Polyethylene powder, molded body, and separator for secondary battery

A polyethylene powder with tailored intrinsic viscosity, amorphous thickness, and crystallite size, along with controlled Ti and Al content, addresses the balance of mechanical strength and thermal shrinkage in secondary battery separators, especially under high-speed molding.

JP2024146773APending Publication Date: 2024-10-15ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024026736
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-02-26
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing polyethylene powders for secondary battery separators face challenges in achieving a balanced mechanical strength and thermal shrinkage rate, particularly when molded at high speeds, with prior art failing to optimize this trade-off effectively.

Method used

The polyethylene powder is formulated with specific ranges for intrinsic viscosity, amorphous part thickness, crystallite size, and crystalline structure ratios, along with controlled Ti and Al content, to enhance mechanical strength while reducing thermal shrinkage, even under high-speed molding conditions.

Benefits of technology

The formulation results in a polyethylene powder that produces molded articles with an excellent balance between mechanical strength and thermal shrinkage rate, suitable for high-speed molding processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146773000001
    Figure 2024146773000001
  • Figure 2024146773000002
    Figure 2024146773000002
Patent Text Reader

Abstract

To provide, for example, polyethylene powder with which it is possible to obtain a molded body having an excellent balance between mechanical strength and heat shrinkage rate even in high-speed molding.SOLUTION: Polyethylene powder has the following features. An intrinsic viscosity IV measured according to ISO 1628-3(2010) is 1.5-15.0 dL / g. A thickness of an amorphous part is 5.3-12.0 nm. A crystal size obtained by reflection X-ray diffraction method is 13.9-18.0 nm.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyethylene powder, a molded body, and a separator for a secondary battery. [Background technology]

[0002] Polyethylene powder is used for various purposes, such as molding into sheets, films, and other shapes, and one of its important uses is as a raw material for separators in secondary batteries. Separators are molded bodies (typically microporous membranes) that are used primarily to prevent short circuits caused by direct contact between the positive and negative electrodes inside the battery and to allow only ions to pass through.

[0003] As described above, the separator for a secondary battery plays a very important role in ensuring the safety of the battery, and is required to have high mechanical strength and a small thermal shrinkage rate. From the viewpoint of thermal shrinkage, for example, Patent Document 1 proposes a polyethylene powder that can obtain a molded product with a small thermal shrinkage by using a catalyst with a saturated active site density for polymerization of the polyethylene powder. Furthermore, from the viewpoint of mechanical strength, for example, Patent Document 2 proposes a polyethylene powder that uses two or more types of catalysts in the polymerization of polyethylene powder and adjusts the degree of molecular entanglement by changing the active site density, thereby obtaining a microporous film with high mechanical strength. It is known that polyethylene is a crystalline polymer, and the crystal structure of polyethylene contributes to the physical properties of a molded article made of polyethylene. From this perspective, for example, Patent Document 3 proposes a technique for adjusting the lamella thickness of ultra-high molecular weight polyethylene powder in order to improve the mechanical strength of a microporous membrane for a lithium ion secondary battery. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2021 / 241411 [Patent Document 2] International Publication No. 2021 / 153520 [Patent Document 3] Patent No. 6868355 Summary of the Invention [Problem to be solved by the invention]

[0005] For secondary battery separators obtained using polyethylene powder, it is important to achieve both high mechanical strength and low thermal shrinkage. Although the mechanical strength and thermal shrinkage of secondary battery separators can be controlled by selecting raw materials and adjusting film formation conditions, there is a trade-off between the two, and it is difficult to achieve both in good condition at the same time using conventional technology. For example, a secondary battery separator obtained from the polyethylene powder described in Patent Document 1 has an excellent heat shrinkage rate, but the balance with the mechanical strength is not adjusted, and there is room for improvement. Furthermore, the secondary battery separator obtained from the polyethylene powder described in Patent Document 2 has excellent mechanical strength, but the balance with the thermal shrinkage rate is not adjusted, and there is room for improvement. Furthermore, in recent years, high-speed molding has been studied to improve the production efficiency of secondary battery separators. In order to mold secondary battery separators at high speed, it is necessary to increase the stretching speed in the stretching process in the separator manufacturing process. Here, a high stretching speed gives high residual stress to the separator, which tends to deteriorate the thermal shrinkage rate of the separator. For example, in the polyethylene powders of Patent Documents 1 and 2, the balance between mechanical strength and heat shrinkage rate in the case of high-speed molding is not adjusted, and there is room for improvement. In addition, the polyethylene powder described in Patent Document 3 is said to have excellent physical properties when the crystal structure is adjusted, but no adjustment is made to improve the balance between the mechanical strength and heat shrinkage rate of the microporous film obtained from the polyethylene powder, and no consideration has been given to adjusting the balance between the mechanical strength and heat shrinkage rate in the case of high-speed molding, leaving room for improvement.

[0006] The present invention has been made in consideration of the above circumstances, and has an object to provide a polyethylene powder and the like which can give a molded product having an excellent balance between mechanical strength and thermal shrinkage rate even in the case of high-speed molding. [Means for solving the problem]

[0007] Means for Solving the Problems The present inventors have conducted intensive research to solve the above-mentioned problems and have found that the above-mentioned problems can be solved by controlling the intrinsic viscosity IV, amorphous portion thickness and crystallite size of a polyethylene powder within specific ranges, thereby completing the present invention.

[0008] That is, the present invention includes the following aspects. [1] The intrinsic viscosity IV measured in accordance with ISO1628-3(2010) is 1.5 dL / g or more and 15.0 dL / g or less, The thickness of the amorphous portion is 5.3 nm or more and 12.0 nm or less, A polyethylene powder having a crystallite size of 13.9 nm or more and 18.0 nm or less, as determined by reflection X-ray diffraction method. [2] The polyethylene powder according to [1], wherein a ratio of monoclinic (010 plane) to orthorhombic (110 plane) obtained by reflection X-ray diffraction method is 1.0 or more and 2.6 or less, expressed as monoclinic (010) plane diffraction peak intensity / orthorhombic (110) plane diffraction peak intensity. [3] The polyethylene powder according to [1] or [2], having a Ti content of 10 ppm or less and an Al content of 20 ppm or less. [4] Average particle size D determined by sieving method 50 The polyethylene powder according to any one of [1] to [3], wherein the average particle size is 80 μm or more. [5] The polyethylene powder according to any one of [1] to [4], having an α-olefin content of less than 0.03 mol %. [6] A molded body comprising the polyethylene powder according to any one of [1] to [5]. [7] A separator for a secondary battery, comprising the molded article according to [6]. Effect of the Invention

[0009] According to the present invention, it is possible to provide a polyethylene powder or the like which can give a molded product having an excellent balance between mechanical strength and thermal shrinkage even when molded at high speed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention (hereinafter, also referred to as "the present embodiment") will be described in detail. Note that the present invention is not limited to the present embodiment, and various modifications can be made within the scope of the gist of the present invention.

[0011] [Polyethylene powder] The polyethylene powder of this embodiment (hereinafter also simply referred to as "powder") has an intrinsic viscosity IV measured in accordance with ISO1628-3 (2010) of 1.5 dL / g or more and 15.0 dL / g or less, an amorphous thickness of 5.3 nm or more and 12.0 nm or less, and a crystallite size obtained by reflection X-ray diffraction method of 13.9 nm or more and 18.0 nm or less. Since the polyethylene powder of the present embodiment has the above-mentioned structure, it is possible to obtain a molded product having an excellent balance between mechanical strength and thermal shrinkage rate even when molded at high speed. In addition, since the polyethylene powder of the present embodiment is configured as described above, it tends to be possible to obtain a molded product having an excellent balance between mechanical strength and thermal shrinkage rate even under typical molding conditions that have been conventionally known.

[0012] The polyethylene powder of this embodiment has an intrinsic viscosity IV of 1.5 dL / g or more. With an intrinsic viscosity IV in the above range, the strength of the molded body tends to be further improved. Furthermore, the polyethylene powder of this embodiment has an intrinsic viscosity IV of 15.0 dL / g or less. With an intrinsic viscosity IV in the above range, the polyethylene powder of this embodiment tends to have further improved moldability. From the above viewpoint, the intrinsic viscosity IV is preferably 2.0 dL / g or more. Also, from the above viewpoint, the intrinsic viscosity IV is preferably 14.0 dL / g or less, more preferably 13.5 dL / g or less. Thus, the intrinsic viscosity IV is preferably 2.0 dL / g or more and 14.0 dL / g or less, more preferably 2.0 dL / g or more and 13.5 dL / g or less.

[0013] The method of controlling the intrinsic viscosity IV within the above range is not particularly limited, but for example, changing the polymerization temperature of the reactor when homopolymerizing ethylene or copolymerizing ethylene with a copolymerizable olefin. The intrinsic viscosity IV tends to be lower as the polymerization temperature is increased, and tends to be higher as the polymerization temperature is decreased. In addition, another method of controlling the intrinsic viscosity IV within the above range is not particularly limited, but for example, changing the type of organometallic compound used as a cocatalyst when homopolymerizing ethylene or copolymerizing ethylene with a copolymerizable olefin. In addition, another method of controlling the intrinsic viscosity IV within the above range is not particularly limited, but for example, adding a chain transfer agent when homopolymerizing ethylene or copolymerizing ethylene with a copolymerizable olefin. By adding a chain transfer agent, the intrinsic viscosity IV of the polyethylene produced at the same polymerization temperature tends to be lower. The chain transfer agent is not particularly limited, but for example, hydrogen and the like can be mentioned. In this embodiment, the intrinsic viscosity IV can be determined by the method described in the Examples section below.

[0014] [Amorphous thickness and crystallite size] In this specification, the amorphous thickness is calculated from the following formula using the crystallinity obtained by subjecting a polyethylene powder to reflection X-ray diffraction and the crystal long period obtained by transmission wide-angle X-ray scattering. Amorphous thickness = (1 - crystallinity) x crystal long period In this specification, the crystallite size means the crystallite size of the (110) plane obtained by subjecting the polyethylene powder to reflection X-ray diffraction method.

[0015] The amorphous portion of the polyethylene powder of this embodiment has a thickness of 5.3 nm or more and 12.0 nm or less. In the polyethylene powder of this embodiment, since the amorphous portion thickness is in the above range, when the polyethylene powder is molded into a microporous membrane, the shish portions in the shish-kebab structure that can be observed become longer and the number of kebab portions becomes smaller, and the stretching load during stretching becomes smaller, which tends to improve the heat shrinkage. Furthermore, even in high-speed molding, the stretching load during stretching is small, which tends to improve the heat shrinkage. From the above viewpoints, the thickness of the amorphous portion is preferably 7.0 nm or more and 12.0 nm or less, and more preferably 9.0 nm or more and 12.0 nm or less.

[0016] The crystallite size of the polyethylene powder of this embodiment is 13.9 nm or more and 18.0 nm or less. Since the polyethylene powder of this embodiment has a crystallite size within the above range, the number of shish-kebab structures per volume of the microporous membrane is small, and the orientation degree of the shish parts is high, which tends to improve strength. From this viewpoint, the crystallite size is preferably 14.5 nm or more and 18.0 nm or less, and more preferably 15.0 nm or more and 18.0 nm or less.

[0017] The method for controlling the amorphous portion thickness and crystallite size to be within the above range is not particularly limited, but examples thereof include a method in which the polyethylene powder is annealed to grow crystals and then rapidly cooled, by containing a strongly entangled polyethylene component to suppress the occurrence of a folded structure, and the like. Specifically, there is a method in which polymerization is performed in an environment of high temperature and pressure in order to incorporate strongly entangled polyethylene components, and then cooling treatment is performed on the polyethylene powder immediately after polymerization. The polymerization temperature for incorporating strongly entangled polyethylene components is preferably 84°C or higher, more preferably 86°C or higher. The polymerization pressure for incorporating strongly entangled polyethylene components is preferably 0.4 MPa or higher, more preferably 0.5 MPa or higher. The cooling treatment conditions are preferably such that the polyethylene powder is exposed to an environment of 40°C or lower, more preferably such that the polyethylene powder is exposed to an environment of 10°C or lower. The cooling treatment is performed immediately after the polymerization step in the polyethylene production process, and there is, for example, a method of adjusting the temperature in the degassing step. In addition to the above-mentioned methods, a method for controlling the amorphous part thickness to a more preferred range is to use a catalyst with a high active site density during polymerization in order to incorporate a strongly entangled polyethylene component. The active site density can be adjusted by the amount of titanium compound used in preparing the catalyst, and is preferably 0.2 or more, more preferably 0.3 or more, and particularly preferably 0.4 or more, in terms of molar ratio to the magnesium atoms contained in the carrier. As a method for controlling the amorphous thickness and crystallite size to a more preferred range, there is a method of subjecting the polyethylene powder to a finish heat treatment. Here, the finish heat treatment refers to a treatment in which the powder is exposed to a high-temperature environment for a certain period of time, and then immediately exposed to a low-temperature environment. The high-temperature environment is preferably 80°C or higher, and more preferably 100°C or higher. The time for exposure to the high-temperature environment is preferably 30 minutes or more, and more preferably 1 hour or more. The low-temperature environment is preferably 0°C or lower, and more preferably -70°C or lower. As a method for controlling the amorphous thickness and the crystallite size within a more preferable range, there is a method in which the polyethylene powder polymerized with a catalyst having a high active site density is subjected to the above-mentioned finish heat treatment. As a method for controlling the amorphous portion thickness and the crystallite size within a more preferred range, there is a method in which polymerization is carried out in an environment of high temperature and pressure, and then the polyethylene powder obtained immediately after polymerization is subjected to a cooling treatment, and then the resulting polyethylene powder is subjected to a finish heat treatment. As a method for controlling the amorphous portion thickness and the crystallite size within a more preferred range, there is a method in which polymerization is carried out in an environment of high temperature and pressure using a catalyst having a high active site density, and then the polyethylene powder obtained immediately after polymerization is cooled, thereby carrying out a finish heat treatment on the obtained polyethylene powder. In this embodiment, the amorphous thickness and the crystallite size can be determined by the method described in the Examples below.

[0018] [Ratio of monoclinic (010 face) and orthorhombic (110 face)] In this specification, the ratio of monoclinic (010 plane) to orthorhombic (110 plane) in a polyethylene powder refers to the diffraction peak intensity ratio obtained by reflection X-ray diffraction method, and can be calculated as the monoclinic (010) plane diffraction peak intensity / orthorhombic (110) plane diffraction peak intensity. The ratio of monoclinic (010 plane) to orthorhombic (110 plane) in the polyethylene powder of this embodiment is preferably 1.0 or more and 2.6 or less. In the polyethylene powder of this embodiment, the ratio of monoclinic (010 plane) to orthorhombic (110 plane) is within the above-mentioned range, and therefore the proportion of orthorhombic crystals, which have a higher melting point than monoclinic crystals, is increased, making it possible to increase the heat setting temperature and reduce the thermal shrinkage rate. From this viewpoint, the ratio is more preferably 1.0 or more and 2.2 or less, and further preferably 1.0 or more and 1.8 or less.

