Fluororesin composition and fluororesin molding
A fluororesin composition with specific spherical carbon and inorganic fillers addresses the issues of high linear expansion and friction in labyrinth seals, providing improved machining and sliding properties for precise sealing applications.
Patent Information
- Application Number
- JP2024038197
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-12
- Publication Date
- 2024-10-15
AI Technical Summary
Existing fluororesin compositions containing PTFE and spherical carbon, used in bearings and sealing members, have insufficient friction properties and wear resistance when applied to stationary parts of labyrinth seals, and precise machining is difficult due to high linear expansion coefficients.
A fluororesin composition comprising a predetermined fluororesin, spherical carbon particles with a D50 particle size of 1 to 100 μm, and spherical inorganic fillers with a D50 particle size of 0.01 to 1 μm, with specific volume percentages, ensuring a low linear expansion coefficient, toughness for machining, and improved sliding properties.
The composition forms a molded article with a low linear expansion coefficient, high toughness for machining, and excellent sliding properties, enhancing the sealing performance of labyrinth seals and other applications.
Smart Images

Figure 2024146798000003 
Figure 2024146798000001 
Figure 2024146798000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a fluororesin composition and a fluororesin molded article. [Background technology]
[0002] Conventionally, PTFE resin compositions containing polytetrafluoroethylene (PTFE) and spherical carbon have been known as materials for constituting, for example, sliding materials used in bearings and sealing members used in hydraulic steering devices and hydraulic shock absorbers (Patent Documents 1 to 3).
[0003] Patent Document 1 describes a PTFE resin composition consisting of PTFE and spherical carbon, and the resin composition is said to have excellent sliding properties and elongation properties, and a low linear expansion coefficient.
[0004] Patent Document 2 describes a sealing member based on PTFE and containing spherical carbon. Unlike conventional carbon fibers, spherical carbon has no edges and is therefore less aggressive to mating materials, and its appropriate surface hardness is said to improve relative abrasion resistance.
[0005] Patent Document 3 describes that the piston seal of a hydraulic shock absorber is made by filling 100 parts by weight of Teflon (registered trademark) base material with 5 to 30 parts by weight of spherical carbon with a particle size of 5 to 50 μm. This piston seal is said to be able to reduce the increase in sliding friction over time and to double the wear resistance compared to cases where conventional fillers such as carbon fiber are used.
[0006] The applicant has also proposed a fluororesin molded body as a material for forming the stationary part of, for example, a rotating shaft and stationary part that form a labyrinth seal (Patent Document 4). This fluororesin molded body is made of a fluororesin composition containing a specific fluororesin such as PTFE and an inorganic filler, and this fluororesin composition contains, as the inorganic filler, fused silica not coated with a silane film and having a D50 particle size of 0.01 to 1 μm, etc., in an amount of 40 to 70% by volume relative to the entire composition. Such a fluororesin molded body has a linear expansion coefficient of a specific value or less and has a strength that is acceptable for practical use. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2002-161181 A [Patent Document 2] JP 2000-38568 A [Patent Document 3] JP 2000-104829 A [Patent Document 4] Patent Publication No. 2022-175901 Summary of the Invention [Problem to be solved by the invention]
[0008] It has been found that various sealing members made of fluororesin compositions containing PTFE and spherical carbon described in Patent Documents 1 to 3 have improved linear expansion coefficients, but when applied to stationary parts of labyrinth seals, for example, the wear resistance and friction are not necessarily sufficient, and further improvement of the sliding characteristics may be required. In addition, the fluororesin molded product made of the fluororesin composition described in Patent Document 4 has a linear expansion coefficient of a predetermined value or less and a practically acceptable strength as described above, and can be used as a stationary part in a labyrinth seal in combination with a rotating shaft having a low linear expansion coefficient. However, it has been found that improvement of toughness is required to perform precise and complex machining on the stationary part in order to make the structure of the gap formed between the rotating shaft and the stationary part precise and complex in order to improve the performance of the labyrinth seal, for example.
