Porous particle, method for manufacturing the same, abrasive and structure

Porous particles with a chain silica and carbon network structure address the issues of conductivity and disintegration in silica particles, providing effective polishing solutions by ensuring electrical conductivity and stable disintegration.

JP2024146877APending Publication Date: 2024-10-15JGC CATALYSTS & CHEMICALS LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024052996
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-28
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing porous silica particles lack electrical conductivity, leading to static electricity and dust adhesion during polishing, while silica/carbon composite particles with uncontrolled porosity and non-spherical shapes result in unstable disintegration during polishing.

Method used

The development of porous particles with a network structure formed by chain silica and carbon particles, achieving a balanced oil absorption, controlled pore distribution, and specific carbon content to ensure electrical conductivity and uniform disintegration during polishing.

Benefits of technology

The particles exhibit both electrical conductivity and stable disintegration properties, preventing static electricity and reducing substrate scratching during polishing, making them suitable for precision polishing applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146877000003
    Figure 2024146877000003
  • Figure 2024146877000001
    Figure 2024146877000001
  • Figure 2024146877000002
    Figure 2024146877000002
Patent Text Reader

Abstract

To provide porous particles having moderate collapsibility and conductivity.SOLUTION: Porous particles have a network structure formed of chain silica and carbon particles. The carbon particles have an oil absorption [ml / 100 g] of 100-500; the porous particles have a carbon content of 0.5-50 wt.%, an average particle size [μm] of 0.5-50, an average compressive strength [N / mm2] of 0.98 or more and less than 9.8, a pore volume [cm3 / g] of 0.5-5.0; and the total volume of pores having a size within ±25% of the mode [nm] of hole diameters is 40% or more of pore volumes.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to easily disintegrable porous particles for use in abrasives and the like, and in particular to porous particles having a network structure formed by the aggregation of chain-like silica and carbon particles. [Background technology]

[0002] Porous particles are used in various applications, and it is known that disintegrable porous particles are used as abrasives for precision polishing. For example, disintegrable porous silica particles have been proposed in which a network structure is formed by non-spherical particles in which multiple spherical primary particles are bonded together (see Patent Document 1). In order to obtain the property that these porous silica particles do not disintegrate during production but disintegrate during polishing, the pore volume, pore size distribution, and average compressive strength are optimized.

[0003] It is also known that in order to impart electrical conductivity to a porous silica body, fine particle carbon is dispersed even inside the silica skeleton (see, for example, Patent Document 2). The silica-carbon composite porous body of Patent Document 2 has a specific surface area of ​​20 to 1000 m. 2 / g, pore volume of 0.3 to 2.0 ml / g, average pore diameter of 2 to 100 nm, and the porous structure is formed by gelling a co-dispersion of silica hydrosol and carbon fine particles. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2019-131873 [Patent Document 2] JP 2013-56792 A Summary of the Invention [Problem to be solved by the invention]

[0005] The porous silica particles of Patent Document 1 are composed of silica only and are therefore not conductive. Therefore, when these porous silica particles are used as polishing particles, there are problems such as the workpiece (wafer, etc.) being charged by static electricity generated during polishing, and dust adhering to the workpiece. In Patent Document 2, a co-dispersion in which silica hydrosol and carbon fine particles are dispersed is prepared, and the silica hydrosol contained in the co-dispersion is gelled to make it porous. Since the porosity is not controlled and the shape is not spherical, stable disintegration cannot be obtained when used for polishing purposes. Thus, the silica-carbon composite porous particles of Patent Document 2 are conductive but do not have stable disintegration and are not suitable for polishing. If carbon fine particles are dispersed in the dispersion of the non-spherical particles of Patent Document 1 and granulated, conductivity is obtained, but disintegration suitable for polishing is lost.

[0006] Therefore, an object of the present invention is to realize porous particles that have both electrical conductivity and the property of easily disintegrating during use, ie, not disintegrating during production. [Means for solving the problem]

[0007] The inventors of the present application have found that by controlling the properties of a mixture of a chain silica dispersion and a dispersion of carbon particles having an oil absorption of 100 to 500 ml / 100 g, granulating the mixture, and firing the resulting particles under conditions that prevent oxidation of carbon, it is possible to obtain porous particles with good disintegrability and electrical conductivity. That is, the porous particles according to the present invention have a network structure formed by chain silica and carbon particles, an average particle size of 0.5 to 50 μm, and an average compressive strength of 0.98 to 9.8 N / mm 2 Less than 0.5-5.0 cm pore volume 3 / g, and the sum of the volumes of pores having a size within ±25% of the most frequent pore diameter is 40% or more of the total pore volume. The carbon content of the porous particles is 0.5 to 50% by weight. This makes it possible to impart electrical conductivity to the porous particles that disintegrate uniformly during polishing.

