Glossy coating material, surface finishing method and top board
A glossy coating material with specific aggregates and resin composition, applied and polished, addresses the lack of hardness and gloss in existing materials, resulting in a durable and glossy finish for surfaces.
Patent Information
- Application Number
- JP2024039595
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-14
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-03-14
AI Technical Summary
Existing glossy coating materials lack the necessary hardness to be applied on surfaces like tabletops and do not possess both glossiness and mechanical strength.
A glossy coating material comprising specific aggregates with varying Mohs hardness, combined with cement and synthetic resin, is applied and polished to create a finishing layer with a hardness of 7H or more, achieving both glossiness and durability.
The solution provides a glossy and durable finishing layer suitable for surfaces like tabletops, with enhanced mechanical strength and scratch resistance.
Smart Images

Figure 2024146809000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a glossy coating material, a surface finishing method, and a countertop. [Background technology]
[0002] Finishing layers with various functions are formed by applying coating materials to target surfaces such as walls, floors, fittings, furniture, tabletops, etc. and then hardening (drying) the materials.
[0003] For example, Patent Document 1 discloses a glossy wall coating material with high designability. Patent Document 2 discloses an inorganic and organic hybrid non-flammable paint that has flexibility, coating film strength, and high toughness. Patent Document 3 discloses a non-flammable wood grain decorative material that is less susceptible to aging such as peeling and swelling. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-115293 A [Patent Document 2] JP 2013-43891 A [Patent Document 3] JP 2009-101607 A Summary of the Invention [Problem to be solved by the invention]
[0005] The material in Patent Document 1 has gloss but does not have the hardness required for use as a tabletop, while the materials in Patent Documents 2 and 3 are non-flammable and have excellent mechanical strength but do not have gloss.
[0006] The present invention has been made in consideration of the above-mentioned matters, and its object is to provide a glossy coating material, a surface finishing method, and a tabletop that have a hardness that makes them usable on target surfaces such as tabletops, while also having a glossy finish. [Means for solving the problem]
[0007] The gloss coating material according to the first aspect of the present invention is 30-65% by weight of aggregate; 10 to 40% by weight of a cement material; 2 to 10% by weight of a synthetic resin; Water; The aggregate includes a powder having a Mohs hardness of greater than 6 and a powder having a Mohs hardness of less than 4, and the average particle size of the powder having a Mohs hardness of greater than 6 is greater than the average particle size of the powder having a Mohs hardness of less than 4. It is characterized by:
[0008] It is also preferable that the powder having a Mohs hardness of greater than 6 is silica sand, and the powder having a Mohs hardness of less than 4 is one or more types selected from the group consisting of talc, calcium carbonate, and aluminum hydroxide.
[0009] The ratio of the average particle size of the powder having a Mohs hardness of greater than 6 to the average particle size of the powder having a Mohs hardness of less than 4 is preferably 1.4:1 to 600:1.
[0010] It is also preferable that the powder having a Mohs hardness of greater than 6 has an average particle size of 100 to 600 μm, and the powder having a Mohs hardness of less than 4 has an average particle size of 1 to 70 μm.
[0011] The blending ratio of the powder having a Mohs hardness of greater than 6 to the powder having a Mohs hardness of less than 4 is preferably 3:1 to 6:1 by weight.
[0012] The gloss coating material may also be used for a tabletop.
[0013] A surface finishing method according to a second aspect of the present invention comprises: A step of applying the gloss coating material according to the first aspect of the present invention to a target surface while pressing the material against the target surface; A step of polishing the surface of the finishing layer formed by hardening the glossy coating material with an abrasive; Equipped with It is characterized by:
[0014] Alternatively, polishing may be performed using a sander equipped with the abrasive material.