[0019] There is no particular limitation on the method for controlling the ratio of monoclinic (010 plane) and orthorhombic (110 plane) crystals within the above range. For example, a method can be considered in which the polyethylene powder is heated to change the monoclinic crystals into the more stable orthorhombic crystals. Specifically, the method for controlling the ratio of monoclinic (010 face) and orthorhombic (110 face) crystals within the above range involves carrying out polymerization in an environment of high temperature and pressure, followed by cooling the polyethylene powder immediately after polymerization. The polymerization temperature is preferably 84°C or higher, more preferably 86°C or higher. The polymerization pressure is preferably 0.4 MPa or higher, more preferably 0.5 MPa or higher. The cooling conditions are preferably such that the polyethylene powder is exposed to an environment of 40°C or lower, more preferably such that the polyethylene powder is exposed to an environment of 10°C or lower. The cooling process is carried out immediately after the polymerization process in the polyethylene production process, and can be regulated, for example, by adjusting the temperature in the degassing process. In addition, a method for controlling the ratio of monoclinic (010 face) and orthorhombic (110 face) to a more preferred range is to subject the polyethylene powder to a finish heat treatment. Here, the finish heat treatment refers to a process in which the powder is exposed to a high-temperature environment for a certain period of time, and then immediately exposed to a low-temperature environment. The high-temperature environment is preferably 80°C or higher, and more preferably 100°C or higher. The time for exposure to the high-temperature environment is preferably 30 minutes or more, and more preferably 1 hour or more. The low-temperature environment is preferably 0°C or lower, and more preferably -70°C or lower. In addition, as a method for controlling the ratio of monoclinic (010 face) and orthorhombic (110 face) to a more preferable range, there is a method in which polymerization is performed in an environment of high temperature and pressure, and then the polyethylene powder obtained immediately after polymerization is cooled, and then a finish heat treatment is performed on the obtained polyethylene powder. In this embodiment, the ratio of monoclinic (010 plane) to orthorhombic (110 plane) can be determined by the method described in the examples below.

[0020] The polyethylene powder of the present embodiment may be, for example, a mixture containing a plurality of polyethylenes having different intrinsic viscosities, molecular weight distributions, and the like.

[0021] The polyethylene powder of the present embodiment may contain a homopolymer of ethylene (hereinafter, also simply referred to as "homopolymer"), or may contain a copolymer of ethylene and an olefin copolymerizable with ethylene (hereinafter, also simply referred to as "comonomer") (hereinafter, also simply referred to as "copolymer"). The copolymer may be a ternary random copolymer. The comonomer is not particularly limited, but examples thereof include α-olefins having 3 to 15 carbon atoms, cyclic olefins having 3 to 15 carbon atoms, and copolymers having the formula CH2=CHR 1 (where R 1 is an aryl group having 6 to 12 carbon atoms.) and straight-chain, branched or cyclic dienes having 3 to 15 carbon atoms. The comonomers may be used alone or in combination of two or more. Among these, α-olefins having 3 to 15 carbon atoms are preferred. The α-olefin is not particularly limited, but examples thereof include propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, and 1-tetradecene. The polyethylene powder of this embodiment preferably has an α-olefin content of less than 0.03 mol%. In this case, the mechanical strength of a molded body such as a microporous film obtained from the polyethylene powder of this embodiment tends to be improved. In this embodiment, when the content of a comonomer containing an α-olefin in the polyethylene powder is less than 0.03 mol%, the polyethylene powder can be evaluated as being composed of a homopolymer. Specifically, the α-olefin content in the polyethylene powder can be measured based on the method described in the examples below (the same applies to the content of comonomers other than α-olefin).

[0022] The polyethylene powder of the present embodiment may contain known additives that can be used in the production of polyethylene powder, if necessary. The additives are not particularly limited, but examples thereof include a neutralizing agent, an antioxidant, a crystal nucleating agent, and a light resistance stabilizer.

[0023] The neutralizing agent is used as a catcher for chlorine contained in polyethylene, a molding processing aid, etc. Examples of the neutralizing agent include, but are not limited to, stearates of alkaline earth metals such as calcium, magnesium, and barium. The content of the neutralizing agent in the polyethylene powder of the present embodiment is not particularly limited, but is preferably 5,000 ppm or less, more preferably 4,000 ppm or less, and even more preferably 3,000 ppm or less, based on the total amount of the polyethylene powder. When the polyethylene powder of the present embodiment is, for example, an ethylene polymer obtained by a slurry polymerization method using a metallocene catalyst, it is possible to exclude halogen components from the catalyst constituent components. In such cases, the above-mentioned neutralizing agent tends not to be used, and therefore the content of the neutralizing agent in the polyethylene powder of the present embodiment tends to be below the detection limit.

[0024] Examples of the antioxidant include, but are not limited to, phenolic antioxidants such as dibutylhydroxytoluene, pentaerythritol-tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], and octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate. The content of the antioxidant in the polyethylene powder of the present embodiment is not particularly limited, but is preferably 5,000 ppm or less, more preferably 4,000 ppm or less, and even more preferably 3,000 ppm or less.

[0025] Examples of the light resistance stabilizer include, but are not limited to, benzotriazole-based light resistance stabilizers such as 2-(5-methyl-2-hydroxyphenyl)benzotriazole and 2-(3-t-butyl-5-methyl-2-hydroxyphenyl)-5-chlorobenzotriazole; and hindered amine-based light resistance stabilizers such as bis(2,2,6,6-tetramethyl-4-piperidine)sebacate and poly[{6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidyl)imino}]. The content of the light resistance stabilizer in the polyethylene powder of the present embodiment is not particularly limited, but is preferably 5,000 ppm or less, more preferably 4,000 ppm or less, and even more preferably 3,000 ppm or less.

[0026] Examples of the crystal nucleating agent include, but are not limited to, calcium stearate, potassium stearate, etc. In addition, examples of polyethylene resin masterbatches containing a crystal nucleating agent include commercially available products such as "Rikemaster" (manufactured by Riken Vitamin Co., Ltd.). The content of the crystal nucleating agent in the polyethylene powder of the present embodiment is not particularly limited, but is preferably 5,000 ppm or less, more preferably 4,000 ppm or less, and even more preferably 3,000 ppm or less.

[0027] The content of additives that may be contained in the polyethylene powder of this embodiment can be determined by extracting the additives in the polyethylene powder by Soxhlet extraction using tetrahydrofuran (THF) for 6 hours, and separating and quantifying the extract by liquid chromatography.

[0028] [Titanium and aluminum content in polyethylene powder] The polyethylene powder of the present embodiment preferably has a titanium (Ti) content of 10 ppm or less and an aluminum (Al) content of 20 ppm or less. Titanium and aluminum are typically derived from residues of the polymerization catalyst, and small amounts of titanium and aluminum mean that the polyethylene powder has a small content of metal components derived from the polymerization catalyst. Therefore, when the titanium content and aluminum content contained in the polyethylene powder of the present embodiment are within the above ranges, the powder tends to be favorably applicable as a raw material for separators for lithium ion secondary batteries. From the above viewpoint, the titanium content is preferably 5 ppm or less, more preferably 2 ppm or less, and from the above viewpoint, the aluminum content is preferably 10 ppm or less, more preferably 4 ppm or less. The lower limits of the titanium content and the aluminum content are not particularly limited, but may be, for example, the detection limit values. The method for controlling the titanium content and aluminum content within the above range is not particularly limited, but they can be controlled, for example, by adjusting the productivity of polyethylene powder per unit catalyst. Specific methods for adjusting the productivity of the polyethylene powder include, for example, increasing the polymerization temperature in a reactor during production, increasing the polymerization pressure, and increasing the slurry concentration. The catalyst used is not particularly limited, and for example, a general Ziegler-Natta catalyst or a metallocene catalyst can be used, but it is preferable to use the catalyst described below. The titanium content and aluminum content can be determined by the method described in the Examples below.

[0029] [Average particle diameter D 50 ] The average particle diameter D of the polyethylene powder of this embodiment 50 It is preferable that the thickness is 80 μm or more. The polyethylene powder of the present embodiment has an average particle diameter D 50 When the viscosity is within the above range, the handling property is further improved and problems during the molding process tend to be reduced. From the above viewpoint, the average particle diameter D 50is more preferably 115 μm or more, even more preferably 140 μm or more, still more preferably 180 μm or more, even more preferably 200 μm or more, and even more preferably 205 μm or more. Average particle diameter D 50 The method for controlling the polymerization temperature within the above range is not particularly limited, but for example, the conditions in the polymerization system (polymerization temperature, ethylene pressure, etc.) can be appropriately adjusted. Specifically, the polymerization temperature and / or polymerization pressure can be increased. In addition, the average particle diameter D of the polyethylene powder of this embodiment 50 It is preferable that the thickness is 400 μm or less. The polyethylene powder of the present embodiment has an average particle diameter D 50 When the molecular weight is in the above range, the solubility in a solvent (e.g., liquid paraffin) becomes even better, and a gel having a more uniform distribution of molecular chains and a high degree of orientation can be obtained, which tends to enable the production of a separator for a lithium ion secondary battery having excellent mechanical strength. From the above viewpoint, the average particle diameter D 50 is more preferably 350 μm or less, and further preferably 300 μm or less. Average particle diameter D 50 The method for controlling the polymerization temperature within the above range is not particularly limited, but for example, the conditions in the polymerization system (polymerization temperature, ethylene pressure, etc.) can be appropriately adjusted. Specifically, the polymerization temperature and / or polymerization pressure can be reduced. In this embodiment, D 50 can be determined by the method described in the Examples below.

[0030] [Method of manufacturing polyethylene powder] (catalyst) The catalyst used for producing the polyethylene powder according to the present embodiment is not particularly limited, but may be, for example, a general Ziegler-Natta catalyst. The Ziegler-Natta catalyst is preferably a catalyst consisting of a solid catalyst [A] and an organometallic compound component [B], the solid catalyst [A] being an olefin polymerization catalyst produced by reacting an organomagnesium compound (hereinafter also referred to as "(A-1)") soluble in an inert hydrocarbon solvent and represented by the following formula 1 with a titanium compound (hereinafter also referred to as "(A-2)") represented by the following formula 2.

[0031] (A-1):(M 1 )α(Mg)β(R 2 ) a (R 3 ) b (Y 1 ) c ...Formula 1 (In the formula, M 1 is a metal atom belonging to the group consisting of groups 12, 13, and 14 of the periodic table, and R 2 and R 3 is a hydrocarbon group having 2 to 20 carbon atoms, and Y 1 is an alkoxy group, a siloxy group, an aryloxy group, an amino group, an amide group, -N=CR 4 , R 5 , -SR 6 (where R 4 , R 5 and R 6 represents a hydrocarbon group having 1 to 20 carbon atoms. When c is 2, Y 1 may be different from each other.) or a β-keto acid residue, and α, β, a, b, and c are real numbers that satisfy the following relationships: 0≦α, 0<β, 0≦a, 0≦b, 0≦c, 0 <a+b、0≦c / (α+β)≦2、nα+2β=a+b+c(ここで、nはM 1 Represents the valence of .

[0032] (A-2): Ti(OR 7 ) d X 1 (4-d) ...Formula 2 (wherein d is a real number between 0 and 4, and R7 is a hydrocarbon group having 1 to 20 carbon atoms, and X 1 is a halogen atom.)

[0033] The inert hydrocarbon solvent used in the reaction of (A-1) and (A-2) is not particularly limited, but specific examples include aliphatic hydrocarbons such as pentane, hexane, and heptane; aromatic hydrocarbons such as benzene and toluene; and alicyclic hydrocarbons such as cyclohexane and methylcyclohexane.

[0034] First, (A-1) will be described. (A-1) is shown in the form of an organomagnesium complex compound soluble in an inert hydrocarbon solvent, and includes all dihydrocarbylmagnesium compounds and complexes of these compounds with other metal compounds. The relational formula nα+2β=a+b+c of the symbols α, β, a, b, and c indicates the stoichiometry of the valence of the metal atom and the substituent.

[0035] In formula 1, R 2 and R 3 The hydrocarbon group having 2 to 20 carbon atoms is not particularly limited, but specifically includes an alkyl group, a cycloalkyl group, or an aryl group, such as an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, an octyl group, a decyl group, a cyclohexyl group, and a phenyl group. Among these, an alkyl group is preferable. When α>0, the metal atom M 1 As the metal atom, a metal atom belonging to the group consisting of groups 12, 13 and 14 of the periodic table can be used, for example, zinc, boron, aluminum, etc. Among these, aluminum and zinc are preferred.

[0036] metal atom M 1 The ratio β / α of magnesium to R is not particularly limited, but is preferably 0.1 to 30, more preferably 0.5 to 10. In addition, when a certain organomagnesium compound with α=0 is used, for example, R 2In the case where R is 1-methylpropyl or the like, it is soluble in an inert hydrocarbon solvent, and such a compound also gives a preferable result in this embodiment. 2 , R 3 It is recommended that patients meet one of the following three groups: (1), (2), or (3). Group(1):R 2 , R 3 At least one of R is a secondary or tertiary alkyl group having 4 to 6 carbon atoms. 2 , R 3 are both alkyl groups having 4 to 6 carbon atoms, and at least one of them is a secondary or tertiary alkyl group. Group(2):R 2 and R 3 and R are alkyl groups having different numbers of carbon atoms. 2 is an alkyl group having 2 or 3 carbon atoms, and R 3 is an alkyl group having 4 or more carbon atoms. Group(3):R 2 , R 3 At least one of R is a hydrocarbon group having 6 or more carbon atoms. 2 , R 3 The alkyl group must have 12 or more carbon atoms when added together.