[0008] The production method of the present invention includes a first step of preparing a first dispersion in which carbon particles are dispersed in water; a second step of applying a shear force to a second dispersion in which chain silica is dispersed in water to obtain a third dispersion having a viscosity adjusted to a range of 8 to 100 mPa·S; a third step of preparing a mixture of the first dispersion and the third dispersion; a fourth step of feeding the mixture at a viscosity of 8 to 100 mPa·S into a spray dryer to granulate dried particles; and a fifth step of calcining the dried particles in an inert gas atmosphere, wherein the pH of the mixture is controlled to be in the range of 2 to 6 or 10 to 12. [Brief description of the drawings]

[0009] [Figure 1] 1 is an electron microscope photograph showing an example of the shape of chain particles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The porous particles according to the present invention have a network structure formed by chain-like silica and carbon particles. The oil absorption of the carbon particles is 100-500 ml / 100 g, and the porous particles contain 0.5-50 wt % of carbon derived from the carbon particles. The aggregate powder of the porous particles has an average particle size of 0.5-50 μm and an average compressive strength of 0.98 N / mm. 2 More than 9.8N / mm 2 Less than 0.5-5.0 cm pore volume 3 / g, and the sum of the volumes of pores with sizes within ±25% of the most common pore size is 40% or more of the total pore volume. This results in porous particles that have both electrical conductivity and uniform disintegratability.

[0011] The carbon content of the porous particles can be adjusted to the range of 0.5 to 50% by weight to obtain the desired conductivity (electrical resistivity). If the carbon content is less than 0.5% by weight, no conductive path is formed, and no conductivity is obtained. On the other hand, if porous particles with a carbon content of more than 50% by weight are used as an abrasive, after the porous particles collapse, polishing is mainly performed by the carbon particles, and fine irregularities cannot be flattened. Therefore, the desired polishing characteristics cannot be obtained.

[0012] In order to achieve both electrical conductivity and disintegrability, carbon particles with an oil absorption of 100 to 500 ml / 100 g are used. When carbon particles with an oil absorption of less than 100 ml / 100 g are used, the density of the network structure formed by the chain silica and carbon particles increases, reducing the pore volume and pore diameter. As a result, good disintegrability cannot be obtained. On the other hand, when carbon particles with an oil absorption of more than 500 ml / 100 g are used, it is difficult to prepare a water dispersion with good dispersibility, and porous particles with a uniform internal structure cannot be obtained. Even if they can be dispersed, the viscosity is high and it is difficult to granulate them into a spherical shape, so stable disintegrability cannot be achieved.

[0013] Since the oil absorption of carbon particles affects the pore distribution of porous particles, a sharp pore distribution cannot be achieved unless a material with an appropriate oil absorption is selected. Furthermore, by balancing the oil absorption of chain silica and carbon particles, it is possible to further sharpen the pore distribution and obtain uniform disintegration. Therefore, it is preferable to set the oil absorption balance represented by the following formula to a range of 75 to 125. When the oil absorption of chain silica is A [ml / 100g], the oil absorption of carbon particles is B [ml / 100g], and the amount of carbon contained in the porous particles is C [wt%], the oil absorption balance is expressed as (A x (100-C) + B x C) / A.

[0014] In addition, the pore volume is 0.5 cm 3 If the particle size is less than 5.0 cm / g, the particles become too hard and the desired disintegratability cannot be obtained. 3 If the pore volume exceeds 1.0 to 4.0 cm3 / g, the particles tend to collapse during production and the desired shape factor cannot be obtained. 3 / g is preferable, and 1.2 to 3.0 cm 3 / g is more preferred.

[0015] The mode of the pore size (the most frequent pore size) is preferably 2 to 50 nm. If the most frequent pore size is less than 2 nm, the particles become hard and the disintegration property is affected. On the other hand, if it exceeds 50 nm, the particles tend to disintegrate during production, and the desired shape factor cannot be obtained. The most frequent pore size is preferably 5 to 45 nm, and more preferably 10 to 45 nm.

[0016] The higher the proportion of pores having a pore size close to the most frequent pore size, the sharper the pore size distribution. The sharper the pore size distribution, the less likely the particles are to form clumps when disintegrating, and the more uniform the disintegration. In the porous particles of the present invention, the sum of the volumes of pores having sizes within ±25% of the most frequent pore size (total pore volume) is 40% or more of the aforementioned pore volume (total pore volume). In other words, pore volume ratio (%) [= total pore volume (V ±25% ) / pore volume (V) × 100] is 40% or more. If the pore volume ratio is less than 40%, the internal structure of the particles becomes non-uniform, and the particles tend to form irregular agglomerates when they collapse. Large agglomerates of irregular size can cause polishing scratches. The pore volume ratio is more preferably 40 to 75%.

[0017] In addition, the average compressive strength is 0.98N / mm 2 If it is less than 9.8N / mm, it will easily collapse during production and the desired particle shape (shape factor, etc.) will not be obtained. 2 Above this, the desired disintegrability cannot be obtained. The average compressive strength is 0.98 to 6.86 N / mm 2 is preferable, and 0.98 to 3.92 N / mm 2 is more preferred.

[0018] Furthermore, if the average particle size of the porous particles exceeds 50 μm, it is difficult to obtain particles with a good shape factor (i.e., high sphericity). On the other hand, if it is less than 0.5 μm, the powder has low fluidity and is difficult to work with. The average particle size is preferably 1 to 20 μm, and more preferably 2 to 15 μm. Particles having such an average particle size are particularly suitable as an abrasive.

