Photocurable composition for adhesive sheet, adhesive sheet, optical laminate, and image display device

The photocurable composition with a specific photopolymerization initiator structure improves polymerization rate and reduces residual initiator content in adhesive sheets, addressing odor and stability issues.

JP2024146805APending Publication Date: 2024-10-15NITTO DENKO CORP

Patent Information

Application Number
JP2024039510
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-13
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Photocurable adhesive sheets have high residual monomer content, leading to odor issues and problems like yellowing and foaming, and increasing the photopolymerization initiator amount exacerbates these issues without adequately addressing polymerization rate and residual amount.

Method used

A photocurable composition for pressure-sensitive adhesive sheets incorporating a specific photopolymerization initiator with a defined chemical structure, which enhances polymerization rate while reducing residual initiator amount.

Benefits of technology

The solution achieves a high polymerization rate of 96% or more with a residual photopolymerization initiator content of 800 wtppm or less, minimizing yellowing and foaming, and maintaining adhesive strength over time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146805000001_ABST
    Figure 2024146805000001_ABST
Patent Text Reader

Abstract

To provide a photocurable composition suitable for improving the polymerization rate and reducing the residual content of a photopolymerization initiator during the formation of an adhesive sheet.SOLUTION: Provided is a photocurable composition for an adhesive sheet comprising monomers and / or a product of partial polymerization of the monomers, and a photopolymerization initiator. The photopolymerization initiator is a compound comprising a chemical structure represented by formula (1) below in its molecule.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photocurable composition for a pressure-sensitive adhesive sheet, a pressure-sensitive adhesive sheet, an optical laminate, and an image display device. [Background technology]

[0002] Various image display devices, such as liquid crystal display devices and electroluminescence (EL) display devices, generally include an optical laminate including an optical film such as a polarizing film and an adhesive sheet. An adhesive sheet is usually used for bonding between the optical films included in the optical laminate and bonding between the optical laminate and an image display panel. A typical adhesive sheet is a sheet obtained by curing a monomer group including an acrylic monomer, a silicone monomer, etc., by polymerization and crosslinking. Patent Document 1 discloses an adhesive sheet formed from a photocurable composition (hereinafter referred to as a photocurable adhesive sheet). Another type of adhesive sheet is an adhesive sheet formed by curing a layer including an adhesive composition and a solvent by heat (hereinafter referred to as a thermosetting adhesive sheet). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-70150 A Summary of the Invention [Problem to be solved by the invention]

[0004] In photocurable adhesive sheets, monomers tend to remain more easily than in thermosetting adhesive sheets. The remaining monomers may generate odors. In order to reduce the remaining amount, it is possible to increase the amount of photopolymerization initiator to improve the polymerization rate. However, according to the study by the present inventors, if the amount is simply increased, the amount of photopolymerization initiator remaining in the adhesive sheet increases, which may cause other problems such as yellowing and foaming. Conventionally, in photocurable compositions for forming adhesive sheets, both the polymerization rate and the remaining amount of photopolymerization initiator have not been sufficiently considered.

[0005] An object of the present invention is to provide a photocurable composition suitable for improving the polymerization rate and reducing the amount of residual photopolymerization initiator during the formation of a pressure-sensitive adhesive sheet. [Means for solving the problem]

[0006] The present invention relates to A photocurable composition for a pressure-sensitive adhesive sheet, comprising a monomer group and / or a partial polymer of the monomer group, and a photopolymerization initiator, The photopolymerization initiator is a compound having a chemical structure represented by the following formula (1) in its molecule: R in the above formula (1) 1 and R 2 are each independently a C1 to C8 alkyl group; -OH, a C1 to C4 alkoxy group, -CN, -COOR 51 , -OOCR 52 , or -NR 53 R 54 an alkyl group having 1 to 4 carbon atoms, the hydrogen atom of which is replaced by -CH2-C6H4-R; an alkenyl group having 3 to 6 carbon atoms, the hydrogen atom of which is replaced by -CH2-C6H4-R 55 and R 1 and R 2 may be bonded to each other to form a C2 to C9 alkylene group, a C3 to C6 oxyalkylene group, or an azaalkylene group, X is -OR 56 , or -NR 57 R 58 and R 51is a C1 to C8 alkyl group, R 52 is a C1 to C4 alkyl group, R 53 and R 54 are each independently a hydrogen atom, a C1-C12 alkyl group; -OH, a C1-C4 alkoxy group, -CN and -COOR 59 a C2-C4 alkyl group, the hydrogen atom of which is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; or a cyclohexyl group, R 53 and R 54 are bonded to each other to form -O- or -N(R 60 )-, and may be a C3 to C9 alkylene group optionally interrupted by -. R 55 is a C1 to C4 alkyl group, R 56 is a hydrogen atom, -SiR 62 3. A C1 to C8 alkyl group or a C3 to C6 alkenyl group; R 57 and R 58 represents an alkyl group having 1 to 12 carbon atoms; -OH, an alkoxy group having 1 to 4 carbon atoms, -CN and -COOR 63 a C2-C4 alkyl group, the hydrogen atom of which is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; or a cyclohexyl group, R 57 and R 58 are bonded to each other to form -O- or -N(R 64 )-, and may be a C3 to C9 alkylene group optionally interrupted by -. R 59 is a C1 to C4 alkyl group, R 60 is a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an allyl group, a hydroxyalkyl group having 1 to 4 carbon atoms, -CH2CH2-COOR 61 or -CHCHCN, R 61 is a C1 to C4 alkyl group, R 62is a C1 to C6 alkyl group, R 63 is a C1 to C4 alkyl group, R 64 is a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an allyl group, a hydroxyalkyl group having 1 to 4 carbon atoms, -CH2CH2-COOR 65 or -CHCHCN, R 65 is a C1 to C4 alkyl group, The chemical structure can be bonded to a hydrogen atom or a hydrogen atom-substituted structure via the carbon atom indicated by * in formula (1). A photocurable composition for pressure-sensitive adhesive sheets is provided.

[0007] [ka]

[0008] Further, the present invention relates to There is provided a pressure-sensitive adhesive sheet formed from the above photocurable composition.

[0009] Further, the present invention relates to There is provided an optical laminate comprising the above pressure-sensitive adhesive sheet and an optical film.

[0010] Further, the present invention relates to There is provided an image display device including the above optical laminate. Effect of the Invention

[0011] According to the present invention, it is possible to provide a photocurable composition suitable for improving the polymerization rate and reducing the amount of residual photopolymerization initiator when forming a pressure-sensitive adhesive sheet. [Brief description of the drawings]

[0012] [Figure 1] 1 is a cross-sectional view illustrating a schematic example of a pressure-sensitive adhesive sheet of the present invention. [Diagram 2] FIG. 2 is a schematic diagram illustrating an example of a method for forming the pressure-sensitive adhesive sheet of the present invention from the photocurable composition of the present invention. [Diagram 3] FIG. 1 is a cross-sectional view illustrating an example of an optical laminate of the present invention. [Figure 4] FIG. 1 is a cross-sectional view illustrating an example of an optical laminate of the present invention. [Diagram 5] FIG. 1 is a cross-sectional view illustrating an example of an optical laminate of the present invention. [Figure 6] FIG. 1 is a cross-sectional view illustrating an example of an optical laminate of the present invention. [Figure 7] FIG. 1 is a cross-sectional view that illustrates an example of an image display device of the present invention. [Figure 8] 1 is a graph showing the relationship between the polymerization rate and the content of a photopolymerization initiator in the pressure-sensitive adhesive sheets of Examples and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The photocurable composition according to the first aspect of the present invention comprises: A photocurable composition for a pressure-sensitive adhesive sheet, comprising a monomer group and / or a partial polymer of the monomer group, and a photopolymerization initiator, The photopolymerization initiator is a compound having a chemical structure represented by the following formula (1) in its molecule: R in the above formula (1) 1 and R 2 are each independently a C1 to C8 alkyl group; -OH, a C1 to C4 alkoxy group, -CN, -COOR 51 , -OOCR 52 , or -NR 53 R 54 an alkyl group having 1 to 4 carbon atoms, the hydrogen atom of which is replaced by -CH2-C6H4-R; an alkenyl group having 3 to 6 carbon atoms, the hydrogen atom of which is replaced by -CH2-C6H4-R 55 and R 1 and R 2 may be bonded to each other to form a C2 to C9 alkylene group, a C3 to C6 oxyalkylene group, or an azaalkylene group, X is -OR 56 , or -NR 57 R 58 and R 51is a C1 to C8 alkyl group, R 52 is a C1 to C4 alkyl group, R 53 and R 54 are each independently a hydrogen atom, a C1-C12 alkyl group; -OH, a C1-C4 alkoxy group, -CN and -COOR 59 a C2-C4 alkyl group, the hydrogen atom of which is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; or a cyclohexyl group, R 53 and R 54 are bonded to each other to form -O- or -N(R 60 )-, and may be a C3 to C9 alkylene group optionally interrupted by -. R 55 is a C1 to C4 alkyl group, R 56 is a hydrogen atom, -SiR 62 3. A C1 to C8 alkyl group or a C3 to C6 alkenyl group; R 57 and R 58 represents an alkyl group having 1 to 12 carbon atoms; -OH, an alkoxy group having 1 to 4 carbon atoms, -CN and -COOR 63 a C2-C4 alkyl group, the hydrogen atom of which is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; or a cyclohexyl group, R 57 and R 58 are bonded to each other to form -O- or -N(R 64 )-, and may be a C3 to C9 alkylene group optionally interrupted by -. R 59 is a C1 to C4 alkyl group, R 60 is a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an allyl group, a hydroxyalkyl group having 1 to 4 carbon atoms, -CH2CH2-COOR 61 or -CHCHCN, R 61 is a C1 to C4 alkyl group, R 62is a C1 to C6 alkyl group, R 63 is a C1 to C4 alkyl group, R 64 is a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an allyl group, a hydroxyalkyl group having 1 to 4 carbon atoms, -CH2CH2-COOR 65 or -CHCHCN, R 65 is a C1 to C4 alkyl group, The chemical structure may be bonded to a hydrogen atom or a hydrogen atom-substituted structure via the carbon atom marked with * in formula (1). [ka]

[0014] In the second aspect of the present invention, for example, in the photocurable composition according to the first aspect, 1 and the above R 2 are each independently a C1 to C8 alkyl group.

