Photosensitive resin composition, method for producing cured film, substrate with cured film, display device and sensor

The photosensitive resin composition addresses the challenge of achieving low refractive index and fine patterning in cured films, improving visibility and reducing reflectance in display devices and sensors by using specific inorganic fillers and alkali-soluble resins.

JP2024146791APending Publication Date: 2024-10-15NIPPON STEEL CHEM & MATERIAL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024035013
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-07
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Conventional resin compositions fail to achieve both low refractive index and fine patterning performance in cured films, which are essential for improving the visibility of display devices by reducing reflectance.

Method used

A photosensitive resin composition comprising inorganic fillers with a refractive index of 1.20 to 1.46, alkali-soluble resins with a refractive index of 1.50 to 1.70, polymerizable compounds, photoinitiators, and solvents, which can be applied, exposed, and developed to form a cured film with low reflectance and precise patterns.

Benefits of technology

The composition enables the production of cured films with low refractive index and fine patterning capabilities, enhancing the visibility and reducing reflectance in display devices and sensors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146791000001
    Figure 2024146791000001
  • Figure 2024146791000002
    Figure 2024146791000002
  • Figure 2024146791000003
    Figure 2024146791000003
Patent Text Reader

Abstract

To provide a photosensitive resin composition that enables the formation of a cured film with a low refractive index, while allowing for fine patterning.SOLUTION: A photosensitive resin composition includes (A) an inorganic filler with a refractive index of 1.20 or more and 1.46 or less, (B) an alkali-soluble resin, (C) a polymerizable compound with at least one ethylenically unsaturated bond, (D) a photopolymerization initiator, and (E) a solvent, where the component (B) has a refractive index of 1.50 or more and 1.70 or less when made into a cured film with a thickness of 1 μm.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photosensitive resin composition, a method for producing a cured film, a substrate with a cured film, a display device, and a sensor. [Background technology]

[0002] In order to improve the visibility of display devices, touch panels, etc., displays used in these devices are required to have a reduced reflectance. For this reason, a coating film that reduces the reflectance by using a refractive index difference may be provided on a black matrix that is prone to reflecting light.

[0003] A layer with a low refractive index is used as such a coating layer. In order to form a layer with a low refractive index, a resin composition with a refractive index such as silica added thereto is known (Patent Document 1, etc.). In addition, since the coating film may be patterned depending on the application, an alkali-soluble resin may be added to the composition for forming the coating film to enable alkaline development. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2018-072634 A Summary of the Invention [Problem to be solved by the invention]

[0005] There is a demand for a photosensitive resin composition that can produce a cured film with a low refractive index and also allows fine patterning. However, the conventional resin compositions described in Patent Document 1 and the like have been unable to achieve both a low refractive index for the cured film and fine patterning performance.

[0006] The present invention has been made in consideration of the above points, and has an object to provide a photosensitive resin composition that can produce a cured film with a low refractive index and also enables fine patterning, a method for producing a cured film using the same, a substrate with a cured film produced by the method, and a display device and a sensor that have the substrate with the cured film. [Means for solving the problem]

[0007] One aspect for solving the above problems relates to the following photosensitive resin compositions [1] to [3]. [1] (A) Inorganic filler having a refractive index of 1.20 or more and 1.46 or less (B) Alkali-soluble resin (C) a polymerizable compound having at least one ethylenically unsaturated bond, (D) a photoinitiator, and (E) Solvent Including, The component (B) has a refractive index of 1.50 or more and 1.70 or less when made into a cured film having a thickness of 1 μm. Photosensitive resin composition. [2] The content of the component (A) is 10% by mass or more and 70% by mass or less based on the total mass of the solid content of the photosensitive resin composition. The photosensitive resin composition according to [1]. [3] The component (A) is sodium hexafluoroaluminate. The photosensitive resin composition according to [1].

[0008] Another aspect for solving the above problem relates to the method for producing a cured film described below in [4]. [4] A step of applying the photosensitive resin composition according to any one of [1] to [3] onto a substrate; a step of exposing the applied photosensitive resin composition through a photomask, removing the unexposed areas by development, and then baking the composition; The method for producing a cured film comprising the steps of:

[0009] Another aspect for solving the above problem relates to a substrate with a cured film as described below in [5]. [5] A substrate with a cured film, comprising a patterned cured film produced by curing the photosensitive resin composition according to any one of [1] to [3], or by the method for producing a cured film according to [4].

[0010] Another aspect for solving the above problem relates to a display device as described below in [6]. [6] A display device having the substrate with the cured film according to [5].

[0011] Another aspect for solving the above problem relates to a sensor as described below in [7]. [7] A sensor having a substrate with a cured film according to [5]. Effect of the Invention

[0012] According to the present invention, there are provided a photosensitive resin capable of producing a cured film having a low refractive index and also capable of fine patterning, a method for producing a cured film using the same, a substrate with a cured film produced by the method, and a display device and a sensor having the substrate with the cured film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, an embodiment of the present invention will be described, but the present invention is not limited to the following embodiment. In addition, in the present invention, when the first decimal place of the content of each component is 0, the notation after the decimal point may be omitted.

[0014] In this specification, "(meth)acrylic acid" is a general term for acrylic acid and methacrylic acid, and means one or both of them. Furthermore, "(meth)acrylate" is a general term for acrylate and methacrylate, and means one or both of them. Furthermore, "(meth)acryloyl group" is a general term for acryloyl group and methacryloyl group, and means one or both of them.

[0015] 1. Photosensitive resin composition The photosensitive resin composition according to one embodiment of the present invention comprises (A) an inorganic filler, (B) an alkali-soluble resin, (C) a polymerizable compound having at least one ethylenically unsaturated bond, (D) a polymerization initiator, and (E) a solvent. Each component will be described below.

[0016] [Component (A)] The component (A) is an inorganic filler having a refractive index of 1.20 or more and 1.46 or less.

[0017] The refractive index of component (A) can be determined from a transparent mixture obtained by mixing component (A) powder with a standard refractive index liquid of known refractive index. In this case, the refractive index of component (A) is calculated based on the change in the refractive index of the above mixture from that of the standard refractive index liquid. The refractive index of component (A) can also be measured using an Abbe refractometer. The refractive index of component (A) refers to the refractive index for light with a wavelength of 550 nm.

[0018] The type of component (A) is not particularly limited, and examples of the material that can be used include sodium hexafluoroaluminate (cryolite), magnesium fluoride, silica, calcium fluoride, lithium fluoride, etc. As the silica, fumed silica, colloidal silica, organosilica sol, etc. can be used.

[0019] Inorganic fillers having a refractive index within the above range make it difficult for light exposed to the photosensitive resin composition applied to a substrate to disperse in the composition, and tend to allow the light to travel in a straight line, which is believed to suppress deterioration in pattern accuracy due to dispersed light, chipping of pattern edges due to insufficient light reaching the bottom of the composition, and the like.

[0020] The average primary particle size of component (A) is preferably 10 nm or more and 100 nm or less. When the average primary particle size is 10 nm or more, the surface energy is not too high, so that the component (A) is less likely to aggregate within the film, and the aggregated component (A) is less likely to diffuse the exposed light, resulting in a decrease in pattern accuracy. When the average primary particle size is 100 nm or less, the average primary particle size is appropriately small, so that the particle alone is less likely to become a diffusion source, resulting in a decrease in pattern accuracy.

[0021] The average primary particle size of component (A) is a value calculated by observing particle size using a transmission electron microscope, randomly selecting 100 particles, measuring the long and short axis lengths of the particles, and taking the arithmetic mean of these. Note that when component (A) forms agglomerates or aggregates, the primary particles refer to the particles that make up these.

[0022] Any known inorganic filler can be used without particular limitation as long as it is dispersed with an average secondary particle diameter of 1 to 1000 nm (average particle diameter measured with a laser diffraction / scattering particle size distribution meter or a dynamic light scattering particle size distribution meter) for component (A). The more preferred average secondary particle diameter is 10 to 300 nm.

[0023] There are no particular limitations on the method for producing the component (A) (gas phase reaction, liquid phase reaction) or its shape (spherical, non-spherical).

[0024] Furthermore, component (A) may be solid particles, hollow particles, or porous particles. Hollow particles and porous particles tend to reduce the refractive index and improve pattern precision.

[0025] The hollow particles are particles having a cavity inside, and there are no particular limitations on the production method (gas phase reaction, liquid phase reaction) or shape (spherical, non-spherical).

[0026] The porosity of the hollow particles is preferably 5% or more and 80% or less, more preferably 5% or more and 60% or less, even more preferably 20% or more and 60% or less, and most preferably 40% or more and 60% or less. When the porosity is 5% or more, a cured film with a low refractive index can be easily obtained. When the porosity is 20% or more, a cured film with a lower refractive index can be obtained. When the porosity is 40% or more, a cured film with an even lower refractive index can be obtained. When the porosity is within the range of 80% or less, excessive scattering of the exposure light is suppressed, and a cured film with good patterning properties and transmittance can be obtained. When the porosity is within the range of 60% or less, a cured film with better patterning properties and transmittance can be obtained.

[0027] The porosity is the ratio of the hollow part in the particle to the total volume of the particle. The porosity can be determined by using a transmission electron microscope. The hollow part of the hollow particle has a low density, and the contrast of the hollow part is low in the transmission electron microscope photograph, so that the shell and the hollow part of the hollow particle can be confirmed. From the above microscope photograph, first, the longest diameter and the shortest diameter of the hollow particle are measured, and the volume (V1) is calculated assuming that the particle shape is a perfect sphere by taking the average value as the particle diameter of the particle. Next, the longest diameter and the shortest diameter of the hollow part of the particle are measured, and the volume (V2) is calculated assuming that the hollow part shape is a perfect sphere by taking the average value as the diameter of the cavity. The same measurement was performed on 10 random particles. The porosity can be expressed by calculating the ratio of the volume (V2) to the volume (V1) for each of the 10 particles, and then averaging them.

[0028] Among the above-mentioned materials, sodium hexafluoroaluminate (cryolite) and hollow silica are preferred from the viewpoint of further improving the patterning precision, and sodium hexafluoroaluminate (cryolite) is more preferred from the viewpoint of further increasing the patterning precision and decreasing the reflectance. Sodium hexafluoroaluminate has a uniform refractive index inside the particle, which makes it easier to suppress scattering and reflection occurring at the interface between layers with different refractive indexes, making it easier to increase the patterning precision and decrease the reflectance.

[0029] The component (A) may be dispersed with a dispersant. As the dispersant, a known dispersant can be used, or the component (B) (particularly the resin (B)-2) can be used.

[0030] The content of the (A) component is preferably 10% by mass or more and 70% by mass or less, and more preferably 20% by mass or more and 60% by mass or less, based on the total mass of the solid content. When the (A) component is cryolite, magnesium fluoride, or solid silica, it is more preferably 40% by mass or more and 60% by mass or less, and particularly preferably 45% by mass or more and 60% by mass or less. When the (A) component is hollow silica, it is even more preferably 30% by mass or more and 60% by mass or less. By making the (A) component content 10% by mass or more, it is possible to reduce the refractive index of the cured film while also increasing the patterning accuracy. By making the (A) component content 70% by mass or less, it is possible to suppress a decrease in patterning properties due to an excess filler.