[0019] The average shape factor is preferably 0.8 to 1.0. If the average shape factor is less than 0.8, the fluidity is poor and it is not practical. Furthermore, the strength in the load direction varies, so stable strength cannot be obtained. The average shape factor is more preferably 0.85 to 1.0, and further preferably 0.87 to 1.0.

[0020] Furthermore, the specific surface area of ​​the porous particles is 30 to 400 m 2If the specific surface area is in this range, it is easy to obtain particles that have both easy disintegration and sphericity. 2 / g is more preferable, and 70 to 200m 2 / g is more preferred.

[0021] Furthermore, the porosity of the porous particles is preferably 50 to 92%. When the porosity is in this range, good disintegrability can be obtained. The porosity is more preferably 55 to 90%, and further preferably 60 to 88%.

[0022] The methods for measuring the above-mentioned characteristic values ​​will be explained in the Examples.

[0023] The network structure of the porous particles is formed by chain silica and carbon particles. Chain silica is a chain particle composed of multiple spherical particles (primary particles) bonded together. The average particle diameter of the primary particles that compose the chain silica (average primary particle diameter d 1 If the average primary particle diameter d is in the range of 5 to 50 nm, the porous particles will have many fine pores and will have good disintegration properties. 1 The average primary particle diameter d is more preferably 5 to 40 nm. 1 is the equivalent sphere conversion formula "d 1 = 6000 / (2.2 × SA) where SA is the specific surface area [m 2 / g], 6000 is the coefficient, and the density of silica is 2.2 g / cm 3 It was decided.

[0024] The carbon particles are preferably similar chain particles. In either case, the average particle diameter (average secondary particle diameter d 2 ) is preferably 50 to 500 nm. When the average particle diameter is in this range, the chain particles are not densely packed, so that the desired pore volume is easily obtained. The average secondary particle diameter is more preferably 50 to 300 nm. Here, the average secondary particle diameter of the chain particles is determined as follows. Particles are observed with a scanning electron microscope, and 100 particles are arbitrarily selected. For each particle, the longest diameter is measured, and the average value is taken as the average secondary particle diameter.

[0025] Average secondary particle diameter d 2 and the average primary particle diameter d 1 The ratio (d 2 / d 1 ) is preferably 1.6 to 100. When it is in this range, a suitable three-dimensional network structure is formed, so that good disintegrability is easily obtained. This ratio is more preferably 3 to 70, and further preferably 4 to 40.

[0026] Chain particles include linear particles in which primary particles are linked to extend in a specific direction, branched particles having a branched structure, and bent particles having a bent structure. In the case of linear particles, the aspect ratio (major axis / minor axis) of the particles is preferably 1.2 or more, more preferably 1.5 or more, and even more preferably 1.8 to 10. Here, the aspect ratios of 100 random particles were measured using electron micrographs. The arithmetic mean value was taken as the average aspect ratio.

[0027] In addition, some chain particles have both a branched structure and a bent structure. An electron microscope photograph of an example of such a particle is shown in FIG. 1. Here, such particles are also classified as branched particles. When the chain particles contain branched particles or bent particles, the gaps between the chain particles constituting the porous particle become larger. Therefore, the porous particle is more likely to collapse. The total content of the branched particles and bent particles contained in the porous particle is preferably 30% by mass or more, more preferably 50% by mass or more, and even more preferably 80% by mass or more.

[0028] In addition, the average particle diameter of the carbon particles d and the average particle diameter of the porous particles d 50 The ratio (d / d 50 ) is less than 1.0. This makes it possible to prevent the carbon particles from jumping out of the porous particles. It is acceptable if the average particle diameter d of the carbon particles is small as long as the desired electrical conductivity is obtained. The average particle diameter d of the carbon particles is the average value of the longest diameters of 100 random particles measured under observation with a scanning electron microscope, and the average particle diameter d of the porous particles is 50 is the median diameter obtained by measuring the particle size distribution. In addition, when the carbon particles are chain-shaped, the average secondary particle diameter d is used instead of the average particle diameter d.2 This ratio is calculated using:

[0029] It is also preferred that the porous particles do not contain a binder component, which results in particles that are more easily disintegrated.

[0030] Furthermore, the porous particles preferably do not contain impurities such as alkali metals such as sodium and potassium, which are factors that cause fusion (factors that cause high strength), and alkaline earth metals such as calcium and magnesium. The content of each element is preferably 10 ppm or less, more preferably 5 ppm or less. Furthermore, the porous particles preferably do not contain uranium or thorium, which are alpha-ray radioactive materials. The uranium content and thorium content are each preferably 0.5 ppb or less, more preferably 0.3 ppb or less.

[0031] The porous particles described above can be used as an abrasive and a structure for polishing industrial products, etc. In an abrasive containing porous particles, the porous particles collapse when a specific load is applied, so that the substrate (object to be polished) is less likely to be scratched. In addition, the average particle size and average primary particle size d of the chain silica after collapse can be obtained. 1 Since the particle size is small, it can polish fine irregularities on the substrate surface. It is particularly suitable for dry polishing of the finish, but can also be used for wet polishing. It can also prevent the substrate from becoming charged by polishing. Therefore, it can be suitably used for polishing semiconductor substrates, display substrates, metal plates, glass plates, etc. In actual polishing, it is molded together with other components and used as a grindstone, or used as a powder or in the form of a slurry dispersed in a liquid, together with a cloth or pad.