[0009] Therefore, an object of the present invention is to provide a fluororesin composition capable of forming a molded article having a small linear expansion coefficient in the range from room temperature to high temperatures, toughness enabling machining, and good sliding properties, and a fluororesin molded article formed using the fluororesin composition. [Means for solving the problem]
[0010] The present inventors have conducted extensive research to solve the above-mentioned problems. As a result, they have found that the above-mentioned problems can be solved by a fluororesin composition containing a specified fluororesin, a specified spherical inorganic filler, and a specified amount of specified spherical carbon particles. The gist of the present invention is as follows.
[0011] The first aspect of the present invention is a melt viscosity of 10 10 The present invention relates to a fluororesin composition comprising a fluororesin having a viscosity of Pa sec or more, spherical carbon particles (excluding graphite particles) having a D50 particle size of 1 to 100 μm, and a spherical inorganic filler (excluding carbon-based inorganic filler) having a D50 particle size of 0.01 to 1 μm, wherein the content of the spherical carbon particles is 10 vol% or more and 55 vol% or less of the entire fluororesin composition.
[0012] In an embodiment of the present invention, the fluororesin composition may contain 30% by volume or more and 50% by volume or less of the fluororesin and 10% by volume or more and 40% by volume or less of the spherical inorganic filler.
[0013] In an embodiment of the present invention, the spherical carbon particles may have a sphericity of 0.9 or more.
[0014] In an embodiment of the present invention, the spherical inorganic filler may be fused silica.
[0015] In an embodiment of the present invention, the fluororesin may be polytetrafluoroethylene produced by an emulsion polymerization method.
[0016] In an embodiment of the present invention, the fluororesin composition may contain 0 to 10% by volume of flaky graphite.
[0017] A second aspect of the present invention is a fluororesin molded article made of the above-mentioned fluororesin composition, The linear expansion coefficient of the fluororesin molded product at 25°C to 90°C is 40 ppm (4.0 × 10 -5 ) / K or less, compressive fracture strain is greater than 55%, and the specific wear rate is 4.0×10 -6 mm 3 / N·m or less.
[0018] In the present invention, the features of the above-described embodiments can be arbitrarily combined. Effect of the Invention
[0019] Effects of the Invention The present invention can provide a fluororesin composition capable of forming a molded article having a small linear expansion coefficient in the range from room temperature to high temperatures, toughness enabling machining, and good sliding properties, and a fluororesin molded article formed using the fluororesin composition. [Brief description of the drawings]
[0020] [Figure 1]FIG. 1 is a diagram showing the configuration of a pin-on-disk type friction and wear tester. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Hereinafter, an embodiment of the present invention will be described. The fluororesin composition according to the embodiment of the present invention has a melt viscosity of 10 10 The fluororesin composition includes a fluororesin having a viscosity of Pa·sec or more (hereinafter, may be simply referred to as "fluororesin"), spherical carbon particles (excluding graphite particles) having a D50 particle size of 1 to 100 μm (hereinafter, may be simply referred to as "carbon particles" or "spherical carbon particles"), and a spherical inorganic filler (excluding carbon-based inorganic filler) having a D50 particle size of 0.01 to 1 μm (hereinafter, may be simply referred to as "inorganic filler" or "spherical inorganic filler"). The content of the spherical carbon particles is 10 volume % or more and 55 volume % or less in the entire fluororesin composition. Here, the volume % adopted as the content of the components contained in the fluororesin composition can be calculated, for example, from the density (specific gravity) of the components used and the blending amount thereof.
[0022] The specific fluororesin contained in the fluororesin composition is a resin that becomes a matrix when the fluororesin is made into a fluororesin molded product (hereinafter, sometimes simply referred to as a "molded product"). 10Any material having a viscosity of Pa·sec or more may be used, and examples thereof include polytetrafluoroethylene (PTFE). PTFE generally has high heat resistance, a small coefficient of friction, excellent chemical resistance, and the like, and has the property that it does not burn even when in contact at high speed, and is therefore suitable, for example, as a constituent material of a sealing member for a metal rotating shaft of a rotating device. In particular, it is suitable as a matrix resin material for constituting a labyrinth seal for a metal rotating shaft. PTFE obtained by a known manufacturing method can be used, and examples thereof include fine powder (emulsion polymerization product) produced by emulsion polymerization and molding powder (suspension polymerization product) produced by suspension polymerization. Among these, PTFE produced by emulsion polymerization is preferred, since it tends to fibrillate when the components are mixed, increasing the adhesion between PTFE particles, and making it easier to uniformly hold spherical carbon particles and spherical inorganic fillers in the PTFE matrix.
