Decorative film
The decorative film with a polyurethane resin and resin particle surface protective layer, combined with an acrylic resin colored layer, addresses scratching and enhances weather resistance and curved surface adherence.
Patent Information
- Application Number
- JP2024049260
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-15
AI Technical Summary
Conventional decorative films for automobile exteriors using polyurethane are prone to scratching during application and lack sufficient weather resistance and curved surface followability.
A decorative film with a surface protective layer containing polyurethane resin and resin particles, and a colored layer made of acrylic resin, with specific particle content and load properties to enhance weather resistance and curved surface followability.
The film exhibits improved weather resistance, pasting workability, and curved surface followability, reducing the risk of scratching and maintaining appearance over time.
Smart Images

Figure 2024146840000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a decorative film. [Background technology]
[0002] In recent years, decorative films have been used instead of painting as a means of decorating the exterior of automobiles, in order to reduce the amount of solvent used in line with the reduction of CO2 emissions in line with the SDGs and to shorten construction times. As an example of a decorative film for the exterior of an automobile, a decorative film for the exterior of an automobile that uses polyurethane, which is flexible and has excellent weather resistance, is known in prior art document 1 (see, for example, Patent Document 1). In addition, as a method for imparting a matte finish to a decorative film for the exterior of an automobile, a technique for transferring the uneven surface of a coating substrate (see, for example, Patent Document 2) and a technique for making the film surface uneven by embossing (see, for example, Patent Document 3) are known. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2007-297569 A [Patent Document 2] JP 2008-110514 A [Patent Document 3] Patent Publication No. 2021-70300 Summary of the Invention [Problem to be solved by the invention]
[0004] However, when a conventional automobile exterior decorative film using polyurethane is applied to an automobile exterior material by pressing with a squeegee, the surface of the flexible polyurethane film may be scratched.
[0005] In view of the above circumstances, one aspect of the present invention aims to provide a decorative film that fully exhibits weather resistance, ease of application, and curved surface conformability. In this specification, the term "curved surface conformability" refers to the property of a decorative film that is difficult to lift off when applied to a curved portion such as an uneven portion. [Means for solving the problem]
[0006] In order to solve the above problems, a decorative film according to one embodiment of the present invention is a decorative film formed by laminating a surface protective layer and a colored layer, the surface protective layer contains a polyurethane resin and resin particles, and contains 2 to 11 parts by mass of the resin particles per 100 parts by mass of the polyurethane resin, the average particle diameter of the resin particles is 3 μm to 12 μm, the colored layer contains an acrylic resin and a colorant, the upper yield point load of the decorative film at 20°C is 14.6 N / 10 mm to 25.0 N / 10 mm, and the stress relaxation rate at 20°C is 53% to 58%. Effect of the Invention
[0007] According to one aspect of the present invention, it is possible to provide a decorative film that satisfactorily exhibits weather resistance, ease of application, and ability to conform to curved surfaces. [Brief description of the drawings]
[0008] [Figure 1] 1 is a diagram showing a layer structure of a decorative film according to an embodiment of the present invention; [Diagram 2] FIG. 2 is a diagram showing a microscope photograph of a cross section of a first example of a surface protective layer in an embodiment of the present invention. [Diagram 3] FIG. 4 is a photomicrograph of a cross section of a second example of a surface protective layer in an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present inventors have investigated the above problems and found that adding resin particles to a protective layer on the surface of an automobile exterior film using polyurethane is effective in preventing damage to the film surface during lamination work by pressing with a squeegee plate. The present inventors have also found that the presence of resin particles in the surface protective layer improves weather resistance. That is, the present inventors have found that the resin particles in the surface protective layer diffuse the ultraviolet light irradiated to the surface protective layer, reducing the amount of ultraviolet light reaching the colored layer, thereby improving weather resistance. The reason why the presence of resin particles in the surface protective layer improved weather resistance is presumably because the resin particles in the surface protective layer diffuse the ultraviolet light irradiated onto the surface protective layer, reducing the amount of ultraviolet light that reaches the colored layer.
[0010] The decorative film according to one embodiment of the present invention has a colored layer and a surface protective layer overlapping the colored layer. The colored layer and the surface protective layer will be described in detail later.
[0011] [Upper yield point load] The upper yield point load of the decorative film of this embodiment at 20° C. is 14.6 N / 10 mm or more and 25.0 N / 10 mm or less.
[0012] The upper yield point load of the decorative film is the boundary load at which the deformation of the decorative film changes from elastic deformation to plastic deformation when a load is applied to the decorative film. The temperature of the decorative film when measuring the upper yield point load is 20°C.
[0013] In this specification, unless otherwise specified, the upper yield point load of the decorative film means the upper yield point load of the laminated structure of the surface protective layer and the colored layer (hereinafter also referred to as the base film). For example, when the decorative film further has an adhesive layer described later, the upper yield point load of the decorative film is the upper yield point load of the laminate (similarly the base film) in which the surface protective layer, the adhesive layer, and the colored layer are laminated in this order. In addition, when the decorative film further has an adhesive layer described later, the upper yield point load of the decorative film is the upper yield point load of the laminate not including the adhesive layer.
[0014] When the upper yield point load of the decorative film is equal to or greater than a predetermined value, the occurrence of wrinkles during application tends to be suppressed, and when it is equal to or less than a predetermined value, the occurrence of lifting after application tends to be suppressed. From the viewpoint of improving application workability, the lower limit of the upper yield point load of the decorative film is 14.6 N / 10 mm or more, preferably 14.8 N / 10 mm or more, more preferably 15.0 N / 10 mm or more, even more preferably 16.0 N / 10 mm or more, even more preferably 16.3 N / 10 mm or more, and particularly preferably 17.0 N / 10 mm or more. In addition, from the viewpoint of improving the curved surface conformability, the upper limit value of the upper yield point load of the decorative film is 25.0 N / 10 mm or less, preferably 22.2 N / 10 mm or less, more preferably 20.0 N / 10 mm or less, even more preferably 19.5 N / 10 mm or less, even more preferably 19.2 N / 10 mm or less, and particularly preferably 18.0 N / 10 mm or less.
[0015] The upper yield point load can be determined by measuring a 10 mm wide sample made from a substrate film with a known measuring device such as a Tensilon universal testing machine. The upper yield point load is the load at the upper yield point of the sample observed in a tensile test, and since it is a load measured using a 10 mm wide sample, it is expressed in units of "N / 10 mm". The upper yield point load of the decorative film can be adjusted by the upper yield point load or material resin and thickness of each of the colored layer and the surface protective layer.
[0016] When the upper yield point load of the surface protective layer at 20°C is a specified value or more, the occurrence of wrinkles when the decorative film is applied tends to be more easily prevented, and when it is below the specified value, the occurrence of lifting after application tends to be more easily prevented. The lower limit of the upper yield point load of the surface protective layer is preferably 4.5N / 10mm or more, more preferably 5.0N / 10mm or more, even more preferably 5.5N / 10mm or more, even more preferably 5.6N / 10mm or more, and particularly preferably 5.8N / 10mm or more, from the viewpoint of improving the application workability. The upper limit of the upper yield point load of the surface protective layer is preferably 7.5N / 10mm or less, more preferably 7.3N / 10mm or less, and even more preferably 7.2N / 10mm or less, from the viewpoint of improving the curved surface conformability. The upper yield point load of the surface protective layer may be achieved by using a relatively soft polyurethane resin material alone, or may be adjusted by using two or more kinds of polyurethane resin materials in combination.
[0017] Similarly, if the upper yield point load of the colored layer at 20°C is a specified value or more, the occurrence of wrinkles when the decorative film is applied tends to be more easily prevented, and if it is a specified value or more, the occurrence of lifting after application tends to be more easily prevented. The lower limit of the upper yield point load of the colored layer is preferably 7.3N / 10mm or more, more preferably 8.3N / 10mm or more, and even more preferably 8.5N / 10mm or more, 9.0N / 10mm or more, or 10.0N / 10mm or more, from the viewpoint of improving the application workability. The upper limit of the upper yield point load of the colored layer is preferably 15.9N / 10mm or less, more preferably 13.2N / 10mm or less, even more preferably 12.0N / 10mm or less, and even more preferably 11.8N / 10mm or less, or 11.0N / 10mm or less, from the viewpoint of improving the curved surface conformability. The upper yield point load of the colored layer may be adjusted by using two or more kinds of acrylic resins having different upper yield point loads in combination in an appropriate ratio.
[0018] In the decorative film, the ratio of the upper yield point load of the colored layer to the upper yield point load of the surface protective layer may be, for example, 1 or more and 3 or less. The lower limit of the ratio may be preferably 1.1 or more, 1.2 or more, 1.4 or more, 1.6 or more, or 1.8 or more. The upper limit of the ratio may be preferably 2.6 or less, 2.2 or less, 2.0 or less, 1.9 or less, or 1.8 or less.
[0019] [Stress relaxation rate] The decorative film of this embodiment has a stress relaxation rate of 53% or more and 58% or less at 20°C. The stress relaxation rate of the decorative film is the rate of change in tensile load before and after stretching when a tensile load that stretches the decorative film by 5% (to 105% of its length) is applied for 5 minutes. The temperature of the decorative film when measuring the stress relaxation rate is 20°C. The stress relaxation rate of the decorative film is calculated from the following formula, where x is the tensile load immediately after 5% stretching and y is the tensile load 5 minutes after 5% stretching. Stress relaxation rate z[%]={(xy) / x}×100
[0020] In this specification, unless otherwise specified, the stress relaxation rate of the decorative film means the stress relaxation rate of the laminated structure (base film) of the surface protective layer and the colored layer. For example, when the decorative film further has an adhesive layer described later, the stress relaxation rate of the decorative film is the stress relaxation rate of the laminate (base film) in which the surface protective layer, the adhesive layer, and the colored layer are laminated in this order. In addition, when the decorative film further has an adhesive layer described later, the stress relaxation rate of the decorative film is the stress relaxation rate of the laminate not including the adhesive layer.