[0037] Specific examples of these groups are shown below. In group (1), the secondary or tertiary alkyl group having 4 to 6 carbon atoms includes, for example, 1-methylpropyl, 2-methylpropyl, 1,1-dimethylethyl, 2-methylbutyl, 2-ethylpropyl, 2,2-dimethylpropyl, 2-methylpentyl, 2-ethylbutyl, 2,2-dimethylbutyl, and 2-methyl-2-ethylpropyl groups. Among these, 1-methylpropyl is particularly preferred. In addition, in group (2), specific examples of the alkyl group having 2 or 3 carbon atoms include ethyl, 1-methylethyl, and propyl groups. Among these, the ethyl group is particularly preferred. In addition, specific examples of the alkyl group having 4 or more carbon atoms include, but are not limited to, butyl, pentyl, hexyl, heptyl, and octyl groups. Among these, the butyl and hexyl groups are particularly preferred. Furthermore, in group (3), the hydrocarbon group having 6 or more carbon atoms is not particularly limited, but specific examples include a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, a phenyl group, a 2-naphthyl group, etc. Among the hydrocarbon groups, an alkyl group is preferable, and among the alkyl groups, a hexyl group and an octyl group are particularly preferable. Generally, the more carbon atoms contained in the alkyl group, the more easily the compound dissolves in an inert hydrocarbon solvent, but the more the viscosity of the solution tends to increase. Therefore, it is preferable to use an alkyl group with a moderately long chain in terms of handling. The above-mentioned organomagnesium compound can be used by diluting it with an inert hydrocarbon solvent, but it can be used without any problem even if a small amount of Lewis basic compound such as ether, ester, or amine is contained or remains in the solution.

[0038] Next, Y 1 In formula 1, Y 1 is an alkoxy group, a siloxy group, an aryloxy group, an amino group, an amide group, -N=CR 4 ,R 5 , -SR 6 (where R 4 , R 5 and R 6 each independently represents a hydrocarbon group having 2 to 20 carbon atoms, or a β-keto acid residue. In formula 1, R 4 , R 5 and R 6The hydrocarbon group represented by the formula (I) is preferably an alkyl group or aryl group having 1 to 12 carbon atoms, particularly preferably an alkyl group or aryl group having 3 to 10 carbon atoms. Although not particularly limited, examples thereof include a methyl group, an ethyl group, a propyl group, a 1-methylethyl group, a butyl group, a 1-methylpropyl group, a 1,1-dimethylethyl group, a pentyl group, a hexyl group, a 2-methylpentyl group, a 2-ethylbutyl group, a 2-ethylpentyl group, a 2-ethylhexyl group, a 2-ethyl-4-methylpentyl group, a 2-propylheptyl group, a 2-ethyl-5-methyloctyl group, an octyl group, a nonyl group, a decyl group, a phenyl group, and a naphthyl group. Among these, a butyl group, a 1-methylpropyl group, a 2-methylpentyl group, and a 2-ethylhexyl group are particularly preferred. In addition, in formula 1, Y 1 is preferably an alkoxy group or a siloxy group. The alkoxy group is not particularly limited, but specifically, for example, a methoxy group, an ethoxy group, a propoxy group, a 1-methylethoxy group, a butoxy group, a 1-methylpropoxy group, a 1,1-dimethylethoxy group, a pentoxy group, a hexoxy group, a 2-methylpentoxy group, a 2-ethylbutoxy group, a 2-ethylpentoxy group, a 2-ethylhexoxy group, a 2-ethyl-4-methylpentoxy group, a 2-propylheptoxy group, a 2-ethyl-5-methyloctoxy group, an octoxy group, a phenoxy group, and a naphthoxy group are preferable. Among these, a butoxy group, a 1-methylpropoxy group, a 2-methylpentoxy group, and a 2-ethylhexoxy group are more preferable. The siloxy group is not particularly limited, but specifically, for example, hydrodimethylsiloxy group, ethylhydromethylsiloxy group, diethylhydrosiloxy group, trimethylsiloxy group, ethyldimethylsiloxy group, diethylmethylsiloxy group, triethylsiloxy group, etc. are preferable. Among these, hydrodimethylsiloxy group, ethylhydromethylsiloxy group, diethylhydrosiloxy group, and trimethylsiloxy group are more preferable.

[0039] In this embodiment, the synthesis method of (A-1) is not particularly limited. For example, 2 MgX 1 , and formula R 2Mg(R 2 has the meaning mentioned above, and X 1 is a halogen atom.) and an organomagnesium compound of the formula M 1 R 3 n and M 1 R 3 (n-1) H(M 1 , and R 3 has the meaning as above, and n is M 1 ) in an inert hydrocarbon solvent at 25° C. to 150° C., and then, if necessary, reacting the compound with an organometallic compound of the formula Y 1 -H(Y 1 has the above-mentioned meaning.) or Y 1 Among these, the compound can be synthesized by reacting an organomagnesium compound and / or an organoaluminum compound having a functional group represented by the formula Y 1 When reacting a compound represented by formula Y with a compound represented by formula -H, the order of the reactions is not particularly limited. 1 -H, a method of adding a compound represented by the formula Y 1 Either a method of adding the organomagnesium compound to the compound represented by --H or a method of adding both simultaneously can be used. In this embodiment, Y relative to all metal atoms in (A-1) 1 The molar composition ratio c / (α+β) of is 0≦c / (α+β)≦2, and preferably 0≦c / (α+β)<1. 1 When the molar composition ratio of is 2 or less, the reactivity of (A-1) with respect to (A-2) tends to be improved.

[0040] Next, (A-2) will be described. (A-2) is a titanium compound represented by formula 2. (A-2): Ti(OR 7 ) d X 1 (4-d) ...Formula 2 (wherein d is a real number between 0 and 4, and R 7 is a hydrocarbon group having 1 to 20 carbon atoms, and X 1 is a halogen atom.) In the above formula 2, d is preferably 0 or more and 1 or less, and more preferably 0. 7 The hydrocarbon group represented by the formula (I) is not particularly limited, but specific examples thereof include aliphatic hydrocarbon groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, 2-ethylhexyl, heptyl, octyl, decyl, and aryl groups; alicyclic hydrocarbon groups such as cyclohexyl, 2-methylcyclohexyl, and cyclopentyl groups; and aromatic hydrocarbon groups such as phenyl and naphthyl groups. Among these, aliphatic hydrocarbon groups are preferred. X 1 Examples of the halogen atom represented by the formula include chlorine, bromine, and iodine. Among these, chlorine is preferred. In this embodiment, (A-2) is particularly preferably titanium tetrachloride. In this embodiment, it is possible to use a mixture of two or more compounds selected from the above.

[0041] Next, the reaction between (A-1) and (A-2) will be described. The reaction is preferably carried out in an inert hydrocarbon solvent, more preferably in an aliphatic hydrocarbon solvent such as hexane or heptane. The molar ratio of (A-1) to (A-2) in the reaction is not particularly limited, but the molar ratio (Ti / Mg) of Ti atoms contained in (A-2) to Mg atoms contained in (A-1) is preferably 0.1 to 10, more preferably 0.3 to 3. The reaction temperature is not particularly limited, but is preferably carried out in the range of -80°C to 150°C, more preferably -40°C to 100°C. The order of addition of (A-1) and (A-2) is not particularly limited, and any of the following methods is possible: adding (A-2) after (A-1), adding (A-2) after (A-1), or adding (A-1) and (A-2) simultaneously, but the method of adding (A-1) and (A-2) simultaneously is preferred. In this embodiment, the solid catalyst [A] obtained by the above reaction is used as a slurry solution using an inert hydrocarbon solvent.

[0042] Another example of the Ziegler-Natta catalyst used in the present embodiment is preferably an olefin polymerization catalyst comprising a solid catalyst [C] and an organometallic compound component [B], the solid catalyst [C] being produced by supporting an organomagnesium compound soluble in an inert hydrocarbon solvent represented by formula 5 (hereinafter also referred to as "(C-4)") and a titanium compound represented by formula 6 (hereinafter also referred to as "(C-5)") on a support (hereinafter also referred to as "(C-3)") prepared by reacting an organomagnesium compound soluble in an inert hydrocarbon solvent represented by formula 3 (hereinafter also referred to as "(C-1)") and a chlorinating agent represented by formula 4 (hereinafter also referred to as "(C-2)")

[0043] (C-1):(M 2 )γ(Mg)δ(R 8 ) e (R 9 ) f (OR 10 ) g ...Formula 3 (In the formula, M 2is a metal atom belonging to the group consisting of groups 12, 13, and 14 of the periodic table, and R 8 , R 9 and R 10 are hydrocarbon groups having 2 to 20 carbon atoms, and γ, δ, e, f, and g are real numbers that satisfy the following relationships: 0≦γ, 0<δ, 0≦e, 0≦f, 0≦g, 0 <e+f、0≦g / (γ+δ)≦2、kγ+2δ=e+f+g(ここで、kはM 2 Represents the valence of .

[0044] (C-2):H h SiCl i R 11 (4-(h+i)) ...Formula 4 (In the formula, R 11 is a hydrocarbon group having 1 to 12 carbon atoms, and h and i are real numbers that satisfy the following relationship: 0 <h、0<i、0<h+i≦4)

[0045] (C-4):(M 1 )α(Mg)β(R 2 ) a (R 3 ) b Y 1 c ...Formula 5 (In the formula, M 1 is a metal atom belonging to the group consisting of groups 12, 13, and 14 of the periodic table, and R 2 and R 3 is a hydrocarbon group having 2 to 20 carbon atoms, and Y 1 is alkoxy, siloxy, aryloxy, amino, amido, -N=CR 4 ,R 5 , -SR 6 (where R 4 , R 5 and R 6 represents a hydrocarbon group having 1 to 20 carbon atoms. When c is 2, Y 1 may be different from each other.) or a β-keto acid residue, and α, β, a, b, and c are real numbers that satisfy the following relationships: 0≦α, 0<β, 0≦a, 0≦b, 0≦c, 0 <a+b、0≦c / (α+β)≦2、nα+2β=a+b+c(ここで、nはM 1Represents the valence of .

[0046] (C-5): Ti(OR 7 ) d X 1 (4-d) ...Formula 6 (wherein d is a real number between 0 and 4, and R 7 is a hydrocarbon group having 1 to 20 carbon atoms, and X 1 is a halogen atom.)

[0047] First, (C-1) will be explained. (C-1) is shown as a form of an organomagnesium complex compound soluble in an inert hydrocarbon solvent, but it includes all dihydrocarbylmagnesium compounds and complexes of this compound with other metal compounds. The relational formula kγ+2δ=e+f+g of the symbols γ, δ, e, f, and g in formula 3 indicates the stoichiometry of the valence of the metal atom and the substituent. In the above formula, R 8 Or R 9 The hydrocarbon group represented by is not particularly limited, but specifically, each is an alkyl group, a cycloalkyl group, or an aryl group, and examples thereof include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, an octyl group, a decyl group, a cyclohexyl group, and a phenyl group. Among these, R 8 and R 9 are alkyl groups. When α>0, the metal atom M 2 As the metal atom, a metal atom belonging to the group consisting of Groups 12, 13 and 14 of the periodic table can be used, such as zinc, boron, aluminum, etc. Among these, aluminum and zinc are particularly preferred. metal atom M 2 The ratio δ / γ of magnesium to R is not particularly limited, but is preferably 0.1 to 30, more preferably 0.5 to 10. When a certain organomagnesium compound with γ=0 is used, for example, R 8 In the case where R is 1-methylpropyl or the like, it is soluble in an inert hydrocarbon solvent, and such a compound also gives a preferable result in this embodiment.8 , R 9 It is recommended that patients be in one of the following three groups: (1), (2), or (3). Group(1):R 8 , R 9 At least one of R is a secondary or tertiary alkyl group having 4 to 6 carbon atoms. 8 , R 9 Both have 4 to 6 carbon atoms, and at least one of them is a secondary or tertiary alkyl group. Group(2):R 8 and R 9 and R are alkyl groups having different carbon numbers. 8 is an alkyl group having 2 or 3 carbon atoms, and R 9 is an alkyl group having 4 or more carbon atoms. Group(3):R 8 , R 9 At least one of R is a hydrocarbon group having 6 or more carbon atoms. 8 , R 9 The sum of the carbon atoms contained in the alkyl group is 12 or more.

[0048] Specific examples of these groups are shown below. In group (1), the secondary or tertiary alkyl group having 4 to 6 carbon atoms includes, for example, 1-methylpropyl, 2-methylpropyl, 1,1-dimethylethyl, 2-methylbutyl, 2-ethylpropyl, 2,2-dimethylpropyl, 2-methylpentyl, 2-ethylbutyl, 2,2-dimethylbutyl, and 2-methyl-2-ethylpropyl groups. Among these, 1-methylpropyl is particularly preferred. In addition, in group (2), examples of the alkyl group having 2 or 3 carbon atoms include ethyl, 1-methylethyl, and propyl groups. Among these, the ethyl group is particularly preferred. Furthermore, examples of the alkyl group having 4 or more carbon atoms include, but are not limited to, butyl, pentyl, hexyl, heptyl, and octyl groups. Among these, butyl and hexyl groups are particularly preferred. Furthermore, in group (3), the hydrocarbon group having 6 or more carbon atoms is not particularly limited, but specific examples include a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, a phenyl group, a 2-naphthyl group, etc. Among the hydrocarbon groups, an alkyl group is preferable, and among the alkyl groups, a hexyl group and an octyl group are particularly preferable. Generally, the more carbon atoms contained in the alkyl group, the more easily the compound dissolves in an inert hydrocarbon solvent, and the more the viscosity of the solution tends to increase. Therefore, it is preferable to use an alkyl group with a moderate chain length in terms of handling. The above-mentioned organomagnesium compound is used as an inert hydrocarbon solution, but it can be used without any problem even if a small amount of Lewis basic compound such as ether, ester, or amine is contained or remains in the solution.

[0049] Next, the alkoxy group (OR 10 ) will be explained. 10 The hydrocarbon group represented by the formula (I) is preferably an alkyl group or aryl group having 1 to 12 carbon atoms, particularly preferably an alkyl group or aryl group having 3 to 10 carbon atoms. 10 is not particularly limited, and specific examples thereof include methyl, ethyl, propyl, 1-methylethyl, butyl, 1-methylpropyl, 1,1-dimethylethyl, pentyl, hexyl, 2-methylpentyl, 2-ethylbutyl, 2-ethylpentyl, 2-ethylhexyl, 2-ethyl-4-methylpentyl, 2-propylheptyl, 2-ethyl-5-methyloctyl, octyl, nonyl, decyl, phenyl, naphthyl, etc. Among these, butyl, 1-methylpropyl, 2-methylpentyl, and 2-ethylhexyl are particularly preferred.