[0023] The content of the predetermined fluororesin in the entire fluororesin composition is not particularly limited, but is preferably 30% by volume to 50% by volume, and more preferably 35% by volume to 45% by volume. When the content of the fluororesin is within this range, the properties of the fluororesin and other components can be satisfactorily exhibited, and a fluororesin molded product having better strength, sliding properties, and a lower linear expansion coefficient can be obtained.
[0024] The melt viscosity of the fluororesin can be measured, for example, in accordance with ASTM D 1238 using a flow tester (manufactured by Shimadzu Corporation).
[0025] The spherical carbon particles contained in the fluororesin composition are spherical with a D50 particle size of 1 to 100 μm, and are not graphite particles. Since the spherical shape has a smaller specific surface area than non-spherical ones, the content can be increased to 10% by volume or more and 55% by volume or less in the entire fluororesin composition, and the carbon particle surface can be efficiently wetted during molding even with the above-mentioned fluororesin having a high melt viscosity. As a result, the carbon particles are uniformly dispersed in the fluororesin, and the strength and toughness of the molded body can be improved. In addition, the thermal expansion of the molded body can be made isotropic, so that the dimensional change of the molded body used in a room temperature to high temperature environment can be suppressed. In addition, the molded body containing the spherical carbon particles is less aggressive to the mating member during sliding. Furthermore, the spherical carbon particles do not contain graphite particles. Graphite has a layered structure of hexagonal plate-like crystals in the shape of a tortoise shell, and the strength between each layer is weak, so that peeling is likely to occur. A fluororesin molded product containing graphite particles, which are aggregates of graphite, tends to have low strength and toughness due to the low interlayer strength of the graphite crystals, and when the graphite particles are highly filled in the entire fluororesin composition at more than 10 volume %, the sliding properties of the molded product tend to be poor. However, as described below, from the viewpoint of adjusting the sliding properties of the molded product, graphite may be contained as a solid lubricant in an amount not exceeding 10 volume % of the entire fluororesin composition.
[0026] The D50 particle size of the spherical carbon particles may be 1 to 100 μm, and more preferably 1 to 20 μm. By setting it in this range, high loading becomes possible. The D50 particle size can be measured, for example, by a laser diffraction / scattering method.
[0027] The spherical carbon particles may have the above-mentioned characteristics, but from the viewpoint of further improving the isotropy of thermal expansion and further reducing the linear expansion coefficient, the sphericity is preferably 0.90 or more, and more preferably 0.95 or more. Specifically, the sphericity is calculated by taking a photograph with a scanning electron microscope (SEM), and using the area and perimeter of the observed particle, (sphericity) = {4π × (area) ÷ (perimeter)} 2The closer the sphericity is to 1, the closer it is to a perfect sphere. The area and perimeter values used to calculate the sphericity can be average values measured for 100 particles using an image processing device, for example.
[0028] As described above, the spherical carbon particles have a structure that is not a crystalline structure that is prone to layer peeling like graphite particles, but it is preferable that the structure is amorphous. Such amorphous carbon particles include, for example, those obtained by carbonizing phenolic resin particles, as described in Patent Document 2. The amorphous carbon particles obtained in this way have a sphericity close to 1 and a narrow particle size range, so that it is possible to more effectively suppress the anisotropy of the thermal expansion of the molded body. In addition, since they have good surface hardness, the strength of the molded body can be improved.
[0029] From the viewpoint of high packing ability for suppressing thermal expansion of the molded body and further suppressing anisotropy of compression fracture strain, the spherical carbon particles preferably have a sphericity close to 1 and a smooth surface.
[0030] The spherical carbon particles preferably have reactive functional groups such as hydroxyl groups and carboxyl groups on their surfaces. When such reactive functional groups are present, the wear powder of the spherical carbon particles and the transfer film containing the fluororesin formed on the sliding surface of the counter material during sliding of the molded body adhere firmly to the counter material, and the lubricating effect can be more effectively exhibited. The amorphous carbon particles obtained by carbonizing the above-mentioned phenolic resin particles are also preferable in that they have such functional groups.