[0021] When the stress relaxation rate of the decorative film is a predetermined value or more, the occurrence of wrinkles during application of the decorative film tends to be more easily suppressed, and when it is less than the predetermined value, the occurrence of lifting after application tends to be more easily suppressed. From the viewpoint of improving application workability, the lower limit of the stress relaxation rate of the decorative film is 53% or more, preferably 54% or more, more preferably 55% or more, and even more preferably 56% or more. Moreover, from the viewpoint of improving curved surface conformability, the upper limit of the stress relaxation rate of the decorative film is 58% or less, preferably 57% or less.
[0022] The stress relaxation rate of the decorative film can be determined by measuring the tensile load with a known measuring device such as a Tensilon universal testing machine. The stress relaxation rate of the decorative film can be adjusted by adjusting the material resins of the colored layer and the surface protective layer or the thicknesses of both layers.
[0023] [Weather resistance] The decorative film of the present embodiment has weather resistance. The weather resistance can be expressed in various forms, and in this specification, it is evaluated by the stability of color (color specified by L* value, a* value, and b* value in the L*a*b* color space). The decorative film of this embodiment has an integrated light quantity of 1200 MJ / m 2 The color difference before and after irradiation with the light may be 3.0 or less, and is preferably 1.5 or less, 1.0 or less, 0.8 or less, 0.6 or less, 0.5 or less, or 0.4 or less. Alternatively, the decorative film of this embodiment has an integrated light amount of 1350 MJ / m 2 The color difference before and after irradiation with the light may be 4.0 or less, and preferably 2.0 or less, 1.0 or less, 0.8 or less, or 0.6 or less. These color differences indicate the same degree of weather resistance. The color difference of the decorative film is the L of the decorative film before the weather resistance test. * , a * , b * value, and L' of the decorative film after weather resistance test * , a' * , and b' * The value is measured, and the color difference ΔE is calculated from the following formula. * is the lightness, a * is the position between red / magenta and green (negative values are toward green, positive values are toward magenta), b * represents a position between yellow and blue (negative values are toward bluer, positive values are toward yellower). ΔE = {(L' * -L * ) 2 +(a' * -a * ) 2 +(b' * -b * ) 2} 1 / 2
[0024] From the viewpoint of the color stability of the decorative film (the stability of the decorative effect), it is preferable that ΔE is low. From such a viewpoint, ΔE is preferably 1.5 or less, more preferably 1.0 or less, and further preferably 0.5 or less.
[0025] The color difference of the decorative film can be measured using a known measuring device such as a colorimeter. The color difference of the decorative film can be realized by using a resin material having sufficient weather resistance, in other words, by using a resin material having sufficient weather resistance for at least one of an acrylic resin and a urethane resin. In addition, the weather resistance test may be accompanied by an accelerated test according to the use environment of the decorative film.
[0026] [Thickness] In the decorative film of this embodiment, the sum of the thickness of the surface protective layer and the thickness of the colored layer can be appropriately determined according to the application of the decorative film. For example, when the sum of the thickness of the surface protective layer and the thickness of the colored layer is a predetermined value or more, the application property and the curved surface conformability tend to be better. From the viewpoint of adjusting at least one of the application property and the curved surface conformability, the sum of the thickness of the surface protective layer and the thickness of the colored layer may be 75 μm or more, preferably 80 μm or more, more preferably 90 μm or more, and even more preferably 100 μm or more, or 120 μm or more.
[0027] In addition, when the total thickness of the surface protective layer and the colored layer is equal to or less than a predetermined value, the curved surface conformability tends to be better. For example, from the viewpoint of fully exhibiting the curved surface conformability, the total thickness of the surface protective layer and the colored layer may be equal to or less than 210 μm, preferably equal to or less than 200 μm, more preferably equal to or less than 180 μm, even more preferably equal to or less than 170 μm, and even more preferably equal to or less than 140 μm.
[0028] When the decorative film has an adhesive layer between the surface protective layer and the colored layer, the lower limit of the thickness of the base film, which is the sum of their thicknesses, may be, for example, 100 μm or more, preferably 120 μm or more, more preferably 140 μm or more, more preferably 150 μm or more, or even more preferably 160 μm or more, from the viewpoint of adjusting at least one of the application property and the curved surface conformability. Also, the upper limit of the thickness of the base film may be 220 μm or less, preferably 200 μm or less, more preferably 180 μm or less, and even more preferably 170 μm or less, from the viewpoint of fully expressing the curved surface conformability.
[0029] From the viewpoint of protecting the colored layer with a sufficient thickness, the lower limit of the thickness of the surface protective layer is preferably 15 μm or more, more preferably 20 μm or more, and even more preferably 25 μm or more. The upper limit of the thickness of the surface protective layer can be appropriately determined from the above viewpoint, and may be, for example, 60 μm or less, 50 μm or less, preferably 40 μm or less, or 35 μm or less.
[0030] The lower limit of the thickness of the colored layer is preferably 60 μm or more, more preferably 70 μm or more, or 90 μm or more. The upper limit of the thickness of the colored layer can be appropriately determined from the above viewpoints, and may be, for example, 150 μm or less, 130 μm or less, or 110 μm or less.
[0031] The decorative film may have a ratio of the thickness of the surface protective layer to the thickness of the colored layer of, for example, 0.10 or more and 1.00 or less. The lower limit of the ratio may be preferably 0.15 or more, 0.20 or more, or 0.25 or more. The upper limit of the ratio may be preferably 0.80 or less, 0.60 or less, 0.50 or less, or 0.40 or less.
[0032] [Colored layer] The colored layer contains an acrylic resin and a colorant, for example, a layer in which the colorant is dispersed in a matrix resin of an acrylic resin.
[0033] [Acrylic resin] The acrylic resin may be appropriately selected from known resins within a range that satisfies the physical properties described below as a decorative film or a colored layer. From the viewpoint of weather resistance, the acrylic resin may be a resin material that imparts sufficient weather resistance to the decorative film by itself, or may be a resin material that imparts sufficient weather resistance to the decorative film by combining with a polyurethane resin (laminated structure). Only one type of acrylic resin may be used, or two or more types may be used. The acrylic resin is a resin material that can realize the upper yield point load and stress relaxation rate of the decorative film. Here, "acrylic resin" is a general term for acrylic resin and methacrylic resin.
[0034] The acrylic resin is preferably a resin that can design the upper yield point load of the colored layer at 20°C to be 7.3N / 10mm or more and 15.9N / 10mm or less. For example, the acrylic resin may be one type of resin whose upper yield point load meets a predetermined requirement, or two or more types of resins with different hardness may be used in combination. When two or more types of resins with different hardness are used in combination, examples of the resin with relatively high hardness include acrylic resins used for films, sheets, etc. formed by melt extrusion. When two or more types of resins with different hardness are used in combination, examples of the resin with relatively low hardness include acrylic resins for adjusting fluidity and acrylic resins for soft materials.
[0035] From the viewpoint of achieving the mechanical strength required for the decorative film while realizing the above-mentioned physical properties, it is preferable that the acrylic resin contains a hard acrylic resin and a soft acrylic resin.
[0036] In this specification, the term "rigid acrylic resin" refers to an acrylic resin that, when made into a sheet material having a thickness of 100 μm and a width of 10 mm, has an upper yield point load of 10.0 N / 10 mm or more at 20° C. The upper yield point load can be measured by a known measuring device such as a Tensilon universal testing machine.
[0037] When the upper yield point load of the hard acrylic resin is a predetermined value or more, the workability of the decorative film (suppression of wrinkles during work) tends to be better, and when it is a predetermined value or less, the curved surface conformability of the decorative film tends to be better. For example, from the viewpoint of improving the workability of the decorative film, the upper yield point load of the hard acrylic resin may be 10.0N / 10mm or more, preferably 15.0N / 10mm or more, and more preferably 20.0N / 10mm or more. In addition, for example, from the viewpoint of improving the curved surface conformability of the decorative film, the upper yield point load of the hard acrylic resin is preferably 35.0N / 10mm or less, more preferably 30.0N / 10mm or less, and even more preferably 28.0N / 10mm or less.
[0038] The hard acrylic resin can be prepared by radical polymerization of known monomers capable of constituting an acrylic resin. Examples of hard acrylic resins include polymethyl methacrylate and methyl methacrylate-styrene copolymers.
[0039] Furthermore, the hard acrylic resin may be an acrylic resin having a Shore A hardness of more than 90. The "Shore A hardness" is, for example, the maximum value measured using a durometer GS-706N manufactured by Techlock Corporation when a Type A sensor is pressed perpendicularly against the surface of the measurement target with a load of 1 kg.
[0040] As the hard acrylic resin, for example, an acrylic resin having a Shore A hardness of more than 90 is selected as a first standard, and from the selected acrylic resins, a resin is selected that provides an upper yield point load of 10.0 N / 10 mm or more for the molded body, which is the sheet material. The hard acrylic resin may be a commercially available product, and examples thereof include Parapet (registered trademark) GR-F1000P (Kuraray Co., Ltd.), Kane Ace (registered trademark) MC-732 (Kaneka Co., Ltd.), Dianale LP-3202, 3207, 3130, and 3121 (all Mitsubishi Chemical Co., Ltd.), and Delpet (Asahi Kasei Co., Ltd.).
[0041] In this specification, the soft acrylic resin refers to an acrylic resin having an upper yield point load of less than 10.0 N / 10 mm at 20° C. when made into a sheet material of the above size. When the upper yield point load of the soft acrylic resin is a predetermined value or more, the application property of the decorative film (suppression of wrinkles during application) tends to be improved, and when it is a predetermined value or less, the curved surface conformability of the decorative film tends to be improved. For example, from the viewpoint of improving the application property of the decorative film, the upper yield point load of the soft acrylic resin is preferably 2.0 N / 10 mm or more, more preferably 3.0 N / 10 mm or more, and even more preferably 3.5 N / 10 mm or more. In addition, the upper limit value of the upper yield point load of the soft acrylic resin is, for example, less than 10.0 N / 10 mm, more preferably 7.0 N / 10 mm or less, and even more preferably 5.0 N / 10 mm or less, from the viewpoint of improving the curved surface conformability of the decorative film.
