion method. The production method, physical properties, etc. of the powder for three-dimensional modeling will be described in detail below.
[0093] <Method of manufacturing powder for 3D modeling> The powdering means for producing the powder for three-dimensional modeling of the present invention include melt granulation, in which the resin composition of the present invention melted near the melting point is made into a fibrous form and then cut, and pulverization, in which the resin composition of the present invention is cut or destroyed by applying impact or shear. In order to improve the coatability of the powder in Powder Bed Fusion modeling, it is preferable that the powder does not contain fine powder of about 10 μm and has a constant particle size and particle size distribution, so that a suitable powder method is selected to obtain powder of such a suitable shape.
[0094] As the pulverizing means, for example, a stamp mill, a ring mill, a stone mill, a mortar, a roller mill, a jet mill, a high-speed rotary mill, a hammer mill, a pin mill, a container-driven mill, a disk mill, a media stirring mill, or the like can be used.
[0095] In addition, in order to prevent the resin material from stretching due to shear heat during grinding, there is a method in which the resin temperature during grinding is lowered by cooling the powder system with liquid nitrogen or the like, and powder is produced by brittle fracture rather than ductile fracture. This is called low-temperature grinding or freeze grinding. Among them, it is preferable to use a high-speed rotary mill for pulverization, which can obtain powder with a particle size distribution and shape suitable for powder bed fusion molding, because this improves the flowability and powder application properties during molding. In addition, it is preferable to use liquid nitrogen to produce powder by brittle fracture of the resin material, in order to suppress changes in the physical properties and color of the resin material due to pulverization.
[0096] In addition, from the viewpoint of removing elongated powder from the pulverized powder to increase the circularity and from the viewpoint of removing fine powder to prevent the powder from flying up during handling, it is preferable to carry out a classification process after pulverization. In this case, classification methods include air classification, sieve classification, etc. In addition, the above-mentioned inorganic particles and reinforcing materials may be added and mixed into the obtained powder as necessary.
[0097] <Average particle size of powder for 3D modeling (D50)> As described above, the thermoplastic resin (A) contained in the resin composition of the present invention in an amount greater than the ultra-high molecular weight polyethylene (B) is preferably larger than the average particle size (D50) of the ultra-high molecular weight polyethylene (B), and therefore the average particle size (D50) of the powder for three-dimensional modeling of the present invention is preferably larger than the average particle size (D50) of the ultra-high molecular weight polyethylene (B). From this viewpoint, the average particle size (D50) of the powder for three-dimensional modeling of the present invention is preferably 1.2 to 30 times, particularly preferably 2 to 20 times, the average particle size (D50) of the ultra-high molecular weight polyethylene (B). Specifically, when the powder for three-dimensional modeling of the present invention is used as a material for the Powder Bed Fusion method, the average particle size (D50) depends on the specifications of the system used to form a molded body by the Powder Bed Fusion method, but from the viewpoint of applying the powder to a thickness within a predetermined range during modeling, it is preferably 20 μm or more, more preferably 30 μm or more, even more preferably 40 μm or more, particularly preferably 50 μm or more, and most preferably 55 μm or more, and is preferably 250 μm or less, more preferably 200 μm or less, even more preferably 150 μm or less, and particularly preferably 120 μm or less.
[0098] [Molded body] The molded body of the present invention is made of the above-mentioned material for three-dimensional modeling of the present invention or the powder for three-dimensional modeling of the present invention. As a method for producing the molded body of the present invention, molding is preferably performed by using a three-dimensional printer. The detailed manufacturing method is described below.
[0099] [Method for producing molded body] In the method for producing a molded body made of the three-dimensional modeling material or powder for three-dimensional modeling of the present invention, the material for three-dimensional modeling or powder for three-dimensional modeling of the present invention is used, and a molded body is obtained by molding with a three-dimensional printer. Examples of molding methods using a three-dimensional printer include the Material Extrusion method, the Powder Bed Fusion method, the Material Jetting method, the Vat PhotoPolymerization method, etc. Among these, in the present invention, it is preferable to use the Powder Bed Fusion method, in which the molding material is in powder form.
[0100] In the Powder Bed Fusion method, particles of a material for three-dimensional modeling spread on a stage, i.e., the powder for three-dimensional modeling of the present invention, are irradiated with a laser or an electron beam to sinter or fuse the particles and form a layer in the height direction. Next, particles of the material for three-dimensional modeling are spread in contact with the layer formed above and irradiated with a laser or an electron beam to form the next layer. This method is a method of obtaining a molded body of a desired shape by successively stacking the layers in this manner. EXAMPLES
[0101] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention.