[0031] The spherical carbon particles obtained by carbonizing phenolic resin particles can be commercially available, for example, GCP manufactured by Unitika Ltd., and Bellpearl C800 and C2000 manufactured by Air Water Bellpearl Co., Ltd.
[0032] The spherical carbon particles are preferably not coated with a coating that can be gasified during melt molding, such as a silane coating as described in Patent Document 4. This makes it possible to suppress the generation of voids due to gas derived from a gasifiable coating such as a silane coating during melt molding using a fluororesin composition. As a result, it becomes possible to obtain a molded product having a dense high-order structure in which the spherical carbon particles are highly packed in the fluororesin, and the linear expansion coefficient of the molded product can be further reduced.
[0033] From the viewpoint of improving the sliding properties, particularly the wear resistance, of the molded body, the content of the spherical carbon particles is from 10 volume % to 55 volume % of the entire fluororesin composition, and more preferably from 10 volume % to 45 volume %.
[0034] The spherical inorganic filler contained in the fluororesin composition is spherical with a D50 particle size of 0.01 to 1 μm and is not carbon-based. Also, fibrous inorganic fillers are not included. The spherical inorganic filler can be uniformly dispersed in the fluororesin matrix and the anisotropy of thermal expansion of the molded body can be suppressed. In addition, by using this spherical inorganic filler in combination with granular carbon particles, the anisotropy of thermal expansion of the molded body due to the granular carbon particles is suppressed, the effect of improving the toughness of the molded body is maintained, and the effect of improving the wear resistance and low friction is obtained. The shape of the spherical inorganic filler may be spherical, but from the viewpoints of uniform dispersion in the fluororesin matrix, high filling property, isotropy of thermal expansion of the molded body, etc., it is preferable that the shape is close to a true sphere. As a standard for true sphere, the same sphericity as that of spherical carbon particles can be used. The sphericity of the spherical inorganic filler is preferably 0.80 or more, more preferably 0.85 or more, even more preferably 0.90 or more, and most preferably 0.95 or more.
[0035] Materials constituting the spherical inorganic filler include silica, mica, talc, glass spheres, metal particles, metal oxides, ceramic spheres, etc. Among these, silica is preferred from the viewpoint of improving the sliding properties of the molded body, particularly the wear resistance, reducing the linear expansion coefficient of the molded body, and uniform dispersion in the fluororesin. Silica may be crystalline or non-crystalline, but since particles with a sphericity close to 1 can be easily obtained, non-crystalline silica is more preferred, and fused silica is even more preferred.
[0036] Moreover, from the same viewpoint as the spherical carbon particles described above, it is preferable that the spherical inorganic filler is not covered with a coating that can be gasified during melt molding.
[0037] The D50 particle size of the spherical inorganic filler may be 0.01 to 1 μm, and more preferably 0.01 to 0.85 μm. By setting it in such a range, high loading becomes possible. The D50 particle size of the spherical inorganic filler can be measured, for example, by a laser diffraction / scattering method.
[0038] As the spherical inorganic filler, commercially available products can be used. An example of fused silica is SFP30M manufactured by Denka Co., Ltd.
[0039] From the viewpoints of abrasion resistance and low friction, the content of the spherical inorganic filler is preferably from 10 to 40% by volume, and more preferably from 15 to 35% by volume, of the entire fluororesin composition.
[0040] From the viewpoint of uniform dispersion in the fluororesin, the spherical carbon particles and the spherical inorganic filler preferably have a specific gravity close to that of the fluororesin. That is, the specific gravity of the spherical carbon particles and the spherical inorganic filler (A) is preferably close to that of the fluororesin (B), and the ratio of the specific gravities (A / B) is preferably 0.7 to 1.5.
[0041] Other components may be added to the fluororesin composition according to the embodiment, as long as the effects of the present invention are not impaired. Examples of such components include graphite, fibrous inorganic fillers, dispersing agents, colorants, etc.
[0042] Graphite functions as a so-called solid lubricant and is different from the spherical carbon particles and spherical inorganic fillers described above. The sliding properties (e.g., low friction, wear resistance, machinability) of the molded body can be adjusted by graphite. From the viewpoint of the strength of the molded body, the size of the graphite is preferably a D50 particle diameter (including the measured value when it is not spherical) of 1 to 50 μm. Examples of the shape of graphite include scaly and spherical. Among these, scaly graphite is preferred from the viewpoint of low friction and wear resistance.