[0042] The soft acrylic resin may be an acrylic resin having a Shore A hardness of 70 or more and 90 or less. As the soft acrylic resin, for example, an acrylic resin having a Shore A hardness of 70 or more and 90 or less may be selected as a first standard, and from the selected acrylic resins, a resin that provides an upper yield point load of less than 10 N / 10 mm for the molded body that is the sheet material may be selected. The soft acrylic resin may be a commercially available product, and an example thereof is Parapet (registered trademark) SA-F1000P (Kuraray Co., Ltd.).
[0043] When a mixture of hard acrylic resin and soft acrylic resin is used as the acrylic resin, the mass-based mixing ratio of the soft acrylic resin to the hard acrylic resin may be, for example, 0.4 or more and 1.4 or less. The lower limit of the mixing ratio may be preferably 0.6 or more, or 0.9 or more. The upper limit of the mixing ratio may be preferably 1.2 or less, or 1.1 or less.
[0044] At least one of the hard acrylic resin and the soft acrylic resin may be formed from a resin composition containing core-shell particles in which a core particle having rubber elasticity is coated with an acrylic resin. The core-shell particles in which a core particle having rubber elasticity is coated with an acrylic resin may be formed by polymerization of a monomer mixture consisting of a core particle, an acrylic acid ester, and a polyfunctional monomer copolymerizable with the acrylic acid ester and another monofunctional monomer contained as necessary. At least one of the hard acrylic resin and the soft acrylic resin may be a thermoplastic elastomer.
[0045] Examples of acrylic acid esters include esters of acrylic acid and saturated aliphatic alcohols having 1 to 18 carbon atoms; esters of acrylic acid and alicyclic alcohols having 5 or 6 carbon atoms; and esters of acrylic acid and phenols or aromatic alcohols. More specifically, examples of acrylic acid esters include methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, s-butyl acrylate, t-butyl acrylate, pentyl acrylate, hexyl acrylate, octyl acrylate, 2-ethylhexyl acrylate, dodecyl acrylate, octadecyl acrylate, cyclohexyl acrylate, phenyl acrylate, and benzyl acrylate.
[0046] Examples of polyfunctional monomers include esters of unsaturated monocarboxylic acids and unsaturated alcohols, diesters of unsaturated monocarboxylic acids and glycols, diesters of dicarboxylic acids and unsaturated alcohols, divinyl compounds, and conjugated diene monomers. Examples of unsaturated monocarboxylic acids include acrylic acid, methacrylic acid, and cinnamic acid. Examples of unsaturated alcohols include allyl alcohol and methallyl alcohol. Examples of glycols include ethylene glycol, propanediol, butanediol, and hexanediol. Examples of dicarboxylic acids include phthalic acid, terephthalic acid, isophthalic acid, and maleic acid. More specifically, examples of the polyfunctional monomer include allyl acrylate, methallyl acrylate, allyl methacrylate, methallyl methacrylate, allyl cinnamate, methallyl cinnamate, diallyl maleate, diallyl phthalate, diallyl terephthalate, diallyl isophthalate, divinylbenzene, ethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, butadiene, iso Examples of the acrylates include methacrylate, ...
[0047] Examples of other monofunctional monomers include methacrylic acid esters, vinyl cyanide monomers, and aromatic vinyl monomers.
[0048] Examples of methacrylic acid esters include esters of methacrylic acid and saturated aliphatic alcohols having 1 to 22 carbon atoms, methacrylic acid and alicyclic alcohols having 5 or 6 carbon atoms, and esters of methacrylic acid and phenols or aromatic alcohols. More specifically, examples of methacrylic acid esters include methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, pentyl methacrylate, hexyl methacrylate, octyl methacrylate, 2-ethylhexyl methacrylate, dodecyl methacrylate, myristyl methacrylate, palmityl methacrylate, stearyl methacrylate, behenyl methacrylate, cyclohexyl methacrylate, phenyl methacrylate, and benzyl methacrylate.
[0049] Examples of aromatic vinyl monomers include styrene, α-methylstyrene, 1-vinylnaphthalene, 3-methylstyrene, 4-propylstyrene, 4-cyclohexylstyrene, 4-dodecylstyrene, 2-ethyl-4-benzylstyrene, 4-(phenylbutyl)styrene, and halogenated styrenes.
[0050] Examples of vinyl cyanide monomers include acrylonitrile and methacrylonitrile.
[0051] [Coloring agent] The colorant may be a known pigment or dye used in paints for printing on resin films. The colorant may be used alone or in combination of two or more. The colorant is used in an amount according to the desired color to be expressed in the decorative film. Examples of white colorants include titanium oxide and barium sulfate. Examples of black colorants include iron black, carbon black, and aniline black. Examples of yellow colorants include cadmium yellow and oil yellow 2G. Examples of orange colorants include chrome vermilion and cadmium orange. Examples of red colorants include cadmium red, permanent red 4R, and oil red. Examples of purple colorants include cobalt violet and anthraquinone violet. Examples of blue colorants include ultramarine, Prussian blue, and cobalt blue. Examples of green colorants include phthalocyanine green and chrome green.
[0052] The content of the colorant in the colored layer may be, for example, 10 parts by mass or more and 30 parts by mass or less, and preferably 15 parts by mass or more or 25 parts by mass or less, relative to 100 parts by mass of the acrylic resin.
[0053] [Surface protective layer] The surface protective layer is a layer overlapping the colored layer, and contains resin particles and polyurethane resin. The polyurethane resin is preferably a resin that can design the upper yield point load of the surface protective layer at 20°C to be 4.5 N / 10 mm or more and 7.5 N / 10 mm or less. The polyurethane resin is a resin material that affects the upper yield point load and stress relaxation rate of the decorative film described above, and the polyurethane resin or its material can be preferably selected from one-component thermoplastic resins used for film and sheet molding, or thermoplastic resins or thermoplastic elastomers for melt molding.
[0054] The polyurethane resin may be a resin material that imparts sufficient weather resistance to the decorative film by itself, or may be a resin material that imparts sufficient weather resistance to the decorative film by using it in combination with an acrylic resin (laminated structure). Only one type of polyurethane resin may be used, or two or more types may be used. Examples of such polyurethane resins include polycarbonate-based urethane resins and polycaprolactone-based urethane resins. These polyurethane resins have a main chain such as polycaprolactone and polycarbonate, and a urethane structure. Here, the urethane structure is preferably a urethane structure derived from an aliphatic isocyanate or an alicyclic isocyanate. The polyurethane resin may be a commercially available product, and examples thereof include Resamine (registered trademark) NE-8836, NE-8850, and NE-8811 (all from Dainichi Seikagaku Kogyo Co., Ltd.), Miractoran (registered trademark) E580, E585, E590, E595, E598, E980, E985, E990, E995, and E998 (all from Nippon Miractoran Co., Ltd.), NY88A10F, NY993-10HB4, and NY585N11A (all from F.C.I. Co., Ltd.), and CRISBON (registered trademark) NY-393, NY-331, and NY-328FTR (all from DIC Corporation).
[0055] [Resin particles] The surface protective layer contains resin particles. It is presumed that the resin particles scatter the light incident on the surface protective layer, thereby reducing the amount of ultraviolet light irradiated onto the colored layer, and thus weather resistance (color stability) is exhibited. In addition, the resin particles scatter the light incident on the surface protective layer, and therefore can impart a matte (matte) appearance to the decorative film. The resin particles are also suitable from the viewpoint of good dispersibility in the surface protective layer.
[0056] The resin particles may be particles having the above-mentioned light scattering properties. The resin particles may be used alone or in combination of two or more. Examples of the resin particles include urethane beads, nylon beads, acrylic beads, silicone beads, styrene beads, melamine beads, urethane acrylic beads, polyester beads, polyethylene beads, etc. The resin particles may include at least one type selected from the group consisting of these.
[0057] From the viewpoint of improving the scratch resistance of the decorative film, it is preferable that the resin particles contain at least one kind selected from the group consisting of urethane beads, nylon beads, and acrylic beads. The urethane beads are preferable from the viewpoint of improving the flexibility, toughness, and scratch resistance of the surface protective layer.
[0058] The particle shape of the resin particles is not limited, and examples thereof include spherical, tufted, long spheroidal, needle-like, etc. A spherical particle shape is preferred from the viewpoint of enhancing the scratch resistance of the surface protective layer.
[0059] The average particle size of the resin particles can be appropriately determined as long as it is 3 μm or more and 12 μm or less. For example, from the viewpoint of uniformly dispersing the resin particles in the surface protective layer, the particle size of the resin particles is preferably equal to or less than the thickness of the surface protective layer. In one embodiment, the resin particles may include particles having a particle size larger than the thickness of the surface protective layer. The particle size of the resin particles can be appropriately determined from the viewpoint of improving desired properties such as weather resistance, appearance, and scratch resistance.
[0060] From the viewpoint of enhancing the above-mentioned desired properties, the particle diameter of the resin particles is 3 μm or more and 12 μm or less in average particle diameter. If the average particle diameter of the resin particles is 3 μm or more and 12 μm or less, it is usually possible to adjust the appearance of the decorative film to a preferred glossy appearance by changing the particle diameter. The average particle diameter of the resin particles may be preferably 4 μm or more, 5 μm or more, or 8 μm or more.
[0061] The average particle size of the resin particles is the volume average particle size measured by the Coulter method. For example, the "Multisizer3" manufactured by Beckman Coulter can be used as a particle size distribution analyzer by the Coulter method. The average particle size of the resin particles can be adjusted by crushing, dividing, or mixing divided products.
[0062] When the content of resin particles in the surface protection layer is a specified value or more, the desired properties tend to be sufficiently expressed, and when it is a specified value or less, the desired properties of the surface protection layer tend to be sufficiently expressed.
[0063] In order to fully exhibit the desired properties of the surface protective layer, the content of the resin particles in the surface protective layer is 2 parts by mass or more and 11 parts by mass or less relative to 100 parts by mass of the polyurethane resin. The content of the resin particles may be 5 parts by mass or more, or 8 parts by mass or more.
[0064] The content of the resin particles per 100 parts by mass of the polyurethane resin is determined from the amount of the resin particles mixed during production, or the content can be determined from material analysis of the polyurethane resin and the resin particles and the ratio of the polyurethane resin and the resin particles in a specific region of the surface protective layer.