[0015] A top plate according to a third aspect of the present invention comprises: A countertop having a finishing layer, The finishing layer is The concrete comprises 30-65% by weight of aggregate, 10-40% by weight of cement material, 2-10% by weight of synthetic resin and water, the aggregate contains powder having a Mohs hardness of greater than 6 and powder having a Mohs hardness of less than 4, and the powder having a Mohs hardness of greater than 6 has an average particle size larger than the powder having a Mohs hardness of less than 4. The concrete is formed by applying a gloss coating material, hardening the material, and polishing the material with an abrasive. The surface of the finishing layer has a scratch hardness of 7H or more as defined in JIS K5600-5-4. It is characterized by:
[0016] A coating layer may also be provided on the finish layer.
[0017] The glossy coating material according to the fourth aspect of the present invention is 30 to 70% by weight of aggregate; 10 to 40% by weight of a cement material; 2 to 10% by weight of a synthetic resin; Water; The aggregate includes a powder having a Mohs hardness of greater than 6 and a powder having a Mohs hardness of less than 4, and the average particle size of the powder having a Mohs hardness of greater than 6 is greater than the average particle size of the powder having a Mohs hardness of less than 4. It is characterized by: Effect of the Invention
[0018] According to the present invention, it is possible to provide a glossy coating material that has a hardness suitable for use on target surfaces such as tabletops, yet also has gloss, a surface finishing method, and a tabletop. [Brief description of the drawings]
[0019] [Figure 1] 1(A) to (C) are schematic diagrams illustrating the surface finishing method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] <Glossy coating material> The gloss coating material becomes a finishing layer by being applied to a target surface such as a table or desk top, a wall, a floor, etc., and hardening. The gloss coating material contains aggregate, cement material, synthetic resin, and water.
[0021] The aggregate includes powders having a Mohs hardness of more than 6 and powders having a Mohs hardness of less than 4. Powders having a Mohs hardness of more than 6 function to increase the mechanical strength of the finishing layer, particularly to increase the hardness. Powders having a Mohs hardness of less than 4 function to increase the gloss. The Mohs hardness is an index of the hardness of a material, and is expressed on a scale of 1 to 10 as the difficulty of scratching a material when scratched with a certain object. The powders having a Mohs hardness of more than 6 in the present invention are preferably powders having a Mohs hardness of 6.5 to 10, and more preferably powders having a Mohs hardness of 7 to 8. The powders having a Mohs hardness of less than 4 in the present invention are preferably powders having a Mohs hardness of 0.5 to 3.5, and more preferably powders having a Mohs hardness of 1 to 3.
[0022] The average particle size of the powder with a Mohs hardness of more than 6 is larger than that of the powder with a Mohs hardness of less than 4. As a result, in the finishing layer, the powder with a Mohs hardness of less than 4 is located so as to fill the gaps between the powders with a Mohs hardness of more than 6. The close contact between the aggregates increases the bonding strength, leading to an improvement in the mechanical strength of the finishing layer. In addition, the powder with a Mohs hardness of less than 4 is easily exposed on the surface of the finishing layer, and as will be explained in the surface finishing method described later, the glossiness of the finishing layer is fully exhibited. The average particle size of the present invention can be measured as follows. Using sieves and trays with different openings, stack the sieves so that the sieve with the larger openings is on the top of the tray. A sample is placed on top of the top sieve, and the sieves with the larger openings are stacked on the tray so that the sieve with the larger openings is on the top. The stacked sieves are set in a sieve shaker and shaken for 10 minutes to perform sieving. The sieve shaker may be used at a vibration frequency of 3600 times per minute and an amplitude of 1 mm. The method and tools (sieves) described in JIS Z 8815 and JIS Z 8801 may be used to measure particle size distribution.
[0023] The ratio of average particle size of the powder having a Mohs hardness of greater than 6 to the powder having a Mohs hardness of less than 4 may be such that the powder having a Mohs hardness of less than 4 sufficiently fills the gaps between the powder having a Mohs hardness of greater than 6 in the finishing layer, and the powder having a Mohs hardness of less than 4 can be exposed on the surface of the finishing layer, and is, for example, 1.4:1 to 600:1, preferably 6:1 to 450:1, more preferably 10:1 to 450:1, and even more preferably 15:1 to 70:1.
