Investigation coating sheet and coating film evaluation method with coating sheet

By using a coating sheet with a test coating layer to evaluate performance in the actual environment, the method addresses the challenge of selecting compatible paints, reducing waste and improving accuracy while being safe and efficient.

JP2024146904APending Publication Date: 2024-10-15CHUGOKU MARINE PAINTS
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024056397
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-29
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing methods struggle to select a paint that is compatible with the actual usage environment, leading to wastage of resources and costs due to excessive application of paints with insufficient or excessive active ingredients.

Method used

A coating sheet with a test coating layer is affixed to the object, exposed to the environment for a period, and information is gathered to evaluate the performance of the coating film, allowing for the selection of a suitable paint.

Benefits of technology

This method enables the selection of a paint that is suitable for the environment without waste, is safe and environmentally friendly, reduces handling hurdles, and prevents on-site painting defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146904000001_ABST
    Figure 2024146904000001_ABST
Patent Text Reader

Abstract

To provide means for selecting a coating material appropriate for actual usage environment.SOLUTION: A method for evaluating the performance of a coating film, comprising: (i) attaching to an object or a substitute object to be covered with a coating film an investigational coating sheet having at least one test coating layer (sp) that is not formed around the object; (ii) placing the investigational coating sheet in an environment in which the object is placed for a certain period of time with at least a portion of the test coating layer (sp) exposed on the surface; and (iii) acquiring information regarding the condition of the investigational coating sheet.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an investigational coating sheet, a method for producing the same, and a coating evaluation method using the investigational coating sheet. [Background technology]

[0002] The purpose of applying paint to a substrate is to protect the substrate and maintain its beauty. The effects of these must be maintained for an expected period of time, but the substrate is expected to be placed in a variety of environments, and the paint is designed to maintain its effects even in the harshest environments imaginable. Specifically, it is required to adjust the active ingredients of the paint to the optimal amount and to make the coating thickness sufficient to perform well, but depending on the usage environment, the expected performance may not be necessary. In such cases, the content of the active ingredients or the use of the paint itself will be excessive, resulting in waste in terms of costs and resources, and in some cases placing an unnecessary burden on the environment.

[0003] For example, in the case of antifouling paints that protect the bottom of ships from the adhesion of marine organisms, ships are placed in a wide variety of environments depending on the sea area, sailing speed, operating rate, etc., and the amount and types of marine organisms that adhere to the ship are also diverse. Therefore, in preparation for the case where the amount of marine organisms that adhere to the ship is large or a wide range of marine organisms adhere to the ship, antifouling paints that contain a sufficient amount of active ingredients are applied to the ship to a sufficient film thickness. However, while the active ingredients of the paint and the paint itself are often expensive and are limited resources, some ships may have less marine organisms than expected or may sail under environmental conditions where only certain types of marine organisms adhere to the ship, and in such cases, costs and resources are wasted.

[0004] To avoid such mismatches, the practice has been to prepare a lineup of multiple grades of products with different amounts of active ingredients, and to recommend paint products that are deemed suitable by making inferences based on advance information about the applications for which the paint will be used, or by conducting small-scale advance tests (under the same environment) in a designated testing facility.

[0005] However, it is difficult to estimate the appropriate paint product from advance information alone, and when no problems due to insufficient performance occur, it is often difficult to distinguish whether a paint product that matches the required performance has been applied, or whether a paint product with excessive performance has been applied beyond what is actually required.In addition, even when conducting small-scale advance tests, there are hurdles to carrying them out, considering the preparation of multiple paints in the lineup, the effort and difficulty of painting, the increase in processes, and the effort of checking the results.

[0006] As a method for evaluating the performance of a paint, for example, Patent Document 1 describes an antifouling performance evaluation method that includes immersing a test piece coated with an antifouling agent in immersion test water containing aquatic organisms for a predetermined immersion time, sampling the attached matter including the attached organisms attached to the test piece, and quantifying the amount of attached matter using a biomolecule analysis method (e.g., amino acid analysis method). Patent Document 1 also describes that in the above antifouling performance evaluation method, in addition to the relationship between the immersion time and the amount of attached matter, it is possible to analyze the relationship between the immersion time and the elution rate of the antifouling agent (sample the test water for analysis and measure it using mass spectrometry), and the relationship between the amount of attached matter and the elution rate of the antifouling agent, and that the above-mentioned immersion test and antifouling agent elution test can be performed in parallel, and changes over time can be examined using a large number of test pieces. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent Publication No. 2018-167654 Summary of the Invention [Problem to be solved by the invention]

[0008] As mentioned above, it is not easy to select a paint that is suitable for the usage environment and that does not waste costs or resources.

[0009] The present invention has been made to solve the above problems, and has an object to provide a means for selecting a paint suitable for each actual use environment. [Means for solving the problem]

[0010] The present inventors have discovered that by attaching an "investigative coating sheet" having a specific "test coating layer" to an object to be covered with a coating, and leaving the object in an environment in which the object will be placed for a certain period of time with part of the test coating layer exposed on the surface, information on the condition of the investigated coating sheet can be obtained, thereby enabling a performance evaluation of a coating that can solve the above-mentioned problems, and have completed the present invention.

[0011] That is, the present invention includes at least the following: [Section 1] (i) applying to an object to be coated with a coating or to a substitute object a coating sheet to be investigated having at least one coating layer (sp) to be tested that is not formed around it; (ii) placing the sample coating layer (sp) in an environment in which the object is placed for a certain period of time with at least a portion of the sample coating layer (sp) exposed on the surface; and (iii) obtaining information regarding the state of the coating sheet for investigation; A method for evaluating the performance of a coating film, comprising: [Section 2] The method according to item 1, wherein the coating sheet for investigation further has an adhesive layer (ad). [Section 3] 3. The method according to claim 2, wherein the adhesive layer (ad) comprises a pressure sensitive adhesive. [Section 4] The method according to item 1, wherein the coating sheet for investigation further has a substrate layer (bs). [Section 5] Item 5. The method according to item 4, wherein the substrate layer (bs) comprises a metal. [Section 6] The method according to item 1, wherein the coating sheet for investigation further has an indication layer (id). [Section 7] The method according to item 1, wherein the investigational coating sheet has two or more different test coating layers (sp). [Section 8] Item 2. The method according to item 1, wherein the step (i) further comprises sealing the periphery of the investigational coating sheet with a coating composition. [Section 9] Item 10. The method of item 1, wherein step (iii) comprises taking a photograph and transmitting the photograph electronically. [Section 10] Item 10. The method according to item 1, wherein the object is an underwater structure. [Section 11] Item 3. The method of item 1, wherein the object is a ship. [Section 12] Item 3. The method according to item 1, wherein the object is a moving object. [Section 13] Item 10. The method according to item 9, further comprising a step of determining a recommended coating method for the subject based on the information obtained in step (iii). [Section 14] A coating sheet having at least one test coating layer (sp) and an indicator layer (id) that are not formed around the periphery. [Section 15] A coating sheet having two or more different test coating layers (sp) that are not formed around it. Effect of the Invention

[0012] According to the present invention, a paint suitable for the usage environment and not wasteful in terms of cost and resources can be selected with little burden. Furthermore, by accumulating and utilizing test information by the method of the present invention, the accuracy of suitable paint selection can be improved when selecting a paint from prior information on the usage environment or a combination of the prior information and test information. In addition, in the present invention, a specific coating sheet is attached to an object (e.g., a ship's hull) instead of directly applying the test paint, so that (1) the test can be performed in a safe manner without using organic solvents and without burdening the environment, (2) the handling is easy and the hurdles of distribution and storage are lowered, so that the test can be performed widely, (3) the coating film formed on the sheet is used for testing, so that the film thickness can be controlled as expected without the difficulty of on-site painting, and (4) the coating film defects occurring in on-site painting can be prevented. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a schematic cross-sectional view showing the laminate structure of the coating sheet for investigation produced in Example 1. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing the laminate structure of the coating sheet for investigation produced in Example 2. [Diagram 3] FIG. 3 is a schematic top view showing the arrangement of each layer of the coating sheet prepared in Example 3. [Figure 4] FIG. 4 is a schematic cross-sectional view showing the laminated structure of the coating sheet for investigation produced in Example 3. [Diagram 5] FIG. 5 is a schematic top view showing the arrangement of each layer of the coating sheet for investigation produced in Example 4. [Figure 6] FIG. 6 is a schematic cross-sectional view showing the laminate structure of the coating sheet for investigation produced in Example 4. [Figure 7] FIG. 7 is a schematic top view showing the arrangement of each layer of the coating sheet for investigation produced in Example 5. [Figure 8] FIG. 8 is a schematic cross-sectional view showing the laminate structure of the coating sheet for investigation produced in Example 5. [Figure 9] FIG. 9 is a schematic top view showing the arrangement of each layer of the coating sheet for investigation produced in Example 6. [Figure 10] FIG. 10 is a schematic cross-sectional view showing the laminate structure of the coating sheet for investigation produced in Example 6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The investigational coating sheet of the present invention, its production method, and a coating evaluation method using the investigational coating sheet will be described in detail below.

[0015] [Coating sheet for investigation] The coating sheet for investigation of the present invention has one or more test coating layers (sp). "One or more test coating layers (sp)" means the "number" of test coating layers (sp), that is, the number of regions (sections) of the test coating layers (sp) that are not continuous with each other formed on one coating sheet for investigation is one or more. One coating sheet for investigation may have only one or more test coating layers (sp) of one type, or may have two or more test coating layers (sp) of two or more types. The "type" of the test coating layer (sp) means a property that can be distinguished from each other, such as the formulation of the test paint composition used to form it, the roughness or shape of the coating surface, and the thickness of the coating. The coating sheet for investigation of the present invention may have two or more types of test coating layers (sp) in the sense that they are formed from coating compositions with different formulations, or may have two or more types of test coating layers (sp) in the sense that they have a common coating composition but different coating surface roughness or film thickness, depending on the purpose of the investigation. Since having more different types of test coating layers (sp) increases the likelihood of finding a coating composition that is more suitable for the environment in which the investigation subject is placed, the number of types of test coating layers (sp) that the coating sheet for investigation has is preferably two or more, more preferably three or more, and even more preferably four or more.

[0016] [Test coating layer (sp)] The coating sheet for investigation of the present invention includes a test coating layer (sp) for evaluating the coating in an actual use environment. This test coating layer (sp) is assumed to be "not formed around" the place to which the coating sheet for investigation is to be applied. In other words, it is required that the area around the place to which the coating sheet for investigation is to be applied is not formed with a coating of the "same type" as the coating layer for investigation (sp), for example, that no coating is formed at all (only the substrate is present), or that the coating is formed but its "type" (mixture composition of the paint composition, surface roughness, film thickness, etc.) is different from that of the coating layer for investigation (sp). In one embodiment of the present invention, the coating sheet for investigation of the present invention has two or more different test coating layers (sp) that are not formed around.

[0017] The test coating layer can be formed, for example, by applying a test coating composition described below to a substrate or the like to obtain a coated body, and then curing and / or drying the coated body.

