Expandable methyl methacrylate resin particle, methyl methacrylate resin foam particle, methyl methacrylate foam molded body, and evaporative pattern
The use of methyl methacrylate and butyl acrylate-based resin particles with controlled properties addresses surface beauty and combustibility issues, enhancing productivity and quality in molded articles.
Patent Information
- Application Number
- JP2024030490
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-02-29
- Publication Date
- 2024-10-15
AI Technical Summary
Conventional expandable methyl methacrylate resin particles suffer from issues related to surface beauty and combustibility, with low foaming stability leading to poor productivity and quality in molded articles.
The development of expandable methyl methacrylate resin particles containing methyl methacrylate and butyl acrylate units, a plasticizer, and a blowing agent, with specific particle size and molecular weight ranges, and absence of aromatic compounds, to enhance foaming stability and surface beauty.
The solution provides expanded particles with improved productivity, surface beauty, and combustibility, ensuring uniform foaming and reduced residue during metal casting.
Smart Images

Figure 2024146783000001
Abstract
Description
[Technical field]
[0001] The present invention relates to expandable methyl methacrylate resin particles, expanded methyl methacrylate resin particles, an expandable methyl methacrylate resin molded article, and a lost model. [Background technology]
[0002] When performing metal casting, a foam molded model is embedded in casting sand, and molten metal is poured into the mold to replace it, forming a casting called the lost foam casting method (full mold method). In the full mold method, a foam molded methyl methacrylate polymer is used to reduce residues during casting.
[0003] As examples of expandable methyl methacrylate-based resin particles for producing foamed molded articles of methyl methacrylate polymers, Patent Documents 1 and 2 disclose expandable methyl methacrylate-based resins having an average particle size of 0.5 mm that use methyl methacrylate and acrylic esters. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Publication No. 2015-183111 [Patent Document 2] Japanese Patent Publication No. 2000-086804 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the above-mentioned conventional techniques have room for improvement from the viewpoints of surface aesthetics and flammability of methyl methacrylate resin foam molded articles.
[0006] One aspect of the present invention is to provide expandable methyl methacrylate resin particles which can provide expanded beads with excellent productivity and can provide methyl methacrylate resin foamed molded articles with excellent surface beauty and combustibility. [Means for solving the problem]
[0007] The present inventors have conducted extensive research to solve the above problems, and have completed the present invention. That is, one embodiment of the present invention includes the following configuration.
[0008] The expandable methyl methacrylate resin particles according to one embodiment of the present invention are expandable methyl methacrylate resin particles comprising a base resin containing methyl methacrylate units and butyl acrylate units as constituent units, a plasticizer, and a foaming agent, the expandable methyl methacrylate resin particles do not contain aromatic compounds and have a volume average particle diameter of 0.30 mm to 0.60 mm, and when the expandable methyl methacrylate resin particles are expanded under a condition of an internal pressure of an expansion machine of 0.025 MPa to 0.030 MPa (gauge pressure), the heating time (A) until the expandable methyl methacrylate resin particles become methyl methacrylate resin expanded particles having a bulk ratio of 50 times is less than 100 seconds, and when 100 cc of the methyl methacrylate resin expanded particles having a bulk ratio of 50 times is heated with steam at 100°C, the time (B) during which the volume is maintained at 150 cc or more is 5.0 minutes or more.
[0009] Further, expandable methyl methacrylate-based resin particles according to another embodiment of the present invention are expandable methyl methacrylate-based resin particles comprising a base resin containing methyl methacrylate units and butyl acrylate units as constituent units, a plasticizer, and a foaming agent, wherein the base resin has a weight average molecular weight of 300,000 to 400,000, the expandable methyl methacrylate-based resin particles do not contain an aromatic compound and have a volume average particle diameter of 0.30 mm to 0.60 mm, the plasticizer contains cyclohexane, and the total amount of the butyl acrylate units and the cyclohexane is 6.0 parts by weight or more and 7.5 parts by weight or less relative to 100 parts by weight of the total amount of the methyl methacrylate units and the butyl acrylate units. Effect of the Invention
[0010] According to one aspect of the present invention, it is possible to provide expandable methyl methacrylate-based resin particles which can provide expanded beads with excellent productivity and methyl methacrylate-based resin foamed molded articles with excellent surface beauty and combustibility. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] An embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to each configuration described below, and various modifications are possible within the scope of the claims. In addition, embodiments or examples obtained by combining the technical means disclosed in different embodiments or examples are also included in the technical scope of the present invention. Furthermore, new technical features can be formed by combining the technical means disclosed in each embodiment. All academic documents and patent documents described in this specification are incorporated herein by reference. In addition, unless otherwise specified in this specification, "A to B" representing a numerical range means "A or more (including A and greater than A) and B or less (including B and smaller than B)".
[0012] In this specification, "expandable methyl methacrylate resin particles" may be referred to as "expandable resin particles," "expanded methyl methacrylate resin particles" may be referred to as "expanded particles," and "expanded methyl methacrylate resin molded body" may be referred to as "expanded molded body." In addition, in the pre-expanding step and the molding step, "heating with water vapor" may be referred to as "heating."
[0013] 1. Technical Concept of One Embodiment of the Present Invention The foamed molded article obtained by using the expandable resin particles disclosed in Patent Documents 1 and 2 has room for improvement from various viewpoints. For example, the expandable resin particles described in Patent Document 1 have a low weight average molecular weight, so that the foaming stability during molding is low, and it is difficult to obtain good surface beauty in a molded article of a complex shape. In addition, the expandable resin particles described in Patent Document 2 use methyl acrylate, so that the foaming speed of the expanded particles is slow, so that the productivity tends to be poor. Furthermore, the expandable resin particles described in Patent Document 2 contain aromatic compounds, so that residues are generated during combustion (in other words, black smoke is generated during combustion), which may adversely affect the quality of the casting. That is, the expandable resin particles described in Patent Document 2 tend to have poor combustibility.
[0014] As a result of intensive research, the present inventors have independently found the following, and have completed the present invention: (i) methyl methacrylate-based resin expanded beads obtained by expanding expandable methyl methacrylate-based resin particles having a relatively small volume average particle diameter of 0.30 mm to 0.60 mm have excellent filling properties into molds of various shapes (for example, narrow areas having a width of about several mm) to produce molded articles (expanded molded articles); (ii) methyl methacrylate-based resin expanded beads obtained by expanding expandable methyl methacrylate-based resin particles having a relatively small volume average particle diameter of 0.30 mm to 0.60 mm have excellent expansion stability (ability to maintain high expansion ratio for a long period of time when heated) and have improved surface beauty of the methyl methacrylate-based resin expanded molded articles obtained by expanding the methyl methacrylate-based resin particles having a relatively small volume average particle diameter of 0.30 mm to 0.60 mm during in-mold molding using the methyl methacrylate-based resin expanded beads, since the surface of the methyl methacrylate-based resin expanded molded article or the expanded beads during molding is stretched.
[0015] In particular, the relationship between the expansion stability of the expanded beads (the time during which the expanded beads continue to maintain a high expansion ratio when heated) and the molding condition range (range of heating conditions) during the production of a molded product is a new finding discovered by the present inventors. When the expanded beads are heated, the expansion ratio of the expanded beads changes depending on the heating time. Specifically, the expansion ratio of the expanded beads gradually increases when heating is started, but when heating is continued for a certain period of time, the expanded beads have the property of gradually decreasing the expansion ratio due to shrinkage at a certain point. The present inventors have focused on the heating time and expansion ratio of the expanded beads and, as a result of intensive investigation, have found that if the expanded beads continue to maintain a high expansion ratio for a predetermined period of time or more even when heated, the molding condition range during the production of a molded product can be widened. For example, when the expanded beads are expanded by steam pressure, the surface beauty of the expanded beads changes depending on the height of the steam pressure. The inventors have focused on high vapor pressure and surface beauty and, as a result of extensive research, have found that the resin particles of the present invention are resistant to heat damage and have good surface beauty even when the expanded particles are expanded at a vapor pressure higher than conventionally used (i.e., when the range of molding conditions during production of the molded product is widened).