[0065] Furthermore, from the viewpoint of fully expressing the intended properties of the resin particles and the surface protective layer, the content of the resin particles in the surface protective layer may be, for example, 1.5 vol.% or more and 10 vol.% or less, and preferably 2.5 vol.% or more, 5 vol.% or more, or 9 vol.% or more.
[0066] The volume % is the ratio of the volume of the resin particles to the volume of the surface protective layer, and is calculated from the volume of the surface protective layer and the volume of the resin particles contained therein.
[0067] In one embodiment, the amount of resin particles present in the surface protective layer can be determined by observing a cross section of the surface protective layer. For example, the number of resin particles in the cross section of the surface protective layer is set to, for example, 280 particles / mm from the viewpoint of fully exhibiting the desired properties of the resin particles and the surface protective layer. 2 More than 2000 pieces / mm 2 The lower limit of the number of resin particles is preferably 500 particles / mm 2 More than 1000 pieces / mm 2 or more than 1800 pieces / mm 2 The upper limit of the number of resin particles is preferably 1900 particles / mm 2 or less than 1870 pieces / mm 2 It may be the following:
[0068] The number of resin particles in a cross section of the surface protection layer can be determined by observing the cross section of the surface protection layer with a microscope. For example, the cross section can be observed using a VHX DIGITAL MICROSCOPE (VHXS770) manufactured by Keyence Corporation, with the observation magnification set to 2000x and the observation mode set to coaxial one-way.
[0069] The urethane film constituting the above-mentioned surface protective layer has good dispersibility of the resin particles and is excellent in weather resistance, scratch resistance, etc., and is therefore suitable not only as a surface protective layer for decorative films but also as a general protective film. That is, as one aspect of the present invention, the present invention also includes a urethane film formed from a resin composition containing a polyurethane resin and resin particles having an average particle size of 3 μm or more and 12 μm or less, and containing 2 parts by mass or more and 11 parts by mass or less of the resin particles per 100 parts by mass of the polyurethane resin.
[0070] [Other ingredients] The colored layer and the surface protective layer may further contain other components other than the resin and the colorant as described above, within a range in which the effects of the present invention can be obtained. The content of the other components in each layer can be appropriately set within a range in which both the effects of the present invention and the effects of the other components can be obtained. Examples of the other components include ultraviolet absorbers, light stabilizers, plasticizers, and extender pigments. An example of the extender pigment is calcium carbonate.
[0071] The ultraviolet absorbing agent and the light stabilizer are preferable from the viewpoint of improving weather resistance. Examples of the ultraviolet absorbing agent include benzotriazole-based, benzophenone-based, cyanoacrylate-based, and ultrafine particle zinc oxide and titanium oxide. Examples of the light stabilizer include hindered amine-based.
[0072] The colored layer and the surface protective layer described above can achieve the effects of the present invention without containing other components. For example, in this embodiment, by using a soft polyurethane resin and two kinds of acrylic resins with different hardness, it is possible to achieve the desired upper yield point load and stress relaxation rate described above without containing a plasticizer. In this way, the embodiment in which the decorative film does not contain other components (such as plasticizers) for adjusting the upper yield point load and stress relaxation rate is a preferred embodiment.
[0073] The "other components for adjusting the upper yield point load and the stress relaxation rate" may be used in an amount that affects the upper yield point load and the stress relaxation rate within the range that satisfies the constitution of the present invention. Components that exhibit a desired function but do not substantially affect the upper yield point load and the stress relaxation rate, such as ultraviolet absorbers and light stabilizers, do not fall under the category of "other components for adjusting the upper yield point load and the stress relaxation rate." An embodiment in which the colored layer and the surface protective layer do not contain a plasticizer is a preferred embodiment from the viewpoint of suppressing bleeding out of the plasticizer.
[0074] [Other layers] The decorative film of the present embodiment may further have layers other than the above-mentioned colored layer and surface protective layer, as long as the effects of the present invention can be obtained. Examples of such layers include an adhesive layer and a pressure-sensitive adhesive layer.
[0075] The decorative film of this embodiment may further have an adhesive layer interposed between the colored layer and the surface protective layer to bond the two layers to each other. That is, the adhesive layer is disposed between the surface protective layer and the colored layer. The decorative film of this embodiment may further have an adhesive layer superposed on the colored layer on the side opposite to the surface protective layer. The thicknesses of the adhesive layer and the adhesive layer may be appropriately set, for example, in the range of 3 μm to 70 μm, preferably in the range of 10 μm to 50 μm, more preferably in the range of 20 μm to 45 μm, and even more preferably in the range of 25 μm to 40 μm, depending on the type of adhesive and the object to be adhered.
[0076] The adhesive layer is, for example, composed of a first adhesive. The adhesive layer is an adhesive layer for attaching the decorative film to an object to be decorated, and is, for example, composed of a second adhesive. For both the first adhesive and the second adhesive, various known adhesives such as rubber-based, acrylic-based, silicone-based, and polyvinyl ether-based adhesives can be applied. The first adhesive and the second adhesive may be the same or different. The first adhesive and the second adhesive may be, for example, an acrylic adhesive.
[0077] The acrylic pressure sensitive adhesive may be composed of a homopolymer of a (meth)acrylic acid ester or a copolymer with a copolymerizable comonomer.
[0078] Examples of the (meth)acrylic acid ester include alkyl esters of (meth)acrylic acid; hydroxyalkyl esters of (meth)acrylic acid; alkylaminoalkyl esters of (meth)acrylic acid; and glycidyl esters of (meth)acrylic acid. Examples of "alkyl esters" of (meth)acrylic acid include methyl ester, ethyl ester, butyl ester, 2-ethylhexyl ester, octyl ester, and isononyl ester. Examples of "hydroxyalkyl esters" of (meth)acrylic acid include hydroxyethyl esters, hydroxybutyl esters, and hydroxyhexyl esters. Examples of (meth)acrylic acid alkylaminoalkyl esters include dimethylaminoethyl methacrylate and t-butylaminoethyl methacrylate.
[0079] Examples of the copolymerizable comonomers include (meth)acrylic acid, itaconic acid, maleic anhydride, (meth)acrylic acid amide, (meth)acrylic acid N-hydroxymethylamide, vinyl acetate, styrene and acrylonitrile.
[0080] The above pressure-sensitive adhesive may further contain additives such as a crosslinking agent, a tackifier, a filler, an antioxidant, and a colorant, as required.
[0081] Examples of the crosslinking agent include an isocyanate-based compound, a melamine resin, a urea resin, a polyamine, an epoxy-based compound, a metal chelate compound, and a carboxyl group-containing polymer.
[0082] The above-mentioned adhesive may be an ultraviolet-curable adhesive composition further containing a polymerization initiator. The ultraviolet-curable adhesive composition may further contain an ultraviolet-curable component as necessary. When the polymer contained in the adhesive is an ultraviolet-curable polymer having a carbon-carbon double bond in the side chain, the adhesive may not contain the ultraviolet-curable component.
[0083] The polymerization initiator may be, for example, a material that is cleaved by ultraviolet light of an appropriate wavelength to produce radicals that can trigger a polymerization reaction. Examples of polymerization initiators include benzoin alkyl ethers, aromatic ketones, aromatic ketals, and thioxanthones. Examples of benzoin alkyl ethers include benzoin methyl ether, benzoin isopropyl ether, and benzoin isobutyl ether. Examples of aromatic ketones include benzil, benzophenone, and α-hydroxycyclohexyl phenyl ketone. An example of an aromatic ketal is benzyl dimethyl ketal. Examples of thioxanthones include chlorothioxanthone, dodecylthioxanthone, dimethylthioxanthone, and diethylthioxanthone.
[0084] Examples of the ultraviolet-curable component include esters of (meth)acrylic acid and polyhydric alcohols, and isocyanurate compounds.
[0085] Examples of esters of (meth)acrylic acid and polyhydric alcohols include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, tetraethylene glycol di(meth)acrylate, 1,6-hexanediol (meth)acrylate, neopentyl glycol di(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.
[0086] Examples of isocyanurate compounds include 2-hydroxyethylbis(2-acryloxyethyl)isocyanurate, tris(2-methacryloxyethyl)isocyanurate, and tris(2-methacryloxyethyl)isocyanurate.
[0087] [Specific Example] The layer structure of a decorative film according to one embodiment of the present invention is shown in Fig. 1. The decorative film 10 is disposed on the release surface of a release sheet 20. More specifically, the decorative film 10 is configured such that a surface protection layer 11, an adhesive layer 12, a colored layer 13, and a pressure-sensitive adhesive layer 14 are stacked on the release surface of the release sheet 20 in this order, starting from the pressure-sensitive adhesive layer 14.
[0088] The surface protective layer 11 may be made of a resin composition (polyurethane resin) containing, for example, at least one of a polycarbonate-based urethane resin and a polycaprolactone-based urethane resin, and an ultraviolet absorbing agent.
[0089] Resin particles are dispersed in the surface protective layer 11. The resin particles may be, for example, urethane resin beads or acrylic resin beads.
[0090] FIG. 2 shows a microscope photograph of a cross section of an example of the surface protective layer 11. The surface protective layer 11 in FIG. 2 contains 2 parts by mass of resin particles per 100 parts by mass of polyurethane resin. The thickness of the surface protective layer 11 in FIG. 2 is 24 μm. The thickness of the surface protective layer 11 is the distance between the portions on both sides where the resin particles are not exposed. The number of resin particles per cross-sectional area of the surface protective layer 11 in FIG. 2 is 280.6 particles / mm 2 The proportion of the resin particles in the surface protective layer 11 is 1.5% by volume.
[0091] Fig. 3 shows a micrograph of a cross section of another example of the surface protective layer 11. The surface protective layer 11 in Fig. 3 contains 10 parts by mass of resin particles per 100 parts by mass of polyurethane resin. The thickness of the surface protective layer 11 in Fig. 3 is also 24 µm. The number of resin particles per cross-sectional area of the surface protective layer 11 in Fig. 3 is 1772.6 particles / mm 2 The proportion of the resin particles in the surface protective layer 11 is 9.3% by volume.
