Graft polyolefin composition containing polar group, and laminate

A graft copolymer with a polyolefin backbone and deprotected aromatic monomer enhances adhesion to hydrophobic resins by forming crosslinked structures, addressing the low affinity issues of conventional adhesive resins and achieving strong bonding with fluorine-containing, ABS, and other hydrophobic resins.

JP2024146792APending Publication Date: 2024-10-15MITSUI CHEMICALS INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024035177
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-07
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Conventional adhesive resins exhibit low affinity for hydrophobic resins such as fluorine-containing resins, styrene resins, polyester resins, and polycarbonate resins, lacking adhesive properties for these materials.

Method used

A graft copolymer with a polyolefin main chain and a graft part derived from an aromatic monomer, where the hydroxy group is protected during graft copolymerization and subsequently deprotected, forming a crosslinked structure that enhances adhesion to hydrophobic resins.

Benefits of technology

The graft copolymer demonstrates high adhesion to both fluorine-containing resins and ABS resins, as well as polyethylene terephthalate and polycarbonate resins, through hydrogen bonding and anchor effects, facilitating strong bonding even on wet surfaces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146792000001
    Figure 2024146792000001
  • Figure 2024146792000002
    Figure 2024146792000002
  • Figure 2024146792000003
    Figure 2024146792000003
Patent Text Reader

Abstract

To provide a graft copolymer which may form an adhesive resin, especially an adhesive resin for a fluorine-containing resin, an ABS resin, a polyethylene terephthalate resin and a polycarbonate resin.SOLUTION: There is provided a graft copolymer which has: a main chain part formed of polyolefin; and a graft part. The graft part is derived from an aromatic monomer expressed by a general formula (1) or is formed by subjecting a monomer, wherein a hydroxy group in the aromatic monomer expressed by the general formula (1) is protected by a protective group, to graft copolymerization with the main chain part, followed by deprotecting the hydroxy group. (In the formula, * is a group including an unsaturated group which can be grafted to the main chain part, r is an integer from 0 to 2, n is an integer of 2 or greater, and RT is a hydrogen atom or the like.)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polar group-containing graft polyolefin composition and a laminate. [Background technology]

[0002] Conventional adhesive resins have an acid anhydride or an epoxy group as an adhesive functional group. These adhesive resins exhibit high affinity for polar resins such as ethylene vinyl alcohol copolymers (EVOH) and polyamides, and therefore exhibit high adhesion and compatibility with polar resins.

[0003] In the natural world, it is known that the proteins produced by mussels have a catechol structure with two hydroxyl groups adjacent to the ortho position of the benzene ring, which allows mussels to firmly attach to the surface of rocks and other objects even in water. Therefore, it is expected that catechol derivatives will be applied to the adhesive field. For example, Patent Document 1 discloses an acrylic resin containing a catechol derivative that has sufficient adhesive strength even on wet surfaces. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent Publication No. 2022-135585 Summary of the Invention [Problem to be solved by the invention]

[0005] Conventional adhesive resins have low affinity to hydrophobic resins such as fluorine-containing resins (PTFE, ETFE, etc.), styrene-based resins (ABS resin, etc.), polyester resins (polyethylene terephthalate resin, etc.), and polycarbonate resins. In fact, adhesive resins that have adhesion to these resins have yet to be developed.

[0006] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide a graft copolymer that can constitute an adhesive resin for hydrophobic resins, specifically an adhesive resin for both fluorine-containing resins and ABS resins, particularly an adhesive resin for fluorine-containing resins, ABS resins, polyethylene terephthalate resins and polycarbonate resins. [Means for solving the problem]

[0007] The present invention has the following aspects. [1] The polymer has a main chain portion made of polyolefin (A) and a graft portion, The graft portion is derived from an aromatic monomer (B) represented by the following general formula (1), or is formed by graft copolymerizing a monomer in which a hydroxy group in the aromatic monomer (B) represented by the following general formula (1) is protected with a protecting group onto the main chain portion, and then deprotecting the hydroxy group after the graft copolymerization. Graft copolymer (X).

[0008] [ka]

[0009] (In formula (1), * represents a group containing an unsaturated group that can be grafted to the main chain portion, r is an integer from 0 to 2; n is an integer from 2 to 5 when r = 0, an integer from 2 to 7 when r = 1, and an integer from 2 to 9 when r = 2; R T is a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 30 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, a halogen atom, a nitro group, an amino group, a carboxy group, or a thiol group. The alkyl group, the aryl group, and the alkenyl group may be bonded to the aromatic ring via an oxygen atom or directly. R T When there are a plurality of them, they may be the same or different. In addition, at least two of the hydroxy groups are present at adjacent positions on the aromatic ring.

[0010] [2] The amount of the grafted portion is 0.01 to 1.5 mmol / gP (mmol / gP represents the amount of substance of the grafted portion per 1 g of the grafted copolymer (X)), according to [1].

[0011] [3] The graft copolymer (X) according to [1] or [2], wherein the aromatic monomer (B) is vinyl catechol.

[0012] [4] A laminate comprising a film containing an adhesive resin and a film containing a resin other than the adhesive resin, the adhesive resin containing the graft copolymer (X) according to any one of [1] to [3].

[0013] [5] The laminate according to [4], wherein the resin other than the adhesive resin is a fluorine-containing resin or an ABS resin. Effect of the Invention

[0014] The graft copolymer of the present invention can constitute an adhesive resin for hydrophobic resins, specifically, an adhesive resin for both fluorine-containing resins and ABS resins, particularly, an adhesive resin for fluorine-containing resins, ABS resins, polyethylene terephthalate resins and polycarbonate resins. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present invention will now be described in further detail. [Graft copolymer (X)] The graft copolymer (X) according to the present invention has a main chain portion made of polyolefin (A) and a graft portion, and the graft portion is derived from the aromatic monomer (B) represented by the general formula (1) above, or is formed by graft copolymerizing a monomer in which a hydroxy group in the aromatic monomer (B) represented by the general formula (1) is protected with a protecting group onto the main chain portion and then deprotecting the hydroxy group after the graft copolymerization.

[0016] <Main chain part> As the polyolefin (A) used in the present invention, various known olefin polymers can be used. Examples of the polyolefin (A) include olefin homopolymers or copolymers containing, as main structural units, structural units derived from an α-olefin having 2 to 20 carbon atoms. Incidentally, containing as main structural units means that the polyolefin (A) contains 51 mol% or more of structural units derived from an α-olefin having 2 to 20 carbon atoms relative to the molar number of all structural units contained in the polyolefin (A).

[0017] The polyolefin (A) used in the present invention may contain a polyolefin obtained from a biomass olefin. The α-olefin having 2 to 20 carbon atoms may be a linear α-olefin or a branched α-olefin.

[0018] Examples of linear α-olefins having 2 to 20 carbon atoms include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene. Among these α-olefins, α-olefins having 2 to 10 carbon atoms are preferred.