[0043] From the viewpoint of wear resistance and low friction, the content of graphite is preferably 0% by volume or more and 10% by volume or less in the entire fluororesin composition. When graphite is added, the lower limit should be greater than 0% by volume. However, since the strength of the molded body tends to decrease, the graphite content is adjusted so that the compression fracture strain (average) of the molded body described later is greater than 55%, for example.
[0044] The fibrous inorganic filler is used to improve the strength and sliding properties of the molded body. Examples of such fibrous inorganic fillers include carbon fiber, glass fiber, metal fiber, whisker, etc. From the viewpoint of wear resistance, carbon fiber is preferred.
[0045] From the viewpoint of abrasion resistance, the content of the fibrous inorganic filler is preferably 0 to 20% by volume in the entire fluororesin composition. When added, the lower limit may be greater than 0% by volume.
[0046] The fluororesin composition can be obtained by mixing the above-mentioned components to a desired volumetric content and stirring with a stirrer. The stirrer is not particularly limited, but from the viewpoint of uniform dispersion of each component, one with strong stirring power is preferred, for example, a Henschel mixer, a juicer mixer (laboratory blender), a super mixer, etc. The properties of the fluororesin composition are appropriately determined according to the properties of each component and the conditions during mixing, etc., but from the viewpoint of ensuring a good mixing state of each component and from the viewpoint of uniform dispersion of each component during melt molding, it is preferable that it is in a powder form. When obtaining such a powder-like fluororesin composition, it is preferable to use each component in a powder form, and it is preferable to adjust the temperature so that each component can be maintained in a powder form during stirring. In addition, it is preferable to use each component in a powder form with a similar specific gravity. The volumetric content of each component can be calculated from the mass of each component added and the density of each component as described above. In addition, the volumetric content of each component in the fluororesin composition is maintained in the molded product.
[0047] The fluororesin molded article according to the embodiment is, for example, a molded article molded using the above-mentioned fluororesin composition. Then, for example, by manufacturing it by the method described later, it is possible to obtain a molded article having a linear expansion coefficient and specific wear amount below a predetermined value, and a compression breaking strain greater than a predetermined value. In addition, the molded article can have good low friction properties. Here, the linear expansion coefficient can be measured by a method conforming to JIS K7197, for example, as described later. In addition, the compression breaking strain is an index of the toughness of the molded article, and can be measured by, for example, performing a compression test (compression speed 5 mm / min) in accordance with JIS K7181, as described later. The wear resistance and low friction properties can be evaluated by, for example, performing a friction wear test using a pin-on-disk type friction wear tester shown in FIG. 1 to measure the specific wear amount, a predetermined wear time, and a friction coefficient. The pin-on-disk friction and wear tester shown in FIG. 1 is configured so that a pin sample (e.g., a cylindrical test piece made of a fluororesin molded body) is pressed against a rotating mating disk (e.g., made of a metal plate with a specified surface roughness) with a desired load adjusted using a weight, the generated friction force is measured with a load cell, and the amount of wear can be measured over time with a displacement meter.
[0048] The fluororesin molded article can be produced, for example, by hot press molding, which is characterized in that the above-mentioned fluororesin composition is pressurized in a molten state and then cooled and solidified under pressure as described below.
[0049] First, the desired fluororesin composition is filled into, for example, a compression molding die, and compressed at room temperature at a predetermined pressure for a predetermined time using a compression press, and then the pressure is released (premolding process). In the free sintering method, the premolded product is then released from the mold and placed in a heating furnace, but when the above-mentioned fluororesin composition is used, it is difficult or impossible to maintain the shape. However, by carrying out the following process, it is possible to finally maintain the shape, and it is possible to impart the desired sliding properties such as linear expansion coefficient, compression fracture strain, and specific wear rate.
[0050] After the preforming step, the compression molding die filled with the fluororesin composition and decompressed is placed in a heating furnace heated to a temperature equal to or higher than the melting point of the fluororesin, or a band heater is wrapped around the outer periphery of the die, and the fluororesin in the compression die is heated for a predetermined time to bring the die into a molten state (in-mold heating and melting step). When a heating furnace is used, it is sufficient if it can uniformly heat the die, and for example, a hot air circulation furnace or the like can be used.