[0092] Both the adhesive layer 12 and the pressure-sensitive adhesive layer 14 may be layers of an acrylic pressure-sensitive adhesive.
[0093] The colored layer 13 may be a layer in which a colorant such as a pigment is dispersed in a matrix resin. The matrix resin may be, for example, a resin composition (acrylic resin) containing at least one of a hard acrylic resin and a soft acrylic resin.
[0094] The decorative film 10 has sufficient weather resistance and can withstand, for example, an irradiation intensity of 75 mW / cm 2 The total light output is 1200MJ / m 2 It is preferable that the color difference before and after irradiation with an integrated light quantity of 1350 MJ / m be 3.0 or less. 2 It is more preferable that the color difference before and after irradiation with light is 4.0 or less.
[0095] The total thickness of the surface protective layer 11 and the colored layer 13 is preferably 75 μm or more. By appropriately setting the total thickness of the surface protective layer 11 and the colored layer 13 and the materials and physical properties of each layer, the upper yield point load of the decorative film 10 at 20° C. can be set to 14.6 N / 10 mm or more and 25.0 N / 10 mm or less, and the stress relaxation rate at 20° C. can be set to 53% or more and 58% or less.
[0096] It is presumed that the resin particles scatter the light incident on the surface protective layer 11, thereby reducing the amount of ultraviolet light irradiated on the colored layer 13 and suppressing color change in the decorative film 10. Furthermore, by including the resin particles, the decorative film 10 has improved scratch resistance and exhibits a stable matte appearance over time.
[0097] [Manufacturing method] The decorative film of the present embodiment can be produced by a method that enables the surface protective layer and the colored layer to be overlaid in this order.
[0098] For example, the decorative film of this embodiment can be manufactured by a method including the steps of preparing a colored layer, preparing a surface protective layer, and attaching the surface protective layer to the colored layer.
[0099] The step of preparing the colored layer may be a step of mixing an acrylic resin and a colorant and forming a film of the mixture obtained. The step of preparing the surface protective layer may be a step of manufacturing a layer of a polyurethane resin in which resin particles are dispersed. For example, the step of preparing the surface protective layer may be a step of mixing a polyurethane resin and resin particles and forming the mixture obtained into a film. The step of preparing the surface protective layer may be a step of applying a material of the surface protective layer to one surface of the colored layer to form a coating film, and then solidifying or curing the coating film.
[0100] The step of attaching the surface protective layer to the colored layer may be, for example, a step of directly bonding the colored layer and the surface protective layer by heat fusion or the like. The step of attaching the surface protective layer to the colored layer may also be a step of supplying the material of the other layer in a layer form to one surface of a colored layer or a surface protective layer prepared in advance, and bonding the other layer onto the one layer to form the other layer. Furthermore, the step of attaching the surface protective layer to the colored layer may be a step of attaching the surface protective layer to an adhesive layer obtained by applying a first adhesive to one surface of the colored layer. Attaching the colored layer and the surface protective layer via an adhesive layer is advantageous from the viewpoint of increasing the degree of freedom in material design of both layers.
[0101] In addition, the production of the decorative film may further include other steps other than the steps described above. Such other steps may be, for example, a step of laminating a colored layer to a coating film obtained by applying a second adhesive to a release sheet. The decorative film having an adhesive layer is advantageous from the viewpoint of increasing the convenience of the decorative film, since the decorative film can be attached to an object to be decorated by peeling off the release sheet.
[0102] [Application] The decorative film of the present embodiment is preferably used for applications in which the film is attached to an object to be decorated to decorate the object to be decorated. The decorative film of the present embodiment has weather resistance and is excellent in curved surface conformability and application workability, and is therefore preferably used as a film for vehicle exterior that is adhered to an exterior part of a vehicle.
[0103] 〔summary〕 As is clear from the above description, the decorative film (10) of the first embodiment of the present invention is a decorative film having a colored layer (13) containing a colorant and made of an acrylic resin, and a surface protective layer (11) containing resin particles and made of a polyurethane resin and overlapping the colored layer. The decorative film of the first embodiment of the present invention has an upper yield point load of 14.6 N / 10 mm or more and 25.0 N / 10 mm or less at 20°C, and a stress relaxation rate of 53% or more and 58% or less at 20°C. According to the first embodiment, a decorative film can be provided in which all of weather resistance, application workability (for example, application workability when applied to a curved surface), and curved surface conformability are fully exhibited. In addition, the dispersion of the resin particles in the surface protective layer is good.
[0104] The decorative film of the second aspect of the present invention is the first aspect, in which the average particle diameter of the resin particles is 3 μm or more and 12 μm or less, and the surface protective layer contains 2 parts by mass or more and 11 parts by mass or less of the resin particles per 100 parts by mass of the polyurethane resin. The second aspect is even more effective from the viewpoint of enhancing various desired properties of the decorative film, including the properties due to the resin particles.
[0105] The decorative film of the third aspect of the present invention is the first or second aspect, in which the acrylic resin contains a hard acrylic resin and a soft acrylic resin, and the polyurethane resin contains one or both of a polycarbonate-based urethane resin and a polycaprolactone-based urethane resin. The third aspect is preferable from the viewpoint of realizing the desired properties of the colored layer and the decorative film, and from the viewpoint of fully exhibiting all of the weather resistance, upper yield point load, and stress relaxation rate of the decorative film.
[0106] The decorative film of the fourth aspect of the present invention is any one of the first to third aspects, and further includes an adhesive layer (12) that is made of a first pressure-sensitive adhesive and is interposed between the colored layer and the surface protective layer to bond the two layers to each other. That is, the adhesive layer is disposed between the surface protective layer and the colored layer. The fourth aspect is even more effective from the viewpoint of increasing the degree of freedom in designing the resin materials of the colored layer and the surface protective layer.
[0107] The decorative film of the fifth aspect of the present invention is any one of the first to fourth aspects, and further includes an adhesive layer (14) made of a second adhesive and laminated on the opposite side of the colored layer to the surface protective layer. That is, the decorative film is formed by laminating the surface protective layer, the colored layer, and the adhesive layer in this order. The fifth aspect is even more effective from the viewpoint of increasing the convenience of the decorative film.
[0108] The decorative film of the sixth aspect of the present invention is a film for vehicle exterior use that is adhered to an exterior part of a vehicle in any one of the first to fifth aspects. Since a film for vehicle exterior use requires all of weather resistance, curved surface conformability, and application workability, the sixth aspect is suitable for use of such a film for vehicle exterior use.
[0109] The urethane film according to the seventh aspect of the present invention is formed from a resin composition containing a polyurethane resin and resin particles having an average particle size of 3 μm or more and 12 μm or less, and containing 2 parts by mass or more and 11 parts by mass or less of the resin particles per 100 parts by mass of the polyurethane resin. The urethane film is suitable as a protective film (e.g., a protective film for a decorative film) because the resin particles have good dispersibility and are excellent in weather resistance, scratch resistance, etc.
[0110] According to the above-mentioned configuration, it is possible to realize exterior decoration more easily than painting, and it is expected to contribute to reducing CO2 emissions in the decoration. The present invention, which has such an effect, is expected to contribute to the achievement of Goal 13 "Take urgent action to combat climate change" of the Sustainable Development Goals (SDGs) proposed by the United Nations, for example.
[0111] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in the different embodiments are also included in the technical scope of the present invention. EXAMPLES
[0112] An embodiment of the present invention will now be described.
[0113] [Material preparation] The following materials were prepared, and in the following, acrylic resin 1 and acrylic resin 3 correspond to hard acrylic resins, and acrylic resin 2 corresponds to soft acrylic resin. The average particle diameter of the resin particles is the volume average particle diameter. [Polyurethane resin] Polyurethane resin 1: Lezamin (registered trademark) NE-8836 (manufactured by Dainichiseika Chemicals Mfg. Co., Ltd., polycarbonate type) Polyurethane resin 2 NY88A10F (manufactured by FCI Co., Ltd., polyether type, melting temperature 150°C) Polyurethane resin 3 NY993-10HB4 (manufactured by FCI Co., Ltd., polycaprolactone type, melting temperature 160°C) Polyurethane resin 4 NY585N11A (manufactured by FCI Co., Ltd., polyester type, melting temperature 130℃) [Fluororesin] Fluorine resin Denka DX Film (manufactured by Denka Co., Ltd., product number 14S0230) [Acrylic resin] Acrylic resin 1: Parapet (registered trademark) GR-F1000P (manufactured by Kuraray Co., Ltd., upper yield point load at a film thickness of 100 μm is 27.1 N / 10 mm, Shore A hardness 100) Acrylic resin 2: Parapet (registered trademark) SA-F1000P (manufactured by Kuraray Co., Ltd., upper yield point load at a film thickness of 100 μm is 3.9 N / 10 mm, Shore A hardness 70) Acrylic resin 3 Kaneace (registered trademark) MC-732 (manufactured by Kaneka Corporation, upper yield point load is 16.0 N / 10 mm when the film thickness is 100 μm) [Vinyl chloride resin] Polyvinyl chloride resin Kanevinyl (registered trademark) S1001N (manufactured by Kaneka Corporation, average degree of polymerization 1050) [Resin particles] Resin particles 1 SE-010T (acrylic resin, average particle size 10 μm) Resin particles 2: Dimic beads (urethane resin, average particle size 10 μm) Resin particles 3 SE-006T (acrylic resin, average particle size 6 μm) [Adhesive] Adhesive: Tg=-37.4℃, adhesive made by crosslinking acrylic resin with a BA / AA composition ratio of 90:10 with aluminum chelate A (Kawaken Fine Chemicals Co., Ltd.) [Additives (UV absorbers)] Additive 1 Tinuvin (registered trademark) 234 (manufactured by BASF Japan Ltd., UVA) Additive 2 Tinuvin® 213 (manufactured by BASF Japan Ltd., UVA)
[0114] [Measurement method] The measurement methods used in the following Examples and Comparative Examples will be described. [Upper yield point load] A rectangular sample with a width of 10 mm and a length of 150 mm was prepared and subjected to a tensile test using a TENSILON (registered trademark, manufacturer: A&D, model number RTG-1310). Specifically, the distance between the chucks of the TENSILON was set to 100 mm, and the sample was clamped and fixed between the chucks. The sample was stretched at a constant tensile speed of 300 mm / min at 20°C, and the tensile load during stretching was measured. The load at the upper yield point was taken as the upper yield point load. [Stress relaxation rate] A rectangular sample with a width of 10 mm and a length of 150 mm was prepared, and a tensile test was performed using TENSILON (registered trademark, manufacturer: A&D, model number RTG-1310). More specifically, the distance between the chucks of the TENSILON was set to 100 mm, and the sample was clamped and fixed between the chucks. The sample was stretched by 5% at a tensile speed of 300 mm / min at 20°C, and the tensile load x immediately after 5% stretching and the tensile load y 5 minutes after 5% stretching were measured. The stress relaxation rate z was then calculated from the following formula. z[%]={(xy) / x}×100 [Weather resistance] Weather resistance test A of the decorative film was carried out using a Daipla Metal Weather (model KW-R7TP-A) manufactured by Daipla Wintes Co., Ltd. The sample stage on which the decorative film was placed was set at an inclination angle of 15°, the black panel temperature (BPT) was 63°C, and the light irradiation intensity was 75mW / cm. 2 The surface of the decorative film was wetted with water by showering for 2 minutes every 120 minutes, and this cycle was repeated for 445 hours. The cumulative light dose in the above test A was 1200MJ / m 2 The conditions of Test A correspond to a 3.0 year service life on an automotive surface.