[0050] In this embodiment, the synthesis method of (C-1) is not particularly limited, but it is preferable to use a compound represented by the formula R 8 MgX 1 and formula R 8 Mg(R 8 has the meaning mentioned above, and X 1 is a halogen atom.) and an organomagnesium compound of the formula M 2R 9 k and formula M 2 R 9 (k-1) H(M 2 , R 9 and k has the same meaning as above) in an inert hydrocarbon solvent at a temperature of 25° C. to 150° C., and if necessary, subsequently reacting with R 9 (R 9 has the above meaning.) R soluble in alcohol or inert hydrocarbon solvent having a hydrocarbon group represented by 9 In another preferred method, the compound is reacted with an alkoxy magnesium compound having a hydrocarbon group represented by the following formula: and / or an alkoxy aluminum compound. Among these, when an organomagnesium compound soluble in an inert hydrocarbon solvent is reacted with an alcohol, the order of the reaction is not particularly limited, and any of the following methods can be used: adding the alcohol to the organomagnesium compound, adding the organomagnesium compound to the alcohol, or adding both at the same time. In this embodiment, the reaction ratio of the organomagnesium compound soluble in an inert hydrocarbon solvent and the alcohol is not particularly limited, but the molar composition ratio g / (γ+δ) of the alkoxy group to the total metal atom in the alkoxy group-containing organomagnesium compound obtained as a result of the reaction is 0≦g / (γ+δ)≦2, and preferably 0≦g / (γ+δ)<1.

[0051] Next, (C-2) will be described. (C-2) is a silicon chloride compound represented by formula 4 and having at least one Si—H bond. (C-2):H h SiCl i R 11 (4-(h+i)) ...Formula 4 (In the formula, R 11 is a hydrocarbon group having 1 to 12 carbon atoms, and h and i are real numbers that satisfy the following relationship: 0 <h、0<i、0<h+i≦4)

[0052] In Equation 4, R 11The hydrocarbon group represented by is not particularly limited, but specifically includes an aliphatic hydrocarbon group, an alicyclic hydrocarbon group, and an aromatic hydrocarbon group, such as a methyl group, an ethyl group, a propyl group, a 1-methylethyl group, a butyl group, a pentyl group, a hexyl group, an octyl group, a decyl group, a cyclohexyl group, and a phenyl group. Among these, an alkyl group having 1 to 10 carbon atoms is preferred, and an alkyl group having 1 to 3 carbon atoms, such as a methyl group, an ethyl group, a propyl group, and a 1-methylethyl group, is more preferred. In addition, h and i are numbers larger than 0 that satisfy the relationship of h+i≦4, and it is preferred that i is 2 to 3. These compounds are not particularly limited, but specific examples include HSiCl3, HSiCl2CH3, HSiCl2C2H5, HSiCl2(C3H7), HSiCl2(2-C3H7), HSiCl2(C4H9), HSiCl2(C6H5), HSiCl2(4-Cl-C6H4), HSiCl2(CH=CH2), HSiCl2(CH2C6H5), HSiCl2(1-C 10 H7), HSiCl2(CH2CH=CH2), H2SiCl(CH3), H2SiCl(C2H5), HSiCl(CH3)2, HSiCl(C2H5)2, HSiCl(CH3)(2-C3H7), HSiCl(CH3)(C6H5), HSiCl(C6H5)2, etc. Silicon chloride compounds consisting of these compounds or mixtures of two or more selected from these compounds are used. Among these, HSiCl3, HSiCl2CH3, HSiCl(CH3)2, and HSiCl2(C3H7) are preferred, and HSiCl3 and HSiCl2CH3 are more preferred.

[0053] Next, the reaction between (C-1) and (C-2) will be described. In the reaction, it is preferable to dilute (C-2) in advance with an inert hydrocarbon solvent, chlorinated hydrocarbon such as 1,2-dichloroethane, o-dichlorobenzene, dichloromethane, etc.; ether medium such as diethyl ether, tetrahydrofuran, etc.; or a mixture of these. Among these, inert hydrocarbon solvents are more preferable in terms of catalyst performance. The reaction ratio between (C-1) and (C-2) is not particularly limited, but the silicon atom contained in (C-2) is preferably 0.01 mol or more and 100 mol or less, more preferably 0.1 mol or more and 10 mol or less, per 1 mol of magnesium atom contained in (C-1).

[0054] There is no particular restriction on the reaction method between (C-1) and (C-2), and any of the following methods can be used: simultaneous addition method in which (C-1) and (C-2) are simultaneously introduced into a reactor and reacted; method in which (C-2) is charged in advance into a reactor and then (C-1) is introduced into the reactor; or method in which (C-1) is charged in advance into a reactor and then (C-2) is introduced into the reactor. Among these, the method in which (C-2) is charged in advance into a reactor and then (C-1) is introduced into the reactor is preferred. The support (C-3) obtained by the above reaction is preferably separated by filtration or decantation, and then thoroughly washed with an inert hydrocarbon solvent to remove unreacted materials or by-products.

[0055] The reaction temperature between (C-1) and (C-2) is not particularly limited, but is preferably 25°C to 150°C, more preferably 30°C to 120°C, and even more preferably 40°C to 100°C. In the simultaneous addition method in which (C-1) and (C-2) are simultaneously introduced into a reactor and reacted, it is preferable to adjust the temperature of the reactor to a predetermined temperature in advance, and adjust the temperature in the reactor to a predetermined temperature while performing the simultaneous addition, thereby adjusting the reaction temperature to a predetermined temperature. In the method in which (C-2) is charged in a reactor in advance and then (C-1) is introduced into the reactor, it is preferable to adjust the temperature of the reactor in which the silicon chloride compound is charged to a predetermined temperature, and adjust the temperature in the reactor to a predetermined temperature while introducing the organomagnesium compound into the reactor, thereby adjusting the reaction temperature to a predetermined temperature. In the method of charging (C-1) into a reactor in advance and then introducing (C-2) into the reactor, it is preferable to adjust the temperature of the reactor into which (C-1) has been charged to a predetermined temperature, and then adjust the temperature inside the reactor to a predetermined temperature while introducing (C-2) into the reactor, thereby adjusting the reaction temperature to a predetermined temperature.

[0056] Next, the organomagnesium compound (C-4) will be described. As (C-4), the compound represented by the above formula 5 (C-4) is preferable.

[0057] (C-4):(M 1 )α(Mg)β(R 2 ) a (R 3 ) b Y 1 c ...Formula 5 (In the formula, M 1 is a metal atom belonging to the group consisting of groups 12, 13, and 14 of the periodic table, and R 2 and R 3 is a hydrocarbon group having 2 to 20 carbon atoms, and Y 1 is alkoxy, siloxy, aryloxy, amino, amido, -N=CR 4 ,R 5 , -SR 6 (where R 4 , R 5 and R6 represents a hydrocarbon group having 1 to 20 carbon atoms. When c is 2, Y 1 may be different from each other.) or a β-keto acid residue, and α, β, a, b, and c are real numbers that satisfy the following relationships: 0≦α, 0<β, 0≦a, 0≦b, 0 <a+b、0≦c / (α+β)≦2、nα+2β=a+b+c(ここで、nはM 1 Represents the valence of .

[0058] The amount of (C-4) used is preferably 0.1 or more and 10 or less, more preferably 0.5 or more and 5 or less, in terms of the molar ratio of magnesium atoms contained in (C-4) to titanium atoms contained in (C-5). The temperature for the reaction of (C-4) and (C-5) is not particularly limited, but is preferably in the range of -80°C or higher and 150°C or lower, and more preferably in the range of -40°C or higher and 100°C or lower. The concentration of (C-4) when used is not particularly limited, but is preferably 0.1 mol / L or more and 2 mol / L or less, and more preferably 0.5 mol / L or more and 1.5 mol / L or less, based on the titanium atoms contained in (C-4). It is preferable to use an inert hydrocarbon solvent to dilute (C-4). There is no particular restriction on the order of addition of (C-4) and (C-5) to (C-3), and any of the following methods is possible: adding (C-4) followed by (C-5), adding (C-4) followed by (C-5), or adding (C-4) and (C-5) simultaneously. Among these, the method of adding (C-4) and (C-5) simultaneously is preferred. The reaction between (C-4) and (C-5) is carried out in an inert hydrocarbon solvent, and it is preferable to use an aliphatic hydrocarbon solvent such as hexane or heptane. The catalyst thus obtained is used as a slurry solution using an inert hydrocarbon solvent.

[0059] Next, (C-5) will be described. In this embodiment, (C-5) is a titanium compound represented by the above formula 6. (C-5): Ti(OR 7 ) d X 1 (4-d)...Formula 6 (wherein d is a real number between 0 and 4, and R 7 is a hydrocarbon group having 1 to 20 carbon atoms, and X 1 is a halogen atom.)

[0060] In Equation 6, R 7 The hydrocarbon group represented by the formula (I) is not particularly limited, but specific examples thereof include aliphatic hydrocarbon groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, 2-ethylhexyl, heptyl, octyl, decyl, and aryl groups; alicyclic hydrocarbon groups such as cyclohexyl, 2-methylcyclohexyl, and cyclopentyl groups; and aromatic hydrocarbon groups such as phenyl and naphthyl groups. Among these, aliphatic hydrocarbon groups are preferred. X 1 The halogen atom represented by is not particularly limited, but specifically includes, for example, chlorine, bromine, and iodine. Among these, chlorine is preferable. The (C-5) selected from the above may be used alone or in combination of two or more. The amount of (C-5) used is not particularly limited, but is preferably 0.2 or more and 20 or less, more preferably 0.3 or more and 10 or less, and particularly preferably 0.4 or more and 5 or less, in terms of the molar ratio to the magnesium atoms contained in the carrier (C-3). The reaction temperature of (C-5) is not particularly limited, but is preferably in the range of -80°C or higher and 150°C or lower, and more preferably in the range of -40°C or higher and 100°C or lower. In this embodiment, the method for supporting (C-5) on (C-3) is not particularly limited. A method of reacting an excess of (C-5) with (C-3) or a method of efficiently supporting (C-5) by using a third component may be used, but a method of supporting (C-5) by reacting (C-5) with an organomagnesium compound (C-4) is preferred.

[0061] Next, the organometallic compound component [B] used in this embodiment will be described. The solid catalyst [A] or solid catalyst [C] used in this embodiment becomes a highly active polymerization catalyst by combining with the organometallic compound component [B]. The organometallic compound component [B] is sometimes called a "co-catalyst." The organometallic compound component [B] is preferably a compound containing a metal belonging to the group consisting of Groups 1, 2, 12, and 13 of the periodic table, and is particularly preferably an organoaluminum compound and / or an organomagnesium compound. As the organoaluminum compound, it is preferable to use a compound represented by the following formula 7 alone or in combination.

[0062] AlR 12 j Z 1 (3-j) ...Formula 7 (In the formula, R 12 is a hydrocarbon group having 1 to 20 carbon atoms, Z 1 is a group consisting of a hydrogen atom, a halogen atom, an alkoxy group, an aryloxy group, and a siloxy group, and j is a number between 2 and 3.

[0063] In the above formula 7, R 12The hydrocarbon group having 1 to 20 carbon atoms represented by the formula (1) is not particularly limited, but specifically includes aliphatic hydrocarbons, aromatic hydrocarbons, and alicyclic hydrocarbons, and for example, trialkylaluminum such as trimethylaluminum, triethylaluminum, tripropylaluminum, tributylaluminum, tri(2-methylpropyl)aluminum (or triisobutylaluminum), tripentylaluminum, tri(3-methylbutyl)aluminum, trihexylaluminum, trioctylaluminum, and tridecylaluminum, halogenated aluminum compounds such as diethylaluminum chloride, ethylaluminum dichloride, bis(2-methylpropyl)aluminum chloride, ethylaluminum sesquichloride, and diethylaluminum bromide, alkoxyaluminum compounds such as diethylaluminum ethoxide and bis(2-methylpropyl)aluminum butoxide, siloxyaluminum compounds such as dimethylhydrosiloxyaluminum dimethyl, ethylmethylhydrosiloxyaluminum diethyl, and ethyldimethylsiloxyaluminum diethyl, and mixtures thereof are preferred. Among these, trialkylaluminum compounds are particularly preferred.

[0064] As the organomagnesium compound, an organomagnesium compound which is soluble in an inert hydrocarbon solvent and is represented by the above formula 3 is preferred.

[0065] (M 2 )γ(Mg)δ(R 8 ) e (R 9 ) f (OR 10 ) g ...Formula 3 (In the formula, M 2 is a metal atom belonging to the group consisting of groups 12, 13, and 14 of the periodic table, and R 8 , R 9 and R 10are hydrocarbon groups having 2 to 20 carbon atoms, and γ, δ, e, f, and g are real numbers that satisfy the following relationships: 0≦γ, 0<δ, 0≦e, 0≦f, 0≦g, 0 <e+f、0≦g / (γ+δ)≦2、kγ+2δ=e+f+g(ここで、kはM 2 Represents the valence of .

[0066] The organomagnesium compound is shown in the form of an organomagnesium complex compound soluble in an inert hydrocarbon solvent, but includes all dialkylmagnesium compounds and complexes of this compound with other metal compounds. 2 , R 8 , R 9 , OR 10 As already mentioned, it is preferable that the organomagnesium compound has high solubility in an inert hydrocarbon solvent, so that δ / γ is preferably in the range of 0.5 to 10. 2 More preferred are compounds in which is aluminum. The combination ratio of the solid catalyst [A] or the solid catalyst [C] and the organometallic compound component [B] is not particularly limited, but it is preferable that the organometallic compound component [B] is 1 mmol or more and 3,000 mmol or less per 1 g of the solid catalyst [A] or the solid catalyst [C].

[0067] (Polymerization conditions) The polymerization method for producing the polyethylene powder of the present embodiment is not limited to the following, but examples thereof include a slurry polymerization method, a gas phase polymerization method, a solution polymerization method, etc. Among these, the slurry polymerization method, which can efficiently remove the heat of polymerization, is preferred. In the slurry polymerization method, an inert hydrocarbon medium can be used as the medium, and further, olefin itself can be used as the medium.The inert hydrocarbon medium is not limited to the following, but can be, for example, aliphatic hydrocarbons such as propane, butane, isobutane, pentane, isopentane, hexane, heptane, octane, decane, dodecane, kerosene, etc.; alicyclic hydrocarbons such as cyclopentane, cyclohexane, methylcyclopentane, etc.; aromatic hydrocarbons such as benzene, toluene, xylene, etc.; halogenated hydrocarbons such as ethyl chloride, chlorobenzene, dichloromethane, etc.; and mixtures thereof.