[0019] Examples of branched α-olefins having 3 to 20 carbon atoms include 2-methyl-1-butene, 3-methyl-1-butene, 3,3-dimethyl-1-butene, 3-methyl-1-pentene, 4-methyl-1-pentene, 3-ethyl-1-pentene, 4,4-dimethyl-1-pentene, trimethyl-1-butene, trimethyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, methylethylpentene-1, diethylbutene-1, and propylpentene-1. The branched α-olefin preferably has 5 to 20 carbon atoms, more preferably 5 to 10 carbon atoms.

[0020] The polyolefin (A) preferably contains, as its main structural units, structural units derived from ethylene, propylene, 1-butene, 1-hexene or 1-octene, more preferably contains, as its main structural units, structural units derived from ethylene, propylene or 1-butene, and even more preferably contains, as its main structural units, structural units derived from ethylene or propylene.

[0021] The polyolefin (A) contains structural units derived from an α-olefin having 2 to 20 carbon atoms in an amount of 51 mol % or more, preferably 60 mol % or more, and more preferably 70 mol % or more, based on the number of moles of all structural units contained in the polyolefin (A). The upper limit of the amount of structural units derived from an α-olefin having 2 to 20 carbon atoms is not particularly specified, and may be 100 mol %.

[0022] The polyolefin (A) may have a structural unit in the main chain derived from a compound other than these α-olefins having 2 to 20 carbon atoms. Examples of the other compound include hydrocarbon compounds (not containing heteroatoms). Examples of the hydrocarbon compound include α-olefins having 21 or more carbon atoms, aromatic vinyl compounds including styrene, dienes, and polyenes.

[0023] The polyolefin (A) is preferably a polymer having structural units derived from ethylene as a main structural unit (hereinafter also simply referred to as an "ethylene-based polymer") or a polymer having structural units derived from propylene as a main structural unit (hereinafter also simply referred to as a "propylene-based polymer").

[0024] The ethylene-based polymer has 51 mol% or more, preferably 60 mol% or more, more preferably 70 mol% or more of structural units derived from ethylene based on the number of moles of all structural units contained in the ethylene-based polymer. The upper limit of the amount of structural units derived from ethylene is not particularly specified, and may be 100 mol% (ethylene homopolymer).

[0025] The propylene-based polymer has 51 mol% or more, preferably 60 mol% or more, more preferably 70 mol% or more of structural units derived from propylene based on the number of moles of all structural units contained in the propylene-based polymer. The upper limit of the amount of structural units derived from propylene is not particularly specified, and may be 100 mol% (propylene homopolymer).

[0026] The polyolefin (A) has a melt flow rate (MFR) of preferably 0.01 to 500 g / 10 min, more preferably 0.05 to 200 g / 10 min, and even more preferably 0.1 to 100 g / 10 min, according to ASTM D1238 at 190° C. under a load of 2.16 kg. When the MFR of the polyolefin (A) is within this range, the MFR of the graft copolymer (X) is also approximately the same, and therefore the graft copolymer (X) has excellent handleability.

[0027] The polyolefin (A) used in the graft copolymerization has a weight average molecular weight (Mw) measured by gel permeation chromatography (GPC) of preferably 100,000 to 700,000, more preferably 150,000 to 500,000. When the weight average molecular weight (Mw) of the polyolefin (A) is within this range, the graft copolymer (X) has excellent handleability.

[0028] The value of the molecular weight distribution (Mw / Mn) calculated from the weight average molecular weight (Mw) and the number average molecular weight (Mn) of the polyolefin (A) is preferably in the range of 1.5 to 6.0, more preferably 1.5 to 5.8, and even more preferably 1.5 to 5.6. The weight average molecular weight (Mw) and the number average molecular weight (Mn) are values ​​calculated by gel permeation chromatography (GPC). The measurement conditions for GPC can be as described below.

[0029] The polyolefin (A) can be produced by a conventional method, for example, by polymerization using a titanium-based catalyst, a vanadium-based catalyst, or a metallocene catalyst. The structure of the polyolefin (A) may be either an isotactic structure or a syndiotactic structure. There is no particular limitation on the stereoregularity of the polyolefin (A). As the polyolefin (A), a commercially available polyolefin may be used as it is.

[0030] <Graft section> The graft copolymer (X) according to the present invention includes a graft moiety derived from an aromatic monomer (B) represented by the following general formula (1), or a graft moiety formed by graft copolymerizing a monomer in which a hydroxy group in the aromatic monomer (B) represented by the following general formula (1) is protected with a protecting group, onto the main chain, and then deprotecting the hydroxy group after the graft copolymerization.

[0031] [ka]

[0032] (In formula (1), * represents a group containing an unsaturated group that can be grafted to the main chain portion, r is an integer from 0 to 2; n is an integer from 2 to 5 when r = 0, an integer from 2 to 7 when r = 1, and an integer from 2 to 9 when r = 2; R Tis a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 30 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, a halogen atom, a nitro group, an amino group, a carboxy group, or a thiol group. The alkyl group, the aryl group, and the alkenyl group may be bonded to the aromatic ring via an oxygen atom or directly. R T When there are a plurality of them, they may be the same or different. In addition, at least two of the hydroxy groups are present at adjacent positions on the aromatic ring (specifically, on one benzene ring). *, R T and the hydroxy group may be bonded to any of the benzene rings.

[0033] The term "may have a substituent" means that the group has a substituent or does not have a substituent. The number of carbon atoms includes the number of carbon atoms in the substituent.

[0034] The graft moiety derived from the aromatic monomer (B) represented by general formula (1) has a structure represented by the following general formula (1').

[0035] [ka]

[0036] In formula (1'), ** represents a bond to the main chain, and r, n, and R T represents r, n and R in formula (1). T is equivalent to

[0037] Examples of the group containing an unsaturated group that can be grafted to the main chain include linear or branched alkenyl groups such as vinyl, allyl, propenyl (prop-1-en-1-yl), cyclohexenyl, iso-propenyl (prop-1-en-2-yl), but-3-en-1-yl, crotyl (but-2-en-1-yl), but-3-en-2-yl, methallyl (2-methylallyl), pent-4-en-1-yl, pent-3-en-1-yl, pent-2-en-1-yl, iso-pentenyl (3-methylbut-3-en-1-yl), 2-methylbut-3-en-1-yl, pent-4-en-2-yl, and prenyl (3-methylbut-2-en-1-yl). Of these, vinyl is preferred.

[0038] Examples of the alkyl group include a methyl group, an ethyl group, a 1-propyl group, a 1-butyl group, a 1-pentyl group, a 1-hexyl group, a 1-heptyl group, a 1-octyl group, a 1-nonyl group, a 1-decanyl group, a 1-undecanyl group, a 1-dodecanyl group, a 1-eicosanyl group, an isopropyl group, a sec-butyl (butan-2-yl) group, a tert-butyl (2-methylpropan-2-yl) group, an isobutyl (2-methylpropyl) group, a pentan-2-yl group, a 2-methylbutyl group, an isopentyl (3-methylbutyl) group, a neopentyl (2,2-dimethylpropyl) group, a tert-pentyl (1,1-dimethylpropyl) group, a siamyl (1,2-dimethylpropyl) group, a pentan-3-yl group, a 2-methylpentyl group, a 3-methylpentyl group, an isohexyl (4-methylpentyl) group, a 2-methylpentyl group, a 3-methylpentyl ... ) group, 1,1-dimethylbutyl (2-methylpentan-2-yl) group, 3-methylpentan-2-yl group, 4-methylpentan-2-yl group, 2,2-dimethylbutyl group, 2,3-dimethylbutyl group, 3,3-dimethylbutyl group, thexyl (2,3-dimethylbut-2-yl) group, 3-methylpentan-3-yl group, 3,3-dimethylbut-2-yl group, hexane-3-yl group, 2-methylpentan-3-yl group, heptan-4-yl group, 2,4-dimethylpentan-3-yl group, 3-ethylpentan-3-yl group, 4,4-dimethylpentyl group, 4-methylheptan-4-yl group, 4-propylheptan-4-yl group, 2,3,3-trimethylbutan-2-yl group, and 2,3,4-trimethylpentan-3-yl group.