[0031] [(B) Component] The (B) component is an alkali-soluble resin. In this embodiment, the refractive index of the alkali-soluble resin used as the (B) component when it is made into a cured film with a thickness of 1 μm is set to 1.50 or more and 1.70 or less. By combining the (A) component with such a (B) component, the refractive index of the cured film can be effectively reduced. The refractive index of the (B) component is preferably 1.50 or more and 1.65 or less, more preferably 1.50 or more and 1.58 or less, even more preferably 1.50 or more and 1.55 or less, and most preferably 1.50 or more and 1.53 or less.

[0032] The refractive index of the component (B) is a value measured by the following method.

[0033] The resin of component (B) was applied to a silicon wafer with a diameter of 125 mm, "5-inch P-type wafer 1-100" (manufactured by Advantec Co., Ltd.) using a spin coater so that the film thickness after post-baking would be 1.0 μm. Pre-baking was performed at 90°C for 1 minute. After that, post-baking was performed in an oven at 230°C for 30 minutes, and the substrate was used to measure the refractive index at 550 nm using a spectroscopic ellipsometry "Alpha-SE" (manufactured by JA Woollam Co., Ltd.). When applying component (B), component (B) may be diluted with a solvent such as propylene glycol monomethyl ether acetate to make it easier to apply, or it may be applied by increasing the rotation speed of the spin coater without diluting it.

[0034] The (B) component may contain a plurality of different resins (for example, resin (B)-1 and resin (B)-2 described below). In this case, the refractive index of the (B) component is measured by forming a coating film as described above in a state where the resins are mixed in the mass ratio contained in the photosensitive resin composition.

[0035] (Resin (B)-1) The component (B) may be a polymerizable unsaturated group-containing alkali-soluble resin (hereinafter simply referred to as "resin (B)-1") that contains 5 to 90 mol % of the structure represented by general formula (1) and 10 to 95 mol % of the structure represented by general formula (2), and is a polymer having a weight average molecular weight of 3000 to 50000 and an acid value of 30 to 200 mg / KOH. The photosensitive resin composition may contain only one type of resin (B)-1 having a single polymerization ratio, or two or more types having different polymerization ratios.

[0036] [ka]

[0037] [ka]

[0038] In the general formulae (1) and (2), R1, R3, and R4 are independently a hydrogen atom or a methyl group. R2 is a hydrogen atom or a monovalent hydrocarbon group having 1 to 20 carbon atoms, and the hydrocarbon group may contain an ether bond, an ester bond, or a urethane bond therein. However, in the structure represented by the general formula (1), R2 is a cyclohexyl group, a dicyclopentanyl group, or a dicyclopentenyl group in 20 mol% or more of the total number of moles of the structure represented by the general formula (1). R5 is a divalent hydrocarbon group having 2 to 10 carbon atoms. p is a number of 0 or 1. X is a hydrogen atom or -OC-L-(COOH) k (wherein L is a divalent or trivalent carboxylic acid residue, and k is a number from 1 to 2.) Note that two or more types of X are contained in one molecule of resin (B)-1.

[0039] Examples of the hydrocarbon group that R2 can be include saturated linear hydrocarbon groups such as methyl, ethyl, propyl, isopropyl, butyl, sec-butyl, isobutyl, tert-butyl, pentyl, isopentyl, neopentyl, tert-pentyl, hexyl, heptyl, octyl, isooctyl, 2-ethylhexyl, decyl, dodecyl, tetradecyl, hexadecyl, octadecyl, and eicosyl groups; unsaturated linear hydrocarbon groups such as vinyl, allyl, and ethynyl groups; cyclopropyl, cyclopentyl, cyclohexyl, 2-methylcyclohexyl, 4-methylcyclohexyl, dicyclopentanyl, and the like. aliphatic hydrocarbon groups such as a cyclic aliphatic hydrocarbon group, a dicyclopentenyl group, a dicyclohexyl group, a norbornyl group, an isobornyl group, an adamantyl group, and a substituent represented by the following general formula (3) (* indicates the bonding portion with the ester moiety in the structure represented by general formula (1)); hydrocarbon groups having an aromatic ring such as a phenyl group, a tolyl group, a mesityl group, a naphthyl group, an anthryl group, a phenanthryl group, a benzyl group, a 2-phenylethyl group, a 2-phenylvinyl group, and a decahydronaphthyl group; aliphatic ethers such as a methoxyethyl group, a 2-(methoxyethoxy)ethyl group, and an isoamyl group; and aliphatic urethanes such as a 2-(ethoxycarbonylamino)ethyl group. However, from the viewpoint of heat resistance, it is preferable that 20 mol% or more of R2 relative to the total number of moles of the structure represented by general formula (1) is a cyclohexyl group, a dicyclopentanyl group, or a dicyclopentenyl group, and 20 mol% or more of R2 relative to the total number of moles of the structure represented by general formula (1) is a dicyclopentanyl group or a dicyclopentenyl group. The structure represented by general formula (1) may include a plurality of structures with different R2.

[0040] [ka]

[0041] Examples of the hydrocarbon group that R5 can take include an ethylene group, a 1,2-propylene group, a 1,4-butylene group, and a 1,6-hexamethylene group. Of these, an ethylene group, a 1,2-propylene group, and a 1,4-butylene group are preferred. The structure represented by the general formula (2) may include a plurality of structures with different R5.

[0042] X is -OC-L-(COOH) k (wherein L represents a divalent or trivalent carboxylic acid residue, and k represents a number from 1 to 2) is formed by reacting a divalent carboxylic acid, a trivalent carboxylic acid, or an acid monoanhydride thereof with a hydroxy group in the copolymer. Examples of the divalent or trivalent carboxylic acid include maleic acid, succinic acid, itaconic acid, phthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, chlorendic acid, and trimellitic acid. Among these, tetrahydrophthalic anhydride, succinic anhydride, and trimellitic anhydride are more preferred.

[0043] The ratio of the structure represented by general formula (1) to the structure represented by general formula (2), when the sum of these is taken as 100 mol%, is preferably 5 mol% to 90 mol% and more preferably 20 mol% to 70 mol%. Also, it is preferable that the structure represented by general formula (2) is 10 mol% to 95 mol% and more preferably 30 mol% to 80 mol%.

[0044] Resin (B)-1 may contain other structures other than the structure represented by general formula (1) and the structure represented by general formula (2). Examples of the other structures include structures derived from unsaturated group-containing carboxylic acids represented by general formula (8) described below, styrene which may have a substituent on the phenyl group, and monomaleimide. Examples of the substituent that styrene may have on the phenyl group include an alkyl group having 1 to 10 carbon atoms. Examples of monomaleimides include N-phenylmaleimide, N-cyclohexylmaleimide, N-laurylmaleimide, and N-(4-hydroxyphenyl)maleimide. Of these, unsubstituted styrene and N-phenylmaleimide are preferred.

[0045] The ratio of the other structures can be from 5 mol % to 50 mol % when all structural units of the resin (B)-1 are taken as 100 mol %.

[0046] Resin (B)-1 can be synthesized by a known method. For example, (meth)acrylic acid esters having the functional group described above as R2 and glycidyl (meth)acrylate are radically copolymerized in a solvent to obtain a copolymer, and then unsaturated group-containing carboxylic acids such as (meth)acrylic acid (including alkylene oxide-modified) are reacted with the glycidyl group in the copolymer, and then dicarboxylic acid compounds, tricarboxylic acid compounds or their acid monoanhydrides are reacted with the hydroxyl group generated by the reaction of the glycidyl group with the unsaturated group-containing carboxylic acid to synthesize resin (B)-1 (hereinafter, the synthesis method described in this paragraph is also referred to as "first synthesis method").

[0047] Examples of (meth)acrylic acid esters having the functional group described above as R2 used in the first synthesis method include cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate (formula (4)), dicyclopentenyl (meth)acrylate (formula (5)), ethylene glycol modified cyclohexyl (meth)acrylate, ethylene glycol modified dicyclopentanyl (meth)acrylate (formula (6)), ethylene glycol modified dicyclopentenyl (meth)acrylate (formula (7)), etc. Two or more of these (meth)acrylic acid esters having a cyclohexyl group, dicyclopentanyl group, or dicyclopentenyl group may be used in combination.

[0048] [ka]

[0049] [ka]

[0050] [ka]

[0051] [ka]

[0052] In addition, R1 in the general formulae (4) to (7) represents a hydrogen atom or a methyl group, similar to R1 in the general formula (1). In addition, the general formulae (6) and (7) exemplify a compound having only one ethylene oxide group in the molecule, but it may have multiple ethylene oxide groups in the molecule, or may have other alkylene oxide groups such as a propylene oxide group. Similarly, the ethylene glycol modified cyclohexyl (meth)acrylate may have only one ethylene oxide group, or may have multiple ethylene oxide groups in the molecule, or may have other alkylene oxide groups such as a propylene oxide group.

[0053] When (meth)acrylic acid esters having the above-mentioned functional group as R2 are radically copolymerized with glycidyl (meth)acrylate, other (meth)acrylic acid esters having a structure represented by general formula (1) may be copolymerized. Examples of the other (meth)acrylic acid esters include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, iso-propyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, neopentyl (meth)acrylate, isoamyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dodecyl (meth)acrylate, cyclopentyl (meth)acrylate, butyl ... Examples of the (meth)acrylic acid esters include (meth)acrylic acid esters having a hydrocarbon group having 1 to 20 carbon atoms, such as cyclohexyl (meth)acrylate, 2-methylcyclohexyl (meth)acrylate, dicyclohexyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, propargyl (meth)acrylate, phenyl (meth)acrylate, naphthyl (meth)acrylate, anthracenyl (meth)acrylate, benzyl (meth)acrylate, phenethyl (meth)acrylate, cresyl (meth)acrylate, triphenylmethyl (meth)acrylate, and cumyl (meth)acrylate. Two or more of these (meth)acrylic acid esters may be used in combination.

[0054] The amount of the other (meth)acrylic esters is adjusted so that the amount of the (meth)acrylic esters having a cyclohexyl group, a dicyclopentanyl group or a dicyclopentenyl group is 20 mol % or more relative to the total of the (meth)acrylic esters having a cyclohexyl group, a dicyclopentanyl group or a dicyclopentenyl group and the other (meth)acrylic esters.

[0055] When resin (B)-1 is synthesized by the first synthesis method, the blending ratio of the (meth)acrylic acid ester having the structure represented by general formula (1) to glycidyl (meth)acrylate may be adjusted so that the blending amount of the (meth)acrylic acid ester having the structure represented by general formula (1) is 5 mol % or more and 90 mol % or less, and the blending amount of glycidyl (meth)acrylate is 10 mol % or more and 95 mol % or less.

[0056] In the radical polymerization, a known radical polymerization initiator such as an azo compound or a peroxide may be used, and the degree of polymerization may be controlled by using a known chain transfer agent or a polymerization inhibitor, etc. The reaction temperature may be appropriately set in consideration of the half-life temperature of the radical polymerization initiator used.

[0057] Next, the glycidyl group in the copolymer obtained by the above copolymerization is reacted with an unsaturated group-containing carboxylic acid such as (meth)acrylic acid to open the ring of the glycidyl group. The amount of the unsaturated group-containing carboxylic acid reacted at this time is preferably 80 mol% or more, more preferably 90 mol% or more, and even more preferably 100 mol% based on the glycidyl group. By increasing the amount of the unsaturated group-containing carboxylic acid used, it is possible to increase the introduction of the unsaturated group and the group corresponding to X in the resin (B)-1, and to improve the photocurability and alkali solubility.