[0068] The polymerization temperature in the method for producing a polyethylene powder according to the present embodiment is preferably 80° C. or higher, and more preferably 84° C. or higher. A polymerization temperature of 80° C. or higher tends to enable more efficient industrial production. Furthermore, a polymerization temperature of 84° C. or higher tends to contain strongly entangled polyethylene components, to have a large amorphous thickness and crystallite size, and to have a small ratio of monoclinic (010 plane) and orthorhombic (110 plane) crystals. Moreover, the polymerization temperature is preferably not higher than 100° C. By keeping the polymerization temperature at not higher than 100° C., more stable continuous operation tends to be possible. The polymerization temperature can also be considered as one of the factors controlling the intrinsic viscosity IV of the polyethylene powder of the present embodiment. That is, the intrinsic viscosity IV of the polyethylene powder of the present embodiment tends to decrease as the polymerization temperature increases, and tends to increase as the polymerization temperature decreases.

[0069] The polymerization pressure in the method for producing the polyethylene powder of this embodiment is 0.3 MPa or more, preferably 0.4 MPa or more. A polymerization pressure of 0.3 MPa or more tends to enable more efficient industrial production. Furthermore, a polymerization pressure of 0.4 MPa or more tends to contain strongly entangled polyethylene components, have a large amorphous thickness and crystallite size, and have a small ratio of monoclinic (010 plane) and orthorhombic (110 plane) crystals. The polymerization pressure is preferably 1.5 MPa or less. By keeping the polymerization pressure at 1.5 MPa or less, localized heat generation due to a rapid polymerization reaction upon introduction of the catalyst can be suppressed, and polyethylene tends to be produced stably.

[0070] The polymerization reaction in the method for producing the polyethylene powder of this embodiment can be carried out in any of a batch system (batch system), a semi-continuous system, and a continuous system. It is also possible to carry out the polymerization in two or more stages having different reaction conditions. In this embodiment, in addition to the above-mentioned components, other known components (such as the above-mentioned additives) that are useful for the production (polymerization) of polyethylene can be used.

[0071] (Cooling process) The polyethylene powder of this embodiment can control the thickness of the amorphous portion by performing a cooling treatment immediately after the polymerization step. Here, the cooling treatment refers to a treatment of exposing to a low-temperature environment for a certain period of time. The low-temperature environment is preferably 40° C. or less, and more preferably 10° C. or less. The time of exposure to the low-temperature environment is preferably 30 minutes or more, and more preferably 1 hour or more. In an industrial production process of polyethylene powder, the cooling treatment is preferably carried out in a degassing treatment step which is carried out following the polymerization step. Specific cooling methods include, but are not limited to, a method in which polyethylene powder immediately after polymerization is introduced into a degassing tank adjusted to 10° C. together with hexane, the polymerization solvent, and held there for 30 minutes. The reason why the thickness of the amorphous portion is controlled by the cooling treatment is believed to be that the thickness of the amorphous portion increases when the polyethylene powder exposed to a high-temperature environment in the polymerization step is rapidly cooled.

[0072] (finishing heat treatment) The polyethylene powder of this embodiment can control the amorphous thickness and crystallite size by subjecting it to a finishing heat treatment. Here, the finishing heat treatment refers to a treatment in which the powder is exposed to a high-temperature environment for a certain period of time, and then immediately exposed to a low-temperature environment. The high-temperature environment is preferably 80°C or higher, and more preferably 100°C or higher. The time for exposure to the high-temperature environment is preferably 30 minutes or more, and more preferably 1 hour or more. The low-temperature environment is preferably 0°C or lower, and more preferably -70°C or lower. The time for exposure to the low-temperature environment is preferably 30 minutes or more, and more preferably 1 hour or more. In an industrial production process of polyethylene powder, the final heat treatment is preferably carried out after the drying step and before the packaging step. Specific examples of the finishing heat treatment method include, but are not limited to, heating the polyethylene powder in an oven at 100°C for 30 minutes, and then immediately immersing the polyethylene powder in a dry ice-ethanol bath to expose it to a temperature of -70°C or lower for 30 minutes. The reason why the thickness of the amorphous portion and the crystallite size are controlled by the above-mentioned finish heat treatment is believed to be that annealing at a temperature below the melting point of polyethylene causes crystals of the polyethylene powder to grow, and that rapid cooling of the annealed polyethylene powder increases the thickness of the amorphous portion.

[0073] [Molded body] The molded article of the present embodiment contains the polyethylene powder of the present embodiment. Here, "containing the polyethylene powder of the present embodiment" can be rephrased as "obtained by molding the polyethylene powder of the present embodiment". The molded article of the present embodiment is not particularly limited as long as it contains the polyethylene powder of the present embodiment, and examples thereof include sheets, films, pellets, and articles having other shapes. Examples of the molded article of the present embodiment include microporous membranes and heat-set membranes obtained by heat-setting the microporous membranes, and these can be preferably used as separators for secondary batteries. The molded body of the present embodiment may be obtained by subjecting the polyethylene powder of the present embodiment alone to molding processing, or may be obtained by combining the polyethylene powder of the present embodiment with a component different from the polyethylene powder of the present embodiment and then subjecting the combined product to molding processing.

[0074] [Separators for secondary batteries] The secondary battery separator of this embodiment includes the molded body of this embodiment. When the molded body of this embodiment is a microporous membrane or a heat-set membrane obtained by heat-setting the microporous membrane, it can be preferably used as a separator substrate in the secondary battery separator of this embodiment. Such a separator substrate alone can be used as the secondary battery separator of this embodiment, or a coating layer formed on the separator substrate can be used as the secondary battery separator of this embodiment. The secondary battery of this embodiment is not particularly limited, but examples thereof include lithium ion secondary batteries. EXAMPLES

[0075] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples in any way.

[0076] [Measurement method and conditions] The physical properties of the polyethylene powders of the Examples and Comparative Examples were measured by the following methods.

[0077] (1) Intrinsic viscosity IV The intrinsic viscosity IV of the polyethylene powders obtained in the examples and comparative examples was measured in accordance with ISO1628-3 (2010). The solvent used was 20 mL of decahydronaphthalene (containing 1 g / L of 2,6-di-t-butyl-4-methylphenol) that had been degassed with a vacuum pump and replaced with nitrogen. The viscosity tube used was a Cannon-Fenske type viscometer (manufactured by Shibata Scientific Instruments Co., Ltd.: product number 100).

[0078] (2) Crystal structure analysis The crystallinity, crystallite size ((110) crystallite size), and ratio of monoclinic (010) to orthorhombic (110) crystals of the polyethylene powder were calculated from the results obtained by reflection X-ray diffraction. The crystal long period used to calculate the amorphous thickness was obtained by analyzing the results obtained by transmission wide-angle X-ray scattering.

[0079] (Reflection X-ray diffraction measurement) XRD measurements were performed using a Rigaku Ultima-IV X-ray diffractometer. Cu-Kα rays were incident on the sample, and diffracted light was detected by a Rigaku D / tex Ultra detector. Measurements were performed under conditions of a sample-detector distance of 285 mm, an excitation voltage of 40 kV, and a current of 40 mA. A focused optical system was used, and measurements were performed under slit conditions of DS=1 / 2°, SS=open, and vertical slit=10 mm. Note that the measurement was performed at 1 s -1 The sample was rotated at .

[0080] (Transmission method X-ray scattering measurement) Small angle X-ray scattering measurements were performed using the transmission method with a Rigaku NANOPIX. As a pretreatment, the samples were impregnated with propylene glycol to reduce scattering from the particle surface. The samples were irradiated with Cu-Kα radiation, and scattering was detected with a semiconductor detector Hypix-6000. The measurement was performed with a sample-to-detector distance of 1312 mm, output of 40 kV, and 30 mA. A point focus optical system was used, and the slit diameters were 1st slit: φ=0.55 mm, 2nd slit: open, and guard slit: φ=0.35 mm.

[0081] (Method of separating crystalline diffraction peaks and amorphous diffraction peaks) A straight line baseline was drawn in the range from 2θ=9.7° to 2θ=29.0° of the obtained XRD profile, and the diffraction peaks were separated into four peaks: the orthorhombic (110) diffraction peak, the orthorhombic (200) diffraction peak, the monoclinic (010) diffraction peak, and the amorphous peak. The (110) diffraction peak and the (200) diffraction peak were approximated by a Voight function, and the (010) diffraction peak and the amorphous peak were approximated by a Gaussian function. The fitting was performed in the following manner. First, the peak position of the amorphous peak was fixed at 2θ=19.6° and the full width at half maximum was fixed at 6.3°, and the monoclinic (010) diffraction peak was not included, and the peak position and full width at half maximum of the diffraction peak derived from the orthorhombic crystal were not particularly fixed. After that, the peak position of the monoclinic (010) diffraction peak was fixed at 2θ=19.4° while the intensity of the amorphous peak was fixed, and peak separation was performed.

[0082] (Ratio of monoclinic (010 face) and orthorhombic (110 face)) The ratio of monoclinic (010 plane) to orthorhombic (110 plane) was calculated from the intensities of the orthorhombic (110) plane diffraction peak and the monoclinic (010) plane diffraction peak calculated by peak separation, using the following formula: Ratio of monoclinic (010 plane) to orthorhombic (110 plane) = Monoclinic (010) plane diffraction peak intensity / Orthorhombic (110) plane diffraction peak intensity

[0083] (Crystallite size, degree of crystallinity) The crystallite size ((110) crystallite size) was calculated from the full width at half maximum of the orthorhombic (110) diffraction peak of polyethylene calculated by peak separation according to Scherrer's formula (see below). The degree of crystallinity was calculated as a percentage by dividing the area of ​​the crystalline peak derived from the orthorhombic crystal by the sum of the separated crystalline peak and amorphous peak derived from the orthorhombic crystal. D(110) = Kλ / (βcosθ) D(110): Crystallite size (nm) K: 0.9 (constant) λ: wavelength of X-rays (nm) β:(β1 2 -β2 2 ) 0.5 β1: Full width at half maximum (rad) of the (hkl) peak calculated as a result of peak separation β2: Full width at half maximum of the incident beam divergence (rad) θ: Bragg angle

[0084] (Amorphous part thickness) For the X-ray scattering pattern obtained from the HyPix-6000, a SAXS profile I(q) was obtained by circular averaging. -1 <q<0.6nm -1 A straight line baseline was drawn in the range and fitted with a Gaussian function. The position of maximum intensity was determined as the peak position q due to the crystal long period. m The crystal long period was calculated from the following formula: d=2π / q m d(nm): Crystal long period q m (mm -1 ): Position of the peaks originating from lamellae in the SAXS profile

[0085] The amorphous thickness was calculated from the following formula using the crystallinity obtained by reflection X-ray diffraction and the crystal long period obtained by transmission wide-angle X-ray scattering. Amorphous thickness = (1 - crystallinity) x crystal long period

[0086] (3)Ti content and Al content The Ti and Al contents of the polyethylene powders obtained in the examples and comparative examples were evaluated by high-frequency plasma mass spectrometry in accordance with JIS K 0133. Samples were prepared by pressure decomposition with nitric acid using a microwave decomposition device (model ETHOS TC, manufactured by Milestone General Co., Ltd.). The elemental concentrations of titanium (Ti) and aluminum (Al) of the prepared samples were measured by the internal standard method using an ICP-MS (inductively coupled plasma mass spectrometer, model X-series X7, manufactured by Thermo Fisher Scientific Co., Ltd.), and these were taken as the Ti content and the Al content, respectively.

[0087] (4) Average particle diameter D 50 Polyethylene powder was classified using a sieve conforming to the JIS Z8801 standard. Sieve openings of 710 μm, 500 μm, 425 μm, 355 μm, 300 μm, 212 μm, 150 μm, 106 μm, 75 μm, and 53 μm were used. The mass of the powder collected for each fraction was measured. The cumulative undersize fraction (mass%) was calculated from the fraction (mass%) of each fraction relative to the total powder mass before classification. The particle diameter at which the cumulative undersize fraction was 50% was defined as the average particle diameter D 50 It was decided.

[0088] (5) α-Olefin Content The α-olefin content in the polyethylene powder was measured according to the method disclosed in GJ Ray et al., Macromolecules, 10, 773 (1977). 13 The intensity was calculated from the area intensity of the methylene carbon signal observed in the C-NMR spectrum. Measuring device: JEOL ECS-500 Observation kernel: 13 C Observation frequency: 100.53MHz Pulse width: 45° (7.5μsec) Pulse program: single pulse dec PD:5s Measurement temperature: 130℃ Accumulation count: 30,000 times or more Reference: PE(-eee-) signal is 29.9ppm Solvent: orthodichlorobenzene-d4 Sample concentration: 5-10wt% Melting temperature: 130~140℃ From the obtained α-olefin content, the polyethylene powder was evaluated as corresponding to a homopolymer or a copolymer (α-olefin copolymer) according to the following evaluation criteria. Note that the presence of olefins copolymerizable with ethylene other than α-olefins was not confirmed in any of the examples. (Evaluation Criteria) Homopolymer: α-olefin content less than 0.03 mol% Copolymer: α-olefin content 0.03 mol% or more

[0089] (6) Evaluation of strength and thermal shrinkage of molded body (heat-set film) When the total amount of polyethylene powder and liquid paraffin was 100 parts by mass, 30 parts by mass of polyethylene powder, 70 parts by mass of liquid paraffin (liquid paraffin (product name: Sumoil P-350P) manufactured by MORESCO Corporation), and 1 part by mass of antioxidant (tetrakis[methylene(3,5-di-t-butyl-4-hydroxyhydrocinnamate)]methane (product name: ANOX20) manufactured by Great Lakes Chemical Japan Co., Ltd.) were mixed and stirred to prepare a slurry liquid.

[0090] The obtained slurry liquid was put into a Labo Plastomill (body model: 4C150) manufactured by Toyo Seiki Seisakusho Co., Ltd., and kneaded at a constant temperature of 200°C for 10 minutes with a screw rotation speed of 50 rpm, and then heat-pressed at 180°C and 1 MPa for 3 minutes, further heat-pressed at 10 MPa for 2 minutes, and then cold-pressed at 25°C and 10 MPa for 5 minutes to form a gel sheet. The thickness of the gel sheet was adjusted to 1.0 mm by using a metal frame with a thickness of 1.0 mm.