[0016] When the filling property of the methyl methacrylate resin foamed particles is poor, when the methyl methacrylate resin foamed particles are filled in a mold, a region where the filling density of the foamed particles is high and a region where the filling density of the foamed particles is low are formed in the mold. When molding is performed in such a state, in the region where the filling density of the foamed particles is low, the foamed particles need to be expanded larger to fill the gaps between the foamed particles compared to the region where the filling density of the foamed particles is high. In other words, the degree of expansion of the foamed particles (in other words, the size of the foamed particles constituting the methyl methacrylate resin foamed molded body) is different between the region where the filling density of the foamed particles is low and the region where the filling density of the foamed particles is high. Therefore, when the filling property of the methyl methacrylate resin foamed particles is poor, the surface beauty of the obtained methyl methacrylate resin foamed molded body is reduced. Therefore, the "filling property of the methyl methacrylate resin foamed particles" can be one of the indicators for evaluating the surface beauty of the methyl methacrylate resin foamed molded body, as described in the examples described later.
[0017] In addition, generally, steam is supplied from the chamber to the inside of the mold (the molding space in which the molded body is formed) through a plurality of steam holes provided in the mold. Therefore, the amount of steam supplied to each expanded particle filled in the mold during molding is not uniform, and heating unevenness tends to occur. For example, expanded particles near the mold in the molding space are likely to come into contact with heated steam. On the other hand, expanded particles far from the mold in the molding space are unlikely to come into contact with heated steam. If the expansion stability of the expanded particles of the expandable methyl methacrylate resin particles is low, the range between the amount of heat that the expanded particles can exert to fill the gaps between the expanded particles when the expanded particles filled in the mold are heated to produce a molded body, and the amount of heat that causes wrinkles and / or deformation in the expanded particles due to dissolution of the expanded particles due to overheating becomes narrow. Therefore, the appearance of the expanded molded body will be different between the places (parts) that are likely to come into contact with heated steam in the mold (molding mold) and the places (parts) that are unlikely to come into contact with heated steam. For example, in a place (part) that is difficult to contact with heated steam, the foaming power of the foamed particles is insufficient due to insufficient heat, and the gaps between the foamed particles are not filled, resulting in large gaps on the surface of the molded body. On the other hand, in a place (part) that is easy to contact with heated steam, the foamed particles melt due to excessive heat, causing wrinkles and deformation of the foamed particles. If the heating temperature is increased or the heating time is extended in order to provide sufficient heat to a place that is difficult to contact with heated steam, the heat will be excessive in places other than the place, causing wrinkles and / or deformation of the foamed particles. In addition, if the heating temperature is lowered or the heating time is shortened in order to reduce the heat provided to a place (part) that is easy to contact with heated steam, the foaming power of the places other than the place (part) will be insufficient. As a result, the gaps on the surface of the molded body become noticeable in places other than the place (part), and the surface beauty of the methyl methacrylate resin foamed molded body will be reduced. When the expanded beads obtained by expanding expandable methyl methacrylate resin particles have high expansion stability, when the expanded beads filled in a molding die are heated to produce a molded body, the range between the amount of heat that allows the expanded beads to exert the expansion force required to fill the gaps between the expanded beads and the amount of heat that will cause the expanded beads to wrinkle and / or deform due to overheating is wide.Therefore, even in molding in a mold having a shape that is prone to uneven heating, it is easy to find heating conditions that prevent wrinkles and / or deformation of the expanded beads over the entire surface of the molded article and prevent gaps from forming between the expanded beads. Therefore, the "expansion stability of the methyl methacrylate resin expanded beads" can be one of the indexes for evaluating the surface beauty of the methyl methacrylate resin foam molded article, as described in the examples below.
[0018] When the volume average particle diameter of the expandable methyl methacrylate resin particles is large, the particle diameter of the methyl methacrylate resin expanded particles derived from the expandable methyl methacrylate resin particles is large. When the methyl methacrylate resin expanded particles are filled into a mold, a region in which the methyl methacrylate resin expanded particles cannot be filled, that is, a region where the expanded particles have a high packing density and a region where the expanded particles have a low packing density, is formed in the mold. When molding is performed in this state, in the region where the expanded particles have a low packing density, the expanded particles need to be expanded larger to fill the gaps compared to the region where the expanded particles have a high packing density. In other words, the degree of expansion of the expanded particles (in other words, the size of the expanded particles constituting the methyl methacrylate resin expanded molded body) is different between the region where the expanded particles have a low packing density and the region where the expanded particles have a high packing density. Therefore, when the volume average particle diameter of the expandable methyl methacrylate resin particles is large, the surface beauty of the obtained methyl methacrylate resin expanded molded body is reduced. Therefore, the "volume average particle diameter of the expandable methyl methacrylate resin particles" can be one of the indexes for evaluating the surface beauty of a methyl methacrylate resin foam molded article, as described in the Examples below.
[0019] [2. Expandable methyl methacrylate resin particles] The expandable methyl methacrylate-based resin particles according to one embodiment of the present invention are expandable methyl methacrylate-based resin particles that do not contain an aromatic compound and contain a base resin that contains methyl methacrylate units and butyl acrylate units as constituent units, a plasticizer, and a foaming agent, and the expandable methyl methacrylate-based resin particles have a volume average particle diameter of 0.30 mm to 0.60 mm, and the expandable methyl methacrylate-based resin particles are expanded to a bulk ratio of 50 times (cm) at an internal pressure of a foaming machine of 0.025 MPa to 0.030 MPa (gauge pressure). 3 The expandable methyl methacrylate resin particles are characterized in that the heating time (A) when the particles are expanded with steam to a bulk volume of 100 cc or more (1 / g) is less than 100 seconds, and when 100 cc of the methyl methacrylate resin expanded particles having a bulk volume of 50 are heated with steam at 100° C., the time (B) during which the volume is maintained at 150 cc or more is 5.0 minutes or more. The "expandable methyl methacrylate resin particles according to one embodiment of the present invention" may hereinafter be referred to as "the present expandable resin particles".
[0020] The present expandable resin particles can be expanded by a known method to provide expanded beads, and the present expandable resin particles can be molded in a mold by a known method to provide a foamed molded article.
[0021] The present expandable resin particles have the above-mentioned structure, and therefore have the advantages of being excellent in productivity of the expanded particles and being able to efficiently provide foamed molded articles having excellent combustibility and surface beauty.
[0022] The present expandable resin particles have a time (A) of less than 100 seconds. The time (A) can be said to be the time (heating time) required for the expandable resin particles to provide expanded particles with a bulk ratio of 50 times. The shorter the time (A), the faster the expansion speed of the expandable resin particles, that is, the better the expandability. Expandable resin particles with excellent expandability can reduce the production time and production costs when using the expandable resin particles to produce expanded particles. Therefore, the present expandable resin particles have the advantage of being able to efficiently provide expanded particles, and as a result, being able to efficiently provide foamed molded articles.