[0051] Next, the compression molding die is removed from the heating furnace while the fluororesin is still in a molten state, or the band heater is removed and immediately installed in a compression press, and pressure is started at room temperature at a pressure equal to or greater than the pressure during the preforming process, and after the die temperature reaches 150°C or less, the pressure is released and the die is demolded (compression molding process). After cooling to room temperature, it can be machined into a desired shape. In this way, by cooling and solidifying a fluororesin composition containing a specific fluororesin in a molten state under pressure, the fluororesin spreads around the highly filled spherical carbon particles and spherical inorganic filler without any gaps, and the spherical carbon particles and spherical inorganic filler are firmly held in the fluororesin matrix, and it is considered that a molded body having toughness that can be machined and capable of maintaining its shape can be obtained. When the fluororesin is PTFE, it is considered that the desired molded body can be obtained by good fusion between PTFE particles.
[0052] The above-mentioned fluororesin molded article has a low linear expansion coefficient of a predetermined value or less, so that dimensional change due to heating can be suppressed, and the compressive fracture strain is greater than a predetermined value, i.e., it has good toughness that allows machining. Therefore, for example, in a labyrinth seal, the structure of the gap formed by the rotating shaft and the stationary part can be made precise and complex, and the effect of improving the sealing property by making it precise and complex can be enjoyed. In addition, it can be applied to various applications in which it is used in combination with a rotating shaft having a linear expansion coefficient lower than that of the stationary part. Since it contains a predetermined fluororesin as a matrix resin, it is suitable as a seal member or sliding material for various rotating devices, etc., and is suitable as a seal member for the metal rotating shaft of the rotating device, particularly as a seal member constituting a labyrinth seal. In the rotating device, it is suitable as a seal member for a turbo compressor. EXAMPLES
[0053] Hereinafter, the embodiments of the present invention will be described in more detail with reference to examples. The D50 particle size and sphericity of each component used in the examples and comparative examples were measured by the methods described above.
[0054] Example 1 Fluoroplastic resin: PTFE (manufactured by Mitsui Chemours Fluoroproducts Co., Ltd., Teflon (registered trademark) 641-J, polymerized by emulsion polymerization method, fine powder, melt viscosity: 10 12 The mixture was mixed so that the volume percentage of the silica (manufactured by Denka Company Limited, SFP-30M, fused silica, D50 particle size: 0.7 μm, specific gravity: 2.2, sphericity: 0.95-1.0) as a spherical inorganic filler was 10% by volume, and stirred for 4 minutes in a small laboratory blender to obtain a powdered fluororesin composition in which the components were uniformly mixed.
[0055] The obtained fluororesin composition was put into a cavity of a compression molding die of φ42 mm so that the molding height after compression in preforming was 40 mm, and preforming was performed in a compression press at room temperature and molding pressure of 10 MPa, and then the die filled with the fluororesin composition was heated to 360°C under normal pressure and held for 2 hours to melt the PTFE. Next, the PTFE was in a molten state and cooled in a compression press under pressure of 30 MPa until the die temperature was 150°C or less, and then demolded to obtain a fluororesin molded article. The obtained fluororesin molded article was used for the evaluation described below.
[0056] (Examples 2 to 5, Comparative Examples 1 to 3 and 5) A fluororesin composition was prepared in the same manner as in Example 1, except that the components were mixed to obtain the composition shown in Table 1. A fluororesin molded product was then produced from the fluororesin composition and evaluated as described below.
[0057] Comparative Example 4 A fluororesin composition was prepared in the same manner as in Example 1, except that the components were mixed to obtain the composition shown in Table 1. An attempt was then made to produce a fluororesin molded article from the fluororesin composition, but no molded article could be produced, and therefore the evaluation described below could not be performed.
[0058] (Examples 6 to 15, 18, and 19) A fluororesin composition was prepared in the same manner as in Example 1, except that the components were blended to obtain the composition shown in Table 2 and stirred for 4 minutes in a small laboratory blender. A fluororesin molded product was then produced from the fluororesin composition and evaluated as described below.