[0039] Examples of the aryl group include a phenyl group, a tolyl group, a dimethylphenyl group, a trimethylphenyl group, an ethylphenyl group, a propylphenyl group, an α- or β-naphthyl group, a methylnaphthyl group, an anthracenyl group, a phenanthryl group, a benzylphenyl group, a pyrenyl group, an acenaphthyl group, a phenalenyl group, an aceanthrylenyl group, a tetrahydronaphthyl group, an indanyl group, and a biphenylyl group.

[0040] Examples of the alkenyl group include linear or branched alkenyl groups such as vinyl group, allyl group, propenyl group (prop-1-en-1-yl group), cyclohexenyl group, iso-propenyl group (prop-1-en-2-yl group), but-3-en-1-yl group, crotyl group (but-2-en-1-yl group), but-3-en-2-yl group, methallyl group (2-methylallyl group), pent-4-en-1-yl group, pent-3-en-1-yl group, pent-2-en-1-yl group, iso-pentenyl group (3-methylbut-3-en-1-yl group), 2-methylbut-3-en-1-yl group, pent-4-en-2-yl group, and prenyl group (3-methylbut-2-en-1-yl group).

[0041] Examples of alkyl groups, aryl groups, and alkenyl groups bonded to an aromatic ring via an oxygen atom include a methoxy group, an ethoxy group, a 1-propoxy group, a 1-butoxy group, an iso-propoxy group, a sec-butoxy group, an allyloxy group, a n-butoxy group, a tert-butoxy group, a prenyloxy group, a benzyloxy group, a phenoxy group, a naphthoxy group, a toluyloxy group, an iso-propylphenoxy group, an iso-butoxy group, an allylphenoxy group, a tert-butylphenoxy group, a cyclopentyloxy group, a cyclohexyloxy group, a methoxyphenoxy group, a biphenyloxy group, a binaphthyloxy group, and a 1-adamantyloxy group.

[0042] The halogen atoms include, for example, fluorine, chlorine, bromine, and iodine. Examples of the substituent include a halogen atom, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, and a phosphorus-containing group. Examples of the substituent that the alkyl group and the alkenyl group may have include the aryl group.

[0043] Examples of the halogen atom include the halogen atoms described above. Examples of the halogen-containing group include a fluoromethyl group, a trifluoromethyl group, a trichloromethyl group, a pentafluoroethyl group, a 2,2,2-trifluoroethyl group, a fluorophenyl group, a difluorophenyl group, a trifluorophenyl group, a tetrafluorophenyl group, a pentafluorophenyl group, a trifluoromethylphenyl group, a bistrifluoromethylphenyl group, and a hexachloroantimonate anion.

[0044] Examples of the silicon-containing group include a trimethylsilyl group, a triethylsilyl group, a tri-iso-propylsilyl group, a diphenylmethylsilyl group, a tert-butyldimethylsilyl group, a tert-butyldiphenylsilyl group, a triphenylsilyl group, a tris(trimethylsilyl)silyl group, and a trimethylsilylmethyl group.

[0045] Examples of the oxygen-containing group include a hydroxy group, a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an allyloxy group, an n-butoxy group, a sec-butoxy group, an isobutoxy group, a tert-butoxy group, a benzyloxy group, a methoxymethoxy group, a phenoxy group, a 2,6-dimethylphenoxy group, a 2,6-di-isopropylphenoxy group, a 2,6-di-tert-butylphenoxy group, a 2,4,6-trimethylphenoxy group, a 2,4,6-tri-isopropylphenoxy group, a carbonyl group, an acetyl group, an acetoxy group, a formyl group, a carboxy group, a pivaloyloxy group, a benzoyloxy group, and a trifluoroacetoxy group.

[0046] Examples of the sulfur-containing group include a thiol group, a mesyl (methanesulfonyl) group, a phenylsulfonyl group, a tosyl (p-toluenesulfonyl) group, a triflyl (trifluoromethanesulfonyl) group, a nonaflyl (nonafluorobutanesulfonyl) group, a mesylate (methanesulfonate) group, a tosylate (p-toluenesulfonate) group, a triflate (trifluoromethanesulfonate) group, and a nonaflate (nonafluorobutanesulfonate) group.

[0047] Examples of the nitrogen-containing group include a nitro group, an amino group, a cyano group, a methylamino group, a dimethylamino group, an ethylamino group, a diethylamino group, an allylamino group, a diallylamino group, a benzylamino group, a dibenzylamino group, a pyrrolidinyl group, a piperidinyl group, a morpholyl group, a pyrrolyl group, and a bistriflylimide group.

[0048] The graft copolymer (X) may be obtained by introducing the aromatic monomer (B) into the polyolefin (A), or by graft copolymerizing the polyolefin (A) with a monomer in which the hydroxy group in the aromatic monomer (B) represented by the general formula (1) is protected with a protecting group, and then deprotecting the hydroxy group after the graft copolymerization, thereby obtaining the graft copolymer (X).

[0049] Examples of the aromatic monomer (B) satisfying the general formula (1) include 4-vinylcatechol, 3-vinylcatechol, 5-vinylbenzene-1,2,3-triol, 5-vinylbenzene-1,2,3,4-tetraol, 4-vinylbenzene-1,2,3-triol, 3-methyl-5-vinylbenzene-1,2-diol, 4-vinylnaphthalene-1,2,8-triol, and 7,8-dimethyl-4-vinylnaphthalene-1,2-diol.

[0050] The aromatic monomer (B) satisfying the general formula (1) is preferably an aromatic monomer in which r=0 in the general formula (1), more preferably an aromatic monomer in which r=0 and n=2, further preferably 4-vinylcatechol or 3-vinylcatechol, and particularly preferably 4-vinylcatechol.

[0051] The reason why the resin containing the graft copolymer (X) has adhesive properties to the fluorine-containing resin is not entirely clear, but the present inventors speculate as follows. Hydrogen bonds are formed between the hydroxyl groups in the aromatic monomer (B) and the fluorine atoms in the fluorine-containing resin, making it easier for the graft copolymer (X) and the fluorine-containing resin to approach each other. When hot-melt treatment is performed to bond the fluorine-containing resin and the resin containing the graft copolymer (X), the grafted portion (i.e., the grafted aromatic monomer (B)) forms a cross-linked structure between the graft copolymers (X). Furthermore, the graft copolymer (X) having a cross-linked structure penetrates into the irregularities on the surface of the fluorine-containing resin and is fixed there (anchor effect), so that the resin containing the graft copolymer (X) exhibits adhesiveness to the fluorine-containing resin.