[0018] [Test paint composition] The test coating composition can be used without any particular limitation as long as it is a coating composition that may be suitable for the actual environment. Examples of such test coating compositions include marine coatings such as antifouling coatings for ship bottoms and anticorrosive coatings for tanks, architectural coatings such as coatings for the interior and exterior of buildings and coatings for building materials, coatings for structures such as bridges and steel towers, coatings for road vehicles such as automobiles, coatings for metal products such as machines and steel furniture, coatings for wood products such as furniture, coatings for transport tools such as containers, and coatings for road markings. Among these, from the viewpoint that the coating film is placed in various environments and it is difficult to select a coating composition suitable for the actual environment, coating compositions for structures used outdoors, in which the coating film performance evaluation method and coating recommendation method using the coating film sheet for investigation of the present invention are effective, are preferred as test coating compositions. In particular, marine paint compositions are more preferable because the navigation area, navigation mode, and usage pattern vary from ship to ship, making it difficult to select a paint composition suitable for the actual environment. Even more preferable are antifouling paints for the bottom of ships, which are inhabited by different marine organisms depending on the navigation area, and weather-resistant topcoat paints for the topside surface and upper deck of the bottom of ships, which are exposed to a complex array of factors such as temperature, humidity, sunlight, and weather depending on the navigation area.

[0019] Any antifouling paint for ship bottoms can be used without any restrictions, and representative examples include a hydrolysis type antifouling paint composition (x), a hydration decomposition type antifouling paint composition (y), and a silicone type antifouling paint composition (z).

[0020] The hydrolyzable antifouling coating composition (x) contains a hydrolyzable (co)polymer. When the coating film thereof comes into contact with water, a hydrolysis reaction of the (co)polymer occurs on the surface, and the coating film is gradually renewed from the hydrophilized surface layer, thereby exerting antifouling properties.

[0021] The hydrolyzable antifouling coating composition (x) can adjust the coating film renewal rate by changing the constituent units of the hydrolyzable (co)polymer contained therein and other contained components, and it is necessary to optimize the composition depending on the conditions of the area in which the ship to be painted travels, i.e., the type and amount of marine organisms that will adhere, the water temperature, and the sailing speed, operation rate, etc.

[0022] Examples of such hydrolyzable antifouling coating compositions (x) include hydrolyzable (co)polymers having a component derived from a metal ester group-containing monomer as described in JP 2002-012630, WO 2011 / 046086, and WO 2021 / 182454, and those using hydrolyzable (co)polymers having a component derived from a triorganosilyl ester group-containing monomer as described in JP 10-030071 and WO 2018 / 088377.

[0023] The hydration decomposition-type antifouling coating composition (y) exhibits antifouling properties as a hydration layer formed by water penetrating from the coating surface is renewed by a water flow or the like.

[0024] The hydration decomposition type antifouling coating composition (y) also needs to have an optimum composition depending on the conditions, similarly to the hydrolysis type antifouling coating composition (x).

[0025] Examples of such hydration decomposition type antifouling coating compositions include coating compositions described in International Publication WO93 / 02146 and International Publication WO2003 / 080747.

[0026] The silicone-type antifouling coating composition (z) forms a coating film from which marine organisms can easily fall off due to the low surface free energy, elasticity and slipperiness of the silicone rubber, which is the main component.

[0027] Examples of such silicone-type antifouling coating compositions include those disclosed in JP 2001-139816, International Publication WO2002 / 074870, International Publication WO2011 / 076856, International Publication WO2013 / 024106, and International Publication WO2022 / 070978.

[0028] Other examples of anti-paint compositions include those described in International Publication WO2014 / 010702, International Publication WO2016 / 008824, JP2001-342432, International Publication WO2012 / 084758, and JP2018-035227.

[0029] There are no particular limitations on the components contained in the test coating composition, but in general, it is preferable for the composition to contain a binder (A), a solvent (B), a pigment (C), an additive (D), and the like.

[0030] The binder (A) is a material that imparts a film-forming function to the coating composition, and is sometimes referred to as a resin. Specific examples of the binder (A) include various thermoplastic or thermosetting synthetic resins such as acrylic resins, silicone resins, acrylic silicone resins, epoxy resins, alkyd resins, vinyl resins, polyurethane resins, polyester resins, phenolic resins, chlorinated polyolefin resins, melamine resins, fluororesins, and petroleum resins; natural resins such as rosin (pine resin), modified rosin, and shellac; inorganic binders such as metal alkoxides such as alkali silicate and silicon alkoxide, and their (hydrolysis) condensates; and the like; and two or more of these may be used in combination. In addition, these binders include organic solvent-soluble type, non-aqueous dispersion type (NAD), water-soluble type, and emulsion type, and the curing method includes room temperature curing type, ultraviolet curing type, and heat curing type, and there is no particular limitation.

[0031] The solvent (B) is blended for the purpose of imparting suitable fluidity to the test coating composition and improving the workability of the coating. Specific examples of the solvent (B) include aromatic hydrocarbon organic solvents such as toluene and xylene, aliphatic hydrocarbon organic solvents such as heptane, alicyclic hydrocarbon organic solvents such as cyclohexane, ketone organic solvents such as methyl isobutyl ketone, ester organic solvents such as butyl acetate, water, etc.

[0032] The pigment (C) is blended for the purpose of coloring, imparting hiding power, imparting weather resistance, improving coating film strength, etc. Specific examples of the pigment (C) include inorganic pigments such as carbon black, red iron oxide (red iron oxide), yellow iron oxide, titanium white (titanium oxide), aluminum flakes, silica, mica, calcium carbonate, aluminum carbonate, magnesium carbonate, barium carbonate, aluminum oxide, aluminum hydroxide, aluminum silicate, magnesium silicate, potassium feldspar, zinc oxide, kaolin, alumina white, barium sulfate, calcium sulfate, zinc oxide, zinc sulfide, short glass fiber, and glass flakes, and organic pigments such as naphthol red and phthalocyanine blue.

[0033] The additives (D) are blended to impart various other functionalities, and examples thereof include wetting and dispersing agents, dehydrating agents, anti-settling agents, anti-sagging agents, defoaming agents, leveling agents, rheology control agents, surface conditioners, hardening accelerators, coupling agents, plasticizers, antifouling agents, slip agents, antibacterial agents, flame retardants, thermal conductive agents, and enzymes.

[0034] [Formation of test coating layer (sp)] A known method can be used to apply the test coating composition to form the test coating layer (sp). Examples of the method include a method using a spray, a brush, a roller, a film applicator, a flow coater, a roll coater, an electrodeposition coating, etc., and a method of immersing the coated object in the test coating composition.

[0035] The method for curing and / or drying the coated body may be drying at room temperature, heating, or irradiation with active energy rays as necessary. In addition, a curing and / or drying method that can form a coated body having a fine shape on the coating film surface, such as that described in International Publication WO2019 / 189412, may be used.

[0036] The thickness of the test coating layer (sp) is not particularly limited and can be adjusted depending on the antifouling paint composition used to form the test coating layer (sp), the embodiment and use of the investigation coating sheet of the present invention, etc., but can be, for example, in the range of 10 to 2000 μm, and preferably in the range of 50 to 500 μm.

[0037] In the coating sheet for investigation of the present invention, it is also preferable that the surface of the test coating layer (sp) has a specific roughness parameter. For example, when a coating film is formed by applying a paint composition by spraying or the like, the surface has a certain roughness, so it is preferable that the test coating layer (sp) also has a surface close to that roughness. It is also preferable to evaluate the effect of roughness by forming two or more test coating layers (sp) with different roughness parameters on the coating sheet for investigation. It is also preferable to measure the surface roughness of the test coating layer (sp) before testing. The roughness can be measured using a contact method such as a stylus method or a non-contact method using a laser displacement meter, and can be expressed by roughness parameters such as Rz, Rzjis, Ra, or parameters such as the average length of the roughness curve element RSm.

[0038] According to the present invention, a coating film can be formed using a coating method, curing and / or drying method that is difficult to employ at a construction site. This has the advantages of reducing the burden of painting work, shortening the time required to form the coating film, and enabling accurate control of the film thickness and ensuring smoothness, compared to construction at an actual construction site.

[0039] ·Uneven structure In one embodiment of the present invention, the test coating layer (sp) has an "irregular structure" on its surface. The "irregular structure" is typically a structure having fine irregularities with a periodic structure formed on the water-contacting surface of the test coating layer (sp), and includes a "riblet surface structure" that suppresses the generation of turbulence when a fluid comes into contact and reduces resistance (friction coefficient), and a surface structure having protrusions such as prismatic, cylindrical, or triangular rod-shaped protrusions, which may or may not be in contact with each other.

[0040] The riblet surface structure is characterized by the difference in height between the projections and recesses, i.e., the riblet height. From the viewpoint of ease of forming the riblet structure, the riblet height (h) is preferably in the range of 0.1 to 1000 μm, more preferably in the range of 0.5 to 500 μm, and even more preferably in the range of 1 to 100 μm. The riblet height (h) can be determined by measuring the 10-point average linear roughness Rzjis (JIS B 0601:2001) of the surface in any cross section of the riblet surface in any range where periodic projections and recesses can be recognized.

[0041] Examples of the riblet surface structure include a groove structure as described in JP-A-2011-530443 and a structure having a specific periodic pattern as described in JP-A-2012-508128, and the groove structure is preferable from the viewpoint of ease of structure formation. When the riblet structure is a groove structure, examples of the groove structure include a V-shaped groove, a U-shaped groove, a rectangular groove, and a trapezoidal groove. From the viewpoint of ease of formation of the riblet structure, the average distance between the peaks of the unevenness in the longitudinal direction and the vertical direction of the groove structure, that is, the period S [μm] of the groove structure, is preferably in the range of 0.5 to 5, more preferably in the range of 0.8 to 4, and even more preferably in the range of 1.5 to 3.5, in terms of the ratio value to the riblet height (h).

[0042] [Optional component layer] The coating sheet for investigation of the present invention may further have at least one selected from the group consisting of an adhesive layer (ad), a substrate layer (bs), a bonding layer (cn), an indication layer (id), a protective layer (pr), and a release layer (rl). These optional layers may be provided in any order, and each layer may have the same or different layers. For example, two or more optional constituent layers may be laminated with the test coating layer (sp) or adhesive layer (ad) sandwiched therebetween, and an example of such a laminate structure is adhesive layer (ad)-substrate layer (bs)-adhesive layer (ad)-bonding layer (cn)-test coating layer (sp). A single optional constituent layer may have two or more of the functions of the above layers, and an example of such a coating film of an epoxy primer may be used as both a bonding layer (cn) and a substrate layer (bs).

[0043] Each layer may be provided only on a part of the adjacent layer. For example, in the case where a magnet is included as described later, an embodiment in which the adhesive layer (ad) is formed only on the end of the sheet can be mentioned, and such an embodiment can reduce the area of ​​the adhesive layer (ad). In addition, if the release layer (rl) adjacent to the test coating layer (sp) is formed except for the end of the test coating layer (sp), it is preferable because the step of curing the test coating layer (sp) can be omitted when sealing the end of the test coating layer (sp) after attaching the test coating sheet of the present invention.