[0102] [Measurement and evaluation methods for physical properties] <Average particle size (D50)> 5 g of powder material was weighed out, and the particle size distribution of the powder was measured on a volume basis using a particle size distribution measuring device (manufactured by Horiba, Ltd.) that uses the laser diffraction method. The particle size at 50% of the frequency distribution of the powder was determined as the average particle size (D50). However, for commercially available products, some catalog values were used.
[0103] <Viscosity average molecular weight (Mv)> The viscosity average molecular weight (Mv) of the thermoplastic resin (A) and the ultra-high molecular weight polyethylene (B) was calculated by approximation using the specific viscosity ηsp (dl / g) of a 0.05% decalin solution at 135°C instead of the intrinsic viscosity [η] (dl / g) in accordance with the method shown in JIS K-7367 for the thermoplastic resin (A) or the method shown in ASTM D4020 for the ultra-high molecular weight polyethylene (B). For the propylene-based copolymer among the thermoplastic resins (A), the calculation was performed according to the following formula (I). Mv = 8.88 × 10 4 ηsp 1.25 …(I) For the ultra-high molecular weight polyethylene (B), the calculation was made according to the following formula (II). Mv = 5.37 × 10 4 ηsp 1.37 …(II)
[0104] <Melting point (Tm)> The melting points (Tm) of the thermoplastic resin (A) and the ultra-high molecular weight polyethylene (B) were measured by the following method. Using a differential scanning calorimeter manufactured by PerkinElmer Co., Ltd., product name "Pyris1 DSC", in accordance with JIS K7121, about 10 mg of powder sample was heated from room temperature to 200°C at a heating rate of 10°C / min, held at that temperature for 1 minute, cooled to 50°C at a heating rate of 10°C / min, and then heated again to 200°C at a heating rate of 10°C / min. The crystal melting temperature (melting point: Tm) (°C) (reheating process) showing the maximum peak in the melting curve detected from the measured thermogram was determined. The measured values were rounded off to one decimal place.
[0105] <Dispersibility> A 0.3 g powder sample for 3D modeling was placed in a recess of a table measuring 25 mm x 30 mm and 0.2 mm deep. The powder in the recess was then leveled by rolling a roller over the table at a speed of approximately 64 mm / sec. The spreadability was evaluated based on the state of the powder filled in the recess, using the following criteria. A: The powder is evenly distributed. B: The powder is not dispersed evenly or there is clumping of powder particles.
[0106] <Formability> Using a Powder Bed Fusion printer Lisa Pro (Sinterit), the printing area (Print bed) was set to a temperature above the cooling crystallization temperature and below the crystal melting temperature of the powder sample for 3D printing, and the material supply area (Feed bed) was set to a temperature above the cooling crystallization temperature of the powder sample. Test pieces with a length of 80 mm, width of 12.7 mm, thickness of 5 mm, and a V-notch of 2 mm were produced by printing with the thickness direction of the test piece as the stacking direction under conditions of a layer pitch of 0.125 mm. The presence or absence of printing defects was observed externally, and the printability was evaluated according to the following criteria. A: It is possible to mold the material, and the mechanical properties can be evaluated using the resulting test pieces. B: Printing is possible, but it is very fragile, or there are defects such as chipping.
[0107] <Impact resistance> The test pieces prepared for the evaluation of moldability were subjected to measurement of Charpy impact strength in accordance with JIS K7111-1. A Charpy impact test was performed on this test piece at a measurement temperature of 25° C., with a hammer capacity of 4 J, and with the striking surface opposite to the notch, to measure the Charpy impact value. The impact resistance of each test piece was calculated as a ratio to the Charpy impact value of Comparative Example 1, in which only the propylene-based copolymer powder was used as the molding material, and evaluated based on this ratio according to the following criteria. A: The ratio of Charpy impact values exceeds 100%. B: Charpy impact value ratio is 100% or less
[0108] <Overall rating> Based on the above evaluation results, the evaluation was made according to the following criteria. A: Both are "A" B: At least one of them is "B"
[0109] [Example 1] As the thermoplastic resin (A), propylene copolymer powder (manufactured by Sinterit) (A-1) (Mv: 119,000, Tm: 135 ° C, D50: 87 μm) powder material for LisaPro 3D printers was used. To this, 30 parts by mass of Mipelon (registered trademark) XM-220U (manufactured by Mitsui Chemicals) (B-1) (Mv: 2 million, Tm: 136 ° C, D50: 30 μm) was added as ultra-high molecular weight polyethylene (B) and dry blended. To this mixed powder, 0.3 parts by mass of carbon powder (fine powder SGP-10, manufactured by SEC Carbon, average particle size 10 μm) as an electromagnetic wave absorber was added to 100 parts by mass of ultra-high molecular weight polyethylene (B) and mixed to obtain a powder for 3D modeling (D50: 70 μm). The obtained powder for three-dimensional modeling was used for the above-mentioned evaluation, and the results are shown in Table 1.