[0115] In addition, a weather resistance test B of the decorative film was conducted using a Daipla Metal Weather (model KW-R7TP-A) manufactured by Daipla Wintes Co., Ltd. The sample stage on which the decorative film was placed was set at an inclination angle of 15°, the black panel temperature (BPT) was 63°C, and the light irradiation intensity was 75mW / cm. 2 The surface of the decorative film was wetted with water by showering for 2 minutes out of every 120 minutes, and this cycle was repeated for 500 hours. The cumulative light intensity in the above test B was 1350 MJ / m 2 The conditions of test B correspond to a 4.5-year service life on an automotive surface. (1) Color difference Using the KONICA MINOLTA SPECTRO PHOTO METER CM-3600A, the L of the decorative film before the weather resistance test was measured. * , a * , b *value, and L' of the decorative film after weather resistance test * , a' * , and b' * The color difference ΔE was calculated from the following formula: * is the lightness, a * is the position between red / magenta and green (negative values are toward green, positive values are toward magenta), b * represents a position between yellow and blue (negative values are toward bluer, positive values are toward yellower). ΔE = {(L' * -L * ) 2 +(a' * -a * ) 2 +(b' * -b * ) 2} 1 / 2 (2) Gloss A digital variable angle gloss meter (type UGV-5) manufactured by Suga Test Instruments Co., Ltd. was used to measure the change in gloss value at 60° of the decorative film before and after the weather resistance test. (3) Appearance The decorative film was visually observed before and after the weather resistance test to see whether there were any changes in appearance, such as scratches or discoloration. [Workability] A decorative film was applied to a portion of the outer surface of a car that included an uneven line, and the state of the decorative film applied to that portion was observed. (4) Floating (ability to follow curved surfaces) The decorative film attached to the above portion was left in an environment at 10° C. Separately, another decorative film attached to the above portion was left in an environment at 23° C. Then, the presence or absence of lifting during the time was visually observed. (5) Wrinkles during application (appliance) When the decorative film was attached to the above-mentioned portion, the occurrence of wrinkles in the decorative film was visually observed. (6) Surface damage during construction The decorative film was attached to the bonnet of an automobile by pressing it with a squeegee plate, and the surface of the decorative film was visually observed for the presence or absence of scratches or squeegee marks resulting from application. (7) Number density of resin particles in the surface protective layer A cross section of the surface protective layer, which is one side of a rectangular parallelepiped sample, was observed using a VHX DIGITAL MICROSCOPE (VHX S770) manufactured by Keyence Corporation at a magnification of 2000 times and in a coaxial single-sided observation mode. From the observation results of this cross section, the number density of resin particles per cross-sectional area of the surface protective layer was calculated using the following formula. In the formula, "Np" is the number of resin particles present in a specific region of the cross section. "Cs" is the area of the specific region of the cross section. Specifically, a rectangular region with one side having a length equal to the thickness of the surface protective layer and the other side having a length of about 150 μm was observed. Number density A [pieces / mm 2 ]=Np / Cs (8) Ratio of resin particles in the surface protective layer The above cross-sectional observation results were used to calculate the following formula. B [volume %] = (Bv × Np / Lv) × 100 "Bv" is the average volume of the resin particles and is calculated from the following formula: "r" is half the average particle diameter of the resin particles. Bv=4 / 3×π×r 3 "Lv" is calculated from the following formula: W is the average particle size of the resin particles. Lv=Cs×W
[0116] [Example 1] <Production of colored film (colored layer)> The following components were dry blended in the amounts shown below, then kneaded in a Henschel mixer, and then molded into a film with a thickness of 100 μm in a calendar molding machine set at 180° C. to produce colored film 1. The carbon black shown below was coated with an acrylic resin. The upper yield point load of the obtained colored film 1 was measured, and the upper yield point load of colored film 1 was 10.6 N / 10 mm. Acrylic resin 1 50 parts by weight Acrylic resin 2 50 parts by weight Carbon black 19 parts by weight Additive 1 0.3 parts by weight
[0117] <Manufacture of surface protective film (surface protective layer)> 2 parts by mass of resin particles 1 and 1.2 parts by mass of additive 2 were mixed into a dispersion liquid containing 100 parts by mass of polyurethane resin 1 in a 1:1 solution of isopropyl alcohol (IPA):toluene so that the solid content was 25% by mass, and then cast. Next, the mixture was dried at 80°C for 3 minutes, and then dried at 140°C for 3 minutes to form a film with a thickness of 30 μm. In this way, surface protection film 1 was produced. The upper yield point load of surface protection film 1 was 5.8 N / 10 mm.
[0118] <Adhesion of both films> An adhesive was applied to one surface of the colored film 1, and the surface protective film 1 was laminated on the coating of the adhesive formed, thereby adhering the surface protective film 1 to the colored film 1. In this way, a base film 1 was produced, which was composed of a colored layer, an adhesive layer made of adhesive, and a surface protective layer laminated in this order. The adhesive layer had a thickness of 30 μm. The upper yield point load of the obtained base film 1 was 17.0 N / 10 mm, and the percent stress relaxation rate of the base film 1 was 56%. The number density of resin particles in the surface protective layer of the base film 1 was 523.5 particles / mm 2 The content of the resin particles in the surface protective layer was 2.7% by volume.
[0119] <Adhesion to release sheet> An adhesive was applied onto a release film, and then the colored film 1 of the laminated film 1 was laminated and stuck onto the formed adhesive coating. In this way, a decorative film 1 was produced in which a release film, an adhesive layer made of an adhesive, the colored film 1, an adhesive layer, and a surface protective film 1 were laminated in this order. The thickness of the adhesive layer was 40 μm.
[0120] [Examples 2 and 3] Surface protection film 2 was produced in the same manner as in Example 1, except that the amount of resin particles 1 was changed to 6 parts by mass in the production of the surface protection film. The upper yield point load of surface protection film 2 was 7.1 N / 10 mm. Base film 2 and decorative film 2 were produced in the same manner as in Example 1, except that surface protection film 2 was used instead of surface protection film 1. The upper yield point load of base film 2 was 18.3 N / 10 mm, and the stress relaxation rate was 56%. The number density of resin particles in the surface protection layer of base film 2 was 1196.2 particles / mm 2 The content of the resin particles in the surface protective layer was 6.3% by volume.
[0121] Surface protection film 3 was produced in the same manner as in Example 1, except that the amount of resin particles 1 was changed to 10 parts by mass in the production of the surface protection film. The upper yield point load of surface protection film 3 was 7.2 N / 10 mm. Base film 3 and decorative film 3 were produced in the same manner as in Example 1, except that surface protection film 3 was used instead of surface protection film 1. The upper yield point load of base film 3 was 18.4 N / 10 mm, and the stress relaxation rate was 56%. The number density of resin particles in the surface protection layer of base film 3 was 1865.2 particles / mm 2 The content of the resin particles in the surface protective layer was 9.8% by volume.
[0122] [Examples 4 and 5] Surface protection film 4 was produced in the same manner as in Example 1, except that 10 parts by mass of resin particles 2 were used instead of 2 parts by mass of resin particles 1 in the production of the surface protection film. The upper yield point load of surface protection film 4 was 7.0 N / 10 mm. Substrate film 4 and decorative film 4 were produced in the same manner as in Example 1, except that surface protection film 4 was used instead of surface protection film 1. The upper yield point load of substrate film 4 was 18.2 N / 10 mm, and the stress relaxation rate was 56%. The number density of resin particles in the surface protection layer of substrate film 4 was 1869.2 particles / mm 2 The content of the resin particles in the surface protective layer was 9.6% by volume.
[0123] Surface protection film 5 was produced in the same manner as in Example 1, except that 10 parts by mass of resin particles 3 were used instead of 2 parts by mass of resin particles 1 in the production of the surface protection film. The upper yield point load of surface protection film 5 was 6.8 N / 10 mm. Base film 5 and decorative film 5 were produced in the same manner as in Example 1, except that surface protection film 5 was used instead of surface protection film 1. The upper yield point load of base film 5 was 18.0 N / 10 mm, and the stress relaxation rate was 56%. The number density of resin particles in the surface protection layer of base film 5 was 1867.0 particles / mm 2 The content of the resin particles in the surface protective layer was 9.6% by volume.
[0124] [Examples 6 to 8] In the production of the colored film, a colored film 6 was produced in the same manner as in Example 1, except that the amount of acrylic resin 1 was 55 parts by mass and the amount of acrylic resin 2 was 45 parts by mass. The upper yield point load of the colored film 6 was 11.8 N / 10 mm. A base film 6 and a decorative film 6 were produced in the same manner as in Example 3, except that the colored film 6 was used instead of the colored film 1. The upper yield point load of the base film 6 was 19.2 N / 10 mm, and the stress relaxation rate was 57%.