[0052] In addition, the affinity between the polyolefin contained in the fluorine-containing resin and the polyolefin (A) contained in the graft copolymer (X) also contributes to the development of adhesiveness. Since the main chain polyolefin (A) and the fluorine-containing resin are hydrophobic, the hydroxyl group in the aromatic monomer (B) is placed in a hydrophobic environment. Therefore, it is presumed that interactions such as hydrogen bonds between the fluorine-containing resin and the graft copolymer (X) are easily formed.

[0053] When the graft copolymerization of the polyolefin (A) with the aromatic monomer (B) represented by the general formula (1) in which the hydroxyl group is protected with a protecting group and the hydroxyl group is deprotected after the graft copolymerization to obtain the graft copolymer (X), the hydroxyl group may be oxidized by heating to deprotect the hydroxyl group, resulting in the generation of quinones. The quinones may react with the aromatic monomer (B) having a hydroxyl group to form a crosslinked structure between the graft copolymers (X).

[0054] The present inventors presume that, in the graft copolymer (X) produced including the deprotection step, similarly to the above, a resin containing the graft copolymer (X) exhibits adhesiveness to a fluorine-containing resin due to hydrogen bonds between the hydroxy groups in the graft moiety and the fluorine atoms in the fluorine-containing resin and the anchor effect due to the hot melt treatment.

[0055] The protecting group includes conventionally known protecting groups, such as an acetyl group, a trialkylsilyl group, a tetrahydropyranyl group, and a monomethoxymethyl group. The graft copolymer (X) may form a crosslinked structure between the graft copolymers during the hot melt treatment and the heat treatment in the deprotection step.

[0056] The aromatic monomer (B) and the aromatic monomer (B) represented by the general formula (1) in which the hydroxy group is protected with a protecting group may be used alone or in combination of two or more kinds.

[0057] The aromatic monomer (B) and the aromatic monomer (B) represented by the general formula (1) in which the hydroxyl group is protected with a protecting group can be produced by a conventionally known production method. As a production method of 4-vinylcatechol among the aromatic monomers (B), for example, a production method of dissolving caffeic acid in DMF and reacting it with triethylamine can be mentioned.

[0058] An example of the aromatic monomer (B) represented by the general formula (1) in which the hydroxyl group is protected with a protecting group is 3,4-diacetoxystyrene. A method for producing 3,4-diacetoxystyrene includes, for example, dissolving caffeic acid in DMF, reacting it with triethylamine to produce 4-vinylcatechol, and then reacting it with acetic anhydride.

[0059] <Graft copolymer (X)> The method of graft copolymerization of the polyolefin (A) with the aromatic monomer (B) or the aromatic monomer (B) represented by the general formula (1) in which the hydroxyl group is protected with a protecting group is not particularly limited. The graft copolymerization method includes conventionally known graft polymerization methods such as a solution method and a melt kneading method carried out in the presence of a radical initiator.

[0060] When the graft copolymer (X) is produced by a deprotection step, a conventionally known method can be used as the deprotection method. In addition, reaction conditions such as acidic conditions or basic conditions can be determined according to the type of protecting group.

[0061] The graft copolymer (X) preferably contains 0.01 to 1.5 mmol / gP of the graft moiety, more preferably 0.02 to 1.2 mmol / gP, further preferably 0.03 to 1.0 mmol / gP, and particularly preferably 0.03 to 0.3 mmol / gP. Here, mmol / gP represents the amount of substance of the graft moiety per 1 g of the graft copolymer (X). The amount of the graft moiety in the graft copolymer (X) may also be referred to as the graft amount.

[0062] The graft copolymer (X) containing 0.01 mmol / gP or more of the graft portion has high adhesion to hydrophobic resins, specifically both fluorine-containing resins and ABS resins, particularly fluorine-containing resins, ABS resins, polyethylene terephthalate resins and polycarbonate resins. The graft copolymer (X) containing 1.5 mmol / gP or less of the graft portion has high fluidity during hot melt treatment.

[0063] The graft amount was determined under the conditions described in the Examples section. 1 It can be calculated by measuring the H-NMR or IR spectrum. The density of the graft copolymer (X) is preferably 0.85 to 1.05 g / cm 3 , more preferably 0.88 to 1.00 g / cm 3 , and more preferably 0.90 to 0.98 g / cm3 It is.

[0064] The melt flow rate (MFR) of the graft copolymer (X) according to ASTM D1238 at 190° C. under a load of 2.16 kg is preferably 0.1 to 30 g / 10 min, more preferably 0.1 to 20 g / 10 min, and further preferably 0.1 to 15 g / 10 min.

[0065] The weight average molecular weight (Mw) of the graft copolymer (X) measured by gel permeation chromatography (GPC) is preferably 100,000 to 700,000, and more preferably 150,000 to 500,000. The graft copolymer (X) having a weight average molecular weight (Mw) within this range has excellent handleability.

[0066] The molecular weight distribution (Mw / Mn) of the graft copolymer (X) calculated from the weight average molecular weight (Mw) and the number average molecular weight (Mn) is preferably in the range of 1.5 to 6.0, more preferably 1.5 to 5.8, and even more preferably 1.5 to 5.6. The weight average molecular weight (Mw) and the number average molecular weight (Mn) are values ​​calculated by gel permeation chromatography (GPC).

[0067] The Mw, Mn and Mw / Mn can be measured using a gel permeation chromatograph (GPC) (e.g., HLC-8321GPC / HT type gel permeation chromatograph (GPC) manufactured by Tosoh Corporation) as follows. As separation columns, TSKgel GMH6-HT (2 columns) and GMH6-HTL (2 columns) (both 7.5 mm I.D. x 30 cm, manufactured by Tosoh Corporation) are used, the column temperature is 140°C, o-dichlorobenzene (containing 0.025% BHT) is used as the mobile phase, the development speed is 1.0 mL / min, the sample concentration is 0.1% (w / v), the sample injection amount is 0.4 mL, and a differential refractometer is used as the detector. The apparatus is calibrated using monodisperse polystyrene (manufactured by Tosoh Corporation, #3std set). The molecular weight distribution (Mw / Mn) is calculated by dividing Mw measured by the above measurement method by Mn measured by the same measurement method.

[0068] [Laminate] The laminate according to the present invention comprises a film containing an adhesive resin and a film containing a resin other than the adhesive resin, and the adhesive resin contains the graft copolymer (X) according to the present invention. Hereinafter, a film containing the adhesive resin may be referred to as a sealant film, and a film containing a resin other than the adhesive resin may be referred to as a base film.

[0069] <Sealant film> The sealant film preferably contains an adhesive resin containing only the graft copolymer (X).

[0070] The thickness of the sealant film is not particularly limited, but from the viewpoint of suitability for use, it is preferably from 2 μm to 1000 μm, more preferably from 5 μm to 800 μm.