[0032] Next, a method for producing the porous particles will be described.

[0033] First, a first dispersion liquid in which carbon particles are dispersed in water is prepared (first step). In parallel, a second dispersion liquid in which chain silica is dispersed in water is prepared. A shear force is applied to the second dispersion liquid to adjust the viscosity of the dispersion liquid to a range of 8 to 100 mPa·S (second step). This results in a third dispersion liquid with an appropriate viscosity. Next, a mixture liquid of the first dispersion liquid and the third dispersion liquid is prepared (third step). This mixture liquid is fed into a spray dryer with a viscosity in the range of 8 to 100 mPa·S to granulate dried particles (fourth step). The dried particles are fired in an inert gas atmosphere (fifth step). At this time, the pH of the mixture liquid is adjusted to be in the range of 2 to 6 or 10 to 12. That is, when the pH of the first dispersion liquid is 7 or more, the pH of the second dispersion liquid is adjusted to be in the range of 10 to 12. Alternatively, when the pH of the first dispersion liquid is less than 7, the pH of the second dispersion liquid is adjusted to be in the range of 2 to 6. If the pH of the mixed liquid falls within the range of 2 to 6 or 10 to 12 without adjusting the pH of the second dispersion, the first dispersion and the third dispersion may be mixed without adjustment.

[0034] It is to be noted that a step other than the above-mentioned steps may be added. For example, a classification step may be added between the granulation step and the firing step.

[0035] The porous particles of the present invention can be obtained by the above-mentioned production method. Each step will be described in detail below.

[0036] [First step] In this step, a first dispersion liquid in which carbon particles are dispersed in water is prepared. At this time, carbon particles with an oil absorption [ml / 100g] of 100 to 500 are used. Carbon black can be exemplified as the carbon particles. The pH of the first dispersion liquid is determined by the type of carbon particles and the concentration of carbon particles in the dispersion liquid. Since carbon particles are highly hydrophobic, it is preferable to add a surfactant to improve dispersibility in water. Furthermore, it is preferable to prepare the first dispersion liquid by applying ultrasonic vibration to promote dispersion. The amount of addition is not particularly specified, but if an excessive amount is added, it remains in the porous particles as an impurity, making it difficult to obtain the desired conductivity. It is preferable that the amount of the surfactant added is less than that of the carbon particles. Examples of the type of surfactant include anionic surfactants, cationic surfactants, nonionic surfactants, and amphoteric surfactants.

[0037] [Second process] First, a second dispersion in which chain silica is dispersed in water is prepared. A shear force is applied to this second dispersion to adjust the viscosity of the dispersion to a range of 8 to 100 mPa·S. This results in a third dispersion. Usually, a dispersion of chain silica has thixotropy. Therefore, it is necessary to apply a shear force continuously or intermittently to the dispersion to lower the viscosity. It is preferable not to crush the chain silica when applying the shear force. If crushed, the particles are densely packed with crushed pieces, etc., and the pore volume of the dry particles obtained by granulation becomes small. In addition, if crushed, the specific surface area of ​​the particles contained in the dispersion increases and the hydroxyl groups on the particle surface also increase, so that the bonds between the primary particles are strengthened, and the average compressive strength of the porous particles may increase.

[0038] Examples of devices for applying shear force to the dispersion include a disper mill, a homogenizer, etc. Using these devices, the viscosity of the dispersion is maintained within a specific range, and the conditions for applying shear force (rotation speed, etc.) can be set as necessary so that the chain silica is not pulverized into primary particles.

[0039] Chain silica can be obtained by binding spherical silica particles. For example, chain silica sols prepared by a wet method or fumed silica prepared by a dry method can be used. Specifically, Aerosil-90, Aerosil-130, Aerosil-200 (above, Nippon Aerosil Co., Ltd.) are commercially available. Also, the manufacturing method of chain silica is described in JP-A-2003-133267, JP-A-2013-032276, etc.

[0040] [Third Step] Next, the first dispersion and the third dispersion are mixed. At this time, it is necessary to make the pH of this mixed solution in the range of 2 to 6 or 10 to 12. When the pH is in the range of "6 < pH < 10", the mixed solution is likely to gel, and it is difficult to granulate by the fourth step (drying step) described later.

[0041] Therefore, when the first dispersion and the third dispersion are mixed, the pH of the second dispersion is adjusted in advance so that the pH is in the appropriate range of 2 to 6 or 10 to 12. That is, the pH is adjusted before applying a shearing force to the second dispersion. Since the pH of the dispersion hardly changes even when a shearing force is applied, the pH of the third dispersion after viscosity adjustment is the same as the pH of the second dispersion. For example, when the pH of the first dispersion is 7 or higher (alkaline), if the pH of the second dispersion is less than 7 (acidic), there is a possibility that the pH of the mixed solution will not fall within the appropriate range. Therefore, the pH of the second dispersion is adjusted to be higher so that the pH of the mixed solution is 10 to 12. Also, for example, when the pH of the first dispersion is less than 7, if the pH of the second dispersion is also less than 7, the pH of the mixed solution can be in the range of 2 to 6. In that case, it is not necessary to adjust the pH of the second dispersion. However, the pH of the second dispersion may be further lowered (to the acidic side). Thus, the pH adjustment of the second dispersion may be appropriately performed according to the actual situations of the first dispersion and the second dispersion used.