[0024] The powder having a Mohs hardness of more than 6 may be any material capable of exerting the above-mentioned functions, and specifically, may be silica sand. The average particle size of the powder having a Mohs hardness of more than 6 may be set according to the thickness of the finishing layer to be formed, and is, for example, 100 to 600 μm, and preferably 200 to 450 μm.
[0025] The powder having a Mohs hardness of less than 4 may be any material capable of exerting the above-mentioned functions, and specifically includes talc, calcium carbonate, aluminum hydroxide, gypsum, mica, clay, and kaolin. Among these, one or more selected from the group consisting of talc, calcium carbonate, and aluminum hydroxide are preferable. The average particle size of the powder having a Mohs hardness of less than 4 is smaller than the average particle size of the powder having a Mohs hardness of more than 6, for example, 1 to 70 μm, preferably 1 to 30 μm, and more preferably 1 to 20 μm. If the average particle size of the powder having a Mohs hardness of less than 4 is larger than the above range, sufficient gloss cannot be obtained. Although the cause is not clear, it is considered that, when the average particle size is larger than the above range, the powder having a Mohs hardness of less than 4 in the finishing layer is difficult to be uniformly arranged, so that the reflection of light is scattered and it is difficult to achieve surface reflection.
[0026] The content of aggregate in the glossy coating material is 30-65% by weight or 30-70% by weight, more preferably 30-65% by weight, and even more preferably 45-65% by weight. If the content of aggregate is less than the above range, the viscosity of the glossy coating material is insufficient, and when the glossy coating material is applied to the target surface, it is easy to drip and the trowel separation is poor. Therefore, the application workability is deteriorated. In addition, the base cannot be concealed, and the base is visible, which may impair the aesthetic appearance. On the other hand, if the content is more than the above range, the glossy coating material becomes rough and difficult to apply to a certain thickness, and the application workability is deteriorated, and the content of cement material and synthetic resin is relatively reduced, and the strength of the finishing layer is reduced.
[0027] The blending ratio of the powder having a Mohs hardness of greater than 6 to the powder having a Mohs hardness of less than 4 is preferably 3:1 to 6:1 by weight.
[0028] The cement material functions as an inorganic binder, and aggregates and connects the aggregate together with the synthetic resin described later. By including the cement material, the mechanical strength can be increased, and the fire resistance and creep resistance of the finishing layer can be improved. Examples of the cement material include ordinary Portland cement, white cement, and fly ash cement. When using the color pigment described later, it is preferable to use white cement from the viewpoint of the color development of the color pigment. The content of the cement material in the gloss coating material is 10 to 40% by weight, and preferably 17 to 35% by weight.
[0029] The synthetic resin functions as an organic binder and exhibits a coating film forming ability. The synthetic resin may be water-soluble or water-dispersible, and any conventionally known synthetic resin may be used without any particular limitation as long as it exhibits the above-mentioned function. Examples of synthetic resins include acrylic resins, polyvinyl acetate resins, polyurethane resins, silicon resins, fluorine resins, epoxy resins, phenolic resins, polyester resins, alkyd resins, polycarbonate resins, and melamine resins, and these can be used alone or in combination of two or more. In addition, these synthetic resins may be modified, such as urethane-modified acrylic resins, or may be graft-polymerized, or may be in the form of dispersed particles. In addition, in order to increase the water resistance of the finishing layer, acrylic resins are preferred as synthetic resins. Examples of acrylic resins include acrylic acid esters, acrylic methacrylic copolymers, acrylic styrene copolymers, and acrylic resin ethylene vinyl acetate copolymers.