[0023] The expandable resin particles have a time (B) of 5.0 minutes or more. As described above, the expansion ratio of the expanded beads gradually increases when heating is started, but when heating is continued for a certain time, the expanded beads shrink at a certain point, and the expansion ratio gradually decreases. The time (B) indicates the time during which the expanded beads maintain a certain volume or more when heated (in other words, maintain a certain expansion ratio or more), and affects the expansion stability of the expanded beads, that is, the surface beauty of the molded body. The longer the time (B), the higher the expansion stability of the expanded beads. By using expanded beads with high expansion stability, even when molding a molded body of a complex shape that is prone to uneven heating, the increase in the gaps between the expanded beads due to insufficient expansion and / or dissolution (wrinkles and / or deformation) due to overheating are unlikely to occur. As a result, the expanded beads that constitute the surface of the molded body have a uniform shape overall, and a molded body with excellent surface beauty can be provided.
[0024] (2-1. Base resin) The base resin contained in the expandable resin particles is composed of a monomer containing a structural unit derived from a methyl methacrylate unit and a butyl acrylate unit. In this specification, a "methyl methacrylate unit" is a structural unit derived from a methyl methacrylate monomer, and a "butyl acrylate unit" is a structural unit derived from a butyl acrylate monomer. In this specification, the notation "monomer" may be omitted. Therefore, in this specification, for example, when simply describing "methyl methacrylate" and "butyl acrylate", it is intended to mean "methyl methacrylate monomer" and "butyl acrylate monomer", respectively.
[0025] The expandable resin particles of the present invention do not contain aromatic compounds as constituents. If aromatic compounds are contained in the constituents, residues are generated during combustion, which adversely affects casting quality. Examples of aromatic compounds include monomers such as styrene and α-methylstyrene, and plasticizers such as toluene and xylene. In this specification, "the expandable resin particles do not contain aromatic compounds as constituents" also means that the base resin of the expandable resin particles does not contain constituent units derived from aromatic compounds (e.g., styrene and α-methylstyrene) as constituent units.
[0026] The content of methyl methacrylate units in the base resin is not particularly limited. The content of methyl methacrylate units in the base resin is preferably 94.0 parts by weight to 97.0 parts by weight, more preferably 94.5 parts by weight to 96.5 parts by weight, in 100 parts by weight of the base resin. When the content of methyl methacrylate units in the base resin is within the above range, there is an advantage that the flammability is improved.
[0027] The content of butyl acrylate units in the base resin is not particularly limited. The content of butyl acrylate units in the base resin is preferably 3.0 parts by weight to 6.0 parts by weight, more preferably 3.5 parts by weight to 5.0 parts by weight, in 100 parts by weight of the base resin. When the content of butyl acrylate units in the base resin is within the above range, there is an advantage that low-pressure moldability is improved.
[0028] The total content of the methyl methacrylate unit and the butyl acrylate unit in the base resin is not particularly limited. The total content of the methyl methacrylate unit and the butyl acrylate unit in the base resin is preferably 70 parts by weight or more, more preferably 80 parts by weight or more, even more preferably 90 parts by weight or more, and particularly preferably 95 parts by weight or more, in 100 parts by weight of the base resin. The total content of the methyl methacrylate unit and the butyl acrylate unit in the base resin may be 100 parts by weight. In other words, the base resin may be composed only of the methyl methacrylate unit and the butyl acrylate unit. When the total content of the methyl methacrylate unit and the butyl acrylate unit in the base resin is within the above range, it has the advantage of being able to achieve both flammability and low-pressure moldability.
[0029] The present expandable resin particles may contain a structural unit derived from a crosslinking agent (hereinafter also referred to as a crosslinking agent unit). When the present expandable resin particles contain a crosslinking agent unit, the expandable resin particles have the advantages that the expandable resin particles can provide expanded particles having excellent shrinkage suppression properties and have excellent expandability.
[0030] Examples of the crosslinking agent include compounds having two or more functional groups exhibiting radical reactivity. Among compounds having two or more functional groups exhibiting radical reactivity, it is preferable to use a bifunctional monomer having two functional groups as the crosslinking agent. In other words, it is preferable that the present expandable resin particles contain a bifunctional monomer unit, which is a structural unit derived from a bifunctional monomer, as a crosslinking agent unit. This configuration has the advantages that (a) the expandable resin particles have excellent expandability, (b) the expanded particles obtained by expanding the expandable resin particles have excellent shrinkage suppression properties, and (c) the expanded molded body obtained by molding the expanded particles in a mold has excellent surface beauty.
[0031] Examples of bifunctional monomers include (a) compounds in which both terminal hydroxyl groups of ethylene glycol are esterified with (meth)acrylic acid, such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, and triethylene glycol di(meth)acrylate, and / or compounds in which both terminal hydroxyl groups of the ethylene glycol oligomer are esterified with (meth)acrylic acid, (b) compounds in which the hydroxyl groups of dihydric alcohols, such as neopentyl glycol di(meth)acrylate, hexanediol di(meth)acrylate (e.g., 1,6-hexanediol diacrylate, etc.), and butanediol di(meth)acrylate, are esterified with acrylic acid or methacrylic acid, and (c) aryl compounds having two alkenyl groups, such as divinylbenzene. Hexanediol di(meth)acrylate is easy to adjust the molecular weight of the base resin. Therefore, hexanediol di(meth)acrylate, such as 1,6-hexanediol diacrylate, is preferred as the bifunctional monomer. As used herein, "(meth)acrylate" refers to methacrylate and / or acrylate, and "(meth)acrylic acid" refers to methacrylic acid and / or acrylic acid.
[0032] In the expandable resin particles, the content of the crosslinking agent unit relative to 100 parts by weight of the base resin is 0.00 parts by weight or more and less than 0.20 parts by weight, preferably 0.00 to 0.19 parts by weight, more preferably 0.00 to 0.17 parts by weight or less, even more preferably 0.00 to 0.15 parts by weight or less, and particularly preferably 0.00 to 0.13 parts by weight. According to the above-mentioned configuration, (a) the expandable resin particles have excellent expandability, (b) the expanded particles obtained by expanding the expandable resin particles have excellent shrinkage suppression properties, and (c) the expanded molded article obtained by molding the expanded particles in a mold has excellent surface beauty.
[0033] (2-2. Foaming Agent) The type of the blowing agent contained in the expandable resin particles is not particularly limited. Examples of the blowing agent include (a) aliphatic hydrocarbons, such as propane, isobutane, normal butane, isopentane, normal pentane, and neopentane, which are hydrocarbons having 3 to 5 carbon atoms, and (b) volatile blowing agents, such as hydrofluorocarbons with an ozone depletion potential of zero, such as difluoroethane and tetrafluoroethane. These blowing agents may be used alone or in combination of two or more.
[0034] In the present expandable resin particles, the content of the blowing agent relative to 100 parts by weight of the base resin is preferably 5 parts by weight to 12 parts by weight, more preferably 7 parts by weight to 10 parts by weight. This configuration has the advantage that expandable resin particles having sufficient expandability can be provided and heavy polymerization equipment is not required.
[0035] (2-3. Other additives) The expandable resin particles may contain, in addition to the base resin and the blowing agent, other additives, such as plasticizers, cell regulators, flame retardants, flame retardant auxiliaries, heat radiation inhibitors, pigments, dyes, and antistatic agents.