[0071] The sealant film is preferably a stretched film or a non-stretched film, and more preferably a stretched film. The stretched film may be either a uniaxially stretched film or a biaxially stretched film, but is preferably a biaxially stretched film from the viewpoint of the balance of strength and rigidity in the machine direction and the perpendicular direction.

[0072] The sealant film is preferably a stretched film that is formed into a film and then subjected to a stretching treatment. When the sealant film is a stretched film, a laminate having excellent rigidity can be provided.

[0073] The method for stretching the sealant film may be a known method for producing a stretched film, such as roll stretching, tenter stretching, tubular stretching, or a combination of the above stretching methods.

[0074] <Base film> Examples of resins contained in the base film other than the adhesive resin include ethylene-based polymers, propylene-based polymers, poly-1-butene, poly-4-methyl-1-pentene, ethylene-vinyl acetate copolymers, ethylene-methacrylate ester copolymers, ethylene-acrylic acid copolymers, ionomers, polyamide resins (nylon 6, nylon 66, nylon 11, nylon 12, etc.), polyester resins (polyethylene terephthalate (PET), polybutylene terephthalate, etc.), polyvinylidene chloride, polyvinyl chloride, polystyrene, polyvinyl alcohol, ethylene-vinyl alcohol copolymers, polycarbonate resins, fluorine-containing resins, and ABS resins.

[0075] Examples of the fluorine-containing resin include ethylene-tetrafluoroethylene copolymer (ETFE) resin, polytetrafluoroethylene (PTFE) resin, and polyvinylidene fluoride (PVDF) resin.

[0076] From the viewpoint of adhesion to the sealant film containing the graft copolymer (X), the resin other than the adhesive resin is preferably a fluorine-containing resin, an ABS resin, a polyethylene terephthalate resin or a polycarbonate resin, more preferably a fluorine-containing resin or an ABS resin. The resin other than the adhesive resin does not include the graft copolymer (X). The base film may contain only one type of resin other than the adhesive resin, or may contain two or more types of resins other than the adhesive resin.

[0077] The laminate can be prepared by a conventional method involving a hot melt treatment, for example, a method in which the sealant film and the base film are overlapped and heat sealed.

[0078] The laminate may include only one layer of the base film, or may include two or more layers of the base film. The method for producing the sealant film and the base film is not particularly limited, and examples thereof include conventionally used film-forming methods such as an extrusion method, a cast molding method, a T-die method, a cutting method, and an inflation method, as well as a multilayer co-extrusion film-forming method using two or more resins.

[0079] Each film constituting the laminate may or may not contain additives that are typically blended into adhesive laminate films, such as antioxidants, heat stabilizers, weather stabilizers, anti-fogging agents, anti-blocking agents, slip agents, lubricants, crystal nucleating agents, antistatic agents, flame retardants, pigments, dyes, or fillers, within the range that does not impair the effects of the present invention. EXAMPLES

[0080] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.

[0081] [Examples 1 to 4, Comparative Examples 1 to 3] The adhesive properties of graft copolymers 1 to 7 produced in the following Examples 1 to 4 and Comparative Examples 1 to 3 were evaluated by the methods described in Adhesion Evaluations 1 and 2 below. [Adhesion rating 1] <Press sheet and adhesive sheet production> The graft copolymers synthesized in the following examples were press molded under the conditions of a temperature of 160°C, a pressure of 100 kPa, a preheating time of 7 minutes, and a pressurizing time of 4 minutes, and then quenched in a press molding machine set at 20°C to obtain a press sheet having a thickness of 300 μm, a length of 80 mm, and a width of 80 mm. A Teflon (registered trademark) sheet (0.2 mm thick) was used as the release film. The press sheet was cut to a width of 20 mm to obtain an adhesive sheet (L).

[0082] (Adhesion method) As the base layer, an ethylene-tetrafluoroethylene copolymer (ETFE) resin sheet (manufactured by AS ONE Corporation) (Q) having a thickness of 50 μm, a length of 80 mm and a width of 20 mm was used.

[0083] An ETFE resin sheet (Q layer), an adhesive sheet (L layer), and an ETFE resin sheet (Q layer) were layered in this order, and the three-layer laminate was sandwiched between Teflon (registered trademark) (PTFE) sheets (thickness: 100 μm). Both the upper and lower press plates were heat sealed using a heat seal tester under the following conditions: heat seal temperature: 260°C, heat seal time: 10 seconds, heat seal pressure: 0.1 MPa, to produce a three-layer laminate structure (T) consisting of an ETFE resin sheet and an adhesive sheet.

[0084] Peel test The average peel strength between the Q layer and the L layer of the laminated structure was determined by T-peel at a peel speed of 300 mm / min and a peel width of 15 mm. The average values ​​and standard errors of the peel strengths obtained in 4 to 5 peel tests are shown in Table 1.

[0085] [Adhesion evaluation 2] Except for using an ABS resin sheet (UMG ABS EX18A, manufactured by Techno UMG Co., Ltd.) with a thickness of 50 μm, length of 80 mm, and width of 20 mm as the base layer, the press sheet, adhesive sheet, and three-layer laminate structure were prepared, and a peel test was performed in the same manner as in Adhesion Evaluation 1. The average values ​​and standard errors of the peel strengths obtained in the peel test are shown in Table 2.

[0086] [Synthesis example] Graft Monomer <4-vinylcatechol> In a nitrogen-purged 200 mL glass container, 5.0 g (28 mmol) of caffeic acid was dissolved in 18 mL of DMF, 11.7 mL (84 mmol) of triethylamine was added, and the mixture was heated to 100°C and stirred for 1 hour. After cooling, the mixture was cooled to 4°C in an ice bath, 50 mg (0.23 mmol) of BHT (dibutylhydroxytoluene) was added, and 1 mol / L of hydrochloric acid was added until the pH of the solution reached about 2.8 to 3.1 (about 100 mL).

[0087] The solution was transferred to a 500 mL separatory funnel, and 150 mL of ethyl acetate was added to perform a separation operation. The organic phase was separated with 150 mL of approximately 0.001 mol / L hydrochloric acid and 150 mL of pure water (twice), and 50 mg (0.23 mmol) of BHT was added to the organic phase, and the solvent was distilled off under reduced pressure at 30°C. 3.8 g (28 mmol) of 4-vinylcatechol was obtained by drying under reduced pressure for 12 hours at room temperature under a nitrogen flow.

[0088] <3,4-diacetoxystyrene> In a nitrogen-purged 200 mL glass container, 5.0 g (28 mmol) of caffeic acid was dissolved in 18 mL of DMF, 11.7 mL (84 mmol) of triethylamine was added, and the mixture was heated to 100°C and stirred for 1 hour. After cooling, the mixture was cooled to 4°C in an ice bath, and 5.3 mL (56 mmol) of acetic anhydride was added dropwise little by little so that the internal temperature did not exceed 10°C. After stirring at room temperature for 2 hours, 50 mL of approximately 1 mol / L hydrochloric acid was slowly added.