[0058] Examples of the unsaturated group-containing carboxylic acid to be reacted with the glycidyl group include the compound represented by the following formula (8): R4, R5 and p are the same as those explained for general formula (2).

[0059] [ka]

[0060] The divalent hydrocarbon group having 2 to 10 carbon atoms, which is R5, is preferably a divalent alkylene group having 2 to 10 carbon atoms or a divalent alkylarylene group having 2 to 10 carbon atoms. These alkylene groups and alkylarylene groups may be linear, branched, or cyclic. Of these, R5 is preferably an ethylene group, a 1,2-propylene group, or a 1,4-butylene group. The unsaturated group-containing carboxylic acid may be a plurality of compounds having different R5. The unsaturated group-containing carboxylic acid is preferably (meth)acrylic acid, where p=0.

[0061] The addition reaction of the unsaturated group-containing carboxylic acids can be carried out in the presence of a catalyst such as triethylbenzylammonium chloride, 2,6-isobutylphenol, or trisdimethylaminomethylphenol by heating and stirring at 90 to 120° C. while blowing in air.

[0062] Examples of dicarboxylic acid compounds, tricarboxylic acid compounds or their monoanhydrides that react with the hydroxyl group generated by the reaction of the above-mentioned glycidyl group with the unsaturated group-containing carboxylic acid include maleic acid, succinic acid, itaconic acid, phthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, chlorendic acid, trimellitic acid, and their monoanhydrides.Two or more of these compounds may be used in combination.Of these, tetrahydrophthalic anhydride, succinic anhydride, and trimellitic anhydride are preferred.

[0063] The above reaction can be carried out in the presence of a catalyst such as triethylamine, tetraethylammonium bromide, or triphenylphosphine, by heating at 90 to 130° C. and stirring.

[0064] The synthesis method of resin (B)-1 is not limited to this. For example, the above-mentioned (meth)acrylic acid esters and (meth)acrylic acid are radically copolymerized in a solvent, and then a (meth)acrylic acid ester compound having a glycidyl group, such as glycidyl (meth)acrylate, is reacted with the carboxy group in the copolymer to obtain resin (B)-1. In some cases, the above-mentioned dicarboxylic acid compound, tricarboxylic acid compound, or their acid monoanhydride may be reacted with the hydroxy group generated to obtain resin (B)-1 (hereinafter, the synthesis method described in this paragraph is also referred to as the "second synthesis method").

[0065] Examples of (meth)acrylic acid esters having the functional group described above as R2 used in the second synthesis method include cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate (formula (4)), dicyclopentenyl (meth)acrylate (formula (5)), ethylene glycol modified cyclohexyl (meth)acrylate, ethylene glycol modified dicyclopentanyl (meth)acrylate (formula (6)), ethylene glycol modified dicyclopentenyl (meth)acrylate (formula (7)), etc. Two or more of these (meth)acrylic acid esters having a cyclohexyl group, dicyclopentanyl group, or dicyclopentenyl group may be used in combination.

[0066] [ka]

[0067] [ka]

[0068] [ka]

[0069] [ka]

[0070] In addition, R1 in the general formulae (4) to (7) represents a hydrogen atom or a methyl group, similar to R1 in the general formula (1). In addition, the general formulae (6) and (7) exemplify a compound having only one ethylene oxide group in the molecule, but it may have multiple ethylene oxide groups in the molecule, or may have other alkylene oxide groups such as a propylene oxide group. The ethylene glycol modified cyclohexyl (meth)acrylate may have only one ethylene oxide group, or may have multiple ethylene oxide groups in the molecule, or may have other alkylene oxide groups such as a propylene oxide group.

[0071] When (meth)acrylic acid esters having the above-mentioned functional group as R2 are radically copolymerized with (meth)acrylic acid, other (meth)acrylic acid esters having a structure represented by general formula (1) may be copolymerized. Examples of the other (meth)acrylic acid esters include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, iso-propyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, neopentyl (meth)acrylate, isoamyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dodecyl (meth)acrylate, cyclopentyl (meth)acrylate, butyl ... Examples of the (meth)acrylic acid esters include (meth)acrylic acid esters having a hydrocarbon group having 1 to 20 carbon atoms, such as cyclohexyl (meth)acrylate, 2-methylcyclohexyl (meth)acrylate, dicyclohexyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, propargyl (meth)acrylate, phenyl (meth)acrylate, naphthyl (meth)acrylate, anthracenyl (meth)acrylate, benzyl (meth)acrylate, phenethyl (meth)acrylate, cresyl (meth)acrylate, triphenylmethyl (meth)acrylate, and cumyl (meth)acrylate. Two or more of these (meth)acrylic acid esters may be used in combination.

[0072] The amount of the other (meth)acrylic esters is adjusted so that the amount of the (meth)acrylic esters having a cyclohexyl group, a dicyclopentanyl group or a dicyclopentenyl group is 20 mol % or more relative to the total of the (meth)acrylic esters having a cyclohexyl group, a dicyclopentanyl group or a dicyclopentenyl group and the other (meth)acrylic esters.

[0073] When resin (B)-1 is synthesized by the second synthesis method, the blending ratio of the (meth)acrylic acid ester having the structure represented by general formula (1) to (meth)acrylic acid may be adjusted so that the blending amount of the (meth)acrylic acid ester having the structure represented by general formula (1) is 5 mol % or more and 90 mol % or less, and the blending amount of (meth)acrylic acid is 10 mol % or more and 95 mol % or less.

[0074] In the radical polymerization, a known radical polymerization initiator such as an azo compound or a peroxide may be used, and the degree of polymerization may be controlled by using a known chain transfer agent or a polymerization inhibitor, etc. The reaction temperature may be appropriately set in consideration of the half-life temperature of the radical polymerization initiator used.

[0075] Next, the carboxyl group in the copolymer obtained by the above copolymerization is reacted with a compound containing an unsaturated group and a glycidyl group to open the ring of the glycidyl group. The amount of the compound containing an unsaturated group and a glycidyl group to be reacted at this time is preferably 50 mol% or more, more preferably 60 mol% or more, based on the carboxyl group. By increasing the amount of the compound containing an unsaturated group and a glycidyl group, the introduction of the unsaturated group in the resin (B)-1 can be increased, and the photocurability can be improved.

[0076] Examples of the compound containing an unsaturated group and a glycidyl group to be reacted with a carboxy group include glycidyl (meth)acrylate, 4-hydroxybutyl acrylate glycidyl ether, etc. Among these, glycidyl (meth)acrylate is preferred.

[0077] The addition reaction of the compound containing the unsaturated group and the glycidyl group can be carried out in the presence of a catalyst such as triethylbenzylammonium chloride, 2,6-isobutylphenol, trisdimethylaminomethylphenol, or triphenylphosphine by heating and stirring at 70 to 130°C while blowing in air.

[0078] The hydroxyl group generated by the reaction of the compound containing the carboxyl group, the unsaturated group and the glycidyl group may be reacted with a dicarboxylic acid compound, a tricarboxylic acid compound or an acid monoanhydride thereof. Examples of the dicarboxylic acid compound, the tricarboxylic acid compound or an acid monoanhydride thereof include maleic acid, succinic acid, itaconic acid, phthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, chlorendic acid, trimellitic acid and an acid monoanhydride thereof. Two or more of these compounds may be used in combination. Among these, tetrahydrophthalic anhydride, succinic anhydride and trimellitic anhydride are preferred.

[0079] The above reaction can be carried out in the presence of a catalyst such as triethylamine, tetraethylammonium bromide, or triphenylphosphine, by heating at 90 to 130° C. and stirring.

[0080] When the resin (B)-1 has other structures such as the above-mentioned styrene and monomaleimide, the above-mentioned styrene and monomaleimide may be copolymerized in the initial radical polymerization in either method.

[0081] The weight average molecular weight (Mw) of resin (B)-1, calculated as polystyrene, as measured by gel permeation chromatography (GPC) is preferably from 3,000 to 50,000, more preferably from 4,000 to 25,000, and even more preferably from 4,000 to 9,000. When the weight average molecular weight is 3,000 or more, the adhesion of the pattern during alkaline development is improved, and when the weight average molecular weight is 50,000 or less, the developability is improved.

[0082] The weight average molecular weight of resin (B)-1 is calculated by dissolving a sampled solution in tetrahydrofuran, measuring the molecular weight distribution using a Tosoh HLC-8220GPC, and calculating the weight average molecular weight in terms of standard polystyrene. The acid value of component A is calculated by dissolving a sampled solution in dioxane, neutralizing titrating with a 0.1N potassium hydroxide aqueous solution, and calculating the acid value in terms of the solid content of the sample solution from the equivalence point.

[0083] The acid value of the resin (B)-1 is preferably 30 mgKOH / g or more and 200 mgKOH / g or less, more preferably 50 mgKOH / g or more and 150 mgKOH / g or less. When the acid value is 30 mgKOH / g or more, residues are less likely to remain during alkaline development, and when it is 200 mgKOH / g or less, the penetration speed of the alkaline developer can be appropriately adjusted to make peeling development less likely to occur.

[0084] (Resin (B)-2) The (B) component may be an epoxy (meth)acrylate acid adduct obtained by reacting an epoxy compound having two glycidyl ether groups derived from a bisphenol with (meth)acrylic acid, and then reacting the resulting compound having a hydroxyl group with a polybasic carboxylic acid or its anhydride (hereinafter referred to as "resin (B)-2"). The epoxy compound derived from a bisphenol means an epoxy compound obtained by reacting a bisphenol with an epihalohydrin, or an equivalent thereof.

[0085] The resin (B)-2 is preferably a bisphenol-type alkali-soluble resin having a fluorene structure represented by the following general formula (9).

[0086] [ka]

[0087] In the general formula (9), Ar is independently an aromatic hydrocarbon group having 6 to 14 carbon atoms, and a part of the hydrogen atoms constituting Ar may be substituted with an alkyl group having 1 to 10 carbon atoms, an aryl group or an arylalkyl group having 6 to 10 carbon atoms, a cycloalkyl group or a cycloalkylalkyl group having 3 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, or a halogen group. R6 is independently an alkylene group having 2 to 4 carbon atoms. l is independently a number of 0 to 3. G is independently a (meth)acryloyl group or a substituent represented by the following general formula (10) or the following general formula (11). Y is a tetravalent carboxylic acid residue. Z is independently a hydrogen atom or a substituent represented by the following general formula (12), and at least one of Z is a substituent represented by the following general formula (12). q is a number having an average value of 1 to 20.

[0088] [ka]

[0089] [ka]

[0090] In general formulas (10) and (11), R7 is a hydrogen atom or a methyl group, R8 is an alkylene group or an alkylarylene group having from 2 to 10 carbon atoms, R9 is a saturated or unsaturated hydrocarbon group having from 2 to 20 carbon atoms, and m is a number from 0 to 10. * indicates a bonding site with the compound shown in general formula (9).

[0091] [ka]

[0092] In general formula (12), W is a divalent or trivalent carboxylic acid residue, and n is the number 1 or 2. * indicates the bonding site with the compound represented by general formula (9).

[0093] The resin represented by the general formula (9) can be synthesized by the following method.

[0094] First, an epoxy compound (a) having a bisarylfluorene skeleton, which may have several alkylene oxide modified groups in one molecule and which is represented by the following general formula (13) (hereinafter, simply referred to as "epoxy compound (a)") is reacted with at least one of (meth)acrylic acid, a (meth)acrylic acid derivative represented by the following general formula (14), and a (meth)acrylic acid derivative represented by the following general formula (15) to obtain a diol compound which is an epoxy (meth)acrylate. The bisarylfluorene skeleton is preferably a bisnaphtholfluorene skeleton or a bisphenolfluorene skeleton.