[0036] The plasticizer is preferably one having a boiling point of 50°C or more, and one not containing an aromatic ring is selected. Examples of the plasticizer include (a) aliphatic hydrocarbons having 6 or more carbon atoms (C6 or more), such as hexane and heptane, and (b) alicyclic hydrocarbons having 6 or more carbon atoms, such as cyclohexane and cyclooctane. Toluene containing aromatics, even if it has a boiling point of 50°C or more, is not selected as a plasticizer. As a plasticizer having a boiling point of 50°C or more, cyclohexane is preferred in terms of obtaining expandability. That is, the present expandable resin particles preferably contain cyclohexane as a plasticizer.
[0037] The content of the plasticizer in the expandable resin particles is not particularly limited. The content of the plasticizer in the expandable resin particles is preferably 1.5 to 5.0 parts by weight, more preferably 2.0 to 4.5 parts by weight, and even more preferably 2.5 to 4.0 parts by weight, relative to 100 parts by weight of the base resin. When the content of the plasticizer in the expandable resin particles is within the above range, the expanded particles have an advantage of having good expansion stability.
[0038] In addition, the total amount of butyl acrylate and plasticizer in the present expandable resin particles is preferably 6.0 to 7.5 parts by weight per 100 parts by weight of the total of methyl methacrylate and butyl acrylate. When cyclohexane is included as a plasticizer, the total amount of butyl acrylate and cyclohexane is preferably 6.0 to 7.5 parts by weight, more preferably 6.0 to 7.0 parts by weight per 100 parts by weight of the total of methyl methacrylate and butyl acrylate. If the total amount of butyl acrylate and plasticizer and / or the total amount of butyl acrylate and cyclohexane is within the above-mentioned range, the expandable resin particles have sufficient expandability and are also excellent in expansion stability of the expanded particles.
[0039] Examples of the cell regulator include (a) aliphatic bisamides such as methylene bis-stearic acid amide and ethylene bis-stearic acid amide, and (b) polyethylene wax, etc. In the present expandable resin particles, the content of the cell regulator relative to 100 parts by weight of the base resin is preferably 0.01 parts by weight to 0.50 parts by weight.
[0040] (2-4. Physical Properties of Expandable Methyl Methacrylate Resin Particles) (Volume average particle size) The volume average particle diameter of the expandable resin particles is 0.30 mm to 0.60 mm, preferably 0.45 mm to 0.50 mm. When the volume average particle diameter of the expandable resin particles is less than 0.30 mm, the expandable resin particles tend to cause a decrease in expandability during expansion and / or an increase in the amount of blocking during expansion. When the volume average particle diameter of the expandable resin particles is greater than 0.60 mm, the expandable resin particles obtained by expanding the expandable resin particles have poor filling properties in a narrow space when the expandable resin particles are filled into a molding machine. The narrow molding space in the molding machine corresponds to a thin part in the obtained foamed molded product. In this specification, the volume average particle diameter of the expandable resin particles is the particle diameter at which the volume cumulative 50% (i.e., D50) is obtained by measuring the particle diameter of the expandable resin particles on a volume basis using a particle size analyzer (for example, an image processing type Millitrac JPA particle size analyzer), and the obtained results are displayed as a cumulative distribution.
[0041] The volume average particle diameter of the expandable resin particles can be adjusted by changing (a) the initial amounts of dispersant (e.g., calcium phosphate tribasic) and surfactant (e.g., sodium α-olefin sulfonate), (b) the amount of dispersant (e.g., calcium phosphate tribasic) added during the polymerization, and (c) the timing of adding the dispersant during the polymerization (e.g., the time from the start of polymerization to the addition of the dispersant), etc.
[0042] (Expandable methyl methacrylate resin particles) When the expandable resin particles are expanded under the condition of an internal pressure of 0.025 MPa to 0.030 MPa (gauge pressure) in an expansion machine, the steam heating time (A) until the expandable methyl methacrylate resin particles become expanded methyl methacrylate resin particles having a bulk ratio of 50 times is less than 100 seconds. The heating time (A) is preferably 100 seconds or less, more preferably 70 seconds or less. There is no lower limit for the heating time (A), but the heating time (A) is at least more than 0 seconds. When the heating time (A) is less than 100, the expandable resin particles can be said to have excellent expandability.
[0043] Here, the method for measuring the time (A) (expansion rate) of the expandable resin particles is not particularly limited, and examples thereof include a method in which the following steps (1) to (4) are carried out in order: (1) the expandable resin particles are placed in a pressurized expansion machine (e.g., BHP manufactured by Daikai Kogyo Co., Ltd.); (2) steam (e.g., water vapor) is blown into the expansion machine under conditions of an internal pressure of the expansion machine of 0.025 MPa to 0.030 MPa (gauge pressure) to heat the expandable resin particles; (3) the expanded particles obtained by expanding the expandable resin particles are taken out of the expansion machine at regular intervals, and the bulk ratio of the expanded particles is measured; (4) the time (A) (which may also be referred to as heating time (A)) from blowing steam into the expandable resin particles to obtaining expanded particles with a bulk ratio of 50 times is measured.
[0044] In this specification, the bulk ratio of the expanded beads is a value obtained by carrying out the following steps (1) to (3) in order: (1) Weigh out 10 g of the expanded beads and measure them on a 1000 cm 3 (2) Measure the volume of 10 g of the expanded beads from the graduations on the graduated cylinder; (3) Calculate the bulk ratio of the expanded beads using the following formula; Bulk magnification (cm 3 / g) = Volume of foam particles (cm 3 ) / 10g.
[0045] In this specification, the bulk ratio of the expanded beads can also be called the expansion ratio. The unit of the bulk ratio is actually "cm 3 / g", but for convenience, the unit of bulk magnification is expressed as "times" in this specification.
[0046] (Expandable methyl methacrylate resin particles foaming stability) The expandable resin particles are heated and expanded with steam under the condition of an internal pressure of 0.025 MPa to 0.030 MPa (gauge pressure) in an expansion machine to obtain expanded beads with a bulk ratio of 50 times, and then when 100 cc of the expanded beads are heated with steam at 100°C, the time (B) during which the expanded beads remain at 150 cc or more is 5.0 minutes or more. The time (B) is more preferably 6.0 minutes or more, further preferably 6.5 minutes or more, and particularly preferably 7.0 minutes or more. The upper limit of the time (B) is not limited, but is, for example, 10.0 minutes or less. When the time (B) is 5.0 minutes or more, the expandable resin particles can be said to have excellent expansion stability.
[0047] Here, the method for measuring the time (B) of the expandable resin particles is not particularly limited, but may be, for example, a method described in detail in the Examples below.
[0048] (Weight average molecular weight) The weight-average molecular weight of the base resin contained in the present expandable resin particles is preferably 300,000 to 400,000, and more preferably 330,000 to 380,000. When the weight-average molecular weight of the base resin is 400,000 or less, the expandable resin particles have an advantage of excellent expandability. When the weight-average molecular weight of the base resin is 300,000 or more, the expandable particles have an advantage of small shrinkage, excellent expansion stability, and excellent surface beauty of the molded product.
[0049] In this specification, the weight average molecular weight obtained by measuring by the following method is the weight average molecular weight of the base resin contained in the expandable resin particles: (1) 0.02 g of expandable resin particles is dissolved in 20 ml of tetrahydrofuran (hereinafter sometimes abbreviated as "THF"); (2) After that, the gel component in the obtained solution is filtered; (3) Next, GPC measurement is performed using a gel permeation chromatograph (GPC) with only the THF-soluble component (i.e., the filtrate) as a sample; (4) The weight average molecular weight (Mw) is calculated from the GPC measurement chart obtained by the GPC measurement. Note that TSKgel superHZM-H is used as the GPC column, and THF is used as the mobile phase. The weight average molecular weight (Mw) of the base resin contained in the expandable resin particles is a relative value converted to polystyrene using a calibration curve obtained as a result of GPC measurement performed under the same conditions for polystyrene with a known weight average molecular weight.