[0089] The solution was transferred to a 500 mL separatory funnel, and 100 mL of diethyl ether was added to perform a separation operation. The organic phase was then separated with 100 mL of approximately 1 mol / L hydrochloric acid, separated with 100 mL of saturated aqueous sodium bicarbonate solution (twice), and separated with 100 mL of pure water (twice), and the solvent was distilled off under reduced pressure at room temperature. The resulting liquid was dried under reduced pressure at room temperature under a nitrogen flow for 12 hours to obtain 5.2 g (24 mmol) of 3,4-diacetoxystyrene.

[0090] <3,4-Bis(triethylsilyl)oxystyrene> In a nitrogen-purged 200 mL glass container, 5.0 g (28 mmol) of caffeic acid was dissolved in 39 mL of DMF, 11.7 mL (84 mmol) of triethylamine was added, and the mixture was heated to 100°C and stirred for 1 hour. After cooling, the mixture was cooled to 4°C in an ice bath, and 9.3 mL (56 mmol) of triethylsilyl chloride was added dropwise little by little so that the internal temperature did not exceed 15°C. The mixture was then stirred at room temperature for 19 hours, and the precipitated solid was removed, after which 200 mL of n-hexane was added.

[0091] The solution was transferred to a 500 mL separatory funnel and separated with 200 mL of approximately 0.1 mol / L hydrochloric acid. The organic phase was then separated with 200 mL of approximately 0.1 mol / L hydrochloric acid, separated with 200 mL of saturated aqueous sodium bicarbonate (twice), and separated with 200 mL of pure water (twice), and the solvent was distilled off under reduced pressure at 35°C.

[0092] The obtained liquid was dried under reduced pressure at room temperature under a nitrogen flow for 12 hours, and then purified by silica gel column chromatography (Wako gel 60 N 38-100 μm, column diameter 70 mm, column length 120 mm, developing solvent: n-hexane / ethyl acetate=90 / 10 (v / v)) to obtain 5.2 g (14 mmol) of 3,4-bis(triethylsilyl)oxystyrene.

[0093] Graft Copolymer [Example 1] <Graft copolymer 1> Under nitrogen flow, 25.0 g of base polymer (LLDPE) (Prime Polymer Co., Ltd., EVOLUE SP-2040) and 110 mL of toluene were charged into a 500 mL glass container, and the internal temperature was raised to 110° C. to dissolve the base polymer. 1.9 g (14 mmol) of 4-vinylcatechol dissolved in 3 mL of 2-butanone was added, and immediately thereafter, 0.97 g (5.5 mmol) of Perbutyl I (t-butylperoxyisopropyl monocarbonate) diluted with 10 mL of toluene was slowly added dropwise.

[0094] The mixture was stirred at a stirring speed of 400 rpm for 5 hours using a single anchor blade. Then, 250 mL of toluene was added, the temperature was raised again to 110°C, and the temperature was lowered to 50°C at 300 rpm to precipitate graft copolymer 1. The precipitated suspension of graft copolymer 1 was transferred to a 1000 mL beaker containing 400 mL of acetone, stirred for 20 minutes, and then filtered. This operation of washing with 400 mL of acetone for 20 minutes was repeated twice, and the obtained graft copolymer 1 was dried under reduced pressure at room temperature for 12 hours under a nitrogen flow.

[0095] The color of the obtained graft copolymer 1 was pale pink.1 H-NMR (solvent: 1,1,2,2-tetrachloroethane, measurement temperature: 120°C) was measured, and the graft amount was calculated to be 0.034 mmol / gP from the integral value of the signal of the aromatic ring of the graft monomer. In addition, IR spectrum measurement revealed that the OH stretching vibration (3580 cm -1 ) was observed.

[0096] [Example 2] <Graft copolymer 2> Under nitrogen flow, 25.0 g of the same base polymer (LLDPE) as in Example 1 and 110 mL of xylene were placed in a 500 mL glass container, and the internal temperature was raised to 110° C. to dissolve the base polymer. Immediately after adding 1.9 g (14 mmol) of 4-vinylcatechol dissolved in 3 mL of 2-butanone, 3.9 g (22 mmol) of Perbutyl I (t-butylperoxyisopropyl monocarbonate) diluted with 10 mL of xylene was slowly added dropwise.

[0097] The mixture was stirred for 3 hours at a stirring speed of 400 rpm using a single anchor impeller (150 mL of xylene was added 30 minutes after the start of the reaction). Then, 50 mL of xylene was added, the temperature was raised again to 120°C, and the temperature was lowered to 50°C at 300 rpm. The suspension of graft copolymer 2 was transferred to a 1000 mL beaker containing 400 mL of acetone, subjected to ultrasonic treatment for 30 minutes, and filtered. Furthermore, ultrasonic treatment for 30 minutes using 500 mL of acetone was repeated three times, and the obtained graft copolymer 2 was dried under reduced pressure at room temperature for 12 hours under a nitrogen flow. IR spectrum measurement revealed that the OH stretching vibration of the graft monomer (3580 cm -1 ) was observed and the graft amount was calculated to be 0.038 mmol / gP.

[0098] [Example 3] <Graft copolymer 3> (Graft copolymerization process) Under nitrogen flow, 25.0 g of the same base polymer (LLDPE) as in Example 1 and 110 mL of xylene were placed in a 500 mL glass container, and the internal temperature was raised to 120° C. to dissolve the base polymer. 3.1 g (14 mmol) of 3,4-diacetoxystyrene was added, and immediately thereafter, 0.39 g (2.2 mmol) of Perbutyl I (t-butylperoxyisopropyl monocarbonate) diluted with 10 mL of xylene was slowly added dropwise.

[0099] The mixture was stirred at a stirring speed of 400 rpm for 3 hours using a single anchor blade. Then, 200 mL of xylene was added, the temperature was raised again to 120°C, and the temperature was lowered to 60°C at 300 rpm to precipitate the graft copolymer. The precipitated suspension of the graft copolymer was transferred to a 1000 mL beaker containing 400 mL of acetone, stirred for 20 minutes, and then filtered. The organic phase was washed twice with 400 mL of acetone for 20 minutes, and the obtained graft copolymer was dried under reduced pressure at 90°C for 12 hours under nitrogen flow.

[0100] The obtained graft copolymer 1 H-NMR (solvent: 1,1,2,2-tetrachloroethane, measurement temperature: 120°C) was measured, and the graft amount was calculated to be 0.17 mmol / gP from the integral value of the aromatic ring signal of the graft monomer and the acetyl group signal. In addition, IR spectrum measurement revealed that the C=O stretching vibration (1775 cm) of the acetoxy group of the graft monomer -1 ) was observed.

[0101] (Deprotection step) Next, 7.5 g of this graft copolymer and 750 mL of toluene were placed in a 1000 mL four-neck flask under a nitrogen flow, and the temperature was raised to 80° C. to dissolve the copolymer. To this solution was added 0.42 g (7.5 mmol) of KOH dissolved in 270 mL of ethanol.

[0102] The mixture was stirred at 400 rpm for 6 hours using a single anchor impeller. The temperature was then lowered to 45°C, and the polymer suspension was poured into a 5L beaker containing 2L of methanol, stirred for 20 minutes, and then filtered. The mixture was then washed with 2L of 5% HCl / methanol solution, 2L of pure water, and 2L of acetone for 20 minutes, and the resulting solid graft copolymer 3 was vacuum-dried at room temperature for 12 hours under nitrogen flow.