[0015] In a third aspect of the present invention, for example, in the photocurable composition according to the first or second aspect, the R 1 and the above R 2 are identical.

[0016] In a fourth aspect of the present invention, for example, in the photocurable composition according to any one of the first to third aspects, X is -OR 56 It is.

[0017] In a fifth aspect of the present invention, for example, in the photocurable composition according to any one of the first to third aspects, X is -OH.

[0018] In a sixth aspect of the present invention, for example, in the photocurable composition according to any one of the first to fifth aspects, the chemical structure is a structure represented by the following formula (2). [ka]

[0019] In a seventh aspect of the present invention, for example, in the photocurable composition according to any one of the first to sixth aspects, the photopolymerization initiator is a compound having two or more of the above chemical structures in one molecule.

[0020] In an eighth aspect of the present invention, for example, in the photocurable composition according to any one of the first to seventh aspects, the photopolymerization initiator is a compound represented by the following formula (3): R in the above formula (3) 1 ' and R 2 ' are each other and the R 1 and R 2 Independently of R 1 and R 2 is a group that can be X' is, independently of X, a group which may be taken as X, A is -O-, -CYR 3 - or -C(CH3)R 4 and Y is a hydrogen atom, -Cl, -Br, -OR 71 , -NR 72 R 73 , or -SR 74 and R 3 is a hydrogen atom, an alkyl group having C1 to C8, an alkenyl group having C3 to C6, a benzyl group, -CH2-C6H4-R 75 or a phenyl group, R 4 is a C1-C6 alkyl or alkylene group, and the alkylene group is bonded to a carbon atom of a phenylene group contained in the compound of formula (3), R 71 is a hydrogen atom, -Si(R 76 )3, C1-C12 alkyl groups, C2-C18 acyl groups, -CO-NH-R 77 , C2-C20 hydroxyalkyl group, C2-C20 methoxyalkyl group, 3-R 78-2-hydroxypropyl group, 3-[1,3,3,3-tetramethyl-1-[(trimethylsilyl)oxy]disiloxanyl]propyl group, 2,3-dihydroxypropyl group, or a C2-C21 hydroxyalkyl group or a C3-C25 alkyl group in which the carbon chain is interrupted by 1 to 9 oxygen atoms, R 72 and R 73 are each independently a C1 to C12 alkyl group; -OH, a C1 to C4 alkoxy group, -CN, or -COOR 79 a C2-C4 alkyl group, the hydrogen atom of which is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; a cyclohexyl group; or a C7-C9 phenylalkyl group, R 72 and R 73 are bonded to each other to form -O- or -N(R 80 )-, and may be a C3 to C9 alkylene group optionally interrupted by -. R 74 is an alkyl group having C1 to C18, a hydroxyethyl group, a 2,3-dihydroxypropyl group, a cyclohexyl group, a benzyl group, a phenyl group, an alkylphenyl group having C1 to C12, -CH2-COOR 81 -CH2CH2-COOR 82 or -CH(CH3)-COOR 83 and R 75 is a C1 to C4 alkyl group, R 76 is a C1 to C6 alkyl group, R 77 is a C1 to C12 alkyl group, R 78 is a C1 to C18 alkoxy group, R 79 is a C1 to C4 alkyl group, R 80 is a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an allyl group, a benzyl group, a hydroxyalkyl group having 1 to 4 carbon atoms, -CH2CH2-COOR 84 or -CHCHCN, R81 , R 82 and R 83 are each independently a C1 to C18 alkyl group, R 84 is a C1 to C4 alkyl group. [ka]

[0021] In the ninth aspect of the present invention, for example, in the photocurable composition according to the eighth aspect, A is -CYR 3 -It is.

[0022] In a tenth aspect of the present invention, for example, in the photocurable composition according to the ninth aspect, the Y and R 3 is a hydrogen atom.

[0023] In an eleventh aspect of the present invention, for example, in the photocurable composition according to any one of the eighth to tenth aspects, the photopolymerization initiator is a compound represented by the following formula (4). [ka]

[0024] In a twelfth aspect of the present invention, for example, in the photocurable composition according to any one of the first to eleventh aspects, the amount of the photopolymerization initiator in the photocurable composition is 0.01 to 1 part by weight per 100 parts by weight in total of the monomer group and the partially polymerized product.

[0025] In a thirteenth aspect of the present invention, for example, in the photocurable composition according to any one of the first to twelfth aspects, the monomer group includes a (meth)acrylic monomer.

[0026] A pressure-sensitive adhesive sheet according to a fourteenth aspect of the present invention is a pressure-sensitive adhesive sheet formed from the photocurable composition according to any one of the first to thirteenth aspects.

[0027] In a fifteenth aspect of the present invention, for example, in the pressure-sensitive adhesive sheet according to the fourteenth aspect, the polymerization rate of the monomer group in the pressure-sensitive adhesive sheet is 96% or more, and the content of the photopolymerization initiator is 800 wtppm or less.

[0028] In a sixteenth aspect of the present invention, for example, in the pressure-sensitive adhesive sheet according to the fourteenth or fifteenth aspect, the pressure-sensitive adhesive sheet has a thickness of 300 μm or less.

[0029] An optical laminate according to a seventeenth aspect of the present invention comprises the pressure-sensitive adhesive sheet according to any one of the fourteenth to sixteenth aspects, and an optical film.

[0030] In an eighteenth aspect of the present invention, for example, in the optical laminate according to the seventeenth aspect, the optical film is a polarizing film, and the pressure-sensitive adhesive sheet is in contact with the polarizing film.

[0031] An image display device according to a nineteenth aspect of the present invention includes the optical laminate according to the seventeenth or eighteenth aspect.

[0032] The present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be modified in any manner without departing from the gist of the present invention.

[0033] [Photocurable composition] The photocurable composition of the present embodiment includes a monomer group and / or a partial polymer of the monomer group and a photopolymerization initiator. The photocurable composition of the present embodiment is for use in an adhesive sheet. An adhesive sheet can be formed from the photocurable composition of the present embodiment.

[0034] (Photopolymerization initiator) The photopolymerization initiator contained in the photocurable composition of this embodiment is a compound having a chemical structure represented by the following formula (1) in the molecule (hereinafter referred to as chemical structure X). [ka]

[0035] R in the above formula (1) 1 and R 2 are each independently a C1 to C8 alkyl group; -OH, a C1 to C4 alkoxy group, -CN, -COOR 51 , -OOCR 52 , or -NR 53 R 54 an alkyl group having 1 to 4 carbon atoms, the hydrogen atom of which is replaced by -CH2-C6H4-R; an alkenyl group having 3 to 6 carbon atoms, the hydrogen atom of which is replaced by -CH2-C6H4-R 55 R 1 and R 2 may be bonded to each other to form a C2 to C9 alkylene group, a C3 to C6 oxyalkylene group, or an azaalkylene group. 51 is a C1 to C8 alkyl group. 52 is a C1 to C4 alkyl group. 53 and R 54 are each independently a hydrogen atom, a C1-C12 alkyl group; -OH, a C1-C4 alkoxy group, -CN and -COOR 59 R is a C2-C4 alkyl group, the hydrogen atom of which is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; or a cyclohexyl group. 53 and R 54 are bonded to each other to form -O- or -N(R 60 R may be a C3 to C9 alkylene group optionally interrupted by -. 55 is a C1 to C4 alkyl group. 59 is a C1 to C4 alkyl group. 60 is a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an allyl group, a hydroxyalkyl group having 1 to 4 carbon atoms, -CH2CH2-COOR 61 Or -CH2CH2CN. 61 is a C1 to C4 alkyl group.

[0036] X is -OR 56 , or -NR 57 R 58 R 56 is a hydrogen atom, -SiR 623. A C1 to C8 alkyl group or a C3 to C6 alkenyl group. R 57 and R 58 represents an alkyl group having 1 to 12 carbon atoms; -OH, an alkoxy group having 1 to 4 carbon atoms, -CN and -COOR 63 R is a C2-C4 alkyl group, the hydrogen atom of which is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; or a cyclohexyl group. 57 and R 58 are bonded to each other to form -O- or -N(R 64 R may be a C3 to C9 alkylene group optionally interrupted by -. 62 is a C1 to C6 alkyl group. 63 is a C1 to C4 alkyl group. 64 is a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an allyl group, a hydroxyalkyl group having 1 to 4 carbon atoms, -CH2CH2-COOR 65 Or -CH2CH2CN. 65 is a C1 to C4 alkyl group.

[0037] The chemical structure X can be bonded to a hydrogen atom or a structure substituted with a hydrogen atom via the carbon atom indicated by * in formula (1).

[0038] The alkyl group, alkoxy group, alkenyl group, alkylene group, oxyalkylene group, azaalkylene group, and hydroxyalkyl group described in the explanation of formula (1) may be unbranched or branched. In addition, the description of "Cn1 to Cn2" (n1 and n2 are natural numbers) in this specification, including the explanation of formula (1), means that the number of carbon atoms is in the range of n1 to n2.

[0039] According to the investigations of the present inventors, chemical structure X is suitable for suppressing inhibition by oxygen during photocuring of the photocurable composition, which is believed to contribute to improving the cleavage efficiency of the photopolymerization initiator.

[0040] R 1 and R 2may be, independently of each other, a C1 to C8 alkyl group, a C3 to C6 alkenyl group, or a C1 to C8 alkyl group. 1 and R 2 may be, independently of each other, a C1 to C4 alkyl group, a C1 to C3 alkyl group, or a C1 to C2 alkyl group. 1 and R 2 may be a methyl group.