[0110] [Example 2] As the thermoplastic resin (A), propylene-based copolymer powder (manufactured by Sinterit) (A-1) as powder material for LisaPro 3D printers was used. 10 parts by mass of Mipelon (registered trademark) PM-200 (manufactured by Mitsui Chemicals) (B-2) (Mv: 1.8 million, Tm: 137 ° C., D50: 10 μm) was added as ultra-high molecular weight polyethylene (B) to 90 parts by mass of the thermoplastic resin (A) and dry blended. To this mixed powder, 0.3 parts by mass of carbon powder (fine powder SGP-10, manufactured by SEC Carbon, average particle size 10 μm) as an electromagnetic wave absorber was added to 100 parts by mass of the ultra-high molecular weight polyethylene (B) and mixed to obtain a powder for 3D modeling (D50: 79 μm). The obtained powder for three-dimensional modeling was used for the above-mentioned evaluation, and the results are shown in Table 1.
[0111] [Comparative Example 1] Without using ultra-high molecular weight polyethylene (B), only propylene copolymer powder (manufactured by Sinterit) (A-1) of powder material for LisaPro3D printer was used, and carbon powder (fine powder SGP-10, manufactured by SEC Carbon, average particle size 10 μm) was not added and mixed to make powder for 3D modeling (D50: 87 μm). Since propylene copolymer powder (manufactured by Sinterit) (A-1) of powder material for LisaPro3D printer contains a laser absorbent, adding and mixing carbon powder is not necessary. The obtained powder for three-dimensional modeling was used for the above-mentioned evaluation, and the results are shown in Table 1.
[0112] [Comparative Example 2] A powder for 3D modeling (D50: 47 μm) was obtained in the same manner as in Example 1, except that the amount of propylene copolymer powder (manufactured by Sinterit) (A-1) used as the powder material for the LisaPro 3D printer was changed from 70 parts by mass to 30 parts by mass, and the amount of Mipelon (registered trademark) XM-220U (manufactured by Mitsui Chemicals, Inc.) (B-1) used was changed from 30 parts by mass to 70 parts by mass. The obtained powder for three-dimensional modeling was used for the above-mentioned evaluation, and the results are shown in Table 1.
[0113] [Comparative Example 3] A powder for 3D modeling (D50: 62 μm) was obtained in the same manner as in Example 1, except that silicone powder KMP-597 (manufactured by Shin-Etsu Chemical Co., Ltd.) (C-1) was used as the impact resistance modifier (C) instead of Mipelon (registered trademark) XM-220U (manufactured by Mitsui Chemicals, Inc.) (B-1), and 0.3 parts by mass of carbon powder (fine powder SGP-10, manufactured by SEC Carbon Co., Ltd., average particle size 10 μm) was added and mixed per 100 parts by mass of the impact resistance modifier (C). The obtained powder for three-dimensional modeling was used for the above-mentioned evaluation, and the results are shown in Table 1.
[0114] [Comparative Example 4] A powder for 3D modeling (D50: 83 μm) was obtained in the same manner as in Comparative Example 3, except that the amount of propylene copolymer powder (manufactured by Sinterit) (A-1) used as the powder material for the LisaPro 3D printer was changed to 95 parts by mass, and the amount of silicone powder KMP-597 (manufactured by Shin-Etsu Chemical Co., Ltd.) (C-1) used was changed to 5 parts by mass. The obtained powder for three-dimensional modeling was used for the above-mentioned evaluation, and the results are shown in Table 1.
[0115] [Comparative Example 5] A powder for 3D modeling (D50: 68 μm) was obtained in the same manner as in Example 1, except that the powdered cellulose KC Flock W-400G (manufactured by Nippon Paper Industries Co., Ltd.) (C-2) was used as the impact resistance modifier (C) instead of Mipelon (registered trademark) XM-220U (manufactured by Mitsui Chemicals, Inc.), and 0.3 parts by mass of carbon powder (fine powder SGP-10, manufactured by SEC Carbon Co., Ltd., average particle size 10 μm) was added and mixed per 100 parts by mass of the impact resistance modifier (C). The obtained powder for three-dimensional modeling was used for the above-mentioned evaluation, and the results are shown in Table 1.