[0095] [ka]

[0096] In general formula (13), Ar are each independently an aromatic hydrocarbon group having 6 to 14 carbon atoms, and some of the hydrogen atoms constituting Ar may be substituted with an alkyl group having 1 to 10 carbon atoms, an aryl group or an arylalkyl group having 6 to 10 carbon atoms, a cycloalkyl group or a cycloalkylalkyl group having 3 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, or a halogen group. R6 are independently an alkylene group having 2 to 4 carbon atoms. 1 are independently a number of 0 to 3.

[0097] [ka]

[0098] [ka]

[0099] In general formulas (14) and (15), R7 is a hydrogen atom or a methyl group, R8 is an alkylene group or an alkylarylene group having 2 to 10 carbon atoms, R9 is a saturated or unsaturated hydrocarbon group having 2 to 20 carbon atoms, and m is a number of 0 to 10.

[0100] The reaction between the epoxy compound (a) and (meth)acrylic acid or its derivative can be carried out by a known method. For example, Japanese Patent Application Laid-Open No. 4-355450 describes that a diol compound containing a polymerizable unsaturated group can be obtained by using about 2 moles of (meth)acrylic acid per mole of an epoxy compound having two epoxy groups. In this embodiment, the compound obtained by the reaction is a diol (d) containing a polymerizable unsaturated group represented by the following general formula (16) (hereinafter, also simply referred to as "diol (d)").

[0101] [ka]

[0102] In general formula (16), Ar are each independently an aromatic hydrocarbon group having 6 to 14 carbon atoms, and some of the hydrogen atoms constituting Ar may be substituted with an alkyl group having 1 to 10 carbon atoms, an aryl group or an arylalkyl group having 6 to 10 carbon atoms, a cycloalkyl group or a cycloalkylalkyl group having 3 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, or a halogen group. G are each independently a (meth)acryloyl group or a substituent represented by general formula (17) or general formula (18), and R6 are independently an alkylene group having 2 to 4 carbon atoms. 1 is independently a number of 0 to 3.

[0103] [ka]

[0104] [ka]

[0105] In general formula (17) and general formula (18), R7 is a hydrogen atom or a methyl group, R8 is an alkylene group or an alkylarylene group having 2 to 10 carbon atoms, R9 is a saturated or unsaturated hydrocarbon group having 2 to 20 carbon atoms, and m is a number of 0 to 10. * indicates a bonding site with the compound shown in general formula (16).

[0106] Next, the diol (d) obtained above is reacted with a dicarboxylic acid or tricarboxylic acid or its monoanhydride (b), and a tetracarboxylic acid or its dianhydride (c) to obtain an unsaturated group-containing curable resin having a carboxy group and a polymerizable unsaturated group in one molecule, as represented by general formula (9).

[0107] The acid component is a polyvalent acid component capable of reacting with a hydroxyl group in the diol (d) molecule. To obtain the resin represented by the general formula (9), it is necessary to use a dicarboxylic acid or tricarboxylic acid or an acid monoanhydride thereof (b) in combination with a tetracarboxylic acid or an acid dianhydride thereof (c). The carboxylic acid residue of the acid component may be either a saturated or unsaturated hydrocarbon group. In addition, the carboxylic acid residue may contain a bond containing a hetero element such as -O-, -S-, or a carbonyl group.

[0108] Examples of the dicarboxylic acid or tricarboxylic acid or the acid monoanhydride (b) thereof include chain hydrocarbon dicarboxylic acid or tricarboxylic acid, alicyclic hydrocarbon dicarboxylic acid or tricarboxylic acid, aromatic hydrocarbon dicarboxylic acid or tricarboxylic acid, and acid monoanhydrides thereof.

[0109] Examples of the above-mentioned chain hydrocarbon dicarboxylic acid or tricarboxylic acid include succinic acid, acetylsuccinic acid, maleic acid, adipic acid, itaconic acid, azelaic acid, citramalic acid, malonic acid, glutaric acid, citric acid, tartaric acid, oxoglutaric acid, pimelic acid, sebacic acid, suberic acid, and diglycolic acid, as well as these dicarboxylic acids or tricarboxylic acids having any substituent introduced therein.

[0110] Examples of the alicyclic hydrocarbon dicarboxylic acid or tricarboxylic acid include cyclobutane dicarboxylic acid, cyclopentane dicarboxylic acid, hexahydrophthalic acid, tetrahydrophthalic acid, methyl tetrahydrophthalic acid, methyl end methylene tetrahydrophthalic acid, chlorendic acid, hexahydrotrimellitic acid, and norbornane dicarboxylic acid, as well as these dicarboxylic acids or tricarboxylic acids having any substituent introduced therein.

[0111] Examples of the aromatic hydrocarbon dicarboxylic acid or tricarboxylic acid include phthalic acid, isophthalic acid, 1,8-naphthalenedicarboxylic acid, 2,3-naphthalenedicarboxylic acid, and trimellitic acid, as well as dicarboxylic acids or tricarboxylic acids having any substituent introduced therein.

[0112] Of these, the dicarboxylic acid or tricarboxylic acid is preferably succinic acid, itaconic acid, tetrahydrophthalic acid, hexahydrotrimellitic acid, phthalic acid, or trimellitic acid, and more preferably succinic acid, itaconic acid, or tetrahydrophthalic acid.

[0113] It is preferable to use the above dicarboxylic acid or tricarboxylic acid as its monoanhydride.

[0114] Examples of the tetracarboxylic acid or the acid dianhydride (c) include chain hydrocarbon tetracarboxylic acids, alicyclic hydrocarbon tetracarboxylic acids, aromatic hydrocarbon tetracarboxylic acids, and acid dianhydrides thereof.

[0115] Examples of the above-mentioned chain hydrocarbon tetracarboxylic acids include butane tetracarboxylic acid, pentane tetracarboxylic acid, hexane tetracarboxylic acid, and these chain hydrocarbon tetracarboxylic acids having substituents such as alicyclic hydrocarbon groups and unsaturated hydrocarbon groups introduced therein.

[0116] Examples of the alicyclic hydrocarbon tetracarboxylic acid include cyclobutane tetracarboxylic acid, cyclopentane tetracarboxylic acid, cyclohexane tetracarboxylic acid, cycloheptane tetracarboxylic acid, and norbornane tetracarboxylic acid, as well as these alicyclic tetracarboxylic acids having substituents such as chain hydrocarbon groups and unsaturated hydrocarbon groups introduced therein.

[0117] Examples of the aromatic hydrocarbon tetracarboxylic acid include pyromellitic acid, benzophenone tetracarboxylic acid, 3,3',4,4'-biphenyl tetracarboxylic acid, diphenyl ether tetracarboxylic acid, diphenyl sulfone tetracarboxylic acid, naphthalene-1,4,5,8-tetracarboxylic acid, and naphthalene-2,3,6,7-tetracarboxylic acid.

[0118] Of these, the tetracarboxylic acids are preferably 3,3',4,4'-biphenyltetracarboxylic acid, benzophenonetetracarboxylic acid, and diphenylethertetracarboxylic acid, and more preferably 3,3',4,4'-biphenyltetracarboxylic acid and diphenylethertetracarboxylic acid.

[0119] It is preferable to use the above tetracarboxylic acid as its acid dianhydride.

[0120] Also, instead of the above-mentioned tetracarboxylic acid or its dianhydride (c), bis(trimellitic anhydride) aryl esters can be used. Bis(trimellitic anhydride) aryl esters are compounds produced, for example, by the method described in International Publication No. 2010 / 074065, and structurally are dianhydrides in the form of ester bonds formed by reaction between two hydroxyl groups of an aromatic diol (such as naphthalenediol, biphenol, and terphenyldiol) and the carboxyl groups of two molecules of trimellitic anhydride.

[0121] The method of reacting the diol (d) with the acid components (b) and (c) is not particularly limited, and any known method can be used. For example, JP-A-9-325494 describes a method of reacting an epoxy (meth)acrylate with a tetracarboxylic dianhydride at a reaction temperature of 90 to 140° C.

[0122] In this case, it is preferable to react the epoxy(meth)acrylate (diol (d)), dicarboxylic acid or tricarboxylic acid or their monoanhydrides (b), and tetracarboxylic acid dianhydride (c) in a molar ratio of (d):(b):(c)=1.0:0.01-1.0:0.2-1.0 so that the terminals of the compounds are carboxy groups.

[0123] For example, when using an acid monoanhydride (b) and an acid dianhydride (c), it is preferable to react them so that the molar ratio [[(b) / 2+(c)] / (d)] of the amount of the acid component to the diol (d) [(b) / 2+(c)] is greater than 0.5 and less than 1.0. If the molar ratio is less than 1.0, the terminal of the unsaturated group-containing curable resin represented by the general formula (9) does not become an acid anhydride, so that the content of unreacted acid dianhydride is prevented from increasing, and the stability of each composition over time can be improved. If the molar ratio is greater than 0.5, the remaining amount of unreacted components in the diol (d) containing a polymerizable unsaturated group is prevented from increasing, and the stability of each composition over time can be improved. In addition, in order to adjust the acid value and molecular weight of the unsaturated group-containing curable resin represented by the general formula (9), the molar ratios of each component (b), (c) and (d) can be arbitrarily changed within the above-mentioned range.

[0124] The synthesis of the diol (d) and the subsequent reaction with the polyvalent carboxylic acid or its anhydride are usually carried out in a solvent, if necessary, using a catalyst.

[0125] Examples of the solvent include cellosolve-based solvents such as ethyl cellosolve acetate and butyl cellosolve acetate, high-boiling ether or ester-based solvents such as diglyme, ethyl carbitol acetate, butyl carbitol acetate, and propylene glycol monomethyl ether acetate, and ketone-based solvents such as cyclohexanone and diisobutyl ketone. There are no particular limitations on the reaction conditions such as the solvent and catalyst used, but it is preferable to use, for example, a solvent that does not have a hydroxyl group and has a boiling point higher than the reaction temperature as the reaction solvent.

[0126] The reaction between the epoxy group and the carboxy group or hydroxy group is preferably carried out using a catalyst, which is described in JP-A-9-325494 as an example of the catalyst.

[0127] Resin (B)-2 preferably has an acid value of 50 mgKOH / g or more and 200 mgKOH / g or less, more preferably 60 mgKOH / g or more and 150 mgKOH / g or less. If the acid value is 50 mgKOH / g or more, residues are less likely to remain during alkaline development, and if it is 200 mgKOH / g or less, the penetration speed of the alkaline developer can be appropriately adjusted to make peeling development less likely to occur. The acid value can be determined by titration with a 1 / 10N-KOH aqueous solution using a potentiometric titration device "COM-1600" (manufactured by Hiranuma Sangyo Co., Ltd.).

[0128] The weight average molecular weight (Mw) of the resin (B)-2, measured by gel permeation chromatography (GPC) in terms of polystyrene, is preferably 1000 to 40000, more preferably 1500 to 30000, and even more preferably 2000 to 15000. When the weight average molecular weight (Mw) is 1000 or more, the adhesion of the pattern during alkaline development is improved. When the weight average molecular weight (Mw) is 40000 or less, the developability is improved.