[0103] The mass of the obtained graft copolymer 3 was 7.4 g and the color was gray brown. -1 A signal thought to be the OH stretching vibration of the graft monomer was observed near the grafted monomer, and the graft amount was calculated to be 0.076 mmol / gP.

[0104] [Example 4] <Graft copolymer 4> (Graft copolymerization process) A graft copolymer was obtained in the same manner as in Example 3, except that in the graft copolymerization step of Example 3, 3.8 g (14 mmol) of 3,4-bis(triethylsilyl)oxystyrene was used instead of 3.1 g (14 mmol) of 3,4-diacetoxystyrene.

[0105] The color of the obtained graft copolymer was white. 1 H-NMR (solvent: 1,1,2,2-tetrachloroethane, measurement temperature: 120°C) was measured, and the graft amount was calculated to be 0.18 mmol / gP from the integral value of the signal of the aromatic ring of the graft monomer. In addition, IR spectrum measurement revealed that the Si-C2H5 symmetric bending vibration (1250 cm) of the triethylsilyl group of the graft monomer -1 ) and 900-1000 cm -1 Si-O-C6H4 vibrations were observed nearby.

[0106] (Deprotection step) Next, 5.0 g of this graft copolymer and 500 mL of toluene were placed in a 1000 mL four-neck flask under a nitrogen flow, and the mixture was heated to 78° C. to dissolve the copolymer. To this solution was added 11 mL of 35% concentrated hydrochloric acid diluted with 100 mL of ethanol.

[0107] The mixture was stirred at 400 rpm for 3 hours using a single anchor impeller. The temperature was then lowered to 60°C, and the suspension of the graft copolymer was poured into a 3 L beaker containing 1.5 L of methanol, stirred for 20 minutes, and then filtered. The mixture was then washed with 500 mL of acetone for 20 minutes, and the resulting solid graft copolymer 4 was vacuum-dried at room temperature for 12 hours under a nitrogen flow.

[0108] The mass of the obtained graft copolymer 4 was 4.8 g and the color was pale pink. 1 H-NMR (solvent: 1,1,2,2-tetrachloroethane, measurement temperature: 120°C) was measured, and the graft amount was calculated to be 0.060 mmol / gP from the integral value of the signals of the aromatic ring and hydroxyl group of the graft monomer. -1 A signal thought to be the OH stretching vibration of the graft monomer was observed in the vicinity.

[0109] [Comparative Example 1] <Graft copolymer 5> Under a nitrogen flow, 25.0 g of the same base polymer (LLDPE) as in Example 1 and 110 mL of xylene were placed in a 500 mL glass container, and the internal temperature was raised to 120° C. to dissolve the base polymer. Immediately after adding 1.1 g (11 mmol) of maleic anhydride, 0.13 g (0.77 mmol) of Perbutyl I (t-butylperoxyisopropyl monocarbonate) diluted with 10 mL of xylene was slowly added dropwise.

[0110] The mixture was stirred at a stirring speed of 400 rpm for 3 hours using a single anchor blade. Then, 200 mL of xylene was added, the temperature was raised again to 120°C, and the temperature was lowered to 60°C at 300 rpm to precipitate the graft copolymer. The precipitated suspension of the graft copolymer was transferred to a 1000 mL beaker containing 400 mL of acetone, stirred for 20 minutes, and then filtered. The organic phase was washed twice with 400 mL of acetone for 20 minutes, and the obtained graft copolymer was dried under reduced pressure at 90°C for 12 hours under nitrogen flow.

[0111] The obtained graft copolymer 1 H-NMR (solvent: 1,1,2,2-tetrachloroethane, measurement temperature: 120° C.) was measured, and the graft amount of 0.050 mmol / gP was calculated from the signal integral value of the maleic anhydride ring of the graft monomer.

[0112] [Comparative Example 2] <Graft copolymer 6> Graft copolymer 6 was obtained in the same manner as in Example 3, except that the deprotection step was not carried out.

[0113] [Comparative Example 3] <Graft copolymer 7> Graft copolymer 7 was obtained in the same manner as in Example 4, except that the deprotection step was not carried out.

[0114] [Table 1]

[0115] [Table 2]

[0116] The graft copolymers of the examples had a high average peel strength to ETFE resin and were well adhered to fluorine-containing resins. On the other hand, the graft copolymer of Comparative Example 1, which used a conventionally used acid anhydride as an adhesive resin, did not adhere to the ETFE resin. Also, the graft copolymers of Comparative Examples 2 and 3, in which the hydroxyl group of the aromatic monomer was protected with a protecting group without carrying out a deprotection step, had low adhesion to the ETFE resin.

[0117] The graft copolymers of the Examples exhibited adhesion to ABS resin at the same level as the graft copolymers of the Comparative Examples. Therefore, the graft copolymer of the example has high adhesion to both the ETFE resin and the ABS resin.

[0118] [Example 5, Comparative Example 4] The adhesive properties of graft copolymers 8 to 9 produced in Example 5 and Comparative Example 4 below were evaluated by the methods described in Adhesion Evaluations 3 to 6 below.

[0119] [Example 5] <Graft copolymer 8> (4-Vinylcatechol manufacturing process) In a nitrogen-purged 200 mL glass container, 5.0 g (28 mmol) of caffeic acid was dissolved in 18 mL of DMF, 11.7 mL (84 mmol) of triethylamine was added, and the mixture was heated to 100° C. and stirred for 1 hour. After cooling, the mixture was cooled to 4° C. in an ice bath, and 1 mol / L of hydrochloric acid was added until the pH of the solution reached about 6. The solution was transferred to a 500 mL separatory funnel, and 150 mL of diethyl ether was added to perform a separation operation. The organic phase was separated with 150 mL of approximately 0.001 mol / L hydrochloric acid and with 150 mL of pure water (twice). After the solvent was distilled off under reduced pressure at 30°C, the residue was purified with a silica gel column to obtain 3.0 g (22 mmol) of 4-vinylcatechol.

[0120] (Graft copolymerization process) Under nitrogen flow, 25.0 g of the same base polymer (LLDPE) as in Example 1 and 110 mL of xylene were charged into a 500 mL glass vessel, and the internal temperature was raised to 110° C. to dissolve the base polymer. 1.9 g (14 mmol) of 4-vinylcatechol obtained above was dissolved in 3 mL of 2-butanone and added to the glass vessel, and then 3.9 g (22 mmol) of Perbutyl I (t-butylperoxyisopropyl monocarbonate) diluted with 10 mL of xylene was slowly added dropwise. The mixture was stirred for 3 hours at a stirring speed of 400 rpm using a single anchor impeller (150 mL of xylene was added 30 minutes after the start of the reaction). Then, 50 mL of xylene was added, the temperature was raised again to 120°C, and the temperature was lowered to 50°C at 300 rpm. The suspension of graft copolymer 8 was transferred to a 1000 mL beaker containing 400 mL of acetone, subjected to ultrasonic treatment for 30 minutes, and filtered. Furthermore, ultrasonic treatment for 30 minutes using 500 mL of acetone was repeated three times, and the obtained graft copolymer was dried under reduced pressure at room temperature for 12 hours under a nitrogen flow. IR spectrum measurement revealed that the OH stretching vibration of the graft monomer (3580 cm -1 ) was observed and the graft amount was calculated to be 0.083 mmol / gP.