[0116] [Comparative Example 6] Instead of Mipelon (registered trademark) XM-220U (manufactured by Mitsui Chemicals), the powder material for LisaPro3D printers, PA11 Onyx (manufactured by Sinterit) (C-3), was used as the impact resistance modifier (C), and carbon powder (fine powder SGP-10, manufactured by SEC Carbon, average particle size 10 μm) was not added and mixed, but a powder for 3D modeling (D50: 74 μm) was obtained in the same manner as in Example 1. Since the powder material for LisaPro3D printers, PA11 Onyx (manufactured by Sinterit) (C-3), contains a laser absorbent, it was not necessary to add and mix carbon powder. The obtained powder for three-dimensional modeling was used for the above-mentioned evaluation, and the results are shown in Table 1.
[0117] [Table 1]
[0118] As is clear from the above results, the three-dimensional modeling material of the present invention, which contains the resin composition comprising thermoplastic resin (A) and ultra-high molecular weight polyethylene (B), in which the content of ultra-high molecular weight polyethylene (B) is less than 50 parts by mass per 100 parts by mass of the combined total of thermoplastic resin (A) and ultra-high molecular weight polyethylene (B), is found to have excellent modeling properties in a 3D printer and excellent impact resistance of the resulting molded body. [Industrial Applicability]
[0119] According to the three-dimensional modeling material of the present invention, even when an existing resin powder for the Powder Bed Fusion method is used, it is possible to provide a three-dimensional modeling material that has excellent impact resistance of a molded body produced by a 3D printer while maintaining the modeling property and the safety of the powder material. Therefore, according to the three-dimensional modeling material of the present invention, the obtained three-dimensional model can be used not only for prototypes but also for practical applications such as components for home appliances, building materials, aircraft, and automobile materials.
Claims
1. A three-dimensional modeling material containing a resin composition, The resin composition includes a thermoplastic resin (A) having a viscosity average molecular weight (Mv) of less than 500,000, and an ultra-high molecular weight polyethylene (B) having a viscosity average molecular weight (Mv) of 500,000 or more and 10 million or less, A three-dimensional modeling material having a content of the ultra-high molecular weight polyethylene (B) of 1 part by mass or more and less than 50 parts by mass per 100 parts by mass of the total of the thermoplastic resin (A) and the ultra-high molecular weight polyethylene (B).
2. The three-dimensional modeling material according to claim 1 , wherein the ultra-high molecular weight polyethylene (B) is in powder form.
3. 2. The three-dimensional modeling material according to claim 1, wherein the powder of the ultra-high molecular weight polyethylene (B) has an average particle size (D50) of 10 μm or more and 200 μm or less, as measured by a laser diffraction method.
4. 2. The three-dimensional modeling material according to claim 1, wherein the three-dimensional modeling material, the thermoplastic resin (A), and the ultra-high molecular weight polyethylene (B) are in powder form, and the average particle size (D50) of the powder of the three-dimensional modeling material and the thermoplastic resin (A) is larger than the average particle size (D50) of the powder of the ultra-high molecular weight polyethylene (B) by a laser diffraction method.
5. 2. The material for three-dimensional modeling according to claim 1, wherein a difference in melting point (Tm) between the thermoplastic resin (A) and the ultra-high molecular weight polyethylene (B) is 70° C. or less, as measured at a heating rate of 10° C. / min in differential scanning calorimetry in accordance with JIS K7121.
6. The material for three-dimensional modeling according to claim 1 , wherein the thermoplastic resin (A) is a polyolefin resin.
7. The three-dimensional modeling material according to claim 6 , wherein the polyolefin resin is a propylene polymer.
8. A powder for three-dimensional modeling obtained by using the material for three-dimensional modeling according to any one of claims 1 to 7.
9. The powder for three-dimensional modeling according to claim 8, wherein the average particle size (D50) measured by a laser diffraction method is 5 μm or more and 250 μm or less.
10. A molded product obtained by using the material for three-dimensional modeling according to any one of claims 1 to 7.
11. A method for producing a molded body, comprising a step of three-dimensionally molding a molded body by a Powder Bed Fusion method using the material for three-dimensional molding according to any one of claims 1 to 7.
12. A molded product obtained by using the powder for three-dimensional modeling according to claim 8.
13. A method for producing a molded body, comprising a step of three-dimensionally molding a molded body by a Powder Bed Fusion method using the powder for three-dimensional molding according to claim 8.
Citation Information
Patent Citations
Powder for stereo-lithography, molding device, molding method and powder
JP2020093515A
Resin powder for three-dimensional molding, three-dimensional molded article, and method for producing three-dimensional molded article
WO2020213586A1