[0030] In addition, the content of synthetic resin in the gloss coating material is 2 to 10% by weight, and more preferably 4 to 6% by weight. If the content of synthetic resin is less than the above range, the water resistance of the finishing layer will decrease. On the other hand, if the content of synthetic resin is more than the above range, the curing speed will be too fast and the trowel separation will be poor, which will lead to a deterioration in application workability, and the relative decrease in the content of aggregate will make it impossible to hide the base, and the base will be visible, which may result in a poor appearance.
[0031] The synthetic resin may be used in the form of a synthetic resin emulsion. In this case, the content of solids (synthetic resin) in the synthetic resin emulsion in the gloss coating material falls within the range of the synthetic resin content described above.
[0032] The water content in the gloss coating material is about 10 to 20% by weight. When the synthetic resin is used as a synthetic resin emulsion, the total water content including the water content in the synthetic resin emulsion falls within the above water content range.
[0033] In addition to the above components, the glossy coating material may contain additives such as thickeners, dispersants, deodorants, preservatives, antifungal agents, antifoaming agents, antifreeze agents, formaldehyde adsorption / decomposition agents, surface skinning prevention agents, water repellents, hardening retarders, air entraining agents (AE agents), water reducing agents, AE water reducing agents, high performance water reducing agents, high performance AE water reducing agents, fluidizing agents, foaming agents, foaming agents, leveling agents, and pH adjusters, if necessary. When additives are contained, the content of the additives in the glossy coating material is 0.001 to 2% by weight, and more preferably 0.01 to 1% by weight.
[0034] Water repellents include silicone-based water repellents such as alkylalkoxysilanes, such as n-propyltrimethoxysilane, hexyltrimethoxysilane, and phenyltrimethoxysilane, organopolysiloxanes, such as dimethylpolysiloxane, and modified silicones obtained by modifying organopolysiloxanes, such as alkyl-modified polysiloxanes, phenyl-modified polysiloxanes, polyester-modified polysiloxanes, and polyether-modified polysiloxanes; Paraffin-based water repellents such as paraffin wax; Examples of the water repellents include glyceryl stearate, stearic acid amide, zinc stearate, calcium stearate, stearic acid diethanolamide, magnesium stearate, aluminum stearate, zirconium stearate, pyridinium salt type such as stearamide methylpyridium chloride, methylol aramid type, ethylene urea type, and other stearin-based water repellents, and these can be used alone or in combination of two or more types.
[0035] As hardening retarders, organic acids such as citric acid, gluconic acid, glucoheptonic acid, arabinic acid, tartaric acid, malic acid, polyphosphoric acid, etc., or inorganic salts thereof such as sodium, potassium, calcium, magnesium, ammonium, etc.; Sugars or derivatives thereof, such as glucose, fructose, galactose, sucrose, xylose, arabinose, ribose, oligosaccharides, and dextran; Water-soluble polymers such as polyvinyl alcohol; Cellulose derivatives such as hydroxyethyl cellulose, carboxymethyl hydroxyethyl cellulose; Lignosulfonates such as sodium lignosulfonate and calcium lignosulfonate; Amino acids or amino acid salts; Peptide compounds; Boric acid or its salts, such as sodium metaborate, sodium tetraborate, potassium pentaborate; Zinc oxide, zinc chloride, zinc carbonate, lead monoxide, phosphates, silicofluorides, silicofluoride and phosphate complexes; Copper hydroxide; Borax; These may be used alone or in combination of two or more.
[0036] The glossy coating material may further contain a coloring pigment. The coloring pigment may be added to and mixed with the glossy coating material before use, that is, may be in the form of a set of the glossy coating material and the coloring pigment. In this way, by preparing a single type of glossy coating material and multiple types of coloring pigments, a coloring pigment that exhibits a desired color at the site of use can be selected and added to the glossy coating material to form a finishing layer of various colors, which is convenient.