[0059] (Examples 16 and 17) A fluororesin composition was prepared in the same manner as in Example 1, except that each component was mixed to obtain the composition shown in Table 2, and stirred for 23 minutes in a super mixer (manufactured by Kawata Corporation, model SMV(G)-100, capacity 100 L). The obtained fluororesin composition was charged into a cavity of a compression molding die having a diameter of 240 to 480 mm so that the molding height after compression in preforming was 70 to 80 mm, and preforming was performed in a compression press at room temperature and a molding pressure of 10 MPa, and then, in a state in which the fluororesin composition was filled in the die, it was heated to 360°C under normal pressure and held for 5 to 6 hours to melt the PTFE. Next, in a compression press with the PTFE in the molten state, it was cooled to a die temperature of 150°C or less while pressurized to 30 MPa, and then demolded to obtain a fluororesin molded article. The obtained fluororesin molded article was used for the evaluation described below.
[0060] (Example 20) Instead of emulsion polymerization PTFE, suspension polymerization PTFE (manufactured by Mitsui-Chemours Fluoroproducts Co., Ltd., Teflon (registered trademark) 7J, molding powder, melt viscosity: 10 12 A fluororesin composition was prepared in the same manner as in Example 6, except that a fluororesin composition was used (polyoxyethylene terephthalate, specific gravity: 2.2 Pa·sec). A fluororesin molded product was then produced from the fluororesin composition and evaluated as described below.
[0061] (evaluation) <Measurement of linear expansion coefficient> The linear expansion coefficient (also referred to as the linear expansion rate) was measured in accordance with JIS K7197. Test pieces of φ5 mm×10 mm were prepared by machining from the fluororesin molded products of Examples 1 to 20 and Comparative Examples 1 to 3 and 5. Next, using a thermomechanical measuring device (Hitachi High-Tech Science Corporation, TMA / SS6100), the linear expansion coefficients in the compression direction (MD) and the perpendicular direction (CD) to the compression direction during molding of the molded product were measured when the temperature was increased at 5° C. / min, and the average value of both was taken as the linear expansion coefficient. In the measurement, the linear expansion coefficient was calculated from the linear expansion amount in the range of 25° C. to 90° C. out of the data measured in the temperature range of −120° C. to 300° C. In the case where the linear expansion coefficient was 40 ppm (4.0×10 -5) / K or less was considered a pass.
[0062] <Compression fracture strain measurement> Compression properties were measured according to JIS K7181. Test pieces of φ8mm×20mm were prepared by machining from the fluororesin molded bodies of Examples 1 to 20 and Comparative Examples 1 to 3 and 5, and compression tests were performed in the MD and CD directions at a test speed of 5mm / min using an autograph AG-X plus (equipped with pressure plates) manufactured by Shimadzu Corporation. The value (%) obtained by dividing the amount of strain (the amount of reduction in the distance between the pressure plates) when the test piece placed between the pressure plates broke by the initial distance between the pressure plates was taken as the compression fracture strain. The average value of the compression strain in the MD and CD directions was adopted as the compression fracture strain of the test piece, and when this average value was greater than 55%, it was deemed to have good strength, especially toughness, and was considered to have passed.
[0063] <Friction and wear test> Test pieces of φ5 mm×10 mm were prepared by machining for each of the fluororesin molded articles in the MD and CD directions of Examples 1 to 20 and Comparative Examples 1 to 3 and 5. Next, a pin-on-disk friction and wear tester (Auto Pin Disk APD-101, manufactured by Starlite Industrial Co., Ltd.) having the configuration shown in Fig. 1 was used to perform a pin-on-disk test under the conditions shown below to determine the friction coefficient, specific wear rate, and time required for the test pieces to wear down by 1 mm. Here, the average values of the measured values in the MD and CD directions were used. Counter disc: SUS304 (Ra=0.3μm) Speed: 3m / sec Load: 1MPa Temperature: room temperature Lubrication: No lubrication Test time: 24 hours or until the wear height exceeds 1 mm
[0064] The specific wear rate was calculated by the following formula. Specific wear rate = wear volume / load x sliding distance
[0065] The smaller the friction coefficient, the better. A value of 0.50 or less was deemed practical, and a value of 0.40 or less was deemed good. The smaller the specific wear rate, the better. -6 mm 3 / N·m or less was rated as good. The longer the time it took for the test piece to wear down by 1 mm, the better, and 24 hours or more was rated as good.