[0042] In this case, if an alkaline reagent is used, the pH of the second dispersion can be increased. A weak alkaline reagent is preferable. If an acidic reagent is used, the pH of the second dispersion can be decreased. A weak acidic reagent is preferable. By using a weak alkaline or weak acidic reagent, it is possible to adjust the pH to the target value, and it is possible to prevent dissolution of chain silica due to a sudden change in pH (occurring at pH 12 or higher) and contamination with metal components due to corrosion of the device (occurring at pH 2 or lower). In addition, the concentration of the reagent to be added may be adjusted to moderate the change in pH.

[0043] [Fourth step] The mixture obtained in the third step is fed into a spray dryer with a viscosity in the range of 8 to 100 mPa·S to granulate and dry the dried particles (the particles obtained in this step are referred to as dried particles). At this time, it is necessary to set the viscosity of the mixture fed into the spray dryer within a certain range (8 to 100 mPa·s). It is preferable to make the viscosity as low as possible. It is more preferable to set it to 10 to 90 mPa·s, and even more preferable to set it to 10 to 80 mPa·s. By lowering the viscosity of the mixture, the variation in the diameter of the dried particles is reduced. At the same time, a uniform internal structure can be achieved, and the variation in the internal structure (individual differences) is also reduced. Therefore, porous particles with appropriate disintegrability can be obtained. Furthermore, by maintaining the viscosity within the above-mentioned range, the content of particles with a shape factor of less than 0.80 can be reduced.

[0044] If the viscosity is within this appropriate range, there is no need to adjust the viscosity by applying shear force. Since the viscosity is adjusted by applying shear force in the above-mentioned second step, if the time elapsed between the second step and the fourth step is short, the appropriate viscosity is maintained without applying shear force in the fourth step. If more than two hours have elapsed between the second step and the fourth step, it is preferable to apply shear force to reduce the viscosity.

[0045] Furthermore, it is preferable to reduce the fluctuation in the viscosity of the dispersion. Specifically, it is preferable to control the viscosity of the mixed liquid within ±30 mPa·s from the start of feeding to the spray dryer to the end of feeding. For example, if the viscosity of the mixed liquid at the start of feeding to the spray dryer is 50 mPa·s, a mixed liquid with a viscosity of 20 to 80 mPa·s is fed into the spray dryer until the end of spray drying. If the viscosity of the mixed liquid at the start of feeding to the spray dryer is 80 mPa·s, a mixed liquid with a viscosity of 50 to 100 mPa·s is fed into the spray dryer so that the viscosity does not exceed 100 mPa·s. At this time, the viscosity of the mixed liquid fed into the spray dryer is adjusted to be within the above-mentioned range. The fluctuation range of the viscosity is more preferably within ±25 mPa·s, and even more preferably within ±20 mPa·s.

[0046] In addition, making the viscosity constant leads to making the droplet size constant, and as a result, it becomes easier to control the particle size distribution. In addition, by controlling the viscosity fluctuation within the above range, the reproducibility of the particle size distribution is also improved. Therefore, porous particles having a similar particle size distribution can be stably produced. In addition, by maintaining the viscosity of the mixed liquid within the above range and feeding it into the spray dryer, it is possible to prevent the mixed liquid from clogging the piping that supplies the mixed liquid to the spray dryer and the nozzle of the spray dryer, etc., and thus improve production efficiency.

[0047] In addition, the temperature of the mixed liquid when it is fed into the spray dryer also affects the viscosity, so the temperature is preferably 10 to 30°C, and more preferably 15 to 25°C.

[0048] The concentration of the dispersion is preferably 5 to 30% by weight. This allows granulation and drying to be carried out more efficiently. If the concentration is too low, granulation does not proceed easily during spray drying, and the particle size tends to become small. If the concentration is too high, the particle size may become large and drying may become insufficient. If the particle size is too large, sufficient mechanical strength may not be obtained, and the particles may be damaged during production. In particular, since the porous particles of the present invention are easily disintegrated, the concentration of the dispersion is important.

[0049] This concentration is more preferably 10 to 20% by weight, and even more preferably 10 to 15% by weight. According to this concentration range, the viscosity becomes high at low shear rates and low at high shear rates. In other words, a mixed liquid with non-Newtonian properties can be obtained. This non-Newtonian mixed liquid is spray-dried while the viscosity is reduced at high shear rates. The mixed liquid is sprayed from a nozzle with good fluidity. The sprayed droplets have a low shear rate and become highly viscous (form an aggregated structure), so beautiful spherical porous particles can be obtained.

[0050] It is preferable to dry the particles until the moisture content of the dried particles is 1 to 10% by weight. This can reduce the collapse of particles due to excessive drying, and the generation of irregularly shaped particles that are fused together due to moisture when fired. By spray drying so that the moisture content is within the above range, the shape factor of the entire dried particles can be increased.