[0041] R 1 and R 2 may be identical.

[0042] X is -OR 56 R 56 may be a hydrogen atom or a C1 to C8 alkyl group, or may be a hydrogen atom In other words, X may be -OH.

[0043] R 1 , R 2 and X may be any combination of the preferred examples above.

[0044] The chemical structure X may be a structure shown in the following formula (2). In the chemical structure X of formula (2), when a hydrogen atom substitution structure is bonded to the carbon atom indicated by *, the substitution structure and -COCR in formula (2) may be bonded to each other. 1 XR 2 The group is in a para-position relationship with respect to the benzene ring of the chemical structure X. [ka]

[0045] The photopolymerization initiator may be a compound having two or more chemical structures X in one molecule. A photopolymerization initiator having two or more chemical structures X in one molecule can reliably contribute to both the formation of a polymer from a monomer and the extension of a polymer chain in a state where the photopolymerization initiator is incorporated into a polymer. The photopolymerization initiator is particularly suitable for improving the polymerization rate and reducing the amount of remaining photopolymerization initiator when forming a pressure-sensitive adhesive sheet.

[0046] The photopolymerization initiator may be a compound represented by the following formula (3). The compound of formula (3) has two chemical structures X in one molecule. The two chemical structures X are located at both ends of the molecule of the photopolymerization initiator, respectively. More specifically, the two chemical structures X are bonded to each other by -A- at the carbon atom of the phenylene group represented by * above. [ka]

[0047] R in Equation (3) 1 ' and R 2 ' are each other and R 1 and R 2 Independently of R 1 and R 2 R is a possible group. 1 ' and / or R 2 ' is R 1 and / or R 2 It may be the same as R 1 , R 2 , R 1 ' and R 2 ' may all be the same.

[0048] X' in formula (3) is a possible group for X, independent of X in formula (1). X' and X may be the same.

[0049] A is -O-, -CYR 3 - or -C(CH3)R 4 It is.

[0050] Y is a hydrogen atom, -Cl, -Br, -OR 71 , -NR 72 R 73 , or -SR 74 R 3 is a hydrogen atom, an alkyl group having C1 to C8, an alkenyl group having C3 to C6, a benzyl group, -CH2-C6H4-R 75 or a phenyl group. 4is a C1 to C6 alkyl or alkylene group, and this alkylene group is bonded to a carbon atom of the phenylene group that the compound of formula (3) has.

[0051] R 71 is a hydrogen atom, -Si(R 76 )3, C1-C12 alkyl groups, C2-C18 acyl groups, -CO-NH-R 77 , C2-C20 hydroxyalkyl group, C2-C20 methoxyalkyl group, 3-R 78 -2-hydroxypropyl group, 3-[1,3,3,3-tetramethyl-1-[(trimethylsilyl)oxy]disiloxanyl]propyl group, 2,3-dihydroxypropyl group, or a C2-C21 hydroxyalkyl group or a C3-C25 alkyl group in which the carbon chain is interrupted by 1 to 9 oxygen atoms. 72 and R 73 are each independently a C1 to C12 alkyl group; -OH, a C1 to C4 alkoxy group, -CN, or -COOR 79 a C2-C4 alkyl group, in which a hydrogen atom is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; a cyclohexyl group; or a C7-C9 phenylalkyl group. R 72 and R 73 are bonded to each other to form -O- or -N(R 80 R may be a C3 to C9 alkylene group optionally interrupted by -. 74 is an alkyl group having C1 to C18, a hydroxyethyl group, a 2,3-dihydroxypropyl group, a cyclohexyl group, a benzyl group, a phenyl group, an alkylphenyl group having C1 to C12, -CH2-COOR 81 -CH2CH2-COOR 82 or -CH(CH3)-COOR 83 R 75 is a C1 to C4 alkyl group. 76 is a C1 to C6 alkyl group. 77 is a C1 to C12 alkyl group. 78 is a C1 to C18 alkoxy group. 79is a C1 to C4 alkyl group. 80 is a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an allyl group, a benzyl group, a hydroxyalkyl group having 1 to 4 carbon atoms, -CH2CH2-COOR 84 , or -CH2CH2CN. 81 , R 82 and R 83 are each independently a C1 to C18 alkyl group. 84 is a C1 to C4 alkyl group.

[0052] The alkyl group, alkenyl group, acyl group, hydroxyalkyl group, methoxyalkyl group, alkoxy group, alkyl moiety in the phenylalkyl group, and alkylene group described in the explanation of formula (3) may be either unbranched or branched.

[0053] R in Equation (3) 1 , R 2 , R 1 ' and R 2 Preferred examples of R 1 and R 2 The preferred examples of X' in formula (3) are the same as the preferred examples of X described above in the explanation of formula (1). A is -CYR 3 Y may be a hydrogen atom. 3 may be a hydrogen atom. 3 - and Y and R 3 and may both be hydrogen atoms. In other words, A may be -CH2-.

[0054] R in Equation (3) 1 , R 2 , R 1 ', R 2 X′, X′, and A may take any combination of the preferred examples above.

[0055] The photopolymerization initiator may be a compound represented by the following formula (4): The compound of formula (4) is a type of compound of formula (3). [ka]

[0056] Specific examples of the photopolymerization initiator are shown in the following formulas (5) to (9). The photopolymerization initiator may be a compound represented by at least one formula selected from the group consisting of formulas (5) to (9), a compound represented by at least one formula selected from the group consisting of formulas (5) to (8), a compound represented by at least one formula selected from the group consisting of formulas (5) to (7), or a compound represented by formula (5). The compound represented by formula (8) is derived from a vinyl compound having a chemical structure X in its side chain. More specifically, it is an oligomer of the vinyl compound.

[0057] [ka]

[0058] [ka]

[0059] [ka]

[0060] [ka]

[0061] [ka]

[0062] The photopolymerization initiators represented by the formulas (5) to (9) are commercially available as Omnirad127, Esacure KIP160, Esacure one, Esacure KIP150, and Omnirad1173 (all manufactured by IGM Resins). The photopolymerization initiator may be at least one selected from these groups.

[0063] The photocurable composition may contain one or more photoinitiators.

[0064] The amount of the photopolymerization initiator in the photocurable composition is, for example, 0.01 to 1 part by weight per 100 parts by weight of the total of the monomer group and the partial polymer. When two or more kinds of photopolymerization initiators are contained, the total amount of each photopolymerization initiator is within the range. The upper limit of the amount may be 0.9 parts by weight or less, 0.8 parts by weight or less, 0.7 parts by weight or less, 0.6 parts by weight or less, 0.5 parts by weight or less, 0.4 parts by weight or less, 0.3 parts by weight or less, 0.25 parts by weight or less, 0.22 parts by weight or less, or even 0.2 parts by weight or less. The lower limit of the amount may be 0.05 parts by weight or more, 0.08 parts by weight or more, 0.1 parts by weight or more, or even 0.15 parts by weight or more.

[0065] (Monomer group) The monomer group may contain a (meth)acrylic monomer. The content of the (meth)acrylic component in the photocurable composition, i.e., the (meth)acrylic monomer and its partial polymer, may be 50% by weight or more, 60% by weight or more, 70% by weight or more, or even 80% by weight or more. In this case, an acrylic adhesive sheet mainly composed of a (meth)acrylic polymer and its crosslinked product can be formed. However, the photocurable composition is not limited to the above examples. In this specification, (meth)acrylic means acrylic and methacrylic. (Meth)acrylate means acrylate and methacrylate.

[0066] An example of the (meth)acrylic monomer is a (meth)acrylic acid alkyl ester having an alkyl group having 1 to 20 carbon atoms on the side chain. The number of carbon atoms in the alkyl group may be 7 or less, 6 or less, 5 or less, or even 4 or less. The alkyl group may be linear or branched. Examples of the (meth)acrylic acid alkyl ester are methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, n-hexyl (meth)acrylate, isohexyl (meth)acrylate, isoheptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and the like. acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, n-dodecyl (meth)acrylate (lauryl (meth)acrylate), n-tridecyl (meth)acrylate, n-tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate and octadecyl (meth)acrylate. The (meth)acrylic acid alkyl ester may be n-butyl (meth)acrylate.

[0067] The content of the (meth)acrylic acid alkyl ester in the monomer group is, for example, 40% by weight or more, and may be 50% by weight or more, 60% by weight or more, 70% by weight or more, 80% by weight or more, 85% by weight or more, 90% by weight or more, or even 95% by weight or more. In calculating the content, the weight of the partially polymerized product is converted into the weight of each monomer before polymerization.

[0068] The monomer group may contain a carboxyl group-containing monomer. The carboxyl group-containing monomer may be a (meth)acrylic monomer, in other words, the (meth)acrylic monomer may contain a carboxyl group-containing monomer. Examples of the carboxyl group-containing monomer are (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid. The content of the carboxyl group-containing monomer in the monomer group may be, for example, 10% by weight or less, 9% by weight or less, 8% by weight or less, 7% by weight or less, 6% by weight or less, 5.5% by weight or less, or even 5% by weight or less. The lower limit of the content may be, for example, 0.1% by weight or more, 0.5% by weight or more, or even 1% by weight or more. The monomer group may not contain a carboxyl group-containing monomer.

[0069] The monomer group may contain a hydroxyl group-containing monomer. The hydroxyl group-containing monomer may be a (meth)acrylic monomer, in other words, the (meth)acrylic monomer may contain a hydroxyl group-containing monomer. The hydroxyl group-containing monomer may contribute to improving the cohesive strength of the adhesive sheet. Examples of the hydroxyl group-containing monomer are 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)-methyl acrylate. The hydroxyl group-containing monomer is preferably 2-hydroxyethyl (meth)acrylate or 4-hydroxybutyl (meth)acrylate. The content of the hydroxyl group-containing monomer in the monomer group is, for example, 10% by weight or less, and may be 5% by weight or less, 4% by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, 0.8% by weight or less, 0.5% by weight or less, 0.3% by weight or less, 0.2% by weight or less, or even 0.1% by weight or less. The lower limit of the content may be, for example, 0.01% by weight or more, 0.03% by weight or more, or even 0.05% by weight or more. The monomer group may not contain a hydroxyl group-containing monomer.