[0129] The acid value and weight average molecular weight (Mw) of the resin (B)-2 can be measured in the same manner as for the resin (B)-1.

[0130] From the viewpoint of facilitating a decrease in the refractive index and reflectance of the cured film, the (B) component preferably contains resin (B)-1, and from the viewpoint of facilitating an increase in patterning ability, the (B) component preferably contains resin (B)-2.

[0131] When resin (B)-2 is used in combination with resin (B)-1, the content of resin (B)-2 is preferably 0.1% by mass or more and less than 10% by mass based on the total amount of resin (B)-1 and resin (B)-2.

[0132] Resin (B)-1 and resin (B)-2 are resins whose refractive index can be 1.50 or more and 1.70 or less, but component (B) may contain an alkali-soluble resin whose refractive index is not 1.50 or more and 1.70 or less. In this case, the amount of each resin is adjusted so that the refractive index of the entire alkali-soluble resin is 1.50 or more and 1.70 or less.

[0133] The content of the (B) component is preferably 15% by mass or more and 90% by mass or less, and more preferably 20% by mass or more and 75% by mass or less, based on the total mass of the solid content. By making the content of the (B) component 15% by mass or more, the photocurability of the photosensitive resin composition can be improved and the patterning property can be improved. By making the content of the (B) component 90% by mass or more, the other components (particularly the (A) component) can be sufficiently blended, and the effect of reducing the refractive index by the (A) component can be sufficiently enhanced.

[0134] [(C) component] The component (C) is a polymerizable compound having at least one ethylenically unsaturated bond.

[0135] Examples of the component (C) include (meth)acrylic acid esters having a hydroxyl group, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate; ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, tetramethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolethane tri(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol di(meth)acrylate, and the like. These include (meth)acrylic acid esters such as erythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, glycerol (meth)acrylate, sorbitol penta(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, sorbitol hexa(meth)acrylate, alkylene oxide modified hexa(meth)acrylate of phosphazene, and caprolactone modified dipentaerythritol hexa(meth)acrylate; and dendrimer type multifunctional acrylates. These photopolymerizable monomers may be used alone or in combination of two or more.

[0136] The (C) component may be one of these polymerizable compounds, or two or more of them may be used in combination. The (C) component can crosslink the molecules of the (B) component, and preferably has three or more unsaturated bonds to achieve this function. The (C) component preferably has an acrylic equivalent, calculated by dividing the molecular weight by the number of (meth)acrylic groups in one molecule, of 50 to 300, more preferably 80 to 200. The (C) component does not have a free carboxy group.

[0137] The content of the (C) component is preferably 3% by mass or more and 50% by mass or less, more preferably 5% by mass or more and 40% by mass or less, and even more preferably 7% by mass or more and 35% by mass or less, based on the total mass of the solid content. By making the content of the (C) component 3% by mass or more, the photocurability of the photosensitive resin composition can be improved. By making the content of the (C) component 50% by mass or less, the other components (particularly the (B) component) can be sufficiently blended, and the effects of the (B) component, such as alkali solubility (developability), can be sufficiently enhanced.

[0138] [(D) component] The component (D) is a polymerization initiator.

[0139] The component (D) is not particularly limited as long as it is a compound that has a polymerizable unsaturated bond and can initiate polymerization of an addition-polymerizable compound. Examples of the component (D) include photopolymerization initiators such as acetophenone compounds, triazine compounds, benzoin compounds, benzophenone compounds, thioxanthone compounds, imidazole compounds, and acyloxime compounds, as well as thermal polymerization initiators used in thermal polymerization. In this specification, the term "polymerization initiator" is used to include sensitizers.

[0140] Examples of the acetophenone compound include acetophenone, diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, benzyl dimethyl ketal, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]propan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-2-morpholino-1-(4-methylthiophenyl)propan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butan-1-one, and oligomers of 2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propan-1-one.

[0141] Examples of triazine compounds include 2,4,6-tris(trichloromethyl)-1,3,5-triazine, 2-methyl-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-phenyl-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(4-chlorophenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(4-methoxynaphthyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, )-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(4-methoxystyryl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(3,4,5-trimethoxystyryl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(4-methylthiostyryl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(pipronyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, and the like.

[0142] Examples of the benzoin compound include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzoin tert-butyl ether, and the like.

[0143] Examples of the benzophenone compound include benzophenone, o-benzoylmethylbenzoate, 4-phenylbenzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone, 2,4,6-trimethylbenzophenone, 4,4'-bis(N,N-diethylamino)benzophenone, and the like.

[0144] Examples of thioxanthone compounds include thioxanthone, 2-chlorothioxane, 2-methylthioxanthone, 2-isopropylthioxanthone, 4-isopropylthioxanthone, 2,4-diethylthioxanthone, 2,4-dichlorothioxanthone, 1-chloro-4-propoxythioxanthone, and the like.

[0145] Examples of the imidazole compound include 2-(o-chlorophenyl)-4,5-phenylimidazole dimer, 2-(o-chlorophenyl)-4,5-di(m-methoxyphenyl)imidazole dimer, 2-(o-fluorophenyl)-4,5-diphenylimidazole dimer, 2-(o-methoxyphenyl)-4,5-diphenylimidazole dimer, 2,4,5-triarylimidazole dimer, and the like.

[0146] Examples of acyl oxime compounds include 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-bicycloheptyl-1-one oxime-O-acetate, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-adamantyl methan-1-one oxime-O-benzoate, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-adamantyl methan-1-one oxime-O-acetate, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol- 3-yl]-tetrahydrofuranylmethan-1-one oxime-O-benzoate, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-tetrahydrofuranylmethan-1-one oxime-O-acetate, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-thiophenylmethan-1-one oxime-O-benzoate, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-thiophenylmethan-1-one oxime-O-acetate, 1-[9-ethyl 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-morphonylmethan-1-one oxime-O-benzoate, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-morphonylmethan-1-one oxime-O-acetate, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-ethan-1-one oxime-O-bicycloheptanecarboxylate, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-ethan-1-one oxime-O-bicycloheptanecarboxylate Oxime-O-tricyclodecane carboxylate, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-ethan-1-one oxime-O-adamantane carboxylate, 1-[4-(phenylsulfanyl)phenyl]octane-1,2-dione = 2-o-benzoyl oxime, 1-[9-ethyl-6-(2-methylbenzoyl)carbazol-3-yl]ethanone-o-acetyl oxime, (2-methylphenyl)(7-nitro-9,9-dipropyl-9H-fluoren-2-yl)-acetyl oxime, ethanone,1-[7-(2-methylbenzoyl)-9,9-dipropyl-9H-fluoren-2-yl]-1-(O-acetyloxime), ethanone, 1-(-9,9-dibutyl-7-nitro-9H-fluoren-2-yl)-1-o-acetyloxime, ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime), 1,2-octanedien, 1-[4-(phenylthio)-, 2-(O-benzoyloxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl ]-,1-(O-acetyloxime), 1-(4-phenylsulfanylphenyl)butane-1,2-dione-2-oxime-O-benzoate, 1-(4-methylsulfanylphenyl)butane-1,2-dione-2-oxime-O-acetate, 1-(4-methylsulfanylphenyl)butan-1-one oxime-O-acetate, 4-ethoxy-2-methylphenyl-9-ethyl-6-nitro-9H-carbazol-3-yl-O-acetyloxime, 5-(4-isopropylphenylthio)-1,2-indandione,2-(O-acetyloxime) and the like. The above photopolymerization initiators may be used alone or in combination of two or more.

[0147] Other examples of the acyloxime photopolymerization initiator include O-acyloxime photopolymerization initiators represented by general formula (19) or general formula (20).

[0148] [ka]

[0149] In formula (19), R 10 , R 11 each independently represents an alkyl group having 1 to 15 carbon atoms, an aryl group having 6 to 18 carbon atoms, an arylalkyl group having 7 to 20 carbon atoms, or a heterocyclic group having 4 to 12 carbon atoms; R 12represents an alkyl group having 1 to 15 carbon atoms, an aryl group having 6 to 18 carbon atoms, or an arylalkyl group having 7 to 20 carbon atoms. Here, the alkyl group and the aryl group may be substituted with an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkanoyl group having 1 to 10 carbon atoms, or a halogen, and the alkylene portion may contain an unsaturated bond, an ether bond, a thioether bond, or an ester bond. The alkyl group may be any of linear, branched, and cyclic alkyl groups.

[0150] [ka]

[0151] In formula (20), R 13 and R 14 R are each independently a linear or branched alkyl group having 1 to 10 carbon atoms, a cycloalkyl group, a cycloalkylalkyl group, or an alkylcycloalkyl group having 4 to 10 carbon atoms, or a phenyl group which may be substituted with an alkyl group having 1 to 6 carbon atoms. 15 are each independently a linear or branched alkyl or alkenyl group having 2 to 10 carbon atoms, and some of the -CH2- groups in the alkyl or alkenyl group may be substituted with -O- groups. 13 ~R 15 A part of the hydrogen atoms in the group may be substituted with halogen atoms.

[0152] Commercially available acyloxime compounds include, for example, 1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)] (IRGACURE OXE-01, manufactured by BASF), ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime) (IRGACURE OXE-02, manufactured by BASF), [8-[5-(2,4,6-trimethylphenyl)-11-(2-ethylhexyl)-11H-benzo[a]carbazolyl][2-(2,2,3,3-tetrafluoropropoxy)phenyl]methanone-(O-acetyloxime) (IRGACURE OXE-03, manufactured by BASF), and OXE-03, BASF), 1-[4-[4-(2-benzofuranylcarbonyl)phenyl]thio]phenyl]-4-methylpentanone-1-(O-acetyloxime) (IRGACURE OXE-04, BASF and Lunar 6, DKSH Japan), 1-[4-(phenylthio)phenyl]-3-cyclopentylpropane-1,2-dione-2-(O-benzoyloxime) (TR-PBG-305, TRONLY), 1,2-propanedione, 3-cyclohexyl-1-[9-ethyl-6-(2-furanylcarbonyl)-9H-carbazol-3-yl]-, 2-(O-acetyloxime) (TR -PBG-326, manufactured by TRONLY Co., Ltd.), 3-cyclohexyl-1-(6-(2-(benzoyloxyimino)hexanoyl)-9-ethyl-9H-carbazol-3-yl)-propane-1,2-dione-2-(O-benzoyloxime) (TR-PBG-391, manufactured by TRONLY Co., Ltd.), ADEKA ARCLES NCI-831E (manufactured by ADEKA Corporation), Omnirad 1312 (manufactured by IGM Resins BV), and DFI-020 (manufactured by Daito Chemistry Co., Ltd.).

[0153] In addition, the molar absorption coefficient of the (D) component at 365 nm is preferably 10,000 L / mol·cm or more. Such photopolymerization initiators have high sensitivity, so that even in a photosensitive resin composition containing the (C) component, which has a relatively large acrylic equivalent, sufficient photosensitivity can be ensured, and the developability (resolution) of the photosensitive resin composition can be sufficiently improved. Examples of such photopolymerization initiators include Omnirad1312 (manufactured by IGM Resins BV, "Omnirad" is a registered trademark of the company), and ADEKA ARCLES NCI-831 (manufactured by ADEKA Corporation, "ADEKA ARCLES" is a registered trademark of the company).