[0044] It is also preferable to expose another layer only at the end of the surface of the sheet having the test coating layer (sp). If the base layer (bs), binding layer (cn), and protective layer (pr) have better adhesion to the coating composition used in the sealing treatment than the test coating layer (sp), exposing these layers at the end is advantageous in that the sealing treatment can be performed more firmly and the area to be sealed can be indicated during the sealing treatment.

[0045] Each layer may be composed of two or more different layers. For example, the adhesive layer (ad) may be strong only at the edge of the sheet where peeling is likely to occur, and the adhesive layer (ad) may be weak at the other areas, thereby reducing costs.

[0046] The color of each of the optional layers may be any color, but if the color is different from the other layers or the object, or if the color is metallic, fluorescent, or other conspicuous color, it has the advantage that the layer can be easily identified, for example, when the other layers are lost due to damage or wear. Also, each of the optional layers may be identifiable by reflecting a specific light when irradiated with ultraviolet or infrared light.

[0047] [Adhesive layer (ad)] The coated sheet for investigation of the present invention preferably has an adhesive layer (ad) in order to obtain excellent adhesion to the object.

[0048] The adhesive used in the adhesive layer (ad) is not particularly limited, and any known adhesive can be used, and may be appropriately selected according to the application. Examples of adhesives include pressure-sensitive adhesives (adhesives), anaerobic curing adhesives, photocuring adhesives, moisture curing adhesives, hot melt adhesives, heat curing adhesives, and dry curing adhesives. Pressure-sensitive adhesives are preferred because they can be easily removed after using the coating sheet for investigation.

[0049] Resins used in these adhesives include, for example, acrylic resins, urethane resins, vinyl chloride resins, vinyl acetate resins, vinyl alcohol resins, vinyl chloride-vinyl acetate copolymers, styrene-acrylic copolymers, polyester resins, amide resins, cyanoacrylate resins, epoxy resins, polyester resins, polyether resins, and silicone resins, and these resins can be used alone or in combination. Two-liquid curing type urethane adhesives and ester adhesives using an isocyanate compound or the like as a curing agent can also be used.

[0050] Examples of pressure-sensitive adhesives include acrylic pressure-sensitive adhesives, silicone pressure-sensitive adhesives, natural or synthetic rubber-based pressure-sensitive adhesives, polyurethane pressure-sensitive adhesives, vinyl alkyl ether pressure-sensitive adhesives, polyester pressure-sensitive adhesives, polyamide pressure-sensitive adhesives, poly-α-olefins, and styrene block copolymer-based pressure-sensitive adhesives, and these may be used in combination. Among them, acrylic pressure-sensitive adhesives are preferred because the adhesive strength can be easily designed and they have excellent weather resistance and heat resistance, and silicone pressure-sensitive adhesives are also preferred because they can handle a wide temperature range and have excellent water resistance and chemical resistance. In addition, when the coating sheet for investigation of the present invention is attached to a target and the sheet is peeled off after use, the adhesive layer (ad) may remain on the coating film, so it is preferable that the resin contained in the adhesive used in the adhesive layer (ad) is the same type as the resin contained in the paint composition to be applied to the surface after peeling. For example, when an acrylic paint composition is applied to the surface after peeling, it is preferable to use an acrylic pressure-sensitive adhesive, and when a silicone paint composition is applied, it is preferable to use a silicone pressure-sensitive adhesive.

[0051] Pressure-sensitive adhesives generally exhibit a dynamic viscoelasticity of 3×10 at a frequency of 1 Hz when measured at room temperature (25°C). 6 It has a storage modulus (E') of less than dynes / cm.

[0052] The pressure sensitive adhesives may be organic solvent based, water based emulsion, hot melt, heat curable, and UV curable pressure sensitive adhesives.

[0053] The acrylic pressure-sensitive adhesive contains at least 20% by weight of an acrylic polymer, the total of which is composed of at least 50% by weight of units derived from one or more low Tg (meth)acrylate ester monomers. Such acrylic polymers can be produced by free radical polymerization techniques such as solution polymerization, bulk polymerization, or emulsion polymerization, and may be of any type, such as random copolymers, block copolymers, or graft polymers. The low Tg (meth)acrylate monomer refers to a polymer having a Tg (glass transition point) of 0° C. or less when it is formed into a homopolymer. The acrylic pressure-sensitive adhesive may further contain a unit derived from a polar monomer. Representative polar monomers include, for example, acid-functional monomers (e.g., acrylic acid, methacrylic acid), hydroxyl-functional (meth)acrylate monomers, nitrogen-containing monomers (e.g., acrylamide), and combinations thereof. In some embodiments, the acrylic pressure sensitive adhesive comprises at least 0.5, 1, 2 or 3% by weight, and typically no more than 10% by weight, of units derived from polar monomers, such as acrylamide and / or acid-functional monomers, such as (meth)acrylic acid.

[0054] The silicone pressure-sensitive adhesive contains at least 20% by mass of silicone in the adhesive. Examples of the silicone pressure-sensitive adhesive that can be used include addition type silicone-based adhesives, peroxide curing type silicone-based adhesives, and condensation type silicone-based adhesives, and these may be used in combination, and either one-component or multi-component adhesives may be used.

[0055] The addition type silicone adhesive is generally an adhesive in which a silicone polymer is produced by addition reaction (hydrosilylation reaction) between an organopolysiloxane having an alkenyl group such as a vinyl group on a silicon atom and an organopolysiloxane having a hydrosilyl group using a platinum compound catalyst such as chloroplatinic acid. Examples of the addition type silicone adhesive include "KR-3700" and "X-40-3291-1" manufactured by Shin-Etsu Chemical Co., Ltd., and "Dow Corning Toray SD 4592 PSA" (vinyl group-containing silicone) / "BY24-742" (Si-H compound) manufactured by Dow Corning Toray Co., Ltd. It is preferable that the addition type silicone adhesive contains a curing catalyst such as a platinum catalyst. Examples of the platinum catalyst that are commercially available include the trade name "CAT-PL-50T" (manufactured by Shin-Etsu Chemical Co., Ltd.) and the trade name "DOWSIL NC-25 Catalyst".

[0056] A peroxide-curable silicone-based adhesive is generally an adhesive in which organopolysiloxane is cured (crosslinked) with peroxide to produce a silicone-based polymer. For example, "KR-100" manufactured by Shin-Etsu Chemical Co., Ltd. is commercially available as a peroxide-curable silicone-based adhesive.

[0057] Condensation type silicone-based pressure-sensitive adhesives are generally pressure-sensitive adhesives that produce silicone-based polymers by a dehydration or dealcoholization reaction between polyorganosiloxanes having hydrolyzable silyl groups such as silanol groups or alkoxysilyl groups at the ends, and these silicone-based polymers may have a linear, branched, or cyclic skeleton, or may be a mixture thereof.

[0058] In addition, as the adhesive layer (ad) using such a pressure-sensitive adhesive, a commercially available substrate-less tape may be used, for example, substrate-less silicone tape "NSD-100" manufactured by Nippa Corporation.

[0059] The pressure-sensitive adhesive may further include one or more suitable additives as required, such as crosslinkers (e.g., multifunctional (meth)acrylate crosslinkers (HDDA, TMPTA, etc.), epoxy crosslinkers, isocyanate crosslinkers, melamine crosslinkers, aziridine crosslinkers), tackifiers (e.g., phenol-modified terpenes, rosin esters (e.g., glycerol esters of rosin, pentaerythritol esters of rosin, etc.), C5 and C9 hydrocarbon tackifiers), thickeners, plasticizers, fillers, antioxidants, UV absorbers, antistatic agents, surfactants, leveling agents, colorants, flame retardants, and silane coupling agents.

[0060] Examples of anaerobic curing adhesives include those described in International Publication WO2007 / 049028 and International Publication WO2014 / 151358.

[0061] Examples of photocurable adhesives include those described in International Publication WO93 / 17078, International Publication WO2004 / 000965, International Publication WO2008 / 152956, International Publication WO2013 / 047435, International Publication WO2013 / 173976, and International Publication WO2016 / 117631.

[0062] Examples of moisture-curing adhesives include those described in International Publication WO2001 / 053423, International Publication WO2004 / 074330, and International Publication WO2007 / 023669.

[0063] An example of the hot melt adhesive is described in JP-A-2002-1886.

[0064] Examples of thermosetting adhesives include those described in International Publication WO98 / 45366.

[0065] The adhesive layer (ad) can be disposed on the film by various conventional coating methods, such as roller coating (such as gravure), flow coating, dip coating, spin coating, spray coating, knife coating, die coating (such as rotary or slit), extrusion coating (such as hot melt), and printing.

[0066] The adhesive may be applied directly to the coating layer (sp) or substrate layer (bs) described herein, or may be transfer coated using a release liner. If a release liner is used, the adhesive is coated onto the liner and then laminated to the film, or coated onto the film and then the release liner is applied to the adhesive layer. The adhesive layer (ad) may be applied immediately prior to application, or may be heated or irradiated after application, if desired.

[0067] The adhesive layer (ad) may be a continuous layer or may be partially or completely structured, for example a pressure-sensitive adhesive layer having a network of channels or similar structures through which air can pass, or a pressure-sensitive adhesive layer that can be repositioned by embossing.

[0068] The thickness of the adhesive layer (ad) is not particularly limited, but in order to obtain excellent adhesion, it is preferably 1 μm or more and 1000 μm or less, and more preferably 5 μm or more and 600 μm or less. The thickness of the adhesive layer (ad) is preferably thicker when stronger adhesion is required or when the surface to be applied has a high roughness, but is preferably thinner in applications where the coating sheet itself for investigation is not preferred to be thick, such as when the smoothness of the target is important.

[0069] The adhesive layer (ad) is preferably capable of adhering to a variety of surfaces, such as various woods, metals, organic polymeric materials, and the like.

[0070] [Base material layer (BS)] The substrate layer (bs) is a preferred constituent layer of the investigated coated sheet of the present invention, since it has the function of increasing the strength of the investigated coated sheet of the present invention.

[0071] The substrate layer (bs) is not particularly limited as long as it has the above-mentioned functions, and examples thereof include coatings, films, and sheets made of materials such as resin, metal, paper, nonwoven fabric, cloth, and glass, or composite materials combining these materials.

[0072] The inclusion of a layer made of metal in the base material layer (bs) has the following advantages: a strong sheet can be obtained even though it is a thin layer; it helps prevent the coating from cracking due to excessive bending during production, transportation, application, etc.; it has excellent adhesion to the coating, the bonding layer (cn) and the adhesive layer (ad) described below; it can prevent water penetration when applied to submerged areas; and it is easy to peel off and not easily torn when peeling off for removal after use.

[0073] Examples of metals used for the material of the base layer (bs) include those composed of one or more metal elements selected from the group consisting of iron, aluminum, titanium, and copper.

[0074] When iron is used as a constituent element, it is possible to use stainless steel alloyed with chromium or surface-plated tinplate, which suppresses rusting, depending on the application. The use of such metals is effective in preventing the purpose of the investigation (particularly the purpose other than the evaluation of the presence or absence of rusting on the base) from being hindered by peeling, peeling, discoloration, etc. due to rusting in an environment that is easily affected by water. As stainless steel, for example, ferritic stainless steel such as SUS430 (containing about 17% chromium, inexpensive, excellent corrosion resistance, and magnetic), austenitic stainless steel such as SUS304 (containing about 18% chromium and about 8% nickel, excellent in high / low temperature change, not magnetic), and martensitic stainless steel such as SUS410 can be used without restrictions, and can be appropriately selected depending on the environment, cost, and method of use.