[0070] The monomer group may include a nitrogen atom-containing monomer. The nitrogen atom-containing monomer means a monomer having at least one nitrogen atom in the molecule (per molecule).

[0071] As the nitrogen atom-containing monomer, from the viewpoint of improving foaming and peeling resistance, N-vinyl cyclic amide, (meth)acrylamide, etc. are preferable. The nitrogen atom-containing monomer may be used alone or in combination of two or more kinds.

[0072] The N-vinyl cyclic amide is preferably one represented by the following formula (10). [ka]

[0073] In formula (10), R 101 is a divalent organic group, preferably a divalent saturated or unsaturated hydrocarbon group, and more preferably a divalent saturated hydrocarbon group (e.g., an alkylene group having 3 to 5 carbon atoms). 101 are directly bonded via a single bond to form a ring structure.

[0074] As the N-vinyl cyclic amide represented by formula (10), from the viewpoint of improving foaming and peeling resistance, N-vinyl-2-pyrrolidone (NVP), N-vinyl-2-piperidone, N-vinyl-2-caprolactam, N-vinyl-3-morpholinone, N-vinyl-1,3-oxazin-2-one, N-vinyl-3,5-morpholinedione, etc. are preferred, more preferably N-vinyl-2-pyrrolidone, N-vinyl-2-caprolactam, and even more preferably N-vinyl-2-pyrrolidone.

[0075] Examples of (meth)acrylamides include (meth)acrylamide, N-alkyl(meth)acrylamide, N,N-dialkyl(meth)acrylamide, etc. Examples of N-alkyl(meth)acrylamide include N-ethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, Nn-butyl(meth)acrylamide, N-octylacrylamide, etc. Examples of N-alkyl(meth)acrylamides include (meth)acrylamides having an amino group, such as dimethylaminoethyl(meth)acrylamide, diethylaminoethyl(meth)acrylamide, and dimethylaminopropyl(meth)acrylamide.

[0076] Examples of N,N-dialkyl(meth)acrylamides include N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-diisopropyl(meth)acrylamide, N,N-di(n-butyl)(meth)acrylamide, and N,N-di(t-butyl)(meth)acrylamide.

[0077] (Meth)acrylamides also include, for example, various N-hydroxyalkyl (meth)acrylamides. Examples of N-hydroxyalkyl (meth)acrylamides include N-methylol (meth)acrylamide, N-(2-hydroxyethyl) (meth)acrylamide, N-(2-hydroxypropyl) (meth)acrylamide, N-(1-hydroxypropyl) (meth)acrylamide, N-(3-hydroxypropyl) (meth)acrylamide, N-(2-hydroxybutyl) (meth)acrylamide, N-(3-hydroxybutyl) (meth)acrylamide, N-(4-hydroxybutyl) (meth)acrylamide, and N-methyl-N-2-hydroxyethyl (meth)acrylamide.

[0078] (Meth)acrylamides also include, for example, various N-alkoxyalkyl(meth)acrylamides, such as N-methoxymethyl(meth)acrylamide and N-butoxymethyl(meth)acrylamide.

[0079] Examples of nitrogen atom-containing monomers other than N-vinyl cyclic amides and (meth)acrylamides include amino group-containing monomers such as aminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, and t-butylaminoethyl (meth)acrylate; cyano group-containing monomers such as acrylonitrile and methacrylonitrile; (meth)acryloylmorpholine, N-vinylpiperazine, N-vinylpyrrole, N-vinylimidazole, N-vinylpyrazine, N-vinylmorpholine, N-vinylpyrazole, vinylpyridine, vinylpyrimidine, vinyloxazole, vinylisoxazole, vinylthiazole, vinylisothiazole, vinylpyridazine, (meth)acryloylpyrrolidone, (meth)acryloylpyrrolidine, (meth)acryloylpiperidine, N-methyl Examples of the monomer include heterocyclic ring-containing monomers such as vinylpyrrolidone; maleimide monomers such as N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, and N-phenylmaleimide; itaconimide monomers such as N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-laurylitaconimide, and N-cyclohexylitaconimide; and succinimide monomers such as N-(meth)acryloyloxymethylenesuccinimide, N-(meth)acryloyl-6-oxyhexamethylenesuccinimide, and N-(meth)acryloyl-8-oxyoctamethylenesuccinimide; and other imide group-containing monomers; and isocyanate group-containing monomers such as 2-(meth)acryloyloxyethylisocyanate.

[0080] The content of the nitrogen atom-containing monomer in the monomer group is, for example, 40% by weight or less, and may be 35% by weight or less, 30% by weight or less, 25% by weight or less, 20% by weight or less, 15% by weight or less, 13% by weight or less, 10% by weight or less, 8% by weight or less, 6% by weight or less, or even 5% by weight or less. The lower limit of the content is, for example, 0.5% by weight or more, and may be 1% by weight or more, 2% by weight or more, 3% by weight or more, 4% by weight or more, 5% by weight or more, 7% by weight or more, or even 10% by weight or more. The monomer group may not contain a nitrogen atom-containing monomer.

[0081] The monomer group may include monomers other than those mentioned above.

[0082] In the photocurable composition, each of the above-mentioned monomers may be contained as a partial polymer. The partial polymer may be either a homopolymer or a copolymer. The photocurable composition may not contain a partial polymer.

[0083] The photocurable composition may contain a crosslinking agent. An example of the crosslinking agent is a polyfunctional monomer having two or more polymerizable functional groups in one molecule. The polyfunctional monomer may be a (meth)acrylic monomer. An example of the polyfunctional monomer is a monomer having two or more C=C bonds in one molecule, and a monomer having one or more C=C bonds and one or more polymerizable functional groups such as epoxy groups, aziridine groups, oxazoline groups, hydrazine groups, methylol groups, etc. in one molecule. The polyfunctional monomer is preferably a monomer having two or more C=C bonds in one molecule.

[0084] Examples of the polyfunctional monomer include (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,2-ethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol diacrylate (N DDA), 1,12-dodecanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, and other polyfunctional acrylates (such as ester compounds of polyhydric alcohols and (meth)acrylic acid); allyl (meth)acrylate, vinyl (meth)acrylate, divinylbenzene, epoxy acrylate, polyester acrylate, urethane acrylate, butyl di(meth)acrylate, and hexyl di(meth)acrylate. The polyfunctional monomer is preferably a polyfunctional acrylate, and more preferably 1,9-nonanediol diacrylate, trimethylolpropane tri(meth)acrylate, hexanediol di(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.

[0085] The amount of the crosslinking agent to be added varies depending on the molecular weight, the number of functional groups, etc., but may be, for example, 5 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, 1 part by weight or less, 0.5 parts by weight or less, or even 0.3 parts by weight or less, based on 100 parts by weight of the total of the monomer group and its partial polymer. The lower limit of the amount to be added is, for example, 0.01 parts by weight or more, or even 0.05 parts by weight or more. The photocurable composition may not contain a crosslinking agent.

[0086] The photocurable composition may contain additives other than those described above. Examples of additives include chain transfer agents, silane coupling agents, viscosity modifiers, tackifiers, plasticizers, softeners, antioxidants, fillers, colorants, antioxidants, surfactants, antistatic agents, and ultraviolet absorbing agents. The photocurable composition may not contain additives.

[0087] The viscosity of the photocurable composition is preferably 5 to 100 poise. A photocurable composition having a viscosity in the above range is particularly suitable for forming a pressure-sensitive adhesive sheet.

[0088] The content of the solvent in the photocurable composition is, for example, 5% by weight or less, and may be 4% by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, or even 0.5% by weight or less. The photocurable composition may be substantially free of a solvent. The phrase "substantially free of a solvent" means that the solvent derived from additives and the like is allowed to be present at a content of, for example, 0.1% by weight or less, preferably 0.05% by weight or less, and more preferably 0.01% by weight or less.

[0089] [Adhesive sheet] An example of the pressure-sensitive adhesive sheet of this embodiment is shown in Fig. 1. The pressure-sensitive adhesive sheet 1 in Fig. 1 is a sheet formed from the photocurable composition of this embodiment.

[0090] The polymerization rate of the monomer group in the pressure-sensitive adhesive sheet 1 is, for example, 90% or more, and may be 91% or more, 92% or more, 93% or more, 94% or more, 95% or more, 96% or more, 97% or more, 98% or more, 98.5% or more, 99% or more, or even 99.5% or more. The upper limit of the polymerization rate is, for example, 99.99% or less.

[0091] The content (residual amount) of the photopolymerization initiator in the adhesive sheet 1 may be, for example, 800wtppm or less, 750wtppm or less, 700wtppm or less, 650wtppm or less, 600wtppm or less, 550wtppm or less, 500wtppm or less, 450wtppm or less, 400wtppm or less, 380wtppm or less, 350wtppm or less, 330wtppm or less, 300wtppm or less, 280wtppm or less, 250wtppm or less, 230wtppm or less, 200wtppm or less, 180wtppm or less, 150wtppm or less, 130wtppm or less, 100wtppm or less, 80wtppm or less, 50wtppm or less, 30wtppm or less, or even 25wtppm or less. The lower limit of the content is 0 wtppm or more. The reduced remaining amount can contribute to suppression of yellowing and foaming in the pressure-sensitive adhesive sheet 1. It can also contribute to suppression of changes in adhesive strength over time in the pressure-sensitive adhesive sheet 1 and to suppression of heavy release of the release liner (especially the release liner on the side irradiated with light such as ultraviolet light) during the formation of the pressure-sensitive adhesive sheet 1.

[0092] The adhesive sheet 1 can achieve an increased polymerization rate and a reduced amount of remaining photopolymerization initiator. The polymerization rate of the monomer group in the adhesive sheet 1 may be 96% or more, and the content of the photopolymerization initiator may be 800 wtppm or less. The polymerization rate and the content may each be within the above-mentioned numerical ranges. The content of the photopolymerization initiator in the adhesive sheet 1 can be evaluated by liquid chromatography.