[0037] <Surface finishing method> In the surface finishing method, first, the above-mentioned glossy coating material is applied to the target surface such as the top plate, wall surface, floor surface, etc. It is preferable to use an applicator such as a trowel that can apply the glossy coating material while pressing it against the target surface.
[0038] When the gloss coating material is applied without pressing it down, powder with a Mohs hardness of more than 6 floats on the top layer, as shown in Figure 1(A). Even if the material is cured (dried) in this state and polished with an abrasive material (described later), sufficient gloss is not achieved.
[0039] On the other hand, by applying the gloss coating material while pressing it against the target surface with an applicator, powder with a Mohs hardness of more than 6 will sink to the bottom layer, as shown in Figure 1(B). The gloss coating material is then cured (dried) in this state to form a finishing layer. Note that the surface of the finishing layer does not have sufficient gloss at this stage.
[0040] The surface of the formed finishing layer is then polished with an abrasive. As shown in FIG. 1(C), the smoother the polished area of the finishing layer, the glossier it becomes. Specifically, when the powder with a Mohs hardness of less than 4 is exposed on the surface and polished to increase the smoothness, the powder with a Mohs hardness of less than 4 becomes glossier. In this way, a finishing layer with a glossy surface can be obtained.
[0041] Abrasives include materials that have abrasive grains coated on a base material such as paper with an adhesive, such as abrasive paper, waterproof abrasive paper, and abrasive cloth, as well as grinding stones and other materials that can be used without restriction as long as they can polish powders, synthetic resins, and cement materials that have a Mohs hardness of less than 4 contained in the finishing layer.
[0042] In addition, the finishing layer can be polished using an electric tool such as an electric sander equipped with an abrasive material. Therefore, since the worker does not need to be highly skilled, anyone can easily produce a glossy finishing layer in a short time.
[0043] The finish layer formed by applying the glossy coating material meets the JIS K5600-5-4 hardness standard of 7H or more. Because the finish layer has a hardness of 7H or more, it is less susceptible to scratches caused by tableware, writing implements, etc. For this reason, it is particularly useful as a finish layer for table tops, desks, etc.
[0044] Alternatively, a base coating material may be applied to the surface of the object, cured (dried) to form a base layer, and then a gloss coating material may be applied as a top coat on the surface of the base layer. The base coating material is used to fill in the unevenness of the surface of the object to make it smooth, and any conventional base coating material, such as those using calcium carbonate or aluminum hydroxide as aggregate, may be used.
[0045] Furthermore, as described above, color pigments that exhibit various colors can be added to the gloss coating material to form finish layers of various colors.
[0046] In addition, various patterns can be applied. For example, a glossy coating material is applied so that it has unevenness. The unevenness can be formed by troweling, or the unevenness can be formed by rolling a roller having an uneven surface before the applied glossy coating material hardens (dries). Then, after the glossy coating material is hardened (dried) to form a finish layer having unevenness on the surface, only the convex parts are polished to increase the smoothness, so that the convex parts become a glossy surface having gloss, while the concave parts do not have gloss. In this way, a finish layer having a pattern represented by glossy parts and non-glossy parts is obtained.
[0047] Furthermore, a topcoat material may be applied to the surface of the finishing layer. By applying a colorless acrylic or urethane topcoat material, a coating layer can be formed, which can provide antifouling, water resistance, heat resistance, etc. These functions allow the glossiness of the finishing layer to be maintained for a long period of time.