[0050] The weight average molecular weight of the base resin can be adjusted by changing the composition (type and amount) of the monomers used in the polymerization (copolymerization) process of the base resin, the type and amount of the chain transfer agent, the polymerization temperature and polymerization time, the type and amount of the initiator, and the type and amount of the crosslinking agent, etc.
[0051] 3. Method for producing expandable methyl methacrylate resin particles The method for producing the expandable methyl methacrylate-based resin particles according to one embodiment of the present invention is not particularly limited. The method for producing the expandable methyl methacrylate-based resin particles according to one embodiment of the present invention includes, for example, a copolymerization step of copolymerizing monomers including a methyl methacrylate monomer and a butyl acrylate monomer, and a blowing agent impregnation step of impregnating the obtained copolymer with a blowing agent.
[0052] The "copolymer" in the method for producing expandable methyl methacrylate-based resin particles of the present invention corresponds to the "base resin" contained in the expandable methyl methacrylate-based resin particles. As a preferred embodiment of the method for producing expandable resin particles of the present invention, for example, the following method can be mentioned.
[0053] (3-1.Copolymerization process) The copolymerization step included in the method for producing expandable methyl methacrylate resin particles of the present invention is, for example, suspension polymerization in which polymerization is carried out in an aqueous suspension.
[0054] In the present invention, the term "aqueous suspension" refers to a state in which resin particles and / or monomer droplets are dispersed in water or an aqueous solution by stirring, etc. A water-soluble surfactant and / or monomer may be dissolved in the aqueous suspension, and water-insoluble dispersants, polymerization initiators, chain transfer agents, crosslinking agents, cell regulators, flame retardants, plasticizers, etc. may also be dispersed therein.
[0055] In the copolymerization step of the present invention, a monomer and a polymerization initiator are added to an aqueous suspension (corresponding to an aqueous medium) containing a poorly water-soluble inorganic salt as a dispersant to initiate the polymerization reaction of the monomer. Examples of dispersants that can be used before the start of the polymerization reaction (hereinafter also referred to as the early stage of polymerization) include poorly water-soluble inorganic salts such as tribasic calcium phosphate, magnesium pyrophosphate, hydroxyapatite, and kaolin. The dispersant may also be used in combination with a water-soluble polymer such as polyvinyl alcohol, methyl cellulose, polyacrylamide, and polyvinylpyrrolidone, and / or an anionic surfactant such as sodium α-olefin sulfonate and sodium dodecylbenzenesulfonate.
[0056] The amount of the poorly water-soluble inorganic salt used in the initial stage of polymerization is preferably 0.15 parts by weight or more and 1.20 parts by weight or less, more preferably 0.20 parts by weight or more and 1.10 parts by weight or less, relative to 100 parts by weight of the monomer. When the amount of the poorly water-soluble inorganic salt used in the initial stage of polymerization is (a) 0.15 parts by weight or more relative to 100 parts by weight of the monomer, it has the advantage that the particle size of the obtained expandable methyl methacrylate resin particles does not become too large, and when it is (b) 1.20 parts by weight or less, it has the advantage that the generation of fine particles is suppressed and the yield of the obtained expandable methyl methacrylate resin particles is increased. When an anionic surfactant and / or a water-soluble polymer is used in combination, the concentration of the anionic surfactant and / or the water-soluble polymer in water is preferably 30 ppm or more and 100 ppm or less.
[0057] In the copolymerization step of the present invention, it is preferable to add 0.08 parts by weight to 0.50 parts by weight of poorly water-soluble inorganic salt relative to 100 parts by weight of monomer at a polymerization conversion rate of 35% to 70%. In the following, the period after the start of polymerization may be referred to as "during polymerization" as opposed to "before the start of polymerization". The poorly water-soluble inorganic salt added during polymerization may function as a dispersant.
[0058] The amount of the poorly water-soluble inorganic salt added during polymerization is preferably 0.08 parts by weight or more and 0.50 parts by weight or less, more preferably 0.10 parts by weight or more and 0.50 parts by weight or less, relative to 100 parts by weight of the monomer. When the amount of the poorly water-soluble inorganic salt added during polymerization is 0.08 parts by weight or more relative to 100 parts by weight of the monomer, the particle size of the obtained expandable methyl methacrylate resin particles does not become too large, and when it is 0.50 parts by weight or less, excessive use of the poorly water-soluble inorganic salt is prevented, and the cost is reduced. In addition, the timing of adding the poorly water-soluble inorganic salt is preferably when the polymerization conversion rate is 35% to 70%, more preferably 40% to 50%. When the poorly water-soluble inorganic salt is added at the above polymerization conversion rate, it has the advantage that expandable resin particles having a desired volume average particle size can be obtained.
[0059] In the copolymerization step of the present invention, it is preferable to carry out the first-stage polymerization reaction using a low-temperature decomposition type initiator when polymerizing at 70° C. to 90° C., and then carry out the second-stage polymerization reaction at a higher temperature (90° C. to 110° C.) than the first-stage polymerization reaction using a high-temperature decomposition type initiator. This configuration can reduce the amount of residual monomers.
[0060] As the polymerization initiator, a radical-generating polymerization initiator generally used in the production of thermoplastic polymers can be used. Representative examples of the radical-generating polymerization initiator include organic peroxides such as benzoyl peroxide, lauroyl peroxide, t-butyl peroxybenzoate, isopropyl-t-butyl peroxycarbonate, butyl perbenzoate, t-butylperoxy-2-ethylhexanoate, t-butyl perpivalate, t-butylperoxyisopropyl carbonate, di-t-butylperoxyhexahydroterephthalate, 1,1-di(t-butylperoxy)3,3,5-trimethylcyclohexane, 1,1-bis(t-amylperoxy)-3,3,5-trimethylcyclohexane, 1,1-di(t-butylperoxy)cyclohexane, t-butylperoxy-2-ethylhexyl monocarbonate, and 1,1-bis(t-butylperoxy)cyclohexane, and azo compounds such as azobisisobutyronitrile and azobisdimethylvaleronitrile. These polymerization initiators may be used alone or in combination of two or more. The amount of the polymerization initiator used, in terms of the total amount of the first and second polymerization steps, is preferably 0.1 to 0.5 parts by weight per 100 parts by weight of the monomer. If the amount is within the above range, expandable methyl methacrylate resin particles having excellent expandability can be obtained.
[0061] In the copolymerization step of the present invention, it is preferable to use a well-known chain transfer agent used in the polymerization of methyl methacrylate resins. Examples of well-known chain transfer agents used in the polymerization of methyl methacrylate resins include (a) monofunctional chain transfer agents such as alkyl mercaptans and thioglycolic acid esters, and (b) polyfunctional chain transfer agents in which the hydroxyl groups of polyhydric alcohols such as ethylene glycol, neopentyl glycol, trimethylolpropane, and sorbitol are esterified with thioglycolic acid or 3-mercaptopropionic acid. Examples of alkyl mercaptans include n-dodecyl mercaptan and t-dodecyl mercaptan.
[0062] The amount of the chain transfer agent used is, for example, preferably 0.100 parts by weight or more and less than 0.500 parts by weight, and more preferably 0.220 parts by weight to 0.265 parts by weight, per 100 parts by weight of the base resin.