[0093] The polymerization rate and the content of the photopolymerization initiator in the pressure-sensitive adhesive sheet 1 may satisfy the formula: photopolymerization initiator content (wtppm)≦233×polymerization rate (%)−22200.

[0094] The weight average molecular weight (Mw) of the polymer contained in the pressure-sensitive adhesive sheet 1 is, for example, 500,000 or more, and may be 600,000 or more, 650,000 or more, 700,000 or more, 750,000 or more, 800,000 or more, 850,000 or more, or even 900,000 or more. The upper limit of Mw is not particularly limited, and may be, for example, 3,000,000 or less. The pressure-sensitive adhesive sheet 1 containing a polymer having Mw in the above range is suitable for suppressing peeling of the pressure-sensitive adhesive sheet 1 from an adhesive object under high temperature environments and the like. The adhesive object is, for example, an optical film. An example of an optical film is a polarizing film. The number average molecular weight (Mn) of the polymer is, for example, 150,000 or more, and may be 170,000 or more, 180,000 or more, 190,000 or more, or even 200,000 or more. The upper limit of Mn is not particularly limited, and may be, for example, 600,000 or less. Mw / Mn, which means the molecular weight distribution, is, for example, 1.8 to 10, and may be 1.8 to 7, or even 1.8 to 5. Mw and Mn are determined from values ​​measured by GPC (gel permeation chromatography) and calculated in terms of polystyrene.

[0095] The gel fraction of the pressure-sensitive adhesive sheet 1 is, for example, 50% or more, and may be 75% or more, 80% or more, or even 85% or more.

[0096] The thickness of the pressure-sensitive adhesive sheet 1 is, for example, 2 to 500 μm, and may be 2 to 300 μm, 2 to 200 μm, or even 2 to 150 μm. The upper limit of the thickness may be 100 μm or less, 70 μm or less, 60 μm or less, 50 μm or less, 40 μm or less, 30 μm or less, 25 μm or less, or even 20 μm or less. The lower limit of the thickness may be 5 μm or more, 10 μm or more, or even 15 μm or more.

[0097] The pressure-sensitive adhesive sheet 1 can be used, for example, in an optical laminate or an image display device. However, the uses of the pressure-sensitive adhesive sheet 1 are not limited to the above examples.

[0098] (Manufacturing method of adhesive sheets) The pressure-sensitive adhesive sheet 1 can be formed, for example, by irradiating light 14 to a first laminate 10 including a base sheet 11, a coating layer 12 containing the photocurable composition of the present embodiment, and a release liner 13 in this order (see FIG. 2). The coating layer 12 is irradiated with light 14 and hardened to become the pressure-sensitive adhesive sheet 1. Irradiation with light 14 is typically performed from the side of the base sheet 11. At this time, the light 14 penetrates the base sheet 11 and reaches the coating layer 12, hardening the coating layer 12. However, irradiation with light 14 may be performed from the side of the release liner 13, or may be performed from both the side of the release liner 13 and the side of the base sheet 11.

[0099] The formed pressure-sensitive adhesive sheet 1 is sandwiched between the base sheet 11 and the release liner 13 until the release liner 13 is peeled off, and constitutes a part of the second laminate 17. By peeling the release liner 13 from the second laminate 17, a third laminate 15 including the base sheet 11 and the pressure-sensitive adhesive sheet 1 is obtained. In the third laminate 15, the surface of the pressure-sensitive adhesive sheet 1 is exposed to the outside. An optical film can be laminated onto the exposed surface of the pressure-sensitive adhesive sheet 1 directly or via another layer.

[0100] The light 14 is, for example, visible light or ultraviolet light having a wavelength shorter than 450 nm. The light may contain light having a wavelength in the same region as the absorption wavelength of the photopolymerization initiator contained in the photocurable composition. Light with a wavelength of 300 nm or less cut by a filter or the like may be irradiated, and cutting short wavelength light is suitable for suppressing deterioration of the base sheet 11 and / or the release liner 13 caused by the light 14. The light source 18 of the light 14 is, for example, a light irradiation device equipped with an ultraviolet irradiation lamp. Examples of the ultraviolet irradiation lamp include an ultraviolet LED, a low pressure mercury lamp, a medium pressure mercury lamp, a high pressure mercury lamp, an ultra-high pressure mercury lamp, a metal halide lamp, a xenon lamp, a microwave excited mercury lamp, a black light lamp, a chemical lamp, a germicidal lamp, a low pressure discharge mercury lamp, and an excimer laser. Two or more ultraviolet irradiation lamps may be combined. With the ultraviolet LED, the band of the irradiated ultraviolet light can be narrowed compared to the case of using other light sources.

[0101] The light source 18 may be an LED. Compared to a black light source, an LED tends to have a long light source life as well as an easy adjustment of illuminance. Compared to a black light source using mercury, an LED is superior in terms of reducing environmental load. When an ultraviolet LED is used as the light source, an LED having a peak wavelength of 325 to 350 nm may be selected. According to the study by the present inventors, the use of an LED having a peak wavelength of 325 to 350 nm may contribute to improving the polymerization rate of the monomer group in the adhesive sheet 1 and / or reducing the amount of remaining photopolymerization initiator compared to, for example, the use of a black light source. Furthermore, an LED that emits light 14 with a peak wavelength of 325 nm to 350 nm tends to generate less heat and to control the temperature of the coating layer 12 more easily than an LED that emits light with a peak wavelength of about 365 nm. As far as the present inventors know, there have been no reports of an adhesive sheet being produced using an LED that emits light with a peak wavelength of 325 nm to 350 nm.

[0102] As an LED having a peak wavelength of 325 to 350 nm, an LED having a peak wavelength of 340±10 nm (hereinafter referred to as LED340) may be selected.

[0103] Focusing on the peak wavelength of the light 14, the peak wavelength of the light 14 irradiated to the first laminate 10 (specifically, the coating layer 12) may be 325 nm to 350 nm. The peak wavelength of the light 14 is preferably 340±10 nm (330 nm to 350 nm), may be 340±5 nm (335 nm to 345 nm), may be 340±2 nm (338 nm to 342 nm), or may be 340 nm. The peak wavelength means a wavelength at which the intensity is a maximum value in a spectrum showing the relationship between the wavelength and intensity of the light 14. The light 14 may further have a peak wavelength in a wavelength range other than 325 nm to 350 nm, but it is preferable that the light 14 does not have such a peak wavelength.

[0104] The illuminance of the light 14 irradiated onto the first laminate 10 (specifically, the coating layer 12) is, for example, 2.0 to 30 mW / cm 2 The illuminance is 2.5mW / cm2 More than 3.0mW / cm 2 More than 3.5mW / cm 2 More than 4.0mW / cm 2 More than 5.0mW / cm 2 More than 6.0mW / cm 2 More than 7.0mW / cm 2 More than 8.0mW / cm 2 More than 9.0mW / cm 2 or even 10mW / cm 2 The upper limit of the illuminance is, for example, 25 mW / cm 2 Less than 20mW / cm 2 Below 15mW / cm 2 It may be the following.

[0105] The time for irradiating the first laminate 10 (specifically, the coating layer 12) with the light 14 is, for example, 10 to 1000 seconds, and may be 60 seconds or more, 100 seconds or more, 150 seconds or more, or even 200 seconds or more. The upper limit of the time is, for example, 800 seconds or less, and may be 600 seconds or less, 500 seconds or less, 400 seconds or less, 300 seconds or less, or even 250 seconds or less. The irradiation with the light 14 may be continuous or intermittent.

[0106] The integrated amount of light 14 applied to the first laminate 10 (specifically, the coating layer 12) is, for example, 25 mJ / cm 2 More than 100 mJ / cm 2 More than 500mJ / cm 2 More than 1000mJ / cm 2 More than 2000mJ / cm 2 More than 2500mJ / cm 2 or even 3000mJ / cm 2 The upper limit of the integrated light amount is not particularly limited, and may be, for example, 30,000 mJ / cm. 2 Less than 10000mJ / cm 2 Below, 5000mJ / cm 2 Below that, and even 4000mJ / cm 2 It may be the following.

[0107] An example of the substrate of the release liner 13 (hereinafter, "liner substrate") is a resin film. Examples of resins that can be contained in the liner substrate are polyesters such as polyethylene terephthalate and polyethylene naphthalate, acetate resins, polyethersulfone, polycarbonate, polyamide, polyimide, polyolefin, (meth)acrylic resins, polyvinyl chloride, polyvinylidene chloride, polystyrene, polyvinyl alcohol, polyarylate, and polyphenylene sulfide. The resin is preferably a polyester such as polyethylene terephthalate.

[0108] The release liner 13 may have a layer other than the liner substrate. The release liner 13 may have a release layer. The release liner 13 has, for example, a liner substrate and a release layer formed on one surface of the liner substrate. This release liner 13 can be used such that the release layer is on the coating layer 12 side. The release layer is typically a cured layer of a release agent composition containing a release agent. As the release agent, various release agents such as silicone-based release agents, fluorine-based release agents, long-chain alkyl-based release agents, fatty acid amide-based release agents, and silica powder can be used.

[0109] The release liner 13 may be in the form of a sheet or a continuous piece.

[0110] An example of the base sheet 11 is a resin film. Examples of the resin contained in the base sheet 11 are the same as the examples of the resin that can be contained in the liner base material.

[0111] The thickness of the base sheet 11 is, for example, 10 to 200 μm, and may be 25 to 150 μm.

[0112] The base sheet 11 may have a release layer on the surface on the side of the coating layer 12. Examples of the release layer that may be provided on the base sheet 11 are the same as the examples of the release layer that may be provided on the release liner 13. Both the release liner 13 and the base sheet 11 may have a release layer.