[0121] [Comparative Example 4] <Graft copolymer 9> Under nitrogen flow, 25.0 g of the same base polymer (LLDPE) as in Example 1 and 110 mL of xylene were placed in a 500 mL glass container, and the internal temperature was raised to 120° C. to dissolve the base polymer. Immediately after adding 2.2 g (22 mmol) of maleic anhydride, 0.26 g (1.54 mmol) of Perbutyl I (t-butylperoxyisopropyl monocarbonate) diluted with 10 mL of xylene was slowly added dropwise.

[0122] The mixture was stirred at a stirring speed of 400 rpm for 3 hours using a single anchor blade. Then, 200 mL of xylene was added, the temperature was raised again to 120°C, and the temperature was lowered to 60°C at 300 rpm to precipitate the graft copolymer. The precipitated suspension of the graft copolymer was transferred to a 1000 mL beaker containing 400 mL of acetone, stirred for 20 minutes, and then filtered. The organic phase was washed twice with 400 mL of acetone for 20 minutes, and the obtained graft copolymer was dried under reduced pressure at 90°C for 12 hours under nitrogen flow.

[0123] The obtained graft copolymer 1 H-NMR (solvent: 1,1,2,2-tetrachloroethane, measurement temperature: 120° C.) was measured, and the graft amount of 0.10 mmol / gP was calculated from the signal integral value of the maleic anhydride ring of the graft monomer.

[0124] [Adhesion rating 3] <Press sheet and adhesive sheet production> Graft copolymers 8-9 were press molded under the conditions of a temperature of 170°C, a pressure of 4 MPa, a preheating time of 8 minutes, and a pressurizing time of 3 minutes, and then quenched in a press molding machine set to 20°C over 3 minutes to obtain a press sheet having a thickness of 500 μm, a length of 80 mm, and a width of 80 mm. A Teflon (registered trademark) sheet (0.2 mm thick) was used as the release film. The press sheet was cut to a width of 20 mm to obtain an adhesive sheet (L).

[0125] (Adhesion method) As the substrate layer, a polyethylene terephthalate (PET) resin sheet (Mitsui PET J005PC, manufactured by Mitsui Chemicals, Inc.) (Q) having a thickness of 50 μm, a length of 80 mm and a width of 20 mm was used.

[0126] A PET resin sheet (Q layer), an adhesive sheet (L layer), and a PET resin sheet (Q layer) were stacked in that order, and the three-layer laminate was sandwiched between Teflon (registered trademark) (PTFE) sheets (thickness: 100 μm). Both the upper and lower press plates were heat sealed using a heat seal tester under the following conditions: heat seal temperature: 200°C, heat seal time: 3 to 10 seconds, heat seal pressure: 0.15 MPa, to produce a three-layer laminate structure (T) consisting of a PET resin sheet and an adhesive sheet.

[0127] Peel test The average peel strength between the Q layer and the L layer of the laminated structure was determined by T-peel at a peel speed of 300 mm / min and a peel width of 15 mm. The average values ​​and standard errors of the peel strengths obtained in 4 to 5 peel tests are shown in Table 3.

[0128] [Table 3]

[0129] [Adhesion rating 4] Except for changing the base layer to an ABS resin sheet (manufactured by Techno UMG Co., Ltd., UMG ABS EX18A) with a thickness of 100 μm, length of 80 mm, and width of 20 mm, changing the heat seal temperature to 230° C., and changing the heat seal time to 5 to 20 seconds, the press sheet, adhesive sheet, and three-layer laminate structure were prepared, and a peel test was performed in the same manner as in adhesion evaluation 3. The average values ​​and standard errors of the peel strengths obtained in the peel test are shown in Table 4.

[0130] [Table 4]

[0131] [Adhesion rating 5] Except for changing the base layer to an ETFE resin sheet (manufactured by AS ONE Corporation) with a thickness of 50 μm, a length of 80 mm, and a width of 20 mm, changing the heat seal temperature to 260°C, and changing the heat seal time to 10 to 30 seconds, the press sheet, adhesive sheet, and three-layer laminated structure were prepared, and a peel test was performed in the same manner as in adhesion evaluation 3. The average values ​​and standard errors of the peel strengths obtained in the peel test are shown in Table 5.

[0132] [Table 5]

[0133] [Adhesion rating 4] Except for changing the base layer to a polycarbonate resin sheet (manufactured by Mitsubishi Engineering Plastics Corporation, NOVAREX 7025IR) with a thickness of 100 μm, length of 80 mm, and width of 20 mm, changing the heat seal temperature to 270° C., and changing the heat seal time to 5 to 20 seconds, the press sheet, adhesive sheet, and three-layer laminated structure were prepared and a peel test was performed in the same manner as in adhesion evaluation 3. The average values ​​and standard errors of the peel strengths obtained in the peel test are shown in Table 6.

[0134] [Table 6]

Claims

1. The polymer has a main chain portion made of polyolefin (A) and a graft portion, The graft portion is derived from an aromatic monomer (B) represented by the following general formula (1), or is formed by graft copolymerizing a monomer in which a hydroxy group in the aromatic monomer (B) represented by the following general formula (1) is protected with a protecting group onto the main chain portion, and then deprotecting the hydroxy group after the graft copolymerization. Graft copolymer (X). 【Chemistry 1】 (In formula (1), * represents a group containing an unsaturated group that can be grafted to the main chain portion, r is an integer from 0 to 2; n is an integer from 2 to 5 when r=0, an integer from 2 to 7 when r=1, and an integer from 2 to 9 when r=2; R T is a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 30 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, a halogen atom, a nitro group, an amino group, a carboxy group, or a thiol group. The alkyl group, the aryl group, and the alkenyl group may be bonded to the aromatic ring via an oxygen atom or directly. R T When there are a plurality of them, they may be the same or different. In addition, at least two of the hydroxy groups are present at adjacent positions on the aromatic ring.

2. The amount of the grafted portion is 0.01 to 1.5 mmol / g-P (mmol / g-P represents the amount of the grafted portion per 1 g of the grafted copolymer (X)).

3. The graft copolymer (X) according to claim 1 or 2, wherein the aromatic monomer (B) is vinylcatechol.

4. A laminate comprising a film containing an adhesive resin and a film containing a resin other than the adhesive resin, the adhesive resin containing the graft copolymer (X) according to claim 1.

5. The laminate according to claim 4, wherein the resin other than the adhesive resin is a fluorine-containing resin, an ABS resin, a polyethylene terephthalate resin or a polycarbonate resin.

Citation Information

Patent Citations

  • Acrylic resin, and adhesive composition, adhesive, adhesive film, adhesive for masking, and adhesive film for masking including the same

    JP2022135585A