[0063] (3-2. Foaming agent impregnation process) Examples of the foaming agent used in the foaming agent impregnation step of the present invention include volatile foaming agents such as aliphatic hydrocarbons, which are hydrocarbons having 3 to 5 carbon atoms, such as propane, isobutane, normal butane, isopentane, normal pentane, and neopentane, and hydrofluorocarbons, such as difluoroethane and tetrafluoroethane, which have an ozone depletion coefficient of zero. In this step, multiple foaming agents and / or plasticizers may be used in combination. The amount of foaming agent used is preferably 5 to 12 parts by weight, more preferably 7 to 10 parts by weight, relative to 100 parts by weight of the base resin. The amount of foaming agent mentioned above ensures sufficient foaming properties, and the resin can be safely produced without aggregation during the impregnation step.
[0064] In addition, when cyclohexane is used as a plasticizer, the timing of addition has almost no effect on the physical properties of the expandable resin particles, so cyclohexane may be added to the aqueous suspension before the start of polymerization, cyclohexane may be added to the aqueous suspension during polymerization, or cyclohexane may be added to the aqueous suspension together with the blowing agent at the timing of impregnation with the blowing agent.
[0065] (3-3. Other processes) The method for producing expandable methyl methacrylate-based resin particles according to one embodiment of the present invention may further include, after (3-2. Foaming agent impregnation step), a step of applying magnesium stearate, which is a fatty acid metal salt, as an anti-blocking agent, and / or castor hydrogenated oil as a fusion promoter to the surfaces of the obtained expandable methyl methacrylate-based resin particles.
[0066] The obtained expandable methyl methacrylate resin particles can be made into expanded particles (also referred to as expanded particles or methyl methacrylate expanded particles in this specification) by a general expansion method. Specifically, the expandable resin particles can be placed in a container equipped with a stirrer and heated with a heat source such as steam to expand to a desired expansion ratio.
[0067] Furthermore, the methyl methacrylate-based expanded beads can be molded into a foamed molded article by a general in-mold molding method. Specifically, the expanded beads are filled into a mold that can be closed but cannot be sealed, and the expanded beads are heat-fused with water vapor to form a foamed molded article.
[0068] The foamed molded article of the methyl methacrylate-based expanded particles of the present invention can be suitably used as a lost model, since even if the foamed molded article is buried in casting sand and molten metal is poured into it to replace it, little residue of the methyl methacrylate-based resin is left behind.
[0069] An embodiment of the present invention includes the following configuration.
[0070] [1] Expandable methyl methacrylate resin particles comprising a base resin containing methyl methacrylate units and butyl acrylate units as constituent units, a plasticizer, and a foaming agent, the expandable methyl methacrylate resin particles do not contain aromatic compounds and have a volume average particle size of 0.30 mm to 0.60 mm, and are characterized in that when the expandable methyl methacrylate resin particles are expanded under a condition of an internal pressure of a foaming machine of 0.025 MPa to 0.030 MPa, the heating time (A) for the expandable methyl methacrylate resin particles to become methyl methacrylate resin expanded particles having a bulk ratio of 50 times is less than 100 seconds, and when 100 cc of the methyl methacrylate resin expanded particles having a bulk ratio of 50 times is heated with steam at 100°C, the time (B) for which the particles remain at 150 cc or more is 5.0 minutes or more.
[0071] [2] The expandable methyl methacrylate resin particles according to [1], wherein the plasticizer contains cyclohexane.
[0072] [3] The expandable methyl methacrylate resin particles according to [1] or [2], wherein the base resin has a weight average molecular weight of 300,000 to 400,000.
[0073] [4] Expandable methyl methacrylate-based resin particles comprising a base resin containing methyl methacrylate units and butyl acrylate units as constituent units, a plasticizer, and a foaming agent, wherein the base resin has a weight-average molecular weight of 300,000 to 400,000, the expandable methyl methacrylate-based resin particles do not contain an aromatic compound and have a volume-average particle diameter of 0.30 mm to 0.60 mm, the plasticizer contains cyclohexane, and the total amount of the butyl acrylate units and the cyclohexane is 6.0 parts by weight or more and 7.5 parts by weight or less per 100 parts by weight of the total amount of the methyl methacrylate units and the butyl acrylate units.
[0074] [5] Expanded methyl methacrylate resin particles obtained by expanding the expandable methyl methacrylate resin particles according to any one of [1] to [4].
[0075] [6] A methyl methacrylate resin foamed molded article obtained by molding the methyl methacrylate resin foamed particles according to [5] in a mold.
[0076] [7] A lost model comprising the methyl methacrylate resin foam molded article according to [6]. EXAMPLES
[0077] An embodiment of the present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these.
[0078] (Weight average molecular weight of base resin) The weight average molecular weight of the base resin was obtained by carrying out the following steps (1) to (4) in order: (1) 0.02 g of expandable resin particles was dissolved in 20 ml of tetrahydrofuran (hereinafter sometimes abbreviated as "THF"); (2) After that, the gel component in the obtained solution was filtered; (3) Next, only the components soluble in THF (i.e., the filtrate) were used as a sample and subjected to GPC measurement using a gel permeation chromatograph (GPC); (4) The weight average molecular weight (Mw) was calculated from the GPC measurement chart obtained by the GPC measurement. The weight average molecular weight (Mw) is a relative value converted into polystyrene.
[0079] (Volume average particle size of expandable methyl methacrylate resin particles) Using an image processing type Millitrac JPA particle size analyzer, the particle size of the expandable methyl methacrylate resin particles was measured at 0.005 mm cut width intervals on a volume basis. The results obtained were displayed as a cumulative distribution, and the particle size at 50% of the cumulative volume was taken as the volume average particle size.
[0080] (Bulk ratio of methyl methacrylate resin foam particles) The bulk ratio of the methyl methacrylate resin expanded beads was obtained by carrying out the following steps (1) to (3) in order: (1) 10 g of the expanded beads were weighed out and measured at 1000 cm 3 (2) The volume of 10 g of the expanded beads was measured from the graduations on the graduated cylinder; (3) The bulk ratio of the expanded beads was calculated by the following formula; Bulk magnification (cm 3 / g) = Volume of foam particles (cm 3 ) / 10g.
[0081] In this specification, the bulk ratio of the expanded beads is also called the expansion ratio. The unit of the bulk ratio is actually cm based on the above formula. 3 / g, but in this specification, for convenience, the unit of bulk magnification is expressed as "times."
[0082] (Expandable methyl methacrylate resin particles) Using the expandable methyl methacrylate resin particles, the following (1) to (3) were carried out in order to obtain methyl methacrylate resin expanded particles with a bulk ratio of 50 times: (1) The expandable methyl methacrylate resin particles were put into a pressurized expansion machine, BHP110, manufactured by Daikai Kogyo Co., Ltd.; (2) Steam was blown into the expansion machine under the conditions of a steam blowing pressure of 0.10 MPa to 0.20 MPa (gauge pressure) and an expansion machine internal pressure of 0.025 MPa to 0.030 MPa (gauge pressure), and the expandable methyl methacrylate resin particles were heated; (3) The expandable methyl methacrylate resin particles were expanded until the bulk ratio reached 50 times by the above (2), and methyl methacrylate resin expanded particles with a bulk ratio of 50 times were obtained. In addition, the heating time (A) until the expandable methyl methacrylate resin particles became methyl methacrylate resin expanded particles with a bulk ratio of 50 times was measured.
[0083] The expandability of the methyl methacrylate resin foam particles was evaluated based on the following indices: ○ (Good): Heating time (A) is less than 100 seconds × (Fail): Heating time (A) is 100 seconds or more.