[0075] In the case of applications involving contact with water, it is preferable to use aluminum or titanium in addition to the above-mentioned stainless steel or tinplate from the viewpoint of corrosion resistance. On the other hand, as described below, when the degree of rust generation is one of the evaluation criteria for the purpose of the test itself, metals that do not have such a rust-inhibiting function may be used.

[0076] The base material layer (bs) including a layer made of resin has the following advantages: excellent shape restoration after deformation; ease of cutting; excellent adhesion to coatings, the bonding layer (cn) and the adhesive layer (ad) described below; ability to prevent water penetration when applied to submerged areas; and ease of peeling off when peeling off for removal after use.

[0077] Examples of resins used as the material of the substrate layer (bs) include silicone resins; (co)polymers of unsaturated monomers such as acrylic resins, polyvinyl chloride resins, polystyrene resins, polyethylene resins, and polypropylene resins; polyester-based resins such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polyurethane resins; epoxy resins; polyacetal; polycarbonate; acetyl cellulose; and composites thereof. Among these resins, polyvinyl chloride is preferred from the viewpoint of excellent strength, processability, and economy. In addition, when the substrate layer (bs) comes into contact with the test coating layer (sp) which is the above-mentioned silicone-type antifouling coating composition (z) or the silicone resin-based tie coat or primer described later, it is preferable to use a silicone resin from the viewpoint of easy adhesion.

[0078] Examples of paper used as the material for the base layer (bs) include uncoated printing paper such as fine paper and medium quality paper, and coated paper such as art paper and coated paper, as well as so-called Japanese paper and tissue paper.

[0079] The base layer (bs) is preferably a combination of nonwoven fabrics, which are easy to cut during manufacturing or operation, and are difficult to tear and easy to peel off when peeled off and removed after use. Examples of such nonwoven fabrics include those made of polyethylene, polypropylene, polyester, rayon, glass, etc., and the strength and hand-tearability can be adjusted depending on the application by adjusting the fiber thickness and density. Examples of the use of such a base layer include those described in International Publication WO2015 / 98983 and International Publication WO2018 / 117264.

[0080] The base layer (bs) may have a barrier function to reduce the movement of water and other liquids. An example of such a base layer (bs) is the water vapor barrier layer described in JP 2015-224334 A.

[0081] The substrate layer (bs) may have fine irregularities on a part or the whole of its surface as required. Methods for forming such fine irregularities include surface polishing with sandpaper or the like, blasting, embossing, etc. When the substrate layer (bs) has such fine irregularities, it has excellent adhesion to the test coating layer (sp) and the bonding layer (cn) that are in contact with this surface.

[0082] If necessary, the substrate layer (bs) may be subjected to a surface treatment on a part or the whole of its surface, for example, a corona treatment or an etching treatment.

[0083] The thickness of the substrate layer (bs) is not particularly limited and can be adjusted depending on the material of the substrate layer (bs) used, the embodiment of the coating sheet for investigation of the present invention, and the application, etc., and is, for example, in the range of 5 to 1000 μm, preferably in the range of 10 to 500 μm.

[0084] [Coupling layer (cn)] The bonding layer (cn) is a preferred constituent layer of the investigated coating sheet of the present invention, since it has the function of increasing the bonding strength with other layers contained in the investigated coating sheet of the present invention.

[0085] The bonding layer (cn) is not particularly limited as long as it has the above-mentioned function. Examples of the bonding layer (cn) include epoxy resin-based tie coats or primers as described in JP-A-10-259351 and WO2017 / 146193, silicone resin-based tie coats or primers as described in WO91 / 14747 and WO2006 / 109600, and other commercially available tie coats or primers that have been dried and cured.

[0086] In particular, when an antifouling coating film containing a curable organopolysiloxane is disposed as a test coating layer (sp) on top of a substrate layer (bs), adhesive layer (ad), etc., it is preferable to dispose a bonding layer (cn) using a silicone resin-based tie coat or a silicone primer between the substrate layer (bs), adhesive layer (ad), etc. and the test coating layer (sp).

[0087] The bonding layer (CN) may further have a barrier function to reduce the movement of water and other liquids. Examples of such a bonding layer (CN) include commercially available anticorrosive paints and those described as water vapor barrier layers in JP 2015-224334 A. In one embodiment of the present invention, the coating sheet for investigation may have a layer that combines the functions of the substrate layer (BS) and the bonding layer (CN).

[0088] The thickness of the bonding layer (cn) is not particularly limited and can be adjusted depending on the resin contained in the bonding layer (cn) used, the embodiment and use of the coating sheet for investigation of the present invention, etc., but is, for example, in the range of 10 to 400 μm, preferably in the range of 20 to 200 μm.

[0089] [Display layer (id)] The investigational coating sheets of the present invention may have an identification layer (ID) for the purpose of indicating the product, type, attributes, properties, individual number, logo, application guidance, etc. of the sheet or coating under test.

[0090] Examples of the display layer (id) include a coating film formed by applying a coating composition similar to the above-mentioned test coating layer (sp) but with a different hue, a coating film formed by applying a coating composition of the tie coat or primer listed in the above-mentioned bonding layer (cn), and other layers printed with printing ink. In particular, when the display layer (id) is not likely to be compatible with the application environment like the test coating layer (sp), it is preferable to form a protective layer (pr) described below on the display layer (id) to protect the display layer (id) from deterioration due to dirt or ultraviolet light degradation.

[0091] The thickness of the indication layer (id) is not particularly limited and can be adjusted depending on the material of the indication layer (id) used, the embodiment and use of the investigation coating sheet of the present invention, etc., but is, for example, in the range of 10 to 400 μm, preferably in the range of 20 to 200 μm.

[0092] The display format of the display layer (id) may be, for example, letters, numbers, symbols, or figures.

[0093] The identification layer (ID) preferably includes letters, numbers, symbols, etc. that allow identification of different test coating layers (SP) when the test coating sheet has multiple different test coating layers (SP). When the test coating sheet includes such an identification layer (ID), it becomes easier to communicate the results of the test.

[0094] It is also preferred that the indicator layer (ID) contains letters, numbers, symbols, etc., that indicate the individual number of the coating sheet for investigation. When the coating sheet for investigation contains such an indicator layer (ID), it becomes easy to identify the recipient of the coating sheet for investigation, the coating layer (SP) that the coating sheet for investigation has, and the investigation results when the investigation results are saved as an image and transmitted.

[0095] In addition to the above, the indication layer (id) may be a mark or enclosure indicating the installation method or precautions for the sheet, the orientation or position in which it should be installed, or the position of the test coating film.

[0096] In one embodiment of the present invention, the investigational coating sheet of the present invention has at least one coating layer to be tested (sp) and an indicator layer (id) that are not formed around the periphery.

[0097] [Protective layer (PR)] The coating sheet for investigation of the present invention may have a protective layer for the purpose of protecting other layers contained in the laminate sheet. In particular, when the display layer (id) is not likely to be compatible with the application environment like the coating layer (sp) to be tested, it is preferable to protect it from deterioration due to dirt or ultraviolet degradation with a protective layer (pr).

[0098] As the protective layer (pr), for example, in the case of antifouling of ship bottoms, an antifouling coating film such as that described in the test coating film layer can be used.

[0099] The thickness of the protective layer (pr) is not particularly limited and can be adjusted depending on the material of the protective layer (pr) used, the embodiment and use of the coating sheet for investigation of the present invention, etc., but is, for example, in the range of 5 to 500 μm, preferably in the range of 10 to 300 μm.

[0100] [Release layer (RL)] The release layer (rl) is a layer that is brought into contact with the test coating layer (sp) and / or adhesive layer (ad) and is peeled off when the coating sheet for investigation of the present invention is used. It is a preferred constituent layer that the coating sheet for investigation of the present invention has, from the viewpoints of protecting the coating layer for investigation (sp) and / or adhesive layer (ad) until then and ensuring ease of application and adhesion.

[0101] The release layer (rl) is typically a layer comprising a paper or film release liner coated or modified with a low surface energy compound such as organosilicon compounds, fluoropolymers, fluorosilicones, polyurethanes, polyolefins, etc. This release liner may be a polymer sheet made from polyethylene, polypropylene, PVC, or polyester with or without the addition of a compound that repels the adhesive of the adhesive layer (ad).

[0102] It is preferable to select the release layer (rl) so as to have an appropriate peel load with respect to the adhesive layer (ad).

[0103] The release liner may have a microstructured or microembossed pattern to impart a predetermined uneven structure to the test coating layer (sp) and / or adhesive layer (ad). For example, the release layer (rl) may have a release liner having a structure that serves as a mold for imparting the above-mentioned "riblet surface structure" to the surface of the test coating layer (sp) that comes into contact with it.

[0104] The thickness of the release layer (rl) is not particularly limited and can be adjusted depending on the material of the release layer (rl) used, the embodiment and application of the coating sheet for investigation of the present invention, etc., but is, for example, in the range of 5 to 200 μm, preferably in the range of 10 to 100 μm.

[0105] [Other components: Magnets] The substrate layer (bs), test coating layer (sp), and binding layer (cn) of the coating sheet for investigation of the present invention may have magnets in part or in whole. If the object reacts to magnets, any of the above layers of the coating sheet for investigation of the present invention may have magnets, so that the sheet can be attached to the object without the adhesive layer (ad). In addition, when the sheet is attached by a magnet, the coating sheet for investigation can be easily peeled off, so that the original state is easily restored after the evaluation using the coating sheet for investigation is completed, the coating sheet for investigation after evaluation can be easily recovered when it is recovered for analysis, and no residue of the adhesive layer (ad) is left on the object when the sheet is peeled off. In addition, even when the adhesive layer (ad) is provided, stronger attachment can be obtained by combining the adhesive force of a magnet.

[0106] [Example of a multi-layer structure] In the first embodiment, the coating sheet for investigation of the present invention is composed of a release layer (rl), an adhesive layer (ad), a substrate layer (bs), a bonding layer (cn), a test coating layer (sp), and a release layer (rl) in this order. In this embodiment, the adhesive layer (ad), substrate layer (bs), and test coating layer (sp) are composed in this order, but it is preferable in terms of securing ease of application and adhesion that the bonding layer (cn) is provided between the substrate layer (bs) and the test coating layer (sp), and that the release layer (rl) is provided adjacent to each of the adhesive layer (ad) and the test coating layer (sp).

[0107] In the second embodiment, the coating sheet for investigation of the present invention is composed of a release layer (rl), an adhesive layer (ad), a substrate layer (bs), an adhesive layer (ad), a substrate layer (bs), a bonding layer (cn), a test coating layer (sp), and a release layer (rl) in that order. In this embodiment, a plurality of adhesive layers (ad) and substrate layers (bs) are provided, but in this configuration, by making the substrate layers (bs) different from one another and / or making the adhesive layers (ad) different from one another, a well-balanced combination of adhesive strength and workability can be achieved.