[0113] For the base sheet 11, a sheet having a greater peeling strength from the adhesive sheet 1 than the release liner 13 can usually be selected.

[0114] The base sheet 11 may be in the form of a sheet or a continuous length.

[0115] The first laminate 10 can be formed, for example, by forming a coating layer 12 on a base sheet 11 (or a release liner 13) and then disposing a release liner 13 (or base sheet 11) on the formed coating layer 12. Alternatively, the first laminate 10 may be formed by applying a photocurable composition in a poured manner into the space between the base sheet 11 and the release liner 13 that are held at a predetermined distance such that their main surfaces face each other.

[0116] The coating layer 12 can be formed by various coating methods such as roll coating, kiss roll coating, gravure coating, reverse coating, roll brush, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, and die coating.

[0117] The thickness of the coating layer 12 can be adjusted according to the desired thickness of the pressure-sensitive adhesive sheet 1, and may be, for example, 2 to 500 μm, 2 to 300 μm, 2 to 200 μm, or even 2 to 150 μm. The upper limit of the thickness may be 100 μm or less, 70 μm or less, 60 μm or less, 50 μm or less, 40 μm or less, 30 μm or less, 25 μm or less, or even 20 μm or less. The lower limit of the thickness may be 5 μm or more, 10 μm or more, or even 15 μm or more.

[0118] The first laminate 10 may include a long base sheet 11, a long coating layer 12, and a long release liner 13, in other words, may be long. The long first laminate 10 can be obtained, for example, by forming the coating layer 12 between the base sheet 11 and the release liner 13 while conveying them, the base sheet 11 and the release liner 13 being unwound from a roll.

[0119] As described above, the present invention further provides a method for producing a pressure-sensitive adhesive sheet, comprising irradiating a coating layer of a photocurable composition containing a monomer group and / or a partial polymer of the monomer group, and a photopolymerization initiator having chemical structure X in its molecule with light 14 to photocure the coating layer.

[0120] [Optical laminate] An example of the optical laminate of this embodiment is shown in Fig. 3. The optical laminate 20A in Fig. 3 includes an adhesive sheet 1 and an optical film 2. The adhesive sheet 1 and the optical film 2 are laminated to each other. The optical laminate 20A can be used as an optical film with an adhesive sheet.

[0121] Examples of the optical film 2 include a polarizing film, a retardation film, and a laminated film including a polarizing film and / or a retardation film. However, the optical film 2 is not limited to the above examples. The optical film 2 may include a glass film.

[0122] The optical film 2 may be a polarizing film, and the pressure-sensitive adhesive sheet 1 may be in contact with the optical film 2 .

[0123] The polarizing film includes a polarizer. The polarizing film typically includes a polarizer and a protective film (transparent protective film). The protective film is disposed, for example, in contact with the main surface (surface having the widest area) of the polarizer. The polarizer may be disposed between two protective films. The protective film may be disposed on at least one surface of the polarizer.

[0124] The polarizer is not particularly limited, and examples thereof include hydrophilic polymer films such as polyvinyl alcohol films, partially formalized polyvinyl alcohol films, and partially saponified ethylene-vinyl acetate copolymer films, which are uniaxially stretched after adsorbing dichroic substances such as iodine and dichroic dyes; polyene-based oriented films such as dehydrated polyvinyl alcohol and dehydrochlorinated polyvinyl chloride; etc. Polarizers are typically made of polyvinyl alcohol films (polyvinyl alcohol films include partially saponified ethylene-vinyl acetate copolymer films) and dichroic substances such as iodine.

[0125] The thickness of the polarizer is not particularly limited, and may be, for example, 80 μm or less, 50 μm or less, 30 μm or less, 25 μm or less, or even 20 μm or less. The lower limit of the thickness of the polarizer is not particularly limited, and may be, for example, 1 μm or more, 5 μm or more, 10 μm or more, or even 15 μm or more. A thin polarizer (for example, a thickness of 20 μm or less) is suppressed in dimensional change, and can contribute to improving the durability of the optical laminate, particularly the durability at high temperatures.

[0126] As the material of the protective film, for example, a thermoplastic resin excellent in transparency, mechanical strength, thermal stability, moisture blocking property, isotropy, etc. is used. Specific examples of such thermoplastic resins include cellulose resins such as triacetyl cellulose, polyester resins, polyethersulfone resins, polysulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, (meth)acrylic resins, cyclic polyolefin resins (norbornene-based resins), polyarylate resins, polystyrene resins, polyvinyl alcohol resins, and mixtures thereof. The material of the protective film may be a thermosetting resin or an ultraviolet-curing resin such as a (meth)acrylic, urethane, acrylic urethane, epoxy, or silicone-based resin. When the polarizing film has two protective films, the materials of the two protective films may be the same or different from each other. For example, a protective film made of a thermoplastic resin may be bonded to one main surface of the polarizer via an adhesive, and a protective film made of a thermosetting resin or an ultraviolet-curing resin may be bonded to the other main surface of the polarizer. The protective film may contain one or more types of optional additives, such as ultraviolet absorbers, antioxidants, lubricants, plasticizers, release agents, color inhibitors, flame retardants, nucleating agents, antistatic agents, pigments, and colorants.

[0127] The thickness of the protective film can be appropriately determined, but is generally about 10 to 200 μm in terms of strength, workability such as handleability, thinness, and the like.

[0128] The polarizer and the protective film are usually adhered to each other via a water-based adhesive or the like. Examples of the water-based adhesive include an isocyanate-based adhesive, a polyvinyl alcohol-based adhesive, a gelatin-based adhesive, a vinyl-based latex, a water-based polyurethane, and a water-based polyester. Examples of adhesives other than the above-mentioned adhesives include an ultraviolet-curable adhesive and an electron beam-curable adhesive. The electron beam-curable polarizing film adhesive exhibits suitable adhesion to various protective films. The adhesive may contain a metal compound filler.

[0129] In the polarizing film, a retardation film or the like can be formed on the polarizer instead of the protective film. Another protective film or a retardation film or the like can be further provided on the protective film.

[0130] The protective film may have a hard coat layer on the surface opposite to the surface bonded to the polarizer, and may also be subjected to treatments for the purposes of anti-reflection, anti-sticking, diffusion, anti-glare, etc.

[0131] The polarizing film may be a circular polarizing film.

[0132] The thickness of the polarizing film is, for example, 500 μm or less, and may be 300 μm or less, 200 μm or less, 100 μm or less, or even 60 μm or less. The lower limit of the thickness is, for example, 10 μm or more, 25 μm or more, or even 40 μm or more.

[0133] The retardation film is a film having birefringence in the in-plane direction and / or the thickness direction, and is, for example, a stretched resin film or a film in which a liquid crystal material is oriented and fixed.

[0134] The retardation film may be a λ / 4 plate, a λ / 2 plate, an anti-reflection retardation film (see, for example, paragraphs 0221, 0222, and 0228 of JP 2012-133303 A), a retardation film for compensating for viewing angles (see, for example, paragraphs 0225 and 0226 of JP 2012-133303 A), or a tilted orientation retardation film for compensating for viewing angles (see, for example, paragraph 0227 of JP 2012-13303 A). The retardation film is not limited to the above examples as long as it has birefringence in the in-plane direction and / or the thickness direction. There are also no limitations on the retardation value, arrangement angle, three-dimensional birefringence, whether it is a single layer or a multilayer, and the like, of the retardation film. A known film can be used for the retardation film.

[0135] The optical film 2 has a thickness of, for example, 1 to 200 μm.

[0136] The optical film 2 may be a single layer or a laminated film composed of two or more layers. When the optical film 2 is a laminated film, the pressure-sensitive adhesive sheet 1 may be used to bond the layers together.

[0137] Another example of the optical laminate of the present embodiment is shown in Fig. 4. The optical laminate 20B in Fig. 4 has a layered structure in which a release liner 3, a pressure-sensitive adhesive sheet 1, and an optical film 2 are layered in this order. By peeling off the release liner 3, the optical laminate 20B can be used as an optical film with a pressure-sensitive adhesive sheet.

[0138] The release liner 3 is typically a resin film. Examples of resins constituting the release liner 3 include polyesters such as polyethylene terephthalate (PET), polyolefins such as polyethylene and polypropylene, polycarbonate, acrylic, polystyrene, polyamide, and polyimide. The surface of the release liner 3 that contacts the pressure-sensitive adhesive sheet 1 may be subjected to a release treatment. The release treatment is, for example, a treatment with a silicone compound. However, the release liner 3 is not limited to the above example. The release liner 3 is peeled off when the optical laminate 20B is used, for example, when it is attached to the image forming layer.

[0139] Another example of the optical laminate of the present embodiment is shown in Fig. 5. The optical laminate 20C in Fig. 5 has a laminated structure in which a release liner 3, a pressure-sensitive adhesive sheet 4, a retardation film 2B, a pressure-sensitive adhesive sheet 1, and a polarizing film 2A are laminated in this order. After the release liner 3 is peeled off, the optical laminate 20C can be used by being attached to, for example, an image forming layer.

[0140] A known adhesive sheet can be used as the adhesive sheet 4. The adhesive sheet 1 may be used as the adhesive sheet 4.

[0141] Another example of the optical laminate of this embodiment is shown in Fig. 6. Optical laminate 20D in Fig. 6 has a laminated structure in which a release liner 3, an adhesive sheet 4, a retardation film 2B, an adhesive sheet 1, a polarizing film 2A, and a protective film 5 are laminated in this order. After peeling off the release liner 3, optical laminate 20D can be used by being attached to, for example, an image forming layer.

[0142] The protective film 5 has a function of protecting the optical film 2 (polarizing film 2A) which is the outermost layer during distribution and storage of the optical laminate 20D and in a state where the optical laminate 20D is incorporated into an image display device. The protective film 5 may also function as a window to the external space in a state where it is incorporated into an image display device. The protective film 5 is typically a resin film. The resin constituting the protective film 5 is, for example, polyester such as PET, polyolefin such as polyethylene and polypropylene, acrylic, cycloolefin, polyimide, and polyamide, and polyester is preferable. However, the protective film 5 is not limited to the above examples. The protective film 5 may be a glass film or a laminated film including a glass film. The protective film 5 may be subjected to surface treatment such as anti-glare, anti-reflection, and anti-static.