[0084] (Exposure stability of methyl methacrylate resin foam particles) Using the methyl methacrylate resin expanded particles obtained above (i.e., obtained by the methods (1) to (3) described in the section (Expandability of Expandable Methyl Methacrylate Resin Particles) above), the following (1) to (8) were carried out in order to obtain a methyl methacrylate resin expanded molded product, and the time (B) was measured to evaluate the expansion stability of the methyl methacrylate resin expanded particles: (1) The methyl methacrylate resin expanded particles having a bulk ratio of 50 were left to stand at room temperature (25°C) for 3 days; (2) 100 cc of the expanded particles were placed in a steamer equipped with an outlet; (3) Steam at 100°C was supplied to the steamer, and the expanded particles were heated for a predetermined time (30 seconds, (4) The resulting expanded beads were removed from the steamer, left at room temperature for 60 seconds or more, and then placed in a 200 cc measuring cylinder; (5) The volume (cc) of each expanded bead that had been heated for a specified time was measured using the graduations on the measuring cylinder; (6) The specified time (heating time) and the volume of the expanded beads obtained were plotted and connected with a line to obtain a secondary expansion curve; (7) The time (B) during which the volume was maintained at 150 cc or more was calculated from the secondary expansion curve; (8) The expansion stability of the expanded beads was evaluated based on the following indexes. ○ (Good): Time (B) during which 150cc or more is continuously maintained is 5.0 minutes or more × (Poor): The time (B) during which 150 cc or more was continuously maintained was less than 5.0 minutes.
[0085] (Filling ability of methyl methacrylate resin foam particles) Using the methyl methacrylate resin foamed particles, the following (1) to (4) were carried out in order to obtain a methyl methacrylate resin foamed molded product: (1) The methyl methacrylate resin foamed particles having a bulk ratio of 50 were left at room temperature (25°C) for 3 days; (2) The methyl methacrylate resin foamed particles having a bulk ratio of 50 prepared in (1) were poured into a mold (DAISEN KR-57) for forming a box-shaped foamed molded product having a bottom thickness of 30 mm, a side thickness of 25 mm, and dimensions of 550 mm length x 350 mm width x 120 mm height, through a filling port located opposite the bottom of the foamed molded product. (3) Steam was blown into the mold at a steam blowing pressure of 0.30 MPa to 0.50 MPa (gauge pressure), and molding was performed in the mold by steam heating until the foaming pressure reached 0.100 MPa to 0.180 MPa (gauge pressure) under the condition of a pressure in the mold of 0.050 MPa to 0.080 MPa (gauge pressure), thereby fusing the methyl methacrylate resin foamed particles together; (4) After the foaming pressure reached 0.100 MPa to 0.180 MPa (gauge pressure), the mold was left for 100 seconds, and then the foamed molded body was removed.
[0086] The obtained methyl methacrylate resin foamed molded article was visually inspected for defective filling locations, and the filling property of the methyl methacrylate resin foamed particles was evaluated based on the following index: 〇(Good): No defective filling × (defective): There are some defective filling areas.
[0087] (Surface beauty of methyl methacrylate resin foam moldings) Steam was blown into the mold at a steam blowing pressure of 0.40 MPa (gauge pressure), and molding was carried out under high-pressure conditions where the pressure inside the mold was 0.100 MPa (gauge pressure).
[0088] Next, the surface of the methyl methacrylate resin foam molded article was visually observed, and the surface beauty of the methyl methacrylate resin foam molded article was evaluated based on the following index. The degree of gaps between the methyl methacrylate resin foam particles constituting the methyl methacrylate resin foam molded article (surface elongation of the molded article) was evaluated on each of the bottom and side surfaces of the molded article using a score at 0.25 point intervals between 0.00 points (gaps between particles not filled at all) and 5.00 points (gaps between particles completely filled). The larger the number, the better the surface beauty is intended to be: ○ (Good): The gaps between the foam particles on all surfaces of the molded body are 3.50 points or more, and the filling property is good. × (Poor): The gap between the foam particles on any of the molding surfaces is less than 3.50 points, or the filling property is poor.
[0089] (Flammability of methyl methacrylate resin foam moldings) The methyl methacrylate resin foam molded article was ignited and visually observed, and the flammability of the methyl methacrylate resin foam molded article was evaluated based on the following index. 〇(Good): No black smoke is observed × (Poor): Black smoke is observed.
[0090] Example 1 Hereinafter, the number of parts by weight is based on 100 parts by weight of the total monomers (that is, the total of butyl acrylate or methyl acrylate and methyl methacrylate).
[0091] In a 6L autoclave equipped with a stirrer, 150 parts by weight of water, 0.46 parts by weight of calcium phosphate tribasic as a dispersant (poorly water-soluble inorganic salt) used in the initial stage of polymerization, 0.0075 parts by weight of α-olefinsulfonic acid sodium as a surfactant, 0.08 parts by weight of lauroyl peroxide and 0.1 parts by weight of 1,1-bis(t-butylperoxy)cyclohexane as a polymerization initiator, 0.1 parts by weight of 1,6-hexanediol diacrylate as a crosslinking agent, 0.240 parts by weight of n-dodecyl mercaptan as a chain transfer agent, and 0.026 parts by weight of "Sumisorb 200" (registered trademark, manufactured by Sumika Chemtex Co., Ltd.) as a light stabilizer were added to prepare a mixture containing poorly water-soluble inorganic salts. Then, 95.0 parts by weight of methyl methacrylate and 5.0 parts by weight of butyl acrylate were added as a monomer mixture to the mixture to prepare an aqueous suspension. Next, the temperature of the aqueous suspension was raised to 80°C to start polymerization, i.e., the initiation step was carried out. After 1 hour and 45 minutes had elapsed since the start of polymerization (after the initiation step), 0.12 parts by weight of tribasic calcium phosphate was added as a poorly water-soluble inorganic salt to the reaction mixture (aqueous suspension) to carry out the addition step.
[0092] After another 2 hours and 35 minutes, 1.5 parts by weight of cyclohexane as a plasticizer and 9 parts by weight of normal-rich butane as a blowing agent (the weight ratio of normal butane to isobutane in normal-rich butane (normal butane / isobutane) is 70 / 30) were added to the aqueous suspension. Thereafter, the temperature of the aqueous suspension was raised to 101°C. Next, the temperature of the aqueous suspension was maintained at 101°C for 10 hours to carry out copolymerization and impregnation of the blowing agent into the copolymer (copolymerization step and blowing agent impregnation step). Thereafter, the aqueous suspension was cooled. After cooling of the aqueous suspension, the obtained product was washed, dehydrated and dried to obtain expandable methyl methacrylate resin particles.
[0093] The obtained expandable methyl methacrylate resin particles were sieved using sieves with mesh sizes of 0.235 mm and 0.700 mm. By this operation, expandable methyl methacrylate resin particles with particle sizes of 0.235 mm to 0.700 mm were collected. Thereafter, 0.05 parts by weight of magnesium stearate, which is a fatty acid metal salt, and 0.05 parts by weight of castor hardened oil, which is a fusion promoter, were applied to the surfaces of the expandable methyl methacrylate resin particles, relative to 100 parts by weight of the expandable methyl methacrylate resin particles.
[0094] According to the above-mentioned method, each measurement item (volume average particle diameter of the expandable methyl methacrylate resin particles and weight average molecular weight of the base resin) was measured, and each evaluation item (expandability of the expandable methyl methacrylate resin particles, expansion stability of the expanded particles, mold filling property, and surface beauty and flammability of the methyl methacrylate resin foam molded body) was evaluated.