[0108] The investigational coating sheet of the present invention may be prepared by attaching and cutting a sheet member including the test coating layer (sp) and the adhesive layer (ad) to another sheet member including the substrate layer (bs) etc.

[0109] [Paint film evaluation method using survey paint film sheets] The coating performance evaluation method of the present invention (sometimes referred to herein as the "coating evaluation method") is a method using an investigation coating sheet described herein, and includes: (i) a step of attaching an investigation sheet having at least one test coating layer (sp) that is not formed on the surrounding area to an object to be covered with a coating or a substitute object (referred to herein as the "attachment step"); (ii) a step of placing the investigation sheet in an environment in which the object is placed for a certain period of time with at least a portion of the test coating layer exposed on the surface (referred to herein as the "exposure step"); and (iii) a step of acquiring information regarding the state of the investigation coating sheet (referred to herein as the "information acquisition step").

[0110] The coating sheet to be investigated used in the coating evaluation method of the present invention may be an embodiment as described herein as the coating sheet to be investigated of the present invention. For example, the coating sheet to be investigated may further have one or more layers selected from the group consisting of an adhesive layer (ad), for example an adhesive layer (ad) containing a pressure-sensitive adhesive, a substrate layer (bs), for example a substrate layer (bs) containing a metal, and an indicator layer (id), in addition to the coating layer to be investigated (sp). The coating sheet to be investigated may also have two or more different coating layers to be investigated (sp).

[0111] The "subject to be coated with a coating film" is an object to be coated with a coating film based on the results of the coating film evaluation method using the coating film sheet of the present invention. The subject is not particularly limited, but it is preferable that the subject is a "water-contacting structure" in that the survey works effectively. The "substitute subject" is not the "subject to be coated with a coating film" itself, but is an object that can achieve the desired performance by covering the "subject to be coated with a coating film" with the "same type of coating film" (details will be described later) as the test coating film layer (sp) based on the survey results using the coating film sheet for survey. For example, if the subject is a ship or other moving body, another subject having a similar movement pattern (navigation pattern, route, etc.) to the "subject to be coated with a coating film" to be covered with the same type of coating film as the test coating film layer (sp) can be the "substitute subject". In this specification, the matters described about the "subject to be coated with a coating film" can be read as the descriptions about the "substitute subject" as long as there is no problem in the context.

[0112] The water-contacting structure is not particularly limited, and may be any structure capable of forming a coating film and exhibiting its function. Examples of the water-contacting structure include substrates that are fully or at least partially submerged in water, preferably in seawater, all or at least partly, permanently or temporarily, such as ships (e.g., large steel ships such as container ships, tankers, and bulk carriers, and hull panels for fishing boats, FRP boats, wooden boats, yachts, and the like, including both newly built and repaired ships), fishing and other marine materials (e.g., ropes, fishing nets, fishing gear, floats, buoys, diver suits, underwater goggles, oxygen cylinders, swimsuits, torpedoes), underwater structures (e.g., oil pipelines, water conveyance piping, circulating water pipes, water supply and drainage outlets of thermal and nuclear power plants, undersea cables, seawater utilization equipment (seawater pumps, etc.), megafloats, coastal roads, undersea tunnels, port facilities, various underwater civil engineering structures in canals, waterways, etc.). As the water-contacting structure, a mobile body which requires high antifouling properties and requires periodic repair such as topcoating, for example, a ship such as a container ship, a tanker, or a bulk carrier (either a newly built ship or a ship already in service), is preferred.

[0113] The water-contacting structure may be a water-contacting structure treated with an anticorrosive agent or other treating agent, or a water-contacting structure having a coating film (non-antifouling coating film) other than an antifouling coating film such as an anticorrosive coating film (e.g., zinc-rich paint), an anticorrosive coating film (e.g., epoxy-based heavy-duty anticorrosive paint), or a binder coating film formed on the surface, or an antifouling coating film (old antifouling coating film) formed from a deteriorated, altered or worn laminated antifouling coating film or other antifouling paint composition. In a water-contacting structure with a laminated antifouling coating film, the laminated antifouling coating film does not need to be formed in direct contact with the surface of the water-contacting structure, and may be formed on the water-contacting structure via a treating agent, another coating film, etc. Thus, the water-contacting structure with a laminated antifouling coating film may further include other treating agents, coating films, etc. in addition to the water-contacting structure and the laminated antifouling coating film. The laminated antifouling coating film can be formed on various non-antifouling coating films, deteriorated antifouling coating films, etc.

[0114] The "non-antifouling coating film" of a water-contacting structure refers to a coating film other than an antifouling coating film, such as an undercoat coating film or an intermediate coating film, which is formed on the surface of the water-contacting structure before forming a laminated antifouling coating film according to the type and use of the substrate. The type of the non-antifouling coating film is not particularly limited, and examples thereof include an anti-rust coating film formed from an anti-rust paint, an anti-corrosion coating film formed from an anti-corrosion paint, and a binder coating film formed from a binder paint. Examples of the anti-corrosion coating film include those formed from an anti-corrosion paint containing an epoxy resin. Examples of the binder coating film include those formed from a binder paint containing one or more types of resin such as an epoxy resin, a vinyl resin, or a (meth)acrylic resin. When coating a water-contacting structure such as a ship, there is no clear distinction between an anti-corrosion coating film (undercoat coating film) and a binder coating film (intermediate coating film), and a coating film that serves both purposes may be used, but the "non-antifouling coating film" may be a binder coating film that also has such an anti-corrosion coating function.

[0115] In a water-contacting structure, the portion to be covered with the laminated antifouling coating film is not particularly limited and can be appropriately selected depending on the application. For example, when the water-contacting structure is a ship, the constantly submerged portion or the alternating wet and dry portion exposed to a biological fouling environment can be the portion (part of the substrate) on which the antifouling coating film is formed. Note that when the water-contacting structure is a ship, the antifouling coating film can be formed not only on the ship bottom (constantly submerged portion) but also on the entire portion on which a general antifouling coating film is formed, including the waterline portion (alternating wet and dry portion).

[0116] The "old antifouling coating film" of a water-contacting structure refers to an antifouling coating film that has been used in contact with water (seawater) for a certain period of time (e.g., the service life of the antifouling coating film) and is in a deteriorated, altered, or worn state compared to the healthy antifouling coating film before use (before immersion in seawater). The degree of deterioration, alteration, or wear of the antifouling coating film is not particularly limited, and it may be to a degree that is deemed necessary or preferable to cover with a laminated antifouling coating film. The type of the old antifouling coating film is not particularly limited, and it may be a laminated antifouling coating film or another antifouling coating film. Examples of antifouling coating films include hydrolysis type (e.g., coating film formed from silyl ester resin-based antifouling paint) and hydration decomposition type (e.g., coating film formed from vinyl chloride-isobutyl vinyl ether resin-based antifouling paint).

[0117] [(i) Attachment process] The application step (i) is a step of applying a coating sheet for investigation, which has at least one test coating layer (sp) that is not formed around the test coating layer, to an object to be covered with the coating. The "object to be covered with the coating" refers to an object to be investigated for covering with the "same type of coating" as the test coating layer (sp). Here, the "same type of coating" includes (i) a coating that is substantially the same as the test coating layer (sp) in composition, thickness, surface structure, and other properties (formed under the same conditions using the same paint composition) and can be directly determined from the results of the investigation using the test coating layer (sp) whether or not the desired performance can be achieved, and (ii) a coating that has a different composition, thickness, surface structure, and other properties within a range that can be adjusted in consideration of other knowledge to achieve the desired performance based on the results of the investigation using the test coating layer (sp). Examples of the above (ii) coating film that is not "substantially the same coating film" as the test coating layer (sp) but can be said to be "the same type of coating film" include coating films that contain the same types of components as the test coating composition used to form the test coating layer but have different component contents, and that are presumed to be able to achieve the desired performance by adjusting the component contents based on the survey results and taking into account other knowledge without retesting. Alternatively, a coating film that has the same general formula of the (co)polymer or resin related to the antifouling performance as the test coating composition used to form the test coating layer, but has different specific matters related to the structure of the monomer-derived composition (chemical structure of the side chain, etc.), the number of repeating units, and other definitions of the general formula, and that are presumed to be able to achieve the desired performance by adjusting the specific matters based on the survey results and taking into account other knowledge without retesting, can also be said to be "the same type of coating film" but not "substantially the same coating film". In addition, a coating film that is presumed to be able to achieve the desired performance by adjusting the thickness, surface structure, and other properties of the coating film based on the survey results and taking into account other knowledge in accordance with the environment, period, and other conditions (for example, fouling load) in which the object to be coated will be placed, without the need for further testing, can also be considered a "similar coating film" rather than a "substantially identical coating film."

[0118] In the pasting step (i), a coating sheet for investigation having at least one test coating layer (sp) that is not formed around the object to be covered with a coating film can be pasted to the object to be covered with the coating film before the coating is performed. A specific embodiment thereof is described in detail below. The pasting step can be performed before the object is covered with the same type of coating film as the test coating film layer (sp) of the coating film sheet for investigation. In such an embodiment, a case where the coating film sheet for investigation is used for an investigation prior to the actual coating to determine whether it is appropriate to cover the object with the same type of coating film as the test coating film layer (sp) (repainting from a different type of coating film) is assumed. The area to be pasted may or may not have a coating of a different type from the test coating film layer (sp) formed around it (it may be in the state of only the substrate), and the area to be pasted may have a coating similar to the surrounding area (not the same as the test coating film layer (sp)) formed in advance, or a coating such as an undercoat or an undercoat may be formed. The application step (i) may also be carried out simultaneously with or after coating the target with the same type of coating as the test coating layer (sp) of the coating sheet to be investigated, i.e. the target area to be applied is an area that is to be coated or has been coated in advance with the same type of coating as the test coating layer (sp), and the coating sheet to be investigated is applied thereto.

[0119] Since the adhesion of the coating sheet for investigation can be improved if the area to be applied is smooth, if the area to be applied has bumps or grooves, it is preferable to smooth the base with a sealant, putty, cement, etc., and paint may be coated on top of that.

[0120] Before the application step (i), the object to which the investigation coating sheet is to be applied may be subjected to a surface treatment, such as polishing with sandpaper or a machine tool, wiping with water or an organic solvent, removing dirt and dust from the surface with a vacuum cleaner or tape, drying, wiping to remove moisture and oil, heating, drying, etc.

[0121] Before or after the application step (i), a groove or a depression may be formed in all or part of the area where the end of the coating sheet to be applied is located. This allows the end to sink lower than the surrounding area, making it difficult for the coating sheet to peel off. The depth of the groove or depression is not particularly limited, but is preferably equal to or greater than the thickness of the sheet, and is preferably less than the thickness of the old antifouling coating layer of the object to be applied, such as a water-contacting structure. Furthermore, the formation of the groove or depression can be combined with the above-mentioned sealing to enhance the effect of preventing peeling. When the groove or depression is formed before the application step, it can be used to confirm the application position of the object to be applied, or as a mark or guide. The groove or depression can be formed by cutting, for example, with a knife, a carving knife, or an electric tool.