[0154] In this specification, the molar absorption coefficient of the photopolymerization initiator can be a value obtained by measuring the absorbance of a 0.001 wt % acetonitrile solution in a quartz cell with an optical path length of 1 cm using an ultraviolet-visible-infrared spectrophotometer "UH4150" (manufactured by Hitachi High-Tech Science Corporation).

[0155] In addition, a thermal polymerization initiator may be used as the component (D). Examples of the thermal polymerization initiator include organic peroxides such as benzoyl peroxide, lauroyl peroxide, di-t-butylperoxyhexahydroterephthalate, t-butylperoxy-2-ethylhexanoate, and 1,1-t-butylperoxy-3,3,5-trimethylcyclohexane, azo compounds such as azobisisobutyronitrile, azobis-4-methoxy-2,4-dimethylvaleronitrile, azobiscyclohexanone-1-carbonitrile, azodibenzoyl, 1,1'-azobis(1-acetoxy-1-phenylethane), and 2,2'-azobis(methyl isobutyrate), water-soluble catalysts such as potassium persulfate and ammonium persulfate, and redox catalysts consisting of a combination of peroxides or persulfates and a reducing agent, and any of those usable for normal radical polymerization can be used. The thermal polymerization initiator can be selected in consideration of the storage stability of the thermosensitive resin composition of the present invention and the conditions for forming the cured product.

[0156] As the component (D), an active radical generator or an acid generator may be used.

[0157] Examples of active radical generators include 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 2,2'-bis(o-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 10-butyl-2-chloroacridone, 2-ethylanthraquinone, benzil, 9,10-phenanthrenequinone, camphorquinone, methyl phenylglyoxylate, titanocene compounds, and the like.

[0158] Examples of the acid generator include onium salts such as 4-hydroxyphenyl dimethylsulfonium p-toluenesulfonate, 4-hydroxyphenyl dimethylsulfonium hexafluoroantimonate, 4-acetoxyphenyl dimethylsulfonium p-toluenesulfonate, 4-acetoxyphenyl methyl benzylsulfonium hexafluoroantimonate, triphenylsulfonium p-toluenesulfonate, triphenylsulfonium hexafluoroantimonate, diphenyliodonium p-toluenesulfonate, and diphenyliodonium hexafluoroantimonate, nitrobenzyl tosylates, and benzoin tosylates.

[0159] Examples of sensitizers include acetophenones such as triethylamine, triethanolamine, methyldiethanolamine, triisopropanolamine, benzophenone, 4,4'-bisdimethylaminobenzophenone (Michler's ketone), 4-phenylbenzophenone, 4,4'-dichlorobenzophenone, hydroxybenzophenone, 4,4'-diethylaminobenzophenone, acetophenone, 2,2-diethoxyacetophenone, p-dimethylacetophenone, p-dimethylaminopropiophenone, dichloroacetophenone, trichloroacetophenone, and p-tert-butylacetophenone; benzoin ethers such as benzoin, benzoin methyl ether, benzoin isopropyl ether, and benzoin isobutyl ether; 2-dimethylaminoethylbenzoic acid, 4-dimethylaminobenzoic acid methyl, 4-dimethylaminobenzoic acid ethyl, 4-dimethylaminobenzoic acid (n-butoxy)ethyl, 4-dimethylaminobenzoic acid Benzophenones such as isoamyl, 2-ethylhexyl 4-dimethylaminobenzoate, N,N-dimethyl-p-toluidine, 2,4-diethylthioxanthone, 2,4-diisopropylthioxanthone, 4-benzoyl-4'-methyl-diphenyl sulfide, acrylated benzophenone, 3,3',4,4'-tetra(t-butylperoxycarbonyl)benzophenone, and 3,3'-dimethyl-4-methoxybenzophenone, 2-isopropylthioxanthone, 2 thioxanthone such as 4,4-dimethylthioxanthone, 2,4-diethylthioxanthone, and 2,4-dichlorothioxanthone; aminobenzophenone such as 4,4'-bis(dimethylamino)benzophenone, 4,4'-bisdiethylaminobenzophenone, and 4,4'-bis(ethylmethylamino)benzophenone; 10-butyl-2-chloroacridone, 2-ethylanthraquinone, 9,10-phenanthrenequinone, and camphorquinone.

[0160] The content of the (D) component is preferably 1 part by mass or more and 30 parts by mass or less, more preferably 2 parts by mass or more and 10 parts by mass or less, based on 100 parts by mass of the total of the (B) component and the (C) component. When an acyloxime-based photopolymerization initiator is used as the (D) component, the content of the (D) component is preferably 0.5 parts by mass or more and 20 parts by mass or less, more preferably 1 part by mass or more and 10 parts by mass or less, based on 100 parts by mass of the total of the (B) component and the (C) component. When the content of the (D) component is equal to or more than the lower limit, the photopolymerization speed is adequate, so that sufficient sensitivity can be ensured. When the content of the (D) component is equal to or less than the upper limit, the line width faithful to the mask can be reproduced and the pattern edge can be sharpened.

[0161] The content of the sensitizer is preferably 0.5 parts by mass or more and 400 parts by mass or less, and more preferably 1 part by mass or more and 300 parts by mass or less, when the total mass of the (D) component is 100 parts by mass. When the content of the sensitizer is 0.5 parts by mass or more, the sensitivity of the polymerization initiator can be improved and the polymerization rate can be increased. In addition, when the content of the sensitizer is 400 parts by mass or less, excessive increase in sensitivity can be suppressed, and scorching, peeling residue, and the like can be suppressed during polymerization (particularly during photopolymerization).

[0162] [(E) component] The component (E) is a solvent that adjusts the viscosity of the photosensitive resin composition and improves the coatability.

[0163] Known solvents can be used as the component (E). Examples of the solvent include terpenes such as α- or β-terpineol; ester solvents such as butyl acetate, cyclohexyl acetate, 3-methoxybutyl acetate, 3-methoxy-3-methylbutyl acetate, and 1,3-butylene glycol diacetate; ketone solvents such as acetone, methyl ethyl ketone, N-methyl-2-pyrrolidone, methyl isobutyl ketone, and cyclohexanone; ether solvents having an ethylene glycol skeleton such as diethylene glycol ethyl methyl ether, methyl cellosolve, ethyl cellosolve, methyl carbitol, dimethyl carbitol, ethyl carbitol, and butyl carbitol; propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monobutyl ether, dipropylene glycol monomethyl ether, dipropylene glycol dimethyl ether, and dipropylene glycol monoethyl ether. , triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol diacetate, and other ester-based and ether-based solvents having a propylene glycol skeleton; ethyl acetate, butyl acetate, cellosolve acetate, ethyl cellosolve acetate, butyl cellosolve acetate, carbitol acetate, ethyl carbitol acetate, butyl carbitol acetate, and other acetate ester-based solvents; methanol, ethanol, n-propanol, isopropanol, ethylene glycol, propylene glycol, 3-methoxybutanol, and ethylene glycol mono-t-butyl ether, and other alcohol-based solvents; toluene, xylene, and tetramethylbenzene, and other aromatic solvents; aliphatic solvents; amine-based solvents, and amide-based solvents. From the viewpoint of safety, ketone-based solvents and ester-based and ether-based solvents having a propylene glycol skeleton are preferable. Two or more of these solvents may be used in combination.

[0164] The content of the (E) component is preferably 60% by mass or more and 98% by mass or less, more preferably 70% by mass or more and 98% by mass or less, and even more preferably 75% by mass or more and 95% by mass or less, based on the total mass of the photosensitive resin composition. When the (E) component content is 60% by mass or more, the coatability of the photosensitive resin composition can be sufficiently improved. When the (E) component content is 98% by mass or less, it is easy to form a cured film with a thicker film thickness.

[0165] [Other ingredients] The photosensitive resin composition can contain other components, as necessary, such as an inorganic filler other than the component (A), an epoxy compound and its curing agent and curing accelerator, a coupling agent, a surfactant, a resin other than the alkali-soluble resin, a thermal polymerization inhibitor and an antioxidant, a plasticizer, a filler, a leveling agent, an antifoaming agent, and an ultraviolet absorber.

[0166] Examples of inorganic fillers other than component (A) include talc, mica, glass fiber, carbon fiber, calcium silicate, magnesium carbonate particles, calcium carbonate particles, calcium sulfate particles, barium sulfate particles, alumina particles, and titanium oxide particles.

[0167] Examples of the epoxy compound include bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, bisphenol fluorene type epoxy compounds, bisnaphthol fluorene type epoxy compounds, diphenyl fluorene type epoxy compounds, phenol novolac type epoxy compounds, cresol novolac type epoxy compounds, phenol aralkyl type epoxy compounds, phenol novolac compounds containing a naphthalene skeleton (e.g., NC-7000L: manufactured by Nippon Kayaku Co., Ltd.), naphthol aralkyl type epoxy compounds, trisphenol methane type epoxy compounds (e.g., EPPN-501H: manufactured by Nippon Kayaku Co., Ltd.), and epoxy compounds having an aromatic structure such as tetrakisphenol ethane type epoxy compounds, glycidyl ethers of polyhydric alcohols, and glycidyl polycarboxylic acids. esters, copolymers of monomers having a (meth)acryloyl group containing glycidyl (meth)acrylate as a unit, such as copolymers of methacrylic acid and glycidyl methacrylate; epoxy compounds having a glycidyl group, such as hydrogenated bisphenol A diglycidyl ether (e.g., Likaresin HBE-100, manufactured by New Japan Chemical Co., Ltd., "Likaresin" is a registered trademark of the company); 1,4-cyclohexanedimethanol-bis-3,4-epoxycyclohexanecarboxylate, 2-(3,4-epoxy)cyclohexyl-5,1-spiro(3,4-epoxy)cyclohexyl-m-dioxane (e.g., Araldite CY175, manufactured by Huntsman, "Araldite" is a registered trademark of the company); bis(3,4-epoxycyclohexylmethyl)adipate (e.g., CYRACURE UVR-6128: manufactured by Dow Chemical Company), 3',4'-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate (e.g., Celloxide 2021P: manufactured by Daicel Corporation, "Celloxide" is a registered trademark of the company), butanetetracarboxylic acid tetra(3,4-epoxycyclohexylmethyl) modified ε-caprolactone (e.g., Epolead GT401: manufactured by Daicel Corporation, "Epolead" is a registered trademark of the company), epoxy compounds having epoxycyclohexyl groups (e.g., HiREM-1: manufactured by Shikoku Chemical Industry Co., Ltd.), multifunctional epoxy compounds having a dicyclopentadiene skeleton (e.g., HP7200 series: manufactured by DIC Corporation), 2,Examples of epoxy compounds include alicyclic epoxy compounds such as 1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2-bis(hydroxymethyl)-1-butanol (e.g., EHPE3150, manufactured by Daicel Corporation), epoxidized polybutadiene (e.g., NISSO-PB JP-100, manufactured by Nippon Soda Co., Ltd., "NISSO-PB" is a registered trademark of the company), and epoxy compounds having a silicone skeleton. Among these, the epoxy compounds having the aromatic structure described above are preferred from the viewpoint of improving the flatness and low gas generation of the cured film.

[0168] Examples of the curing agent include amine compounds that contribute to the curing of epoxy resins, polycarboxylic acid compounds or their anhydrides, thermally decomposable esters of polycarboxylic acids, phenol resins, amino resins, dicyandiamide, Lewis acid complex compounds, etc. Among these, it is preferable to select from the group consisting of polycarboxylic acids or their anhydrides, and thermally decomposable esters of polycarboxylic acids.