[0048] <Tabletop> The top plate is a top plate for a table or a desk, and has a finish layer made of the above-mentioned glossy coating material formed on the surface. The finish layer has a scratch hardness of 7H or more as specified in JISK5600-5-4, so it is not easily scratched by tableware or writing implements, and has gloss and high designability. In addition, a coating layer made of the above-mentioned top coating material may be formed on the finish layer of the top plate. The coating layer enhances the anti-fouling properties, water resistance, heat resistance, etc. This protects the top plate even if a hot liquid or the like is spilled on it. In addition, dirt attached to the coating layer can be easily removed, so the finish layer will have a glossy finish for a long time. EXAMPLES
[0049] Each coating material (Examples 1 to 11, Comparative Examples 1 and 2) was prepared as follows. The raw materials used are shown below. <Aggregate> · Silica sand (average particle size: 600 μm, Shinozawa Silica Sand Industry Co., Ltd.) Silica sand (average particle size: 350 μm, Tokai Kiko Co., Ltd.) · Silica sand (average particle size: 100 μm, Shinozawa Silica Sand Industry Co., Ltd.) ·Kansuiseki (average particle size: 270 μm, product name: K-1 (1 rin), Sankyo Seifun Co., Ltd.) ·Talc (average particle size: 5 μm, product name: CL-100, Tamura Nameshi Kogyo Co., Ltd.) Calcium carbonate (average particle size: 5 μm, product name: #100, Sankyo Seifon Co., Ltd.) Calcium carbonate (average particle size: 20 μm, Sankyo Seifon Co., Ltd.) Calcium carbonate (average particle size: 65 μm, product name: G-100, Sankyo Seifon Co., Ltd.) Aluminum hydroxide (average particle size: 18 μm, product name: B-316, Armolix Co., Ltd.) <Cement materials> · White Cement (Pacific Cement Corporation) <Thickener> Carrageenan (product name: GENUVISCO carrageenan type JJ, Sansho Corporation) <Water repellent> Aluminum stearate (Kawamura Chemical Industries Co., Ltd.) Modified silane / siloxane (product name: Sitren P750, SKW East Asia Co., Ltd.) <Cure retarder> Citric acid (Fuso Chemical Co., Ltd.) Amino acid salts and peptide compounds (product name: R-Base, Marusen Chemical Co., Ltd.) <Coloring pigments> ·SK Select Color (product name) (Shikoku Kasei Building Materials Co., Ltd.) <Synthetic resin> Acrylic emulsion (product name: Polysol (registered trademark) AE-820, Resonac Co., Ltd.)
[0050] According to the composition shown in Tables 1 to 3, thickener and color pigment were added to water, and then the mixture was stirred to homogenize. Then, aggregate, cement material, water repellent, hardening retarder, and synthetic resin were added, and the mixture was stirred to homogenize, to prepare each of the coating materials of Examples 1 to 11 and Comparative Examples 1 and 2. The numbers in parentheses for each aggregate shown in Tables 1 to 3 indicate the average particle size of each aggregate.
[0051] [Table 1]
[0052] [Table 2]
[0053] [Table 3]
[0054] Each of the coating materials of Examples 1 to 11 and Comparative Examples 1 and 2 was applied to the surface of a vertically placed gypsum board (product name: Tiger Board, Yoshino Gypsum Co., Ltd.) while pressing it down with a trowel.
[0055] After each coating material was cured to form the respective finish layer, the surface of the finish layer was polished with an electric sander equipped with an abrasive (sandpaper). The polishing was performed by changing the grit size of the sandpaper in the order of 240, 400, 1000, and 2000.
[0056] The surface hardness, gloss and coating workability of each sample were evaluated by the following evaluation methods. The evaluation results are shown in Tables 4 and 5. Surface hardness evaluation (based on JISK5600-5-4) ○:Hardness 7H or higher ×: Hardness less than 7H Gloss evaluation ○: High gloss after polishing △: Slightly shiny after polishing ×: No gloss after polishing -Evaluation of application workability ○: No dripping of paint during work, and easy removal of trowel △: No dripping of paint during work ×: Paint drips during work
[0057] [Table 4]
[0058] [Table 5]
[0059] In Examples 1 to 4 and 8 to 11, the hardness met the hardness of 7H, and the gloss and application workability were also good. In Examples 5 and 6, the hardness met the hardness of 7H or more, and the gloss was also good, but the application workability was slightly poor. In Example 7, the hardness met the hardness of 7H or more, but the gloss and application workability were slightly poor. On the other hand, in Comparative Examples 1 and 2, the gloss and application workability were good, but the hardness did not meet the hardness of 7H.