[0122] When the coating sheet to be examined does not have an adhesive layer (ad), an adhesive may be applied to the application target area and / or the application surface of the coating sheet to be examined before the application step (i). The adhesive and adhesive method in such an embodiment may be the same as those described above for the adhesive layer (ad) that the coating sheet to be examined optionally has, but it is also possible to use a primer paint for the application target area. For example, when the object is made of steel, an anticorrosive paint such as an epoxy resin paint is generally applied, but if the coating sheet to be examined is applied using such an anticorrosive paint that has both anticorrosive and adhesive properties, the adhesive layer (ad) will also have an anticorrosive function.

[0123] There are no particular limitations on the method of applying the coating sheet for investigation, but a general tool such as a rubber roller may be used, or a machine that can move and apply using magnetic force as described in International Publication WO2016 / 193326, or a remotely controlled machine that can fly and apply to the target location may be used. The coating sheet for investigation may also be applied underwater.

[0124] The pasting step (i) preferably further includes a process of sealing and connecting the surface edge of the investigation coating sheet and the surrounding target surface with a test coating composition or other coating composition by a method such as that described in International Publication WO2018 / 100108, or a process of overlapping and connecting the surface edge and the surrounding target surface with tape, in order to prevent the investigation coating sheet from peeling off from the substrate. Among these, a process of sealing and connecting the surface edge of the investigation coating sheet and the surrounding target surface with a test coating composition or other coating composition is more preferable in terms of excellent workability and adhesion. Examples of the coating composition used for such a sealing treatment include those containing the above-mentioned binder (A), and can be used without any particular limitation, but it is more preferable to use a thermosetting coating composition such as an epoxy resin-based coating composition in terms of obtaining stronger adhesion. In such a sealing treatment, two or more coating compositions may be applied in layers. For example, it is preferable to apply a coating composition listed as being used for the bonding layer (cn) described below as the first layer (lower layer) and a coating composition used for the test coating layer (sp) as the second layer (upper layer).

[0125] In cases where it is undesirable for the surface of the target to have unevenness, the unevenness can be smoothed out by such sealing or overlapping treatment. In addition, such sealing treatment has the advantage that, in addition to preventing peeling from the substrate, the position where the coating sheet to be investigated was attached can be confirmed after peeling, and if peeling is thought to be artificial based on the surrounding circumstances, it can be assumed.

[0126] When carrying out this sealing treatment, in order to prevent the coating composition used in the sealing treatment from adhering to the test coating layer (sp), it is preferable that a release layer (rl) is provided on the test coating layer (af). In this case, it is preferable that the release layer (rl) is fixed with something that is easy to peel off, such as masking tape.

[0127] In addition, when multiple coating sheets for investigation are arranged and attached, sealing tape may be attached so as to cover the ends of adjacent sheets by a method such as that described in JP 2016-124994 A.

[0128] The survey coating sheet may be applied to multiple locations of the object, and in particular, when the object is placed in different environments depending on the location, it is preferable to apply a survey coating sheet to each environment. For example, in the case of the bottom of a ship, the conditions of sunlight, temperature, water current, etc. are different between the vertical and flat bottom of the ship, so the types and amounts of marine organisms that adhere to the bottom of the ship are different, and therefore the suitable antifouling paint for the bottom of the ship is not necessarily the same for each location. For this reason, it is preferable to conduct the survey by applying a survey coating sheet to each location. In the case of the bottom of the ship, in addition to this, the survey coating sheet may be applied to the bow, center, and stern of the ship, since the influence of the water current is significantly different, and the survey coating sheet may be applied to the propeller blade surface, shaft, rudder, sea chest, bilge keel, and their surroundings, which are placed in different environments from the general part.

[0129] In addition, when the target is a ship or other moving body, it is also possible to carry out the coating evaluation method of the present invention by carrying out the application step and the subsequent exposure step and information acquisition step not on the target itself that is to be coated with the same type of coating as the test coating layer (sp), but on another target that has a similar movement pattern (navigation pattern, route, etc.) to the target.

[0130] [(ii) Exposure process] The exposure step (ii) carried out after the attachment step (i) is a step of placing the test coating layer (sp) in an environment in which the object is placed for a certain period of time with at least a part of the test coating layer (sp) exposed on the surface. This step allows the test coating layer (sp) to actually be affected and changed in the environment as the coating would be if the object were covered with the same type of coating. For example, in the case of a coating sheet for investigating anti-bottom paint for ships, the coating sheet for investigation attached to the bottom of a ship is immersed in water to place it in an environment where aquatic organisms attach to the coating and the coating deteriorates due to water and sunlight.

[0131] The duration of the exposure step (ii) may be the same as, or may be shorter or longer than, the expected period of protective effect of the coating. For example, antifouling paint is generally expected to be effective over the interval between docking or laying out of a ship, but a short exposure step may be carried out to estimate the expected period of effect from the changes in condition during that period.

[0132] [(iii) Information acquisition process] The information acquisition step (iii) carried out after the exposure step (ii) is a step for acquiring information on the state of the coating sheet to be investigated.

[0133] The information to be obtained includes, for example, the color of the test coating layer (sp), the appearance such as gloss, surface adhesions and their amount, the shape such as cracks and scratches, the surface roughness of the coating film, the thickness (film thickness) of the coating film, the thickness of the altered layer on the coating film surface, and chemical information of the components contained in the coating film. For example, in the case of a coating film sheet for investigating antifouling paint for ship bottoms, information on the adhesions and their amount on the surface indicates the antifouling performance, the film thickness indicates the renewal speed in the case of antifouling paint for ship bottoms that is of the type in which the coating film is renewed as described above, and the presence or absence of scratches and the surface roughness of the coating film are also useful references.

[0134] Methods for obtaining information include visual inspection of the appearance and surface deposits and their amount, and obtaining image information captured by a recording device such as a camera, and the method of obtaining image information is preferable in terms of transmitting and recording information. The image information may be a still image or a moving image, and the recording device may be an underwater camera if the recording device is underwater, or a recording device that uses infrared light, near-infrared light, ultraviolet light, etc., may be used as appropriate when taking pictures in dark places, etc.

[0135] When acquiring image information, if the coating sheet to be investigated has an indication layer (id), it is preferable to record this in the image information as well.

[0136] A color difference meter or a gloss meter may be used to measure the color and gloss of the coating film.

[0137] Methods for obtaining information on the adhesions and amount of material on the coating surface, the shape of cracks and scratches, and the surface roughness of the coating can be performed by visual inspection or by using a laser roughness meter as described in International Publication WO2018 / 021210.

[0138] Methods for obtaining film thickness information include, for example, a method of cutting out the coating film and measuring its cross section, a method of making an incision in the coating film at a specific inclination angle from the front of the coating film and measuring from the cross section, a method of measuring using an electromagnetic film thickness meter when the coating sheet to be investigated has a layer containing a corresponding metal between the test coating layer (sp) and the target, and a method of measuring using the difference in hue between the test coating layer (sp) and the coating layer adjacent to it.

[0139] When measuring film thickness using an electromagnetic film thickness gauge, the electromagnetic induction type, eddy current type, or dual type can be used depending on the magnetism of the layer involved.

[0140] As a method for measuring the film thickness by utilizing the difference in hue between the test coating layer (sp) and the coating layer adjacent to it, for example, a method utilizing the exposure of the lower coating layer as described in U.S. Patent No. 7,739,974 and International Publication WO2019 / 244299 can be used.

[0141] Depending on the test coating layer (sp), when it is placed in the environment in which it is used, the coating may change in quality from the surface to a certain depth direction. Information on this coating thickness may be obtained, and a method for doing so may include, for example, cutting out the coating as described above and measuring its cross section.

[0142] Methods for obtaining chemical information on the components contained in the coating film include, for example, various spectroscopic analyses such as infrared spectroscopy, contact angle measurement, mass spectrometry, and X-ray fluorescence analysis.

[0143] As information on the coating, in addition to the test coating layer (sp), information on the state of other layers such as the protective layer (pr), substrate layer (bs), and display layer (id) may also be obtained.

[0144] [Subsequent process] The coating evaluation method of the present invention further includes (iv) a step of evaluating the performance of each layer of the coating sheet to be investigated based on the information acquired in the information acquisition step (iii) and determining a coating method recommended for the target, for example, a step of selecting a recommended blending composition of the coating composition to be applied and a recommended film thickness (referred to as a "recommendation step" in this specification). The evaluation, selection, recommendation, etc. processes in the recommendation step (iv) may be performed using a computer as necessary, or may be performed automatically mechanically. For example, the information acquired in the information acquisition step (iii) may be transmitted to a computer that executes the recommendation step (iv) by an electronic method, and the results of the evaluation, selection, recommendation, etc. of the coating composition based on the information may also be transmitted by an electronic method. In addition, when the information and results from these steps are accumulated as a database, they may be stored together with other information regarding the environment in which the coating film is placed, and the database including such additional information may be utilized for evaluation, selection, recommendation, etc. of the coating composition according to the environment.

[0145] After evaluation using the coating sheet for investigation of the present invention, the sheet may be peeled off from the object and collected as necessary, or may be left attached as is, or a coating composition may be applied over the sheet. When the sheet is peeled off from the object and collected, the collected coating may be analyzed.

[0146] -Other aspects of the present invention- The investigational coating sheets and coating evaluation methods described herein can be converted into inventions of different categories based on patent practice and common general technical knowledge.

[0147] For example, in one aspect, the present invention provides "a use (method) of an investigation coating sheet having at least one test coating layer (sp) for evaluating the performance of a coating, the use comprising: (i) attaching the investigation coating sheet having at least one test coating layer (sp) that is not formed around an object to be covered with a coating, (ii) placing the investigation coating sheet in an environment in which the object is placed for a certain period of time with at least a part of the test coating layer (sp) exposed on the surface, and (iii) acquiring information regarding the state of the investigation coating sheet." Regarding various technical matters related to the invention relating to such "use," the various technical matters described in this specification as related to the invention relating to the "investigation coating sheet" and / or the "coating evaluation method" can basically be applied (the description can be read differently).

[0148] In one aspect of the present invention, a coating sheet for investigation having at least one test coating layer (sp) and an indicator layer (id) that are not formed around the surroundings can be used for purposes other than investigation, i.e., for purposes other than use in the coating evaluation method of the present invention. That is, in one aspect, the present invention provides a coating sheet having at least one test coating layer (sp) and an indicator layer (id) that are not formed around the surroundings (whether for investigation or for other purposes is not limited, and has both uses).

[0149] In one aspect of the present invention, a coating sheet for investigation having two or more different test coating layers (sp) that are not formed around the surroundings can be used for purposes other than investigation, i.e., for purposes other than use in the coating evaluation method of the present invention. That is, in one aspect, the present invention provides a coating sheet having two or more different test coating layers (sp) that are not formed around the surroundings (whether for investigation or for other purposes is not limited, and can be used for both purposes). EXAMPLES

[0150] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.

[0151] The "solid content" of each component described in the examples refers to the components excluding the volatile components contained in each component as a solvent, and the material obtained by drying each component in a hot air dryer at 125°C for 1 hour is considered to be the "solid content," and the ratio to the mass of each component before drying is calculated. The "Gardner viscosity" described in the examples is the value obtained by measuring each component at a liquid temperature of 25°C using a Gardner bubble viscometer. Furthermore, the "viscosity (mPa s)" is the value obtained by measuring each component at a liquid temperature of 25°C using an E-type viscometer (TV-25, manufactured by Toki Sangyo Co., Ltd.).