[0051] As the method of spray drying, known methods such as a rotating disk method, a pressure nozzle method, a two-fluid nozzle method, etc. can be adopted, and in particular, the two-fluid nozzle method is preferable. The drying temperature in the drying step is preferably 30 to 150°C, more preferably 40 to 100°C, in terms of the outlet hot air temperature. Drying under these conditions allows for sufficient drying, and can reduce adhesion or fusion between particles in the firing step.

[0052] [Fifth step] Next, the dried particles are fired to reduce the moisture content. In this step, in order to prevent oxidation of the carbon particles, the dried particles are fired in an inert gas atmosphere to obtain porous particles. The firing temperature is preferably 250 to 800°C, more preferably 300 to 600°C, and even more preferably 400°C to 500°C. By firing within this range, porous particles with a low moisture content are obtained, and the stability of quality is improved. In addition, it is possible to prevent the chain particles that form the porous particles from fusing together due to heat. In other words, it is possible to prevent the strength from increasing. Nitrogen or rare gases (helium, argon, etc.) can be used as the inert gas. Nitrogen, which is widely used industrially and is inexpensive, is the most preferable.

[0053] [Classification process] Classification may be performed between granulation / drying (spray drying) and calcination. Classification is performed under conditions that the dried particles granulated by spray drying do not collapse. By providing a classification process between the granulation / drying process and the calcination process, coarse particles are removed. Specifically, coarse particles having a particle size of 4 times or more of the average particle size are removed. The ratio of coarse particles having a particle size of 4 times or more of the average particle size is preferably 5% by weight or less, more preferably 2% by weight or less. Examples of classification devices include Dreserec manufactured by Donaldson Co., Ltd., Spin Air Sieve manufactured by Seishin Enterprise Co., Ltd., Aero Fine Classifier manufactured by Nisshin Engineering Co., Ltd., Hiplex Classifier manufactured by Powder Systems Co., Ltd., and Twin Turboplex manufactured by Hosokawa Micron Corporation.

[0054] Examples of the present invention will now be described in detail. EXAMPLES

[0055] [Example 1] 2.0 kg of pure water and 0.1 kg of a nonionic surfactant (Kao Chemicals: Rheodol TW-O120V) were added to a 10 L tank, and 0.3 kg of carbon particle powder (Denka: Denka Black) was added while stirring. Ultrasonic vibration was then applied to obtain a carbon particle dispersion. The pH of this dispersion was 9.2.

[0056] In addition, 14.3 kg of chain silica powder (Aerosil-90G, manufactured by Nippon Aerosil Co., Ltd.) was gradually added to a tank (capacity 200 L) containing 100 L of pure water while stirring. The mixture was mixed until no powder lumps were visible. The pH of the resulting chain silica dispersion was 3.8. Since the pH of the carbon particle dispersion was 9.2, it was necessary to increase the pH of the chain silica dispersion and adjust the pH of the mixture to be in the appropriate range (10 to 12). Therefore, 15% ammonia water was added to this chain silica dispersion so that the pH became 11. At this time, the chain silica dispersion gelled once near its isoelectric point (pH 6.0), but when further ammonia water was added while stirring, it was dispersed again at a pH of 10 or higher. The viscosity of the chain silica dispersion after pH adjustment was 121 mPa·s. Furthermore, this chain silica dispersion was supplied from the tank to a disper mill (manufactured by Hosokawa Micron Corporation), where shear force was applied and then discharged into the tank. The viscosity of the dispersion was adjusted by circulating the dispersion in this manner, and a chain silica dispersion with a viscosity of 26 mPa·s (silica concentration 12.5% ​​by weight) was obtained. Aerosil-90G is a chain silica containing branched and bent particles, and the average secondary particle diameter d 2 is 200 nm, and the average primary particle diameter d 1 was 30 nm.

[0057] The chain silica dispersion was added to the carbon particle dispersion to obtain a mixture of chain silica and carbon particles (pH 11). The mixture was supplied to the opposing two-fluid nozzle of the spray dryer while stirring. The spray drying conditions were: throughput 60 L / Hr, air / liquid ratio = 2,100, air flow rate Mach 1.1, dry atmosphere (temperature 120°C, humidity 7.2 vol%). This resulted in dry particles (moisture content 2 wt%). The viscosity of the mixture was measured using a Toki Sangyo Co., Ltd. B-type viscometer (TVB-10, rotor No. 1) at a liquid temperature of 25°C, a rotation speed of 100 rpm, and a measurement time of 60 seconds. The viscosity of the mixture in the tank at the start of supply was 30 mPa·s, and the viscosity of the dispersion in the tank at the end of supply was 71 mPa·s. The dried particles were classified to remove coarse particles, and then the dried particles were left to stand and fired in a nitrogen atmosphere at 400°C for 3 hours to obtain porous particles.

[0058] The physical properties of the porous particles were measured and evaluated as follows. The same procedures were carried out for other examples and comparative examples. Table 1 shows the preparation conditions of the porous particles, and Table 2 shows the measurement and evaluation results of the physical properties of the porous particles.