Claims
1. 30 to 65% by weight of aggregate; 10 to 40% by weight of a cement material; 2 to 10% by weight of a synthetic resin; Water; The aggregate includes a powder having a Mohs hardness of greater than 6 and a powder having a Mohs hardness of less than 4, and the average particle size of the powder having a Mohs hardness of greater than 6 is greater than the average particle size of the powder having a Mohs hardness of less than 4. A glossy coating material characterized by:
2. The powder having a Mohs hardness of greater than 6 is silica sand, and the powder having a Mohs hardness of less than 4 is one or more selected from the group consisting of talc, calcium carbonate, and aluminum hydroxide.
2. The gloss coating material according to claim 1 .
3. the ratio of the average particle size of the powder having a Mohs hardness of greater than 6 to the average particle size of the powder having a Mohs hardness of less than 4 is 1.4:1 to 600:1; 3. The gloss coating material according to claim 2.
4. The powder having a Mohs hardness of greater than 6 has an average particle size of 100 to 600 μm, and the powder having a Mohs hardness of less than 4 has an average particle size of 1 to 70 μm.
4. The gloss coating material according to claim 3.
5. the blending ratio of the powder having a Mohs hardness of greater than 6 to the powder having a Mohs hardness of less than 4 is 3:1 to 6:1 by weight; 3. The gloss coating material according to claim 2.
6. the blending ratio of the powder having a Mohs hardness of greater than 6 to the powder having a Mohs hardness of less than 4 is 3:1 to 6:1 by weight; 5. The gloss coating material according to claim 4.
7. The glossy coating material for the top plate, 2. The gloss coating material according to claim 1 .
8. A step of applying the gloss coating material according to any one of claims 1 to 7 to a target surface while pressing the material against the target surface; A step of polishing the surface of the finishing layer formed by hardening the glossy coating material with an abrasive; Equipped with A surface finishing method comprising the steps of:
9. Polishing is performed using a sander equipped with the abrasive material. The surface finishing method according to claim 8.
10. A countertop having a finishing layer, The finishing layer is The concrete comprises 30-65% by weight of aggregate, 10-40% by weight of cement material, 2-10% by weight of synthetic resin and water, the aggregate includes powder having a Mohs hardness of greater than 6 and powder having a Mohs hardness of less than 4, and the aggregate is formed by applying a gloss coating material in which the average particle size of the powder having a Mohs hardness of greater than 6 is greater than the average particle size of the powder having a Mohs hardness of less than 4, hardening the gloss coating material, and then polishing the coating material with an abrasive; The surface of the finishing layer has a scratch hardness of 7H or more as defined in JIS K5600-5-4. A top plate characterized by the above.
11. A coating layer is provided on the finishing layer. The top plate according to claim 10 .
12. 30 to 70% by weight of aggregate; 10 to 40% by weight of a cement material; 2 to 10% by weight of a synthetic resin; Water; The aggregate includes a powder having a Mohs hardness of greater than 6 and a powder having a Mohs hardness of less than 4, and the average particle size of the powder having a Mohs hardness of greater than 6 is greater than the average particle size of the powder having a Mohs hardness of less than 4. A glossy coating material characterized by:
Citation Information
Patent Citations
Compounded polymer cement mortar powder composition for spraying surface preparation and method for execution of spraying surface preparation
JP1994024820A
Seismic retrofit decorative finishing covering structure
JP3038259U
Manufacturing method of decorative material
JP2009101607A
Inorganic or organic hybrid nonflammable coating
JP2013043891A
Paint material for glossy wall surfaces and wall surface finishing method
JP2018115293A