[0169] Examples of the curing accelerator include imidazoles such as 2-methylimidazole, 2-ethylimidazole, and 2-ethyl-4-methylimidazole, 2-(dimethylaminomethyl)phenol, tertiary amines such as 1,8-diaza-bicyclo(5,4,0)undecene-7 and 1,5-diazabicyclo[4.3.0]non-5-ene, phosphines such as triphenylphosphine, tricyclohexylphosphine, and triphenylphosphinetriphenylborane, and metal compounds such as tin octylate. Among these, 1,8-diazabicyclo[5.4.0]undec-7-ene or 1,5-diazabicyclo[4.3.0]non-5-ene or a salt thereof is preferred.

[0170] Examples of the coupling agent include silane coupling agents such as 3-glycidoxypropyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, and 3-ureidopropyltriethoxysilane, titanium-based coupling agents, and aluminum-based coupling agents. Among these, the silane coupling agent 3-glycidoxypropyltrimethoxysilane is preferred.

[0171] Examples of the surfactant include fluorine-based surfactants, silicone-based surfactants, nonionic surfactants, anionic surfactants, cationic surfactants, betaine surfactants, etc. Among these, fluorine-based surfactants are preferred.

[0172] Examples of resins other than the alkali-soluble resin include vinyl resins, polyester resins, polyamide resins, polyimide resins, polyurethane resins, polyether resins, and melamine resins.

[0173] Examples of the thermal polymerization inhibitor and the antioxidant include hydroquinone, hydroquinone monomethyl ether, pyrogallol, tert-butylcatechol, phenothiazine, and hindered phenol compounds.

[0174] Examples of the plasticizer include dibutyl phthalate, dioctyl phthalate, tricresyl phosphate, etc. Examples of the filler include glass fiber, silica, mica, alumina, etc.

[0175] Examples of the defoaming agent and leveling agent include silicone-based, fluorine-based, and acrylic-based compounds.

[0176] Examples of the ultraviolet absorbing agent include benzotriazole compounds, benzophenone compounds, triazine compounds, and the like.

[0177] [Method for producing photosensitive resin composition] The photosensitive resin composition can be obtained by mixing the above-mentioned components.

[0178] 2.Cured film The photosensitive resin composition can be applied to the flexible substrate described above to form a coating film, the coating film is exposed to position-selective light to cure, the coating film cured by the exposure is developed to form a pattern, and the coating film with the pattern formed thereon is baked (post-cured / baked), thereby forming the substrate with the cured film described above.

[0179] The photosensitive resin composition can be applied by a known application method. Examples of the application method include a known solution immersion method, a spray method, a method using a roller coater, a land coater, a slit coater, or a spinner. By using these methods, the photosensitive resin composition can be applied to a desired thickness.

[0180] The coating film thus formed is preferably dried before exposure. The coating film can be dried by a known drying method. Examples of the drying method include heating with an oven, a hot air blower, a hot plate, an infrared heater, etc., vacuum drying, and combinations thereof. The heating temperature and heating time during drying can be appropriately selected depending on the solvent used, and it is preferable to perform, for example, drying at 60 to 110°C for 1 to 5 minutes.

[0181] The exposure can be carried out by irradiating a part of the coating film with radiation through a photomask, whereby the part of the coating film corresponding to the pattern is photocured.

[0182] The photomask may be a known one. Examples of the photomask include multi-tone masks such as halftone masks and graytone masks. In the graytone mask, a light-shielding portion and a diffraction grating are formed on a light-transmitting substrate. In the diffraction grating, the spacing between light-transmitting regions such as slits, dots, and meshes is equal to or less than the resolution limit of the light used for exposure, and this configuration controls the light transmittance. In the halftone mask, a light-shielding portion and a semi-transmitting portion are formed on a light-transmitting substrate. The semi-transmitting portion controls the transmittance of the light used for exposure.

[0183] The exposure apparatus used for exposure and the exposure irradiation conditions can be appropriately selected. Examples of the radiation to be irradiated include visible light, ultraviolet light, far ultraviolet light, electron beams, and X-rays. Of the above-mentioned radiation, ultraviolet light is preferable. Furthermore, as the apparatus for irradiating radiation, known exposure apparatuses (ultra-high pressure mercury lamps, high pressure mercury lamps, metal halide lamps, far ultraviolet lamps, etc.) can be used. Furthermore, the wavelength of the irradiated radiation is preferably 250 nm or more and 400 nm or less. The radiation exposure dose is 25 mJ / cm. 2 More than 3000mJ / cm 2 It is preferable that:

[0184] After exposure, the irradiated coating film is developed with an alkali to remove the unexposed areas of the coating film.

[0185] Examples of the developing method of the coating film include shower developing method, spray developing method, dip (immersion) developing method, puddle (liquid puddle) developing method, etc. The above development can be carried out using a commercially available developing machine, ultrasonic cleaner, etc.

[0186] Examples of developers suitable for development include aqueous solutions of carbonates of alkali metals or alkaline earth metals, aqueous solutions of hydroxides of alkali metals, etc. Among these, it is preferable to use a weakly alkaline aqueous solution containing 0.05 to 3 mass % of an alkali metal hydroxide such as potassium hydroxide, or a carbonate such as sodium carbonate, potassium carbonate, or lithium carbonate, at a temperature of 23 to 28° C. In addition, in the development step, a commercially available developing machine, ultrasonic cleaner, etc. can be used.

[0187] Thereafter, the exposed portion (coating film) after development is heat treated (baked) to completely harden it (post-bake).

[0188] The exposed portion (coating film) after development can be heated by a known method (heating with an oven, hot air blower, hot plate, infrared heater, etc., vacuum drying, or a combination of these). The heating temperature is not particularly limited as long as it is a temperature at which the coating film is fully cured (post-baked). The heating temperature is preferably 60 to 250°C for 20 to 60 minutes.

[0189] After heat curing, the coating film (cured film) may be washed with short-wavelength radiation to remove organic contaminants on the surface of the coating film.

[0190] The cleaning can be carried out, for example, by irradiating ultraviolet rays with wavelengths of 184.9 nm and 253.7 nm using a low-pressure mercury lamp, with an irradiation dose of 1000 mJ.

[0191] The above-mentioned substrate with the cured film can be used as various functional layers such as a black matrix of a display device or a sensor, a color filter, a light-shielding film, a protective film, and a wavelength conversion layer.

[0192] The light source of the display device may be a known light source such as an organic electroluminescence (EL) light source or a laser light emitting diode (LED) light source. The display device may also be configured such that a wavelength conversion layer containing quantum dots or a phosphor compound is disposed between the light source and the above-mentioned substrate with a cured film. The above-mentioned substrate with a cured film has good flexibility resistance, particularly when the substrate has a thickness of 2 μm or 3 μm or more, and is therefore useful as a light shielding film disposed laterally of the LED light source in an LED display having such a thickness to prevent light leakage to the side.

[0193] Suitable sensors include sensors for light (laser) detection and ranging (LiDAR) for autonomous vehicles, and sensors used in components that require precise light receiving sensitivity, such as encoder light receiving elements. EXAMPLES

[0194] Hereinafter, the embodiments of the present invention will be described in detail based on examples and comparative examples, but the present invention is not limited to these.

[0195] In addition, when the same model of measuring equipment is used, the name of the equipment manufacturer is omitted from the second place. Also, all glass substrates used in the examples are treated in the same way. In addition, when the first decimal place of the content of each component is 0, the notation after the decimal point may be omitted.

[0196] [Method of measuring physical properties] (solid content concentration) The solids concentration was calculated from the weight [W1(g)] of 1 g of the resin solution obtained in the synthesis example impregnated into a glass filter [weight: W0(g)] and the weight [W2(g)] after heating at 160°C for 2 hours, using the following formula. Solid content concentration (weight%) = 100 × (W2-W0) / (W1-W0)

[0197] (Acid value) The acid value was determined by dissolving the resin solution in dioxane and titrating it with a 1 / 10N aqueous KOH solution using a potentiometric titrator "COM-1600" (manufactured by Hiranuma Sangyo Co., Ltd.).

[0198] (molecular weight) The molecular weight was measured using gel permeation chromatography (GPC) "HLC-8220GPC" (manufactured by Tosoh Corporation, solvent: tetrahydrofuran, columns: TSKgelSuper H-2000 (2 columns) + TSKgelSuper H-3000 (1 column) + TSKgelSuper H-4000 (1 column) + TSKgelSuper H-5000 (1 column) (manufactured by Tosoh Corporation), temperature: 40°C, rate: 0.6 ml / min), and the weight average molecular weight (Mw) was calculated as a value converted into standard polystyrene (manufactured by Tosoh Corporation, PS-oligomer kit).

[0199] (Primary particle size) The particle-containing solution was diluted with a solvent to a particle concentration of about 0.1 wt%, and the resulting dispersion was dropped onto a metal mesh with a carbon support film to create a measurement sample. The particle diameter obtained by observing the sample with a transmission electron microscope (TEM; JEOL Ltd., JEM-2000EX) was taken as the primary particle diameter.

[0200] (Average secondary particle size) The dispersion of component (A) was measured for the average secondary particle diameter calculated by the cumulant method using a dynamic light scattering particle size distribution meter (Otsuka Electronics Co., Ltd., Particle Size Analyzer FPAR-1000). The measurement sample was prepared by diluting with a solvent to a particle concentration of 1 to 10% by mass so as to obtain a measurable scattering intensity.

[0201] (Refractive Index) The refractive index of the component (B) was measured by the following method.

[0202] Component (B) was diluted with propylene glycol monomethyl ether acetate to a solids concentration of 20% by mass, and applied to a 125 mm diameter silicon wafer "5 inch P type wafer 1-100" (manufactured by Advantec Co., Ltd.) using a spin coater so that the film thickness after post-baking would be 1.0 μm. Pre-baking was performed at 90°C for 1 minute. Then, post-baking was performed in an oven at 230°C for 30 minutes, and the refractive index at 550 nm was measured using the substrate with a spectroscopic ellipsometry "Alpha-SE" (manufactured by JA Woollam Co., Ltd.).

[0203] [Synthesis example] The abbreviations used in the synthesis examples are as follows. DCPMA: dicyclopentanyl methacrylate GMA: glycidyl methacrylate St: styrene AA: Acrylic acid MA: methacrylic acid MMA: Methyl methacrylate CHMA: Cyclohexyl methacrylate AIBN: Azobisisobutyronitrile TDMAMP: Trisdimethylaminomethylphenol HQ: Hydroquinone TEA: Triethylamine BPFE: Bisphenol fluorene type epoxy resin TEAB: Tetraethylammonium bromide BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride THPA: Tetrahydrophthalic anhydride PGMEA: Propylene glycol monomethyl ether acetate

[0204] (Synthesis Example 1) In a 1 L four-neck flask equipped with a reflux condenser, 300.0 g of PGMEA was placed, and the inside of the flask was replaced with nitrogen, and then the temperature was raised to 120° C. A monomer mixture (a mixture of 66.1 g (0.3 mol) of DCPMA, 85.3 g (0.6 mol) of GMA, and 10.4 g (0.10 mol) of St dissolved in 10 g of AIBN) was added dropwise from a dropping funnel to the flask over 2 hours, and the mixture was further stirred at 120° C. for 2 hours to obtain a copolymer solution.