[0143] The protective film 5 may be bonded to the optical film 2 by any pressure-sensitive adhesive. Bonding by a pressure-sensitive adhesive sheet 1 is also possible.

[0144] The optical laminate may have any configuration as long as it includes the pressure-sensitive adhesive sheet 1 and the optical film 2.

[0145] The optical laminate of this embodiment can be distributed and stored, for example, as a rolled body obtained by rolling up a strip-shaped optical laminate, or as a sheet-shaped optical laminate.

[0146] The optical laminate of the present embodiment is typically used in an image display device, such as a liquid crystal display, an organic EL display, or an inorganic EL display.

[0147] [Image display device] An example of the image display device of this embodiment is shown in Fig. 7. The image display device 21 in Fig. 7 has a laminated structure in which a substrate 7, an image forming layer (e.g., an organic EL layer or a liquid crystal layer) 6, an adhesive sheet 4, a retardation film 2B, an adhesive sheet 1, a polarizing film 2A, and a protective film 5 are laminated in this order. The image display device 21 has the optical laminates 20A, 20B, 20C, and 20D of Figs. 3 to 6 (excluding the release liner 3). The substrate 7 and the image forming layer 6 may have the same configurations as the substrate and the image forming layer, respectively, of a known image display device.

[0148] The image display device 21 in Fig. 7 may be an organic EL display or a liquid crystal display. However, the image display device 21 is not limited to this example. The image display device 21 may be an electroluminescence (EL) display, a plasma display (PD), a field emission display (FED), or the like. The image display device 21 may be used for home appliances, in-vehicle applications, public information displays (PID), and the like.

[0149] The image display device 21 may have any configuration as long as it includes the pressure-sensitive adhesive sheet 1 and / or the optical laminate 20. EXAMPLES

[0150] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the examples shown below.

[0151] [Monomer Syrup A1] 95.2 parts by weight of n-butyl acrylate (BA), 4.75 parts by weight of acrylic acid (AA), 0.05 parts by weight of 4-hydroxybutyl acrylate (HBA), and 0.2 parts by weight of 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)2-methylpropan-1-one (Omnirad127, IGM Resins) as a photopolymerization initiator were placed in a four-neck flask. Next, the liquid in the flask was irradiated with ultraviolet light under a nitrogen atmosphere to obtain a monomer syrup A1 in which the monomer was partially photopolymerized. The ultraviolet light irradiation was continued until the viscosity of the liquid in the flask (measurement conditions: BH viscometer No. 5 rotor, 10 rpm, measurement temperature 30°C) reached approximately 20 Pa·s.

[0152] [Monomer syrup A2~A14] Monomer syrups A2 to A14 were prepared in the same manner as for the monomer syrup A1, except that the monomers and photopolymerization initiators were changed as shown in Table 1.

[0153] [Table 1]

[0154] The abbreviations in Table 1 are as follows. BA: n-butyl acrylate AA: Acrylic acid HBA: 4-hydroxybutyl acrylate Omnirad127: 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)2-methylpropan-1-one (Omnirad127, IGM Resin) Omnirad1173: 2-hydroxy-2-methyl-1-phenylpropanone (Omnirad1173, IGM Resin) Omnirad184: 1-Hydroxycyclohexyl-phenyl ketone (Omnirad184, IGM Resin) Omnirad651: 2,2-dimethoxy-1,2-diphenylethan-1-one (Omnirad651, IGM Resins) Omnirad819: Bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (Omnirad819, IGM Resins) Omnirad907: 2-Methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one (Omnirad907, IGM Resins)

[0155] Omnirad184, Omnirad651, Omnirad819 and Omnirad907 do not have the chemical structure X in their molecules.

[0156] [Photocurable composition C1~C14] Next, the monomer syrup, the monomer, and the crosslinking agent were mixed so as to have the compositions shown in Table 2 below, thereby obtaining photocurable compositions C1 to C14.

[0157] [Table 2]

[0158] The abbreviations in Table 2 are as follows. AA: Acrylic acid NVP: N-vinyl-2-pyrrolidone NDDA: 1,9-nonanediol diacrylate

[0159] The final compositions of the monomers contained in the photocurable compositions C13 and C14 are shown in Table 3 below.

[0160] [Table 3]

[0161] The abbreviations in Table 3 are as follows. BA: n-butyl acrylate AA: Acrylic acid HBA: 4-hydroxybutyl acrylate NVP: N-vinyl-2-pyrrolidone

[0162] Example 1 [Preparation of release liner] Addition reaction curing type silicone (LTC761 containing hexenyl group-containing polyorganosiloxane, 30 wt% toluene solution, manufactured by Dow Corning Toray) 30 parts by weight, release control agent (BY24-850 containing unreactive silicone resin, manufactured by Dow Corning Toray) 0.9 parts by weight, curing catalyst (SRX212 containing platinum catalyst, manufactured by Dow Corning Toray) 2 parts by weight, and toluene / hexane mixed solvent (volume ratio 1: 1) as a dilution solvent were mixed to obtain a silicone-based release agent composition. The concentration of silicone solids in the release agent composition was 1.0 wt%. Next, the release agent composition was applied to one side of a liner substrate (Lumirror XD500P, a polyester film, thickness 75 μm) with a wire bar and heated at 130 ° C for 1 minute to prepare a release liner having a release layer (thickness 60 nm) on one side.

[0163] [Preparation of adhesive sheet] The photocurable composition C1 was applied to one side of a substrate sheet (Lumirror XD500P, a polyester film without a release layer, thickness 75 μm) using an applicator to form a coating layer (thickness 20 μm). Next, a release liner was placed on the formed coating layer to obtain a first laminate. The release liner was placed so that the release layer was in contact with the coating layer. Next, a light with an illuminance of 4 mW / cm was applied from the substrate sheet side of the first laminate. 2 The LED light was irradiated under the condition of 1000 nm, 1000 nm, and 200 seconds of irradiation time. The peak wavelength of this light was 340 nm. As a result, the coating layer was photocured, and the adhesive sheet of Example 1 (thickness 20 μm) sandwiched between the base sheet and the release liner was obtained. The illuminance of the light was measured using an illuminance meter (UD-T3040T2, manufactured by Topcon Technohouse Co., Ltd.) near the ultraviolet ray incident surface of the base sheet.

[0164] (Examples 2 to 3, 9 to 10 and Comparative Example 1) Pressure-sensitive adhesive sheets of Examples 2 to 3, 9 to 10 and Comparative Example 1 were obtained in the same manner as in Example 1, except that the photocurable composition used was changed as shown in Table 4.

[0165] (Examples 4 to 8 and Comparative Examples 2 to 5) The photocurable composition used was changed as shown in Table 4, and the illuminance of the irradiated light was changed to 14 mW / cm 2 Except for this change, pressure-sensitive adhesive sheets of Examples 4 to 8 and Comparative Examples 2 to 5 were obtained by the same method as in Example 1. In Example 7, an LED (LED365) having a peak wavelength at 365 nm was used as the light source.

[0166] [Polymerization rate of monomer group] The polymerization rate of the monomer group in each of the pressure-sensitive adhesive sheets of the Examples and Comparative Examples was calculated from the change in weight of the pressure-sensitive adhesive sheet before and after 2 hours of heat drying at 130° C. Specifically, the weight of the pressure-sensitive adhesive sheet immediately after peeling off the base sheet and release liner was defined as W0 (weight before drying), and the weight of the pressure-sensitive adhesive sheet after cooling for about 20 minutes at room temperature (23° C.) after the above heating was defined as W1 (weight after drying), and the polymerization rate was calculated from the formula: polymerization rate (%) = W1 / W0 × 100.

[0167] [Remaining amount of photopolymerization initiator] The composition of each pressure-sensitive adhesive sheet of the Examples and Comparative Examples was analyzed, and the remaining amount (content) of the photopolymerization initiator was calculated based on the results obtained. The composition analysis was performed using liquid chromatography (LC) under the following conditions. Equipment used: 1290 Infinity II (Agilent Technologies) Column: Acquity UPLC BEH C18 (Waters, 2.1 mmφ×100 mm, 1.7 μm) Eluent composition: Gradient conditions of ultrapure water / acetonitrile Column temperature: 40℃ Column flow rate: 0.2mL / min ·Injection volume: 2μL Detector: Photodiode array detector (PDA) Measurement wavelength: 190-400nm ·Extraction wavelength: Omnirad127=262nm, Omnirad1173=246nm, Omnirad184=246nm, Omnirad651=253nm, Omnirad819=296nm, Omnirad907=309nm Sample preparation method: Approximately 0.5 g of sample (adhesive sheet) was weighed, 2 mL of chloroform was added, and the mixture was shaken overnight. 8 mL of methanol was added to the resulting solution, and the supernatant was filtered through a 0.45 μm membrane filter. The filtrate was injected into the LC for analysis.

[0168] The evaluation results are shown in Table 4 below, together with the type and amount of the photopolymerization initiator used.

[0169] [Table 4]

[0170] As shown in Table 4, when compared at the same polymerization rate, the adhesive sheets of the examples formed from the photocurable composition containing the photopolymerization initiator having the chemical structure X in the molecule were able to reduce the amount of remaining photopolymerization initiator compared to Comparative Examples 1 and 5. In addition, in the adhesive sheets of Comparative Examples 2 to 4, the polymerization rate did not exceed 90%, and the amount of remaining monomer was excessive. The relationship between the polymerization rate and the amount of remaining photopolymerization initiator in each adhesive sheet of the examples and comparative examples is shown in FIG. 8. As shown in Table 4 and FIG. 8, the adhesive sheets of the examples were able to achieve a higher polymerization rate and a lower amount of remaining photopolymerization initiator compared to the adhesive sheets of the comparative examples. The dashed line in the graph shown in FIG. 8 corresponds to the formula: content of photopolymerization initiator (wtppm)=233×polymerization rate (%)−22200. Comparative Examples 2 to 4 are located to the left of the dashed line in the graph.