[0066] The compositions and evaluation results of the fluororesin compositions of the examples and comparative examples are shown in Tables 1 and 2. The test time for the friction and wear test is the time when the test piece was worn down by 1 mm (time until the test stopped). If the wear height was less than 1 mm after 24 hours of testing, it was marked as ">24."
[0067] [Table 1]
[0068] As shown in Table 1, when the fluororesin compositions of Examples 1 to 5 were used, the average linear expansion coefficients in the MD and CD directions of the fluororesin molded products were 39 ppm (×10 -6 ) / K or less, the compressive fracture strain (average value in MD and CD) is 58.5% or more, showing good toughness, and the friction coefficient is 0.36 or less, and the specific wear rate is 3.7×10 -6 mm 3 / N·m or less, and the time for the test piece to wear down by 1 mm exceeds 24 hours, it is clear that the test piece has good sliding properties. On the other hand, a fluororesin molded product could not be obtained in Comparative Example 4, and none of the fluororesin compositions in Comparative Examples 1 to 3 and 5 had fluororesin molded products with average linear expansion coefficients in MD and CD and compressive fracture strain (average values in MD and CD) within the specified ranges and good sliding properties like those of the Examples.
[0069] [Table 2]
[0070] As shown in Table 2, in Examples 16 and 17, which have the same composition as Examples 2 and 4, respectively, the mixer used in producing the fluororesin composition was changed from a small laboratory blender to a super mixer, but it can be seen that the molded articles obtained had evaluation results comparable to those of Examples 2 and 4. Also, it can be seen that in the case of Examples 9 to 15, which contain a predetermined amount of predetermined flaky graphite or carbon fiber in addition to the essential components used in Examples 1 to 3, etc. (PTFE (emulsion polymerization), silica, spherical carbon particles), a particular improvement in the specific wear rate can be expected. Furthermore, in Example 18, in which the PTFE composition ratio was reduced compared to Examples 1 to 8, the friction coefficient was high and the compression strain at break was low, while in Example 19, in which the PTFE composition ratio was increased, the friction coefficient was low and the compression strain at break tended to be high. Example 20, in which the fluororesin used as the matrix resin was changed from PTFE (fine powder) produced by emulsion polymerization to PTFE (molding powder) produced by suspension polymerization, which is widely used for molded products, exhibited properties comparable to those of Example 1 with the same composition ratio, but the thermal expansion coefficient was slightly higher.
Claims
1. Melt viscosity is 10 10 A fluororesin composition comprising a fluororesin having a viscosity of Pa·sec or more, spherical carbon particles (excluding graphite particles) having a D50 particle size of 1 to 100 μm, and a spherical inorganic filler (excluding carbon-based inorganic filler) having a D50 particle size of 0.01 to 1 μm, A fluororesin composition, wherein the content of the spherical carbon particles is 10% by volume or more and 55% by volume or less based on the entire fluororesin composition.
2. 2. The fluororesin composition according to claim 1, wherein the fluororesin composition contains 30% by volume or more and 50% by volume or less of the fluororesin and 10% by volume or more and 40% by volume or less of the spherical inorganic filler.
3. 3. The fluororesin composition according to claim 1, wherein the spherical carbon particles have a sphericity of 0.9 or more.
4. 3. The fluororesin composition according to claim 1, wherein the spherical inorganic filler is fused silica.
5. 3. The fluororesin composition according to claim 1, wherein the fluororesin is polytetrafluoroethylene prepared by an emulsion polymerization method.
6. 3. The fluororesin composition according to claim 1, wherein the flake graphite is contained in an amount of 0 to 10% by volume of the entire fluororesin composition.
7. A fluororesin molded article made of the fluororesin composition according to claim 1 or 2, The linear expansion coefficient of the fluororesin molded article at 25° C. to 90° C. is 40 ppm (4.0×10 -5 ) / K or less, compression fracture strain is greater than 55%, and specific wear rate is 4.0 x 10 -6 mm 3 / N·m or less.
Citation Information
Patent Citations
Sealing member
JP2000038568A
Piston seal material of hydraulic buffer
JP2000104829A
Polytetrafluoroethylene resin composition
JP2002161181A
Fluororesin molded article and production method thereof
JP2022175901A