[0091] 24 hours after molding the gel sheet, the gel sheet was stretched under the following conditions using a Bruckner batch-type biaxial stretching machine KARO V. (Stretching conditions) Gel sheet size: 95mm x 95mm Clip pressure: 4.5MPa Preheating / stretching temperature: 120℃ Fan airflow: 50% Preheat time: 45 seconds Stretching speed: 16mm / s Stretching ratio: 7x Stretching method: simultaneous biaxial

[0092] The stretched gel sheet was immersed in hexane to extract and remove the liquid paraffin, and then the hexane was dried and removed to obtain a microporous membrane. The microporous membrane was heat-set under the following conditions using a Bruckner batch-type biaxial stretching machine KARO V to obtain a heat-set membrane. The heat-setting temperature was set to a temperature at which the porosity of the heat-set membrane became 35%. (Heat setting treatment conditions) Microporous membrane size: 280mm x 280mm Clip pressure: 2MPa Fan airflow: 50% Preheat time: 0 seconds Stretching speed: 16.2% / s Relaxation speed: 6.2% / s TD maximum magnification: 1.97x TD relaxation rate: 0.812 times

[0093] The porosity of the heat-set film was evaluated as follows: A 10 cm × 10 cm square sample was cut from the heat-set film, and its thickness (cm) and basis weight (g / cm 2 ) and compare them with the true density (g / cm 3 ) was calculated using the following formula: Porosity (%) = (1-weight / (film thickness x true density)) x 100 Here, the true density of the polyethylene powder is 0.95 g / cm 3 was applied. 24 hours after obtaining the heat-set film, the puncture strength converted into basis weight and the heat shrinkage rate were evaluated.

[0094] (Evaluation of puncture strength converted into basis weight) Using a handy compression tester "KES-G5" manufactured by Kato Tech Co., Ltd., the heat-set film was first fixed with a sample holder with an opening diameter of 10 mm. Next, a puncture test was performed on the center of the fixed heat-set film with a needle tip curvature radius of 0.5 mm and a puncture speed of 10 mm / min to obtain the puncture strength (gf) as the maximum puncture load. The obtained puncture strength (gf) was expressed as the basis weight (g / m 2 ) to obtain the puncture strength converted into unit weight (gf / (g / m 2This procedure was carried out three times for three heat-set films, and the average value was calculated as the basis weight converted puncture strength (gf / (g / m 2 )) was decided.

[0095] (Evaluation of heat shrinkage rate) A 6 cm x 6 cm square sample cut from the heat-set film was placed in an envelope and heated at 120°C for 1 hour using a Yamato Scientific Co., Ltd. DKM600 low-temperature incubator. The sample was then cooled at room temperature for 15 minutes, and the length of the sides (perimeter) of the sample was measured with a curved ruler. The shrinkage rate from the circumference before heating was calculated using the following formula to calculate the heat shrinkage rate. This operation was performed three times with three heat-set films, and the average value of the three measurements was taken as the heat shrinkage rate (%). (Heat shrinkage rate) Heat shrinkage rate (%) = (1-L / 24) x 100 L: Circumference of the sample after heating (cm) From the obtained puncture strength converted into basis weight and heat shrinkage rate, the performance balance was evaluated from the values ​​of the puncture strength converted into basis weight and the heat shrinkage rate according to the following evaluation criteria. (Evaluation Criteria) ◎: Heat shrinkage rate ≦ 0.0625 × puncture strength converted into basis weight - 0.3750 〇: 0.0625 x puncture strength converted to unit area - 0.3750 < heat shrinkage rate ≦ 0.1875 x puncture strength converted to unit area - 5.1250 △: 0.1875 x puncture strength converted to unit weight - 5.1250 < heat shrinkage rate ≦ 0.2500 x puncture strength converted to unit weight - 6.5000 ×: 0.2500 × puncture strength converted into basis weight - 6.5000 < heat shrinkage rate

[0096] (7) Evaluation of strength and thermal shrinkage of molded body (heat-set film) when stretched at high speed A heat-set film was prepared in the same manner as in (6) above, except that the stretching speed when stretching the gel sheet was 32 mm / s, and the pin puncture strength converted into basis weight and the heat shrinkage rate were evaluated. From the obtained puncture strength converted into basis weight and heat shrinkage rate, the performance balance was evaluated from the values ​​of puncture strength converted into basis weight and heat shrinkage rate according to the following evaluation criteria. (Evaluation Criteria) ◎: Heat shrinkage rate ≦ 0.1250 × basis weight equivalent puncture strength - 1.7500 〇: 0.1250 x puncture strength converted to unit weight - 1.7500 < heat shrinkage rate ≦ 0.2500 x puncture strength converted to unit weight - 6.5000 △: 0.2500 x puncture strength converted to unit weight - 6.500 < heat shrinkage rate ≦ 0.3125 x puncture strength converted to unit weight - 6.8750 ×: 0.3125 × puncture strength converted to unit area - 6.8750 < heat shrinkage rate

[0097] [Catalyst synthesis method] [Catalyst [A]] (1) Synthesis of raw material [a-1] In an 8L stainless steel autoclave that had been thoroughly purged with nitrogen, 1 mol / L of Mg6(C4H9) 12 2,000mL of Al(C2H5)3 hexane solution (equivalent to 2000mmol of magnesium and aluminum) was charged, and 146mL of 5.47mol / L n-butanol hexane solution was added dropwise over 3 hours while stirring at 50℃, and the line was washed with 300mL of hexane after completion. Stirring was continued for another 2 hours at 50℃. After the reaction was completed, the mixture was cooled to room temperature and used as raw material [a-1]. The magnesium concentration of raw material [a-1] was 0.704mol / L.

[0098] (2) Synthesis of raw material [a-2] In an 8L stainless steel autoclave that had been thoroughly purged with nitrogen, 1 mol / L of Mg6(C4H9) 12 2,000mL of hexane solution of Al(C2H5)3 (equivalent to 2000mmol of magnesium and aluminum) was charged and stirred at 80℃, while 240mL of hexane solution of 8.33mol / L methylhydrogenpolysiloxane (Shin-Etsu Chemical Co., Ltd.) was pumped in, and stirring was continued for another 2 hours at 80℃. After the reaction was completed, the mixture was cooled to room temperature and used as raw material [a-2]. The total concentration of magnesium and aluminum in raw material [a-2] was 0.786mol / L.

[0099] (3) [A-1] Synthesis of carrier 1,000mL of 1mol / L hydroxytrichlorosilane hexane solution was charged into an 8L stainless steel autoclave that had been thoroughly purged with nitrogen, and 1,340mL of the hexane solution of the organomagnesium compound (raw material [a-1]) (equivalent to 943mmol of magnesium) was added dropwise over 3 hours at 65°C, and the reaction was continued for another 1 hour with stirring at 65°C. After the reaction was completed, the supernatant was removed and the mixture was washed four times with 1,800mL of hexane to obtain the [A-1] carrier. Analysis of this carrier revealed that it contained 7.5mmol of magnesium per 1g of solid.

[0100] (4) Preparation of catalyst [A] To 1,970 mL of hexane slurry containing 110 g of the above-mentioned [A-1] carrier, 400 mL of a 1 mol / L hexane solution of titanium tetrachloride and 131 mL of the raw material [a-2] were added simultaneously over a period of 3 hours while stirring at 10°C. After the addition, the reaction was continued for 1 hour at 10°C. After the reaction was completed, the supernatant was removed and the unreacted raw material components were removed by washing four times with hexane, and a solid catalyst [A] was prepared.

[0101] [Catalyst [B]] To 1,970 mL of hexane slurry containing 110 g of the above-mentioned [A-1] carrier, 103 mL of a 1 mol / L hexane solution of titanium tetrachloride and 131 mL of the raw material [a-2] were added simultaneously over a period of 3 hours while stirring at 10°C. After the addition, the reaction was continued for 1 hour at 10°C. After the reaction was completed, the supernatant was removed and the unreacted raw material components were removed by washing four times with hexane to prepare a solid catalyst [B].

[0102] [Catalyst [C]] As the solid catalyst [C], a metallocene catalyst was used, which was composed of the following silica support [C1], transition metal compound component [D] and activator [E].

[0103] (Preparation of Silica Support [C1]) As a precursor of the silica support [C1], the average particle size is 7 μm and the specific surface area is 660 m 2Silica with a molecular weight of 1.01 g / g, pore volume of 1.4 mL / g, and compressive strength of 7 MPa was used. The heat-treated silica (130 g) was dispersed in 2500 mL of hexane in an 8 L autoclave with nitrogen substitution to obtain a slurry. 195 mL of a hexane solution (concentration 1 M) of triethylaluminum, a Lewis acid compound, was added to the obtained slurry at 20°C under stirring. After that, the mixture was stirred for 2 hours to react triethylaluminum with the surface hydroxyl groups of the silica to prepare 2695 mL of a hexane slurry of the silica carrier [C1] with triethylaluminum adsorbed thereon.

[0104] (Preparation of transition metal compound component [D]) As the transition metal compound (D-1), [(N-t-butylamido)(tetramethyl-η 5 [-cyclopentadienyl)dimethylsilane]titanium-1,3-pentadiene (hereinafter abbreviated as "complex 1"). In addition, as an organomagnesium compound (D-2), a composition formula of Mg(C2H5)(C4H9) (hereinafter abbreviated as "Mg1") was used. 200 mmol of complex 1 was dissolved in 1000 mL of isoparaffin hydrocarbon (Isopar E manufactured by Exxon Mobil Corporation), 40 mL of a hexane solution of Mg1 (concentration 1 M) was added, and further hexane was added to adjust the concentration of complex 1 to 0.1 M, to obtain a transition metal compound component [D].

[0105] (Preparation of activator [E]) As the borate compound (E-1), 17.8 g of bis(hydrogenated tallow alkyl)methylammonium-tetrakis(pentafluorophenyl)borate (hereinafter abbreviated as "borate") was added and dissolved in 156 mL of toluene to obtain a 100 mmol / L toluene solution of borate. To this toluene solution of borate, 15.6 mL of a 1 mol / L hexane solution of ethoxydiethylaluminum was added as (E-2) at room temperature, and toluene was further added to adjust the borate concentration in the solution to 70 mmol / L. After that, the mixture was stirred at room temperature for 1 hour to prepare an activator [E] containing borate.

[0106] (Preparation of catalyst [C]) To 2695 mL of the slurry of the silica carrier [C1] obtained by the above operation, 219 mL of the activator [E] obtained by the above operation and 175 mL of the transition metal compound component [D] were simultaneously added from a separate line using a metering pump while stirring at 400 rpm at 25°C. The addition time was 30 minutes, and the reaction was continued for 3 hours thereafter, thereby preparing a solid catalyst [C].

[0107] (Preparation of liquid component [F]) As an organomagnesium compound [F1], the composition formula is AlMg6(C2H5)3(C4H9) 12 (hereinafter abbreviated as "Mg2") was used. 40 mL of hexane and Mg2 (total amount of Mg and Al: 38.0 mmol) were added to a 200 mL flask with stirring, and 40 mL of hexane containing 2.27 g (37.8 mmol) of methylhydrogenpolysiloxane (viscosity 20 centistokes at 25°C) was added at 20°C with stirring, and the temperature was then raised to 80°C and reacted for 3 hours with stirring to prepare liquid component [F].

[0108] (Preparation of hydrogenation catalyst [G]) 37.3 g of titanocene dichloride was introduced into a 2.0 L SUS autoclave equipped with a stirrer and purged with nitrogen, with 1 L of hexane. While stirring at 500 rpm, 429 mL of a 0.7 mol / L mixture of triisobutylaluminum and diisobutylaluminum hydride (9:1) was added by pump at room temperature over 1 hour. After addition, the line was washed with 71 mL of hexane. Stirring was continued for 1 hour to obtain a uniform 100 mM / L deep blue hydrogenation catalyst [G].

[0109] [Example 1] Polyethylene powder was polymerized by the method described below using a 1.5 L stainless steel autoclave polymerization reactor that had been thoroughly purged with nitrogen. First, 800 mL of hexane was charged as a solvent into a polymerization reactor heated to 86°C, and 0.4 mmol of the raw material [a-2] was added. Next, ethylene was added so that the internal pressure became 0.476 MPa, and hydrogen was added so that the internal pressure became 0.500 MPa. Furthermore, 10.0 mg of the catalyst [A] was added. The internal temperature was kept at 86°C, and polymerization was carried out for 60 minutes while stirring at a stirring speed of 1000 rpm. During the polymerization, the internal pressure was maintained at 0.500 MPa by supplying ethylene from time to time. After the polymerization was completed, the reaction mixture (polymer slurry) was extracted from the polymerization reactor, and the catalyst was deactivated with methanol. Thereafter, the reaction mixture was cooled to 8° C. and held for 30 minutes for cooling treatment. The reaction mixture was then filtered and air-dried to obtain a polyethylene powder. The polyethylene powder was then heated in an oven at 110°C for 30 minutes, and immediately thereafter subjected to a final heat treatment by immersing the polyethylene powder in a dry ice-ethanol bath and exposing it to a temperature of -70°C or lower for 30 minutes. The polymerization activity in the polymerization reactor was 13,600 g per 1 g of catalyst. Scale and extremely coarse particles were removed using a sieve with 425 μm openings, and the physical properties of the polyethylene powder were evaluated. The evaluation results are shown in Table 1.

[0110] [Example 2] Polyethylene powder was polymerized by the method described below using a 1.5 L stainless steel autoclave polymerization reactor that had been thoroughly purged with nitrogen. First, 800 mL of hexane was charged as a solvent into a polymerization reactor heated to 86°C, and 0.4 mmol of the raw material [a-2] was added. Next, ethylene was added so that the internal pressure became 0.493 MPa, and hydrogen was added so that the internal pressure became 0.500 MPa. Furthermore, 10.0 mg of the catalyst [A] was added. The internal temperature was kept at 86°C, and polymerization was carried out for 60 minutes while stirring at a stirring speed of 1000 rpm. During the polymerization, the internal pressure was maintained at 0.500 MPa by supplying ethylene from time to time. After the polymerization was completed, the reaction mixture (polymer slurry) was extracted from the polymerization reactor, and the catalyst was deactivated with methanol. Thereafter, the reaction mixture was cooled to 8° C. and held for 30 minutes for cooling treatment. The reaction mixture was then filtered and air-dried to obtain a polyethylene powder. The polyethylene powder was then heated in an oven at 110°C for 30 minutes, and immediately thereafter subjected to a final heat treatment by immersing the polyethylene powder in a dry ice-ethanol bath and exposing it to a temperature of -70°C or lower for 30 minutes. The polymerization activity in the polymerization reactor was 19,400 g per 1 g of catalyst. Scale and extremely coarse particles were removed using a sieve with 425 μm openings, and the physical properties of the polyethylene powder were evaluated. The evaluation results are shown in Table 1.