[0152] <Binder Production Example 1: Production of Metal Ester Group-Containing Hydrolyzable Copolymer Solution (A-1)> [Production Example M1: Production of Metal Ester Group-Containing Monomer Mixture (M1)] In a four-neck flask equipped with a condenser, a thermometer, a dropping funnel and a stirrer, 85.4 parts by mass of PGM (propylene glycol monomethyl ether) and 40.7 parts by mass of zinc oxide were charged and heated to 75°C while stirring. Then, a mixture consisting of 43.1 parts by mass of methacrylic acid, 36.1 parts by mass of acrylic acid and 5 parts by mass of water was dropped at a constant rate from the dropping funnel over 3 hours. After further stirring for 2 hours, 36 parts by mass of PGM was added to obtain a transparent metal ester group-containing monomer mixture M1. The solid content was 44.8% by mass.

[0153] In a pressure-polymerizable autoclave equipped with a cooler, a thermometer, a dropping tank, and a stirrer, 15 parts by mass of PGM (propylene glycol methyl ether), 60 parts by mass of xylene, and 4 parts by mass of ethyl acrylate were charged, and the mixture was pressurized to 350 kPa with stirring and heated to 135° C. Subsequently, a transparent mixture consisting of 15 parts by mass of methyl methacrylate, 48 parts by mass of ethyl acrylate, 15 parts by mass of n-butyl acrylate, 40 parts by mass of the metal ester group-containing monomer mixture (M1) obtained in Production Example M1, 10 parts by mass of xylene, 1.2 parts by mass of a chain transfer agent (NOFMER MSD manufactured by NOF Corporation), 3 parts by mass of 2,2'-azobisisobutyronitrile (hereinafter also referred to as AIBN), and 1 part by mass of 2,2'-azobis(2-methylbutyronitrile) (hereinafter also referred to as AMBN) was dropped at a constant speed from the dropping tank over 3 hours. After the dropwise addition, the temperature was lowered to 110°C over 30 minutes, 0.5 parts by mass of t-butyl peroctoate and 7 parts by mass of xylene were dropped over 30 minutes, and the mixture was stirred for another 1 hour and 30 minutes, after which 8 parts by mass of xylene was added. The resulting solution was filtered through a 300 mesh to obtain a pale yellow transparent hydrolyzable copolymer solution (A-1) with no insoluble matter, a heating residue of 45.7%, and a Gardner viscosity of +V.

[0154] <Binder Production Example 2: Production of Silyl Ester Group-Containing Hydrolyzable Copolymer Solution (A-2)> All reaction steps were carried out under a nitrogen stream. 53.85 parts by mass of xylene was charged into a reaction vessel equipped with a stirrer, condenser, thermometer, dropping device, nitrogen inlet tube, and heating / cooling jacket, and heated to 80±3°C while stirring. While maintaining the same temperature, a monomer mixture consisting of 50.0 parts by mass of triisopropylsilyl methacrylate, 28.0 parts by mass of methoxyethyl methacrylate, 14.0 parts by mass of methyl methacrylate, 8.0 parts by mass of butyl acrylate, and 1.3 parts by mass of AIBN was dropped into the reaction vessel from the dropping device over 2 hours. After stirring for 1 hour at the same temperature and for 1 hour at 85°C, the temperature was raised to 105°C over 3 hours while adding 0.4 parts by mass of AIBN in 4 portions. 12.81 parts by mass of xylene was added to the obtained reaction solution to obtain a pale yellow transparent hydrolyzable copolymer solution (A-2) with a heating residue of 60.6% and a viscosity of 1765 mPa·s.

[0155] <Binder Production Example 3: Production of Curable Silicone Mixture (A-4)> Oxime group-containing silicone (MEKO)2(CH2=CH-)SiO-[Si(CH3)2-O-] with a viscosity of 1500mPa·s n 100 parts by mass of -Si(CH=CH2)(MEKO)2 (wherein "MEKO" represents a 2-methylethylketoxime group) was kneaded with 10 parts by mass of "AEROSIL 200" (untreated silica) manufactured by Nippon Aerosil Co., Ltd. to obtain a curable silicone mixture (A-4) with a viscosity of 40 mPa s.

[0156] <Binder Production Example 4: Production of Curable Silicone Mixture (A-5)> Oxime group-containing silicone (MEKO)2(CH2=CH-)SiO-[Si(CH3)2-O-] with a viscosity of 1500mPa·s n 100 parts by mass of -Si(CH=CH2)(MEKO)2 (wherein "MEKO" represents a 2-methylethylketoxime group) was kneaded with 10 parts by mass of "AEROSIL RX200" (hydrophobic treated silica) manufactured by Nippon Aerosil Co., Ltd. to obtain a curable silicone mixture (A-5) with a viscosity of 800 mPa s.

[0157] <Synthesis of acrylic polymer (D-1) having hydrophilic groups> Synthesis Example 1 (Synthesis of Polymer (D-1)) The reaction was carried out under normal pressure and nitrogen atmosphere. 42.86 parts by mass of methyl amyl ketone was charged into a reaction vessel equipped with a stirrer, reflux condenser, thermometer, nitrogen inlet tube, and dropping funnel, and heated with stirring until the methyl amyl ketone reached 100°C. While maintaining the temperature of the reaction mixture at 100±5°C, a mixture consisting of 40.0 parts by mass of NK Ester AM-90G (methoxypolyethylene glycol acrylate, average number of polyethylene glycol units 9, manufactured by Shin-Nakamura Chemical Co., Ltd.), 60.0 parts by mass of isobutyl acrylate, and 4.0 parts by mass of AMBN was dropped into the reaction vessel over 4 hours. After that, the mixture was stirred for 2 hours while maintaining the temperature at 100±5°C, and a solution of polymer (D-1) was obtained. The solid content of the obtained solution was 70.3% by mass, and the viscosity was 109 mPa·s.

[0158] Details of each component used in the following paint production examples are shown in Table 1. [Table 1]

[0159] <Preparation of antifouling coating compositions C1 to C8> Antifouling coating compositions C1 to C8 were prepared by mixing and stirring the components in the amounts (parts by mass) shown in Tables 2 and 3. The amount of each component shown in Table 2 indicates the amount blended in its entirety. For example, in Example 1, the amount of fatty acid amide blended in its entirety (as a whole) was 1.5 parts by mass, and the solid content was 20% by mass, so the amount of fatty acid amide itself blended was 0.3 parts by mass.

[0160] [Table 2]

[0161] [Table 3]

[0162] <Preparation of coating composition C9 for bonding layer (cn)> A coating composition C9 for the bonding layer was prepared by mixing and stirring each component in the amounts (parts by mass) shown in Table 4. When applying this coating composition, the base agent and curing agent are mixed and stirred before use.

[0163] [Table 4]

[0164] <Preparation of a member having an adhesive layer (ad) sandwiched between release layers (rl)> A reaction vessel equipped with a cooling tube, a nitrogen inlet tube, a thermometer, a dropping device, a heating / cooling jacket, and a stirrer was charged with 30 parts by mass of methyl ethyl ketone, and while maintaining the temperature at 80±5°C under a nitrogen stream, a mixture consisting of 90 parts by mass of 2-ethylhexyl acrylate (manufactured by Nippon Shokubai Co., Ltd., "AEH"), 10 parts by mass of acrylic acid (manufactured by Toa Gosei Co., Ltd., "98% acrylic acid"), 1 part by mass of 2,2'-azobis(2,4-dimethylvaleronitrile) (manufactured by Nippon Finechem Co., Ltd., "ABN-V") as a polymerization initiator, and 16 parts by mass of methyl ethyl ketone was dropped over 1 hour from the dropping device. After that, the mixture was stirred at the same temperature for 1 hour, and then the methyl ethyl ketone was removed by vacuum distillation, and 90 parts by mass of 2-ethylhexyl acrylate (manufactured by Nippon Shokubai Co., Ltd., "AEH") and 10 parts by mass of acrylic acid (manufactured by Toa Gosei Co., Ltd., and "98% acrylic acid") were added to obtain an acrylic monomer mixture. To 100 parts by mass of this acrylic monomer mixture, 0.1 parts by mass of 2,2-dimethoxy-1,2-diphenylethan-1-one (BASF Japan Ltd., "Irgacure 651") as a photopolymerization initiator and 0.5 parts by mass of 1,6-hexanediol diacrylate (MIWON, "MIRAMER M200") as a crosslinking agent were added, and this was applied to the release surface of a release film (silicone-treated PET film, 50 μm thick, Mitsui Chemicals Tohcello Inc., "SP-PET-O1-50-BU") with a film applicator, and the release surface of the same release film as above was laminated on top of it. Furthermore, ultraviolet light was irradiated from an ultraviolet lamp (mercury lamp) (ultraviolet illuminance: 50 mW / cm 2 , cumulative irradiation dose: 2000mJ / cm 2) to obtain an acrylic pressure-sensitive adhesive layer 1 having an average thickness of 50 μm sandwiched between two release films.

[0165] <Preparation of coating sheet for investigation> [Example 1] The antifouling coating composition C1 was applied to the release surface of a 20 cm square release film (silicone-treated PET film, 50 μm thick, Mitsui Chemicals Tohcello Co., Ltd. "SP-PET-O1-50-BU", corresponding to the release layer (rl)) using a film applicator, and dried at room temperature for 1 hour and at 50°C for 24 hours to form a C1 coating film (corresponding to the test coating layer (sp)) with a thickness of about 200 μm. Next, this C1 coating film was covered with double-sided tape (Nitto Denko Corporation "Multipurpose double-sided adhesive tape No. 5015", substrate: nonwoven fabric, adhesive: acrylic, tape thickness 0.12 mm, with release paper on one side, corresponding to the substrate layer (bs) and two adhesive layers (ad)) to prepare a coating sheet for investigation. The layered structure of this coating sheet is shown in Figure 1 and Table 5. The sixth layer, the release layer (RL), is peeled off and the fifth layer, the adhesive layer (AD), is attached to the object to be investigated. The first layer, the release layer (RL), is peeled off and the second layer, the test coating layer (SP), is exposed to the environment in which the object will be placed, and the suitability of the test coating layer (SP) in that environment can be evaluated.

[0166] [Table 5]

[0167] [Example 2] The antifouling coating composition C2 was applied to the release surface of a 20 cm square release film (silicone-treated PET film, 50 μm thick, Mitsui Chemicals Tohcello Co., Ltd. "SP-PET-O1-50-BU". Corresponding to the release layer (rl)) using a film applicator, and dried at room temperature for 1 hour and at 50 ° C for 24 hours to form a C2 coating film (corresponding to the test coating layer (sp)) with a thickness of about 200 μm. Next, a mixture of the main agent and hardener of the bonding layer coating composition C9 was applied on top of this C2 coating film using a film applicator, and dried at room temperature for 1 hour and at 50 ° C for 24 hours to form a C9 coating film (corresponding to the bonding layer (cn)) with a thickness of about 100 μm. This C9 coating was covered with double-sided tape (Teraoka Seisakusho Co., Ltd. "Airtight and waterproof acrylic double-sided tape", base material: polyethylene cloth, adhesive: acrylic, tape thickness: 0.22 mm, with release paper on one side. Corresponding to the base material layer (bs) and two adhesive layers (ad)) to prepare a coating sheet for investigation. The layered structure of this coating sheet is shown in Figure 2 and Table 6. The sixth layer, the release layer (rl), is peeled off and the fifth layer, the adhesive layer (ad), is attached to the object to be investigated. The first layer, the release layer (rl), is peeled off and the second layer, the test coating layer (sp), is exposed to the environment in which the object will be placed, allowing the suitability of the test coating layer (sp) in that environment to be evaluated.