[0205] Next, the atmosphere in the flask was replaced with air, and then 43.2 g (0.6 mol) of AA, 0.8 g of TDMAMP, and 0.15 g of HQ were added to the resulting copolymer solution, which was then stirred for 6 hours under heating at 120°C to obtain a copolymer solution containing polymerizable unsaturated groups.

[0206] Further, 59.3 g (0.39 mol) of THPA and 0.5 g of TEA were added to the obtained polymerizable unsaturated group-containing copolymer solution and reacted at 120° C. for 4 hours to obtain a polymerizable unsaturated group-containing alkali-soluble copolymer resin solution (B)-1. The solid content concentration of the resin solution was 48 mass%, the acid value (solid content equivalent) was 79 mg KOH / g, and the Mw by GPC analysis was 8500 and the refractive index was 1.52.

[0207] (Synthesis Example 2) BPFE (114.4g, 0.23mol), AA (33.2g, 0.46mol), PGMEA (157g) and TEAB (0.48g) were charged into a 500ml four-neck flask equipped with a reflux condenser, and the mixture was stirred at 100-105°C for 20 hours to react. Next, BPDA (35.3g, 0.12mol) and THPA (18.3g, 0.12mol) were charged into the flask, and the mixture was stirred at 120-125°C for 6 hours to obtain an alkali-soluble resin (B)-2. The solid content concentration of the obtained resin solution was 56.1% by mass, the acid value (solid content equivalent) was 103mgKOH / g, and the Mw by GPC analysis was 3600 and the refractive index was 1.62.

[0208] (Synthesis Example 3) In a 1000 ml four-neck flask equipped with a nitrogen inlet tube and a reflux condenser, 48.21 g (0.56 mol) of MA, 33.64 g (0.40 mol) of MMA, 37.68 g (0.22 mol) of CHMA, 5.91 g (0.036 mol) of AIBN, and 325 g of PGMEA were charged, and the mixture was polymerized by stirring for 8 hours under a nitrogen stream at 80 to 85 ° C. Furthermore, 57.31 g (0.40 mol) of GMA, 1.44 g (0.0055 mol) of TPP, and 0.055 g of 2,6-di-tert-butyl-p-cresol were charged in the flask, and the mixture was stirred for 16 hours at 80 to 85 ° C. to obtain a polymerizable double bond-containing (meth)acrylate resin (B)-3. The solid content of the obtained resin solution was 36.2% by mass, the acid value (solid content equivalent) was 50 mgKOH / g, and the Mw by GPC analysis was 20600 and the refractive index was 1.57.

[0209] [Preparation of photosensitive resin composition] A photosensitive resin composition was prepared using the following components.

[0210] (A) Inorganic filler A-1: Cryolite MMPG (1-methoxy-2-propanol) dispersion "CNP-P" (Stella Chemifa Corporation, cryolite concentration 10% by mass, MMPG concentration 90% by mass, average primary particle size 20 nm, refractive index at 550 nm 1.34) A-2: Magnesium fluoride MMPG dispersion "Magnesium Fluoride Dispersion RP" (manufactured by Stella Chemifa Corporation, magnesium fluoride concentration 10% by mass, MMPG concentration 90% by mass, average primary particle size 50 nm or less, refractive index at 550 nm 1.38 to 1.40) A-3: MMPG dispersion of hollow silica (hollow silica concentration 20.5% by mass, MMPG concentration 79.5% by mass, average secondary particle diameter 70 nm, porosity 26%, refractive index at 550 nm 1.30) A-4: PGMEA (propylene glycol methyl ether acetate) dispersion of hollow silica (hollow silica concentration 20.0% by mass, PGMEA concentration 80.0%, average primary particle size 60 nm, porosity 55%, refractive index at 550 nm 1.24) A-5: PGMEA (propylene glycol methyl ether acetate) dispersion of solid silica (solid silica concentration 19.7% by mass, dispersant concentration 2.3% by mass, PGMEA concentration 78% by mass, average secondary particle diameter 76 nm, refractive index at 550 nm 1.43) A-6: PGMEA dispersion of solid silica (solid silica concentration 30% by mass, PGMEA concentration 70% by mass, average primary particle size 70 nm, refractive index at 550 nm 1.43) A-7: PGMEA dispersion of solid silica "SIRPMA25WT%-H98" (CIK Nanotech Co., Ltd., solid silica concentration 25% by mass, dispersant concentration 5.0% by mass, PGMEA concentration 70% by mass, average secondary particle diameter 125 nm, refractive index at 550 nm 1.43) A-8: PGMEA dispersion of silica "Y10SP-AL2" (manufactured by Admatechs Co., Ltd., silica concentration 20% by mass, PGMEA concentration 80% by mass, average primary particle size 10 nm, refractive index at 550 nm 1.43) A'-9: PGMEA dispersion of titanium oxide (titanium oxide concentration 20% by mass, dispersant 9% by mass, PGMEA concentration 71% by mass, average secondary particle diameter 62 nm, refractive index at 550 nm 2.50)

[0211] In addition, the dispersants A-5, A-7, and A'-9 do not fall under component (B).

[0212] (B) Alkali-soluble resin B-1-1: Alkali-soluble resin synthesized in Synthesis Example 1 (solid content concentration: 48% by mass) B-2-1: Alkali-soluble resin synthesized in Synthesis Example 2 (solid content concentration: 56.1% by mass) B-1-2: Alkali-soluble resin synthesized in Synthesis Example 3 (solid content concentration 36.2% by mass)

[0213] (C) a photopolymerizable monomer having at least one ethylenically unsaturated group C: Mixture of dipentaerythritol pentaacrylate and hexaacrylate (DPHA (acrylic equivalent: 96-115) (manufactured by Nippon Kayaku Co., Ltd.)

[0214] (D) Photopolymerization initiator D: TR-PBG-305 (TRONLY Co., Ltd.)

[0215] (E) Solvent E-1: PGMEA (propylene glycol monomethyl ether acetate) E-2: ANON (cyclohexanone)

[0216] Additive: Silicone surfactant DOWSIL SH 3775 M Fluid (manufactured by Dow Toray Industries, Inc.; DOWSIL is a registered trademark of The Dow Chemical Company)

[0217] The components shown above were mixed in the mixing ratios shown in Tables 1 and 2 below to prepare photosensitive resin compositions of Examples 1 to 9 and Comparative Example 1. The values ​​shown in Tables 1 and 2 are in parts by mass.

[0218] [Table 1]

[0219] [Table 2]

[0220] Resin B-1-1 and resin B-2-1 were mixed in the mass ratio (9.51×0.48:0.61×0.561=4.56:0.34) described in the Examples, and the refractive index measured by the above method was 1.53.

[0221] [evaluation] (Refractive Index) The above photosensitive resin composition was applied onto a silicon wafer having a diameter of 125 mm, "5-inch P-type wafer 1-100" (manufactured by Advantec Co., Ltd.), using a spin coater so that the film thickness after post-baking would be 1.0 μm. Pre-baking was carried out at 90° C. for 1 minute. Thereafter, post-baking was carried out at 230° C. for 30 minutes using an oven to obtain a substrate for refractive index evaluation.

[0222] Using the obtained refractive index evaluation substrate, the refractive index of the cured film after post-baking was measured using a spectroscopic ellipsometer "Alpha-SE" (JA Woollam Co., Ltd.) Based on the results of the refractive index at 550 nm, the following criteria were used for evaluation. ◎:n<1.40 ○: 1.40≦n<1.50 △: 1.50≦n<1.55 ×:1.55≦n

[0223] (reflectance) The above photosensitive resin composition was applied onto a 125 mm x 125 mm glass substrate "#1737" (manufactured by Corning Incorporated) using a spin coater so that the film thickness after post-baking would be 1.0 μm. Pre-baking was performed at 90°C for 1 minute. Thereafter, post-baking was performed using an oven at 230°C for 30 minutes to obtain a substrate for reflectance evaluation.

[0224] Using the obtained reflectance evaluation substrate, the SCI reflectance of the cured film side was measured using a spectrophotometer "SD7000" (manufactured by Nippon Denshoku Co., Ltd.) under conditions of C light source, incident angle of 2°, and wavelength range of 380 to 780 nm, and was judged according to the following criteria. ◎:R%≦7.0% Good: 7.0% <R%≦7.5% △:7.5% <R%≦8.0% ×:8.0% <R%

[0225] (Patterning ability) The above photosensitive resin composition was applied onto a 125 mm x 125 mm glass substrate "#1737" (manufactured by Corning Incorporated) using a spin coater so that the film thickness after post-baking would be 1.0 μm. Pre-baking was performed at 90°C for 1 minute. After that, the substrate was exposed to an I-line illuminance of 20 mW / cm. 2 The coated substrate was irradiated with ultraviolet light for 2.5 seconds through a 10 μm wide stripe pattern mask using an ultra-high pressure mercury lamp, and a photocuring reaction was carried out. The exposed coated substrate was then immersed in a 0.05 wt % potassium hydroxide aqueous solution (23°C) at 1 kgf / cm 2 The development time was 1.5 times the number of seconds required to confirm the target pattern, and then the shower pressure was 5kgf / cm 2 The unexposed areas were removed by spray washing with water. The development time was an additional 20 seconds after the pattern was confirmed. Thereafter, post-baking was performed at 230° C. for 30 minutes using an oven to obtain a substrate for evaluating patterning properties.

[0226] The obtained substrate for evaluating patterning properties was observed under an optical microscope, and evaluated according to the following criteria based on the number of chips at the pattern ends within a visual field of 600 μm×400 μm. ◎: Less than 5 chips on the edge ○: 5 to 7 chipped edges △: 7 or more but less than 10 chipped edges ×: 10 or more chipped edges

[0227] The evaluation results are shown in Tables 3 and 4.

[0228] [Table 3]

[0229] [Table 4]

[0230] The results in Tables 3 and 4 show that by using (A) an inorganic filler having a refractive index of 1.20 or more and 1.46 or less and (B) an alkali-soluble resin having a refractive index of 1.50 or more and 1.70 or less when formed into a cured film with a thickness of 1 μm, a cured film with a low refractive index and good patterning properties can be obtained. [Industrial Applicability]

[0231] According to the photosensitive resin composition of the present invention, a cured film having a low refractive index and good patterning properties can be obtained.

Claims

1. (A) Inorganic filler having a refractive index of 1.20 or more and 1.46 or less (B) Alkali-soluble resin (C) a polymerizable compound having at least one ethylenically unsaturated bond, (D) a photopolymerization initiator, and (E) Solvent Including, The component (B) has a refractive index of 1.50 or more and 1.70 or less when formed into a cured film having a thickness of 1 μm. Photosensitive resin composition.

2. The content of the component (A) is 10% by mass or more and 70% by mass or less based on the total mass of the solid content of the photosensitive resin composition. The photosensitive resin composition according to claim 1 .

3. The component (A) is sodium hexafluoroaluminate. The photosensitive resin composition according to claim 1 .

4. A step of applying the photosensitive resin composition according to any one of claims 1 to 3 onto a substrate; a step of exposing the applied photosensitive resin composition through a photomask, removing the unexposed areas by development, and then baking the composition; The method for producing a cured film comprising the steps of:

5. A substrate having a patterned cured film produced by the method for producing a cured film according to claim 4.

6. A display device comprising the substrate with the cured film according to claim 5 .

7. A sensor comprising a substrate with the cured film according to claim 5 .

Citation Information

Patent Citations

  • Photosensitive resin composition for low refractive index film formation, low refractive index film, optical device, and method for producing low refractive index film

    JP2018072634A