[0125] In addition, in the production of the colored film, a colored film 7 was produced in the same manner as in Example 1, except that the amount of acrylic resin 1 was 45 parts by mass and the amount of acrylic resin 2 was 55 parts by mass. The upper yield point load of the colored film 7 was 8.5 N / 10 mm. A base film 7 and a decorative film 7 were produced in the same manner as in Example 3, except that the colored film 7 was used instead of the colored film 1. The upper yield point load of the base film 7 was 16.3 N / 10 mm, and the stress relaxation rate was 56%.
[0126] Furthermore, in the production of the colored film, a colored film 8 was produced in the same manner as in Example 1, except that 30 parts by mass of acrylic resin 2 and 70 parts by mass of acrylic resin 3 were used instead of 50 parts by mass of acrylic resin 1 and 50 parts by mass of acrylic resin 2. The upper yield point load of the colored film 8 was 10.2 N / 10 mm. A base film 8 and a decorative film 8 were produced in the same manner as in Example 3, except that the colored film 8 was used instead of the colored film 1. The upper yield point load of the base film 8 was 18.0 N / 10 mm, and the stress relaxation rate was 56%.
[0127] [Examples 9 and 10] Surface protection film 9 was produced in the same manner as in Example 1, except that 50 parts by mass of polyurethane resin 1 and 50 parts by mass of polyurethane resin 3 were used instead of 100 parts by mass of polyurethane resin 1 in the production of the surface protection film. The upper yield point load of surface protection film 9 was 6.5 N / 10 mm. Substrate film 9 and decorative film 9 were produced in the same manner as in Example 1, except that surface protection film 9 was used instead of surface protection film 1. The upper yield point load of substrate film 9 was 17.7 N / 10 mm, and the stress relaxation rate was 56%. The number density of resin particles in the surface protection layer of substrate film 9 was 1865.2 particles / mm 2 The content of the resin particles in the surface protective layer was 9.8% by volume.
[0128] In addition, a surface protection film 10 was produced in the same manner as in Example 1, except that polyurethane resin 3 was used instead of polyurethane resin 1 in the production of the surface protection film. The upper yield point load of the surface protection film 10 was 5.8 N / 10 mm. A base film 10 and a decorative film 10 were produced in the same manner as in Example 1, except that surface protection film 10 was used instead of surface protection film 1. The upper yield point load of the base film 10 was 17.0 N / 10 mm, and the stress relaxation rate was 56%. In addition, the number density of resin particles in the surface protection layer of the base film 10 was 1865.2 particles / mm 2 The content of the resin particles in the surface protective layer was 9.8% by volume.
[0129] [Comparative Examples 1 and 2] Surface protection film C1 was produced in the same manner as in Example 1, except that the amount of resin particles 1 was changed to 12 parts by mass in the production of the surface protection film. The upper yield point load of surface protection film C1 was 7.3 N / 10 mm. Substrate film C1 and decorative film C1 were produced in the same manner as in Example 1, except that surface protection film C1 was used instead of surface protection film 1. The upper yield point load of substrate film C1 was 17.5 N / 10 mm, and the stress relaxation rate was 56%. The number density of resin particles in the surface protection layer of substrate film C1 was 2089.0 particles / mm 2 The content of the resin particles in the surface protective layer was 11.3% by volume.
[0130] In addition, in the production of the surface protection film, a surface protection film C2 was produced in the same manner as in Example 1, except that resin particles 1 were not used. The upper yield point load of the surface protection film C2 was 5.9 N / 10 mm. A base film C2 and a decorative film C2 were produced in the same manner as in Example 1, except that the surface protection film C2 was used instead of the surface protection film 1. The upper yield point load of the base film C2 was 17.1 N / 10 mm, and the stress relaxation rate was 56%.
[0131] [Comparative Example 3] In the production of the colored film, the colored film was formed to a thickness of 50 μm, and the same procedure as in Example 1 was used to produce the colored film C3. The upper yield point load of the colored film C3 was 6.5 N / 10 mm. The base film C3 and the decorative film C3 were produced in the same manner as in Example 1, except that the colored film C3 was used instead of the colored film 1. The upper yield point load of the base film C3 was 12.3 N / 10 mm, and the stress relaxation rate was 50%.
[0132] [Comparative Examples 4 and 5] In the production of the colored film, a colored film C4 was produced in the same manner as in Example 1, except that 60 parts by mass of acrylic resin 1 and 40 parts by mass of acrylic resin 2 were used. The upper yield point load of the colored film C4 was 14.2 N / 10 mm. The base film C4 and the decorative film C4 were produced in the same manner as in Example 3, except that the colored film C4 was used instead of the colored film 1. The upper yield point load of the base film C4 was 22.3 N / 10 mm, and the stress relaxation rate was 59%.
[0133] In addition, in the production of the colored film, a colored film C5 was produced in the same manner as in Example 1, except that 40 parts by mass of acrylic resin 1 and 60 parts by mass of acrylic resin 2 were used. The upper yield point load of the colored film C5 was 6.5 N / 10 mm. The base film C5 and the decorative film C5 were produced in the same manner as in Example 3, except that the colored film C5 was used instead of the colored film 1. The upper yield point load of the base film C5 was 14.5 N / 10 mm, and the stress relaxation rate was 54%.
[0134] [Comparative Examples 6 to 9] In the production of the colored films, the same procedure as in Example 1 was used except that 100 parts by mass of each of acrylic resins 1 to 3 and vinyl chloride resin was used instead of 50 parts by mass of acrylic resin 1 and 50 parts by mass of acrylic resin 2. The upper yield point load of colored film C6 was 27.1 N / 10 mm, the upper yield point load of colored film C7 was 3.9 N / 10 mm, the upper yield point load of colored film C8 was 16.0 N / 10 mm, and the upper yield point load of colored film C9 was 18.3 N / 10 mm.
[0135] Then, the base film C6 to C8 and the decorative film C6 to C8 were produced in the same manner as in Example 3, except that the colored film C6 to C8 were used instead of the colored film 1. The base film C9 and the decorative film C9 were produced in the same manner as in Example 1, except that the colored film C9 was used instead of the colored film 1. The upper yield point load of the base film C6 was 35.2 N / 10 mm, and the stress relaxation rate was 62%. The upper yield point load of the base film C7 was 12.0 N / 10 mm, and the stress relaxation rate was 50%. The upper yield point load of the base film C8 was 24.1 N / 10 mm, and the stress relaxation rate was 60%. The upper yield point load of the base film C9 was 23.9 N / 10 mm, and the stress relaxation rate was 68%.
[0136] [Comparative Examples 10 to 12] 100 parts by mass of each of polyurethane resin 4 to polyurethane resin 2 was mixed with 10 parts by mass of resin particles 1, 1.2 parts by mass of additive 2, and 19 parts by mass of carbon black, and then the composition was formed into a film having a thickness of 160 μm using an extruder under the conditions of a rotation speed of 7 rpm, a load of 30 A, and a line speed of 1.0 m / min at 160 ° C. Thus, each of surface protection films C10 to C12 was produced. The upper yield point load of surface protection film C10 was 9.8 N / 10 mm, the upper yield point load of surface protection film C11 was 11.3 N / 10 mm, and the upper yield point load of surface protection film C12 was 10.7 N / 10 mm.
[0137] Then, the base films C10 to C12 and the decorative films C10 to C12 were produced in the same manner as in Example 1, except that no adhesive layer or colored film was used. The upper yield point load of the base film C10 was 9.8 N / 10 mm, and the stress relaxation rate was 49%. The number density of the resin particles in the surface protective layer of the base film C10 was 1758.3 particles / mm 2The content of resin particles in the surface protective layer was 9.2% by volume. The upper yield point load of the base film C11 was 11.3 N / 10 mm, and the stress relaxation rate was 50%. The upper yield point load of the base film C12 was 10.7 N / 10 mm, and the stress relaxation rate was 50%. The number density of resin particles in the surface protective layer of the base film C11 was 1865.2 particles / mm 2 The content of the resin particles in the surface protective layer was 9.8% by volume. The number density of the resin particles in the surface protective layer of the base film C12 was 1865.2 particles / mm 2 The content of the resin particles in the surface protective layer was 9.8% by volume.
[0138] [Comparative Example 13] 10 parts by mass of resin particles 1, 1.2 parts by mass of additive 2, and 19 parts by mass of carbon black were mixed into a dispersion containing 100 parts by mass of polyurethane resin 1 in an IPA: toluene = 1: 1 solution so that the solid content was 25 mass%, and then cast. Next, it was dried at 80 ° C for 3 minutes, and then dried at 140 ° C for 3 minutes to form a film with a thickness of 160 μm. In this way, a surface protection film C13 was produced. The upper yield point load of the surface protection film C13 was 14.7 N / 10 mm. Then, the substrate film C13 and the decorative film C13 were produced in the same manner as in Example 1, except that the adhesive layer and the colored film were not used. The upper yield point load of the substrate film C13 was 14.7 N / 10 mm, and the stress relaxation rate was 51%. In addition, the number density of the resin particles in the surface protection layer of the substrate film C13 was 1865.2 pieces / mm 2 The content of the resin particles in the surface protective layer was 9.8% by volume.
[0139] [Comparative Examples 14 to 17] In the production of the colored films, the same procedure as in Example 1 was repeated except that 100 parts by mass of each of polyurethane resins 1 to 4 was used instead of 50 parts by mass of acrylic resin 1 and 50 parts by mass of acrylic resin 2. The upper yield point load of colored film C14 was 7.0 N / 10 mm, the upper yield point load of colored film C15 was 5.2 N / 10 mm, the upper yield point load of colored film C16 was 5.3 N / 10 mm, and the upper yield point load of colored film C17 was 5.0 N / 10 mm.