[0168] [Table 6]

[0169] [Example 3] A mixture of the base material and the cured product of the bonding layer coating composition C9 was applied to the release surface of a release film (silicone-treated PET film, 50 μm thick, manufactured by Mitsui Chemicals Tohcello Co., Ltd., "SP-PET-O1-50-BU"; equivalent to the release layer (rl)) measuring 20 cm x 50 cm, using a film applicator, and dried at room temperature for 1 hour and at 50°C for 24 hours to form a C9 coating film with a thickness of about 200 μm. In this embodiment, the C9 coating film serves as both the bonding layer (cn) and the substrate layer (bs). On this C9 coating film, antifouling coating compositions C1, C2, C3, and C4 were applied from the left as the test coating film layer (sp) in the arrangement shown in FIG. 3 using a film applicator, and dried at room temperature for 24 hours to form C1 to C4 coating films with a thickness of 200 μm. On the areas other than the areas where these test coating layers (sp) were applied, antifouling paint composition C1 was applied with a brush so that the dry film thickness was about 200 μm, and the coating film C1 was formed by drying at room temperature for 1 hour and at 50° C. for 24 hours, and was used as a protective layer (pr). The dashed lines in FIG. 3 indicate the position of the cross-sectional structure shown in the following FIG. 4. After that, a part of this protective layer (pr) was painted with paint composition C5 with a brush so that the dry film thickness was 200 μm, while removing the edges with masking tape in the arrangement shown in FIG. 3, to form an indication layer (id).

[0170] The release film in contact with the surface of the C9 coating film (third layer: bonding layer (cn) and substrate layer (bs)) that is not in contact with the C1 coating film (test coating film layer (sp)) was peeled off, and the release film on one side of the member having the acrylic pressure-sensitive adhesive layer sandwiched between the two release films was peeled off and the surface was attached to this surface. The laminate structure of the coating film sheet for investigation of this example produced in this way is as shown in Figure 4 at the portion indicated by the dashed line in Figure 3.

[0171] The laminated structure of the coating sheet for investigation in this embodiment is as shown in Table 7. The fifth release layer (rl) is peeled off and the fourth adhesive layer (ad) is attached to the object to be investigated, and the first release layer (rl) is peeled off and the first test coating layer (sp) is exposed to the environment in which the object will be placed, so that the suitability of the test coating layer (sp) in that environment can be evaluated.

[0172] [Table 7]

[0173] [Example 4] A piece of "Silicone Rubber Adhesive Tape No. 9013" manufactured by Teraoka Seisakusho Co., Ltd. (having a laminated structure of silicone rubber-polyester film-acrylic adhesive, total thickness 0.10 mm, adhesive strength 18.8 N / width 25 mm) was cut into a size of 30 cm x 50 cm. The release surface of a release film (silicone-treated PET film, thickness 50 μm, manufactured by Mitsui Chemicals Tohcello Co., Ltd., "SP-PET-O1-50-BU") was attached to the side of the tape having the acrylic adhesive. Then, the antifouling coating compositions C6 and C7 were applied from the left to the side of the tape having the silicone rubber in the arrangement shown in FIG. 5 as the test coating layer (sp) using a film applicator, and the coating was dried at room temperature for 1 hour and at 50°C for 24 hours to form the C6 and C7 coating films with a thickness of 200 μm. On the other parts than the parts coated with the test coating film layer (sp), the antifouling paint composition C8 was applied with a brush so that the dry film thickness was about 100 μm, and the coating film C8 was formed by drying at room temperature for 1 hour and at 50° C. for 24 hours, and used as the protective layer (pr). The dashed line in FIG. 5 indicates the position of the cross-sectional structure shown in FIG. 4.

[0174] The laminated structure of the coating sheet for investigation in this example is as shown in FIG. 6 in the area indicated by the dashed line in FIG.

[0175] The laminated structure of the coating sheet for investigation in this embodiment is as shown in Table 8. The fifth release layer (rl) is peeled off and the fourth adhesive layer (ad) is attached to the object to be investigated, and the first release layer (rl) is peeled off and the first test coating layer (sp) is exposed to the environment in which the object will be placed, thereby enabling the suitability of the test coating layer (sp) in that environment to be evaluated.

[0176] [Table 8]

[0177] [Example 5] An addition-curing silicone adhesive (a mixture of 100 parts by mass of Dow Corning Toray SD 4592 PSA (vinyl group-containing silicone), 1.0 parts by mass of BY24-742 (Si-H compound), 0.9 parts by mass of NC-25 CATALYST (platinum catalyst), and 50 parts by mass of toluene, manufactured by Dow Corning Toray Co., Ltd., was applied to one side of a 30 cm square stainless steel (SUS430) foil (corresponding to the base layer (bs)) using a film applicator, and dried (cured) for 5 minutes at 100°C to form a 100 μm thick silicone-based pressure-sensitive adhesive layer (corresponding to the adhesive layer (ad)). The surface of this silicone-based pressure-sensitive adhesive layer was bonded to the surface of a fluorine-type release film (PET film with fluorosilicone release agent, 50 μm thick, "FSC6" manufactured by Nippa Co., Ltd., peel load 70 mN, corresponding to the release layer (rl)). Next, the surface of the stainless steel foil on which the silicone-based pressure-sensitive adhesive layer was not formed was polished using #240 sandpaper, washed with xylene, and then the mixture of the base agent and the curing agent of the bonding layer coating composition C9 was spray-painted to a dry film thickness of 100 μm, and dried at room temperature for 24 hours to form a bonding layer (cn). After the end of the formed bonding layer (cn) was cured with masking tape in a 1 cm wide area, the antifouling coating composition C4 was spray-painted on the uncured area to a dry film thickness of about 200 μm, and dried at room temperature for 1 hour and at 50 ° C for 24 hours to form a test coating layer (sp). Then, a release paper as a release layer (rl) was attached so that the release surface faced the test coating layer (sp) so as to cover the test coating layer (sp), and a coating sheet for investigation was obtained.

[0178] The laminated structure of the coating sheet for investigation in this example was finally as shown in FIG. 8 at the portion indicated by the dashed line in FIG.

[0179] The laminated structure of the coating film sheet for investigation in this embodiment is as shown in Table 9. The sixth layer of release layer (rl) is peeled off, and the fifth layer of adhesive layer (ad) is attached to the object to be investigated, and the surroundings of the attached area and the third layer of bonding layer (cn) are painted with the paint composition (for example, an antifouling paint composition different from the antifouling paint composition C1) that is applied to the object to be affixed to, and sealed. The first layer of release layer (rl) is then peeled off, and the second layer of test coating film layer (sp) is exposed to the environment in which the object is placed, whereby the suitability of the test coating film layer (sp) in that environment can be evaluated.

[0180] [Table 9]

[0181] [Example 6] One side of a 30 cm square PVC board (corresponding to the base layer (bs)) with a thickness of 0.3 mm was surface-polished using #240 sandpaper, washed with xylene, and then spray-painted with a mixture of the base agent and curing agent of the bonding layer coating composition C9 so that the dry film thickness was 100 μm, and dried at room temperature for 24 hours to form a bonding layer (cn). After curing a 1 cm wide area at the end of the formed bonding layer (cn) with masking tape, the antifouling coating composition C4 was spray-painted on the uncured area so that the dry film thickness was about 200 μm, and dried at room temperature for 1 hour and at 50 ° C for 24 hours to form a test coating layer (sp). Thereafter, a release paper as a release layer (rl) was attached using masking tape so that the release surface faced the test coating layer (sp) so as to cover the test coating layer (sp). Next, the unpainted surface of the PVC board was covered with double-sided tape ("Cut Ace" manufactured by Sumika Plastec Co., Ltd., base material: polyethylene, adhesive: acrylic, tape thickness 0.1 mm, with release paper on one side, corresponding to the base material layer (bs) and two adhesive layers (ad)) to prepare a coating sheet for investigation.

[0182] The laminated structure of the coating sheet for investigation in this example was finally as shown in FIG. 10 at the portion indicated by the dashed line in FIG.

[0183] The laminated structure of the coating sheet for investigation in this embodiment is as shown in Table 10. The release layer (rl) of the 8th layer is peeled off and the 7th adhesive layer (ad) is attached to the object to be investigated, and the periphery of the affixed area and the periphery of the bonding layer (cn) of the 3rd layer are painted with a mixture of the base agent and hardener of the bonding layer coating composition C9, dried and hardened to seal, and then the coating composition that is applied to the object to be affixed (for example, an antifouling coating composition different from the antifouling coating composition C4) is painted, and the release layer (rl) of the 1st layer is peeled off and the test coating layer (sp) of the 1st layer is exposed to the environment in which the object is placed, so that the suitability of the test coating layer (sp) in that environment can be evaluated.

[0184] [Table 10]

Claims

1. (i) applying to an object to be coated with a coating or to a substitute object a coating sheet to be investigated having at least one coating layer (sp) to be tested that is not formed around it; (ii) placing at least a portion of the test coating layer (sp) exposed on the surface in an environment in which the object is placed for a certain period of time; and (iii) acquiring information regarding the state of the coating sheet for investigation; A method for evaluating the performance of a coating film, comprising:

2. The method according to claim 1, wherein the coating sheet for investigation further comprises an adhesive layer (ad).

3. The method of claim 2 , wherein the adhesive layer (ad) comprises a pressure sensitive adhesive.

4. The method according to claim 1, wherein the coating sheet to be investigated further comprises a substrate layer (bs).

5. The method of claim 4 , wherein the substrate layer (bs) comprises a metal.

6. The method according to claim 1, wherein the coating sheet for investigation further comprises an indication layer (id).

7. The method according to claim 1, wherein the investigation coating sheet has two or more different test coating layers (sp) different from each other.

8. 2. The method of claim 1, wherein step (i) further comprises sealing the perimeter of the investigational coating sheet with a coating composition.

9. The method of claim 1 , wherein step (iii) comprises taking a photograph and transmitting the photograph electronically.

10. The method of claim 1 , wherein the object is an underwater structure.

11. The method of claim 1 , wherein the object is a watercraft.

12. The method of claim 1 , wherein the object is a moving object.

13. 10. The method of claim 9, further comprising the step of determining a recommended coating method for the object based on the information obtained in step (iii).

14. A coating sheet having at least one test coating layer (sp) and an indicator layer (id) that are not formed around the periphery.

15. A coating sheet having two or more different test coating layers (sp) that are not formed around it.

Citation Information

Patent Citations

  • Antifouling performance evaluation method by quantitative analysis of attached matters, and antifouling performance evaluation system

    JP2018167654A