[0095] Example 2 The same operation as in Example 1 was carried out to obtain expandable methyl methacrylate-based resin particles, except that the amount of methyl methacrylate used was changed to 94.5 parts by weight and the amount of butyl acrylate was changed to 5.5 parts by weight. Each measurement item was measured in the same manner as in Example 1. Each evaluation item was evaluated in the same manner as in Example 1.
[0096] Example 3 The same operation as in Example 1 was carried out to obtain expandable methyl methacrylate-based resin particles, except that the amount of methyl methacrylate used was changed to 96.5 parts by weight, the amount of butyl acrylate was changed to 3.5 parts by weight, and the amount of cyclohexane was changed to 3.5 parts by weight. Each measurement item was measured in the same manner as in Example 1. Each evaluation item was evaluated in the same manner as in Example 1.
[0097] Example 4 The same operation as in Example 1 was carried out to obtain expandable methyl methacrylate-based resin particles, except that the amount of methyl methacrylate used was changed to 96.5 parts by weight, the amount of butyl acrylate was changed to 3.5 parts by weight, and the amount of cyclohexane was changed to 2.5 parts by weight. Each measurement item was measured in the same manner as in Example 1. Each evaluation item was evaluated in the same manner as in Example 1.
[0098] Comparative Example 1 The same operation as in Example 1 was carried out to obtain expandable methyl methacrylate-based resin particles, except that the amount of methyl methacrylate used was changed to 96.5 parts by weight and the amount of butyl acrylate was changed to 3.5 parts by weight. Each measurement item was measured in the same manner as in Example 1. Each evaluation item was evaluated in the same manner as in Example 1.
[0099] Comparative Example 2 The amount of methyl methacrylate used was changed to 96.5 parts by weight, the amount of butyl acrylate was changed to 3.5 parts by weight, and 1.0 part by weight of toluene was used for 100 parts by weight of the total of methyl methacrylate and butyl acrylate in the initial stage of polymerization. The same operation as in Example 1 was performed to obtain expandable methyl methacrylate-based resin particles. Each measurement item was measured in the same manner as in Example 1. Each evaluation item was evaluated in the same manner as in Example 1.
[0100] Comparative Example 3 The amount of methyl methacrylate used was changed to 97.5 parts by weight, the amount of butyl acrylate was changed to 2.5 parts by weight, and 1.0 part by weight of toluene was used for 100 parts by weight of methyl methacrylate and butyl acrylate in the initial stage of polymerization. The same operation as in Example 1 was performed to obtain expandable methyl methacrylate-based resin particles. Each measurement item was measured in the same manner as in Example 1. Each evaluation item was evaluated in the same manner as in Example 1.
[0101] Comparative Example 4 The same operation as in Example 1 was carried out to obtain expandable methyl methacrylate resin particles, except that the amount of tricalcium phosphate used in the initial polymerization step was changed to 0.18 parts by weight, and the mesh size of the sieve used to sieve the expandable methyl methacrylate resin particles was changed to 500 μm to 1400 μm. Each measurement item was measured in the same manner as in Example 1. Each evaluation item was evaluated in the same manner as in Example 1.
[0102] Comparative Example 5 The same procedure as in Example 1 was carried out to obtain expandable methyl methacrylate resin particles, except that the amount of n-dodecyl mercaptan used was changed to 0.300 parts by weight. Each measurement item was measured in the same manner as in Example 1. Each evaluation item was evaluated in the same manner as in Example 1.
[0103] Comparative Example 6 The same procedure as in Example 1 was carried out to obtain expandable methyl methacrylate resin particles, except that the amount of n-dodecyl mercaptan used was changed to 0.210 parts by weight. Each measurement item was measured in the same manner as in Example 1. Each evaluation item was evaluated in the same manner as in Example 1.
[0104] Comparative Example 7 The same operation as in Example 1 was carried out to obtain expandable methyl methacrylate-based resin particles, except that the amount of methyl methacrylate used was changed to 93.5 parts by weight and the amount of butyl acrylate was changed to 6.5 parts by weight. Each measurement item was measured in the same manner as in Example 1. Each evaluation item was evaluated in the same manner as in Example 1.
[0105] Comparative Example 8 The amount of methyl methacrylate used was changed to 94.5 parts by weight, 5.0 parts by weight of butyl acrylate was changed to 5.5 parts by weight of methyl acrylate, and 1.0 part by weight of toluene was used for 100 parts by weight of methyl methacrylate and butyl acrylate in the initial stage of polymerization. The same operation as in Example 1 was performed to obtain expandable methyl methacrylate-based resin particles. Each measurement item was measured in the same manner as in Example 1. Each evaluation item was evaluated in the same manner as in Example 1.
[0106] [Table 1] [Industrial Applicability]
[0107] According to one aspect of the present invention, it is possible to provide expandable methyl methacrylate resin particles which can provide expanded beads with excellent productivity and can provide a methyl methacrylate resin foamed molded article with excellent surface beauty and combustibility. Therefore, one embodiment of the present invention can be suitably used as a lost pattern when performing metal casting by the full mold method.
Claims
1. Expandable methyl methacrylate-based resin particles comprising a base resin containing methyl methacrylate units and butyl acrylate units as constituent units, a plasticizer, and a foaming agent, The expandable methyl methacrylate resin particles are Contains no aromatic compounds The volume average particle size is 0.30 mm to 0.60 mm, when the expandable methyl methacrylate-based resin particles are expanded under a condition of an internal pressure of 0.025 MPa to 0.030 MPa in an expansion machine, the heating time (A) with steam until the expandable methyl methacrylate-based resin particles become expanded methyl methacrylate-based resin particles having a bulk ratio of 50 times is less than 100 seconds, The expandable methyl methacrylate resin particles are characterized in that when 100 cc of the methyl methacrylate resin expanded particles having a bulk ratio of 50 times are heated with steam at 100°C, the time (B) during which the expanded particles maintain a volume of 150 cc or more is 5.0 minutes or more.
2. The expandable methyl methacrylate resin particles according to claim 1 , wherein the plasticizer comprises cyclohexane.
3. 3. The expandable methyl methacrylate resin particles according to claim 1, wherein the base resin has a weight average molecular weight of 300,000 to 400,000.
4. Expandable methyl methacrylate-based resin particles comprising a base resin containing methyl methacrylate units and butyl acrylate units as constituent units, a plasticizer, and a foaming agent, The weight average molecular weight of the base resin is 300,000 to 400,000; The expandable methyl methacrylate resin particles are Contains no aromatic compounds The volume average particle size is 0.30 mm to 0.60 mm, The plasticizer comprises cyclohexane, The expandable methyl methacrylate-based resin particles are characterized in that the total amount of the butyl acrylate units and the cyclohexane is 6.0 parts by weight or more and 7.5 parts by weight or less per 100 parts by weight of the total amount of the methyl methacrylate units and the butyl acrylate units.
5. 5. A methyl methacrylate resin expanded particle obtained by expanding the expandable methyl methacrylate resin particle according to claim 1.
6. A methyl methacrylate resin foamed article obtained by molding the expanded methyl methacrylate resin particles according to claim 5 in a mold.
7. A lost model comprising the methyl methacrylate resin foam molded article according to claim 6.
Citation Information
Patent Citations
Preparation of foamable, methyl methacrylate resin particle
JP2000086804A
Expandable acrylic resin particle, acrylic resin expanded particle, and acrylic resin expanded particle molding