[0140] Then, the base film C14 to C17 and the decorative film C14 to C17 were produced in the same manner as in Example 3, except that the colored film C14 to C17 were used instead of the colored film 1. The upper yield point load of the base film C14 was 15.2 N / 10 mm, and the stress relaxation rate was 50%. The upper yield point load of the base film C15 was 13.3 N / 10 mm, and the stress relaxation rate was 50%. The upper yield point load of the base film C16 was 13.4 N / 10 mm, and the stress relaxation rate was 50%. The upper yield point load of the base film C17 was 13.1 N / 10 mm, and the stress relaxation rate was 50%.
[0141] [Comparative Examples 18 and 19] In the production of the surface protection film, a fluororesin was used instead of the polyurethane resin 1, the resin particles 1 was not used, and the thickness was 50 μm. The surface protection film C18 was produced in the same manner as in Example 1, except that the upper yield point load was 19.3 N / 10 mm. In addition, in the production of the colored film, a colored film C18 was produced in the same manner as in Example 1, except that 100 parts by mass of polyvinyl chloride vinyl chloride resin was used instead of 50 parts by mass of acrylic resin 1 and 50 parts by mass of acrylic resin 2. The upper yield point load of the colored film C18 was 22.3 N / 10 mm. And, the surface protection film C18 was used instead of the surface protection film 1, and the colored film C18 was used instead of the colored film 1. The upper yield point load of the base film C18 was 48.5 N / 10 mm, and the stress relaxation rate was 64%.
[0142] In addition, in the manufacture of the surface protection film, a surface protection film C19 was produced in the same manner as in Comparative Example 18, except that the thickness was 30 μm. The upper yield point load of the surface protection film C19 was 13.1 N / 10 mm. The substrate film C19 and the decorative film C19 were produced in the same manner as in Example 1, except that the surface protection film C19 was used instead of the surface protection film 1. The upper yield point load of the substrate film C19 was 23.4 N / 10 mm, and the stress relaxation rate was 60%.
[0143] The compositions and layer structures of the base films 1 to 10 and the decorative films 1 to 10 are shown in Table 1. The compositions and layer structures of the base films C1 to C9 and the decorative films C1 to C9 are shown in Table 2. The compositions and layer structures of the base films C10 to C19 and the decorative films C10 to C19 are shown in Table 3.
[0144] [Table 1]
[0145] [Table 2]
[0146] [Table 3]
[0147] [evaluation] The weather resistance and workability evaluations described above were carried out for each of the decorative films 1 to 10 and C1 to C19, and the results were evaluated based on the following criteria. The upper yield point load and stress relaxation rate were evaluated using the measurement results of a tensile test on the state (laminate consisting of the combination of the surface protection layer, adhesive layer, and colored layer, i.e., the base film) before bonding with the release film coated with adhesive. <Upper yield point load> A was between 15.0N / 10mm and 20.0N / 10mm. B: Greater than 20.0N / 10mm and less than 25.0N / 10mm. It was outside the range of CA and B (less than 15.0N / 10mm or greater than 25.0N / 10mm). <Stress relaxation rate> A: 53% or more and 58% or less. B: 48% or more but less than 53%. The range was outside CA and B (less than 48% or greater than 58%). <Color difference ΔE1200 (Test A, cumulative light amount 1200MJ / m 2 )> S ΔE≦1.0 A 1.0<ΔE≦1.5 B 1.5<ΔE≦3.0 C ΔE>3.0 <Color difference ΔE1350 (Test B, accumulated light amount 1350MJ / m 2 )> S ΔE≦1.0 A 1.0<ΔE≦1.5 B 1.5<ΔE≦4.0 C ΔE>4.0 <Gloss change> A The change in gloss value before and after the weather resistance test was within ±5. C The change in gloss value before and after the weather resistance test was greater than ±5. <Abnormal appearance> A There were no visible abnormalities. B: Minor abnormalities in appearance such as small scratches were observed. C: Visible scratches or yellowing or other obvious abnormalities in appearance were observed. <Float> S: No floating was observed even after more than two weeks in both floating evaluations at 10℃ and 23℃. A When evaluated for floating at 10°C, floating occurred within 72 hours but not later than 2 weeks. B Floating occurred within 72 hours after 24 hours at 10°C. C Floating occurred within 24 hours in both the 10℃ and 23℃ floatation evaluations. <Wrinkles during application> No (A) No wrinkles were generated when applied to the uneven lines of a car. Yes (C) Wrinkles occurred during application <Damage during construction> None (A) When the decorative film was pressed against the bonnet of a car with a squeegee plate, no scratches or squeegee marks were visible on the surface. (C) When the decorative film was pressed onto the bonnet of a car with a squeegee plate, scratches or squeegee marks were visually confirmed on the surface.
[0148] <Overall rating> The above evaluation results were converted into scores based on the following criteria. S 2 points A 1 point B 0 points C -1 point The scores for each decorative film were then totaled, and the decorative films were evaluated according to the scores according to the following criteria. A Total of 10 points or more B Total of 5 points or more and 9 points or less C Total of 4 points or less
[0149] The upper yield point load and stress relaxation rate of the base films 1 to 10, as well as the weather resistance, workability, and overall evaluation of the decorative films 1 to 10, are shown in Table 4. The upper yield point load and stress relaxation rate of the base films C1 to C9, as well as the weather resistance, workability, and overall evaluation of the decorative films C1 to C9 are shown in Table 5. The upper yield point load and stress relaxation rate of the base films C10 to C19, as well as the weather resistance, workability, and overall evaluation of the decorative films C10 to C19 are shown in Table 6. In addition, when observing the appearance of the decorative film C1, cracks were confirmed on the surface. In addition, when observing the appearance of the decorative film C10, yellowing was confirmed. In addition, when observing the appearance of the decorative film C12, yellowing and cracks were confirmed.
[0150] [Table 4]
[0151] [Table 5]
[0152] [Table 6]
[0153] [Consideration] All of the decorative films 1 to 10 have sufficient curved surface conformability and application workability. This is thought to be because the surface protective layer is made of urethane resin and the colored layer is made of acrylic resin, which realizes an appropriate upper yield point load and stress relaxation rate of the decorative film. More specifically, if the stress relaxation rate is within the range of the examples, the decorative film will not float when applied to a curved surface, and if the upper yield point load is within the range of the examples, it is thought that wrinkles in the decorative film during application can be suppressed.
[0154] Furthermore, it is believed that the presence of resin particles in the surface protective layer causes the resin particles protruding from the surface of the decorative film to come into contact with the squeegee plate during the process of attaching the decorative film by pressing it with the squeegee plate, which prevents the surface of the polyurethane resin portion of the surface protective layer from being pressed by the squeegee plate, thereby preventing damage to the surface protective layer (polyurethane resin portion).
[0155] Moreover, all of the decorative films 1 to 10 have sufficient weather resistance. This is believed to be because the presence of resin particles in the surface protective layer causes the ultraviolet rays irradiated to the surface protective layer in an ultraviolet environment to be diffused by the resin particles. As a result, the amount of ultraviolet rays reaching the colored layer is reduced, and weather resistance is improved compared to conditions in which resin particles are not added to the surface protective layer. Furthermore, since it is a laminated film of a layer containing a polyurethane resin and a layer containing an acrylic resin, it is believed that the combination of these resins also has an effect of improving weather resistance.
[0156] In all of the decorative films C1 to C19, at least one of the upper yield point load, stress relaxation rate, and appearance of the decorative film was outside the specific range, and as a result, the overall evaluation was lower than the evaluation of the examples.
[0157] In addition, decorative films C9, C10, C12, C15, and C17 tended to have a higher ΔE, and at least one of the changes in gloss over time and abnormalities in appearance was insufficient. From these results, it is considered that the laminated structure of urethane resin and acrylic resin sufficiently enhances weather resistance.
[0158] Also, in the decorative films C1, C9, C10, C15 and C17, abnormalities in appearance were confirmed. This is thought to be due to the inclusion of factors that reduce the flexibility of the entire decorative film, such as a relatively large amount of resin particles, a relatively hard matrix resin in the colored layer, or a relatively hard polyurethane resin in the surface protective layer.
[0159] In addition, as is clear from the comparison with the decorative films 1 to 5, the decorative film C2 has a slightly higher ΔE and a slightly lower weather resistance. In addition, the decorative film C2 has scratches on its surface due to the application using a squeegee plate. [Industrial Applicability]
[0160] The present invention can be suitably used as a matte decorative film for decorating an object to be decorated, which may have a curved or uneven surface, and which requires weather resistance, such as a film for the exterior of a vehicle. [Explanation of symbols]
[0161] 10 Decorative film 11 Surface protective layer 12 Adhesive layer 13 Colored layer 14 Adhesive layer 20 Release sheet
Claims
1. A decorative film having a surface protective layer and a colored layer laminated thereon, the surface protective layer contains a polyurethane resin and resin particles, and contains 2 parts by mass or more and 11 parts by mass or less of the resin particles per 100 parts by mass of the polyurethane resin; The average particle size of the resin particles is 3 μm or more and 12 μm or less, The colored layer contains an acrylic resin and a colorant, The upper yield point load of the decorative film at 20° C. is 14.6 N / 10 mm or more and 25.0 N / 10 mm or less, and A decorative film having a stress relaxation rate of 53% or more and 58% or less at 20°C.
2. The decorative film according to claim 1 , wherein the acrylic resin comprises a hard acrylic resin and a soft acrylic resin, and the polyurethane resin comprises one or both of a polycarbonate-based urethane resin and a polycaprolactone-based urethane resin.
3. The decorative film according to claim 1 , further comprising an adhesive layer, the adhesive layer being disposed between the surface protective layer and the coloring layer.
4. The decorative film according to claim 1 , further comprising an adhesive layer, the adhesive layer being disposed on a surface of the colored layer opposite to the surface protective layer.
5. The polyurethane resin includes resin particles having an average particle size of 3 μm or more and 12 μm or less, The urethane film is formed from a resin composition containing 2 parts by mass or more and 11 parts by mass or less of the resin particles per 100 parts by mass of the polyurethane resin.
Citation Information
Patent Citations
Film for forming ornamental layer, ornamental article and production process for ornamental article
JP2007297569A
Rubber compounding polyester film and polyester film laminate
JP2008110514A
Decorative film, method for producing decorative film, decorative molding, and method for producing decorative molding
JP2021070300A