[0059] (1) Oil absorption amount (a) Oil absorption of chain silica and carbon particles A sample (chain silica powder or carbon particle powder) was placed on a measuring plate, and four drops of boiled linseed oil were dropped onto the sample using a burette, thoroughly kneading the mixture with a palette knife after each drop. After repeating the dropping and kneading process, when the mixture had become a hard putty-like mass, each drop was kneaded further until it could be rolled into a spiral shape using a palette knife. The total amount of boiled linseed oil added up to that point was converted into the amount added per 100g of sample, and this was taken as the oil absorption.

[0060] (b) Oil absorption of carbon particles within porous particles Hydrofluoric acid was added to the powder of porous particles to dissolve the silica in the powder. After that, the components that were not dissolved in hydrofluoric acid (carbon) were filtered out, washed with water, and dried at 100°C to obtain carbon powder. This was used as a sample to determine the oil absorption amount using the same method as in (a).

[0061] (2) Carbon content of porous particles Weigh out 0.1 g of the sample (powders of porous particles) and place it in a crucible. Add iron, tungsten, and tin as combustion improvers. Place the crucible in a carbon and sulfur analyzer (LECO CS844) and burn it to measure the CO and CO 2 The weight of carbon contained was calculated from the peak intensity of the gas, and the ratio of this weight to the weight of the sample (weight of carbon contained / weight of sample) was taken as the carbon content.

[0062] (3) Electrical resistivity 0.05g of the powder of the porous particles was weighed out, spread inside a cylindrical insulator ring, and a load of 70kgf / cm was applied using a hydraulic device manufactured by RIKEN SEIKI. The electrical resistance value at this time was measured using an Agilent resistance meter, and the electrode distance was measured using a vernier caliper. The powder thickness was calculated from the measured electrode distance and the electrode distance measured beforehand without any particles, and the electrical resistivity was calculated from the electrical resistance value and the powder thickness.

[0063] (4) Average particle size (a) Average particle size of carbon particles Particles are observed under a scanning electron microscope, and 100 particles are randomly selected. The longest diameter of each particle is measured, and the average value is taken as the average particle diameter. According to this measurement, if the carbon particles are chain-shaped, it is measured as the average secondary particle diameter.

[0064] (b) Average particle size of porous particles The particle size distribution of the porous particle powder was measured using a particle size distribution analyzer (Multisizer 3) manufactured by Beckman Coulter, and the median diameter d 50 was taken as the average particle size.

[0065] (5) Pore volume, most common pore size, specific surface area, and pore volume ratio 10 g of sample (powders of porous particles) was placed in a crucible, dried at 300°C for 1 hour, then cooled to room temperature in a desiccator. 0.15 g was placed in a glass cell, and nitrogen gas was adsorbed and desorbed from the sample using a Belsorpmini II (manufactured by Japan Bell Co., Ltd.). The pore volume (V) at a relative pressure of 0.990 was calculated from the resulting adsorption isotherm, and the mode (peak value) of the pore diameter was calculated by the BJH method. The specific surface area was also calculated by the BET method.

[0066] The pore volume ratio is the total pore volume (V ±25% ) and the pore volume (V) of the porous silica particles, using the following formula: Pore ​​volume ratio (%) = V ±25% / V×100

[0067] (6) Porosity The density of silica is 2.2 g / cm 3 (=0.4545cm 3 / g) was calculated from the pore volume (V) determined by the nitrogen adsorption method described above using the following formula. Porosity (%)=V / (V+0.4545)×100

[0068] (7) Average shape factor The circularity of approximately 50,000 particles was measured using a Morphologi 4 manufactured by Malvern Panalytical, and the arithmetic mean value was used as the average shape factor. The circularity is calculated as the ratio of the circumference of a circle with the same area as the projected object to the perimeter of the object.

[0069] (8) Average compressive strength The compressive strength was measured using a Shimadzu Micro Compression Tester (MCT-W500). A load was applied to one sample particle, the load at which the sample broke was measured, and the compressive strength was calculated. Five samples were measured, and the arithmetic mean value was taken as the average compressive strength.

[0070] (9) Polishing evaluation Furthermore, a polishing wheel was produced using the powder of porous particles as abrasive grains. That is, 100 parts by weight of the powder was uniformly mixed with 100 parts by weight of rubber particles (NBR cured rubber, average particle size 120 μm) as a matrix, and the mixture was subjected to a pressure of 100 kgf / cm 2 The resultant was compressed and molded into a ring shape under a pressure of 10 ... Polishing conditions Grindstone rotation speed: 30m / sec (periphery) Grindstone pressure: 150g / cm 2 Polishing liquid: water Workpiece: Glass substrate (borosilicate glass) Polishing time: 2 minutes 30 seconds Scratch Evaluation Criteria The surface is smooth and almost no scratches are observed: ○ The surface is smooth but there are some scratches: △ The surface is smooth and chipped or scratched: ×

[0071] [Example 2] As the carbon particle powder, "EC600JD (Ketjen Black)" manufactured by Lion Specialty Chemicals was used. Except for this, porous particles were prepared in the same manner as in Example 1.

[0072] [Example 3] The carbon particle powder used was "SEAST 3" manufactured by Tokai Carbon Co., Ltd. Except for this, porous particles were prepared in the same manner as in Example 1.