[0111] [Example 3] Polyethylene powder was polymerized by the method described below using a 1.5 L stainless steel autoclave polymerization reactor that had been thoroughly purged with nitrogen. First, 800 mL of hexane was charged as a solvent into a polymerization reactor heated to 86°C, and 0.4 mmol of the raw material [a-2] was added. Next, ethylene was added so that the internal pressure became 0.490 MPa, and hydrogen was added so that the internal pressure became 0.500 MPa. Furthermore, 10.0 mg of the catalyst [B] was added. The internal temperature was kept at 86°C, and polymerization was carried out for 60 minutes while stirring at a stirring speed of 1000 rpm. During the polymerization, the internal pressure was maintained at 0.500 MPa by supplying ethylene from time to time. After the polymerization was completed, the reaction mixture (polymer slurry) was extracted from the polymerization reactor, and the catalyst was deactivated with methanol. Thereafter, the reaction mixture was cooled to 8° C. and held for 30 minutes for cooling treatment. The reaction mixture was then filtered and air-dried to obtain a polyethylene powder. The polyethylene powder was then heated in an oven at 110°C for 30 minutes, and immediately thereafter subjected to a final heat treatment by immersing the polyethylene powder in a dry ice-ethanol bath and exposing it to a temperature of -70°C or lower for 30 minutes. The polymerization activity in the polymerization reactor was 18,600 g per 1 g of catalyst. Scale and extremely coarse particles were removed using a sieve with 425 μm openings, and the physical properties of the polyethylene powder were evaluated. The evaluation results are shown in Table 1.

[0112] [Example 4] Polyethylene powder was polymerized by the method described below using a 1.5 L stainless steel autoclave polymerization reactor that had been thoroughly purged with nitrogen. First, 800 mL of hexane was charged as a solvent into a polymerization reactor heated to 86°C, and 0.4 mmol of the raw material [a-2] was added. Next, ethylene was added so that the internal pressure became 0.480 MPa, and hydrogen was added so that the internal pressure became 0.500 MPa. Furthermore, 10.0 mg of the catalyst [B] was added. The internal temperature was kept at 86°C, and polymerization was carried out for 60 minutes while stirring at a stirring speed of 1000 rpm. During the polymerization, the internal pressure was maintained at 0.500 MPa by supplying ethylene from time to time. After the polymerization was completed, the reaction mixture (polymer slurry) was extracted from the polymerization reactor, and the catalyst was deactivated with methanol. Thereafter, the reaction mixture was cooled to 8° C. and held for 30 minutes for cooling treatment. The reaction mixture was then filtered and air-dried to obtain a polyethylene powder. The polyethylene powder was then heated in an oven at 110°C for 30 minutes, and immediately thereafter subjected to a final heat treatment by immersing the polyethylene powder in a dry ice-ethanol bath and exposing it to a temperature of -70°C or lower for 30 minutes. The polymerization activity in the polymerization reactor was 16,700 g per 1 g of catalyst. Scale and extremely coarse particles were removed using a sieve with 425 μm openings, and the physical properties of the polyethylene powder were evaluated. The evaluation results are shown in Table 1.

[0113] [Example 5] Polyethylene powder was polymerized by the method described below using a 1.5 L stainless steel autoclave polymerization reactor that had been thoroughly purged with nitrogen. First, 800 mL of hexane was charged as a solvent into a polymerization reactor heated to 84°C, and 0.4 mmol of the raw material [a-2] was added. Next, ethylene was added so that the internal pressure became 0.396 MPa, and hydrogen was added so that the internal pressure became 0.400 MPa. Furthermore, 10.0 mg of the catalyst [B] was added. The internal temperature was kept at 84°C, and polymerization was carried out for 60 minutes while stirring at a stirring speed of 1000 rpm. During the polymerization, the internal pressure was maintained at 0.400 MPa by supplying ethylene from time to time. After the polymerization was completed, the reaction mixture (polymer slurry) was extracted from the polymerization reactor, and the catalyst was deactivated with methanol. Thereafter, the reaction mixture was cooled to 35° C. and held for 30 minutes for cooling treatment. The reaction mixture was then filtered and air-dried to obtain a polyethylene powder. The polyethylene powder was then heated in an oven at 110°C for 30 minutes, and immediately thereafter subjected to a final heat treatment by immersing the polyethylene powder in a dry ice-ethanol bath and exposing it to a temperature of -70°C or lower for 30 minutes. The polymerization activity in the polymerization reactor was 12,000 g per 1 g of catalyst. Scale and extremely coarse particles were removed using a sieve with 425 μm openings, and the physical properties of the polyethylene powder were evaluated. The evaluation results are shown in Table 1.

[0114] [Example 6] Polyethylene powder was polymerized by the method described below using a 1.5 L stainless steel autoclave polymerization reactor that had been thoroughly purged with nitrogen. First, 800 mL of hexane was charged as a solvent into a polymerization reactor heated to 84°C, and 0.4 mmol of the raw material [a-2] was added. Next, ethylene was added so that the internal pressure was 0.374 MPa, 1-butene was added so that the internal pressure was 0.386 MPa, and hydrogen was added so that the internal pressure was 0.400 MPa. Furthermore, 10.0 mg of the catalyst [B] was added. The internal temperature was kept at 84°C, and polymerization was carried out for 60 minutes while stirring at a stirring speed of 1000 rpm. During the polymerization, the internal pressure was maintained at 0.400 MPa by supplying ethylene from time to time. After the polymerization was completed, the reaction mixture (polymer slurry) was extracted from the polymerization reactor, and the catalyst was deactivated with methanol. Thereafter, the reaction mixture was cooled to 35° C. and held for 30 minutes for cooling treatment. The reaction mixture was then filtered and air-dried to obtain a polyethylene powder. The polyethylene powder was then heated in an oven at 110°C for 30 minutes, and immediately thereafter subjected to a final heat treatment by immersing the polyethylene powder in a dry ice-ethanol bath and exposing it to a temperature of -70°C or lower for 30 minutes. The polymerization activity in the polymerization reactor was 12,700 g per 1 g of catalyst. Scale and extremely coarse particles were removed using a sieve with 425 μm openings, and the physical properties of the polyethylene powder were evaluated. The evaluation results are shown in Table 1.

[0115] [Example 7] Polyethylene powder was polymerized by the method described below using a 1.5 L stainless steel autoclave polymerization reactor that had been thoroughly purged with nitrogen. First, 800 mL of hexane was charged as a solvent into a polymerization reactor heated to 86°C, and 0.4 mmol of the raw material [a-2] was added. Next, ethylene was added so that the internal pressure became 0.491 MPa, and hydrogen was added so that the internal pressure became 0.500 MPa. Furthermore, 10.0 mg of the catalyst [A] was added. The internal temperature was kept at 86°C, and polymerization was carried out for 60 minutes while stirring at a stirring speed of 1000 rpm. During the polymerization, the internal pressure was maintained at 0.500 MPa by supplying ethylene from time to time. After the polymerization was completed, the reaction mixture (polymer slurry) was extracted from the polymerization reactor, and the catalyst was deactivated with methanol. Thereafter, the reaction mixture was cooled to 8° C. and held for 30 minutes for cooling treatment. The reaction mixture was then filtered and air-dried to obtain a polyethylene powder. The polyethylene powder was then heated in an oven at 110°C for 30 minutes, and immediately thereafter subjected to a final heat treatment by immersing the polyethylene powder in a dry ice-ethanol bath and exposing it to a temperature of -70°C or lower for 30 minutes. The polymerization activity in the polymerization reactor was 15,800 g per 1 g of catalyst. Scale and extremely coarse particles were removed using a sieve with 425 μm openings, and the physical properties of the polyethylene powder were evaluated. The evaluation results are shown in Table 1.

[0116] [Example 8] Polyethylene powder was polymerized by the method described below using a 1.5 L stainless steel autoclave polymerization reactor that had been thoroughly purged with nitrogen. First, 800 mL of hexane was charged as a solvent into a polymerization reactor heated to 80°C, and 0.4 mmol of the raw material [a-2] was added. Next, ethylene was added so that the internal pressure became 0.289 MPa, and hydrogen was added so that the internal pressure became 0.300 MPa. Furthermore, 10.0 mg of the catalyst [A] was added. The internal temperature was kept at 80°C, and polymerization was carried out for 60 minutes while stirring at a stirring speed of 1000 rpm. During the polymerization, the internal pressure was maintained at 0.300 MPa by supplying ethylene from time to time. After the polymerization was completed, the reaction mixture (polymer slurry) was extracted from the polymerization reactor, and the catalyst was deactivated with methanol. Thereafter, the reaction mixture was cooled to 50° C. and held for 30 minutes for a cooling treatment. The reaction mixture was then filtered and air-dried to obtain a polyethylene powder. The polyethylene powder was then heated in an oven at 110°C for 30 minutes, and immediately thereafter subjected to a final heat treatment by immersing the polyethylene powder in a dry ice-ethanol bath and exposing it to a temperature of -70°C or lower for 30 minutes. The polymerization activity in the polymerization reactor was 16,500 g per 1 g of catalyst. Scale and extremely coarse particles were removed using a sieve with 425 μm openings, and the physical properties of the polyethylene powder were evaluated. The evaluation results are shown in Table 1.

[0117] [Example 9] Polyethylene powder was polymerized by the method described below using a 1.5 L stainless steel autoclave polymerization reactor that had been thoroughly purged with nitrogen. First, 800 mL of hexane was charged as a solvent into a polymerization reactor heated to 80°C, and 0.4 mmol of the raw material [a-2] was added. Next, ethylene was added so that the internal pressure became 0.286 MPa, and hydrogen was added so that the internal pressure became 0.300 MPa. Furthermore, 10.0 mg of the catalyst [B] was added. The internal temperature was kept at 80°C, and polymerization was carried out for 60 minutes while stirring at a stirring speed of 1000 rpm. During the polymerization, the internal pressure was maintained at 0.300 MPa by supplying ethylene from time to time. After the polymerization was completed, the reaction mixture (polymer slurry) was extracted from the polymerization reactor, and the catalyst was deactivated with methanol. Thereafter, the reaction mixture was cooled to 50° C. and held for 30 minutes for a cooling treatment. The reaction mixture was then filtered and air-dried to obtain a polyethylene powder. The polyethylene powder was then heated in an oven at 110°C for 30 minutes, and immediately thereafter subjected to a final heat treatment by immersing the polyethylene powder in a dry ice-ethanol bath and exposing it to a temperature of -70°C or lower for 30 minutes. The polymerization activity in the polymerization reactor was 16,000 g per 1 g of catalyst. Scale and extremely coarse particles were removed using a sieve with 425 μm openings, and the physical properties of the polyethylene powder were evaluated. The evaluation results are shown in Table 1.

[0118] [Example 10] Polyethylene powder was polymerized by the method described below using a 1.5 L stainless steel autoclave polymerization reactor that had been thoroughly purged with nitrogen. First, 800 mL of hexane was charged as a solvent into a polymerization reactor heated to 86°C, and 0.4 mmol of the raw material [a-2] was added. Next, ethylene was added so that the internal pressure became 0.498 MPa, and hydrogen was added so that the internal pressure became 0.500 MPa. Furthermore, 10.0 mg of the catalyst [A] was added. The internal temperature was kept at 86°C, and polymerization was carried out for 60 minutes while stirring at a stirring speed of 1000 rpm. During the polymerization, the internal pressure was maintained at 0.500 MPa by supplying ethylene from time to time. After the polymerization was completed, the reaction mixture (polymer slurry) was extracted from the polymerization reactor, and the catalyst was deactivated with methanol. Thereafter, the reaction mixture was cooled to 8° C. and held for 30 minutes for cooling treatment. The reaction mixture was then filtered and air-dried to obtain a polyethylene powder. The polyethylene powder was then heated in an oven at 110°C for 30 minutes, and immediately thereafter subjected to a final heat treatment by immersing the polyethylene powder in a dry ice-ethanol bath and exposing it to a temperature of -70°C or lower for 30 minutes. The polymerization activity in the polymerization reactor was 22,000 g per 1 g of catalyst. Scale and extremely coarse particles were removed using a sieve with 425 μm openings, and the physical properties of the polyethylene powder were evaluated. The evaluation results are shown in Table 1.

[0119] [Example 11] Polyethylene powder was polymerized by the method described below using a 1.5 L stainless steel autoclave polymerization reactor that had been thoroughly purged with nitrogen. First, 800 mL of hexane was charged as a solvent into a polymerization reactor heated to 86°C, and 0.4 mmol of the raw material [a-2] was added. Next, ethylene was added so that the internal pressure became 0.49985 MPa, and hydrogen was added so that the internal pressure became 0.500 MPa. Furthermore, 10.0 mg of the catalyst [A] was added. The internal temperature was kept at 86°C, and polymerization was carried out for 60 minutes while stirring at a stirring speed of 1000 rpm. During the polymerization, the internal pressure was maintained at 0.500 MPa by supplying ethylene from time to time. After the polymerization was completed, the reaction mixture (polymer slurry) was extracted from the polymerization reactor, and the catalyst was deactivated with methanol. Thereafter, the reaction mixture was cooled to 8° C. and held for 30 minutes for cooling treatment. The reaction mixture was then filtered and air-dried to obtain a polyethylene powder. The polyethylene powder was then heated in an oven at 110°C for 30 minutes, and immediately thereafter subjected to a final heat treatment by immersing the polyethylene powder in a dry ice-ethanol bath and exposing it to a temperature of -70°C or lower for 30 minutes. The polymerization activity in the polymerization reactor was 25,900 g per 1 g of catalyst. Scale and extremely coarse powder were removed using a sieve with 425 μm openings, and the physical properties of the polyethylene powder were evaluated. The evaluation results are shown in Table 2.

[0120] [Example 12] Polyethylene powder was polymerized by the method described below using a 1.5 L stainless steel autoclave polymerization reactor that had been thoroughly purged with nitrogen. First, 800 mL of hexane was charged as a solvent into a polymerization reactor heated to 86°C, and 0.4 mmol of the raw material [a-2] was added. Next, ethylene was added so that the internal pressure became 0.495 MPa, and hydrogen was added so that the internal pressure became 0.500 MPa. Furthermore, 10.0 mg of the catalyst [A] was added. The internal temperature was kept at 86°C, and polymerization was carried out for 60 minutes while stirring at a stirring speed of 1000 rpm. During the polymerization, the internal pressure was maintained at 0.500 MPa by supplying ethylene from time to time. After the polymerization was completed, the reaction mixture (polymer slurry) was extracted from the polymerization reactor, and the catalyst was deactivated with methanol. Thereafter, the reaction mixture was cooled to 8° C. and held for 30 minutes for cooling treatment. The reaction mixture was then filtered and air-dried to obtain a polyethylene powder. The polyethylene powder was then heated in an oven at 110°C for 30 minutes, and immediately thereafter subjected to a final heat treatment by immersing the polyethylene powder in a dry ice-ethanol bath and exposing it to a temperature of -70°C or lower for 30 minutes. The polymerization activity in the polymerization reactor was 17,700 g per 1 g of catalyst. Scale and extremely coarse powder were removed using a sieve with 425 μm openings, and the physical properties of the polyethylene powder were evaluated. The evaluation results are shown in Table 2.