[0171] <<Further Examples>> [Monomer syrup A15~A17] Monomer syrups A15 to A17 were prepared in the same manner as for Monomer syrup A1, except that the monomers and photopolymerization initiators were changed as shown in Table 5. Table 5 also shows Monomer syrup A1, which has the same monomer composition and photopolymerization initiator blending amount.

[0172] [Table 5]

[0173] [Photocurable composition C15~C17] Next, photocurable compositions C15 to C17 were obtained by mixing the monomer syrup and the crosslinking agent so as to obtain the compositions shown in Table 6. Table 6 also shows photocurable composition C1, which has the same monomer composition of the monomer syrup and the same blending amount of the photopolymerization initiator.

[0174] [Table 6]

[0175] (Examples 11 to 14) The photocurable composition used was changed as shown in Table 7, and the illuminance of the irradiated light was changed to 9 mW / cm 2 Pressure-sensitive adhesive sheets of Examples 11 to 14 were obtained by the same method as in Example 1, except for changing the above. For each of the obtained pressure-sensitive adhesive sheets, the polymerization rate of the monomer group and the remaining amount of photopolymerization initiator were evaluated by the same methods as in Examples 1 to 10. The evaluation results are shown in Table 7 below, together with the type and amount of the photopolymerization initiator blended.

[0176] [Table 7]

[0177] As shown in Table 7, when compared at similar polymerization rates, the pressure-sensitive adhesive sheets of Examples 11 to 14 formed from photocurable compositions containing a photopolymerization initiator having chemical structure X in its molecule had a reduced amount of remaining photopolymerization initiator compared to Comparative Examples 1 and 5. Furthermore, the relationship between the polymerization rate and the remaining amount of photopolymerization initiator in the pressure-sensitive adhesive sheets of Examples 11 to 14 is located to the right of the dashed line shown in the graph of FIG. [Industrial Applicability]

[0178] The curable composition of the present invention can be used to form a pressure-sensitive adhesive sheet. [Explanation of symbols]

[0179] 1 Adhesive sheet 2. Optical Film 20A, 20B, 20C, 20D Optical laminate 21 Image display device

Claims

1. A photocurable composition for a pressure-sensitive adhesive sheet, comprising a monomer group and / or a partial polymer of the monomer group, and a photopolymerization initiator, The photopolymerization initiator is a compound having a chemical structure represented by the following formula (1) in its molecule: R in the above formula (1) 1 and R 2 are each independently a C1 to C8 alkyl group; -OH, a C1 to C4 alkoxy group, -CN, -COOR 51 , -OOCR 52 , or -NR 53 R 54 a C1-C4 alkyl group in which a hydrogen atom is replaced by; a C3-C6 alkenyl group; or 2 -C 6 H 4 -R 55 and R 1 and R 2 may be bonded to each other to form a C2 to C9 alkylene group, a C3 to C6 oxyalkylene group, or an azaalkylene group, X is -OR 56 , or -NR 57 R 58 and R 51 is a C1 to C8 alkyl group, R 52 is a C1-C4 alkyl group, R 53 and R 54 are each independently a hydrogen atom, a C1 to C12 alkyl group; -OH, a C1 to C4 alkoxy group, -CN and -COOR 59 a C2-C4 alkyl group, the hydrogen atom of which is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; or a cyclohexyl group, R 53 and R 54 are bonded to each other to form -O- or -N(R 60 )--, R 55 is a C1-C4 alkyl group, R 56 is a hydrogen atom, -SiR 62 3 , a C1 to C8 alkyl group, or a C3 to C6 alkenyl group; R 57 and R 58 represents an alkyl group having 1 to 12 carbon atoms; —OH, an alkoxy group having 1 to 4 carbon atoms, —CN, and —COOR 63 a C2-C4 alkyl group, the hydrogen atom of which is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; or a cyclohexyl group, R 57 and R 58 are bonded to each other to form -O- or -N(R 64 )--, R 59 is a C1-C4 alkyl group, R 60 represents a hydrogen atom, a C1-C4 alkyl group, an allyl group, a C1-C4 hydroxyalkyl group, -CH 2 CH 2 -COOR 61 or -CH 2 CH 2 CN, R 61 is a C1-C4 alkyl group, R 62 is a C1 to C6 alkyl group, R 63 is a C1-C4 alkyl group, R 64 represents a hydrogen atom, a C1-C4 alkyl group, an allyl group, a C1-C4 hydroxyalkyl group, -CH 2 CH 2 -COOR 65 or -CH 2 CH 2 CN, R 65 is a C1-C4 alkyl group, The chemical structure can be bonded to a hydrogen atom or a hydrogen atom-substituted structure via the carbon atom marked with * in formula (1). Photocurable composition for adhesive sheets. 【Chemistry 1】

2. The R 1 and the R 2 The photocurable composition of claim 1, wherein each of the groups is independently a C1 to C8 alkyl group.

3. The R 1 and the R 2 The photocurable composition of claim 1 , wherein:

4. The X is -OR 56 2. The photocurable composition of claim 1, wherein

5. The photocurable composition of claim 1, wherein X is --OH.

6. The photocurable composition according to claim 1 , wherein the chemical structure is a structure represented by the following formula (2): 【Chemistry 2】

7. The photocurable composition according to claim 1 , wherein the photopolymerization initiator is a compound having two or more of the chemical structures in one molecule.

8. The photopolymerization initiator is a compound represented by the following formula (3): R in the above formula (3) 1 ' and R 2 ' are each other and the R 1 and R 2 Independently of R 1 and R 2 is a group that can be X′ is, independently of X, a group which may be taken as X; A is -O-, -CYR 3 - or -C(CH 3 ) R 4 and Y is a hydrogen atom, -Cl, -Br, or -O-R 71 , -NR 72 R 73 , or -S-R 74 and R 3 represents a hydrogen atom, a C1-C8 alkyl group, a C3-C6 alkenyl group, a benzyl group, -CH 2 -C 6 H 4 -R 75 or a phenyl group, R 4 is a C1-C6 alkyl or alkylene group, the alkylene group being bonded to a carbon atom of a phenylene group contained in the compound of formula (3), R 71 is a hydrogen atom, -Si(R 76 ) 3 , a C1 to C12 alkyl group, a C2 to C18 acyl group, —CO—NH—R 77 , a C2 to C20 hydroxyalkyl group, a C2 to C20 methoxyalkyl group, 3-R 78 -2-hydroxypropyl, 3-[1,3,3,3-tetramethyl-1-[(trimethylsilyl)oxy]disiloxanyl]propyl, 2,3-dihydroxypropyl, or a C2-C21 hydroxyalkyl group or a C3-C25 alkyl group, the carbon chain of which is interrupted by 1 to 9 oxygen atoms; R 72 and R 73 are each independently a C1 to C12 alkyl group; -OH, a C1 to C4 alkoxy group, -CN, and -COOR 79 a C2-C4 alkyl group, the hydrogen atom of which is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; a cyclohexyl group; or a C7-C9 phenylalkyl group, R 72 and R 73 are bonded to each other to form -O- or -N(R 80 )--, R 74 represents a C1 to C18 alkyl group, a hydroxyethyl group, a 2,3-dihydroxypropyl group, a cyclohexyl group, a benzyl group, a phenyl group, a C1 to C12 alkylphenyl group, -CH 2 -COOR 81 -CH 2 CH 2 -COOR 82 or -CH(CH 3 )-COOR 83 and R 75 is a C1-C4 alkyl group, R 76 is a C1 to C6 alkyl group, R 77 is a C1 to C12 alkyl group, R 78 is a C1 to C18 alkoxy group, R 79 is a C1-C4 alkyl group, R 80 represents a hydrogen atom, a C1-C4 alkyl group, an allyl group, a benzyl group, a C1-C4 hydroxyalkyl group, -CH 2 CH 2 -COOR 84 or -CH 2 CH 2 CN, R 81 , R 82 and R 83 are each independently a C1 to C18 alkyl group, R 84 The photocurable composition according to claim 1, wherein is a C1 to C4 alkyl group. 【Chemistry 3】

9. The A is -CYR 3 The photocurable composition according to claim 8, wherein

10. The Y and R 3 The photocurable composition according to claim 9 , wherein is a hydrogen atom.

11. The photocurable composition according to claim 8 , wherein the photopolymerization initiator is a compound represented by the following formula (4): 【Chemistry 4】

12. 2. The photocurable composition according to claim 1, wherein the amount of the photopolymerization initiator in the photocurable composition is 0.01 to 1 part by weight per 100 parts by weight of the total of the monomer group and the partially polymerized product.

13. The photocurable composition of claim 1 , wherein the monomer group includes a (meth)acrylic monomer.

14. A pressure-sensitive adhesive sheet formed from the photocurable composition according to claim 1 .

15. The pressure-sensitive adhesive sheet according to claim 14 , wherein the polymerization rate of the monomer group in the pressure-sensitive adhesive sheet is 96% or more, and the content of the photopolymerization initiator is 800 wtppm or less.

16. The pressure-sensitive adhesive sheet according to claim 14, wherein the pressure-sensitive adhesive sheet has a thickness of 300 μm or less.

17. An optical laminate comprising the pressure-sensitive adhesive sheet according to any one of claims 14 to 16 and an optical film.

18. The optical film is a polarizing film, The optical laminate according to claim 17 , wherein the pressure-sensitive adhesive sheet is in contact with the polarizing film.

19. An image display device comprising the optical laminate according to claim 17.

Citation Information

Patent Citations

  • Adhesive composition, adhesive layer, adhesive sheet, optical member, and touch panel

    JP2019070150A

Cited By

  • Optical laminate and image display device using same

    CN122776376A

  • Optical laminate and image display device using same

    CN122794574A