[0073] [Example 4] A dispersion of carbon particles was prepared as follows: 0.54 kg of pure water and 0.02 kg of a nonionic surfactant (Rheodol TW-O120V, manufactured by Kao Chemical Co., Ltd.) were added to a tank having a capacity of 1 L, and 0.08 kg of carbon particle powder (Denka Black, manufactured by Denka Co., Ltd.) was added while stirring. Except for this, porous particles were prepared in the same manner as in Example 1.

[0074] [Example 5] A dispersion of carbon particles was prepared as follows: 100.0 kg of pure water and 4.0 kg of a nonionic surfactant (Rheodol TW-O120V, manufactured by Kao Chemical Co., Ltd.) were added to a 200 L tank, and 14.4 kg of carbon particle powder (Denka Black, manufactured by Denka Co., Ltd.) was added while stirring. Except for this, porous particles were prepared in the same manner as in Example 1.

[0075] [Example 6] "TOKABLACK♯5500" manufactured by Tokai Carbon Co., Ltd. was used as the powder of carbon particles. A dispersion of carbon particles was prepared in the same manner as in Example 1 except for this. Since this dispersion had a pH of 5.9, the dispersion of carbon particles and the dispersion of chain silica were mixed without adjusting the pH of the dispersion of chain silica. A porous particle was prepared in the same manner as in Example 1 except for this.

[0076] [Example 7] "TOKABLACK♯4400" manufactured by Tokai Carbon Co., Ltd. was used as the powder of carbon particles. A dispersion of carbon particles was prepared in the same manner as in Example 1 except for this. Since this dispersion had a pH of 6.4, nitric acid with a concentration of 1% was added to the dispersion of chain silica to adjust the pH of the dispersion of chain silica to 2.5. The dispersion of carbon particles and the dispersion of chain silica thus obtained were mixed. A porous particle was prepared in the same manner as in Example 1 except for this.

[0077] [Comparative Example 1] In Example 1, the chain silica dispersion was mixed with the carbon particle dispersion without adjusting the pH of the chain silica dispersion. The resulting mixture had a pH of 6.5. The mixture gelled, so it was not possible to granulate it with a spray dryer.

[0078] [Comparative Example 2] The carbon particle powder used was "SEAST S" manufactured by Tokai Carbon Co., Ltd. Except for this, porous particles were prepared in the same manner as in Example 1.

[0079] [Comparative Example 3] A dispersion of carbon particles was prepared as follows: 0.13 kg of pure water and 0.01 kg of a nonionic surfactant (Rheodol TW-O120V, manufactured by Kao Chemical Co., Ltd.) were added to a tank having a capacity of 1 L, and 0.02 kg of carbon particle powder (Denka Black, manufactured by Denka Co., Ltd.) was added while stirring. Except for this, porous particles were prepared in the same manner as in Example 1.

[0080] [Comparative Example 4] A dispersion of carbon particles was prepared as follows: 150 kg of pure water and 7.0 kg of a nonionic surfactant (Rheodol TW-O120V, manufactured by Kao Chemical Co., Ltd.) were added to a tank having a capacity of 200 L, and 22.0 kg of carbon particle powder (Denka Black, manufactured by Denka Co., Ltd.) was added while stirring. Except for this, porous particles were prepared in the same manner as in Example 1.

[0081] [Comparative Example 5] In the calcination step of Example 1, the dried particles were calcined by leaving them to stand in an air atmosphere for 3 hours at 400° C. Except for this, porous particles were prepared in the same manner as in Example 1.

[0082] [Table 1]

[0083] [Table 2]

Claims

1. Porous particles having a network structure formed by chain-like silica and carbon particles, The carbon particles have an oil absorption of 100 to 500 ml / 100 g. The carbon content of the porous particles is 0.5 to 50% by weight, the average particle diameter [μm] is 0.5 to 50, and the average compressive strength [N / mm 2 ] is 0.98 or more and less than 9.8, and the pore volume [cm 3 / g] is 0.5 to 5.0, and the sum of the volumes of pores having a size within ±25% of the mode [nm] of the pore diameter is 40% or more of the pore volume.

2. An abrasive and a structure comprising the porous particles according to claim 1.

3. A first step of preparing a first dispersion in which carbon particles are dispersed in water; a second step of applying a shear force to a second dispersion in which chain silica is dispersed in water to prepare a third dispersion having a viscosity in the range of 8 to 100 mPa·S; a third step of preparing a mixture of the first dispersion and the third dispersion; A fourth step of feeding the mixture at a viscosity in the range of 8 to 100 mPa·S into a spray dryer to granulate dried particles; A fifth step of calcining the dried particles in an inert gas atmosphere, The method for producing porous particles, wherein the pH of the mixture is in the range of 2 to 6 or 10 to 12.

4. 4. The method according to claim 3, wherein the pH of the second dispersion is adjusted so that the pH of the mixture is 10 to 12 when the pH of the first dispersion is 7 or more.

5. The inert gas is N 2 The method according to claim 3, wherein the gas is argon.

6. 4. The method according to claim 3, wherein the total content of the silica component and the carbon component in the mixed liquid is 5 to 30% by weight.

Citation Information

Patent Citations

  • Porous silica-carbon composite body and method for producing the same