[0121] [Example 13] Polyethylene powder was polymerized by the method described below using a 1.5 L stainless steel autoclave polymerization reactor that had been thoroughly purged with nitrogen. First, 800 mL of hexane was charged as a solvent into a polymerization reactor heated to 86°C, and 0.4 mmol of the raw material [a-2] was added. Next, ethylene was added so that the internal pressure became 0.342 MPa, and hydrogen was added so that the internal pressure became 0.500 MPa. Furthermore, 10.0 mg of the catalyst [A] was added. The internal temperature was kept at 86°C, and polymerization was carried out for 60 minutes while stirring at a stirring speed of 1000 rpm. During the polymerization, the internal pressure was maintained at 0.500 MPa by supplying ethylene from time to time. After the polymerization was completed, the reaction mixture (polymer slurry) was extracted from the polymerization reactor, and the catalyst was deactivated with methanol. Thereafter, the reaction mixture was cooled to 8° C. and held for 30 minutes for cooling treatment. The reaction mixture was then filtered and air-dried to obtain a polyethylene powder. The polyethylene powder was then heated in an oven at 110°C for 30 minutes, and immediately thereafter subjected to a final heat treatment by immersing the polyethylene powder in a dry ice-ethanol bath and exposing it to a temperature of -70°C or lower for 30 minutes. The polymerization activity in the polymerization reactor was 15,600 g per 1 g of catalyst. Scale and extremely coarse powder were removed using a sieve with 425 μm openings, and the physical properties of the polyethylene powder were evaluated. The evaluation results are shown in Table 2.

[0122] [Example 14] Polyethylene powder was polymerized by the method described below using a 1.5 L stainless steel autoclave polymerization reactor that had been thoroughly purged with nitrogen. First, 800 mL of hexane was charged as a solvent into a polymerization reactor heated to 86°C, and 0.4 mmol of the raw material [a-2] was added. Next, ethylene was added so that the internal pressure was 0.489 MPa, 1-butene was added so that the internal pressure was 0.494 MPa, and hydrogen was added so that the internal pressure was 0.500 MPa. Furthermore, 10.0 mg of the catalyst [A] was added. The internal temperature was kept at 86°C, and polymerization was carried out for 60 minutes while stirring at a stirring speed of 1000 rpm. During the polymerization, the internal pressure was maintained at 0.500 MPa by supplying ethylene from time to time. After the polymerization was completed, the reaction mixture (polymer slurry) was extracted from the polymerization reactor, and the catalyst was deactivated with methanol. Thereafter, the reaction mixture was cooled to 8° C. and held for 30 minutes for cooling treatment. The reaction mixture was then filtered and air-dried to obtain a polyethylene powder. The polymerization activity in the polymerization reactor was 24,100 g per 1 g of catalyst. Scale and extremely coarse powder were removed using a sieve with 425 μm openings, and the physical properties of the polyethylene powder were evaluated. The evaluation results are shown in Table 2.

[0123] [Example 15] Polyethylene powder was polymerized by the method described below using a 1.5 L stainless steel autoclave polymerization reactor that had been thoroughly purged with nitrogen. First, 800 mL of hexane was charged as a solvent into a polymerization reactor heated to 86°C, and 0.4 mmol of the raw material [a-2] was added. Next, ethylene was added so that the internal pressure became 0.476 MPa, and hydrogen was added so that the internal pressure became 0.500 MPa. Furthermore, 10.0 mg of the catalyst [B] was added. The internal temperature was kept at 86°C, and polymerization was carried out for 60 minutes while stirring at a stirring speed of 1000 rpm. During the polymerization, the internal pressure was maintained at 0.500 MPa by supplying ethylene from time to time. After the polymerization was completed, the reaction mixture (polymer slurry) was extracted from the polymerization reactor, and the catalyst was deactivated with methanol. Thereafter, the reaction mixture was cooled to 8° C. and held for 30 minutes for cooling treatment. The reaction mixture was then filtered and air-dried to obtain a polyethylene powder. The polymerization activity in the polymerization reactor was 16,200 g per 1 g of catalyst. Scale and extremely coarse powder were removed using a sieve with 425 μm openings, and the physical properties of the polyethylene powder were evaluated. The evaluation results are shown in Table 2.

[0124] [Comparative Example 1] Polyethylene powder was polymerized by the method described below using a 1.5 L stainless steel autoclave polymerization reactor that had been thoroughly purged with nitrogen. First, 800 mL of hexane was charged as a solvent into a polymerization reactor heated to 80°C, and 0.4 mmol of the raw material [a-2] was added. Next, ethylene was added so that the internal pressure became 0.282 MPa, and hydrogen was added so that the internal pressure became 0.300 MPa. Furthermore, 10.0 mg of the catalyst [B] was added. The internal temperature was kept at 80°C, and polymerization was carried out for 60 minutes while stirring at a stirring speed of 1000 rpm. During the polymerization, the internal pressure was maintained at 0.300 MPa by supplying ethylene from time to time. After the polymerization was completed, the reaction mixture (polymer slurry) was extracted from the polymerization reactor, and the catalyst was deactivated with methanol. Thereafter, the reaction mixture was cooled to 50° C. and held for 30 minutes for a cooling treatment. The reaction mixture was then filtered and air-dried to obtain a polyethylene powder. The polymerization activity in the polymerization reactor was 6,800 g per 1 g of catalyst. Scale and extremely coarse powder were removed using a sieve with 425 μm openings, and the physical properties of the polyethylene powder were evaluated. The evaluation results are shown in Table 2.

[0125] [Comparative Example 2] Polyethylene powder was polymerized by the method described below using a 1.5 L stainless steel autoclave polymerization reactor that had been thoroughly purged with nitrogen. First, 800 mL of hexane was charged as a solvent into a polymerization reactor heated to 80°C, and 0.4 mmol of the raw material [a-2] was added. Next, ethylene was added so that the internal pressure became 0.295 MPa, and hydrogen was added so that the internal pressure became 0.300 MPa. Furthermore, 10.0 mg of the catalyst [A] was added. The internal temperature was kept at 80°C, and polymerization was carried out for 60 minutes while stirring at a stirring speed of 1000 rpm. During the polymerization, the internal pressure was maintained at 0.300 MPa by supplying ethylene from time to time. After the polymerization was completed, the reaction mixture (polymer slurry) was extracted from the polymerization reactor, and the catalyst was deactivated with methanol. Thereafter, the reaction mixture was cooled to 50° C. and held for 30 minutes for a cooling treatment. The reaction mixture was then filtered and air-dried to obtain a polyethylene powder. The polymerization activity in the polymerization reactor was 18,100 g per 1 g of catalyst. Scale and extremely coarse powder were removed using a sieve with 425 μm openings, and the physical properties of the polyethylene powder were evaluated. The evaluation results are shown in Table 2.

[0126] [Comparative Example 3] Polyethylene powder was polymerized by the method described below using a 1.5 L stainless steel autoclave polymerization reactor that had been thoroughly purged with nitrogen. First, 800 mL of hexane was charged as a solvent into a polymerization reactor heated to 86°C, and 0.4 mmol of the raw material [a-2] was added. Next, ethylene was added so that the internal pressure became 0.500 MPa. Furthermore, 10.0 mg of the catalyst [A] was added. The internal temperature was kept at 86°C, and polymerization was carried out for 60 minutes while stirring at a stirring speed of 1000 rpm. During the polymerization, the internal pressure was maintained at 0.500 MPa by supplying ethylene from time to time. After the polymerization was completed, the reaction mixture (polymer slurry) was extracted from the polymerization reactor, and the catalyst was deactivated with methanol. Thereafter, the reaction mixture was cooled to 8° C. and held for 30 minutes for cooling treatment. The reaction mixture was then filtered and air-dried to obtain a polyethylene powder. The polyethylene powder was then heated in an oven at 110°C for 30 minutes, and immediately thereafter subjected to a final heat treatment by immersing the polyethylene powder in a dry ice-ethanol bath and exposing it to a temperature of -70°C or lower for 30 minutes. The polymerization activity in the polymerization reactor was 25,900 g per 1 g of catalyst. Scale and extremely coarse powder were removed using a sieve with 425 μm openings, and the physical properties of the polyethylene powder were evaluated. The evaluation results are shown in Table 2.

[0127] [Comparative Example 4] Polyethylene powder was polymerized by the method described below using a 1.5 L stainless steel autoclave polymerization reactor that had been thoroughly purged with nitrogen. First, 800 mL of hexane was charged as a solvent into a polymerization reactor heated to 86°C, and 0.4 mmol of the raw material [a-2] was added. Next, ethylene was added so that the internal pressure became 0.219 MPa, and hydrogen was added so that the internal pressure became 0.500 MPa. Furthermore, 10.0 mg of the catalyst [A] was added. The internal temperature was kept at 86°C, and polymerization was carried out for 60 minutes while stirring at a stirring speed of 1000 rpm. During the polymerization, the internal pressure was maintained at 0.500 MPa by supplying ethylene from time to time. After the polymerization was completed, the reaction mixture (polymer slurry) was extracted from the polymerization reactor, and the catalyst was deactivated with methanol. Thereafter, the reaction mixture was cooled to 8° C. and held for 30 minutes for cooling treatment. The reaction mixture was then filtered and air-dried to obtain a polyethylene powder. The polyethylene powder was then heated in an oven at 110°C for 30 minutes, and immediately thereafter subjected to a final heat treatment by immersing the polyethylene powder in a dry ice-ethanol bath and exposing it to a temperature of -70°C or lower for 30 minutes. The polymerization activity in the polymerization reactor was 16,700 g per 1 g of catalyst. Scale and extremely coarse powder were removed using a sieve with 425 μm openings, and the physical properties of the polyethylene powder were evaluated. The evaluation results are shown in Table 2.

[0128] [Comparative Example 5] Polyethylene powder was polymerized by the method described below using a 1.5 L stainless steel autoclave polymerization reactor that had been thoroughly purged with nitrogen. First, 800 mL of hexane was charged as a solvent into a polymerization reactor heated to 80°C, and 0.4 mmol of the raw material [a-2] was added. Next, ethylene was added so that the internal pressure became 0.285 MPa, and hydrogen was added so that the internal pressure became 0.300 MPa. Furthermore, 10.0 mg of the catalyst [B] was added. The internal temperature was kept at 80°C, and polymerization was carried out for 60 minutes while stirring at a stirring speed of 1000 rpm. During the polymerization, the internal pressure was maintained at 0.300 MPa by supplying ethylene from time to time. After the polymerization was completed, the reaction mixture (polymer slurry) was extracted from the polymerization reactor, and the catalyst was deactivated with methanol. Thereafter, the reaction mixture was cooled to 50° C. and held for 30 minutes for a cooling treatment. The reaction mixture was then filtered and air-dried to obtain a polyethylene powder. The polymerization activity in the polymerization reactor was 10,300 g per 1 g of catalyst. Scale and extremely coarse particles were removed using a sieve with 425 μm openings, and calcium stearate and potassium stearate were added at 1,000 ppm each before the physical properties of the polyethylene powder were evaluated. The evaluation results are shown in Table 2.

[0129] [Comparative Example 6] The following solvent, raw materials, and catalyst were fed into a vessel-type 300L polymerization reactor equipped with a stirrer. The polymerization temperature was kept at 75°C by jacket cooling. Normal hexane was fed as a solvent at 60L / h. Catalyst [C] was fed so that the production rate was 10kg / h. Liquid component [F] was fed at 6mmol / h as the total amount of Mg and Al. Hydrogen was fed into the feed pipe of catalyst [C] at 2NL / h. Hydrogenation catalyst [G] was separately fed into this feed pipe so that the concentration in the reactor was 0.3μmol / L. Ethylene was fed and continuous polymerization was carried out under the conditions of polymerization temperature 75°C, polymerization pressure 0.8MPa, and average residence time 2.2 hours. The polymerization slurry in the polymerization reactor was led to a flash tank at a pressure of 0.05MPaG and a temperature of 60°C so that the level in the polymerization reactor was kept constant, and unreacted ethylene and hydrogen were separated. The slurry of the ultra-high molecular weight ethylene polymer thus obtained was continuously sent from the flash tank to a centrifuge by a pump to separate the polymer and the solvent, and the separated powder of the ultra-high molecular weight ethylene polymer was sent to a dryer controlled at 80°C and dried while blowing nitrogen. The polymerization activity in the polymerization reactor was 13,000 g per 1 g of catalyst. Scale and extremely coarse powder were removed using a sieve with 425 μm openings, and the physical properties of the polyethylene powder were evaluated. The evaluation results are shown in Table 2.

[0130] [Table 1]

[0131] [Table 2] [Industrial Applicability]

[0132] INDUSTRIAL APPLICABILITY The polyethylene powder of the present invention can provide molded articles such as microporous membranes which have an excellent balance between mechanical strength and heat shrinkage rate and further have an excellent balance between mechanical strength and heat shrinkage rate even when molded at high speed, and has industrial applicability.

Claims

1. The intrinsic viscosity IV measured in accordance with ISO 1628-3 (2010) is 1.5 dL / g or more and 15.0 dL / g or less, The thickness of the amorphous portion is 5.3 nm or more and 12.0 nm or less, A polyethylene powder having a crystallite size of 13.9 nm or more and 18.0 nm or less, as determined by reflection X-ray diffraction method.

2. 2. The polyethylene powder according to claim 1, wherein a ratio of monoclinic (010 plane) to orthorhombic (110 plane) obtained by reflection X-ray diffraction method is from 1.0 to 2.6 inclusive, expressed as monoclinic (010) plane diffraction peak intensity / orthorhombic (110) plane diffraction peak intensity.

3. 3. The polyethylene powder according to claim 1 or 2, having a Ti content of 10 ppm or less and an Al content of 20 ppm or less.

4. Average particle size D determined by sieving method 50 The polyethylene powder according to claim 1 or 2, wherein the average particle diameter is 80 μm or more.

5. The polyethylene powder according to claim 1 or 2, having an α-olefin content of less than 0.03 mol%.

6. A molded body comprising the polyethylene powder according to claim 1 or 2.

7. A separator for a secondary battery, comprising the molded article according to claim 6 .

Citation Information

Patent Citations

  • Ultra-high molecular weight polyethylene powder

    JP6868355B2

  • Polyethylene powder and shaped object thereof

    WO2021153520A1

  • Polyethylene powder and molded body of same

    WO2021241411A1